Method for producing lactone polymer
The method for producing lactone polymers using nonmetal halides and heteropolyacids as catalysts with controlled water content addresses the issues of wide molecular weight distribution and high color number, achieving monodisperse polymers with enhanced resin properties and heat resistance.
Patent Information
- Application Number
- JP2020139409
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-20
- Filing Date
- 2020-08-20
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-08-20
AI Technical Summary
Conventional methods for producing lactone polymers result in wide molecular weight distribution, high color number, and insufficient physical properties, leading to issues with moldability, handling, and resin performance.
A method involving ring-opening polymerization using nonmetal halides or heteropolyacids as catalysts, active hydrogen atom-containing compounds as initiators, and controlled water content, with specific reaction conditions to achieve a monodisperse molecular weight distribution and low color number.
The method produces lactone polymers with narrow molecular weight distribution, low color number, and low acid value, resulting in improved resin properties, processability, and heat resistance.
Smart Images

Figure 0007572184000001 
Figure 0007572184000002 
Figure 0007572184000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a lactone polymer, and also to a method for producing a polyurethane or polyester using the lactone polymer obtained by the production method. [Background technology]
[0002] Lactone polymers with a molecular weight of 500 to 5000 are particularly useful as raw materials for polyurethane resins, polyester resins, artificial leather, coating materials, etc. Lactone polymers can be obtained by ring-opening polymerization of lactones such as ε-caprolactone and δ-valerolactone. In conventional methods for producing lactone polymers, the use of an anionic ring-opening polymerization catalyst such as tetrabutyl orthotitanate or a high temperature reaction at 100 to 200°C causes side reactions such as transesterification reactions, resulting in a wide molecular weight distribution (weight average molecular weight (M w ) / number average molecular weight (M n )=1.5 to 3.5), some of the obtained products contained a large amount of low polymers, and the color number was high and the hue was insufficient.
[0003] Methods for improving the molecular weight distribution of lactone polymers have been proposed (Patent Documents 1 and 2, etc.), but the resulting lactone polymers have a low molecular weight distribution, w / M n = 1.2 to 1.8, and the molecular weight distribution is wide, and the number of colors is high, which is unsatisfactory. The lactone polymers having a wide molecular weight distribution and a high number of colors are used to obtain various resins such as polycaprolactone and polyurethane, which have insufficient physical properties (strength, elongation, heat resistance, etc.), have high viscosity, and have many practical problems in terms of moldability, handling, etc. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 57-155230 [Patent Document 2] WO 2015 / 60192 Summary of the Invention [Problem to be solved by the invention]
[0005] The problem to be solved by the present invention is to provide a method for producing a lactone polymer having a narrow molecular weight distribution and excellent hue. Another object of the present invention is to provide a resin material (polyurethane, polyester, etc.) having excellent various resin properties, viscosity, moldability, and heat resistance by using the lactone polymer obtained by the production method of the present invention as a resin raw material. [Means for solving the problem]
[0006] In order to solve the above problems, the inventors have intensively studied methods for improving the molecular weight distribution and color number of lactone polymers, and as a result have found a method for obtaining lactone polymers which have a low color number, excellent hue, a low acid value, and a molecular weight distribution close to monodispersion.
[0007] 1. A lactone compound represented by the following general formula (1): A method for producing a lactone polymer obtained by ring-opening polymerization, comprising the steps of: A non-metal halide or a heteropoly acid is used as a catalyst, In the ring-opening polymerization, an active hydrogen atom-containing compound is used as an initiator, A method for producing a lactone polymer, comprising adjusting the water content of the active hydrogen atom-containing compound.
[0008] [ka]
[0009] [In formula (1), R 1 ~R 3 each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms, and n represents an integer of 0 to 6.
[0010] 2. The active hydrogen atom-containing compound is a polyhydric alcohol, The method for producing the lactone polymer, wherein 0.01 to 10 mol of a polyhydric alcohol is used per 1 mol of the lactone compound.
