Resin composition

A combination of polycarbonate and acrylic resins with specific structural features addresses the need for a balanced resin composition, achieving high transparency and hardness with low photoelasticity without melt-kneading, suitable for optical applications.

JP7572236B2Active Publication Date: 2024-10-23NIPPON SHOKUBAI CO LTD

Patent Information

Application Number
JP2020218023
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-25
Publication Date
2024-10-23
Estimated Expiration
2040-12-25

AI Technical Summary

Technical Problem

Existing polycarbonate and acrylic resins, while having excellent properties, lack a composition that balances transparency, hardness, heat resistance, and optical properties effectively.

Method used

A novel resin composition combining a polycarbonate resin with an alicyclic skeleton and an acrylic resin having a ring structure, with a refractive index difference of 0.030 or less, allowing for high transparency and low coloration without melt-kneading.

Benefits of technology

The composition achieves high transparency, low coloration, and excellent physical properties such as surface hardness and low photoelasticity, enabling the production of molded articles with balanced performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572236000001
    Figure 0007572236000001
  • Figure 0007572236000002
    Figure 0007572236000002
  • Figure 0007572236000003
    Figure 0007572236000003
Patent Text Reader

Abstract

To provide a novel resin composition capable of forming a molding having excellent transparency, hardness, thermostability, optical properties or the like.SOLUTION: The inventive composition is (i) or (ii) described below: (i) a composition that contains a polycarbonate resin (A) containing a polycarbonate resin (A1) having an alicyclic skeleton and an acrylic resin (B) having a ring structure; and (ii) a composition that contains a polycarbonate resin (A) and an acrylic resin (B) having a ring structure, wherein the absolute value of difference between the refractive index RA of the polycarbonate resin (A) (wavelength 589 nm) and the refractive index RB of the acrylic resin (B) (wavelength 589 nm) is 0.030 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a novel composition (resin composition) and the like. [Background technology]

[0002] Polycarbonate resin is a resin that is excellent in, for example, high temperature stability, dimensional stability, impact resistance, rigidity, transparency, and the like. On the other hand, acrylic resins, such as polymethyl methacrylate (PMMA), are used as optical materials because of their high transparency. Among these acrylic resins, acrylic polymers having a ring structure in the main chain are being developed because of their heat resistance. For example, Patent Document 1 discloses a copolymer having methyl (meth)acrylate units, methacrylic acid units, and glutaric anhydride units. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2017 / 022393 Brochure Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to provide a novel composition (resin composition) and the like. [Means for solving the problem]

[0005] As described above, polycarbonate resins and acrylic resins each have excellent physical properties (characteristics), but further novel resins (resin materials) are desired.

[0006] In this situation, the present inventors have discovered that a novel resin material (resin composition) can be obtained by combining a specific polycarbonate resin with a specific acrylic resin, and that such a combination of resins can produce a resin material (a molded article) that is excellent or well-balanced in physical properties such as transparency, hardness, heat resistance, and optical properties (low photoelastic coefficient, low retardation expression), and have completed the present invention.

[0007] That is, the present invention relates to the following inventions, etc. [1] A composition comprising a polycarbonate resin (A) containing a polycarbonate resin (A1) having an alicyclic skeleton, and an acrylic resin (B) having a ring structure. [2] A composition containing a polycarbonate resin (A) and an acrylic resin (B) having a ring structure, the refractive index (wavelength 589 nm) of the polycarbonate resin (A) is R A and the refractive index of acrylic resin (B) (wavelength 589 nm) R B The absolute value of the difference between the above and the above formula is 0.030 or less. [3] The composition according to [2], wherein the polycarbonate resin (A) contains a polycarbonate resin (A1) having an alicyclic skeleton. [4] The composition according to [1] or [3], wherein the polycarbonate resin (A1) has a structural unit derived from an alicyclic dihydroxy compound. [5] The composition according to [1], [3] or [4], wherein the polycarbonate resin (A1) has a structural unit derived from an alicyclic dihydroxy compound represented by the following formula (X): [ka] [6] The composition according to any one of [1] to [5], wherein the proportion of the polycarbonate resin (A1) having an alicyclic skeleton in the entire polycarbonate resin (A) is 30 mass % or more. [7] The composition according to any one of [1] to [6], wherein the polycarbonate resin (A) has a refractive index (at a wavelength of 589 nm) of 1.540 or less. [8] The composition according to any one of [1] to [7], wherein the polycarbonate resin (A) has a glass transition temperature of 90 to 140° C. or a melt flow rate of 5 to 25 g / 10 min at 230° C. under a load of 3.8 kg. [9] The composition according to any one of [1] to [8], wherein the acrylic resin (B) has at least one ring structure selected from a cyclic imide structure, a cyclic amide structure, and a cyclic ester structure.

[10] The composition according to any one of [1] to [9], wherein the acrylic resin (B) has a cyclic ester structure (lactone ring structure).

[11] The composition according to any one of [1] to

[10] , wherein the acrylic resin (B) has a glass transition temperature of 115° C. or higher.

[12] The composition according to any one of [1] to

[11] , wherein the acrylic resin (B) has a melt flow rate of 0.5 to 8 g / 10 min at 230° C. under a load of 3.8 kg, and a weight average molecular weight of 50,000 to 200,000.

[13] The composition according to any one of [1] to

[12] , wherein the acrylic resin (B) has a refractive index (at a wavelength of 589 nm) of 1.492 to 1.510.

[14] The composition according to any one of [1] to

[13] , wherein a mass ratio of the polycarbonate resin (A) to the acrylic resin (B) is 30 / 70 to 97 / 3.

[15] the polycarbonate resin (A) has a refractive index (at a wavelength of 589 nm) of 1.520 or less and contains a polycarbonate resin (A1) having an alicyclic skeleton in a proportion of 30% by mass or more; The acrylic resin (B) has a refractive index (wavelength 589 nm) of 1.494 or more and a glass transition temperature of 120° C. or more, Refractive index of polycarbonate resin (A) (wavelength 589 nm) R A and the refractive index of acrylic resin (B) (wavelength 589 nm) RB The absolute value of the difference between is 0.020 or less, The composition according to any one of [1] to

[14] , wherein a mass ratio of the polycarbonate resin (A) to the acrylic resin (B) is 40 / 60 to 95 / 5.

[16] The composition according to any one of [1] to

[15] , which is not melt-kneaded (for example, is a dry blend).

[17] A molded article comprising the composition according to any one of [1] to

[16] .

[18] The molded article according to

[17] , which is an optical component.

[19] Total light transmittance is 89% or more, haze is 20% or less, pencil hardness is H or more, and photoelastic coefficient is 26×10 -12 / Pa or less.

[20] A method for producing a molded article, comprising a step of molding (for example, melt molding) the composition according to any one of [1] to

[16] . [twenty one] The method according to

[20] , comprising mixing (e.g., dry blending) at least a polycarbonate resin (A) and an acrylic resin (B) having a ring structure without melting them to obtain a composition, and subjecting (using) this composition (e.g., a dry blend) to melt molding. Effect of the Invention

[0008] According to the present invention, a novel composition (resin composition) can be provided.

[0009] This composition is a novel composition containing a specific polycarbonate resin and a specific acrylic resin. Although this composition contains different resins, they are mutually highly dispersible, and therefore, not only can the composition (and even a molded product) be formed, but also high transparency and low colorability can be achieved.

[0010] In particular, in another embodiment of the composition of the present invention, a molded article (melt-molded article) can be produced that has such high transparency and low colorability (or does not impair it) and is also excellent in various physical properties (for example, has high surface hardness, low photoelastic coefficient, low retardation expression, etc.).

[0011] In particular, the composition (or a molded article thereof) according to such another embodiment can unexpectedly achieve both high surface hardness and excellent optical properties (low photoelastic coefficient, low retardation expression, etc.).

[0012] In another embodiment of the present invention, the above-mentioned molded article (e.g., a molded article having high transparency) can be provided without subjecting the resin composition to prior melt mixing (kneading). Although the reason for this is unclear, one possible factor is that in the present invention, by combining specific resins, a resin composition (and even a molded article thereof) can be formed even if the resins are not compatible with each other. By using such a resin composition, it is possible to provide a molded article that is advantageous in terms of lower colorability (and further transparency) and the like, possibly because the thermal history can be reduced as much as possible. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The composition (resin composition, and further molded article) of the present invention contains a polycarbonate resin (hereinafter, may be referred to as polycarbonate resin (A), resin (A), etc.) and an acrylic resin having a ring structure (hereinafter, may be referred to as acrylic resin having a ring structure (B), resin (B), etc.).

[0014] [Polycarbonate resin] Examples of polycarbonate resins (polycarbonate-based resins) include those having an aliphatic skeleton (alicyclic skeleton, non-alicyclic aliphatic skeleton), those having an aromatic skeleton, and those having a combination of these. Preferably, the polycarbonate resin has (at least) an aliphatic skeleton.

[0015] When combined with the resin (B) described below, such a polycarbonate resin having an aliphatic skeleton easily achieves the excellent physical properties described above in addition to high transparency and low coloration.

[0016] Furthermore, by incorporating an aliphatic skeleton, it is easy to efficiently reduce the refractive index of the polycarbonate resin (and further to reduce the refractive index difference with resin (B) described below), and thus it is easy to achieve the physical properties described above in combination with resin (B).

[0017] In particular, among aliphatic skeletons, alicyclic skeletons are particularly preferred in terms of balance of physical properties (e.g., heat resistance, strength, etc.), and therefore the polycarbonate resin may contain a polycarbonate resin having (at least) an alicyclic (alicyclic) skeleton (hereinafter, sometimes referred to as polycarbonate resin (A1)).

[0018] The polycarbonate resin (A) may be any resin having a carbonate bond, but may usually be a resin having at least a dihydroxy compound as a polymerization component (having a structural unit derived from a dihydroxy compound).

[0019] Examples of the dihydroxy compound include an aliphatic dihydroxy compound and an aromatic dihydroxy compound.

[0020] Examples of the aliphatic dihydroxy compound include alicyclic dihydroxy compounds [for example, alicyclic dihydroxy compounds having 70 or less carbon atoms (e.g., 50 or less, 30 or less, about 4 to 20 carbon atoms), alicyclic dihydroxy compounds having at least a 5-membered or 6-membered ring structure, alicyclic dihydroxy compounds having 70 or less carbon atoms (e.g., 50 or less, 30 or less, about 4 to 20 carbon atoms) and having at least a 5-membered or 6-membered ring structure, etc.], non-alicyclic (aliphatic) dihydroxy compounds, etc.

[0021] Examples of the alicyclic dihydroxy compound include cycloalkanediols {or dihydroxycycloalkanes, for example, mono(monocyclic)cycloalkanediols [for example, cyclohexanediols (e.g., 1,2-cyclohexanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, 2-methyl-1,4-cyclohexanediol) and the like C 4-10 (mono)cycloalkanediols), etc.], poly(polycyclic)cycloalkanediols or bridged cyclic cycloalkanediols [e.g., tricyclodecanediol, pentacyclopentadecanediol, decalindiol (or tricyclotetradecanediol, e.g., 2,6-decalindiol, 1,5-decalindiol, 2,3-decalindiol), norbornanediol (e.g., 2,3-norbornanediol, 2,5-norbornanediol), adamantanediol (e.g., 1,3-adamantanediol), etc.], etc.}, di(hydroxyalkyl)cycloalkanes {or cycloalkanedialkanols, for example, mono(monocyclic)cycloalkanedialkanols [e.g., cyclohexanedimethanols (e.g., 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol), etc. 4-10 (Mono)cycloalkane diC 1-4alkanols), etc.], poly(polycyclic) cycloalkane dialkanols or bridged cyclic cycloalkane dialkanols [for example, tricyclodecane dimethanol, pentacyclopentadecanedimethanol, decalin dimethanol (or tricyclotetradecane dimethanol, for example, 2,6-decalin dimethanol, 1,5-decalin dimethanol, 2,3-decalin dimethanol), norbornane dimethanol (for example, 2,3-norbornane dimethanol, 2,5-norbornane dimethanol), adamantane dimethanol (for example, 1,3-adamantanedimethanol), etc.], etc.}, heterocyclic aliphatic dihydroxy compounds {for example, heteromonocyclic aliphatic dihydroxy compounds (for example, tetrahydro furan-2,2-dimethanol, etc.), heteropolycyclic aliphatic dihydroxy compounds [for example, a compound represented by the following formula (X), a compound having an oxacyclospiroalkane skeleton (for example, 3,9-bis(2-hydroxyethyl)-2,4,8,10-tetraoxaspiro(5.5)undecane, 3,9-bis(2-hydroxy-1,1-dimethylethyl)-2,4,8,10-tetraoxaspiro(5.5)undecane, 3,9-bis(2-hydroxy-1,1-diethylethyl)-2,4,8,10-tetraoxaspiro(5.5)undecane, 3,9-bis(2-hydroxy-1,1-dipropylethyl)-2,4,8,10-tetraoxaspiro(5.5)undecane, etc.], etc.].

[0022] [ka]

[0023] Examples of the compound represented by the above formula (X) (compound (X)) include isosorbide, isomannide, isoidet, and the like. Compound (X) may be a mixture (mixture of isomers). Compound (X) may contain at least isosorbide.

[0024] Examples of non-alicyclic dihydroxy compounds include alkanediols (e.g., C 1,4-butylene diol, 1,3-butylene diol, 1,2-butylene diol, 1,5-butylene diol, 1,6-butylene diol, etc.) 2-20 Alkanediols), polyalkanediols (e.g., polyC such as diethylene glycol, triethylene glycol, and tetraethylene glycol) 2-6 Alkanediols) and the like.

[0025] The aliphatic dihydroxy compounds may be used alone or in combination of two or more kinds.

[0026] Examples of aromatic dihydroxy compounds include biphenols (e.g., 4,4'-dihydroxybiphenyl, 3,3',5,5'-tetramethyl-4,4'-dihydroxybiphenyl), bisphenols {e.g., bis(hydroxyphenyl)alkanes [e.g., 2,2-bis(4-hydroxyphenyl)propane (bisphenol A), 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, 2,2-bis(4-hydroxy-3,5-diethylphenyl)propane, , 2,2-bis(4-hydroxy-(3,5-diphenyl)phenyl)propane, 2,2-bis(4-hydroxy-3,5-dibromophenyl)propane, 2,2-bis(4-hydroxyphenyl)pentane, 2,4'-dihydroxy-diphenylmethane, bis(4-hydroxyphenyl)methane, bis(4-hydroxy-5-nitrophenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 3,3-bis(4-hydroxyphenyl)pentane, and other bis(hydroxyphenyl)C 1-10 alkanes], bis(hydroxyphenyl)cycloalkanes [e.g., bis(hydroxyphenyl)C such as 1,1-bis(4-hydroxyphenyl)cyclohexane], 4-20cycloalkanes], bis(hydroxyphenyl)sulfones [e.g., bis(4-hydroxyphenyl)sulfone, 2,4'-dihydroxydiphenyl sulfone], bis(hydroxyphenyl)ethers [e.g., 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxy-3,3'-dichlorodiphenyl ether, 4,4'-dihydroxy-2,5-diethoxydiphenyl ether], bis(hydroxyphenyl)sulfides [e.g., bis(4-hydroxyphenyl)sulfide, etc.], Bis(hydroxyphenyl)ketones [e.g., bis(4-hydroxyphenyl)ketone, etc.], dihydroxy compounds having a fluorene skeleton {e.g., bis(hydroxyphenyl)fluorenes [e.g., 9,9-bis(4-hydroxyphenyl)fluorene], bis(hydroxyalkoxy)fluorenes [e.g., 9,9-bis[(hydroxyC) such as 9,9-bis(4-(2-hydroxyethoxy)phenyl)fluorene, 9,9-bis(4-(2-hydroxyethoxy-2-methyl)phenyl)fluorene, etc. 2-4 alkoxy)phenyl]fluorenes], and the like.

[0027] The aromatic dihydroxy compounds may be used alone or in combination of two or more kinds.

[0028] The dihydroxy compounds may be used alone or in combination of two or more kinds.

[0029] As described above, the polycarbonate resin preferably has at least an aliphatic skeleton (particularly, an alicyclic skeleton), and therefore the dihydroxy compound also preferably contains at least an aliphatic dihydroxy compound (particularly, an alicyclic dihydroxy compound).

[0030] Among alicyclic dihydroxy compounds (structural units derived therefrom), the compound represented by the formula (X) (e.g., isosorbide) (structural units derived therefrom) is preferred in terms of transparency and other physical properties, ease of various adjustments in combination with the acrylic resin (B) (e.g., ease of reducing the difference in glass transition temperature with the acrylic resin (B)), etc. Therefore, the polycarbonate resin may have at least a structural unit derived from the compound represented by the formula (X).

