Polyhydric hydroxyl resin, epoxy resin, their methods of manufacture, epoxy resin composition and cured product using them
A novel polyhydric hydroxy resin and epoxy resin composition improve thermal conductivity and dielectric properties, overcoming the limitations of existing epoxy resins for semiconductor encapsulation and printed wiring boards.
Patent Information
- Application Number
- JP2020206111
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-11
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-12-11
AI Technical Summary
Existing epoxy resins fail to meet the requirements of high thermal conductivity, low dielectricity, and moisture resistance necessary for advanced semiconductor encapsulation and printed wiring boards, with known materials exhibiting issues such as moisture resistance, heat resistance, and moldability.
A novel polyhydric hydroxy resin and epoxy resin composition are developed, characterized by specific molecular structures and production methods, including the reaction of aromatic dihydroxy compounds with aromatic fluorine compounds and epichlorohydrin, to enhance thermal conductivity and dielectric properties.
The cured products exhibit excellent heat resistance, low dielectricity, and moisture resistance, suitable for applications like lamination, molding, and bonding, addressing the limitations of existing epoxy resins.
Smart Images

Figure 0007572226000010 
Figure 0007572226000011 
Figure 0007572226000012
Abstract
Description
[Technical field]
[0001] The present invention relates to an epoxy resin which gives a cured product having excellent low dielectric properties as well as excellent thermal conductivity, moisture resistance, heat resistance, etc., an intermediate thereof, a curing agent, and an epoxy resin composition using them, as well as a cured product thereof, which are suitably used as insulating materials in the electrical and electronic fields such as printed wiring boards and semiconductor encapsulation. [Background technology]
[0002] In recent years, with the progress of advanced materials, there is a demand for the development of base resins with higher performance. For example, in the field of semiconductor encapsulation, the problem of package cracks has become more serious due to the recent trend of thinner and larger packages for high-density packaging, and the spread of surface mounting methods, and these base resins are strongly required to have improved moisture resistance, heat resistance, adhesion to metal substrates, etc. Recently, in addition to the need for materials with high thermal decomposition stability and thermal conductivity from the perspective of improving heat resistance and heat dissipation, mainly in the power device field, materials with excellent dielectric properties are required from the perspective of high-speed communication.
[0003] However, among the conventionally known epoxy resins, none that satisfy these requirements have yet been known. For example, the well-known bisphenol type epoxy resin is liquid at room temperature, has excellent workability, and is easily mixed with curing agents, additives, etc., and is therefore widely used, but has problems with heat resistance and moisture resistance. In addition, phenol novolac type epoxy resins are known as those that have improved heat resistance, but have problems with moisture resistance and impact resistance. In addition, Patent Document 1 proposes an epoxy compound of a phenol aralkyl resin for the purpose of improving moisture resistance and impact resistance, but the heat resistance and flame retardancy are insufficient.
[0004] Patent Document 2 proposes an example in which an aralkyl-type epoxy resin having a biphenyl structure is applied to a semiconductor encapsulation material, but the heat resistance is insufficient. Patent Documents 3, 4, and 5 propose liquid crystal epoxy resins having rigid mesogen groups and epoxy resin compositions using the same, but there are problems with moldability and the effect of improving thermal conductivity is not sufficient.
[0005] Patent Document 6 discloses various epoxy resins having fluorine atoms, but none of them are sufficient for use as electrical insulating materials in terms of heat resistance, thermal conductivity, etc. Non-Patent Document 1 discloses a polymer having an aromatic ether structure containing fluorine atoms, but the disclosure is limited to a high molecular weight substance and does not relate to oligomers or epoxy resins using the same. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Publication No. 63-238122 [Patent Document 2] Japanese Patent Application Publication No. 11-140166 [Patent Document 3] Japanese Patent Application Publication No. 11-323162 [Patent Document 4] JP 2004-331811 A [Patent Document 5] Japanese Patent Application Publication No. 9-118673 [Patent Document 6] JP 2003-321409 A [Non-Patent Document 1] F. Schonberger,et.al.,Polymer,51,4299(2010) Summary of the Invention [Problem to be solved by the invention]
[0007] Accordingly, an object of the present invention is to provide a polyhydric hydroxy resin and an epoxy resin thereof which can give a cured product having excellent moldability as well as excellent heat resistance, high thermal conductivity, low dielectric properties, etc. and are useful for applications such as lamination, molding, casting, adhesion, etc., as well as methods for producing them, and an epoxy resin composition using them, and further, a cured product thereof. [Means for solving the problem]
[0008] That is, the present invention relates to a novel polyhydric hydroxy resin represented by the following general formula (1). [ka] (wherein, A independently represents a divalent aromatic group; n represents a repeating number of 1 to 10; m represents a number of 0 to 1; and p, q, x, and y independently represent the number of substitutions of 0 to 4; and either x or y is not 0.)