[0011] 3. The method for producing a lactone polymer as described above, wherein 0.0001 to 10 mol of the catalyst is used per 1 mol of the lactone compound.
[0012] 4. The method for producing a lactone polymer, wherein the ring-opening polymerization is carried out at a reaction temperature of 60 to 100°C.
[0013] 5. The method for producing a lactone polymer as described above, wherein the water content of the active hydrogen atom-containing compound is 1 to 500 ppm.
[0014] 6. A method for producing a polyurethane, comprising the step of reacting the lactone polymer obtained by the method for producing a lactone polymer described above with a polyisocyanate compound to produce a polyurethane.
[0015] 7. A method for producing a polyester, comprising the step of reacting a lactone polymer obtained by the method for producing a lactone polymer described above with a polyol compound to produce a polyester. Effect of the Invention
[0016] The production method of the present invention can provide a lactone polymer having a molecular weight distribution close to monodisperse, containing no low polymers, a low color number, a low acid value, and a low viscosity. In addition, the lactone polymer obtained by the production method of the present invention can be used as a raw material to produce polyurethanes, polyesters, and the like having excellent resin properties, processability, heat resistance, and the like. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, the embodiments of the present invention will be described in detail. Note that the present invention is not limited to the following embodiments, and can be practiced with various modifications within the scope of the gist of the present invention. Hereinafter, the lactone compound represented by the general formula (1) will be specifically described, but the present invention is not limited thereto.
[0018] In the general formula (1), R 1 ~R 3 each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms; n R 1 , and n R 2 may be the same or different. n represents an integer of 0 to 6. n is preferably an integer of 0 to 2, 4 or 5, and more preferably 4 or 5.
[0019] In the general formula (1), R 1 ~R 3 Specific examples of the "straight-chain or branched alkyl group having 1 to 4 carbon atoms" represented by the formula (1) include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, a butyl group, an isobutyl group, and a t-butyl group. 1 ~R 3 are each preferably independently a hydrogen atom or a methyl group.
[0020] Specific examples of the lactone compound represented by general formula (1) include β-propiolactone, β-butyrolactone, β-valerolactone, γ-butyrolactone, γ-valerolactone, γ-caprylolactone, γ-octanolactone, δ-valerolactone, β-methyl-δ-valerolactone, δ-stearolactone, ε-caprolactone, 2-methyl-ε-caprolactone, 4-methyl-ε-caprolactone, ε-caprylolactone, and ε-palmitolactone.
[0021] The present invention relates to a method for producing a lactone polymer obtained by ring-opening polymerization of a lactone compound represented by the general formula (1). Further, the production method according to the present invention uses a non-metallic halide or a heteropolyacid as a catalyst, uses an active hydrogen atom-containing compound as an initiator in the ring-opening polymerization, and adjusts the water content of the active hydrogen atom-containing compound. It relates to a method for producing a lactone polymer characterized by the above.
[0022] Examples of the catalyst in the method for producing the lactone polymer of the present invention include non-metallic halides as Lewis acids and heteropolyacids as solid acids. Examples of non-metallic halides include non-metallic halides such as boron trifluoride (BF3) and phosphorus pentafluoride (PF5). Examples of heteropolyacids include phosphotungstic acid (H3(PW 12 O 40 )·nH2O (n≈30), abbreviated as PWA), silicotungstic acid (H4(SiW 12 O 40 )·nH20 (n≈30)), phosphomolybdic acid (H3(PMo 12 O 40 )·nH20 (n≈30)), sodium phosphomolybdate (Na3(PMo 12 O 40 )·nH20 (n≈30)), phosphotungstomolybdic acid (H3(PW 12-x Mo x O 40 )·nH20 (0 < x < 12, n≈30)), phosphovanadomolybdic acid (H 15-x (PV 12-x Mo x O 40 )·nH2O (6 < x < 12, n≈30)), and other heteropolyacids. Further, examples of the form when using these catalysts include complexes of boron trifluoride (BF3) and the like with chain and cyclic ethers such as diethyl ether and tetrahydrofuran (THF) (for example, boron trifluoride tetrahydrofuran (C4H8O·BF3, abbreviated as BF3THF)).
