Method for producing copolymers of 5-membered cyclic ethers and lactones
The copolymerization of 5-membered cyclic ethers and lactones using a trace heteropolyacid catalyst at controlled temperatures addresses molecular weight control issues, producing high-quality polyethers without waste acid treatments, enhancing industrial efficiency.
Patent Information
- Application Number
- JP2020139410
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-26
- Filing Date
- 2020-08-20
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-08-20
AI Technical Summary
Conventional methods for copolymerizing 3- or 4-membered cyclic ethers and lactones face challenges in controlling molecular weight, leading to high blockiness and the production of low polymers due to side reactions, and require costly waste acid treatments.
A method involving the copolymerization of 5-membered cyclic ethers and lactones using a trace amount of heteropolyacid catalyst at controlled temperatures (10°C to 50°C) with a hydroxyl group-containing initiator, allowing easy catalyst removal and molecular weight control.
The method enables the production of high-quality polyethers with controlled molecular weight, avoiding side reactions and simplifying the process by eliminating waste acid treatments, thus being industrially efficient and cost-effective.
Smart Images

Figure 0007572185000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a copolymer of a five-membered cyclic ether and a lactone. [Background technology]
[0002] It has been known for some time that cyclic ethers, such as tetrahydrofuran (THF), can be polymerized with cationic catalysts such as protonic acids, Lewis acids, and ion complexes. It is also known that lactones, such as β-propiolactone and ε-caprolactone, can be easily polymerized with either cationic or anionic catalysts. Polymers such as polytetramethylene ether glycol and polycaprolactone glycol obtained in this way are useful materials as soft segments for polyurethane resins and polyester resins.
[0003] Polytetramethylene ether glycol has a polyether as its main chain, while ring-opening polymers of lactones such as polycaprolactone glycol have a polyester as their main chain, and therefore have opposing advantages and disadvantages in terms of hydrolysis resistance, heat resistance, light resistance, and the like. As a solution to complement these mutual disadvantages, polyether polyester glycol obtained by copolymerization of THF and lactones is considered. However, there is a large difference in the polymerizability between THF and lactones, and copolymerization is difficult. As a method for copolymerizing THF and ε-caprolactone, a method using a Lewis acid as a catalyst (Non-Patent Document 1) is known, but the resulting copolymer has a high blocking property, that is, THF and ε-caprolactone are not randomly polymerized, and the resulting copolymer becomes something like a block copolymer of polytetrahydrofuran and poly ε-caprolactone or a mixture of polytetramethylene ether and polycaprolactone glycol.
[0004] In order to solve these problems, a copolymerization method of THF and ε-caprolactone has been reported, which is characterized by using a Lewis acid catalyst such as boron trifluoride (BF3)-based, fuming sulfuric acid-based, or fluorosulfuric acid-based catalyst in combination with a 3- or 4-membered cyclic ether (e.g., Patent Document 1).
[0005] Also, a method for copolymerizing lactones with cyclic ethers has been reported using an anionic ring-opening polymerization catalyst such as tetrabutyl titanate or by carrying out the reaction at high temperatures of 100° C. to 200° C. (eg, Patent Document 2). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Laid-Open No. 63-178131 [Patent Document 2] JP 2019-23256 A [Non-patent literature]
[0007] [Non-Patent Document 1] "Polymer Journal", (Japan), 1971, Volume 3, No. 3, p.389-393 Summary of the Invention [Problem to be solved by the invention]
[0008] The molecular weight of the copolymer cannot be controlled by only using 3- or 4-membered cyclic ethers, and therefore it is not possible to obtain a copolymer with a target molecular weight. Furthermore, catalyst systems such as boron trifluoride, fuming sulfuric acid, and fluorosulfuric acid have problems such as the need for fluorination treatment in the subsequent treatment and the disposal of a large amount of waste acid. In addition, anionic polymerization at high temperatures involves side reactions such as ester exchange reactions, resulting in a large amount of low polymers, and so conventional manufacturing methods have problems such as the inability to control the molecular weight of the copolymer, the need to dispose of a large amount of waste acid, and impurities due to side reactions in polymerization at high temperatures. [Means for solving the problem]
[0009] In view of the above-mentioned circumstances, the inventors of the present invention have conducted intensive research and have found a production method in which a 5-membered cyclic ether can be copolymerized with a lactone by a polymerization process in which a 3- or 4-membered cyclic ether is used in combination as an initiator under conditions in which the amount of heteropolyacid catalyst used is reduced to a trace amount, thereby completing the present invention.