[0009] The present invention also provides a method for producing the polyhydric hydroxy resin of the above general formula (1), characterized in that 0.1 to 0.9 mol of an aromatic fluorine compound is reacted with 1 mol of an aromatic dihydroxy compound.
[0010] Furthermore, the present invention relates to a novel epoxy resin represented by the following general formula (3). [ka] (wherein, A independently represents a divalent aromatic group, G independently represents a glycidyl group, A and n independently represent a repeat number of 1 to 10, m independently represents a number of 0 to 1, and p, q, x, and y independently represent a substitution number of 0 to 4, and either x or y is not 0.)
[0011] Furthermore, the present invention relates to a method for producing a novel epoxy resin represented by the above general formula (3), which comprises reacting a polyhydric hydroxy resin represented by the above general formula (1) with epichlorohydrin.
[0012] Furthermore, the present invention relates to an epoxy resin composition comprising at least one of the above-mentioned epoxy resin and polyhydroxy resin as an essential component of an epoxy resin component or a curing agent component, and also to a cured product obtained by curing this epoxy resin composition. Effect of the Invention
[0013] The cured product obtained by curing the epoxy resin composition obtained from the epoxy resin or polyhydric hydroxy resin of the present invention has excellent heat resistance, low dielectric properties and moisture resistance, and can be suitably used for applications such as lamination, molding, casting, adhesion, etc. [Brief description of the drawings]
[0014] [Figure 1] 1 shows a GPC chart of the polyhydric hydroxy resin A obtained in Example 1. [Diagram 2] 1 shows a GPC chart of polyhydric hydroxy resin D obtained in Example 4. [Diagram 3] 1 shows an IR spectrum of polyhydric hydroxy resin D obtained in Example 4. [Figure 4] FD-MS spectrum of epoxy resin D obtained in Example 4 is shown. [Diagram 5] 1 shows an IR spectrum of epoxy resin A obtained in Example 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The present invention will be described in detail below. The polyhydric hydroxy resin of the present invention is represented by the above general formula (1). Here, A independently represents a divalent aromatic group. The divalent aromatic group is a benzene ring, a naphthalene ring, or a ring represented by the following formula (2): [ka] (X is a single bond, oxygen atom, sulfur atom, -SO 2 -, -CO-, -CH 2 -, -CH(CH3 )-, -C(CH 3 ) 2 -, -CH(φ)-, -Cφ(CH 3 )-, 1,1-cycloalkane group, and 9,9-fluorenyl group. Here, φ represents a phenylene group. R 1 , R 2 each independently represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, an aryl group, an alkoxy group, an aralkyl group, or a halogen atom, and n represents a number from 1 to 50. Examples of the bisphenylene group include those represented by the following formula: Preferred are unsubstituted or methyl-substituted benzene rings, naphthalene rings, and biphenyl rings. n represents the average number of repetitions and is from 1 to 50, preferably from 1 to 10. If it is smaller than this, the effect of low dielectric property etc. due to the introduction of fluorine atoms is small, and if it is larger than this, the viscosity becomes difficult to handle. m represents a number from 0 to 2, and is preferably 0 or 1. If it is greater than this, the viscosity increases and handling becomes difficult. Furthermore, p, q, x, and y each independently represent the number of substitutions of 0 to 4. Either x or y is not 0, and each is preferably 1 or more, more preferably 2 to 4. Desirably, p+x=4 and q+y=4 are satisfied, and desirably, p and q are independently 0 or 1.
[0016] The polyhydric hydroxy resin of the present invention may be a single compound or a mixture of compounds satisfying formula (1), in which case it is desirable that the mixture contains 50 wt % or more of compounds in which p=q=0 and x=y=4. According to GPC analysis, the content of unreacted aromatic dihydroxy compound is preferably 70 area % or less, n=1 isomer is 10 to 50 area %, n=2 isomer is 10 to 40 area %, and n=3 or more isomer is 50 area % or less.
[0017] The polyhydric hydroxy resin of the present invention preferably has a hydroxyl equivalent of 150 to 1500 g / eq. and a melting point of 130 to 300°C.
