Manufacturing method of resin film

A controlled manufacturing process for resin films with crystalline polymers enhances slipperiness by pre-stretching, heating, and stretching to specific conditions, resulting in films with low friction and minimal haze.

JP7572144B2Active Publication Date: 2024-10-23ZEON CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2019178380
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-09-30
Publication Date
2024-10-23
Estimated Expiration
2039-09-30

AI Technical Summary

Technical Problem

Conventional methods for manufacturing resin films with crystalline polymers containing an alicyclic structure struggle to achieve excellent slip properties.

Method used

A manufacturing method involving pre-stretching a film made of crystalline resin containing an alicyclic structure, followed by controlled heating, stretching, and cooling to specific temperature and time parameters, with optional intermediate layers of thermoplastic resin, to create a resin film with enhanced slipperiness.

Benefits of technology

The method produces a resin film with a static friction coefficient of 0.7 or less, internal haze of 1.0% or less, and minimal coloration, achieving excellent slip properties and transparency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572144000001
    Figure 0007572144000001
  • Figure 0007572144000002
    Figure 0007572144000002
Patent Text Reader

Abstract

To provide a manufacturing method capable of easily manufacturing a resin film that excels in slipperiness.SOLUTION: A manufacturing method for a resin film includes the steps for: 1 preparing a pre-stretched film provided with a resin layer comprising a crystalline resin that includes a crystalline polymer containing an alicyclic structure; 2 heating the pre-stretched film at a specific temperature Tp in a specific time tp; 3 stretching the pre-stretched film at a specific stretch temperature Ts by a specific area ratio to obtain a stretched film; and 4 lowering a temperature of the stretched film to a room temperature. After obtaining the stretched film in the step 3, a temperature of the stretched film is maintained to Ts or lower until the temperature of the stretched film reaches the room temperature in the step 4.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a resin film, and a resin film. [Background technology]

[0002] Regarding a film of a resin containing a polymer having an alicyclic structure and crystallinity, a technique is known in which the film is heated to promote crystallization of the polymer. For example, Patent Documents 1 to 3 propose a technique for producing a film by stretching a film of a resin containing a polymer having an alicyclic structure and crystallinity, and then heating the film to promote crystallization (see Patent Documents 1 to 3). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2016 / 052303 [Patent Document 2] International Publication No. 2018 / 061841 [Patent Document 3] International Publication No. 2018 / 062067 Summary of the Invention [Problem to be solved by the invention]

[0004] However, in the conventional manufacturing method for producing a film using a resin containing a polymer having an alicyclic structure and crystallinity, it has been difficult to produce a resin film having excellent slip properties.

[0005] The present invention has been devised in consideration of the above-mentioned problems, and aims to provide a manufacturing method for producing a resin film having excellent slip properties using a resin containing a polymer that contains an alicyclic structure and has crystallinity, and a resin film produced by the manufacturing method. [Means for solving the problem]

[0006] The present inventors have conducted extensive research to solve the above-mentioned problems, and as a result, have found that the above-mentioned problems can be solved by a production method including step 1 of preparing a pre-stretched film having a crystalline resin layer made of a crystalline resin containing a polymer having an alicyclic structure and crystallinity, step 2 of heating the pre-stretched film at a specific temperature for a specific time, step 3 of stretching the pre-stretched film at a specific stretching temperature and a specific areal ratio to obtain a stretched film, and step 4 of lowering the temperature of the stretched film to room temperature, thereby completing the present invention. That is, the present invention includes the following.

[0007] [1] Step 1 of preparing a pre-stretched film having a resin layer made of a crystalline resin containing a polymer having an alicyclic structure and crystallinity; A step 2 of heating the pre-stretched film at a temperature Tp of not less than "Tc-10°C" and not more than "Tc+35°C" for a time tp (where Tc represents the crystallization peak temperature [°C] of the crystalline resin); A step 3 of stretching the pre-stretched film subjected to the step 2 at a stretching temperature Ts equal to or lower than the temperature Tp at an areal magnification of 1.6 times or more and 6.3 times or less to obtain a stretched film; Step 4 of lowering the temperature of the stretched film to room temperature; The temperature Tp [° C.] and the time tp [seconds] satisfy the following formula (i), 10000≦{Tp-(Tc-15)} 2 ×tp≦30000 (i) A method for producing a resin film, wherein after the stretched film is obtained in step 3, the temperature of the stretched film is maintained at or below Ts until the temperature of the stretched film reaches room temperature in step 4. [2] The method for producing a resin film according to [1], wherein the polymer containing an alicyclic structure and having crystallinity is a hydrogenated product of a ring-opening polymer of dicyclopentadiene. [3] The pre-stretched film has two or more of the resin layers, The method for producing a resin film according to [1] or [2], further comprising providing one or more intermediate layers made of a thermoplastic resin other than the crystalline resin between the resin layers. [4] The method for producing a resin film according to [3], wherein the glass transition temperature of the thermoplastic resin is equal to or higher than the glass transition temperature of the crystalline resin and equal to or lower than "Ts+20°C". [5] A resin film produced by the production method according to any one of [1] to [4], The resin film has a surface having a static friction coefficient of 0.7 or less. [6] The resin film according to [5], wherein the internal haze of the resin film is 1.0% or less. [7] The b of the CIE-Lab color system of the resin film * The resin film according to [5] or [6], wherein the refractive index is 1.0 or less. Effect of the Invention

[0008] According to the present invention, there is provided a manufacturing method for easily producing a resin film having excellent slip properties using a resin containing a polymer that contains an alicyclic structure and has crystallinity, and a resin film produced by the manufacturing method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present invention will be described in detail below with reference to embodiments and examples. However, the present invention is not limited to the embodiments and examples shown below, and may be modified and implemented as desired without departing from the scope of the claims of the present invention and their equivalents.

[0010] In the following description, a "long" film refers to a film having a length of 5 times or more, preferably 10 times or more, the width, specifically a film having a length that can be wound into a roll for storage or transportation. There is no particular upper limit on the length, but it is usually 100,000 times or less the width.

[0011] In the following description, the longitudinal direction of a long film is usually parallel to the film conveying direction in the production line. The MD direction is the film conveying direction in the production line, and is usually parallel to the longitudinal direction of the long film. The TD direction is a direction parallel to the film surface, perpendicular to the MD direction, and usually parallel to the width direction of the long film.

[0012] In the following description, the in-plane retardation Re of the film is a value expressed by Re = (nx - ny) x d, unless otherwise specified. Here, nx represents the refractive index in the direction perpendicular to the thickness direction of the film (in-plane direction) that gives the maximum refractive index. ny represents the refractive index in the in-plane direction perpendicular to the direction of nx. d represents the thickness of the film. The measurement wavelength is 590 nm, unless otherwise specified.

[0013] [1. Overview of resin film manufacturing method] The method for producing a resin film according to one embodiment of the present invention is a method for producing a resin film having a resin layer made of a crystalline resin by using a crystalline resin as a resin containing a polymer having a crystalline structure and an alicyclic structure. In the following description, a polymer having a crystalline structure and an alicyclic structure may be referred to as an "alicyclic crystalline polymer". Also, a resin layer made of a crystalline resin may be referred to as a "crystalline resin layer". The crystalline resin layer is a layer formed by a crystalline resin, and therefore may usually be a layer containing only a crystalline resin.

[0014] A method for producing a resin film according to one embodiment of the present invention includes the steps of: A step 1 of preparing a pre-stretched film having a crystalline resin layer made of a crystalline resin containing an alicyclic crystalline polymer; Step 2 of heating the pre-stretched film at a specific temperature Tp for a specific time tp; A step 3 of stretching the pre-stretched film subjected to the step 2 at a specific stretching temperature Ts and a specific areal ratio to obtain a stretched film; and step 4 of lowering the temperature of the stretched film to room temperature.

[0015] According to this manufacturing method, a resin film having a crystalline resin layer made of a crystalline resin containing an alicyclic crystalline polymer can be obtained. The resin film thus obtained can have excellent slip properties.

[0016] In the following description, the temperature Tp to which the unstretched film is heated in step 2 may be referred to as the "preheating temperature." Also, the time tp for which the unstretched film is heated to the preheating temperature Tp in step 2 may be referred to as the "preheating time."