[0010] That is, the method for producing the copolymer of the present invention comprises the steps of: [1] A method for producing a copolymer of a 5-membered cyclic ether (A) and a lactone (B), comprising carrying out a copolymerization reaction in the temperature range of 10°C to 50°C using a Lewis acid and / or a solid acid (preferably a heteropolyacid) as a catalyst, optionally using an active hydrogen atom-containing compound having a hydroxyl group, an amino group, or a mercapto group as a reaction initiator (C), and also using a 3- or 4-membered cyclic ether (D).
[0011] [2] The method for producing a copolymer according to [1], wherein the 5-membered cyclic ether (A) is a tetrahydrofuran, and the amount added (mixing ratio) is 1 to 90 mol % based on the total number of moles of the 5-membered cyclic ether (A) and the lactone (B).
[0012] [3] The method for producing a copolymer according to [1], wherein the lactone (B) is β-propiolactone, γ-butyrolactone, δ-valerolactone, or ε-caprolactone, each of which may have a substituent, and the amount of lactone (B) added (blending ratio) is 1 to 90 mol % based on the total number of moles of the five-membered cyclic ether (A) and the lactone (B).
[0013] [4] The method for producing a copolymer according to [1], wherein the reaction initiator (C) is a hydroxy compound having one or more hydroxyl groups, and the amount added is 0 to 20 mol % based on the total number of moles of the five-membered cyclic ether (A) and the lactone (B).
[0014] [5] The method for producing a copolymer according to [1], wherein the 3- or 4-membered cyclic ether (D) is an epoxide or an oxetane, and the amount added is 0.1 to 50 mol % based on the total moles of the 5-membered cyclic ether (A) and the lactone (B).
[0015] [6] The method for producing a copolymer according to [1], wherein the catalyst is an untreated heteropolyacid, and the amount of the catalyst added is 0.01 to 2 mol % based on the total number of moles of the five-membered cyclic ether (A) and the lactone (B).
[0016] [7] A method for producing a copolymer of a 5-membered cyclic ether (A) and lactones (B), comprising carrying out a copolymerization reaction in a temperature range of 10°C to 50°C, using 0.01 to 2 mol% of a heteropolyacid as a catalyst relative to the total molar number of the 5-membered cyclic ether (A) and lactones (B), using 0 to 5 mol% of a hydroxy compound having one or more hydroxyl groups as a reaction initiator (C), and using in combination 40 to 80 mol% of the 5-membered cyclic ether (A) which is a tetrahydrofuran, 20 to 60 mol% of the lactone (B) which is ε-caprolactone, and 5 to 20 mol% of the 3- or 4-membered cyclic ether (D).
[0017] [8] A method for producing polyurethane, comprising reacting the copolymer obtained by the method for producing polyurethane according to any one of [1] to [7] with a polyisocyanate compound. Effect of the Invention
[0018] In the method for producing a copolymer of a 5-membered cyclic ether and a lactone in the present invention, a small amount of untreated heteropolyacid is used, so that the heteropolyacid can be easily adsorbed and removed with an ion exchange resin, and then the copolymer of the 5-membered cyclic ether and the lactone can be obtained simply by distilling off the unreacted cyclic ether. The method for producing a copolymer of a 5-membered cyclic ether and a lactone in the present invention is an extremely simple method since it does not require any steps such as hydrolysis or washing, and does not require any treatment of the waste acid or wastewater generated.
[0019] In addition, in the method for producing a copolymer of a five-membered ring cyclic ether and a lactone according to the present invention, the polymerization reaction can be carried out even in an inert organic solvent by determining the optimum polymerization reaction temperature based on the type and amount of initiator, the quality and molecular weight of the target polymer, etc. Moreover, the copolymer obtained at a temperature of 50° C. or less is free from quality deterioration due to side reactions, such as coloration.