[0031] In dihydroxy compounds including aliphatic dihydroxy compounds, the ratio of the aliphatic dihydroxy compounds to the total dihydroxy compounds can be selected depending on the type and desired physical properties (and further refractive index), and may be, for example, 1 mol % or more (e.g., 5 mol % or more), preferably 10 mol % or more (e.g., 20 mol % or more), more preferably 30 mol % or more (e.g., 40 mol % or more), or may be 50 mol % or more (e.g., 60 mol % or more, 70 mol % or more, 80 mol % or more, 90 mol % or more, 95 mol % or more, or (substantially) 100 mol %).

[0032] When the aliphatic dihydroxy compound contains an alicyclic dihydroxy compound, the ratio of the alicyclic dihydroxy compound to the total aliphatic dihydroxy compounds can be selected depending on the type and desired physical properties (and further refractive index), and may be, for example, 10 mol % or more (e.g., 30 mol % or more), preferably 50 mol % or more (e.g., 60 mol % or more), more preferably 70 mol % or more (e.g., 80 mol % or more), or may be 85 mol % or more (e.g., 90 mol % or more, 93 mol % or more, 95 mol % or more, 98 mol % or more, (substantially) 100 mol %).

[0033] When the alicyclic dihydroxy compound contains a compound represented by the formula (X) (compound (X)), the ratio of compound (X) to the entire alicyclic dihydroxy compound can be selected depending on the desired physical properties (furthermore, the refractive index) and the like, and may be, for example, 1 mol% or more (e.g., 2 mol% or more), preferably 3 mol% or more (e.g., 5 mol% or more), more preferably 7 mol% or more (e.g., 10 mol% or more), or may be 100 mol% or less (e.g., (substantially) 100 mol%, 99 mol% or less, 98 mol% or less, 97 mol% or less, 96 mol% or less, 95 mol% or less, 94 mol% or less, 93 mol% or less, 90 mol% or less).

[0034] As described above, polycarbonate resins usually contain at least a dihydroxy compound as a polymerization component, but such polymerization components may contain other polymerization components in addition to the dihydroxy compound, if necessary.

[0035] Examples of such other polymerization components include compounds having three or more hydroxy groups {e.g., aromatic polyhydroxy compounds [e.g., phloroglucin, 4,6-dimethyl-2,4,6-tris(4-hydroxyphenyl)heptene-2, 4,6-dimethyl-2,4,6-tris(4-hydroxyphenyl)heptane, 2,6-dimethyl-2,4,6-tris(4-hydroxyphenyl)heptene-3, 1,3,5-tris(4-hydroxyphenyl)benzene, 1,1,1-tris(4-hydroxyphenyl)ethane, 3,3-bis(4-hydroxyaryl)oxindole, 5-chloruisatin, 5,7-dichloruisatin, 5-bromisatin], and the like}.

[0036] The other polymerization components may be used alone or in combination of two or more kinds.

[0037] When the polycarbonate resin has structural units derived from other polymerization components (compounds having three or more hydroxy groups), the ratio of the other polymerization components (compounds having three or more hydroxy groups) (structural units derived from) to the dihydroxy compound and the other polymerization components (compounds having three or more hydroxy groups) (structural units derived from) as a whole may be, for example, 10 mol% or less (e.g., about 5 mol% or less, 3 mol% or less, 2 mol% or less, 1 mol% or less) or may be 0.001 mol% or more (e.g., 0.005 mol% or more, 0.01 mol% or more, 0.05 mol% or more, 0.1 mol% or more, etc.).

[0038] Incidentally, polycarbonate resin is generally a thermoplastic resin.

[0039] The polycarbonate resins may be used alone or in combination of two or more kinds.

[0040] Among them, the polycarbonate resin (A) preferably contains at least a polycarbonate resin having an aliphatic skeleton (particularly, a polycarbonate resin (A1) having an alicyclic skeleton) as described above.

[0041] In such a polycarbonate resin (A), the proportion of the polycarbonate resin having an aliphatic skeleton relative to the entire polycarbonate resin (A) may be, for example, 1 mass% or more (e.g., 5 mass% or more), preferably 10 mass% or more (e.g., 20 mass% or more), more preferably 30 mass% or more (e.g., 40 mass% or more), or may be 50 mass% or more (e.g., 60 mass% or more, 70 mass% or more, 80 mass% or more, 90 mass% or more, 95 mass% or more, or (substantially) 100 mass%).

[0042] In particular, when the polycarbonate resin (A) contains a polycarbonate resin (A1) having an alicyclic skeleton, the proportion of the polycarbonate resin (A1) having an alicyclic skeleton relative to the entire polycarbonate resin (A) may be, for example, 10 mass% or more (e.g., 20 mass% or more), preferably 30 mass% or more (e.g., 40 mass% or more), more preferably 50 mass% or more (e.g., 60 mass% or more), or may be 70 mass% or more (e.g., 80 mass% or more, 90 mass% or more, 95 mass% or more, or (substantially) 100 mass%).

[0043] When the polycarbonate resin having an aliphatic skeleton contains a polycarbonate resin (A1) having an alicyclic skeleton, the proportion of the polycarbonate resin (A1) having an alicyclic skeleton relative to the entire polycarbonate resin having an aliphatic skeleton can be selected depending on the type and desired physical properties (and further refractive index), and may be, for example, 10 mass% or more (e.g., 30 mass% or more), preferably 50 mass% or more (e.g., 60 mass% or more), more preferably 70 mass% or more (e.g., 80 mass% or more), or may be 85 mass% or more (e.g., 90 mass% or more, 93 mass% or more, 95 mass% or more, 98 mass% or more, (substantially) 100 mass%).

[0044] When the polycarbonate resin (A1) having an alicyclic skeleton contains a polycarbonate resin having a structural unit derived from the compound (X), the ratio of the polycarbonate resin having a structural unit derived from the compound (X) to the entire polycarbonate resin (A1) having an alicyclic skeleton can be selected according to the desired physical properties (furthermore, the refractive index) and the like, and may be, for example, 1 mass% or more (e.g., 2 mass% or more), preferably 3 mass% or more (e.g., 5 mass% or more), more preferably 7 mass% or more (e.g., 10 mass% or more), or may be 100 mass% or less (e.g., (substantially) 100 mass%, 99 mass% or less, 98 mass% or less, 97 mass% or less, 96 mass% or less, 95 mass% or less, 94 mass% or less, 93 mass% or less, 90 mass% or less).

[0045] Melt flow rate (MA The viscosity (sometimes referred to as the viscosity) depends on the type, composition, etc., but may be, for example, about 0.1 to 50 g / 10 min (e.g., 0.5 to 45 g / 10 min), preferably about 1 to 40 g / 10 min (e.g., 2 to 35 g / 10 min), and more preferably about 3 to 30 g / 10 min (e.g., 5 to 25 g / 10 min) at a temperature of 230° C. and a load of 3.8 kg.

[0046] The melt flow rate of the polycarbonate resin may be measured in accordance with JIS K 7210.

[0047] Shear viscosity (V A The viscosity (sometimes referred to as the viscosity) depends on the type, composition, etc., but may be, for example, 100 to 500 Pa·s, preferably 120 to 480 Pa·s (e.g., 130 to 450 Pa·s), and more preferably about 150 to 400 Pa·s at a temperature of 240° C. and a shear rate of 1000 / s.

[0048] Specifically, the shear viscosity of the polycarbonate resin may be measured by the method described later.

[0049] Glass transition temperature (Tg) of polycarbonate resin (A) (Tg A The heating temperature (sometimes called the heating temperature) depends on the type and composition, but may be, for example, about 70 to 200° C., preferably about 80 to 160° C., and more preferably about 90 to 140° C. (eg, 95 to 130° C.).

[0050] The Tg may be measured, for example, by the method described below.

[0051] Refractive index of polycarbonate resin (A) (wavelength 589 nm) (R AThe refractive index (which may be referred to as the refractive index) varies depending on the type, composition, and the like, but may be, for example, 1.650 or less (e.g., 1.600 or less), preferably 1.580 or less (e.g., 1.560 or less), more preferably 1.550 or less (e.g., 1.540 or less), or may be 1.530 or less (e.g., 1.520 or less, 1.515 or less, 1.510 or less, 1.505 or less, 1.502 or less, 1.500 or less).

[0052] The refractive index may be a value at 23° C., and may be measured, for example, by the method described below.

[0053] The polycarbonate resin (A) may be a commercially available product or may be produced by a conventional method.

[0054] For example, the polycarbonate resin may be produced by any of a phosgene method (e.g., a solution polymerization method using phosgene) and a method using a carbonate diester (e.g., a melt polymerization method in which a carbonate diester is reacted), and typically, the polycarbonate resin may be produced by a method using a carbonate diester.

[0055] In the method using such a carbonate diester, for example, the polymer may be produced by reacting [polymerizing (solution polymerization)] a dihydroxy compound [and, if necessary, other polymerization components (e.g., a compound having three or more hydroxy groups)] with a carbonate diester [for example, a diaryl carbonate (e.g., diphenyl carbonate, ditolyl carbonate), a dialkyl carbonate (e.g., dimethyl carbonate, diethyl carbonate, di-t-butyl carbonate), etc.] in the presence of a polymerization catalyst (e.g., an alkali metal compound, an alkaline earth metal compound), etc., if necessary.

[0056] [Acrylic resin] Acrylic resins (acrylic polymers) have a ring structure. Such acrylic resins are usually thermoplastic (resins, polymers). The method for producing such acrylic resins is not particularly limited, but may be the method described below.

[0057] The acrylic resin (which may be referred to as acrylic resin (B), resin (B), etc.) may usually have a (meth)acrylic acid ester unit [a unit (structural unit) derived from a (meth)acrylic acid ester].

[0058] The (meth)acrylic acid ester constituting the (meth)acrylic acid ester unit is not particularly limited, but examples thereof include aliphatic (meth)acrylates [e.g., (meth)acrylic acid alkyl esters (e.g., (meth)acrylic acid C such as methyl (meth)acrylate, ethyl (meth)acrylate, and butyl (meth)acrylate]. 1-18 alkyl), etc.], alicyclic (meth)acrylates [e.g., (meth)acrylic acid cycloalkyl esters (e.g., (meth)acrylic acid C such as cyclopropyl (meth)acrylate and cyclobutyl (meth)acrylate, etc. 3-20 cycloalkyl), bridged cyclic (meth)acrylates (e.g., isobornyl (meth)acrylate), etc.], aromatic (meth)acrylates [e.g., aryl (meth)acrylate esters (e.g., phenyl (meth)acrylate, o-tolyl (meth)acrylate, etc. (meth)acrylic acid C 6-20 aryl), (meth)acrylic acid aralkyl esters (e.g., (meth)acrylic acid C such as benzyl (meth)acrylate, 6-10 Aryl C 1-4 alkyl), phenoxyalkyl (meth)acrylate (e.g., phenoxy (meth)acrylate C such as phenoxyethyl (meth)acrylate, 1-4 alkyl), etc.

[0059] The (meth)acrylic acid ester also includes a (meth)acrylic acid ester having a substituent (e.g., a hydroxy group, an alkoxy group, a glycidyl group, etc.). Such a (meth)acrylic acid ester includes, for example, a methacrylic acid ester having a hydroxy group [e.g., a (meth)acrylic acid hydroxyalkyl ester (e.g., a (meth)acrylic acid hydroxyalkyl ester such as 2-hydroxyethyl (meth)acrylate], 1-12alkyl), etc.], (meth)acrylic acid esters having an alkoxy group [for example, (meth)acrylic acid alkoxyalkyl esters (for example, methacrylic acid C such as 2-methoxyethyl (meth)acrylate, etc. 1-12 Alkoxy C 1-12 alkyl)], and (meth)acrylic acid esters having a glycidyl group (for example, glycidyl (meth)acrylate, etc.).

[0060] The (meth)acrylic acid ester unit may be constituted by one kind or a combination of two or more kinds of (meth)acrylic acid ester.

[0061] The (meth)acrylic acid ester unit preferably contains at least a methacrylic acid ester unit, although this depends on the desired physical properties.

[0062] Examples of the methacrylic acid ester constituting the (meth)acrylic acid ester unit include aliphatic methacrylates [e.g., methacrylic acid alkyl esters (e.g., methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, sec-butyl methacrylate, tert-butyl methacrylate, pentyl methacrylate, amyl methacrylate, isoamyl methacrylate, n-hexyl methacrylate, 2-ethylhexyl methacrylate, heptyl methacrylate, octyl methacrylate, decyl methacrylate, dodecyl methacrylate, pentadecyl methacrylate, hexadecyl methacrylate, heptadecyl methacrylate, octadecyl methacrylate, etc. 1-18 Alkyl, preferably methacrylic acid C 1-12 alkyl), etc.], alicyclic methacrylates [e.g., methacrylic acid cycloalkyl esters (e.g., methacrylic acid C such as cyclopropyl methacrylate, cyclobutyl methacrylate, cyclopentyl methacrylate, and cyclohexyl methacrylate, etc. 3-20 Cycloalkyl, preferably methacrylic acid C 3-12cycloalkyl), bridged cyclic methacrylates (e.g., isobornyl methacrylate, etc.), etc.), aromatic methacrylates [e.g., methacrylic acid aryl esters (e.g., phenyl methacrylate, o-tolyl methacrylate, m-tolyl methacrylate, p-tolyl methacrylate, 2,3-xylyl methacrylate, 2,4-xylyl methacrylate, 2,5-xylyl methacrylate, 2,6-xylyl methacrylate, 3,4-xylyl methacrylate, 3,5-xylyl methacrylate, 1-naphthyl methacrylate, 2-naphthyl methacrylate, binaphthyl methacrylate, anthryl methacrylate, etc. 6-20 Aryl, preferably methacrylic acid C 6-10 aryl), methacrylic acid aralkyl esters (e.g., methacrylic acid C such as benzyl methacrylate, 6-10 Aryl C 1-4 alkyl), phenoxy alkyl methacrylate (e.g., phenoxy methacrylate C such as phenoxyethyl methacrylate, 1-4 alkyl), etc.

[0063] Among the methacrylic acid ester units, from the viewpoint of improving transparency, etc., it is preferable to use a methacrylic acid alkyl ester unit (e.g., methacrylic acid C 1-18 It is preferable that the copolymer contains at least one alkyl unit, and more preferable that the copolymer contains at least one methyl methacrylate unit.

[0064] The acrylic resin may contain units derived from other polymerizable monomers (monomers) than the (meth)acrylic acid ester units, if necessary. Examples of such other monomers include acid group-containing monomers (methacrylic acid, acrylic acid, etc.), styrene-based monomers [e.g., styrene, vinyl toluene, styrenes having substituents (e.g., halogen groups, alkoxy groups, alkyl groups, hydroxy groups, etc.) (e.g., α-methylstyrene, chlorostyrene, etc.), styrenesulfonic acid or salts thereof, etc.], vinyl esters (e.g., vinyl acetate, etc.), unsaturated nitriles (e.g., acrylonitrile, methacrylonitrile, etc.), olefin-based monomers (e.g., C olefins such as ethylene, propylene, 1-butene, isobutylene, 1-octene, etc.), and the like. 2-10 alkenes), amide group-containing vinyl monomers [for example, (meth)acrylamide, N-substituted (meth)acrylamides (for example, N-alkyl(meth)acrylamides such as N-methyl(meth)acrylamide; N-cycloalkyl(meth)acrylamides such as N-cyclohexyl(meth)acrylamide; N-aryl(meth)acrylamides such as N-phenyl(meth)acrylamide; N-aralkyl(meth)acrylamides such as N-benzyl(meth)acrylamide, etc.)], 2-(hydroxymethyl)acrylic acid esters (for example, alkyl esters such as ethyl 2-(hydroxymethyl)acrylate), etc.

[0065] The other monomers may be one type or two or more types may be combined to form units derived from the other monomers.

[0066] The content ratio of (meth)acrylic acid ester units in the acrylic resin (or the constituent units of the acrylic resin) can be selected from the range of, for example, 10 mass% or more (e.g., 20 mass% or more) and may be preferably 30 mass% or more (e.g., 35 mass% or more), more preferably 40 mass% or more (e.g., 45 mass% or more), or may be 50 mass% or more, 55 mass% or more, 60 mass% or more, 65 mass% or more, etc.

[0067] When the acrylic resin contains methacrylic acid ester units, the content of the methacrylic acid ester units in the acrylic resin (or the constituent units of the acrylic resin) can be selected from the range of, for example, 10% by mass or more, and may be 20% by mass or more, preferably 30% by mass or more (e.g., 35% by mass or more), more preferably 40% by mass or more (e.g., 45% by mass or more), or may be 50% by mass or more, 55% by mass or more, 60% by mass or more, 65% by mass or more, etc.