[0017] [2. Step 1 (Preparation of pre-stretched film)] In step 1, a pre-stretched film having a crystalline resin layer made of a crystalline resin is prepared. The crystalline resin is a resin containing an alicyclic crystalline polymer as a polymer containing an alicyclic structure and having crystallinity, and may contain any component other than the alicyclic crystalline polymer as necessary. This crystalline resin is preferably a thermoplastic resin.

[0018] The polymer containing an alicyclic structure refers to a polymer containing an alicyclic structure in the molecule. Such a polymer containing an alicyclic structure can be, for example, a polymer obtained by polymerization reaction using a cyclic olefin as a monomer, or a hydrogenated product thereof. By using an alicyclic crystalline polymer as the polymer containing an alicyclic structure, the mechanical properties, heat resistance, transparency, low moisture absorption, dimensional stability and light weight of the resin film can be improved.

[0019] Examples of the alicyclic structure include a cycloalkane structure and a cycloalkene structure. Among these, a cycloalkane structure is preferred because it is easy to obtain a resin film having excellent properties such as thermal stability. The number of carbon atoms contained in one alicyclic structure is preferably 4 or more, more preferably 5 or more, and preferably 30 or less, more preferably 20 or less, and particularly preferably 15 or less. When the number of carbon atoms contained in one alicyclic structure is within the above range, mechanical strength, heat resistance, and moldability are highly balanced.

[0020] In the alicyclic crystalline polymer, the ratio of the structural unit containing an alicyclic structure to all structural units is preferably 30% by weight or more, more preferably 50% by weight or more, and particularly preferably 70% by weight or more. When the ratio of the structural unit containing an alicyclic structure is high as described above, heat resistance can be improved. The ratio of the structural unit containing an alicyclic structure to all structural units can be 100% by weight or less. In addition, in the alicyclic crystalline polymer, the remainder other than the structural unit containing an alicyclic structure is not particularly limited and can be appropriately selected according to the purpose of use.

[0021] The alicyclic crystalline polymer has crystallinity. The term "polymer having crystallinity" refers to a polymer having a melting point Tm (i.e., the melting point can be observed by differential scanning calorimetry (DSC)).

[0022] The melting point Tm of the alicyclic crystalline polymer is preferably 200° C. or higher, more preferably 230° C. or higher, and preferably 290° C. or lower. By using an alicyclic crystalline polymer having such a melting point Tm, a resin film having an even better balance between formability and heat resistance can be obtained.

[0023] The melting point Tm of a polymer can be measured by the following method. First, the polymer is melted by heating, and the melted polymer is quenched with dry ice. Then, the melting point Tm of the polymer can be measured by using this polymer as a test specimen at a heating rate of 10° C. / min (heating mode) using a differential scanning calorimeter (DSC).

[0024] Examples of the alicyclic crystalline polymer include the following polymers (α) to (δ): Among these, polymer (β) is preferred because a resin film having excellent heat resistance can be easily obtained from it. Polymer (α): A ring-opening polymer of a cyclic olefin monomer, which has crystallinity. Polymer (β): A hydrogenated product of polymer (α) and has crystallinity. Polymer (γ): An addition polymer of a cyclic olefin monomer, which has crystallinity. Polymer (δ): A hydrogenated polymer (γ) having crystallinity.

[0025] Specifically, the alicyclic crystalline polymer is preferably a dicyclopentadiene ring-opening polymer having crystallinity, and a dicyclopentadiene ring-opening polymer hydrogenation product having crystallinity.Among them, a dicyclopentadiene ring-opening polymer hydrogenation product having crystallinity is particularly preferred.Here, the dicyclopentadiene ring-opening polymer refers to a polymer in which the ratio of dicyclopentadiene-derived structural units to all structural units is usually 50% by weight or more, preferably 70% by weight or more, more preferably 90% by weight or more, and even more preferably 100% by weight.

[0026] The hydrogenated ring-opening polymer of dicyclopentadiene preferably has a high ratio of racemo dyads. Specifically, the ratio of racemo dyads in the repeating units of the hydrogenated ring-opening polymer of dicyclopentadiene is preferably 51% or more, more preferably 70% or more, and particularly preferably 85% or more. A high ratio of racemo dyads indicates high syndiotactic stereoregularity. Therefore, the higher the ratio of racemo dyads, the higher the melting point of the hydrogenated ring-opening polymer of dicyclopentadiene tends to be. The ratio of racemo-dyads is described in the Examples below. 13 It can be determined based on C-NMR spectrum analysis.

[0027] The above polymers (α) to (δ) can be produced, for example, by the production method disclosed in WO 2018 / 062067.

[0028] The weight average molecular weight (Mw) of the alicyclic crystalline polymer is preferably 1,000 or more, more preferably 2,000 or more, and is preferably 1,000,000 or less, more preferably 500,000 or less. The alicyclic crystalline polymer having such a weight average molecular weight has an excellent balance between moldability and heat resistance.

[0029] The molecular weight distribution (Mw / Mn) of the alicyclic crystalline polymer is preferably 1.0 or more, more preferably 1.5 or more, and preferably 4.0 or less, more preferably 3.5 or less. Here, Mn represents the number average molecular weight. The alicyclic crystalline polymer having such a molecular weight distribution has excellent moldability.

[0030] The weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn) of the polymer can be measured in terms of polystyrene by gel permeation chromatography (GPC) using tetrahydrofuran as a developing solvent.

[0031] The crystallinity of the alicyclic crystalline polymer contained in the crystalline resin layer of the pre-stretched film before step 2 is preferably small, from the viewpoint of particularly easily producing a resin film with excellent slip properties. The specific crystallinity is preferably less than 10%, more preferably less than 5%, and particularly preferably less than 3%. In addition, the alicyclic crystalline polymer contained in the crystalline resin layer of the pre-stretched film does not have to be crystallized. The crystallinity of the polymer can be measured by X-ray diffraction.

[0032] The alicyclic crystalline polymer may be used alone or in combination of two or more kinds in any ratio.

[0033] The proportion of the alicyclic crystalline polymer in the crystalline resin is preferably 50% by weight or more, more preferably 70% by weight or more, and particularly preferably 90% by weight or more. When the proportion of the alicyclic crystalline polymer is equal to or more than the lower limit of the above range, the birefringence expression and heat resistance of the resin film can be improved. The upper limit of the proportion of the alicyclic crystalline polymer can be 100% by weight or less.

[0034] The crystalline resin may further contain optional components in combination with the alicyclic crystalline polymer. The optional components include, for example, antioxidants such as phenol-based antioxidants, phosphorus-based antioxidants, and sulfur-based antioxidants; light stabilizers such as hindered amine-based light stabilizers; waxes such as petroleum wax, Fischer-Tropsch wax, and polyalkylene wax; nucleating agents such as sorbitol-based compounds, metal salts of organic phosphoric acids, metal salts of organic carboxylic acids, kaolin, and talc; diaminostilbene derivatives, coumarin derivatives, and azole-based derivatives (e.g., benzoxazole derivatives, benzotriazole derivatives, benzimidazolate derivatives, and benzotriazole derivatives); and benzotriazole derivatives such as benzotriazole derivatives. Examples of the optional components include fluorescent brighteners such as benzothiazole derivatives, carbazole derivatives, pyridine derivatives, naphthalic acid derivatives, and imidazolone derivatives; ultraviolet absorbers such as benzophenone-based ultraviolet absorbers, salicylic acid-based ultraviolet absorbers, and benzotriazole-based ultraviolet absorbers; inorganic fillers such as talc, silica, calcium carbonate, and glass fibers; colorants; flame retardants; flame retardant assistants; antistatic agents; plasticizers; near-infrared absorbers; lubricants; fillers; and any polymer other than alicyclic crystalline polymers, such as soft polymers. One type of optional component may be used alone, or two or more types may be used in any ratio.

[0035] A crystalline resin containing an alicyclic crystalline polymer usually has a crystallization peak temperature Tc. The crystallization peak temperature Tc is not particularly limited, but is preferably 120°C or higher and preferably 220°C or lower.