[0020] Furthermore, in the method for producing a copolymer of a five-membered ring cyclic ether and a lactone according to the present invention, the molecular weight can be easily controlled by changing the amount of catalyst used and the amount of initiator charged, so that it is possible to control the molecular weight of the copolymer.
[0021] Therefore, the method for producing a copolymer of a five-membered cyclic ether and a lactone according to the present invention is an excellent method which is industrially very simple and efficient in terms of production process, and which can produce a high-quality polyether. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] The present invention will now be described in more detail with reference to preferred embodiments.
[0023] Specific examples of lactones (B) include β-propiolactone, β-butyrolactone, β-valerolactone, γ-butyrolactone, γ-valerolactone, γ-caprylolactone, δ-valerolactone, β-methyl-δ-valerolactone, δ-stearolactone, ε-caprolactone, 2-methyl-ε-caprolactone, 4-methyl-ε-caprolactone, ε-caprylolactone, and ε-palmitolactone.
[0024] Examples of the 3- to 4-membered cyclic ether (D) include epoxides such as ethylene oxide, propylene oxide, and epichlorohydrin, and oxetanes such as 3-methyloxetane and 3,3-bis(chloromethyl)-oxetane.
[0025] When using the 3- or 4-membered cyclic ether (D), the amount of addition is preferably 0.1 to 50 mol %, particularly preferably 0.1 to 10 mol %, based on the total number of moles of the 5-membered cyclic ether (A) and the lactones (B). When the 3- or 4-membered cyclic ether (D) is not used, the copolymerization does not proceed and the product becomes something like a mixture of the cyclic ether polymer and the lactones polymer. When the 3- or 4-membered cyclic ether (D) exceeds 50 mol %, the composition ratio of the polymer changes significantly, causing a decrease in physical properties, and a large amount of unreacted material is generated, which is costly to remove, and is therefore undesirable.
[0026] Examples of the five-membered cyclic ether (A) include tetrahydrofurans such as tetrahydrofuran, 2-methyltetrahydrofuran, and 3-methyltetrahydrofuran, and dioxolane.
[0027] This is a method for copolymerizing a 5-membered cyclic ether (A) and a lactone (B), characterized in that when the 5-membered cyclic ether (A) is used, the amount of the 5-membered cyclic ether (A) added is preferably 1 to 90 mol %, and particularly preferably 10 to 80 mol %, based on the total moles of the 5-membered cyclic ether (A) and the lactone (B).
[0028] The active hydrogen atom-containing compound is one that contains a hydroxyl group, an amino group, or a mercapto group, and is used as the reaction initiator (C). Examples of compounds that contain a hydroxyl group include aliphatic alcohols such as methanol, ethanol, propanol, n-butanol, secondary and tertiary butanol, allyl alcohol, and 2-hydroxyethyl methacrylate, aromatic alcohols such as benzyl alcohol and phenylmethylcarbinol, alicyclic alcohols such as cyclohexanol and trimethylhexanol, ethylene glycol, propylene glycol, 1,4-butanediol, polyethylene glycol, polypropylene glycol, polyoxytetramethylene glycol, and polyols such as glycerin, trimethylolpropane, cyclohexanediol, and xylylene glycol, as well as various phenols, organic carboxylic acids, and examples of compounds that contain an amino group include methyl-, ethyl-, n-propyl-, isopropyl-, n-butyl-, and the like. Examples of the mercapto group-containing compounds include primary aliphatic amines such as butyl-, sec-, and tert-butyl amines and the corresponding secondary aliphatic amines such as dialkylamines; aromatic, alicyclic, and heterocyclic amines such as aniline, triidine, diphenylamine, cyclohexylamine, and piperidine; and aliphatic, aromatic, alicyclic, and heterocyclic polyamines such as ethylenediamine, propylenediamine, hexamethylenediamine, o-, m-, and p-phenylenediamine, 1,4-cyclohexanediamine, piperazine, diethylenetriamine, and 4,4',4"-methylidynetrianiline. Examples of the mercapto group-containing compounds include aliphatic mercaptans such as methyl-, ethyl-, propyl-, and butyl-, aromatic mercaptans such as benzyl mercaptan, ethylenedithioglycol, xylylenedimercaptan, and mercaptoethanol.