[0018] The polyhydric hydroxy resin of the present invention is obtained by reacting an aromatic dihydroxy compound with an aromatic fluorine compound. Here, the aromatic dihydroxy compound is a dihydric dihydroxybenzene or dihydroxynaphthalene having 1 to 6 carbon atoms and having or without an alkyl group, or a dihydric dihydroxybenzene or dihydroxynaphthalene having the following formula (4): [ka] (However, X, R 1 and R 2 has the same meaning as in general formula (2). Specifically, examples of dihydroxybenzenes include hydroquinone, 2,5-dimethylhydroquinone, 2,3,5-trimethylhydroquinone, resorcinol, and catechol, and examples of dihydroxynaphthalenes include 1,4-naphthalenediol, 1,5-naphthalenediol, 1,6-naphthalenediol, 1,7-naphthalenediol, 2,6-naphthalenediol, and 2,7-naphthalenediol. Examples of bisphenol compounds include bisphenol A, bisphenol F, 3,3',5,5'-tetramethyl-4,4'-dihydroxydiphenylmethane, 4,4'-dihydroxybiphenyl, 3,3',5,5'-tetramethyl-4,4'-dihydroxybiphenyl, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxybenzophenone, 4,4'-dihydroxydiphenyl sulfone, 4,4'-dihydroxydiphenyl sulfide, and fluorene bisphenol.
[0019] Regarding the substitution position of the dihydroxy group, the dihydroxybenzenes are preferably 1,4-dihydroxy or 1,3-dihydroxy, the dihydroxynaphthalenes are preferably 1,5-dihydroxy, 1,6-dihydroxy, 2,6-dihydroxy or 2,7-dihydroxy, and the bisphenol compounds are preferably 4,4'-dihydroxy. In the aromatic dihydroxy compound used, it is preferable that these dihydroxy substitutions account for 50 mol % or more.
[0020] Among these aromatic dihydroxy compounds, dihydroxybenzenes, dihydroxynaphthalenes, and dihydroxybiphenyls are preferred from the viewpoints of heat resistance, thermal conductivity, mechanical strength, etc. The above aromatic dihydroxy compounds may be used alone or in combination of two or more kinds.
[0021] The aromatic fluorine compound may be represented by the following general formula (5): [ka] (wherein m is a number from 0 to 1, and r and s are independently a number from 0 to 4.) Of these, hexafluorobenzene or decafluorobiphenyl is preferred.
[0022] In the reaction between an aromatic dihydroxy compound and an aromatic fluorine compound, an excess amount of the aromatic dihydroxy compound is used relative to the aromatic fluorine compound. The amount of the aromatic fluorine compound used is in the range of 0.1 to 0.9 moles relative to 1 mole of the aromatic dihydroxy compound, and preferably in the range of 0.1 to 0.6 moles. If it is more than this, the softening point of the resin increases, hindering molding workability. Furthermore, gelation may occur. If it is less than this, the amount of the aromatic dihydroxy compound used in excess after the reaction is completed increases. The remaining excess amount of the aromatic dihydroxy compound can be used as it is as a raw material or curing agent for epoxy resin without being removed, but the content of the resin of general formula (1) or (3) decreases, so the effect of improving properties such as heat resistance, low dielectric property, and low water absorption is reduced.
[0023] This reaction is preferably carried out in the presence of a basic catalyst, and at least one compound selected from the group consisting of a tertiary amine compound, a quaternary ammonium compound, an imidazole compound, a tertiary phosphine compound, a quaternary phosphonium compound, an alkali metal hydroxide compound, an alkaline earth metal hydroxide compound, an alkali metal carbonate, and an alkali metal hydrogen carbonate can be used.
[0024] Examples of the tertiary amine compound include triethylamine, tri-n-propylamine, triisopropylamine, tri-n-butylamine, tri-sec-butylamine, tri-n-hexylamine, dimethylbenzylamine, diethylbenzylamine, tribenzylamine, and 1,8-diazabicyclo[5.4.0]undec-7-ene.
[0025] Examples of the quaternary ammonium compound include quaternary ammonium hydroxide compounds such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetra-n-propylammonium hydroxide, tetra-n-butylammonium hydroxide, trimethylbenzylammonium hydroxide, and triethylbenzylammonium hydroxide; quaternary ammonium chloride compounds such as tetramethylammonium chloride, tetraethylammonium chloride, tetra-n-propylammonium chloride, tetra-n-butylammonium chloride, trimethylbenzylammonium chloride, and triethylbenzylammonium chloride; quaternary ammonium bromide compounds such as tetramethylammonium bromide, tetraethylammonium bromide, tetra-n-propylammonium bromide, tetra-n-butylammonium bromide, trimethylbenzylammonium bromide, and triethylbenzylammonium bromide; and quaternary ammonium iodide compounds such as tetramethylammonium iodide, tetraethylammonium iodide, tetra-n-propylammonium iodide, tetra-n-butylammonium iodide, trimethylbenzylammonium iodide, and triethylbenzylammonium iodide.
[0026] Examples of the imidazole compound include 2-methylimidazole, 2-ethylimidazole, 2-phenylimidazole, 2-ethyl-4-methylimidazole, 1-(2',4',6'-trimethylbenzoyl)-2-ethylimidazole, 1-(2',6'-dichlorobenzoyl)-2-methylimidazole, 1-(2',4',6'-trimethylbenzoyl)-2-methylimidazole, and 1-(2',4',6'-trimethylbenzoyl)-2-phenylimidazole.