[0068] When the acrylic polymer contains methacrylic acid ester units, the content of the methacrylic acid ester units in the (meth)acrylic acid ester units may be, for example, 10 mass% or more (e.g., 20 mass% or more), preferably 30 mass% or more (e.g., 40 mass% or more), more preferably 50 mass% or more (e.g., 60 mass% or more), and may be 70 mass% or more, 80 mass% or more, 90 mass% or more, etc.

[0069] When the acrylic resin contains methacrylic acid alkyl ester units, the content ratio of the methacrylic acid alkyl ester units in the (meth)acrylic acid ester units may be, for example, 10 mass% or more (e.g., 20 mass% or more), preferably 30 mass% or more (e.g., 40 mass% or more), more preferably 50 mass% or more (e.g., 60 mass% or more), and may be 70 mass% or more, 80 mass% or more, 90 mass% or more, etc.

[0070] In addition, when the acrylic resin contains methyl methacrylate units, the content ratio of methyl methacrylate units in the (meth)acrylic acid ester units may be, for example, 10 mass% or more (e.g., 20 mass% or more), preferably 30 mass% or more (e.g., 40 mass% or more), more preferably 50 mass% or more (e.g., 60 mass% or more), and may be 70 mass% or more, 80 mass% or more, 90 mass% or more, etc.

[0071] When the acrylic resin contains acrylic ester units, the content of the acrylic ester units in the acrylic resin may be relatively small from the viewpoint of heat resistance and refractive index, and may be selected, for example, from the range of less than 10 mass % (e.g., 8 mass % or less), preferably 5 mass % or less (e.g., 4 mass % or less), and more preferably 3 mass % or less (e.g., 2 mass % or less).

[0072] When the acrylic resin contains a unit derived from another polymerizable monomer, the content of the unit in the acrylic resin is not particularly limited and can be appropriately selected. In particular, when the acrylic resin contains an acid group-containing monomer as the other polymerizable monomer, the content of the acid group-containing monomer unit may be relatively low from the viewpoint of transparency, coloring, etc., and may be, for example, 10 mass% or less (e.g., 5 mass% or less), preferably 2 mass% or less (e.g., 1 mass% or less), more preferably 0.5 mass% or less, etc.

[0073] The acrylic resin (B) has a ring structure. This ring structure is usually present in the main chain of the acrylic resin (polymer chain, acrylic polymer).

[0074] In addition, by having a ring structure in the acrylic resin, various physical properties [e.g., heat resistance, moist heat resistance, yellowing resistance, hardness (strength), solvent resistance, surface hardness, barrier properties against oxygen and water vapor, optical properties, dimensional stability, shape stability, etc.] can be imparted, improved or enhanced in the acrylic resin. In addition, since the acrylic resin has a ring structure, it is possible to efficiently produce a molded article (for example, a lens) having a thinner film thickness than polymethyl methacrylate or the like.

[0075] Specific examples of the ring structure include a cyclic imide structure (e.g., a structure derived from an N-substituted maleimide monomer, a glutarimide structure, etc.), a cyclic amide structure (e.g., a lactam structure, etc.), a cyclic ester structure (e.g., a lactone ring structure, etc.), an acid anhydride structure (e.g., a structure derived from a maleic anhydride monomer, a glutaric anhydride structure), and the like.

[0076] The ring structure may in particular be a non-anhydride structure [for example, a ring structure that is not a structure derived from a maleic anhydride monomer, a glutaric anhydride structure, or the like (for example, a cyclic imide structure, a cyclic amide structure, a cyclic ester structure, etc.)].

[0077] The acrylic resin may have one or more ring structures. When the acrylic resin has two or more ring structures, the two or more ring structures may be ring structures of the same system (e.g., two or more cyclic imide structures, etc.) or ring structures of different systems (e.g., a combination of a cyclic imide structure and a lactone structure, etc.).

[0078] Examples of the glutarimide structure and glutaric anhydride structure include a structure represented by the following formula (1).

[0079] [ka] (In the formula, R 1 and R 2 are each independently a hydrogen atom or an alkyl group; R 3 is a hydrogen atom or a substituent, and X 1 is an oxygen atom or a nitrogen atom. 1 When is an oxygen atom, n=0, and X 1 is a nitrogen atom, n=1.)

[0080] R in Equation (1) 1 and R 2 In the above, examples of the alkyl group include C 1-8 Examples of the alkyl group include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, n-hexyl, isohexyl, n-heptyl, isoheptyl, n-octyl, and 2-ethylhexyl groups.

[0081] R 1 and R 2 is in particular a hydrogen atom or C 1-4 It is preferably an alkyl group.

[0082] R in Equation (1) 3 In the above formula, examples of the substituent include a hydrocarbon group. Examples of the hydrocarbon group include an aliphatic group, an alicyclic group, an aromatic group, etc. The hydrocarbon group may further have a substituent such as a halogen.

[0083] R in Equation (1) 3 In the above, examples of the aliphatic group include C 1-10 Examples of the alkyl groups include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, n-hexyl, isohexyl, n-heptyl, isoheptyl, n-octyl, and 2-ethylhexyl groups. 1-4 Alkyl groups, particularly methyl groups, are preferred.

[0084] R in Equation (1) 3 In the above, the alicyclic group is, for example, 3-12 Cycloalkyl groups (e.g., cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, etc.) are included. Among these cycloalkyl groups, 3-7 Cycloalkyl groups, particularly cyclohexyl groups, are preferred.

[0085] R in Equation (1) 3 In the above, examples of the aromatic group include C 6-20 Aromatic groups [e.g., C 6-20 Aryl groups (e.g., phenyl, o-tolyl, m-tolyl, p-tolyl, 2,3-xylyl, 2,4-xylyl, 2,5-xylyl, 2,6-xylyl, 3,4-xylyl, 3,5-xylyl, 1-naphthyl, 2-naphthyl, binaphthyl, anthryl, etc.), C 7-20 aralkyl groups (for example, benzyl group, etc.) etc. Among these aromatic groups, phenyl group and tolyl group are preferred.

[0086] Typically, in formula (1), R1 and R 2 are each independently a hydrogen atom or a methyl group, R 3 But, C 1-10 Alkyl group, C 3-12 Cycloalkyl group or C 6-20 It may be an aromatic group, preferably R 1 and R 2 are each independently a hydrogen atom or a methyl group, R 3 But, C 1-4 Alkyl group, C 3-7 Cycloalkyl groups, C 6-20 Aryl group or C 7-20 R may be an aralkyl group, and more preferably 1 and R 2 are each independently a hydrogen atom or a methyl group, R 3 is a methyl group, a cyclohexyl group, a phenyl group or a tolyl group, and most preferably R 1 and R 2 are each independently a hydrogen atom or a methyl group, R 3 may be a cyclohexyl group or a phenyl group. From the viewpoint of suppressing coloration of the acrylic polymer, R 3 may be a hydrogen atom, a methyl group, or a cyclohexyl group, and from the viewpoint of improving the strength of the molded article, R 3 may be a hydrogen atom or a methyl group.

[0087] The ring structure may have one or more types of structures represented by formula (1).

[0088] In particular, when the ring structure has a structure represented by formula (1), a glutarimide structure which is a cyclic non-anhydride structure (i.e., in formula (1), X 1 is a nitrogen atom).

[0089] In addition, the glutaric anhydride structure (i.e., in formula (1), X 1A ring structure in which is an oxygen atom) may be hydrolyzed or have an increased acid value, which may reduce water resistance or hot water resistance or cause fluctuations in optical properties. Therefore, it may be preferable that the ring structure does not substantially have a glutaric anhydride structure, or contains only a small amount of the glutaric anhydride structure.

[0090] Examples of structures derived from maleimide monomers (particularly N-substituted maleimide monomers) and maleic anhydride monomers include the structure represented by the following formula (2).

[0091] [ka] (In the formula, R 4 , R 5 are each independently a hydrogen atom or a methyl group, and R 6 is a hydrogen atom or a substituent, and X 2 is an oxygen atom or a nitrogen atom. X 2 When is an oxygen atom, n=0, and X 2 is a nitrogen atom, n=1.)

[0092] R in Equation (2) 6 In the above formula, examples of the substituent include a hydrocarbon group. The hydrocarbon group may be, for example, an aliphatic group {e.g., an alkyl group [e.g., C 1-6 Straight-chain alkyl groups (e.g., methyl, ethyl, etc.), C 1-6 Branched alkyl groups (e.g., isopropyl groups, etc.) 1-6 alkyl group, etc.}, alicyclic groups (e.g., cyclopentyl group, cyclohexyl group, etc. 3-20 cycloalkyl groups, etc.), aromatic groups {e.g., C 6-20 Aromatic groups [e.g., C 7-20 Aralkyl groups (e.g., benzyl groups, etc.), C 6-20 aryl group (for example, phenyl group, etc.)}. The hydrocarbon group may further have a substituent such as a halogen.

[0093] X 2When is an oxygen atom, the ring structure represented by formula (2) is a structure derived from maleic anhydride monomer.

[0094] On the other hand, X 2 When is a nitrogen atom, the ring structure represented by formula (2) is a structure derived from an N-substituted maleimide monomer.

[0095] In formula (2), X 2 When is a nitrogen atom, preferably, R 4 and R 5 are each independently a hydrogen atom, R 6 C 3-20 Cycloalkyl group or C 6-20 It may be an aromatic group, more preferably R 4 and R 5 are each independently a hydrogen atom, R 6 may be a cyclohexyl group, a benzyl group, or a phenyl group. From the viewpoint of suppressing coloration of the acrylic polymer, R 6 may be a hydrogen atom, a methyl group, or a cyclohexyl group, and from the viewpoint of improving the strength of the molded article, R 6 may be a hydrogen atom or a methyl group.

[0096] The ring structure may have one or more types of structures represented by formula (2).

[0097] In particular, when the ring structure has a structure represented by formula (2), a structure derived from a maleimide monomer which is a cyclic non-anhydride structure (i.e., in formula (2), X 2 is a nitrogen atom).

[0098] In the above formula (2), X 2 When n is an oxygen atom (and n=0), the above formula (2) is a structure derived from a maleic anhydride monomer. Such a structure derived from a maleic anhydride monomer may be hydrolyzed or have an increased acid value, which may reduce water resistance or hot water resistance or cause fluctuations in optical properties. Therefore, it may be preferable that the ring structure does not substantially have a structure derived from a maleic anhydride monomer, or contains only a small amount of such a structure.

[0099] The lactone ring structure is not particularly limited and may be, for example, a 4- to 8-membered ring, but is preferably a 5- or 6-membered ring, and more preferably a 6-membered ring, due to its excellent stability as a ring structure.

[0100] The lactone ring structure may be, for example, a structure disclosed in JP-A-2004-168882, and examples thereof include a structure represented by the following formula (3).

[0101] [ka] (In the formula, R 7 , R 8 and R 9 are each independently a hydrogen atom or a substituent.

[0102] In the formula (3), examples of the substituent include organic residues such as hydrocarbon groups. Examples of the hydrocarbon group include aliphatic groups (e.g., C groups such as methyl, ethyl, and propyl groups). 1-20 C such as alkyl group, ethenyl group, propenyl group, etc. 2-20 unsaturated aliphatic hydrocarbon groups, aromatic groups (e.g., phenyl groups, naphthyl groups, etc.) 6-20 Aromatic hydrocarbon groups, etc.

[0103] The hydrocarbon group may contain an oxygen atom, and one or more hydrogen atoms may be substituted with at least one type of group selected from a hydroxyl group, a carboxyl group, an ether group, and an ester group.

[0104] In formula (3), preferably, R 9 is a hydrogen atom or a methyl group, R 7 and R 8 are each independently a hydrogen atom or C 1-20 More preferably, R 9 is a hydrogen atom or a methyl group, R 7 and R 8may each independently be a hydrogen atom or a methyl group.

[0105] The ring structure may contain one or more types of structures represented by formula (3).

[0106] The lactam ring structure is not particularly limited, and examples thereof include a pyrrolidinone ring structure represented by the following formula (4).

[0107] The pyrrolidinone ring structure has a five-membered amide ring structure (cyclic amide structure) as a basic skeleton. This cyclic amide structure is also a five-membered lactam structure (γ-lactam structure). Having a pyrrolidinone ring structure in the main chain means that at least one atom of the five atoms constituting the basic skeleton of the five-membered pyrrolidinone ring structure, typically three carbon atoms not constituting an amide bond (—N(R)CO—), is located in the main chain of the polymer and constitutes the main chain.

[0108] [ka] (In the formula, R 10 ~R 12 are each independently a hydrogen atom or a substituent.

[0109] R in Equation (4) 10 In the above, the substituents include, for example, a hydrocarbon group or -NHCOR 13 Group(R 13 is a hydrogen atom or a hydrocarbon group).

[0110] R 10 or R 13 Examples of the hydrocarbon group in include an aliphatic group, an alicyclic group, and an aromatic group. Examples of the aliphatic group include C 1-18 Alkyl groups (e.g., methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, and other C 1-18 Linear or branched alkyl groups, etc. Examples of the alicyclic group include C3-18 Examples of the cycloalkyl group include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, and a cyclohexyl group. Examples of aromatic groups include C 6-20 Aromatic groups [e.g., C 6-20 Aryl groups (e.g., phenyl, tolyl, xylyl, naphthyl, anthryl, etc.), C 7-20 aralkyl groups (for example, benzyl groups, etc.).

[0111] R 10 In particular, hydrogen atom, C 1-18 Straight-chain alkyl groups (eg, methyl groups, etc.) are preferred. Also, R 13 In particular, hydrogen atom, C 1-18 A straight chain alkyl group (preferably C 1-12 A straight chain alkyl group, more preferably C 1-4 Straight chain alkyl groups, etc.), C 6-20 Aryl groups (e.g., phenyl groups, etc.), C 3-18 Cycloalkyl groups (preferably C 3-12 Cycloalkyl groups, more preferably C 3-6 Cycloalkyl groups and the like are preferred.

[0112] R in Equation (4) 11 In the above, examples of the substituent include -COOR 14 Group(R 14 is a hydrogen atom or a hydrocarbon group).

[0113] R 14 Examples of the hydrocarbon group in 10 or R 13 Examples of the hydrocarbon groups include those exemplified by Also, R 14 Particularly preferred embodiments of the invention are also 13 This is the same as the particularly preferred embodiment of the above.

[0114] R in Equation (4) 12 In the above, examples of the substituent include -COR 15 Group(R 15is a hydrogen atom or a hydrocarbon group).

[0115] R 15 Examples of the hydrocarbon group in 10 or R 13 Examples of the hydrocarbon groups include those exemplified by Also, R 15 Particularly preferred embodiments of the invention are also 13 This is the same as the particularly preferred embodiment of the above.

[0116] The ring structure of the acrylic resin may be appropriately selected depending on the desired physical properties (e.g., heat resistance, hardness (strength), solvent resistance, surface hardness, oxygen or water vapor barrier properties, optical properties, dimensional stability, shape stability, etc.). For example, from the viewpoint of heat resistance, etc., the ring structure may suitably contain a lactone ring structure or a cyclic imide structure (e.g., a structure derived from an N-substituted maleimide monomer, a glutarimide structure, etc.).

[0117] From the viewpoint of water resistance, hot water resistance, and the like, the ring structure may suitably contain a cyclic non-anhydride structure [for example, a lactone ring structure, a cyclic imide structure (particularly, a glutarimide structure, or a structure derived from an N-substituted maleimide monomer)].

[0118] Furthermore, from the viewpoints of surface hardness, solvent resistance, barrier properties, optical properties, and the like, the ring structure may suitably contain a lactone ring structure, a glutarimide structure, or the like.

[0119] In particular, the ring structure may contain at least one ring structure selected from a cyclic imide structure (particularly, a glutarimide structure or a structure derived from an N-substituted maleimide monomer) and a lactone ring structure, and may particularly contain at least a lactone ring structure. Such a ring structure makes it easy to adjust the balance of various physical properties (e.g., heat resistance and refractive index) when combined with the polycarbonate resin (A).

[0120] The content of the ring structure can be selected depending on the application, desired physical properties, and the like, and is not particularly limited. For example, it can be selected from a range of about 0.1% by mass or more (e.g., 0.5% by mass or more) in the acrylic resin, and may be 1% by mass or more, preferably 3% by mass or more, more preferably 5% by mass or more, 10% by mass or more, 15% by mass or more, 20% by mass or more, etc.

[0121] The content ratio of the ring structure (or its upper limit) is not particularly limited, and may be, for example, 90 mass% or less, 80 mass% or less, 70 mass% or less, 60 mass% or less, 55 mass% or less, 50 mass% or less, 45 mass% or less, 40 mass% or less, 35 mass% or less, etc., in the acrylic resin.