[0029] This is a method for copolymerizing a 5-membered cyclic ether (A) and a lactone (B), characterized in that when a polyhydric alcohol is used as the initiator (C), the amount used is preferably 0 to 20 mol % (preferably excluding 0 mol %), particularly preferably 0.1 to 1.0 mol, based on the total number of moles of the 5-membered cyclic ether (A) and the lactone (B). When the amount of the initiator (C) used exceeds 20 mol %, the molecular weight of the product is small, and sufficient polymer may not be produced. When the initiator (C) is not used, the molecular weight cannot be controlled, and the product with the desired molecular weight may not be obtained.
[0030] Examples of solid acids used in the present invention include silicon dioxide, titanium dioxide, zirconium dioxide, aluminum oxide, and heteropolyacids (e.g., phosphotungstic acid, silicotungstic acid, phosphomolybdic acid, and silicomolybdic acid). Examples of Lewis acids include metal or nonmetal halides such as boron trifluoride, phosphorus pentafluoride, antimony pentafluoride, antimony pentachloride, aluminum chloride, titanium tetrachloride, and tin tetrachloride. Examples of the form of these catalysts when used include complexes of boron trifluoride, antimony pentachloride, and the like with chain and cyclic ethers such as diethyl ether and tetrahydrofuran.
[0031] The present invention relates to a method for copolymerizing a 5-membered cyclic ether (A) and a lactone (B), characterized in that the amount of Lewis acid and / or solid acid catalyst used is preferably 2 mol% or less, particularly preferably 0.1 to 1.0 mol, based on the total moles of the 5-membered cyclic ether (A) and the lactone (B). The method is characterized in that the amount of catalyst used is extremely small, and therefore easy to remove. When the amount of catalyst used exceeds 2 mol%, heat generation becomes significant, the molecular weight distribution becomes extremely wide, and quality deterioration due to side reactions, such as coloring, may occur. In addition, since it becomes difficult to remove the catalyst using an ion exchange resin, a water washing step is required, and the removal of the catalyst may be costly and undesirable.
[0032] The polymerization reaction temperature is preferably 50°C or less, and more preferably 0°C to 40°C, but the optimum temperature is determined by the type and amount of initiator (C), the quality and molecular weight of the target polymer, etc., and is usually 20°C to 40°C. The polymerization reaction can also be carried out in an inert organic solvent. In bulk polymerization at a relatively low temperature, crystallization is likely to occur as the polymerization proceeds, so it is preferable to carry out the polymerization in an inert organic solvent such as benzene, toluene, or xylene. At temperatures exceeding 100°C, the molecular weight distribution is extremely broadened and quality deterioration due to side reactions, such as coloring, is significant. On the other hand, the polymerization reaction time is related to the reaction rate and varies depending on the temperature, the type and amount of initiator (C) used, etc. It is generally set to 2 to 10 hours or more. In this polymerization system, it is preferable to carry out the polymerization until the unreacted lactone disappears in order to simplify the purification operation of the polymer and improve the quality, and it is necessary to carry out sufficient aging.
[0033] The method for producing a polyurethane resin using the copolymer of the five-membered cyclic ether (A) and lactones (B) obtained in the present invention is not particularly limited, and the resin can be produced by a known method, etc. For example, a polyisocyanate component may be charged all at once into a polyol, a chain extender, and an organometallic catalyst and reacted, or a polyol and a polyisocyanate component may be reacted to obtain a prepolymer terminated with an isocyanate group, and then a chain extender may be added to carry out an elongation reaction.
[0034] Examples of the polyisocyanate compound include aromatic, alicyclic, and aliphatic polyisocyanates having two or more isocyanate groups.
[0035] Specific examples include polyisocyanates such as tolylene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), polymethylene polyphenyl polyisocyanate (MDI), xylylene diisocyanate (XDI), isophorone diisocyanate (IPDI), and hexamethylene diisocyanate (HMDI). Among these, MDI is particularly preferred from the viewpoints of ease of availability and control of the reaction with hydroxyl groups.