[0027] Examples of the tertiary phosphine compound include triethylphosphine, tri-n-butylphosphine, triphenylphosphine, trinonylphenylphosphine, etc. Examples of the quaternary phosphonium compound include quaternary phosphonium hydroxide compounds such as tetramethylphosphonium hydroxide, quaternary phosphonium halogenide compounds such as tetramethylphosphonium chloride, tetra-n-butylphosphonium chloride, tetraphenylphosphonium chloride, tetra-n-butylphosphonium bromide, methyltriphenylphosphonium bromide, n-butyltriphenylphosphonium bromide, methyltriphenylphosphonium bromide, and ethyltriphenylphosphonium bromide, and quaternary phosphonium acetate compounds such as ethyltriphenylphosphonium acetate.
[0028] Examples of the alkali metal hydroxide compounds include lithium hydroxide, sodium hydroxide, potassium hydroxide, etc. Examples of the alkaline earth metal hydroxide compounds include magnesium hydroxide, calcium hydroxide, barium hydroxide, etc.
[0029] Examples of the alkali metal carbonate include lithium carbonate, sodium carbonate, and potassium carbonate, and examples of the alkali metal hydrogen carbonate include lithium hydrogen carbonate, sodium hydrogen carbonate, and potassium hydrogen carbonate.
[0030] These basic catalysts may be used alone or may be dissolved in water or a solvent in advance and then added to the reaction system. The proportion of the basic catalyst used is usually 0.001 to 10 mol %, preferably 0.05 to 5 mol %, per mol of the phenolic hydroxyl group of the aromatic dihydroxy compound.
[0031] This reaction is usually carried out for 1 to 20 hours at 10 to 250° C. Furthermore, as a reaction solvent, alcohols such as methanol, ethanol, propanol, butanol, ethylene glycol, methyl cellosolve, and ethyl cellosolve, benzene, toluene, chlorobenzene, and dichlorobenzene can be used.
[0032] After the reaction is completed, the catalyst is removed by neutralization, washing with water, etc., and the remaining solvent is removed from the system as necessary by washing with water, distillation under reduced pressure, etc. to obtain a hydroxy resin. Unreacted aromatic dihydroxy compound may or may not be removed from the system by washing with water, distillation under reduced pressure, etc.
[0033] In the epoxy resin of the present invention, the phenolic hydroxyl group of the polyhydric hydroxyl resin is replaced with a glycidyl group, and the molecular weight distribution of the epoxy resin almost reflects the molecular weight distribution of the polyhydric hydroxyl resin. The epoxy resin of the present invention preferably has an epoxy equivalent of 170 to 2000 g / eq., more preferably 180 to 500 g / eq., and has a hydrolyzable chlorine content of 500 ppm or less.
[0034] The epoxy resin of the present invention can be obtained by reacting the polyhydric hydroxy resin represented by the above general formula (1) with epichlorohydrin. This reaction can be carried out in the same manner as in a conventional epoxidation reaction.
[0035] For example, the polyhydric hydroxy resin represented by the above general formula (1) is dissolved in excess epichlorohydrin, and then reacted in the presence of an alkali metal hydroxide such as sodium hydroxide or potassium hydroxide at 50 to 150°C, preferably 60 to 120°C, for 1 to 10 hours. In this case, the amount of the alkali metal hydroxide used is 0.8 to 2 moles, preferably 0.9 to 1.2 moles, per mole of hydroxyl groups in the polyhydric hydroxy resin. In addition, epichlorohydrin is used in excess relative to the hydroxyl groups in the polyhydric hydroxy resin, and is usually 1.5 to 15 moles, preferably 2 to 8 moles, per mole of hydroxyl groups in the polyhydric hydroxy resin. In addition, a quaternary ammonium salt or the like can be added during the reaction. Examples of the quaternary ammonium salt include tetramethylammonium chloride, tetrabutylammonium chloride, and benzyltriethylammonium chloride, and the amount added is preferably 0.1 to 2.0 wt% relative to the polyhydric hydroxy resin. If the amount is less than this, the effect of the addition of the quaternary ammonium salt is small, and if the amount is more than this, the generation of hardly hydrolyzable chlorine increases, making it difficult to achieve high purification. Furthermore, a polar solvent such as dimethyl sulfoxide or diglyme may be used, and the amount added is preferably in the range of 10 to 200 wt% relative to the polyhydric hydroxy resin. If the amount is less than this, the effect of the addition is small, and if the amount is more than this, the volume efficiency decreases and is not economically preferable. After the reaction is completed, the excess epichlorohydrin is distilled off, and the residue is dissolved in a solvent such as toluene or methyl isobutyl ketone, filtered, washed with water to remove inorganic salts, and then the solvent is distilled off to obtain the desired epoxy resin. This epoxy resin is mainly composed of a substance represented by general formula (3), but may also contain a glycidyl etherified product of a compound in which one or more naphthylmethane groups are added to the aromatic ring of the novel polyhydric hydroxy resin of general formula (1). Furthermore, it may also contain a product in which the epoxy group in the epoxy resin of the present invention is oligomerized as an ether bond.