[0036] A crystalline resin containing an alicyclic crystalline polymer usually has a glass transition temperature Tg. Hereinafter, the glass transition temperature of the crystalline resin may be abbreviated as "Tg(1)" to distinguish it from the glass transition temperatures of other components. The glass transition temperature Tg(1) of the crystalline resin is not particularly limited, but is usually 85°C or higher and usually 170°C or lower.

[0037] The glass transition temperature Tg and the crystallization peak temperature Tc of a resin can be measured by the following method. The resin is heated to 300°C in a nitrogen atmosphere to melt it, and the molten resin is quenched with liquid nitrogen. Using this resin as a sample, a differential scanning calorimeter (DSC) is used to increase the temperature at 10°C / min to determine the glass transition temperature Tg and the crystallization peak temperature Tc of the resin.

[0038] The number of crystalline resin layers in the pre-stretched film may be 1 or 2 or more. When the pre-stretched film has two or more crystalline resin layers, the compositions and thicknesses of the crystalline resin layers may be the same or different.

[0039] The thickness of each crystalline resin layer contained in the pre-stretched film is preferably 5 μm or more, more preferably 10 μm or more, and particularly preferably 15 μm or more, and is preferably 300 μm or less, more preferably 200 μm or less, even more preferably 100 μm or less, and particularly preferably 80 μm or less.

[0040] The pre-stretching film may be a film having only a crystalline resin layer. In this case, a resin film having only a crystalline resin layer can usually be produced. The pre-stretching film may also have an optional layer made of a resin other than a crystalline resin in combination with the crystalline resin layer. In this case, a resin film having a crystalline resin layer and an optional layer in combination can usually be produced.

[0041] The number and position of the optional layer are arbitrary within a range that does not significantly impair the effects of the present invention. For example, the optional layer may be provided on one side of the crystalline resin layer, or the optional layer may be provided on both sides of the crystalline resin layer. When the optional layer is provided on both sides of the crystalline resin layer, for example, the optional layer is peeled off after the fourth step to expose the crystalline resin layer, thereby making it possible to utilize the excellent slipperiness of the exposed crystalline resin layer surface.

[0042] In particular, in a pre-stretched film having two or more crystalline resin layers, the optional layer is preferably provided between the crystalline resin layers. The optional layer provided between the crystalline resin layers in this way may be called an "intermediate layer". The number of intermediate layers may be one or more. By providing an intermediate layer between the crystalline resin layers, the intermediate layer can exhibit mechanical or optical properties while utilizing the excellent slip properties exhibited by the crystalline resin layer. Therefore, a resin film having various properties and excellent slip properties can be obtained depending on the composition of the intermediate layer.

[0043] Any layer such as the intermediate layer may be formed by a thermoplastic resin other than the above-mentioned crystalline resin. Such a thermoplastic resin may usually contain a polymer other than the alicyclic crystalline polymer and, if necessary, any component. Examples of the polymer include a polymer containing an alicyclic structure and not having crystallinity, polyethylene terephthalate, polyethylene naphthalate, an acrylic polymer, a methacrylic polymer, polyethylene, polypropylene, polycarbonate, polystyrene, triacetyl cellulose, polyvinyl chloride, polyimide, polyphenylene sulfide, polytetrafluoroethylene, polyether ether ketone, polyether sulfone, aramid, and combinations thereof. Among these, a polymer containing an alicyclic structure and not having crystallinity is preferred from the viewpoints of excellent adhesion to the crystalline resin layer, high orientation control, transparency, low moisture absorption, dimensional stability, and light weight. As a polymer containing an alicyclic structure and not having crystallinity, a norbornene-based polymer is more preferred. These polymers may be used alone or in combination of two or more at any ratio.

[0044] Examples of optional components that may be contained in the thermoplastic resin contained in the optional layer include the same examples as the optional components that may be contained in the crystalline resin. In addition, the optional components may be used alone or in combination of two or more kinds in any ratio.

[0045] The thermoplastic resin contained in any layer such as the intermediate layer usually has a glass transition temperature Tg. Hereinafter, the glass transition temperature of this thermoplastic resin may be abbreviated as "Tg(2)" to distinguish it from the glass transition temperature Tg(1) of the crystalline resin. The glass transition temperature Tg(2) of the thermoplastic resin is preferably Tg(1) or higher, more preferably "Tg(1)+10°C" or higher, particularly preferably "Tg(1)+20°C" or higher, and is preferably "Ts+20°C" or lower, more preferably "Ts+15°C" or lower, particularly preferably "Ts+10°C" or lower. The "Ts" represents the stretching temperature of the film before stretching in step 3. When the glass transition temperature Tg(2) of the thermoplastic resin is equal to or higher than the lower limit of the range, breakage during the stretching process can be suppressed. When the glass transition temperature Tg(2) of the thermoplastic resin is equal to or lower than the upper limit of the range, the film thickness controllability after stretching can be sufficiently ensured.

[0046] The thickness of the pre-stretched film can be appropriately set depending on the thickness of the resin film. The specific thickness of the pre-stretched film is preferably 1 μm or more, more preferably 5 μm or more, and is preferably 1 mm or less, more preferably 200 μm or less.

[0047] The pre-stretch film may be a sheet film, but is preferably a long film. By using a long pre-stretch film, the resin film can be continuously produced by the roll-to-roll method, and the productivity of the resin film can be effectively increased.

[0048] There is no limitation on the manufacturing method of the pre-stretched film. Since the pre-stretched film does not contain an organic solvent, the manufacturing method of the pre-stretched film is preferably a resin molding method such as injection molding, extrusion molding, press molding, inflation molding, blow molding, calendar molding, cast molding, compression molding, etc. Among these, the extrusion molding method is preferred because it is easy to control the thickness.

[0049] In addition, a pre-stretched film having a multilayer structure having two or more layers can be produced, for example, by molding resins corresponding to each layer by a co-extrusion molding method. Examples of the co-extrusion molding method include a co-extrusion T-die method, a co-extrusion inflation method, and a co-extrusion lamination method. Among them, the co-extrusion T-die method is preferred. The co-extrusion T-die method includes a feed block method and a multi-manifold method, and the multi-manifold method is particularly preferred in that it can reduce thickness variation.

[0050] The manufacturing conditions in the extrusion molding method are preferably as follows. The cylinder temperature (molten resin temperature) is preferably Tm or higher, more preferably "Tm+20°C" or higher, and preferably "Tm+100°C" or lower, more preferably "Tm+50°C" or lower. The cooling body that the molten resin extruded into a film first comes into contact with is not particularly limited, but a cast roll is usually used. The cast roll temperature is preferably "Tg(1)-50°C" or higher, preferably "Tg(1)+70°C" or lower, more preferably "Tg(1)+40°C" or lower. Furthermore, the cooling roll temperature is preferably "Tg(1)-70°C" or higher, more preferably "Tg(1)-50°C" or higher, and preferably "Tg(1)+60°C" or lower, more preferably "Tg(1)+30°C" or lower. When a pre-stretched film is manufactured under such conditions, a pre-stretched film having a thickness of 1 μm to 1 mm can be easily manufactured. Here, "Tm" represents the melting point of the alicyclic crystalline polymer, and "Tg(1)" represents the glass transition temperature of the crystalline resin.

[0051] [3. Step 2 (preheating step)] After obtaining the pre-stretch film in step 1, step 2 is performed in which the pre-stretch film is heated at a specific pre-heating temperature Tp for a pre-heating time tp. According to step 2, the temperature of the pre-stretch film can be adjusted to about the stretching temperature Ts before performing step 3 described below, so that stretching in step 3 can be performed smoothly. Furthermore, in such step 2, crystallization of the alicyclic crystalline polymer contained in the crystalline resin may partially proceed.

[0052] The preheating temperature Tp is usually "Tc-10°C" or higher, preferably "Tc-5°C" or higher, and usually "Tc+35°C" or lower, preferably "Tc+30°C" or lower, and particularly preferably "Tc+25°C" or lower. "Tc" represents the crystallization peak temperature of the crystalline resin. When the preheating temperature Tp is within the above range, the slipperiness of the resin film obtained by the manufacturing method according to this embodiment can be improved, and furthermore, the internal haze and coloration can usually be reduced.