[0122] A larger content of the ring structure is preferable in terms of heat resistance, hardness (strength), solvent resistance, surface hardness, dimensional stability, and the like.

[0123] In addition, these upper and lower limits may be appropriately combined to set an appropriate range (for example, 1 to 70 mass%, 3 to 60 mass%, 5 to 60 mass%, 5 to 50 mass%, etc.) (the same applies to others).

[0124] In particular, when the acrylic resin has a glutarimide structure, the content of the glutarimide structure may be preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, and may be 90% by mass or less, preferably 60% by mass or less, more preferably 50% by mass or less, and even more preferably 40% by mass or less.

[0125] When the acrylic resin has a structure derived from an N-substituted maleimide monomer, the content of the structure derived from the N-substituted maleimide monomer may be, for example, 5 to 90 mass%, preferably 5 to 60 mass%, more preferably 10 to 50 mass%, and even more preferably 10 to 30 mass%.

[0126] When the acrylic resin has a lactone ring structure, the content of the lactone ring structure may be, for example, 1 to 80 mass%, preferably 3 to 70 mass%, and more preferably 5 to 60 mass% (e.g., 10 to 50 mass%), and can also be 15 mass% or more (e.g., 18 to 55 mass%), 20 mass% or more (e.g., 23 to 50 mass%), 25 mass% or more (e.g., 26 to 45 mass%, 28 to 40 mass%, etc.), and the like.

[0127] When the acrylic resin has a lactam ring structure, the content of the lactam ring structure may be, for example, about 1 to 80 mass %, preferably about 5 to 70 mass %, and more preferably about 10 to 50 mass %.

[0128] The content of the ring structure may be, for example, 1 to 80 mass%, preferably 3 to 70 mass%, and more preferably 5 to 60 mass% (e.g., 10 to 50 mass%), and can also be a relatively high content, for example, 10 mass% or more [for example, 13 to 60 mass%, 15 mass% or more (e.g., 18 to 55 mass%), 20 mass% or more (e.g., 23 to 50 mass%), 25 mass% or more (e.g., 26 to 45 mass%, 28 to 40 mass%, etc.)].

[0129] By introducing a ring structure into the acrylic resin at a relatively high content, a resin composition having very excellent heat resistance (for example, high glass transition temperature) and moist heat resistance can be efficiently obtained.

[0130] In the composition of the present invention, coloring (yellowing) can be efficiently suppressed even when the acrylic resin contains a high proportion of a ring structure (for example, a ring structure containing at least a lactone ring structure).

[0131] The proportion of ring structures in the acrylic resin can be determined by a conventional method depending on the type of ring structure, etc. For example, the proportion of cyclic ester structures (lactone ring structures) can be determined based on the dealcoholization reaction rate, and the proportion of non-cyclic ester structures (e.g., cyclic imide structures, cyclic amide structures, acid anhydride structures, etc.) can be determined by NMR (e.g., 1 H-NMR, 13The NMR analysis (NMR measurement) may be performed based on an analysis (measurement) condition, which may be appropriately selected, for example, using a predetermined measurement solvent (e.g., CDCl3, DMSO-d6) and at a predetermined measurement temperature (e.g., 40°C).

[0132] As an example, a method based on the dealcoholization reaction rate will be described.

[0133] First, the weight loss that occurs when all hydroxyl groups from the polymer composition obtained by polymerization are dealcoholized as methanol was used as the basis, and the dealcoholization reaction rate was calculated from the weight loss due to the dealcoholization reaction from 150°C, before weight loss began, to 300°C, before polymer decomposition began, in dynamic TG measurements. That is, in dynamic TG measurement of a polymer having a lactone ring structure, the weight loss rate is measured between 150°C and 300°C, and the actual weight loss rate obtained is designated as (X). On the other hand, based on the composition of the polymer, it is assumed that all hydroxyl groups contained in the polymer composition are involved in the formation of lactone rings and become alcohols, which are then dealcoholized, and the theoretical weight loss rate (i.e., the weight loss rate calculated on the assumption that a 100% dealcoholization reaction occurs in that composition) is designated as (Y). More specifically, the theoretical weight reduction rate (Y) can be calculated from the molar ratio of the raw material monomer having a structure (hydroxyl group) involved in the dealcoholization reaction in the polymer, i.e., the content of the raw material monomer in the polymer composition. These values ​​(X) and (Y) are used to calculate dealcoholization: 1-(Actual weight reduction rate (X) / Theoretical weight reduction rate (Y)) Substituting the value into the above equation and expressing it as a percentage gives the dealcoholization reaction rate.

[0134] The acrylic resin may contain atoms or groups derived from components used during polymerization.

[0135] For example, the acrylic resin may contain a sulfur atom. In a more specific embodiment, the acrylic resin may have a sulfur-containing group (sulfur-containing skeleton) at least at the molecular terminal.

[0136] Such an acrylic resin having a sulfur atom or a sulfur-containing group can be obtained, for example, by using a thiol compound (such as the thiol compound described below) as a chain transfer agent.

[0137] When the acrylic resin is a copolymer, the form of the copolymerization is not particularly limited, and it may be a random copolymer, a block copolymer, an alternating copolymer, a graft copolymer, or the like.

[0138] For example, since an acrylic resin has a ring structure, it can usually be called a copolymer, but the manner in which the ring structure is introduced is not particularly limited, and the ring structure may be introduced randomly, or may be introduced in a block, alternating, graft, or other manner.

[0139] Melt flow rate of acrylic resin (B) (M B At a temperature of 230° C. and a load of 3.8 kg, the viscosity may be, for example, 0.1 g / 10 min or more (e.g., 0.2 g / 10 min or more), preferably 0.3 g / 10 min or more (e.g., 0.4 g / 10 min or more), and more preferably 0.5 g / 10 min or more (e.g., 0.6 g / 10 min or more), or may be 0.7 g / 10 min or more (e.g., 0.8 g / 10 min or more).

[0140] The upper limit of the melt flow rate of the acrylic resin (B) at a temperature of 230°C and a load of 3.8 kg may be, for example, 10 g / 10 min or less, 9.8 g / 10 min or less, 9.6 g / 10 min or less, 9.4 g / 10 min or less, 9.2 g / 10 min or less, 9 g / 10 min or less, 8.8 g / 10 min or less, 8.6 g / 10 min or less, 8.4 g / 10 min or less, 8.2 g / 10 min or less, 8 g / 10 min or less, 7.8 g / 10 min or less, 7.6 g / 10 min or less, 7.4 g / 10 min or less, 7.2 g / 10 min or less, or 7 g / 10 min or less.

[0141] Specific ranges of the melt flow rate of the acrylic resin (B) include combinations of the above ranges, and may be, for example, 0.1 to 10 g / 10 min, 0.3 to 9 g / 10 min, 0.5 to 8 g / 10 min, etc. at a temperature of 230° C. and a load of 3.8 kg.

[0142] The melt flow rate of the acrylic resin may be measured in accordance with JIS K 7210.

[0143] Shear viscosity of acrylic resin (B) (V B The viscosity (sometimes referred to as the viscosity) depends on the type, composition, etc., but may be, for example, 100 to 500 Pa·s, preferably 120 to 480 Pa·s (e.g., 130 to 450 Pa·s), and more preferably about 150 to 400 Pa·s at a temperature of 240° C. and a shear rate of 1000 / s.

[0144] Specifically, the shear viscosity of the acrylic resin may be measured by the method described later.

[0145] By having excellent melt fluidity (high melt fluidity), coloring during molding (for example, melt molding such as injection molding) is reduced, and molded products (melt molded products such as injection molded products) with low yellowness can be easily obtained efficiently.

[0146] In addition, the high melt fluidity enables molding processing at lower temperatures, and by suppressing the thermal history during the molding process, discoloration of the molded product can be reduced. In addition, the time required for the heating and cooling processes of the injection device can be shortened, so that improved productivity can be expected.

[0147] The melt flow rate may be selected for each combination of resins. For example, the melt flow rate M of polycarbonate resin (A) is A and the melt flow rate M of the acrylic resin (B) B Absolute value of difference with |M A -M B| may be, for example, 50 g / 10 min or less, preferably 40 g / 10 min or less, and more preferably 30 g / 10 min or less (e.g., 28 g / 10 min or less, 25 g / 10 min or less, 22 g / 10 min or less, 20 g / 10 min or less).

[0148] The shear viscosity may be selected for each resin combination. For example, the shear viscosity V of polycarbonate resin (A) is A and the shear viscosity V of the acrylic resin (B) B Absolute value of difference between |V A -V B |(Pa·s) may be, for example, 300 or less, preferably 280 or less, and more preferably 250 or less (eg, 220 or less, 200 or less, 180 or less, 170 or less, 160 or less).

[0149] By not making the difference in melt flow rate or shear viscosity between the two resins too large (making it relatively small), the two resins can be mixed stably, and perhaps also related to this, a composition (and even a molded product) that is relatively uniform (with little variation) in physical properties, etc. can be efficiently obtained.

[0150] The weight average molecular weight (Mw) of the acrylic resin (B) may be selected from a range of 5000 or more (for example, about 7000 or more, for example, 10000 or more (for example, 12000 or more), preferably 15000 or more (for example, 18000 or more), and more preferably 20000 or more (for example, 25000 or more), or may be 30000 or more (for example, 35000 or more, 38000 or more, 40000 or more, 42000 or more, 45000 or more, 48000 or more, 50000 or more, 52000 or more, 55000 or more, 58000 or more, 60000 or more, 62000 or more, 65000 or more, etc.).

[0151] The upper limit of the weight average molecular weight (Mw) of the acrylic resin (B) may be, for example, 500,000, 400,000, 300,000, 250,000, 200,000, 180,000, 150,000, 120,000, or the like.

[0152] A specific range of the weight average molecular weight (Mw) of the acrylic resin (B) may be, for example, 20,000 to 200,000, 30,000 to 150,000, or 50,000 to 200,000, from the viewpoint of moldability and the like.

[0153] The acrylic resin (B) may have a relatively narrow molecular weight distribution (Mw / Mn) from the viewpoints of melt flowability, strength of a molded product, and the like. The molecular weight distribution (Mw / Mn) of the acrylic resin (B) may be, for example, about 1 to 10 (e.g., 1.1 to 7.0), preferably about 1.2 to 5.0 (e.g., 1.5 to 4.0), or may be about 1.5 to 3.0, or may be 2.8 or less, 2.7 or less, 2.6 or less, 2.5 or less, etc.

[0154] The molecular weight (and molecular weight distribution) may be measured, for example, using GPC and converted into polystyrene.

[0155] The acid value of the acrylic resin (B) varies depending on the application, etc., but is usually preferably small, and may be, for example, about 10 mmol / g or less, preferably 5 mmol / g or less, and more preferably 3 mmol / g or less (e.g., 1.5 mmol / g or less), or may be 1.2 mmol / g or less (e.g., 1 mmol / g or less, 0.8 mmol / g or less, 0.7 mmol / g or less, 0.6 mmol / g or less, 0.5 mmol / g or less, 0.4 mmol / g or less, 0.35 mmol / g or less, etc.).

[0156] The acid value may be measured, for example, by the method described below.

[0157] Glass transition temperature (Tg) of acrylic resin (B) BThe heating temperature (sometimes referred to as "temperature") may be, for example, 70°C or higher (e.g., 80 to 200°C), preferably 90°C or higher (e.g., 100 to 180°C), and more preferably about 110°C or higher (e.g., 112 to 170°C), may be about 115°C or higher (e.g., 118 to 160°C), or may be 120°C or higher [e.g., 120 to 160°C, 125°C or higher (e.g., 126 to 155°C), 128°C or higher (e.g., 129 to 150°C)], etc. The glass transition temperature can be efficiently adjusted, for example, by the content ratio of the ring structure introduced into the acrylic resin. The acrylic resin (B) has a ring structure and often has a relatively high glass transition temperature.

[0158] The Tg may be measured, for example, by the method described below.

[0159] The glass transition temperature may be selected depending on the combination of each resin. For example, the glass transition temperature Tg A and the glass transition temperature Tg of acrylic resin (B) B Absolute value of difference between |Tg A -Tg B | may be, for example, 70°C or less (e.g., 60°C or less), preferably 50°C or less (e.g., 45°C or less), and more preferably 40°C or less (e.g., 38°C or less, 35°C or less, 32°C or less, 30°C or less). By not making the difference in glass transition temperature between the two resins too large (making it relatively small), it becomes easier to efficiently obtain a composition (and even a molded product) that has relatively uniform (less variation) physical properties (heat resistance, etc.).

[0160] Refractive index of acrylic resin (B) (wavelength 589 nm) (R BThe molecular weight ratio (Mn) of the ring structure varies depending on its type and composition (type and content of ring structure), but may be, for example, about 1.450 to 1.550 (e.g., 1.470 to 1.530), preferably about 1.480 to 1.520 (e.g., 1.490 to 1.515), more preferably about 1.492 to 1.510 (e.g., 1.495 to 1.505, 1.496 to 1.502), or may be 1.494 or more.

[0161] The refractive index may be a value at 23° C., and may be measured, for example, by the method described below.

[0162] The refractive index may be selected depending on the combination of each resin. For example, the refractive index R of the polycarbonate resin (A) is A and the refractive index R of acrylic resin (B). B Absolute difference between |R A -R B | may be selected, for example, from a range of about 0.100 or less (e.g., 0.090 or less), and may be 0.080 or less (e.g., 0.060 or less), preferably 0.050 or less (e.g., 0.030 or less), and more preferably 0.020 or less (e.g., 0.015 or less, 0.012 or less, 0.010 or less, 0.008 or less, 0.006 or less, 0.005 or less, 0.004 or less, 0.003 or less, 0.0025 or less, 0.002 or less). By not making the difference in refractive index between the two resins too large (making it relatively small), a composition (and even a molded article) can be easily formed without impairing transparency and the like.

[0163] The acrylic resin (B) may be a commercially available product or may be prepared by manufacturing. The method for manufacturing the acrylic resin (B) will be described below.

[0164] (Method of manufacturing acrylic resin)

[0165] The acrylic resin (acrylic polymer) can be produced through at least a step of polymerizing a polymerization component (polymerization step).

[0166] The polymerization components are monomers that are raw materials for acrylic resins, and correspond to the above-exemplified (meth)acrylic acid esters and other monomers. The types and preferred embodiments of the monomers are the same as those described above.

[0167] The acrylic resin has a ring structure, and depending on the type of ring structure, the polymerization components may contain a monomer that constitutes the ring structure or a monomer that is a raw material for the ring structure.

[0168] For example, in the case of producing an acrylic resin having a structure derived from a maleimide monomer or a maleic anhydride monomer, the polymerization components include, for example, maleic anhydride, maleimide-based monomers [e.g., maleimide; N-alkylmaleimide (e.g., N-methylmaleimide, N-ethylmaleimide, etc.); 1-10 N-alkylmaleimides, N-cycloalkylmaleimides (e.g., cyclohexylmaleimide, etc.) 3-20 cycloalkylmaleimides), N-arylmaleimides (e.g., N-phenylmaleimide, etc. 6-10 N-arylmaleimides, N-aralkylmaleimides (e.g., N-benzylmaleimide, etc. 7-10 The compound may include N-substituted maleimides such as aralkylmaleimides.

[0169] When producing an acrylic resin having a lactone ring structure, the polymerization components may contain a monomer that serves as a raw material for the lactone ring, such as a 2-(hydroxymethyl)acrylic acid ester (for example, an alkyl ester such as ethyl 2-(hydroxymethyl)acrylate).

[0170] In the case of producing an acrylic resin having a lactam ring structure, the polymerization components may contain lactam monomers [for example, N-vinylpyrrolidone monomers (for example, N-vinylpyrrolidone, N-vinyl-4-butylpyrrolidone, N-vinyl-4-propylpyrrolidone, N-vinyl-4-ethylpyrrolidone, N-vinyl-4-methylpyrrolidone, N-vinyl-4-methyl-5-ethylpyrrolidone, N-vinyl-4-methyl-5-propylpyrrolidone, N-vinyl-5-methyl-5-ethylpyrrolidone, N-vinyl-5-propylpyrrolidone, N-vinyl-5-butylpyrrolidone, etc.), N-vinylcaprolactam monomers (for example, N-vinylcaprolactam, N-vinyl-6-methylcaprolactam, N-vinyl-6-propylcaprolactam, N-vinyl-7-butylcaprolactam, etc.)], etc.

[0171] The polymerization may generally be a radical polymerization.

[0172] The polymerization may be carried out in the presence of a polymerization initiator (particularly a radical polymerization initiator).

[0173] The polymerization initiator (radical polymerization initiator) is not particularly limited, but examples thereof include organic peroxides [e.g., peroxides (dialkyl peroxides, diacyl peroxides, etc.), peroxy monocarbonates, peroxy esters, peroxy ketals, etc.], azo compounds, and the like.