[0036] The epoxy resin composition of the present invention comprises an epoxy resin and a curing agent, and contains, as an essential component, at least one of an epoxy resin represented by general formula (3) as an epoxy resin component and a polyhydric hydroxyl resin represented by the above general formula (1) as a curing agent component. An epoxy resin represented by the general formula (3) may be blended as the epoxy resin component, and a polyhydric hydroxy resin represented by the general formula (1) may be blended as the curing agent component.
[0037] As a curing agent when the epoxy resin represented by the general formula (3) is used as an essential component, any curing agent generally known as an epoxy resin curing agent can be used. For example, dicyandiamide, polyhydric phenols, acid anhydrides, aromatic and aliphatic amines, etc. are available. Specific examples of polyhydric phenols include dihydric phenols such as bisphenol A, bisphenol F, bisphenol S, fluorene bisphenol, 4,4'-biphenol, 2,2'-biphenol, hydroquinone, resorcin, and naphthalenediol, and trihydric or higher phenols such as tris-(4-hydroxyphenyl)methane, 1,1,2,2-tetrakis(4-hydroxyphenyl)ethane, phenol novolac, o-cresol novolac, naphthol novolac, and polyvinylphenol, and further phenols, naphthols, or bisphenol A, bisphenol 2, bisphenol 1, bisphenol 2, bisphenol 1, bisphenol 2, bisphenol 1, bisphenol 2, bisphenol 1, bisphenol 2, bisphenol 3, bisphenol 4, bisphenol 5, bisphenol 6, bisphenol 7, bisphenol 8, bisphenol 9, bisphenol 10, bisphenol 11, bisphenol 12, bisphenol 13, bisphenol 14, bisphenol 15, bisphenol 16, bisphenol 17, bisphenol 18, bisphenol 19, bisphenol 20, bisphenol 21, bisphenol 22, bisphenol 23, bisphenol 24, bisphenol 25, bisphenol 26, bisphenol 27, bisphenol 28, bisphenol 29, bisphenol 30, bisphenol 31, bisphenol 32, bisphenol 33, bisphenol Examples of the polyhydric phenol compounds include those synthesized by condensing dihydric phenols such as phenol F, bisphenol S, fluorene bisphenol, 4,4'-biphenol, 2,2'-biphenol, hydroquinone, resorcin, and naphthalenediol with condensing agents such as formaldehyde, acetaldehyde, benzaldehyde, p-hydroxybenzaldehyde, and p-xylylene glycol. Examples of the acid anhydrides include phthalic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylhimic anhydride, nadic anhydride, and trimellitic anhydride. Examples of amines include aromatic amines such as 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylpropane, 4,4'-diaminodiphenylsulfone, m-phenylenediamine, and p-xylylenediamine, aliphatic amines such as ethylenediamine, hexamethylenediamine, diethylenetriamine, and triethylenetetramine, and polyhydric hydroxyl resins represented by the general formula (1). The resin composition of the present invention can use one or more of these curing agents in combination. In this case, the blending amount of the epoxy resin of the present invention is preferably in the range of 5 to 100 wt %, more preferably in the range of 50 to 100 wt %, and further preferably in the range of 80 to 100 wt %, of the total epoxy resin.
[0038] When the polyhydric hydroxyl resin represented by the general formula (1) is used as an essential component of the curing agent component, any ordinary epoxy resin having two or more epoxy groups in the molecule can be used as the epoxy resin. Examples include divalent phenols such as bisphenol A, bisphenol S, fluorene bisphenol, 4,4'-biphenol, 2,2'-biphenol, hydroquinone, and resorcin, or trivalent or higher phenols such as tris-(4-hydroxyphenyl)methane, 1,1,2,2-tetrakis(4-hydroxyphenyl)ethane, phenol novolac, and o-cresol novolac, or glycidyl ethers derived from halogenated bisphenols such as tetrabromobisphenol A, or polyfunctional epoxy resins represented by the general formula (1). These epoxy resins can be used alone or in a mixture of two or more. In this case, the blending amount of the polyhydric hydroxy resin of the present invention is preferably in the range of 5 to 100 wt %, more preferably in the range of 50 to 100 wt %, and further preferably in the range of 80 to 100 wt % based on the total weight of the curing agent.