[0053] The preheating time tp is usually set so that the preheating temperature Tp [°C] and the preheating time tp [seconds] satisfy the following formula (i): In formula (i), the units of the preheating temperature Tp and the crystallization peak temperature Tc of the crystalline resin are "°C", and the unit of the preheating time tp is "seconds". 10000≦{Tp-(Tc-15)} 2 ×tp≦30000 (i)

[0054] More specifically, {Tp-(Tc-15)} 2 The parameter represented by ×tp is usually 10,000 or more, preferably 12,000 or more, particularly preferably 14,000 or more, and usually 30,000 or less, preferably 28,000 or less, more preferably 26,000 or less, particularly preferably 24,000 or less. In the following description, "{Tp-(Tc-15)} 2The parameter represented by "×tp" is sometimes referred to as the "preheating parameter". When the preheating parameter is within the above range, the slipperiness of the resin film obtained by the production method according to this embodiment can be increased, and furthermore, internal haze and coloration can usually be reduced. Furthermore, when the preheating parameter is equal to or greater than the lower limit of the above range, crystallization of the alicyclic crystalline polymer can be promoted in step 2. Furthermore, when the preheating parameter is equal to or less than the upper limit of the above range, excessive progress of crystallization of the alicyclic crystalline polymer can be suppressed.

[0055] Step 2 can be performed, for example, by exposing the pre-stretched film to an atmosphere adjusted to a pre-heating temperature Tp for a pre-heating time tp. In this case, step 2 can be performed by a temperature control device capable of controlling the temperature of the atmosphere of the pre-stretched film, such as an oven. Since the pre-stretched film is generally thin, when the above-mentioned temperature control device is used, the temperature of the pre-stretched film can usually be the same as the temperature of the atmosphere adjusted by the temperature control device. Therefore, the pre-heating temperature Tp can be the same as the set temperature of the temperature control device.

[0056] Alternatively, step 2 can be performed, for example, by contacting the pre-stretched film with a heating section whose temperature is adjusted to the pre-heating temperature Tp for a pre-heating time tp. In this case, step 2 can be performed by a heating device having the heating section, such as a hot plate. When the heating device is used, the temperature of the pre-stretched film can usually be the same as the temperature of the heating section. Therefore, the pre-heating temperature Tp can be the same as the set temperature of the heating device.

[0057] Among them, it is preferable to use an apparatus capable of heating the pre-stretched film in a non-contact manner in step 2. Specific examples of such an apparatus include an oven and a heating furnace.

[0058] As a preferred specific example, step 2 can be performed using a temperature-adjustable oven. For example, step 2 can be performed by storing the unstretched film in an oven and adjusting the temperature of the oven to satisfy the above-mentioned conditions. As another preferred specific example, step 2 can be performed using an oven having a film transport path therein. For example, step 2 can be performed by transporting the pre-stretched film through the film transport path of an oven whose temperature is adjusted to satisfy the above-mentioned conditions for a time period that satisfies the above-mentioned conditions.

[0059] Step 2 is usually carried out so that the pre-stretched film is not substantially stretched. The term "substantially stretched" means that the pre-stretched film is stretched to a stretch ratio of 1.1 or more in any direction.

[0060] Furthermore, in step 2, the pre-stretch film is preferably in a taut state. The term "taut state" of the pre-stretch film refers to a state in which tension is applied to the pre-stretch film. However, this taut state does not include a state in which the pre-stretch film is substantially stretched.

[0061] For example, the pre-stretched film can be put in a tensile state by holding a part or the whole of the pre-stretched film with an appropriate holder. Usually, an edge of the pre-stretched film is held with a holder. The holder may be capable of continuously holding the entire length of the edge of the pre-stretched film, or may be capable of holding it intermittently at intervals. For example, the edge of the pre-stretched film may be held intermittently by holders arranged at predetermined intervals.

[0062] It is preferable that at least two sides of the pre-stretch film are held and put into a tensed state. In this case, deformation of the pre-stretch film due to thermal shrinkage is prevented in the region between the held sides. In order to prevent deformation over a wide area of ​​the pre-stretch film, it is preferable to hold the sides including the two opposing sides and put the region between the held sides into a tensed state. For example, in a rectangular sheet of pre-stretch film, deformation can be prevented over the entire surface of the sheet of pre-stretch film by holding two opposing sides (e.g., the long sides or the short sides) and putting the region between the two sides into a tensed state. In addition, in a long pre-stretch film, deformation can be prevented over the entire surface of the long pre-stretch film by holding two sides (i.e., the long sides) at the ends in the width direction and putting the region between the two sides into a tensed state. In the pre-stretch film prevented from deformation in this way, even if stress occurs in the film due to thermal shrinkage, the occurrence of deformation such as wrinkles is suppressed.

[0063] In order to more reliably suppress deformation due to heating, it is preferable to hold more sides. Thus, for example, in the case of a sheet of pre-stretched film, it is preferable to hold all sides. As a specific example, in the case of a rectangular sheet of pre-stretched film, it is preferable to hold all four sides.

[0064] As a holder capable of holding the sides of the pre-stretched film, one that does not come into contact with the pre-stretched film at any portion other than the sides of the pre-stretched film is preferred. By using such a holder, a resin film having superior smoothness can be obtained.

[0065] In addition, the holders are preferably ones that can fix the relative positions of the holders while they hold the pre-stretched film, since such holders do not move relative to each other, making it easier to suppress substantial stretching of the pre-stretched film.

[0066] Suitable holders include, for example, holders for rectangular pre-stretched films, such as grippers such as clips that are provided at a predetermined interval on a frame material and can grip the sides of the pre-stretched film. Also, for example, holders for holding two sides at the ends in the width direction of a long pre-stretched film include grippers that are provided on a tenter stretching machine and can grip the sides of the pre-stretched film.

[0067] When a long pre-stretched film is used, the side at the end in the longitudinal direction of the pre-stretched film (i.e., the short side) may be held, but instead of holding the side, both sides in the longitudinal direction of the region of the pre-stretched film to be subjected to process 2 may be held. For example, a holding device that can hold the pre-stretched film in a tensed state so as not to cause thermal shrinkage may be provided on both sides in the longitudinal direction of the region of the pre-stretched film to be subjected to process 2. Examples of such a holding device include a combination of two rolls, a combination of an extruder and a take-up roll, and the like. By applying tension such as a conveying tension to the pre-stretched film by these combinations, it is possible to suppress the thermal shrinkage of the pre-stretched film in the region to be subjected to process 2. Therefore, if the above combination is used as a holding device, the pre-stretched film can be held while being conveyed in the longitudinal direction, and therefore a resin film can be efficiently manufactured.

[0068] [4. Process 3 (stretching process)] After step 2, step 3 is performed in which the unstretched film is stretched at a specific stretching temperature Ts and a specific areal ratio. The stretching in step 3 provides a stretched film having a crystalline resin layer and, if necessary, any other layer after stretching. Usually, steps 2 and 3 are performed consecutively, so no other steps are performed between steps 2 and 3.

[0069] The stretching temperature Ts of the film before stretching in step 3 is usually equal to or lower than the preheating temperature Tp. The stretching temperature Ts may be lower than the preheating temperature Tp, for example, equal to or lower than Tp-5°C, equal to or lower than Tp-10°C, etc. The lower limit of the stretching temperature Ts is preferably equal to or higher than "Tg+5°C", more preferably equal to or higher than "Tg+10°C", from the viewpoint of obtaining a resin film having excellent uniformity by sufficiently softening the crystalline resin and performing uniform stretching.

[0070] The areal stretching ratio of the pre-stretched film in step 3 is usually 1.6 times or more, preferably 1.8 times or more, particularly preferably 2.0 times or more, and usually 6.3 times or less, preferably 5.0 times or less, particularly preferably 4.0 times or less. The areal stretching ratio is a stretching ratio expressed as the ratio of the "area of ​​the stretched film" to the "area of ​​the film before stretching", and is therefore expressed by the following formula (ii). Area ratio = {(area of ​​stretched film) / (area of ​​film before stretching)} (ii)

[0071] When the areal stretching ratio in step 3 is within the above range, the slipperiness of the resin film obtained by the manufacturing method according to the present embodiment can be improved, and furthermore, internal haze and coloration can usually be reduced. When the areal stretching ratio is equal to or greater than the lower limit of the above range, the stretching can form sufficiently high unevenness on the surface of the crystalline resin layer. Furthermore, when the areal stretching ratio is equal to or less than the upper limit of the above range, excessive progress of oriented crystallization can be suppressed.