[0174] Specific examples of the polymerization initiator include organic peroxides [e.g., tert-amylperoxyisononanoate, t-amylperoxy-2-ethylhexanoate, tert-butylperoxy-3,5,5-trimethylhexanate, tert-butylperoxylaurate, tert-butylperoxyisopropyl monocarbonate, tert-hexylperoxyisopropyl monocarbonate, tert-butylperoxyacetate, 1,1-bis(tert-butylperoxy)3,3,5-trimethylcyclohexane, 1,1-bis(tert-butylperoxy)cyclohexane, tert-butylperoxy2-ethylhexanoate, tert-butyl ...cyclohexane, tert-butylperoxy2-ethylhexanoate, tert-butylperoxyisopropyl monocarbonate, tert-butylperoxyisopropyl monocarbonate, tert-butylperoxyacetate, 1,1-bis(tert-butylperoxy)cyclohexane, tert-butylperoxy2-ethylhexanoate, xanate, tert-butylperoxyisobutyrate, tert-hexylperoxy 2-ethylhexanate, di-tert-butyl peroxide, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, etc.], azo compounds [for example, 2-(carbamoylazo)-isobutyronitrile, 1,1'-azobis(1-cyclohexanecarbonitrile), 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), dimethyl 2,2'-azobisisobutyrate, 2,2'-azobis(2,4,4-trimethylpentane), 2,2'-azobis(2-methylpropane), etc.], etc.

[0175] The polymerization initiators may be used alone or in combination of two or more kinds.

[0176] In particular, at least an organic peroxide (such as a peroxy ester) may be suitably used as the polymerization initiator.

[0177] The amount (usage ratio) of the polymerization initiator used will vary depending on the type of polymerization initiator, and may be, for example, 0.01 part by mass or more, preferably 0.05 parts by mass or more, more preferably 0.1 part by mass or more, and particularly 0.15 parts by mass or more, relative to 100 parts by mass of the polymerization components, or may be 0.2 parts by mass or more (e.g., 0.25 parts by mass or more, 0.28 parts by mass or more, 0.3 parts by mass or more, 0.32 parts by mass or more, 0.35 parts by mass or more, 0.38 parts by mass or more, 0.4 parts by mass or more, 0.42 parts by mass or more, 0.45 parts by mass or more, 0.48 parts by mass or more, 0.5 parts by mass or more, 0.52 parts by mass or more).

[0178] The upper limit of the amount of the polymerization initiator used is not particularly limited, and may be, for example, 10 parts by mass, 9 parts by mass, 8 parts by mass, 7 parts by mass, 6 parts by mass, 5 parts by mass, 4.5 parts by mass, 4 parts by mass, 3.5 parts by mass, 3.2 parts by mass, 3 parts by mass, 2.8 parts by mass, 2.5 parts by mass, 2.2 parts by mass, 2 parts by mass, 1.8 parts by mass, 1.5 parts by mass, 1.2 parts by mass, 1 part by mass, 0.9 parts by mass, 0.8 parts by mass, 0.7 parts by mass, or the like, relative to 100 parts by mass of the polymerization components.

[0179] In particular, the proportion of the polymerization initiator used relative to 100 parts by mass of the polymerization components may be relatively large [for example, 0.2 parts by mass or more, 0.3 parts by mass or more, 0.4 parts by mass or more (for example, 0.4 to 0.8 parts by mass)].

[0180] By using a relatively large amount of the polymerization initiator in this way, it is easy to efficiently obtain an acrylic resin that is advantageous in terms of melt fluidity, etc. Even when a chain transfer agent is used, it is easy to ensure a sufficient polymerization reaction rate, and an acrylic resin with good melt fluidity can be efficiently obtained.

[0181] The polymerization may be carried out in the presence of a chain transfer agent.

[0182] The chain transfer agent is not particularly limited, but examples thereof include thiol compounds {e.g., primary thiols [e.g., aliphatic primary thiols (e.g., primary alkyl mercaptans such as butanethiol, octanethiol, decanethiol, dodecanethiol (n-dodecyl mercaptan), hexadecanethiol, octadecanethiol, and decanetrithiol, preferably primary C 3―30 alkyl mercaptans), etc.], secondary thiols [for example, aliphatic secondary thiols (e.g., secondary alkyl mercaptans such as 2-propanethiol, 2-butanethiol, 2-methyl-1-propanethiol, 3-methyl-2-butanethiol, 3-pentanethiol, 2-decanethiol, 3-decanethiol, 4-decanethiol, 5-decanethiol, 2-hexadecanethiol, 5-hexadecanethiol, and 8-octadecanethiol, preferably secondary C 3―30 alkyl mercaptans), alicyclic secondary thiols (e.g., cycloalkyl mercaptans such as cyclohexanethiol and cyclopentanethiol, preferably C 3―20 Cycloalkyl mercaptans), aromatic secondary thiols (e.g., aryl mercaptans such as thiophenol, preferably C 6-20 aryl mercaptans), etc.], tertiary thiols [for example, aliphatic tertiary thiols (for example, tert-alkyl mercaptans such as tert-butyl mercaptan, tert-dodecyl mercaptan, tert-nonyl mercaptan, tert-hexyl mercaptan, etc., preferably C 3―30 tert-alkyl mercaptans, etc.}

[0183] In addition, when the chain transfer agent contains a polyfunctional thiol, the proportion of the polyfunctional thiol in the chain transfer agent may be small. The amount (proportion) of the polyfunctional thiol used in the chain transfer agent may be, for example, 20% by mass or less (e.g., 15% by mass or less), preferably 10% by mass or less (e.g., 5% by mass or less), more preferably 3% by mass or less, 1% by mass or less, 0.5% by mass or less, etc.

[0184] The chain transfer agent may be used alone or in combination.

[0185] The amount (usage ratio) of the chain transfer agent used may be, for example, 0.001 part by mass or more, preferably 0.005 part by mass or more, more preferably 0.01 part by mass or more, particularly preferably 0.015 part by mass or more, or may be 0.02 part by mass or more, relative to 100 parts by mass of the polymerization components.

[0186] The upper limit of the amount of the chain transfer agent used is not particularly limited, and may be, for example, 5 parts by mass, 4 parts by mass, 3 parts by mass, 2 parts by mass, 1.5 parts by mass, 1 part by mass, 0.5 parts by mass, 0.25 parts by mass, 0.2 parts by mass, 0.15 parts by mass, 0.1 parts by mass, 0.08 parts by mass, 0.07 parts by mass, or the like, relative to 100 parts by mass of the polymerization components.

[0187] In particular, even when a chain transfer agent is used, the proportion of the chain transfer agent used relative to 100 parts by mass of the polymerization components may be relatively small [for example, 0.5 parts by mass or less, 0.1 parts by mass or less (for example, 0.001 to 0.1 parts by mass)] from the viewpoint of reducing coloration, and it is not necessary to use a chain transfer agent.

[0188] In this way, even if no chain transfer agent is used or even if a relatively small amount of chain transfer agent is used, an acrylic resin which is advantageous in terms of melt flowability and the like can be easily and efficiently obtained.

[0189] The mass ratio of the chain transfer agent and the polymerization initiator may be preferably 1 / 2 or less, more preferably 1 / 3 or less, 1 / 4 or less, or 1 / 5 or less, from the viewpoints of suppressing coloration of the acrylic resin, melt fluidity, etc. The mass ratio of the chain transfer agent and the polymerization initiator is calculated by (mass of the chain transfer agent) / (mass of the polymerization initiator).

[0190] The polymerization may be carried out in the presence of a polymerization initiator, a chain transfer agent, and other components (eg, a pH adjuster, various catalysts, etc.) as necessary.

[0191] The polymerization may be any of bulk polymerization, solution polymerization, suspension polymerization, emulsion polymerization, etc., and may be solution polymerization from the viewpoint of obtaining a polymer that does not contain impurities and has stable fluidity. In solution polymerization, since it can polymerize relatively uniformly, it seems that the generation of a polymer with a significantly high molecular weight is suppressed compared to bulk polymerization, and it is easy to efficiently obtain a polymer with stable fluidity. In addition, since it does not contain impurities such as emulsifiers compared to suspension polymerization and emulsion polymerization, it is easy to efficiently obtain a polymer with high transparency.

[0192] When the polymerization is carried out in a solvent (for example, in the case of solution polymerization), the solvent can be appropriately selected depending on the types of polymerization components and the like, and is not particularly limited. For example, organic solvents [aromatic hydrocarbons (for example, benzene, toluene, xylene, ethylbenzene, etc.), aliphatic or alicyclic hydrocarbons (for example, cyclohexane, methylcyclohexane, etc.), halogenated solvents (for example, chloroform, methylene chloride, carbon tetrachloride, etc.)], ketones (for example, acetone, methyl ethyl ketone, etc.), esters (for example, ethyl acetate, butyl acetate, etc.), ethers [for example, chain ethers (for example, diethyl ether, etc.), cyclic ethers (e.g., tetrahydrofuran, dioxane, etc.), amides [e.g., N-substituted amides (N-alkyl-substituted alkanamides such as N,N-dimethylformamide)], alcohols (e.g., alkanols such as methanol, ethanol, isopropanol), glycol ethers (e.g., monoalkyl ethers of alkanediols or polyalkanediols such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, propylene glycol monomethyl ether, diethylene glycol monoethyl ether, etc.)], and the like.

[0193] The solvents may be used alone or in combination of two or more kinds.

[0194] In the polymerization, the concentration of the polymerization components in the entire polymerization system may be, for example, 20% by mass or more (e.g., 20 to 70% by mass), preferably 35% by mass or more (e.g., 35 to 65% by mass), more preferably 40% by mass or more (e.g., 40 to 60% by mass), and particularly preferably 45% by mass or more (e.g., 45 to 55% by mass), from the viewpoints of suppressing an increase in molecular weight and productivity.

[0195] Each component (e.g., polymerization components, polymerization initiator, chain transfer agent, other components, solvent, etc.) may be present (charged) in the reaction system (reactor) at the start of polymerization, may be added (or mixed) as the polymerization progresses, or may be a combination of these. In such cases, the addition speed and addition time of each component can be appropriately selected.

[0196] Each component may be added to the reaction system in multiple portions (two or more portions, for example, 2 to 5 portions). In particular, the polymerization components (monomers) may be added to the reaction system as the polymerization proceeds, in which case the polymerization components may be added in multiple portions or may be added dropwise. When the polymerization components are added dropwise to the reaction system, an acrylic resin having a relatively narrow molecular weight distribution is easily obtained. Also, a polymerization initiator may be added to the reaction system as the polymerization proceeds. In particular, when the polymerization components are added to the reaction system by dropping, it is preferable to add the polymerization initiator to the reaction system by dropping. By adding the polymerization initiator to the reaction system as the polymerization proceeds, it is expected that safety can be ensured or a polymer having a relatively narrow molecular weight distribution can be obtained. When the polymerization components and the polymerization initiator are added dropwise, the dropping speed is not particularly limited. However, from the viewpoint of easily obtaining an acrylic resin having a relatively small molecular weight, it is preferable to add them slowly, and they may be added over one hour or more (for example, 1 to 10 hours).

[0197] The polymerization is usually carried out at a predetermined temperature (or under heating). The polymerization temperature (reaction temperature) can be appropriately selected depending on the types of polymerization components, polymerization initiator, solvent, etc., and may be, for example, 20°C or higher, preferably 30°C or higher (e.g., 35 to 180°C), more preferably 40°C or higher (e.g., 45 to 170°C), particularly preferably 50°C or higher (e.g., 55 to 160°C), particularly preferably 60°C or higher (e.g., 65 to 150°C), and may usually be about 70 to 140°C (e.g., 80 to 130°C).

[0198] The polymerization temperature may be changed as the polymerization proceeds. Even in such a case, the polymerization is usually carried out within the above-mentioned temperature range.

[0199] The polymerization may be carried out under stirring, in air, or in an inert atmosphere (such as nitrogen, helium, or argon).

[0200] The polymerization time (when maturation is performed) can be appropriately selected depending on the amount of polymerization components, polymerization temperature, etc., and is not particularly limited, but may be, for example, 30 minutes or more (e.g., 40 minutes to 24 hours), preferably 1 hour or more (e.g., 1.5 to 16 hours), and more preferably 2 hours or more (e.g., 2.5 to 12 hours).

[0201] The acrylic resin (B) has a ring structure. Such a ring structure may be formed during the above-mentioned polymerization depending on the type of ring structure (for example, in the case of a structure derived from a maleimide monomer or a maleic anhydride monomer, a lactam ring structure, etc.), and can be formed or introduced into the acrylic resin through a step of forming or introducing a ring structure after polymerization. The method of forming or introducing the ring structure is not particularly limited, and can follow a known method.

[0202] For example, the lactone ring structure can be formed or introduced by cyclizing (cyclization condensation, cyclization treatment) an acrylic resin containing a unit derived from a monomer that is a raw material for the lactone ring [e.g., 2-(hydroxymethyl)acrylic acid ester] as described above. The cyclization may be carried out in the presence of a cyclization catalyst [e.g., a phosphorus-based catalyst (e.g., a phosphoric acid ester such as stearyl phosphate)].

[0203] The glutarimide structure can be formed or introduced into the acrylic polymer by known methods such as imidizing (meth)acrylic acid ester units (for example, the methods described in JP-A-2006-309033, JP-A-2006-317560, JP-A-2006-328329, JP-A-2006-328334, JP-A-2006-337491, JP-A-2006-337492, JP-A-2006-337493, JP-A-2007-009182, etc.).

[0204] The glutaric anhydride structure can be formed or introduced into an acrylic polymer, for example, by a method of intramolecular dealcoholization reaction between adjacent (meth)acrylic acid ester units and (meth)acrylic acid units (for example, the methods described in JP-A-2006-283013, JP-A-2006-335902, and JP-A-2006-274118).

[0205] Through such a polymerization step (and a cyclization step, if necessary), an acrylic resin is obtained.

[0206] The resin obtained through the polymerization step may be appropriately purified and separated by a conventional method.

[0207] [Other resins] The composition (molded article) of the present invention may contain other resins as necessary.

[0208] The other resins can be appropriately selected depending on the desired physical properties, applications, etc., and are not particularly limited. They may be thermoplastic resins, curable resins, or combinations of these. The other resins may be used alone or in combination of two or more kinds.

[0209] Specific examples of other resins include olefin-based polymers (e.g., polyethylene, polypropylene, ethylene-propylene copolymers, poly(4-methyl-1-pentene), etc.), halogen-based polymers (e.g., vinyl halide polymers such as polyvinyl chloride, polyvinylidene chloride, polyvinyl chloride, etc.), styrene-based polymers [e.g., polystyrene, styrene-based copolymers (e.g., styrene-methyl methacrylate copolymers, styrene-acrylonitrile copolymers, acrylonitrile-butadiene-styrene block copolymers (ABS resins), acrylate-styrene-acrylonitrile copolymers (ASA resins), etc.)], polyethylene, Examples of the polymer include steric polymers (e.g., aromatic polyesters such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate), polyamide resins (e.g., aliphatic polyamide resins such as polyamide 6, polyamide 66, and polyamide 610), polyacetal resins, polyphenylene oxide resins, polyphenylene sulfide resins, polyether ether ketone resins, polysulfone resins, polyethersulfone resins, and rubber polymers (e.g., styrene resins (e.g., styrene copolymers such as ABS resin and ASA resin) blended with rubber (polybutadiene rubber, acrylic rubber, and the like)).

[0210] The other resins include acrylic resins. Examples of the acrylic resins include acrylic resins that do not belong to the category of the acrylic resin (B) [for example, methacrylic resins having structural units derived from methacrylic acid esters (for example, the above-mentioned exemplified methacrylic acid esters such as methyl methacrylate) (for example, acrylic resins that do not have a ring structure, such as polymers having methacrylic acid esters as a polymerization component, such as polymethyl methacrylate, and polymers having methacrylic acid esters and aromatic vinyl compounds as polymerization components, such as methyl methacrylate-styrene copolymers)].

[0211] The other resins include cellulose-based resins. Examples of cellulose-based resins (cellulose derivatives) include cellulose esters [e.g., cellulose acetate (cellulose diacetate, cellulose triacetate), cellulose propionate, cellulose butyrate, cellulose acetate propionate, cellulose acetate butyrate, and other cellulose acylates], cellulose ethers [e.g., alkyl celluloses (e.g., methyl cellulose, ethyl cellulose, and other), hydroxyalkyl celluloses (e.g., hydroxyethyl cellulose, hydroxyalkyl cellulose, and other), carboxyalkyl celluloses (e.g., carboxymethyl cellulose, and other)], and cyanoethyl cellulose.