[0023] The active hydrogen atom-containing compound in the method for producing a lactone polymer of the present invention specifically contains a hydroxyl group (-OH), an amino group (-NH2, mono-substituted amino group, di-substituted amino group), or a mercapto group (thiol group, -SH), and is used as a reaction initiator (or simply initiator) in the polymerization reaction of the present invention. Specific examples of compounds containing a hydroxyl group include aliphatic alcohols such as methanol, ethanol, propanol, n-butanol, 2-butanol, isobutyl alcohol, t-butyl alcohol, allyl alcohol, and 2-hydroxyethyl methacrylate; Aromatic alcohols or various phenols such as benzyl alcohol, 2-methylbenzyl alcohol, phenylmethylcarbinol (2-phenyl-2-propanol), 4-hydroxybenzyl alcohol, 4-methoxyphenol, triphenylmethanol; Alicyclic alcohols such as cyclohexanol, 3,3,5-trimethylcyclohexanol, and cyclohexaneethanol; Polyhydric alcohols (or polyols), such as ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, polyethylene glycol, polypropylene glycol, polyoxytetramethylene glycol, glycerin, trimethylolpropane, 1,2-cyclohexanediol, 1,4-cyclohexanediol, m-xylylene glycol, p-xylene glycol, and thiodiglycol; Examples include organic carboxylic acids such as acetic acid, propanoic acid, benzoic acid, phthalic acid, oxalic acid, and fumaric acid. Specific examples of the compound containing an amino group include alkylamines such as methylamine, ethylamine, n-propylamine, isopropylamine, n-butylamine, isobutylamine, and t-butylamine, and dialkylamines such as dimethylamine, diethylamine, and dibutylamine; Aromatic, alicyclic and heterocyclic amines such as aniline, o-toluidine, diphenylamine, cyclohexylamine, piperidine; Examples of the polyamines include aliphatic, aromatic, alicyclic and heterocyclic polyamines such as ethylenediamine, propylenediamine, hexamethylenediamine, o-, m- or p-phenylenediamine, 1,4-cyclohexanediamine, piperazine, diethylenetriamine, and 4,4',4''-methylidynetrianiline. Examples of mercapto group (thiol group)-containing compounds include aliphatic mercaptans such as methyl mercaptan (methanethiol), ethyl mercaptan (ethanethiol), propyl mercaptan (propanethiol), and n-butyl mercaptan (1-butanethiol); Aromatic mercaptans such as benzyl mercaptan and triphenylmethanethiol; Examples include ethylenedithioglycol, 1,4-benzenedimethanethiol, xylylenedimercaptan, 2-mercaptoethanol, and bis(2-mercaptoethyl) ether.
[0024] The method for producing the lactone polymer of the present invention will be specifically described. The lactone compound represented by the general formula (1) and the active hydrogen atom-containing compound are mixed in appropriate amounts in a reaction vessel, an appropriate amount of a suitable catalyst is added, and the mixture is heated at an appropriate temperature for an appropriate time to react, thereby obtaining a reaction mixture containing the lactone polymer of the present invention. The reaction mixture thus obtained can be purified into a lactone polymer product by a known method using an appropriate solvent and an appropriate purification device.
[0025] The active hydrogen atom-containing compound used in the present invention is characterized by having an adjusted water content. The active hydrogen atom-containing compound with an adjusted water content may be a commercially available product, and it is preferable to perform a dehydration operation on a commercially available product or product before purification, specifically, purification using a distillation apparatus, dehydration operation using a molecular sieve, etc., but is not limited thereto. It is preferable to use a purified active hydrogen atom-containing compound whose water content has been measured using a moisture meter or the like. In addition, in order to prevent moisture from the outside air from being mixed in when performing ring-opening polymerization, it is preferable to perform the ring-opening polymerization reaction under anaerobic conditions, and it is preferable to perform it under a nitrogen or inert gas atmosphere. The water content of the active hydrogen atom-containing compound preferable for implementing the present invention is preferably 1 to 500 ppm, more preferably 1 to 200 ppm. If the water content exceeds 500 ppm, the Mw / Mn may become too large due to the generation of oligomer components.