[0072] There is no particular limitation on the stretching method, and any stretching method can be used. For example, uniaxial stretching methods such as a method of uniaxially stretching a pre-stretched film in the longitudinal direction (longitudinal uniaxial stretching method) or a method of uniaxially stretching a pre-stretched film in the width direction (transverse uniaxial stretching method), biaxial stretching methods such as a simultaneous biaxial stretching method in which a pre-stretched film is stretched in the longitudinal direction and at the same time in the width direction, and a sequential biaxial stretching method in which a pre-stretched film is stretched in one of the longitudinal direction and the width direction and then stretched in the other direction, and a method of stretching a pre-stretched film in an oblique direction that is neither parallel nor perpendicular to the width direction (oblique stretching method), etc. can be mentioned.

[0073] The longitudinal uniaxial stretching method may be, for example, a stretching method that utilizes the difference in peripheral speed between rolls. The transverse uniaxial stretching method may be, for example, a stretching method using a tenter stretching machine. Furthermore, examples of the simultaneous biaxial stretching method include a stretching method in which a tenter stretching machine having a plurality of clips that are movably arranged along guide rails and can fix the pre-stretched film is used to stretch the pre-stretched film in the longitudinal direction by opening the clips, and at the same time, the pre-stretched film is stretched in the width direction by the spread angle of the guide rails. In addition, examples of the sequential biaxial stretching method include a stretching method in which a pre-stretched film is stretched in the longitudinal direction by utilizing the difference in peripheral speed between rolls, and then both ends of the pre-stretched film are held with clips and stretched in the width direction by a tenter stretching machine. Further, examples of the oblique stretching method include a stretching method in which a pre-stretched film is continuously stretched in an oblique direction using a tenter stretching machine that can apply a feeding force, a tensile force or a take-up force at different speeds to the left and right in the longitudinal or width direction of the pre-stretched film.

[0074] [5. Process 4 (cooling process)] After step 3, step 4 is performed to lower the temperature of the stretched film to room temperature. Room temperature refers to an environmental temperature where no particular temperature control is performed, and may be, for example, a temperature of 10°C or higher and 40°C or lower. By lowering the temperature of the stretched film to room temperature in this manner, the stretched film can be obtained as a resin film. Usually, steps 3 and 4 are performed consecutively, and no other steps are performed between steps 3 and 4.

[0075] The above-mentioned step 4 is usually carried out so that the temperature of the stretched film is maintained at or below the stretching temperature Ts during the period from when the stretched film is obtained in step 3 until the temperature of the stretched film reaches room temperature in step 4. Thus, step 4 usually does not include a case in which the temperature of the stretched film temporarily becomes higher than the stretching temperature Ts.

[0076] During the period in which the temperature of the stretched film is reduced in step 4, the stretched film is preferably in a tensed state. This makes it possible to suppress the occurrence of deformation such as wrinkles due to shrinkage. When tension is applied to the stretched film, for example, the stretched film may be in a tensed state by holding the stretched film with an appropriate holder. For example, the same holder as that described as the holder that can be used to apply tension to the pre-stretched film in step 2 can be used as this holder.

[0077] Usually, by removing the stretched film from the stretching machine used in step 3, the stretched film is cooled rapidly, and the temperature of the stretched film is reduced to room temperature in a short time. In detail, since the stretching in step 3 is usually performed in a stretching machine equipped with an oven, the stretched film is cooled by being removed from the oven of the stretching machine. Since the stretched film is generally thin, the cooling proceeds quickly, and the temperature of the stretched film can reach room temperature in a short time. Therefore, step 4 can be performed, for example, by removing the stretched film from the stretching machine.

[0078] [6. Optional process] The method for producing a resin film according to the embodiment described above may further include any optional step in combination with the steps described above.

[0079] According to the above-mentioned manufacturing method, a long resin film can be manufactured using a long pre-stretched film. Therefore, the manufacturing method of the resin film may include, for example, a step of winding the long resin film thus manufactured into a roll. Furthermore, the manufacturing method of the resin film may include a step of cutting the long resin film into a desired shape.

[0080] [7. Resin film produced] According to the above-mentioned manufacturing method, a resin film having a crystalline resin layer and further having any layer as necessary can be manufactured. In this resin film, the surface of the crystalline resin layer has excellent slip properties. Therefore, according to the above-mentioned manufacturing method, it is not necessary to apply a slip treatment to the surface or to attach a masking film, and a resin film having excellent slip properties can be easily manufactured.

[0081] The slipperiness can be expressed by the static friction coefficient. The resin film produced by the above-mentioned production method can have a surface with a small static friction coefficient. The specific static friction coefficient is preferably 0.70 or less, more preferably 0.60 or less, and particularly preferably 0.50 or less. Usually, the surface of the crystalline resin layer of the resin film can have a small static friction coefficient as described above. The static friction coefficient can be measured in accordance with JIS K 7125. Specifically, the static friction coefficient between the surfaces of resin films can be measured by the method described in the examples below.

[0082] The resin film produced by the above-mentioned production method can usually have a small internal haze. The specific internal haze is preferably 1.0% or less, more preferably 0.8% or less, and particularly preferably 0.5% or less. Since a resin film having such a small internal haze has excellent transparency, it can improve the image clarity of an image display device including the resin film. The lower limit of the internal haze of the resin film is ideally 0.0%, but may be more than 0.0%.

[0083] Generally, haze includes light scattering caused by minute irregularities on the surface of the film and refractive index distribution inside the film. Internal haze refers to the total haze of the film minus the haze caused by light scattering caused by minute irregularities on the surface of the film. The internal haze of such a film can be measured by the following method. A laminate is formed having a cycloolefin film, a transparent optically adhesive film, a transparent optically adhesive film, and a cycloolefin film in this order. The haze value of this laminate is measured using a haze meter. The measured haze value of the laminate corresponds to the sum of the haze value of two cycloolefin films and the haze value of two transparent optically adhesive films. On the other hand, the cycloolefin film is laminated on both sides of the resin film via the transparent optical adhesive film to obtain a laminated test piece.Then, the haze of this laminated test piece is measured using a haze meter.The haze value of the laminated test piece obtained as a result of measurement is subtracted from the sum of the haze value of the two cycloolefin films and the haze value of the two transparent optical adhesive films to obtain the internal haze of the resin film.

[0084] The resin film produced by the above-mentioned production method can usually reduce coloration. The degree of coloration of the resin film can be measured by the b * The specific value of b for the resin film can be expressed as * The value of b is preferably 1.0 or less, more preferably 0.8 or less, and particularly preferably 0.5 or less. * A resin film with a small refractive index has a small coloring, and therefore can suppress coloring on the screen of an image display device.

[0085] Resin film b * The value of b can be measured by the following method. The transmittance of the resin film from 380 nm to 780 nm is measured at 1 nm intervals using a JASCO V-7200. From the measurement results, the value of b * can be calculated.

[0086] The present inventors speculate that the mechanism by which a resin film having the above-mentioned properties can be produced by the above-mentioned production method is as follows: However, the present invention is not limited to the mechanism described below, and can be arbitrarily modified and carried out within the scope of the effect of the present invention.

[0087] When heat is applied to the pre-stretch film containing the crystalline resin layer in step 2, the heat can cause the crystallization of the alicyclic crystalline polymer contained in the crystalline resin layer to proceed. This crystallization usually proceeds partially in the alicyclic crystalline polymer. As a result, the crystalline resin layer has domains in which the alicyclic crystalline polymer is crystallized (hereinafter, sometimes referred to as "crystallized domains") and domains in which the alicyclic crystalline polymer is not crystallized (hereinafter, sometimes referred to as "non-crystalline domains"). Usually, it is considered that minute crystallized domains are uniformly dispersed in the crystalline resin layer, and the non-crystalline domains fill the spaces between the crystallized domains. Then, when the pre-stretch film is stretched in step 3, the orientation of the molecules of the alicyclic crystalline polymer proceeds. At this time, the molecules of the alicyclic crystalline polymer in the non-crystalline domain are relatively highly oriented because the molecules are easy to move. On the other hand, the molecules of the alicyclic crystalline polymer in the crystallized domain are relatively less oriented or are not oriented at all because the molecules are difficult to move. Therefore, the crystalline resin layer of the stretched film obtained by stretching contains amorphous domains containing relatively large oriented molecules and crystallized domains containing relatively small oriented molecules. The surface of the crystalline resin layer may have a difference in surface shape depending on the difference in the degree of orientation between the domains. Such a difference in surface shape may appear as minute irregularities corresponding to the size of the crystallized domain.