[0036] Chain extenders include low molecular weight dihydric alcohols such as 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, and the like.
[0037] The organometallic catalyst is not particularly limited, but specific examples include organotin catalysts such as dibutyltin oxide, dibutyltin diacetate, dibutyltin dilaurate, dibutyltin dichloride, dioctyltin dilaurate, etc., nickel octylate, nickel naphthenate, cobalt octylate, cobalt naphthenate, bismuth octylate, bismuth naphthenate, etc. Among these, preferred compounds are organotin catalysts, and more preferred is dibutyltin dilaurate.
[0038] The amount of the organometallic catalyst used is usually in the range of 0.0001 to 5.0 parts by weight, and more preferably in the range of 0.001 to 3.0 parts by weight, based on 100.0 parts by weight of the copolymer of the five-membered cyclic ether (A) and the lactone (B).
[0039] The measurement methods used in the present invention will be described below.
[0040] [Method for measuring number average molecular weight (Mn) of 5-membered cyclic ether and lactone copolymer] The number average molecular weight (Mn) of the lactone polymer in the present invention can be measured by gel permeation chromatography (hereinafter abbreviated as GPC) under the following conditions, for example. Equipment: TOSOH HPLC-8320GPC (Tosoh Corporation) Column: TSKgel G4000H + G2500H (same as above) Detector: RI Eluent: Tetrahydrofuran Standard substance: Polytetramethylene ether glycol Injection volume 100μL Flow rate 1.0mL / min Measurement temperature 40℃
[0041] [Method for measuring the color number of 5-membered cyclic ether and lactone copolymers] The color number in the present invention can be determined by JIS K4101-1993-13 method. EXAMPLES
[0042] The present invention will be described below with reference to examples, but these are not intended to limit the present invention in any way.
[0043] [Example 1] [Synthesis of THF-polycaprolactone copolymer] A 500 mL four-necked separable flask was charged with 63.3 g of ε-caprolactone (B) (0.56 mol, 50 mol% relative to the total number of moles of the 5-membered cyclic ether (A) and lactones (B), manufactured by Tokyo Chemical Industry Co., Ltd.), 40.0 g of THF (A) (0.56 mol, 50 mol% relative to the total number of moles of the 5-membered cyclic ether (A) and lactones (B), 1.7 g of 1,4-butanediol (C) (0.02 mol, 1.6 mol% relative to the total number of moles of the 5-membered cyclic ether (A) and lactones (B), manufactured by Kishida Chemical Co., Ltd.), and 0.6 g of phosphotungstic acid (catalyst) (0.0003 mol, 0.02 mol% relative to the total number of moles of the 5-membered cyclic ether (A) and lactones (B), manufactured by Japan New Metals Co., Ltd.), and was equipped with a thermometer, a nitrogen seal, and a stirrer. After stirring for 15 minutes at 25°C, 6.4 g of propylene oxide (D) (0.11 moles, 10.0 mol% based on the total moles of the 5-membered cyclic ether (A) and lactones (B), manufactured by Kishida Chemical Co., Ltd.) was added and reacted at 25°C for 4 hours. Next, 100 mL of THF and 50 g of ion exchange resin IRA-96S (manufactured by Organo Corporation) were added to this reaction mixture as a washing solvent and stirred for 2 hours. This reaction mixture was filtered, and THF was removed from the filtrate by distillation under reduced pressure to obtain a polymer. The composition ratio of each raw material, reaction temperature / stirring time, and the yield, number average molecular weight (Mn), and color number of the obtained polymer are shown in Table 1.
[0044] [Example 2] [Synthesis of THF-polycaprolactone copolymer] A polymerization reaction was carried out under the same conditions and by the same operation as in Example 1, except that the amount of ε-caprolactone and the amount of THF were changed to 37.7 g (0.33 mol) and 55.5 g (0.77 mol), respectively. The composition ratio of each raw material, the reaction temperature / stirring time, and the analysis results of the yield, number average molecular weight (Mn), and color number of the obtained polymer are shown in Table 1.