[0026] The active hydrogen atom-containing compound used as an initiator in the method for producing a lactone polymer of the present invention is preferably a polyhydric alcohol. In the method for producing a lactone polymer of the present invention, preferably 0.01 to 10 mol, more preferably 0.1 to 1.0 mol of the polyhydric alcohol is used per mol of the lactone compound. If the amount of the initiator used per mol of the lactone compound exceeds 10 mol, the molecular weight of the product becomes too small, and it may be difficult to produce a polymer with a sufficiently high molecular weight.
[0027] The amount of the catalyst, Lewis acid or solid acid, used in the lactone polymer production method of the present invention is preferably 0.0001 to 10 mol, more preferably 0.0001 to 1 mol, and particularly preferably 0.0001 to 0.1 mol, per mol of lactone compound. The amount of catalyst used is extremely small relative to the lactone compound, so it is easy to remove. If the amount of catalyst used exceeds 10 mol, heat generation becomes significant, the molecular weight distribution of the product may be extremely widened, and quality deterioration due to side reactions, such as coloring, may occur. In addition, the cost of removing the catalyst may be too high, which is not preferable.
[0028] The reaction temperature range of the ring-opening polymerization in the method for producing the lactone polymer of the present invention is preferably 60 to 100°C, more preferably 60 to 90°C, and the optimum temperature is determined by the type and amount of the initiator, the quality and molecular weight of the target polymer, and is usually more preferably 60 to 80°C. The polymerization reaction can also be carried out in an inert organic solvent. In bulk polymerization at a relatively low temperature, crystallization is likely to occur as the polymerization proceeds, so it is preferable to carry out the polymerization in an inert organic solvent such as benzene, toluene, or xylene. At temperatures exceeding 100°C, the molecular weight distribution of the product may be extremely broadened, and quality deterioration due to side reactions, such as coloring, may occur. On the other hand, the polymerization reaction time is related to the reaction rate and can be appropriately adjusted depending on the temperature, the type and amount of the initiator used, and a reaction time of 2 to 10 hours or more can be selected. In the production method of the present invention, it is preferable to carry out the polymerization reaction until the unreacted lactone compound disappears in order to simplify the purification operation of the lactone polymer and improve the quality, and in that case, it is recommended to carry out sufficient aging.
[0029] The lactone polymer product can be purified from the reaction mixture containing the lactone polymer obtained by the production method of the present invention by known methods, and specific examples are described below. The lactone polymer product can be dissolved or dispersed using an appropriate amount of organic solvent such as toluene (and specifically, esters such as alcohol, acetone, ethyl acetate, and n-butyl acetate; ethers such as diethyl ether, propylene glycol monomethyl ether (PGME), and ethylene glycol monoethyl ether (ethyl cellosolve); ether esters such as propylene glycol monomethyl ether acetate (PGMEA); ketones such as acetone and cyclohexanone; alcohols such as methanol, ethanol, and 2-propanol; diacetone alcohol (DAA); aromatic hydrocarbons such as benzene, toluene, and xylene; amides such as N,N-dimethylformamide (DMF) and N-methylpyrrolidone (NMP); and dimethyl sulfoxide (DMSO)) and an appropriate amount of ion exchange resin, and stirred at an appropriate temperature for an appropriate time, the reaction mixture is filtered, and the solvent is removed by a method such as distillation under reduced pressure to obtain the produced lactone polymer. The ion exchange resin can be selected according to the raw materials and polymerization conditions used in the polymerization.
[0030] The water content of the materials and products used in the production method of the present invention can be measured with a moisture meter according to the Karl Fischer volumetric titration method.