[0088] In step 2, the preheating temperature Tp and preheating time tp are set to satisfy specific preheating parameters, thereby adjusting the degree of progress of crystallization of the alicyclic crystalline polymer. Therefore, in step 2, not all of the alicyclic crystalline polymer in the film is crystallized, but a specific amount of incomplete crystallization progresses, so that the size and degree of dispersion of the above-mentioned crystallized domains are adjusted to an appropriate range. Furthermore, in step 3, the stretching temperature Ts and the areal stretching ratio are set to satisfy specific conditions, thereby adjusting the degree of molecular orientation of the alicyclic crystalline polymer, so that the size of the unevenness on the film surface is adjusted to an appropriate range. And, the unevenness on the film surface provides excellent slip properties.

[0089] If the crystallization of the alicyclic crystalline polymer further proceeds after the stretching in step 3, the degree of molecular orientation of the alicyclic crystalline polymer will improve as a whole film due to the progression of crystallization, and the surface irregularities will be reduced, resulting in a decrease in slipperiness. In contrast, in the manufacturing method according to the above-mentioned embodiment, in step 4, the stretched film is cooled to room temperature while controlling the temperature of the stretched film not to be higher than the stretching temperature Ts, to obtain a resin film. Therefore, in step 4, crystallization does not proceed to such an extent that slipperiness is impaired. Therefore, cooling is performed in step 4 without impairing the excellent slipperiness of the stretched film obtained in step 3, and a resin film with excellent slipperiness is obtained.

[0090] In addition, in the manufacturing method according to the embodiment described above, the size of the crystallized domains generated in step 2 is small. Furthermore, since the areal ratio of the stretching in step 3 is not excessively large, the progress of strong oriented crystallization is suppressed, and the expansion of the crystallized domains can be suppressed. Therefore, since the crystallized domains contained in the resin film are small, not only can the size of the unevenness of the film surface be adjusted to an appropriate range as described above, but also the scattering of light due to the crystallized domains can be suppressed. Therefore, whitening of the resin due to crystallization is suppressed, and the internal haze of the resin film can be reduced.

[0091] Furthermore, in the manufacturing method according to the embodiment described above, excessive heat is not applied to the crystalline resin in steps 2 to 4. This suppresses deterioration of the crystalline resin due to heat, and thus suppresses coloring of the resin. Generally, coloring of a resin due to deterioration appears yellow. Therefore, by suppressing the above-mentioned deterioration, it is possible to suppress the film from turning yellow, and the b of the resin film can be improved. * can be made smaller.

[0092] In the past, in the manufacturing method using an alicyclic crystalline polymer, in order to utilize the excellent properties of the crystallized alicyclic crystalline polymer, it was often the case that the process of actively promoting the crystallization of the alicyclic crystalline polymer was included. However, since such crystallization is promoted by heat treatment, there was a tendency for the degradation of the polymer and the associated coloring to occur. In view of such conventional circumstances, the above-mentioned manufacturing method capable of suppressing coloring is excellent as a manufacturing method for a film containing an alicyclic crystalline polymer, and in particular, it can be said that the above-mentioned manufacturing method was the first to realize a resin film that can simultaneously improve slipperiness and suppress coloring.

[0093] In addition, when the resin film has an intermediate layer provided between a plurality of crystalline resin layers, the intermediate layer can be protected by the crystalline resin layer. Since the crystalline resin layer is usually excellent in mechanical strength, chemical resistance, heat resistance, etc., the resin film having the intermediate layer can also have the above-mentioned properties as a whole. Therefore, a resin film having excellent slip properties and excellent durability due to the action of the crystalline resin layer can be obtained.

[0094] The in-plane retardation Re of the resin film is arbitrary depending on the application of the resin film. According to the manufacturing method of the present embodiment, the birefringence in the in-plane direction of the resin film can be adjusted in a wide range, so that the resin film can have an in-plane retardation Re according to the application.

[0095] For example, the in-plane retardation Re of the resin film may be preferably 10 nm or less, more preferably 5 nm or less, and particularly preferably 3 nm or less, in which case the resin film can function as an optically isotropic film with respect to light passing through the resin film in the thickness direction.

[0096] For example, the in-plane retardation Re of the resin film is preferably 100 nm or more, more preferably 110 nm or more, particularly preferably 120 nm or more, and is preferably 180 nm or less, more preferably 170 nm or less, particularly preferably 160 nm or less. In this case, the resin film can function as a quarter-wave plate.

[0097] Further, for example, the in-plane retardation Re of the resin film can be preferably 245 nm or more, more preferably 265 nm or more, particularly preferably 270 nm or more, and can be preferably 320 nm or less, more preferably 300 nm or less, particularly preferably 295 nm or less. In this case, the resin film can function as a 1 / 2 wavelength plate.

[0098] Since the crystallization of the alicyclic crystalline polymer proceeds in step 2, the alicyclic crystalline polymer contained in the obtained resin film can have a certain degree of crystallinity or higher. The specific range of the crystallinity can be appropriately selected according to the desired performance, but is preferably 5% or higher, more preferably 10% or higher, even more preferably 20% or higher, and particularly preferably 30% or higher. By having an alicyclic crystalline polymer in which crystallization has proceeded in this way, the resin film can have even higher bending resistance and chemical resistance in addition to the excellent effects described above. The crystallinity can be measured by X-ray diffraction.

[0099] The total light transmittance of the resin film is preferably 80% or more, more preferably 85% or more, and particularly preferably 88% or more. The total light transmittance of the resin film can be measured in the wavelength range of 400 nm to 700 nm using an ultraviolet-visible spectrometer.

[0100] The thickness of the resin film can be appropriately set according to the desired application, and is preferably 5 μm or more, more preferably 10 μm or more, particularly preferably 20 μm or more, and also preferably 200 μm or less, more preferably 100 μm or less, even more preferably 50 μm or less, particularly preferably 30 μm or less. When the thickness of the resin film is equal to or more than the lower limit of the above range, the handling property can be improved and the strength can be increased. When the thickness of the resin film is equal to or less than the upper limit, the long resin film can be easily wound up.

[0101] The resin film may be a sheet film or a long film.

[0102] The resin film can be used for any purpose. Among them, the resin film is suitable as, for example, an optical film such as an optical isotropic film and a retardation film, an electric / electronic film, a substrate film for a barrier film, and a substrate film for a conductive film. Examples of the optical film include a retardation film for a liquid crystal display device, a polarizing plate protective film, and a retardation film for a circular polarizing plate of an organic EL display device. Examples of the electric / electronic film include a flexible wiring board and an insulating material for a film capacitor. Examples of the barrier film include a substrate for an organic EL element, a sealing film, and a sealing film for a solar cell. Examples of the conductive film include a flexible electrode for an organic EL element or a solar cell, a touch panel member, and the like. EXAMPLES

[0103] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to the examples shown below, and can be modified and carried out as desired without departing from the scope of the claims of the present invention and the scope of equivalents thereto.

[0104] In the following description, the units "%" and "parts" that represent amounts are by weight unless otherwise specified. Furthermore, the operations described below were carried out under normal temperature and pressure conditions unless otherwise specified.

[0105] [Evaluation method] [Method of measuring weight average molecular weight Mw and number average molecular weight Mn] The weight average molecular weight Mw and number average molecular weight Mn of the polymer were measured as polystyrene equivalent values ​​using a gel permeation chromatography (GPC) system (Tosoh Corporation, "HLC-8320"). In the measurement, an H-type column (Tosoh Corporation) was used as the column, and tetrahydrofuran was used as the solvent. The temperature during the measurement was 40°C.