[0039] In addition, in the epoxy resin composition of the present invention, which contains either or both of the epoxy resin represented by the general formula (3) and the polyhydric hydroxyl resin represented by the general formula (1) as essential components, oligomers or polymer compounds such as polyesters, polyamides, polyimides, polyethers, polyurethanes, petroleum resins, indene coumarone resins, and phenoxy resins may be appropriately blended, and additives such as inorganic fillers, pigments, flame retardants, thixotropy imparting agents, coupling agents, and flowability improvers may also be blended. Examples of inorganic fillers include spherical or crushed fused silica, silica powder such as crystalline silica, alumina powder, glass powder, mica, talc, calcium carbonate, alumina, hydrated alumina, and the like, and examples of pigments include organic or inorganic extender pigments, scaly pigments, and the like. Examples of thixotropy imparting agents include silicone-based, castor oil-based, aliphatic amide wax, oxidized polyethylene wax, and organic bentonite-based agents. Furthermore, if necessary, a conventionally known curing accelerator can be used. Examples include amines, imidazoles, organic phosphines, Lewis acids, etc. The amount of addition is usually in the range of 0.2 to 5 parts by weight per 100 parts by weight of the epoxy resin. Furthermore, if necessary, the resin composition of the present invention may further contain a release agent such as carnauba wax or OP wax, a coupling agent such as γ-glycidoxypropyltrimethoxysilane, a colorant such as carbon black, a flame retardant such as antimony trioxide, a stress reducing agent such as silicone oil, a lubricant such as calcium stearate, etc.
[0040] The cured product of the present invention can be obtained by molding the above-mentioned epoxy resin composition by a method such as casting, compression molding, transfer molding, etc. The temperature during molding is usually in the range of 120 to 220°C. EXAMPLES
[0041] The present invention will be specifically described below based on examples and comparative examples. Example 1 (Production of Polyhydric Hydroxy Resin A) In a 1L 4-neck separable flask, 90.2 g of 4,4'-dihydroxybiphenyl was dissolved in 360 g of N-methylpyrrolidone (NMP), and then 19.9 g of potassium carbonate was added and the mixture was heated to 50°C while stirring under a nitrogen stream. Then, 40.9 g of decafluorobiphenyl (DFBP) was added and reacted at 60°C for 2 hours. After neutralizing the reaction liquid with 17.3 g of acetic acid, it was poured into a large amount of water and the precipitate was collected by filtration. After washing with water and drying, 96 g of powdered polyhydric hydroxy resin was obtained (polyhydric hydroxy resin A). The hydroxyl equivalent of the obtained hydroxyl resin A was 136g / eq., and the melting point was 269℃. The GPC chart is shown in Figure 1. The unreacted 4,4'-dihydroxybiphenyl accounted for 52.6%, the compound represented by formula (1) with n=1, m=1, p=q=0, x=y=4 accounted for 30.3%, the compound represented by n=2, m=1, p=q=0, x=y=4 accounted for 14.0%, and the compound represented by n=3, m=1, p=q=0, x=y=4 accounted for 1.5%. The melt viscosity was measured using a Brookfield CAP2000H, and the GPC measurement was performed using an apparatus: HLC-8320 (Tosoh Corporation) and columns: 2 TSKgel SuperHZ2500 and 2 TSKgel SuperHZ2000 (both manufactured by Tosoh Corporation) under the following conditions: solvent: tetrahydrofuran, flow rate: 0.35 ml / min, temperature: 40°C, and detector: RI.
[0042] Example 2 (Production of Polyhydric Hydroxy Resin B) In a 1L 4-necked separable flask, 93.2 g of 3,3',5,5'-tetramethyl-4,4'-dihydroxydiphenylmethane (TMBPF) was dissolved in 360 g of NMP, and then 19.9 g of potassium carbonate was added and the temperature was raised to 50°C while stirring under a nitrogen stream. Then, 40.9 g of DFBP was added and reacted at 60°C for 2 hours. After neutralizing the reaction liquid with 17.3 g of acetic acid, it was poured into a large amount of water and the precipitate was collected by filtration. After washing with water and drying, 60 g of powdered polyhydric hydroxy resin was obtained (polyhydric hydroxy resin B). The resulting hydroxyl resin C had a hydroxyl equivalent of 290 g / eq. and a melting point of 157°C. As a result of GPC measurement, the unreacted TMBPF was 39.9%, the compounds of formula (1) with n=1, m=1, p=q=0, x=y=4 were 26.0%, the compounds of n=2, m=1, p=q=0, x=y=4 were 16.5%, the compounds of n=3, m=1, p=q=0, x=y=4 were 9.0%, the compounds of n=4, m=1, p=q=0, x=y=4 were 4.6%, the compounds of n=5, m=1, p=q=0, x=y=4 were 2.2%, the compounds of n=6, m=1, p=q=0, x=y=4 were 1.1%, the compounds of n=7, m=1, p=q=0, x=y=4 were 0.5%, and the compounds of n=8, m=1, p=q=0, x=y=4 were 0.2%.