[0031] The molecular weight distribution of the lactone polymer of the present invention is determined by the number average molecular weight (M n ), number average molecular weight (M w ), M w / M n The M of the lactone polymer of the present invention can be measured by gel permeation chromatography (GPC). w / M n is preferably less than 1.3.
[0032] The acid value of the lactone polymer of the present invention can be determined according to Japanese Industrial Standards (JIS K 0070-1992 "Testing methods for acid value, saponification value, ester value, iodine value, hydroxyl value and unsaponifiable matter of chemical products"). The acid value is preferably 0.1 to 1.5 mgKOH / g, more preferably 0.1 to 1.0 mgKOH / g.
[0033] The color number in the present invention can be determined according to Japanese Industrial Standards (JIS K 4101-1993 "General Test Method for Organic Intermediate Materials 13. Color Number Test Method", Hazen Unit Color Number Test, APHA).
[0034] The lactone polymer obtained in the present invention can be used to produce polyurethane resins or polyester resins. The method for producing these resins is not particularly limited, and they can be produced by known methods. For example, in the case of producing polyurethane, a polyisocyanate component may be charged all at once into a lactone polymer, a polyol, a chain extender, and an organometallic catalyst and reacted, or a polyol and a polyisocyanate component may be reacted to obtain a prepolymer having an isocyanate group terminal, and then a chain extender may be added to carry out an elongation reaction. Similarly, in the case of producing polyester, a known method may be used to synthesize the lactone polymer and a polyol by dehydration condensation or the like.
[0035] Examples of the polyisocyanate compound include aromatic, alicyclic, and aliphatic polyisocyanates having two or more isocyanate groups. Specific examples include polyisocyanates such as tolylene diisocyanate (TDI), 4,4'-diphenylmethane diisocyanate (MDI), polymethylene polyphenyl polyisocyanate (MDI), xylylene diisocyanate (XDI), isophorone diisocyanate (IPDI), and hexamethylene diisocyanate (HMDI). Among these, MDI is preferred because it is easily available and easy to control the reaction with hydroxyl groups.
[0036] Chain extenders include low molecular weight dihydric alcohols such as 1,3-propanediol, 1,4-butanediol, and 1,5-pentanediol.
[0037] The organometallic catalyst is not particularly limited, but specific examples include organotin catalysts such as dibutyltin oxide, dibutyltin diacetate, dibutyltin dilaurate, dibutyltin dichloride, and dioctyltin dilaurate; nickel octylate, nickel naphthenate; cobalt octylate, cobalt naphthenate; bismuth octylate, bismuth naphthenate, etc. Among these organometallic catalysts, organotin catalysts are preferred, and dibutyltin dilaurate (dibutyltin dilaurate) is more preferred.
[0038] The amount of the organometallic catalyst used in the method for producing a polyurethane of the present invention is preferably from 0.0001 to 5 parts by weight, and more preferably from 0.001 to 3 parts by weight, based on 100 parts by weight of the polyol.