[0045] [Example 3] [Synthesis of 3-methyl-THF-polycaprolactone copolymer] A polymerization reaction was carried out under the same conditions and by the same operation as in Example 1, except that 48.2 g (0.56 mol) of 3-methyl-THF was used instead of 40.0 g (0.56 mol) of THF in Example 1. The composition ratio of each raw material, reaction temperature / mixing time, and the yield, number average molecular weight (Mn), and color number of the obtained polymer are shown in Table 1.
[0046] [Example 4] [Synthesis of dioxolane-polycaprolactone copolymer] A polymerization reaction was carried out under the same conditions and by the same operation as in Example 1, except that 41.5 g (0.56 mol) of 1,3-dioxolane (Kishida Chemical Co., Ltd.) was used instead of 40.0 g (0.56 mol) of THF in Example 1. The composition ratio of each raw material, reaction temperature / mixing time, and the yield, number average molecular weight (Mn), and color number of the obtained polymer are shown in Table 1.
[0047] [Example 5] [Synthesis of THF-polycaprolactone copolymer] A polymerization reaction was carried out under the same conditions and by the same operation as in Example 1, except that 0.6 g (0.0003 mol) of phosphotungstic acid in Example 1 was replaced with 1.5 g (0.01 mol, manufactured by Sigma-Aldrich Japan) of boron trifluoride tetrahydrofuran complex. The composition ratio of each raw material, reaction temperature / mixing time, and the yield, number average molecular weight (Mn), and color number of the obtained polymer are shown in Table 1.
[0048] [Example 6] [Synthesis of THF-polycaprolactone copolymer] The polymerization reaction was carried out under the same conditions and with the same operations as in Example 1, except that 1.7 g (0.02 mol) of 1,4-butanediol in Example 1 was changed to 2.4 g (0.03 mol). The composition ratios of the respective raw materials, the reaction temperature / stirring time, and the analysis results of the yield, number average molecular weight (Mn), and color number of the obtained polymer are listed in Table 1.
[0049] [Example 7] [Synthesis of THF-Polycaprolactone Copolymer] The polymerization reaction was carried out under the same conditions and with the same operations as in Example 1, except that 1.7 g (0.02 mol) of 1,4-butanediol in Example 1 was changed to 3.2 g (0.04 mol). The composition ratios of the respective raw materials, the reaction temperature / stirring time, and the analysis results of the yield, number average molecular weight (Mn), and color number of the obtained polymer are listed in Table 1.
[0050] [Example 8] <Synthesis of THF-Polycaprolactone Copolymer> The polymerization reaction was carried out under the same conditions and with the same operations as in Example 1, except that 1.7 g (0.02 mol) of 1,4-butanediol in Example 1 was not used. The type of THF, the composition ratios of the respective raw materials, the reaction temperature / stirring time, and the analysis results of the yield, number average molecular weight (Mn), and color number of the obtained polymer are listed in Table 1.
[0051] [Comparative Example 1] <Synthesis of THF-Polycaprolactone Copolymer> The polymerization reaction was carried out under the same conditions and with the same operations as in Example 1, except that the reaction temperature in Example 1 was set to 60°C. The composition ratios of the respective raw materials, the reaction temperature / stirring time, and the analysis results of the yield, number average molecular weight (Mn), and color number of the obtained polymer are listed in Table 1.
[0052] [Comparative Example 2] <Synthesis of THF-Polycaprolactone Copolymer> A polymerization reaction was carried out under the same conditions and by the same operation as in Example 1, except that the catalyst addition amount in Example 1 was 2.1 mol%. 100 mL of THF and 50 g of ion exchange resin IRA-96S (manufactured by Organo Corporation) were added to the obtained reaction mixture as a washing solvent, and the mixture was stirred for 2 hours, and the reaction mixture was filtered. The filtrate was cloudy and had an acidic pH, clearly indicating the presence of the catalyst. Therefore, 100 g of ion exchange water was added to the filtrate, and the mixture was stirred at 60°C for 1 hour, and then allowed to stand for 1 hour, and the aqueous layer was separated and discarded. This operation was repeated three times. 50 g of ion exchange resin IRA-96S (manufactured by Organo Corporation) was added to the obtained oil layer, and the mixture was stirred for 2 hours. The reaction mixture was filtered. THF was removed from the filtrate by distillation under reduced pressure to obtain a polymer. The composition ratio of each raw material, reaction temperature / stirring time, and the yield, number average molecular weight (Mn), and color number of the obtained polymer are shown in Table 1.