[0212] The other resins include thermoplastic elastomers. The thermoplastic elastomers are not particularly limited, and examples thereof include styrene-based elastomers, olefin-based elastomers, urethane-based elastomers, and amide-based elastomers.

[0213] The other resin may be selected in combination with each resin. For example, the refractive index R C and the refractive index R of polycarbonate resin (A). A or the refractive index R of acrylic resin (B) B Absolute difference between |R A -R C |or|R B -R C Although | depends on the compatibility with the resin (A) and / or (B), from the viewpoint of transparency and the like, it may be selected, for example, from a range of about 0.100 or less (e.g., 0.09 or less) and may be 0.080 or less (e.g., 0.060 or less), preferably 0.050 or less (e.g., 0.030 or less), and more preferably 0.020 or less (e.g., 0.015 or less, 0.012 or less, 0.010 or less, 0.008 or less, 0.006 or less, 0.005 or less, 0.004 or less, 0.003 or less, 0.0025 or less, 0.002 or less).

[0214] [Other ingredients] The composition (molded article) of the present invention may contain other components as necessary. Such other components can be selected according to the desired application, physical properties, etc., and may contain other components (additives). The other components (additives other than colorants) are not particularly limited, and examples thereof include ultraviolet absorbers, colorants, antioxidants (e.g., phenol-based antioxidants, thioether-based antioxidants, phosphoric acid-based antioxidants, etc.), stabilizers, reinforcing materials, flame retardants, antistatic agents, organic fillers, inorganic fillers, antiblocking agents, resin modifiers, organic fillers, inorganic fillers, plasticizers, lubricants, retardation reducers, etc.

[0215] The other components may be used alone or in combination of two or more.

[0216] The ultraviolet absorbing ability of the ultraviolet absorber (UVA) may be within the wavelength range of 300 to 380 nm, and the molar extinction coefficient (chloroform solution) for the light of the wavelength at which the absorption by UVA is maximum is 10,000 (L mol -1 ·cm -1 ) or more.

[0217] The ultraviolet absorbing agent (UVA) is not particularly limited, but examples thereof include benzophenone-based compounds, salicylate-based compounds, benzoate-based compounds, triazole-based compounds, and triazine-based compounds.

[0218] Examples of triazole compounds include 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazol-2-yl)phenol], 2-(3,5-di-t-butyl-2-hydroxyphenyl)-5-chlorobenzotriazole, 2-(2H-benzotriazol-2-yl)-p-cresol, 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol, 2-benzotriazol-2-yl-4,6-di-t-butylphenol, 2-[5-chloro(2H)-benzotriazol-2-yl]-4-methyl-6-(t-butyl)phenol, 2-(2H-benzotriazol-2-yl)-4,6-di-t-butylphenol, 2-(2H-benzotriazol-2-yl)-4,6-di-t-butylphenol, )-4-(1,1,3,3-tetramethylbutyl)phenol, 2-(2H-benzotriazol-2-yl)-4-methyl-6-(3,4,5,6-tetrahydrophthalimidylmethyl)phenol, reaction products of methyl-3-(3-(2H-benzotriazol-2-yl)-5-t-butyl-4-hydroxyphenyl)propionate / polyethylene glycol 300, 2-(2H-benzotriazol-2-yl)-6-(linear and branched chain dodecyl)-4-methylphenol, 2-(5-methyl-2-hydroxyphenyl)benzotriazole, 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl]-2H-benzotriazole, 3-(2H-benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxy-C 7-9 Side chain and straight chain alkyl esters, etc. Triazole compounds having a halogen atom, for example a chlorine atom, are preferred because of their high ultraviolet absorbing ability.

[0219] Examples of the triazine compounds include 2,4-diphenyl-6-(2-hydroxy-4-methoxyphenyl)-1,3,5-triazine, 2,4-diphenyl-6-(2-hydroxy-4-ethoxyphenyl)-1,3,5-triazine, 2,4-diphenyl-(2-hydroxy-4-propoxyphenyl)-1,3,5-triazine, 2,4-diphenyl-(2-hydroxy-4-butoxyphenyl)-1,3,5-triazine, 2,4-diphenyl-6-(2-hydroxy-4-butoxyphenyl)-1,3,5-triazine, 2,4-diphenyl-6-(2-hydroxy-4-hexyloxyphenyl)-1,3,5-triazine, 2,4-diphenyl-6-(2-hydroxy-4-octyloxyphenyl)-1,3,5-triazine, and 2,4-diphenyl-6-(2-hydroxy-4-dodecyloxyphenyl). 2,4-bis(2-hydroxy-4-butoxyphenyl)-6-(2,4-dibutoxyphenyl)-1,3,5-triazine, 2,4-bis(2-hydroxy-4-butoxyphenyl)-6-(2,4-dibutoxyphenyl)-1,3-5-triazine, 2,4,6-tris(2-hydroxy-4-hexyloxy-3-methylphenyl)-1,3,5-triazine, 2,4-bis(2,4-dimethylphenyl)-6-[2-hydroxy-4-(3-alkyloxy-2-hydroxypropyloxy)-5-α-cumylphenyl]-s-triazine skeleton (alkyloxy; long-chain alkyloxy groups such as octyloxy, nonyloxy, and decyloxy) UVAs. Among these, UVAs having a 2,4-bis(2,4-dimethylphenyl)-6-[2-hydroxy-4-(3-alkyloxy-2-hydroxypropyloxy)-5-α-cumylphenyl]-s-triazine skeleton (alkyloxy; long-chain alkyloxy groups such as octyloxy, nonyloxy, and decyloxy) are preferred because of their excellent ultraviolet absorbing performance.

[0220] The molecular weight of the UVA is not particularly limited, but is preferably at least 600. The upper limit of the molecular weight of the UVA may be, for example, 10,000, 8,000, 5,000, or the like.

[0221] The ultraviolet absorbents may be used alone or in combination of two or more kinds.

[0222] The colorant is not particularly limited and can be appropriately selected depending on the application of the composition, and may be, for example, a pigment (eg, inorganic pigment, organic pigment), a dye, or the like.

[0223] The colorant may also have bluing properties (the property of compensating (countering) and reducing the color (eg, yellow) of the acrylic resin or composition). Such a colorant may be a colorant (compound) having a maximum absorption wavelength in the range of 520 to 600 nm, 540 to 580 nm, or the like, depending on the color to be corrected.

[0224] Such a colorant can be appropriately selected depending on the type (wavelength) of the color to be corrected, and examples thereof include compounds having an anthraquinone skeleton (anthraquitone-based compounds), compounds having a phthalocyanine skeleton (phthalocyanine-based compounds), compounds having an azo skeleton (azo-based compounds), and compounds having a triarylmethane skeleton (triarylmethane-based compounds). Among these, compounds having an anthraquinone skeleton may be preferably used from the viewpoint of heat resistance and the like.

[0225] Specific examples of colorants (colorants having bluing properties, bluing agents) include anthraquinone dyes [e.g., Solvent Violet 13 (CA. No. (Color Index Number) 60725), Solvent Violet 14, Solvent Violet 31 (CA. No. 68210), Solvent Violet 33 (CA. No. 60725), Solvent Violet 36 (CA. No. 68210), Solvent Blue 45 (CA. No. 61110), Solvent Blue 94 (CA. No. 61500), Solvent Blue 87, Solvent Blue 97, Disperse Violet 28, etc.], phthalocyanine dyes [e.g., Solvent Blue 25 (CA. No. 74350), etc.], monoazo dyes [e.g., Solvent Violet 21, etc.], triarylmethane dyes [e.g., Solvent Blue 2 (CA.No.42563), etc.

[0226] As such colorants, commercially available products such as "Macrolex (registered trademark) Violet B", "Macrolex (registered trademark) Violet 3R", "Macrolex (registered trademark) Blue RR" (manufactured by LANXESS KK), "Sumiplast (registered trademark) Violet B", "Sumiplast (registered trademark) Green G" (manufactured by Sumika Chemtex Co., Ltd.), "Polysynthren (registered trademark) Blue RLS" (manufactured by Clariant), "Diaresin Violet D", "Diaresin Blue G", "Diaresin Blue N" (manufactured by Mitsubishi Chemical Corporation) and the like may be used.

[0227] The colorants may be used alone or in combination of two or more kinds.

[0228] [Composition and molded article] In the composition (molded article), the proportion of the polycarbonate resin (A) relative to the entire composition (or resin component) can be selected, for example, from the range of 1 mass % or more (e.g., 1 to 99 mass %) and may be 5 mass % or more (e.g., 10 mass % or more), preferably 20 mass % or more (e.g., 25 mass % or more), and more preferably 30 mass % or more (e.g., 40 mass % or more).

[0229] In the composition (molded article), the proportion of the acrylic resin (B) can be selected from the range of, for example, 0.5 mass% or more (e.g., 1 to 99 mass%) relative to the entire composition (or resin component), and may be 2 mass% or more (e.g., 3 mass% or more), preferably 4 mass% or more (e.g., 5 mass% or more), and more preferably 7 mass% or more (e.g., 8 mass% or more).

[0230] In the composition (molded article), the mass ratio of the polycarbonate resin (A) to the acrylic resin (B) (former / latter (mass ratio)) may be, for example, in the range of about 1 / 99 to 99.5 / 0.5, or may be about 5 / 95 to 99 / 1, preferably about 10 / 90 to 98 / 2 (e.g., 20 / 80 to 97 / 3), more preferably about 30 / 70 to 97 / 3 (e.g., 35 / 65 to 96 / 4), or may be 40 / 60 to 95 / 5 (e.g., 45 / 55 to 93 / 3, 50 / 50 to 90 / 10).

[0231] When the composition (molded article) contains other resins, the content of the other resins relative to the entire composition [or resin components (the total amount of polycarbonate resin (A), acrylic resin (B) and other resins)] can be selected from the range of, for example, about 70 mass % or less (e.g., 0.1 to 60 mass %), and may be 50 mass % or less (e.g., 0.5 to 40 mass %), preferably about 30 mass % or less (e.g., 1 to 25 mass %), or may be 20 mass % or less (e.g., 15 mass % or less, 10 mass % or less, 5 mass % or less, 3 mass % or less, 1 to 10 mass %, etc.).

[0232] From the viewpoint of efficiently expressing the physical properties and the like resulting from the combination of the polycarbonate resin (A) and the acrylic resin (B), even when other resins are contained, it is preferable that the proportion of the other resins (especially the other non-acrylic resins) is not too large.

[0233] When the composition contains other components (additives), the proportion of the other components may be, for example, about 0.01 to 10 mass % (eg, 0.05 to 5 mass %) with respect to the entire composition.

[0234] In the composition (and further in the molded article), the form (mixture) in which the polycarbonate resin (A) and the acrylic resin (B) are present is not particularly limited, and they may be either compatible or incompatible with each other. The presence or absence of compatibility may be confirmed by, for example, thermal analysis (DSC) or the like.

[0235] In addition, the composition may be a mixture that has been melt-mixed (melt-kneaded) (molten mixture), or a mixture that has not been melt-mixed (melt-kneaded) (dry blend).

[0236] As described below, the composition of the present invention can be molded without melt mixing (melt kneading). In relation to this, the composition (and further the molded article) can be constituted even if the two resins are not compatible with each other or even if the two resins are not melt mixed, and the composition can efficiently exhibit desired physical properties.

[0237] In particular, by using a composition that is not melt-mixed (or even in an incompatible state), the thermal history up to molding can be reduced as much as possible, making it easier to obtain molded articles with low coloration (and even high transparency).

[0238] The composition (resin composition) of the present invention may generally be thermoplastic (thermoplastic resin composition).

[0239] The total light transmittance of the composition (molded article) may be relatively high, depending on its constituent components, and may be, for example, 88% or more (e.g., 88.5% or more), preferably 89% or more (e.g., 89.5% or more), and more preferably 90% or more (e.g., 90.5% or more, 91% or more).

[0240] The upper limit of the total light transmittance may be 100%, or may be, for example, 99.9%, 99%, 98%, 97%, 96%, 95%, or the like.

[0241] The haze of the composition (molded body) may be relatively high, depending on its constituent components, and may be, for example, 35% or less (e.g., 30% or less), preferably 25% or less (e.g., 20% or less), and more preferably 15% or less (e.g., 12% or less, 10% or less, 8% or less, 5% or less, 4% or less, 3% or less, 2% or less, 1.5% or less).

[0242] The lower limit of the haze may be 0% (or the detection limit), and may be, for example, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, or the like.

[0243] The total light transmittance and the haze may be, for example, values ​​in a thickness of 3 mm {e.g., a sheet [sheet-shaped molded body (injection molded body)] having a thickness of 3 mm} [e.g., values ​​measured in accordance with the provisions of JIS K7361 using a turbidity meter (NDH 5000, manufactured by Nippon Denshoku Industries Co., Ltd.)], or in detail, values ​​measured by the method described below.

[0244] The yellowness index (YI) of the composition (molded product) may vary depending on its constituent components, and may be, for example, 4 or less, preferably 3.5 or less, more preferably 3 or less, or may be 2.8 or less, 2.6 or less, 2.5 or less, 2.4 or less, 2.3 or less, 2.2 or less, 2.1 or less, 2.0 or less, 1.9 or less, 1.8 or less, etc.

[0245] The lower limit of the yellowness index may be 0 (or the detection limit) or a finite value (e.g., 0.01, 0.02, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, etc.).

[0246] The yellowness index may be, for example, a value in a thickness of 3 mm {e.g., a sheet [sheet-shaped molded product (injection molded product)] having a thickness of 3 mm} [e.g., a value measured in accordance with the provisions of JIS K7373 using a spectrophotometer (Shimadzu Corporation, UV-3600) with a C2 light source and a wavelength range of 380 nm to 780 nm], or in detail, a value measured by the method described below.

[0247] The pencil hardness of the composition (molded product) may be, for example, H or higher (eg, 2H or higher), although this depends on the constituent components.

[0248] The pencil hardness may be, for example, a value in a thickness of 3 mm {e.g., a sheet [sheet-shaped molded body (injection molded body)] having a thickness of 3 mm} (e.g., a value measured in accordance with the provisions of JIS K5600-5-4:1999 using a pencil scratch hardness tester (manufactured by Yasuda Seiki Seisakusho Co., Ltd.) at a load of 750 g), or in detail, a value measured by the method described below.

[0249] The Martens hardness of the composition (molded body) varies depending on its components, but is, for example, 100 N / mm 2 or more (e.g., 105 to 250 N / mm 2 ), preferably 110N / mm 2 or more (e.g., 115 to 220 N / mm 2 ), more preferably 120N / mm 2 or more (e.g., 125N / mm 2 More than 130N / mm 2 More than 135N / mm 2 Above, 132~200N / mm 2 etc.)

[0250] The Martens hardness may be, for example, a value in a thickness of 3 mm {e.g., a sheet [sheet-shaped molded product (injection molded product)] having a thickness of 3 mm} (e.g., a value measured in accordance with the provisions of ISO-14577-1 using an ultra-microhardness tester (Fisher Scope HM-2000, manufactured by Fisher Instruments)), or in detail, a value measured by the method described below.

[0251] Photoelastic coefficient of the composition (molded body) (×10 -12 / Pa) (or its absolute value) may vary depending on the constituent components, but may be, for example, 30 or less (e.g., 28 or less), preferably 27 or less, and more preferably 26 or less (e.g., 25 or less, 22 or less, 20 or less, 18 or less, 16 or less, 15 or less, 14 or less, 13 or less, 12 or less), etc.

[0252] The photoelastic coefficient may be, for example, a value in a thickness of 100 mm {for example, a film (unstretched film, sheet) having a thickness of 100 mm}, and in detail, may be a value measured by the method described later.

[0253] The physical properties of the composition (molded article) as described above can be adjusted by selecting the composition of each resin, etc.

[0254] The composition of the present invention can usually be produced by mixing the respective components (at least the polycarbonate resin (A) and the acrylic resin (B)). The mixing method is not particularly limited and may be melt mixing (melt kneading) or non-melt mixing (dry blending, etc.), but in particular, the polycarbonate resin (A) and the acrylic resin (B) may be non-melt mixed.

[0255] Such mixing can also be performed during molding (or, for example, in a molding machine during molding). For example, the resins can be fed from two fixed quantity feeders to a hopper of a molding machine in a predetermined ratio, and blended in the molding machine (during molding).

[0256] When the composition contains other resins, the mixing of the other resins may be either melt-mixing or non-melt-mixing.

[0257] The mixing of such other resins may be carried out simultaneously when the polycarbonate resin (A) and the acrylic resin (B) are mixed, or the other resins may be mixed (melt mixed or non-melt mixed) in advance with at least one of these resins (for example, the acrylic resin (B)). In particular, when the other resin is compatible with either the resin (A) or the acrylic resin (B) and incompatible (difficult to) with the other resin or has a large difference in refractive index, the other resin may be melt-mixed with one of the resins in advance. On the other hand, if the difference in refractive index between the two resins is small, the resins may be simultaneously mixed or may be non-melt mixed.