[0039] The physical properties of the polyurethane obtained by the polyurethane production method of the present invention can be evaluated in terms of physical properties, thermal properties, electrical properties, and chemical properties. In the present invention, the physical properties may be evaluated by measuring the breaking strength (breaking stress) (MPa) and breaking elongation (%) at the breaking point using a tensile tester. In addition, the thermal properties / chemical properties may be evaluated by measuring the thermal decomposition temperature (°C) by thermogravimetry-differential thermal analysis (TG-DTA). EXAMPLES
[0040] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the following examples. In the examples, the water content (ppm) of the initiator (ethylene glycol, etc.) was measured by Karl Fischer volumetric titration using the following moisture meter. Device name: Volumetric automatic moisture measuring device Model: KF-31 (Mitsubishi Chemical Analytech Co., Ltd.), Detector: RI The GPC measurement was performed using a high-speed GPC device (model: HLC-8320GPC, manufactured by Tosoh Corporation) and a column (model: TSKgel G4000H+G2500H, manufactured by Tosoh Corporation) under the following conditions. Eluent: Tetrahydrofuran Standard: Polytetramethylene ether glycol Injection volume: 100 μL Flow rate: 1.0 mL / min Measurement temperature: 40°C Detector: RI
[0041] [Example 1] Synthesis of polycaprolactone In a nitrogen-purged 500 mL reaction vessel, 114.0 g (1.00 mol) of ε-caprolactone (abbreviated as CL, manufactured by Tokyo Chemical Industry Co., Ltd.) and 3.2 g (0.05 mol, moisture content 200 ppm, manufactured by Kishida Chemical Co., Ltd.) of ethylene glycol (EG) were placed, and 1.0 g (0.0003 mol, manufactured by Japan New Metals Co., Ltd.) of phosphotungstic acid (PWA) was added and stirred at 70°C for 5 hours. 100 mL of toluene and 50 g of ion exchange resin IRA-96SB (manufactured by Organo Corporation) were added to the reaction mixture, and the mixture was stirred at room temperature for 2 hours. After stirring, the reaction mixture was filtered, and the solvent was removed from the filtrate by distillation under reduced pressure, yielding a polymer as a colorless solid (at room temperature) (107 g, yield 94%). The GPC measurement results of the obtained lactone polymer (polycaprolactone) (M n , M w / M n The analytical results of the acid value (mgKOH / g) and color number (APHA) are shown in Table 1.
[0042] [Example 2] Synthesis of polycaprolactone A lactone polymer was obtained as a colorless solid (at room temperature) (108 g, yield 95%) in the same manner as in Example 1, except that 5.0 g (0.06 mol, water content 200 ppm, manufactured by Kishida Chemical Co., Ltd.) of 2-methyl-1,3-propanediol (MPD) was used instead of the ethylene glycol in Example 1. The analytical results of the obtained polymer were measured in the same manner as in Example 1 and are summarized in Table 1.
[0043] [Example 3] Synthesis of polycaprolactone A lactone polymer was obtained as a colorless solid (at room temperature) (107 g, yield 94%) in the same manner as in Example 1, except that 10.0 g (0.07 mol, water content 200 ppm, manufactured by Kishida Chemical Co., Ltd.) of trimethylolpropane (TMP) was used instead of ethylene glycol in Example 1. The analytical results of the obtained polymer were measured in the same manner as in Example 1 and are summarized in Table 1.
[0044] [Example 4] Synthesis of polycaprolactone A lactone polymer was obtained as a colorless solid (at room temperature) (104 g, yield 91%) in the same manner as in Example 1, except that 13.6 g (0.10 mol, water content 200 ppm, manufactured by Kishida Chemical Co., Ltd.) of pentaerythritol (PEN) was used instead of the ethylene glycol in Example 1. The analytical results of the obtained polymer were measured in the same manner as in Example 1 and are summarized in Table 1.
[0045] [Example 5] Synthesis of polycaprolactone A lactone polymer was obtained as a colorless solid (at room temperature) (109 g, yield 96%) in the same manner as in Example 1, except that 4.0 g (0.03 mol, manufactured by Sigma-Aldrich Japan) of boron trifluoride tetrahydrofuran (BF3THF) was used instead of the phosphotungstic acid in Example 1. The analytical results of the obtained polymer were measured in the same manner as in Example 1 and are summarized in Table 1.
[0046] [Example 6] Synthesis of polyurethane In a 200 mL reaction vessel, 100.0 g (0.04 mol) of the lactone polymer (polycaprolactone, PCL) synthesized in Example 1 was placed, heated to 70° C., 34.6 g (0.14 mol, manufactured by Tosoh Corporation) of 4,4'-diphenylmethane diisocyanate (MDI) was added, and the mixture was stirred at 80° C. for 3 hours. The vessel was depressurized to degas the reaction liquid, and then 8.2 g (0.09 mol, manufactured by Kishida Chemical Co., Ltd.) of 1,4-butanediol was added, and the mixture was stirred at 85 to 90° C. for 3 minutes. The mixture was then poured into a glass plate mold, aged in a dryer at 110° C. for 3 hours, and allowed to cool to give a (poly)urethane sheet (thickness 2 mm).