[0106] [Method of measuring glass transition temperature Tg and crystallization peak temperature Tc] The resin was heated to 300°C in a nitrogen atmosphere to melt it, and the molten resin was quenched with liquid nitrogen. Using this resin as a sample, the glass transition temperature Tg and the crystallization peak temperature Tc of the resin were determined by heating at a rate of 10°C / min using a differential scanning calorimeter (DSC).

[0107] [Method for measuring hydrogenation rate of polymer] The hydrogenation rate of the polymer is 4 as a solvent at 145°C, 1 Measured by H-NMR measurement.

[0108] [Method for measuring the ratio of racemo-dyads in polymers] Orthodichlorobenzene-d 4 The inverse-gated decoupling method was applied to the polymer at 200°C using 13 C-NMR measurements were performed. 13 From the results of C-NMR measurement, o-dichlorobenzene-d 4 Using the peak at 127.5 ppm as the reference shift, the signal at 43.35 ppm from the meso-dyad and the signal at 43.43 ppm from the racemo-dyad were identified. The ratio of the racemo-dyads in the polymer was calculated based on the intensity ratio of these signals.

[0109] [Method of measuring thickness of film before stretching and thickness of resin film] The thickness of the film was measured using a snap gauge ID-C112BS (manufactured by Mitutoyo Corporation).

[0110] [Method for measuring the static friction coefficient between resin films] The resin film was cut into a size of 50 mm x 50 mm to obtain a test piece. Using this test piece, the static friction coefficient of the surface of the resin film was measured using a surface property measuring instrument "Type 32" manufactured by Shinto Scientific Co., Ltd. in accordance with JIS K7125. The same resin film from which the test piece was cut was used as the counter member for this measurement (the member that comes into contact with the surface of the test piece during measurement).

[0111] [Method for measuring internal haze of resin film] The resin film was cut into a size of 50 mm x 50 mm to obtain a test piece. Then, a cycloolefin film (Zeon Corporation's "ZEONOR FILM ZF14-040", thickness 40 μm) was attached to both sides of the test piece via a transparent optical adhesive film (3M Corporation's "8146-2") having a thickness of 50 μm to obtain a laminated test piece. The haze of this laminated test piece was measured using a haze meter (Nippon Denshoku Industries Co., Ltd.'s "NDH5000").

[0112] Separately, the sum of the haze value of two cycloolefin films and the haze value of two transparent optical adhesive films was determined by the following method. A laminate was formed having a cycloolefin film, a transparent optical adhesive film, a transparent optical adhesive film, and a cycloolefin film in this order. The haze value of the laminate was measured as the sum of the haze value of two cycloolefin films and the haze value of two transparent optical adhesive films using the haze meter.

[0113] The internal haze of the test piece as a resin film was calculated by subtracting the sum (0.04) of the haze value of the two cycloolefin films and the haze value of the two layers of transparent optical adhesive film from the haze value of the laminated test piece.

[0114] [Color of resin film (b * Measurement method for The resin film was cut into a size of 50 mm x 50 mm to obtain a test piece. The transmittance of this test piece from 380 nm to 780 nm was measured at 1 nm intervals using a JASCO V-7200. From the measurement results, the b * was calculated.

[0115] [Production Example 1. Production of hydrogenated product of ring-opened polymer of dicyclopentadiene] A metallic pressure-resistant reactor was thoroughly dried and then purged with nitrogen. 154.5 parts of cyclohexane, 42.8 parts of a 70% cyclohexane solution of dicyclopentadiene (endo isomer content of 99% or more) (30 parts as dicyclopentadiene), and 1.9 parts of 1-hexene were added to the metallic pressure-resistant reactor and heated to 53°C.

[0116] A catalyst solution was prepared by adding 0.061 parts of a 19% diethylaluminum ethoxide / n-hexane solution to a solution prepared by dissolving 0.014 parts of tetrachlorotungsten phenylimide (tetrahydrofuran) complex in 0.70 parts of toluene, and stirring for 10 minutes. The catalyst solution was added to the pressure-resistant reactor to initiate the ring-opening polymerization reaction. The reaction was then continued for 4 hours while maintaining the temperature at 53°C, yielding a solution of a ring-opening polymer of dicyclopentadiene. The number average molecular weight (Mn) and weight average molecular weight (Mw) of the obtained ring-opened polymer of dicyclopentadiene were 8,750 and 28,100, respectively, and the molecular weight distribution (Mw / Mn) calculated from these was 3.21.

[0117] To 200 parts of the obtained solution of the ring-opening polymer of dicyclopentadiene, 0.037 parts of 1,2-ethanediol was added as a terminator, heated to 60°C, and stirred for 1 hour to terminate the polymerization reaction. One part of a hydrotalcite-like compound (Kyowa Chemical Industry Co., Ltd.'s "Kyoward (registered trademark) 2000") was added, heated to 60°C, and stirred for 1 hour. Thereafter, 0.4 parts of a filter aid (Showa Chemical Industry Co., Ltd.'s "Radiolight (registered trademark) #1500") was added, and the adsorbent and the solution were filtered using a PP pleated cartridge filter (ADVANTEC Toyo Co., Ltd.'s "TCP-HX").

[0118] 100 parts of cyclohexane was added to 200 parts of the filtered ring-opening polymer solution (polymer amount 30 parts), and 0.0043 parts of chlorohydridocarbonyltris(triphenylphosphine)ruthenium was added, and hydrogenation reaction was carried out at 180°C and hydrogen pressure of 6 MPa for 4 hours. As a result, a reaction liquid containing a hydrogenated product of the ring-opening polymer of dicyclopentadiene was obtained. The reaction liquid was a slurry solution in which the hydrogenated product was precipitated.

[0119] The hydrogenated product and the solution contained in the reaction solution were separated using a centrifuge and dried under reduced pressure at 60°C for 24 hours to obtain 28.5 parts of a hydrogenated product of a ring-opening polymer of dicyclopentadiene having crystallinity. The hydrogenation rate of this hydrogenated product was 99% or more, and the rate of racemo-dyads was 89%.

[0120] [Production Example 2: Production of resin pellets] A crystalline resin that is a material for a film was obtained by mixing 1.1 parts of an antioxidant (tetrakis[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane; "Irganox (registered trademark) 1010" manufactured by BASF Japan Ltd.) with 100 parts of the hydrogenated product of the ring-opening polymer of dicyclopentadiene obtained in Production Example 1. The glass transition temperature Tg(1) of the crystalline resin was 93°C, and the crystallization peak temperature Tc was 135°C.

[0121] The crystalline resin was fed into a twin-screw extruder (Toshiba Machine Co., Ltd., "TEM-37B") equipped with four die holes with an inner diameter of 3 mm. The twin-screw extruder molded the crystalline resin into a strand-shaped molded body by hot melt extrusion molding. The molded body was chopped with a strand cutter to obtain pellets of the crystalline resin. The operating conditions of the twin-screw extruder are shown below. Barrel temperature setting: 270℃~280℃ Die temperature setting: 250℃ Screw speed: 145 rpm Feeder speed: 50 rpm

[0122] [Example 1] The pellets of the crystalline resin obtained in Production Example 2 were supplied to a hot melt extrusion film molding machine equipped with a T-die. The supplied crystalline resin was melted in the film molding machine, extruded through the T-die, and wound on a roll at a winding speed of 15 m / min to produce a long pre-stretched film (thickness 50 μm, width 1350 mm) made of the crystalline resin (step 1). The operating conditions of the film molding machine are shown below. Barrel temperature setting: 280℃~290℃ Die temperature: 270℃ Screw speed: 30 rpm

[0123] The pre-stretched film thus obtained was cut into a size of 200 mm in the MD direction and 200 mm in the TD direction to obtain a rectangular pre-stretched film. The cut pre-stretched film was attached to a batch-type biaxial stretching device (manufactured by Toyo Seiki Seisakusho). This attachment was performed by fixing the four sides of the pre-stretched film with clips of the biaxial stretching device so that the pre-stretched film was in a tensed state. With the four sides of the pre-stretched film thus fixed with clips, the pre-stretched film was held at a constant pre-heating temperature Tp = 130 ° C. for a pre-heating time tp = 180 seconds (step 2).