[0043] Example 3 (Production of Polyhydric Hydroxy Resin C) In a 1L 4-neck separable flask, 137.8 g of TMBPF was dissolved in 280 g of NMP, and then 55.1 g of potassium carbonate was added and the mixture was heated to 50°C while stirring under a nitrogen stream. Then, 25.0 g of hexafluorobenzene (HFBZ) was added and reacted at 55°C for 8 hours. After neutralizing the reaction liquid with 47.9 g of acetic acid, it was poured into a large amount of water and the precipitate was collected by filtration. After washing with water and drying, 142 g of powdered polyhydric hydroxyl resin was obtained (polyhydric hydroxyl resin C). The hydroxyl equivalent of the obtained hydroxyl resin C was 172 g / eq., and the melting point was 170° C. GPC analysis showed that the unreacted TMBPF was 69.5%, that of formula (1) where n=1, m=0, p=0, x=4 was 22.1%, that of n=2, m=0, p=0, x=4 was 6.0%, and that of n=3, m=0, p=0, x=4 was 1.4%.
[0044] Example 4 (Production of Polyhydric Hydroxy Resin D) In a 1L 4-neck separable flask, 49.5 g of 3,3',5,5'-tetramethyl-4,4'-dihydroxybiphenyl (TMBP) was dissolved in 250 g of NMP, and then 20.7 g of potassium carbonate was added and the mixture was heated to 120°C while stirring under a nitrogen stream. Then, 17.0 g of DFBP was added, the mixture was heated to 140°C, and reacted for 2 hours. After neutralizing the reaction liquid with 18.0 g of acetic acid, the mixture was poured into a large amount of water, and the precipitate was collected by filtration. After washing with water and drying, 42 g of powdered polyhydric hydroxy resin was obtained (polyhydric hydroxy resin CD). The resulting polyhydric hydroxyl resin B had a melting point of 255° C. and a hydroxyl equivalent of 392 g / eq. The content of unreacted TMBP was 4.1%. The GPC chart is shown in Figure 2, the infrared absorption spectrum in Figure 3, and the field desorption ionization mass spectrometry (FD-MS) spectrum in Figure 4. The infrared absorption spectrum was measured by the KBr pellet method using a Hitachi 270-50 infrared absorption analyzer. The FD-MS spectrum was measured in the range of m / Z = 100 to 1600 using a JEOL JMS-AX505HA mass spectrometer.
[0045] Example 5 (Production of Epoxy Resin A) 30 g of the polyhydric hydroxyl resin A obtained in Example 1 was dissolved in 300 g of epichlorohydrin (ECH) and 60 g of diglyme, and 21.6 g of 48.8% aqueous sodium hydroxide solution was added dropwise at 60°C under reduced pressure (about 100 mmHg) over 4 hours. During this time, the water generated was removed from the system by azeotropy with ECH, and the distilled ECH was returned to the system. After the dropwise addition was completed, the reaction was continued for another 1 hour. Then, ECH and diglyme were distilled off under reduced pressure, and the mixture was dissolved in 120 mL of toluene, and the salt generated was removed by filtration. After washing with water, the toluene was distilled off under reduced pressure to obtain 20 g of white powdery epoxy resin (epoxy resin A). DSC measurement of the obtained epoxy resin A showed peaks at 125℃ and 154℃ corresponding to the melting point. The infrared absorption spectrum is shown in Figure 5. The epoxy equivalent was 194g / eq. and the hydrolyzable chlorine was 350ppm. The hydrolyzable chlorine was determined by dissolving 0.5g of the resin sample in 30ml of 1,4-dioxane, boiling and refluxing it in 5ml of 1N-KOH / methanol solution for 30 minutes, and then performing potentiometric titration with silver nitrate solution.
[0046] Example 6 (Production of Epoxy Resin B) 30 g of the polyhydric hydroxy resin B obtained in Example 2 was dissolved in 200 g of ECH and 30 g of diglyme, and 9.4 g of 48.8% aqueous sodium hydroxide solution was added dropwise at 60°C under reduced pressure (about 100 mmHg) over 4 hours. During this time, the water generated was removed from the system by azeotropy with ECH, and the distilled ECH was returned to the system. After the dropwise addition was completed, the reaction was continued for another 1 hour. Then, ECH and diglyme were distilled off under reduced pressure, and the mixture was dissolved in 120 mL of toluene, and the salt generated was removed by filtration. After washing with water, the toluene was distilled off under reduced pressure to obtain 32 g of an epoxy resin that was slightly viscous at room temperature (epoxy resin B). The epoxy equivalent was 329 g / eq., the melt viscosity at 150°C was 0.05 Pa·s, and the hydrolyzable chlorine content was 80 ppm.