[0047] [Example 7] Synthesis of polyurethane 100.0g (0.04mol) of the lactone polymer (polycaprolactone, PCL) synthesized in Example 2 was placed in a 200mL reaction vessel, heated to 70°C, 35.3g (0.14mol, Tosoh Corporation) of 4,4'-diphenylmethane diisocyanate (MDI) was added, and the mixture was stirred at 80°C for 3 hours. The vessel was depressurized to degas the reaction liquid, and then 8.2g (0.09mol, Kishida Chemical Co., Ltd.) of 1,4-butanediol was added and the mixture was stirred at 85-90°C for 3 minutes. The mixture was then poured into a glass plate mold, aged in a dryer at 110°C for 3 hours, and cooled to obtain a (poly)urethane sheet (thickness 2mm).
[0048] [Example 8] Synthesis of polyurethane 100.0g (0.08mol) of the lactone polymer (polycaprolactone, PCL) synthesized in Example 4 was placed in a 200mL reaction vessel, heated to 70°C, 45.8g (0.18mol, Tosoh Corporation) of 4,4'-diphenylmethane diisocyanate (MDI) was added, and the mixture was stirred at 80°C for 3 hours. The vessel was depressurized to degas the reaction liquid, and then 8.9g (0.10mol, Kishida Chemical Co., Ltd.) of 1,4-butanediol was added and the mixture was stirred at 85-90°C for 3 minutes. The mixture was then poured into a glass plate mold, aged in a dryer at 110°C for 3 hours, and cooled to obtain a (poly)urethane sheet (thickness 2mm).
[0049] [Measurement of breaking strength and elongation at break of polyurethane] The 2 mm thick urethane sheet prepared as described above was cut into a No. 3 dumbbell shape and aged for 5 days at 23°C and 50% RH to prepare an evaluation sample for tensile testing. The tensile strength (MPa) and elongation at break (%) of this sample were measured at 23°C and 50% RH using a Tensilon tensile tester (Shimadzu Corporation, model: AG-1) with a chuck distance of 20 mm and a tensile speed of 500 mm / min. Three measurements were made, and the average values were calculated. The measurement results for each physical property of the obtained polyurethane are shown in Table 2.
[0050] [Measurement of thermal decomposition temperature of polyurethane] The following equipment was used to measure the thermal decomposition temperature of polyurethane. Device name: Thermogravimetry-differential thermal analysis device (TG-DTA) (manufactured by Mac Science Co., Ltd., model: DSC 3100S) Sample size: 10mg Heating conditions: 20 to 500°C, heating rate: 20°C / min The thermal decomposition temperature was measured at a weight change of 1%. The measurement results of the thermal decomposition temperatures (°C) of the obtained polyurethanes are shown in Table 2.
[0051] [Comparative Example 1]: Synthesis of polycaprolactone A polymer was obtained as a colorless solid (at room temperature) (106 g, yield 93%) by the same procedure and under the same conditions as in Example 1, except that 5.0 g (0.05 mol, water content 600 ppm) of 2-methyl-1,3-propanediol was used instead of ethylene glycol in Example 1. The analytical results of the obtained polymer were measured in the same manner as in Example 1 and are summarized in Table 1.
[0052] [Comparative Example 2] Synthesis of polycaprolactone A lactone polymer was obtained as a colorless solid (at room temperature) (108 g, yield 95%) in the same manner as in Example 1, except that the ethylene glycol used in Example 1 had a water content of 800 ppm. The obtained polymer was analyzed in the same manner as in Example 1, and the analytical results are summarized in Table 1.
[0053] [Comparative Example 3] Synthesis of polycaprolactone A polymer was obtained as a brown solid (room temperature) (112 g, yield 98%) in the same manner as in Example 1, except that the reaction temperature in Example 1 was 120° C. The obtained polymer was analyzed in the same manner as in Example 1, and the results are summarized in Table 1.