[0124] Immediately thereafter, the unstretched film was stretched simultaneously in the MD and TD directions using the biaxial stretching machine at a constant stretching temperature Ts = 130 ° C. for 20 seconds (step 3). The stretching ratio in the MD direction was 1.6 times, and the stretching ratio in the TD direction was 1.6 times, so the areal stretching ratio was 2.6 times. This stretching gave a stretched film as the stretched film.

[0125] Immediately thereafter, the obtained stretched film was removed from the biaxial stretching machine and allowed to cool naturally. By allowing to cool, the temperature of the stretched film immediately dropped to room temperature without becoming higher than the stretching temperature Ts (step 4). As a result, a resin film having a single-layer structure including a layer made of a crystalline resin was obtained. The obtained resin film was evaluated by the method described above.

[0126] [Example 2] In step 2, the preheating time tp was changed to 290 seconds. Except for the above, the same operations as in Example 1 were carried out to produce and evaluate a resin film.

[0127] [Example 3] In step 2, the preheating temperature Tp was changed to 145° C., and the preheating time tp was changed to 40 seconds. Except for the above, the same operations as in Example 1 were used to produce and evaluate a resin film.

[0128] [Example 4] In step 2, the preheating temperature Tp was changed to 127° C., and the preheating time tp was changed to 250 seconds. Furthermore, in step 3, the stretching temperature Ts was changed to 127° C. Except for the above, a resin film was produced and evaluated by the same operations as in Example 1.

[0129] [Example 5] In step 1, the film winding speed was changed to 7.5 m / min, so that the dimensions of the long unstretched film were changed to a thickness of 100 μm and a width of 1350 mm. In step 3, the stretching ratio in the MD direction was changed to 2.45 times, and the stretching ratio in the TD direction was changed to 2.45 times, so that the areal stretching ratio was changed to 6.0 times. Except for the above, the resin film was produced and evaluated by the same operations as in Example 1.

[0130] [Example 6] In step 1, the film winding speed was changed to 25 m / min, so that the dimensions of the long unstretched film were changed to a thickness of 30 μm and a width of 1350 mm. In step 3, the stretching ratio in the MD direction was changed to 1.3 times, and the stretching ratio in the TD direction was changed to 1.3 times, so that the areal stretching ratio was changed to 1.7 times. Except for the above, the resin film was produced and evaluated by the same operations as in Example 1.

[0131] [Example 7] In step 1, the film winding speed was changed to 25 m / min, so that the dimensions of the long unstretched film were changed to a thickness of 30 μm and a width of 1350 mm. In step 3, the stretching temperature Ts was changed to 110° C., and the stretching ratio in the MD direction was changed to 1.3 times, and the stretching ratio in the TD direction was changed to 1.3 times, so that the areal stretching ratio was changed to 1.7 times. Except for the above, the resin film was produced and evaluated by the same operations as in Example 1.

[0132] [Example 8] In step 2, the preheating temperature Tp was changed to 160° C., and the preheating time tp was changed to 10 seconds. Furthermore, in step 3, the stretching temperature Ts was changed to 160° C. Except for the above, a resin film was produced and evaluated by the same operations as in Example 1.

[0133] [Example 9] The pellets of the crystalline resin obtained in Production Example 2 and the pellets of a norbornene-based resin (ZEONOR 1430 manufactured by Zeon Corporation; glass transition temperature Tg(2)=143° C.) as a thermoplastic resin were supplied to a hot melt extrusion film molding machine equipped with a T-die. The supplied resins were melted in the film molding machine, co-extruded through the T-die, and wound up on a roll at a winding speed of 15 m / min to produce a long co-extruded film (thickness 50 μm, width 1350 mm) (step 1). The obtained co-extruded film had a two-type, three-layer structure of "crystalline resin layer (thickness 10 μm) / norbornene-based resin layer (thickness 30 μm) / crystalline resin layer (thickness 10 μm)". The operating conditions of the film molding machine are shown below. Each barrel temperature setting: 280℃~290℃ Die temperature: 270℃ Each screw rotation speed: 10 rpm

[0134] The above-mentioned co-extruded film was used as the pre-stretch film. Except for the above, the resin film was produced and evaluated in the same manner as in Example 1.

[0135] [Example 10] In step 2, the co-extruded film produced in Example 9 was used as the pre-stretched film, and the preheating temperature Tp was changed to 145° C. and the preheating time tp was changed to 40 seconds. Except for the above, the resin film was produced and evaluated by the same operations as in Example 1.

[0136] [Comparative Example 1] In step 2, the preheating time tp was changed to 90 seconds. Except for the above, the same operations as in Example 1 were carried out to produce and evaluate a resin film.

[0137] [Comparative Example 2] In step 2, the preheating time tp was changed to 360 seconds. Except for the above, the same operations as in Example 1 were used to produce and evaluate a resin film.

[0138] [Comparative Example 3] In step 1, the film winding speed was changed to 25 m / min, so that the dimensions of the long unstretched film were changed to a thickness of 30 μm and a width of 1350 mm. In step 2, the preheating temperature Tp was changed to 115° C. In step 3, the stretching temperature Ts was changed to 115° C., and the stretching ratio in the MD direction was changed to 1.3 times, and the stretching ratio in the TD direction was changed to 1.3 times, so that the areal stretching ratio was changed to 1.7 times. Except for the above, the resin film was produced and evaluated by the same operations as in Example 1.

[0139] [Comparative Example 4] In step 1, the film winding speed was changed to 25 m / min, so that the dimensions of the long unstretched film were changed to a thickness of 30 μm and a width of 1350 mm. In step 3, the stretching ratio in the MD direction was changed to 1.1 times, and the stretching ratio in the TD direction was changed to 1.1 times, so that the areal stretching ratio was changed to 1.2 times. Except for the above, the resin film was produced and evaluated by the same operations as in Example 1.

[0140] [result] The results of the above-mentioned Examples and Comparative Examples are shown in Tables 1 and 2, respectively.

[0141] [Table 1]

[0142] [Table 2]

Claims

1. A step 1 of preparing a pre-stretched film having a resin layer made of a crystalline resin containing a polymer having an alicyclic structure and crystallinity; A step 2 of heating the pre-stretched film at a temperature Tp of not less than "Tc-10°C" and not more than "Tc+35°C" for a time tp (where Tc represents the crystallization peak temperature [°C] of the crystalline resin); A step 3 of stretching the pre-stretched film subjected to the step 2 at a stretching temperature Ts equal to or lower than the temperature Tp at an areal magnification of 1.6 times or more and 6.3 times or less to obtain a stretched film; A step 4 of lowering the temperature of the stretched film to room temperature; The steps 3 and 4 are carried out consecutively, The temperature Tp [° C.] and the time tp [seconds] satisfy the following formula (i), 10000≦{Tp-(Tc-15)} 2 ×tp≦30000 (i) A method for producing a resin film, wherein after the stretched film is obtained in step 3, the temperature of the stretched film is maintained at or below Ts until the temperature of the stretched film reaches room temperature in step 4.

2. 2. The method for producing a resin film according to claim 1, wherein the polymer containing an alicyclic structure and having crystallinity is a hydrogenated product of a ring-opening polymer of dicyclopentadiene.

3. The pre-stretched film has two or more of the resin layers, The method for producing a resin film according to claim 1 or 2, further comprising providing one or more intermediate layers between the resin layers, the intermediate layers being made of a thermoplastic resin other than the crystalline resin.

4. The method for producing a resin film according to claim 3 , wherein the glass transition temperature of the thermoplastic resin is equal to or higher than the glass transition temperature of the crystalline resin and equal to or lower than “Ts+20° C.”

5. The method for producing a resin film according to any one of claims 1 to 4, wherein the resin film has a surface having a static friction coefficient of 0.7 or less.

6. The method for producing a resin film according to any one of claims 1 to 5, wherein the resin film has an internal haze of 1.0% or less.

7. The resin film has a CIE-Lab color system b * The method for producing a resin film according to any one of claims 1 to 6, wherein the linear modulus is 1.0 or less.

Citation Information

Patent Citations

  • Film capacitor

    WO2016052303A1

  • Resin film, conductive film and method for producing these films

    WO2018061841A1

  • Resin film, barrier film, and electrically conductive film, and production methods therefor

    WO2018062067A1