[0053] [Table 1]
[0054] The abbreviations listed in Table 1 are explained below. CL: ε-caprolactone 3MeTHF: 3-methyl-tetrahydrofuran DOX: 1,3-dioxolane PO: Propylene oxide [Industrial Applicability]
[0055] As is clear from the examples and comparative examples, the molecular weight of the polymer obtained by the production method of the present invention can be easily controlled by changing the amount of initiator (C). In addition, even if a small amount of catalyst, heteropolyacid, metal or nonmetal halide, is added (1 mol% or less based on the total mole number of the 5-membered cyclic ether (A) and lactones (B)), the copolymerization reaction can proceed smoothly. Furthermore, if the amount added is 2 mol% or less based on the total mole number of the 5-membered cyclic ether (A) and lactones (B), the waste acid, which is the remaining catalyst, can be easily and completely removed by ion exchange resin, and the copolymer can be obtained by simply distilling off the unreacted THF. In addition, since the reaction is carried out at room temperature, the copolymer can be obtained with a satisfactory number of colors with little coloring or impurity generation. The production method of the present invention is an excellent production method that is industrially very simple and waste-free, and can obtain high-quality polyether.
Claims
1. A method for producing a copolymer of a 5-membered cyclic ether (A) and a lactone (B), comprising carrying out a copolymerization reaction in a temperature range of 10°C to 50°C using a heteropolyacid as a catalyst, optionally using an active hydrogen atom-containing compound having a hydroxyl group, an amino group, or a mercapto group as a reaction initiator (C), and also using a 3- or 4-membered cyclic ether (D), The method for producing a copolymer, wherein the amount of the catalyst added is 0.01 to 2 mol % based on the total number of moles of the five-membered cyclic ether (A) and the lactone (B).
2. 2. The method for producing a copolymer according to claim 1, wherein the five-membered cyclic ether (A) is a tetrahydrofuran, and the amount of the tetrahydrofuran added is 1 to 90 mol % based on the total moles of the five-membered cyclic ether (A) and the lactone (B).
3. 2. The method for producing a copolymer according to claim 1, wherein the lactone (B) is β-propiolactone, γ-butyrolactone, δ-valerolactone, or ε-caprolactone, each of which may have a substituent, and the amount of the lactone (B) added is 1 to 90 mol % based on the total number of moles of the five-membered cyclic ether (A) and the lactone (B).
4. The method for producing a copolymer according to claim 1, wherein the reaction initiator (C) is a hydroxy compound having one or more hydroxyl groups, and the amount of the reaction initiator (C) added is 0 to 20 mol % based on the total number of moles of the five-membered cyclic ether (A) and the lactone (B).
5. The method for producing a copolymer according to claim 1, wherein the 3- or 4-membered cyclic ether (D) is an epoxide or an oxetane, and the amount of the 3- or 4-membered cyclic ether (D) added is 0.1 to 50 mol % based on the total moles of the 5-membered cyclic ether (A) and the lactone (B).
6. 2. The method for producing a copolymer according to claim 1, wherein the catalyst is an untreated heteropolyacid.
7. 2. A method for producing a copolymer of a 5-membered cyclic ether (A) and a lactone (B), comprising using, as a reaction initiator (C), a hydroxy compound having one or more hydroxyl groups, which accounts for 0 to 5 mol % of the total number of moles of the 5-membered cyclic ether (A) and the lactone (B), in combination with the 5-membered cyclic ether (A) which is 40 to 80 mol % of a tetrahydrofuran, the lactone (B) which is 20 to 60 mol % of ε-caprolactone, and the 3- or 4-membered cyclic ether (D) which is 5 to 20 mol %.
8. A method for producing polyurethane, comprising reacting the copolymer obtained by the method according to any one of claims 1 to 7 with a polyisocyanate compound to produce a polyurethane.
Citation Information
Patent Citations
JP1971、3
Production of lactone-modified compound
JP1986200120A
Copolymerization of tetrahydrofuran with lactones
JP1988178131A