[0054] [Comparative Example 4] Synthesis of polyurethane 100.0g (0.05mol) of polycaprolactone synthesized in Comparative Example 2 was placed in a 200mL reaction vessel, heated to 70°C, 36.6g (0.15mol) of 4,4'-diphenylmethane diisocyanate (MDI) was added, and the mixture was stirred at 80°C for 3 hours. After decompressing the vessel and degassing, 8.3g (0.09mol) of 1,4-butanediol was added and the mixture was stirred at 85-90°C for 3 minutes. The mixture was then cast onto a glass plate, aged in a dryer at 110°C for 3 hours, and cooled to obtain a (poly)urethane sheet (thickness 2mm). The results of the measurement of each physical property of the obtained polyurethane in the same manner as in Example 6 are summarized in Table 2.
[0055] [Table 1]
[0056] [Table 2]
[0057] As described above, the urethane polymer of the embodiment of the present invention has a molecular weight distribution M w / M n The molecular weight distribution (Mg / mol) is 1.08 to 1.23, which is close to monodispersity, and the color number and acid value are low, which are superior to the urethane polymers of the comparative examples. The polyurethanes produced using the lactone polymers of the examples of the present invention are superior in terms of breaking strength, breaking elongation, and thermal decomposition temperature, which are higher than those of the comparative examples. These features make it possible to improve the physical properties, processability, handling, heat resistance, and other problems that conventional lactone polymers have as raw materials for polyurethanes, polyesters, and the like. [Industrial Applicability]
[0058] The method for producing a lactone polymer of the present invention can provide a lactone polymer having a molecular weight distribution close to monodisperse, a low color number, and a low acid value. In addition, the lactone polymer obtained by the method for producing a lactone polymer of the present invention can be used as a raw material to produce polyurethanes and polyesters having excellent resin properties, processability, heat resistance, etc.
Claims
1. A lactone compound represented by the following general formula (1): A method for producing a lactone polymer obtained by ring-opening polymerization at a reaction temperature of 100° C. or less, comprising the steps of: A heteropolyacid is used as a catalyst in an amount of 0.0001 to 0.1 mol per 1 mol of the lactone compound, In the ring-opening polymerization, an active hydrogen atom-containing compound is used as an initiator, The method for producing a lactone polymer comprises adjusting the water content of the active hydrogen atom-containing compound to 1 to 500 ppm. 【Chemistry 1】 [In formula (1), R 1 ~R 3 each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms, and n represents an integer of 0 to 6.
2. The method for producing a lactone polymer described in claim 1, wherein the reaction temperature for the ring-opening polymerization is 90°C or lower.
3. A method for producing a lactone polymer described in claim 1 or 2, wherein the lactone polymer has a number average molecular weight of 1,264 or more.
4. The active hydrogen atom-containing compound is a polyhydric alcohol, The method for producing a lactone polymer according to any one of claims 1 to 3, wherein 0.01 to 10 mol of a polyhydric alcohol is used per 1 mol of the lactone compound.
5. The method for producing a lactone polymer described in any one of claims 1 to 4, characterized in that the reaction temperature for the ring-opening polymerization is 60°C or higher.
6. A method for producing a polyurethane, comprising a step of reacting a lactone polymer obtained by the method for producing a lactone polymer according to any one of claims 1 to 5 with a polyisocyanate compound to produce a polyurethane.
7. A method for producing a polyester, comprising a step of reacting a lactone polymer obtained by the method for producing a lactone polymer according to any one of claims 1 to 5 with a polyol compound to produce a polyester.
Citation Information
Patent Citations
Lactone polymer having narrow molecular weight distribution and its preparation
JP1982155230A
Production of lactone-modified compound
JP1986200120A
Production of lactone polymer
JP1988196623A
Preparation of lactone polyol
JP1990043217A
Composition containing reactive monomer and its preparation
JP1992089822A