[0047] Example 7 (Production of Epoxy Resin C) 50g of polyhydric hydroxy resin C obtained in Example 3 was dissolved in 400g of ECH and 60g of diglyme, and 26.3g of 48.8% aqueous sodium hydroxide solution was added dropwise at 60℃ under reduced pressure (about 100mmHg) over 4 hours. During this time, the water generated was removed from the system by azeotropy with ECH, and the distilled ECH was returned to the system. After the dropwise addition was completed, the reaction was continued for another hour. Then, ECH and diglyme were distilled off under reduced pressure, and the mixture was dissolved in 200mL of toluene, and the salt generated was removed by filtration. After washing with water, the toluene was distilled off under reduced pressure to obtain 32g of epoxy resin (epoxy resin C) which was viscous at room temperature. The epoxy equivalent was 219g / eq., the melt viscosity at 150℃ was 0.01Pa·s, and the hydrolyzable chlorine was 30ppm.
[0048] Examples 8 to 11 and Comparative Example 1 The polyhydric hydroxy resins or epoxy resins synthesized in Examples 1 to 7, biphenyl-based epoxy resin (epoxy resin D: Mitsubishi Chemical, YX-4000H, epoxy equivalent 193, melting point 105°C), and phenol novolak (polyhydric hydroxy resin E; OH equivalent 104, softening point 83°C, melt viscosity at 150°C 0.3 Pa s; BRG-557, Aica Corporation) were used, and triphenylphosphine was used as a curing accelerator to prepare resin compositions according to the formulation shown in Table 1. This was used for molding (150°C, 5 minutes), and then post-cured (175°C, 4 hours) to obtain test pieces, which were then subjected to various physical property tests. The test methods are as follows. The glass transition point and thermal expansion coefficient were determined using a Hitachi High-Tech Science Corporation TMA7100 type thermomechanical measuring device at a heating rate of 10°C / min. The thermal decomposition temperature and carbon residue ratio were determined using a Hitachi High-Tech Science Corporation TG / DTA7300 type thermogravimetric measuring device at a heating rate of 10°C / min under a nitrogen gas flow, at the time of a 5 wt% weight loss, and at 700°C. The water absorption rate was determined as the weight change rate when a test piece with a diameter of 50 mm and a thickness of 3 mm was allowed to absorb moisture for 100 hours after post-curing at 85°C and 85% RH. The results are shown in Table 1.
[0049] [Table 1]
Claims
1. The following general formula (1): 【Chemistry 1】 (wherein A independently represents a divalent aromatic group; n represents a repeating number of 1 to 10; m represents a number of 0 to 1; and p, q, x, and y independently represent the number of substitutions of 0 to 4; and neither x nor y is 0), A in the general formula (1) is a benzene ring, a naphthalene ring, or a ring represented by the following formula (2): 【Chemistry 2】 (wherein X represents a single bond, -SO 2 -, -CO-, -CH 2 -, -CH(CH 3 )-, -C(CH 3 ) 2 -, -CH(φ)-, -Cφ(CH 3 )-, or a 1,1-cycloalkane group, in which φ represents a phenylene group; R 1 and R 2 each independently represent a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, an aryl group, an alkoxy group, an aralkyl group, or a halogen atom; and n represents a number from 1 to 50.) A polyhydric hydroxyl resin characterized in that
2. 2. The polyhydric hydroxy resin according to claim 1, which is a resin mixture containing 30 to 95 wt % of the component represented by general formula (1) where n=1, p=q=0, and x=y=4.
3. 2. The method for producing a polyhydric hydroxy resin according to claim 1, wherein 0.1 to 0.9 moles of an aromatic fluorine compound are reacted with 1 mole of an aromatic dihydroxy compound.
4. The following general formula (3): 【Chemistry 3】 (wherein A independently represents a divalent aromatic group, G represents a glycidyl group, n represents a repeating number of 1 to 10, m represents a number of 0 to 1, and p, q, x, and y independently represent the number of substitutions of 0 to 4, and either x or y is not 0).
5. 5. The method for producing an epoxy resin according to claim 4, which comprises reacting the polyhydric hydroxy resin according to claim 1 with epichlorohydrin.
6. 10. An epoxy resin composition comprising an epoxy resin and a curing agent, comprising at least one of the polyhydric hydroxy resin according to claim 1 and the epoxy resin according to claim 4 as an essential component.
7. A cured product obtained by curing the epoxy resin composition according to claim 6.
Citation Information
Patent Citations
Epoxy resin and production thereof
JP1988238122A
Liquid crystal epoxy monomer and liquid crystal epoxy resin
JP1997118673A
Organic insulation film material and its production
JP1998087816A
Epoxy resin composition for semiconductor sealing and semiconductor device
JP1999140166A
Insulation composition
JP1999323162A