[0258] The present invention includes a molded article comprising (or formed from) the composition.

[0259] The shape of such a molded product is not particularly limited, and may be any of a two-dimensional shape [for example, a film (or sheet)] and a three-dimensional shape (for example, a block shape).

[0260] The molded article may have the same physical properties as the composition, and the physical property values ​​can be selected from the same ranges as above.

[0261] The method for producing the molded article (molding method) can be selected depending on the shape of the molded article, and known molding methods (for example, extrusion molding, injection molding, cast molding, blow molding, foam molding, casting method, etc.) can be used.

[0262] In particular, the composition of the present invention can provide a molded article having the above-mentioned physical properties even after being subjected to melt molding (injection molding, etc.).

[0263] Therefore, the molded body may in particular be a melt molded body [injection molded body (injection molded article)].

[0264] The molded article can be used for various purposes, but since it often has excellent transparency (and even low colorability) and excellent optical properties due to the composition, it may be suitable for use in optical purposes (even as an optical component), for example.

[0265] Specific examples of applications include light guiding components, film applications [for example, protective films (optical protective films, etc.), optical films (optical sheets), etc.], lenses (optical lenses, etc.), covers (lens covers, etc.), foam (foam molded products) applications (for example, cushioning materials, heat retention / insulation materials, vibration damping materials, soundproofing materials, sealing materials, packing materials, etc.), and interior material applications [for example, interior material applications for vehicles (automobiles, etc.) such as front panels of in-vehicle displays and meter covers]. Examples of lenses (optical lenses, etc.) include Fresnel lenses, linear Fresnel lenses, lenticular lenses, flat prisms, fly's eye lenses, aspheric lenses, condenser lenses, microlenses, collimator lenses, concave lenses, convex lenses, and diffractive lenses. Examples of applications of lenses (lens components) include head-up displays, cameras (e.g., in-vehicle cameras), LIDAR devices, etc. Examples of lenses for such applications include Fresnel lenses and condenser lenses used in head-up displays, and Fresnel lenses, condenser lenses, collimator lenses, convex lenses, etc. used in LIDAR devices.

[0266] Examples of light guide members include light guides [or lighting devices, such as lamps or lights]. The light guides may be for automobiles, motorcycles, etc. The location (or application) where the light guide is provided is not particularly limited, and examples of light guides for automobiles include headlamps, tail lamps, brake lamps, side mirror lamps, and daytime running lights (DRLs).

[0267] Specific examples of the member (light guide member) include a light cover and a light guide {a light guide for a vehicle lamp [for example, a light guide for an automobile headlamp (for example, a light guide for a DRL)]}.

[0268] Examples of the protective film include protective films for substrates of various optical disks (VD, CD, DVD, MD, LD, etc.) and polarizer protective films used in polarizing plates for liquid crystal displays.

[0269] Examples of optical films (optical sheets) include retardation films, zero retardation films (in-plane and thickness direction retardation is infinitesimally small), viewing angle compensation films, light diffusion films, reflective films, anti-reflection films, anti-glare films, brightness enhancement films, conductive films for touch panels, diffusion plates, light guides, retardation plates, zero retardation plates, and prism sheets.

[0270] In particular, since the composition of the present invention can be used for melt molding methods such as injection molding, as described above, the molded article may be a molded article having a three-dimensional shape.

[0271] In particular, molded articles for optical applications (optical components) may require high transparency (and further low colorability, high surface hardness, etc.), and the composition of the present invention can be suitably used to form such molded articles.

[0272] The present invention is not limited to the above-described embodiments, and various modifications are possible. The present invention also includes embodiments obtained by appropriately combining the technical means disclosed in the different embodiments. EXAMPLES

[0273] The present invention will be described in more detail below with reference to examples, but the present invention is not limited thereto.

[0274] In the following description, unless otherwise specified, "%" means "% by mass (by weight)" and "parts" means "parts by mass (by weight)".

[0275] The measurement and evaluation of various physical properties were carried out by the following methods.

[0276] [Weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn)] The weight average molecular weight and molecular weight distribution of the resin were determined in terms of polystyrene using gel permeation chromatography (GPC) using the following apparatus and conditions: System: Tosoh GPC system HLC-8320 Measurement column configuration Guard column: Tosoh, TSKguardcolumn SuperHZ-L Separation column: Tosoh TSKgel SuperHZM-M, 2 columns connected in series Reference column configuration Reference column: Tosoh, TSKgel SuperH-RC Developing solvent: Chloroform (Wako Pure Chemical Industries, special grade) Flow rate of developing solvent: 0.6mL / min Standard sample: TSK standard polystyrene (Tosoh, PS-oligomer kit) Column temperature: 40℃

[0277] [Glass transition temperature (Tg)] The glass transition temperature was measured in accordance with the provisions of JIS K7121-1987. Specifically, a differential scanning calorimeter (Rigaku's "Thermo plus EVO DSC-8230") was used to measure the glass transition temperature by the starting point method from a DSC curve obtained by heating about 10 mg of a sample from room temperature to 200°C (heating rate 20°C / min) under a nitrogen gas atmosphere. α-alumina was used as a reference.

[0278] [Melt flow rate (MFR)] The melt flow rate was measured in accordance with JIS K 7210-1:2014 Method A at a temperature of 230°C and a load of 3.8 kg (37 N).

[0279] [Shear Viscosity] The shear viscosity was measured using a twin-bore barrel type capillary rheometer RH10 manufactured by Rosand. A long die with a diameter of 1 mm and a length of 16 mm and a short die with a diameter of 1 mm and a length of 0.25 mm were used, and the measurement was performed at a measurement temperature of 240°C and a shear rate of 1000 / s. The shear viscosity was calculated by applying Burgley correction to the values ​​obtained.

[0280] [Refractive index] The refractive index was measured on a 3 mm thick molded body using a refractometer (Atago Co., Ltd., multi-wavelength Abbe refractometer, DR-M2) in accordance with the provisions of JIS K7142:2008 Method A. The molded body was produced by drying the obtained pellets at 100°C for 12 hours or more, and then using an injection molding machine (Nissei Plastics Co., Ltd., NS40-5A) at a molding temperature of 230°C, a mold temperature of 100°C, and a mold size of 100 mm x 100 mm x 3 mm thick. The refractive index (nD) was measured at 23° C. and a wavelength of 589 nm using Atago RE-1196 (bromonaphthalene solution (nD: 1.65)) as an intermediate liquid.

[0281] [Total light transmittance (Tt)] The total light transmittance was measured on a 3 mm thick molded body using a turbidity meter (NDH 5000, manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with the provisions of JIS K7361-1: 1997. The molded body was produced by drying the obtained pellets at 100°C for 12 hours or more, and then using an injection molding machine (NS40-5A, manufactured by Nissei Plastics Co., Ltd.) at a molding temperature of 230°C, a mold temperature of 100°C, and a mold size of 100 mm x 100 mm x 3 mm thick.

[0282] [Hayes] The haze was measured on a 3 mm thick molded body using a turbidity meter ("NDH-5000" manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with the provisions of JIS K7136. The molded body was produced by drying the obtained pellets at 100°C for 12 hours or more, and then using an injection molding machine (NS40-5A manufactured by Nissei Plastics Co., Ltd.) at a molding temperature of 230°C, a mold temperature of 100°C, and a mold size of 100 mm x 100 mm x 3 mm thick.

[0283] [Yellowness (YI)] The yellowness index was measured on a 3 mm thick molded body using a spectrophotometer (Shimadzu Corporation, UV-3600) with a C2 light source and a wavelength range of 380 nm to 780 nm in accordance with the regulations of JIS K7373: 2006. The obtained pellets were dried at 100°C for 12 hours or more, and then molded using an injection molding machine (Nissei Plastics, NS40-5A) at a molding temperature of 230°C, a mold temperature of 100°C, and a mold size of 100 mm x 100 mm x 3 mm thick.

[0284] [Pencil hardness] The pencil hardness was measured on a 3 mm thick molded body under a load of 750 g using a pencil scratch hardness tester (manufactured by Yasuda Seiki Seisakusho Co., Ltd.) in accordance with JIS K5600-5-4:1999. The pellets obtained were dried at 100°C for 12 hours or more, and then molded using an injection molding machine (manufactured by Nissei Plastics Co., Ltd., NS40-5A) at a molding temperature of 230°C, a mold temperature of 100°C, and a mold size of 100 mm x 100 mm x 3 mm thick.

[0285] [Martens hardness] The Martens hardness was evaluated for a 3 mm thick molded body using an ultra-microhardness tester (Fisher Scope HM-2000, manufactured by Fisher Instruments) according to a method conforming to ISO-14577-1. The molded body was produced by drying the obtained pellets at 100°C for 12 hours or more, and then using an injection molding machine (NS40-5A, manufactured by Nissei Plastics Co., Ltd.) at a molding temperature of 230°C, a mold temperature of 100°C, and a mold size of 100 mm x 100 mm x 3 mm thick. The measurement conditions were as follows: a square pyramidal Vickers indenter (facing angle a = 136°); maximum test load 3 mN; application time when load was applied 60 seconds; creep time 5 seconds; application time when load was reduced 20 seconds; measurement temperature room temperature; and the values ​​measured three times were averaged.

[0286] [Phase difference] The in-plane retardation Re and the thickness retardation Rth were determined using a retardation film and optical material inspection device (RETS-100, manufactured by Otsuka Electronics Co., Ltd.). The thickness retardation Rth was calculated by the formula Rth = {(nx + ny) / 2 - nz} × d using the average refractive index of the molded body measured by an Abbe refractometer, the in-plane retardation Re (40 °) measured by the above device with the film tilted 40 ° with respect to the tilt axis, and the thickness d (nm) of the molded body. nx is the refractive index in the slow axis direction in the plane of the molded body, ny is the refractive index in the direction perpendicular to the slow axis direction in the plane of the molded body (fast axis direction), and nz is the refractive index in the thickness direction of the molded body. Note that Re (40 °) was the larger value selected from Re (S40 °) obtained with the slow axis as the tilt axis and Re (F40 °) obtained with the direction perpendicular to the slow axis in the plane of the molded body as the tilt axis.

[0287] [Photoelastic coefficient (Cd)] The photoelastic coefficient (Cd) was evaluated as follows. First, the resin composition to be evaluated was heat-press molded to obtain a film (unstretched film) with a thickness of 100 μm. Next, the obtained film was cut into a rectangle with a width of 7 mm to prepare a test piece. Next, the test piece was attached to a tensile tester stage installed on a retardation film / optical material inspection device (manufactured by Otsuka Electronics Co., Ltd., RETS-100) with a chuck distance of 30 mm, and the birefringence Δn for light with a wavelength of 590 nm was measured while applying an elongation stress (σR) to the test piece. The measurement temperature was 23°C, and the tensile speed (chuck movement speed) was 5 mm / min. The slope Δn / σR was calculated by the least squares method from the relationship between the measured birefringence Δn and the elongation stress (σR) applied to the test piece, and this was used as the photoelastic coefficient (Cd) of the resin composition. In addition, data in which the elongation stress σR was in the range of 2.5 MPa≦σR≦10 MPa was used to calculate Cd. Δn is Δn=|nx-ny|.

[0288] [Ratio of lactone ring structure contained in acrylic resin] First, the weight loss that occurs when all hydroxyl groups from the polymer composition obtained by polymerization are dealcoholized as methanol was used as the basis, and the dealcoholization reaction rate was calculated from the weight loss due to the dealcoholization reaction from 150°C, before weight loss began, to 300°C, before polymer decomposition began, in dynamic TG measurements. That is, in dynamic TG measurement of a polymer having a lactone ring structure, the weight loss rate is measured between 150°C and 300°C, and the actual weight loss rate obtained is designated as (X). On the other hand, based on the composition of the polymer, it is assumed that all hydroxyl groups contained in the polymer composition are involved in the formation of lactone rings and become alcohols, which are then dealcoholized, and the theoretical weight loss rate (i.e., the weight loss rate calculated on the assumption that a 100% dealcoholization reaction occurs in that composition) is designated as (Y). More specifically, the theoretical weight reduction rate (Y) can be calculated from the molar ratio of the raw material monomer having a structure (hydroxyl group) involved in the dealcoholization reaction in the polymer, i.e., the content of the raw material monomer in the polymer composition. These values ​​(X) and (Y) are used to calculate dealcoholization: 1-(Actual weight reduction rate (X) / Theoretical weight reduction rate (Y)) Substituting the value into the above equation and expressing it as a percentage gives the dealcoholization reaction rate. The ratio of lactone ring structures in the pellets obtained in Production Example 1 described below is calculated. The theoretical weight loss rate (Y) of this polymer is calculated as follows: the molecular weight of methanol is 32, the molecular weight of methyl 2-(hydroxymethyl)acrylate is 116, and the content (mass ratio) of methyl 2-(hydroxymethyl)acrylate in the polymer is 13 mass% in the composition, so that (32 / 116)×13≒3.59 mass%. On the other hand, the actual weight loss rate (X) measured by dynamic TG measurement was 0.08 mass%. Applying these values ​​to the above dealcoholization calculation formula, 1-(0.08 / 3.59)≒0.978, so the dealcoholization reaction rate is 97.8%. In the case of Production Example 1, the content of methyl 2-(hydroxymethyl)acrylate in the copolymer was 13.0% by mass, the calculated dealcoholization reaction rate was 97.8% by mass, and the formula weight of the lactone cyclized structural unit produced when methyl 2-(hydroxymethyl)acrylate having a molecular weight of 116 is condensed with methyl methacrylate is 170, so the content of lactone rings in the copolymer was 8.6 (13.0 × 0.978 × 170 / 116)% by mass.

[0289] [Acid value] The acid value was measured by the following method. First, 0.15 g of the polymer was dissolved in 24.94 g of methylene chloride. 14.85 g of methanol was added to the obtained solution and stirred for 3 hours. Next, 2 drops of a 1 wt% phenolphthalein ethanol solution were added to the solution. While stirring the obtained solution, a 0.1 N aqueous sodium hydroxide solution was added, and stirring was continued for 1 hour at room temperature. At this time, the amount of the 0.1 N aqueous sodium hydroxide solution added was defined as A ml. Next, 0.1 N hydrochloric acid was dropped into the solution. The amount of 0.1 N hydrochloric acid added until the color of the solution (red purple) disappeared was defined as B ml. Next, a mixed solution of 24.94 g of methylene chloride and 14.85 g of methanol was prepared. Two drops of a 1 wt% phenolphthalein ethanol solution were added to this mixed solution. Next, while stirring this mixed solution, a 0.1 N aqueous sodium hydroxide solution was added, and stirring was continued for one hour at room temperature. At this time, the amount of the 0.1 N aqueous sodium hydroxide solution added is defined as C ml. Next, 0.1 N hydrochloric acid was dropped into this mixed solution. The amount of 0.1 N hydrochloric acid added until the color of the mixed solution (reddish purple) disappeared is defined as D ml. The acid value (mmol / g) of the polymer was calculated from the following formula. The acid value represents the amount of sodium hydroxide required to neutralize the acid groups contained in 1 g of the polymer and the acid groups generated by hydrolysis of the acid anhydride groups. [Acid value (mmol / g)]=0.1×[(AB)-(CD)] / 0.15

[0290] (Production Example 1 [Production of Acrylic Resin (B1)]) A reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping pump was charged with 6.5 parts by mass of methyl 2-(hydroxymethyl)acrylate (RHMA), 43.5 parts by mass of methyl methacrylate (MMA), 90.7 parts by mass of toluene, and 0.05 parts by mass of tris(2,4-di-tert-butylphenyl)phosphite, and the temperature was raised to 105°C while passing nitrogen through. As an initial initiator, a solution consisting of 4.3 parts by mass of toluene and 0.22 parts by mass of t-amyl peroxy isononanoate (manufactured by Arkema Yoshitomi Co., Ltd., Luperox (registered trademark) 570) was dropped over 8 minutes, while solution polymerization was performed at 105 ° C. to 110 ° C. Then, 22 minutes later, a solution consisting of 5.0 parts by mass of toluene and 0.28 parts by mass of t-amyl peroxy isononanoate (manufactured by Arkema Yoshitomi Co., Ltd., Luperox (registered trademark) 570) was dropped over 180 minutes as a dropping initiator. In addition, 25 minutes after the initial initiator was added, a solution consisting of 6.5 parts by mass of 2-(hydroxymethyl) methyl acrylate (RHMA) and 43.5 parts by mass of methyl methacrylate (MMA) was dropped over 180 minutes, while solution polymerization was performed at 105 ° C. to 110 ° C., and further aging was performed for 1.5 hours. To the obtained polymerization solution, a solution consisting of 1.25 parts by mass of toluene and 0.075 parts by mass of stearyl phosphate (Phoslex A-18, manufactured by Sakai Chemical Industry Co., Ltd.) was added as a catalyst for the cyclization condensation reaction (cyclization catalyst), and the cyclization condensation reaction to form a lactone ring structure was allowed to proceed for 1.5 hours under reflux at approximately 90°C to 110°C. Next, the obtained polymerization solution was passed through a multi-tube heat exchanger maintained at 220°C to complete the cyclization condensation reaction, and then introduced into a vent-type screw twin-screw extruder (L / D=52) equipped with a leaf disk-type polymer filter (filtration accuracy 5μm) at the tip at a processing rate of 90 parts by mass / hour in terms of resin amount to devolatilize the polymerization solution. The number of rear vents of the vent-type screw twin-screw extruder used was 1, and the number of fore vents was 4 (referred to as the first, second, third, and fourth vents from the upstream side), the barrel temperature was 220°C, and the degree of vacuum was 13.3 to 400hPa (10 to 300mmHg). During devolatilization, ion-exchanged water was introduced from behind the first, second, and third vents at an introduction rate of 1.3 parts by mass / hour.

[0291] The weight average molecular weight of the obtained resin pellets (B1) was 88,000, the molecular weight distribution was 2.2, the glass transition temperature was 123°C, the melt flow rate was 4.5, the shear viscosity was 221 Pa s, the refractive index was 1.4974, the proportion of ring structures was 18.6 mass%, and the acid value was 0.2 mmol / g or less.

[0292] (Production Example 2 [Production of Acrylic Resin (B2)]) In a reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube and a nitrogen inlet tube, 10 parts by mass of 2-(hydroxymethyl)methyl acrylate (RHMA), 40 parts by mass of methyl methacrylate (MMA), 0.025 parts by mass of tris(2,4-di-tert-butylphenyl)phosphite and 50 parts by mass of toluene as a polymerization solvent were charged. Next, the reaction vessel was heated to 105°C while introducing nitrogen gas, and when refluxing accompanying the temperature increase began, 0.05 parts by mass of tertiary amyl peroxy isononanoate (manufactured by Arkema Yoshitomi Co., Ltd., Luperox (registered trademark) 570) was added as a polymerization initiator. At the same time, the drop of 0.10 parts by mass of the above tertiary amyl peroxy isononanoate was started, and while dropping this over 2 hours, solution polymerization was allowed to proceed under reflux at about 105 to 110°C. After the dropwise addition, the reaction vessel was heated for 4 hours to continue maturing.

[0293] Next, 0.05 parts by mass of stearyl phosphate (Phoslex A-18, manufactured by Sakai Chemical Industry Co., Ltd.) was added as a catalyst for the cyclization reaction to the polymerization solution thus obtained, and the cyclization condensation reaction to form a lactone ring structure was carried out under reflux at approximately 90°C to 110°C for 2 hours.

[0294] Next, the obtained polymerization solution was passed through a multi-tube heat exchanger maintained at 240°C to complete the cyclization condensation reaction, and then introduced into a vent-type screw twin-screw extruder (L / D=52) with a leaf disk-type polymer filter (filtration accuracy 5μm) at the tip at a processing rate of 90 parts by mass / hour in terms of resin amount to devolatilize the polymerization solution. The vent-type screw twin-screw extruder used had one rear vent and four fore vents (referred to as the first, second, third, and fourth vents from the upstream side), a side feeder was placed between the third and fourth vents, the barrel temperature was 240°C, and the vacuum degree was 13.3 to 400hPa (10 to 300mmHg). During devolatilization, ion-exchanged water was introduced from behind the second vent at a rate of 1.3 parts by mass / hour, and a solution of a cyclization catalyst deactivator that had been separately prepared was introduced from behind the third vent at a rate of 0.6 parts by mass / hour. As a solution of the cyclization catalyst deactivator, a solution in which 1.0 part by mass of zinc octylate (manufactured by Nippon Chemical Industry Co., Ltd., trade name: Nikka Octyx Zinc 10% by mass) was dissolved in 0.3 parts by mass of toluene was used.

[0295] The weight average molecular weight of the obtained resin pellets (B2) was 116,000, the molecular weight distribution was 2.6, the glass transition temperature was 130°C, the melt flow rate was 0.8, the shear viscosity was 321 Pa s, the refractive index was 1.4999, the proportion of ring structures was 28.6 mass%, and the acid value was 0.3 mmol / g or less.

[0296] (Production Example 3 [Production of Acrylic Resin (B3)] A reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping pump was charged with 11.5 parts by mass of methyl 2-(hydroxymethyl)acrylate (RHMA), 38.5 parts by mass of methyl methacrylate (MMA), 90.7 parts by mass of toluene, and 0.05 parts by mass of tris(2,4-di-tert-butylphenyl)phosphite, and the temperature was raised to 105°C while passing nitrogen through. As an initial initiator, a solution consisting of 4.3 parts by mass of toluene and 0.22 parts by mass of t-amyl peroxy isononanoate (manufactured by Arkema Yoshitomi Co., Ltd., Luperox (registered trademark) 570) was dropped over 8 minutes, while solution polymerization was performed at 105 ° C. to 110 ° C. Then, 22 minutes later, a solution consisting of 5.0 parts by mass of toluene and 0.22 parts by mass of t-amyl peroxy isononanoate (manufactured by Arkema Yoshitomi Co., Ltd., Luperox (registered trademark) 570) was dropped over 170 minutes as a dropping initiator. In addition, 25 minutes after the initial initiator was added, a solution consisting of 11.5 parts by mass of 2-(hydroxymethyl) methyl acrylate (RHMA) and 38.5 parts by mass of methyl methacrylate (MMA) was dropped over 180 minutes, while solution polymerization was performed at 105 ° C. to 110 ° C., and further aging was performed over 1.5 hours. To the obtained polymerization solution, a solution consisting of 1.25 parts by mass of toluene and 0.30 parts by mass of stearyl phosphate (Phoslex A-18, manufactured by Sakai Chemical Industry Co., Ltd.) was added as a catalyst for the cyclization condensation reaction (cyclization catalyst), and the cyclization condensation reaction to form a lactone ring structure was allowed to proceed for 2 hours under reflux at approximately 90°C to 110°C. Next, the obtained polymerization solution was passed through a multi-tube heat exchanger maintained at 240°C to complete the cyclization condensation reaction, and then introduced into a vent-type screw twin-screw extruder (L / D=52) with a leaf disk-type polymer filter (filtration accuracy 5μm) at the tip at a processing rate of 90 parts by mass / hour in terms of resin amount to devolatilize the polymerization solution. The number of rear vents of the vent-type screw twin-screw extruder used was 1, and the number of fore vents was 4 (referred to as the first, second, third, and fourth vents from the upstream side), the barrel temperature was 240°C, and the degree of vacuum was 13.3 to 400hPa (10 to 300mmHg). During devolatilization, ion-exchanged water was introduced from behind the first and third vents at a rate of 1.3 parts by mass / hour, and a mixed solution of a bluing agent and an antioxidant that had been prepared separately was introduced from behind the second vent at a rate of 0.30 parts by mass / hour. As a mixed solution of bluing agent and antioxidant, a solution consisting of 0.27 parts by mass of a solution obtained by dissolving 1.0 part by mass of bluing agent (Sumiplast (registered trademark) Violet B manufactured by Sumika Chemtex Corporation) in 99 parts by mass of toluene, 3.6 parts by mass of two types of antioxidants (Irganox 1010 manufactured by BASF Japan Ltd. and Adeka STAB AO-412S manufactured by ADEKA Corporation), and 112.5 parts by mass of toluene was used.

[0297] The weight average molecular weight of the obtained resin pellets (B3) was 85,000, the molecular weight distribution was 2.0, the glass transition temperature was 132°C, the melt flow rate was 3.1, the shear viscosity was 290 Pa s, the refractive index was 1.5004, the proportion of ring structures was 28.8 mass%, and the acid value was 0.3 mmol / g or less.

[0298] (Production Example 4 [Production of Acrylic Resin (B4)]) A reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, a nitrogen inlet tube, and a dropping pump was charged with 12 parts by mass of methyl 2-(hydroxymethyl)acrylate (RHMA), 83.5 parts by mass of methyl methacrylate, 90.4 parts by mass of toluene, 0.05 part by mass of tris(2,4-di-tert-butylphenyl)phosphite, and 0.07 part by mass of n-dodecyl mercaptan as a chain transfer agent, and the temperature was raised to 105°C while passing nitrogen through. 0.09 parts by mass of t-amyl peroxy isononanoate (Arkema Yoshitomi Co., Ltd., Luperox (registered trademark) 570) was added as an initial initiator, and 5 minutes later, a solution consisting of 4.5 parts by mass of styrene, 8.14 parts by mass of toluene, and 0.179 parts by mass of the dropping initiator t-amyl peroxy isononanoate (Arkema Yoshitomi Co., Ltd., Luperox (registered trademark) 570) was added dropwise over 2 hours while carrying out solution polymerization at 100°C to 110°C, and then aging was carried out for a further 4 hours. To the obtained polymerization solution, 0.075 parts by mass of stearyl phosphate (Phoslex A-18, manufactured by Sakai Chemical Industry Co., Ltd.) was added as a catalyst for the cyclization condensation reaction (cyclization catalyst), and the cyclization condensation reaction for forming a lactone ring structure was allowed to proceed for 1.5 hours under reflux at approximately 90°C to 110°C. Next, the obtained polymerization solution was passed through a multi-tube heat exchanger maintained at 240°C to complete the cyclization condensation reaction, and then introduced into a vent-type screw twin-screw extruder (L / D=52) with a leaf disk-type polymer filter (filtration accuracy 5μm) at the tip at a processing rate of 90 parts by mass / hour in terms of resin amount to devolatilize the polymerization solution. The number of rear vents of the vent-type screw twin-screw extruder used was 1, and the number of fore vents was 4 (referred to as the first, second, third, and fourth vents from the upstream side), the barrel temperature was 240°C, and the degree of vacuum was 13.3 to 400hPa (10 to 300mmHg). During devolatilization, ion-exchanged water was introduced from behind the first and second vents at a rate of 1.3 parts by mass / hour, and a solution of a cyclization catalyst deactivator that had been separately prepared was introduced from behind the third vent at a rate of 0.3 parts by mass / hour. As a solution of the cyclization catalyst deactivator, a solution in which 1.0 part by mass of zinc octylate (manufactured by Nippon Chemical Industry Co., Ltd., trade name: Nikka Octyx Zinc 10% by mass) was dissolved in 0.3 parts by mass of toluene was used.

[0299] The weight average molecular weight of the obtained resin pellets (B4) was 130,000, the molecular weight distribution was 2.7, the glass transition temperature was 123°C, the melt flow rate was 1.6, the shear viscosity was 262 Pa s, the refractive index was 1.5013, the proportion of ring structures was 16.9 mass%, and the acid value was 0.2 mmol / g or less.

[0300] (Production Example 5 [Production of Acrylic Resin (Acrylic Resin Composition) (B5)] The acrylic resin (B1) obtained in Production Example 1 and pellets of AS resin (styrene-acrylonitrile copolymer, styrene / acrylonitrile ratio 73% by mass / 27% by mass, weight average molecular weight 220,000) were kneaded at 240°C using a twin-screw extruder (φ=30 mm, L / D=40) to a mass ratio of B1 / AS resin = 100 / 4, to obtain resin pellets (B5). The resulting resin pellets (B5) had a weight average molecular weight of 90,000, a molecular weight distribution of 2.3, a glass transition temperature of 122°C, a melt flow rate of 4.2, a shear viscosity of 221 Pa·s, and a refractive index of 1.5002.

[0301] (Production Example 6 [Production of acrylic resin (B6)] A 30 L reaction kettle equipped with a stirrer, a temperature sensor, a cooling tube, and a nitrogen inlet tube was charged with 70 parts by mass of methyl methacrylate (MMA), 30 parts by mass of methyl 2-(hydroxymethyl)acrylate (RHMA), and 67 parts by mass of a mixed solvent (mass ratio 9:1) consisting of methyl isobutyl ketone (MIBK) and methyl ethyl ketone (MEK). Next, while flowing nitrogen into the reactor, the contents of the reactor were heated to 105°C, and after refluxing began, 0.06 parts by mass of t-amyl peroxy isononanoate (trade name: Lupasol 570, manufactured by Atofina Yoshitomi Co., Ltd.) was added as an initiator, and at the same time, an initiator solution consisting of 0.12 parts by mass of t-amyl peroxy isononanoate and 33 parts by mass of a mixed solvent of MIBK and MEK (mass ratio 9:1) was added dropwise over 3 hours, while solution polymerization was carried out under reflux (about 95 to 110°C). After the dropwise addition of the initiator solution, the mixture was further aged for 4 hours. To the obtained polymer solution, 0.2 parts by mass of an octyl phosphate / dioctyl phosphate mixture (product name: Phoslex A-8, manufactured by Sakai Chemical Industry Co., Ltd.) was added, and a cyclization condensation reaction for forming a lactone ring structure was carried out under reflux at approximately 85°C to 100°C for 2 hours. Next, the obtained polymerization solution was passed through a multi-tube heat exchanger maintained at 240°C to complete the cyclization condensation reaction, and then introduced into a vent-type screw twin-screw extruder (L / D=52) with a leaf disk-type polymer filter (filtration accuracy 5μm) at the tip at a processing rate of 90 parts by mass / hour in terms of resin amount to devolatilize the polymerization solution. The number of rear vents of the vent-type screw twin-screw extruder used was 1, and the number of fore vents was 4 (referred to as the first, second, third, and fourth vents from the upstream side), the barrel temperature was 240°C, and the degree of vacuum was 13.3 to 400hPa (10 to 300mmHg). During devolatilization, ion-exchanged water was introduced from behind the first and second vents at a rate of 1.3 parts by mass / hour, and a solution of a cyclization catalyst deactivator that had been separately prepared was introduced from behind the third vent at a rate of 0.3 parts by mass / hour. As a solution of the cyclization catalyst deactivator, a solution in which 1.0 part by mass of zinc octylate (manufactured by Nippon Chemical Industry Co., Ltd., trade name: Nikka Octyx Zinc 10% by mass) was dissolved in 0.3 parts by mass of toluene was used.

[0302] The weight average molecular weight of the obtained pellets (B6) was 127,000, the molecular weight distribution was 2.8, the glass transition temperature was 140°C, the melt flow rate was 0.5, the shear viscosity was 366 Pa s, the refractive index was 1.5041, the proportion of ring structures was 41.9 mass%, and the acid value was 0.4 mmol / g or less.

[0303] Table 1 shows a summary of the acrylic resin (or resin composition) (B) obtained in each production example. In Table 1 below, the values ​​in parentheses for the refractive index and shear viscosity of Production Example 5 are those for the composition with AS resin (acrylic resin composition).

[0304] [Table 1]

[0305] For the polycarbonate resin (A), commercially available products [polycarbonate resin with an alicyclic skeleton (Mitsubishi Chemical Corporation, Durabio, a polycarbonate resin with isosorbide and other alicyclic diols (molar ratio of approximately 50 / 50 to 70 / 30) as the dihydroxy compound) and polycarbonate resin with an aromatic skeleton (Mitsubishi Engineering Plastics Corporation, Iupilon HL4000, a polycarbonate resin with 2,2-bis(4-hydroxyphenyl)propane as the dihydroxy compound)] were used.

[0306] The details and physical properties are shown in Table 2 below.

[0307] [Table 2]

[0308] Example 1 Pellets of a polycarbonate resin (A1) having an alicyclic skeleton and the acrylic resin (B1) obtained in Production Example 1 were kneaded at 240°C using a twin-screw extruder (φ=30 mm, L / D=40) so that the mass ratio of A1 / B1 was 70 / 30, thereby obtaining resin pellets. The obtained pellets were used to produce a molded body (for example, after drying at 100°C for 12 hours or more, a molded body of 100 mm x 100 mm x 3 mm thickness was produced using an injection molding machine (NS40-5A, manufactured by Nissei Plastics Co., Ltd.) at a molding temperature of 230°C and a mold temperature of 100°C).

[0309] Example 2 Resin pellets and a molded product were produced in the same manner as in Example 1, except that the pellets of the acrylic resin (B2) obtained in Production Example 2 were used.

[0310] Example 3 Resin pellets and a molded product were produced in the same manner as in Example 1, except that the pellets of the acrylic resin (B3) obtained in Production Example 3 were used.

[0311] Example 4 Pellets of the polycarbonate resin (A2) having an alicyclic skeleton and the acrylic resin (B3) obtained in Production Example 3 were kneaded at 240°C using a twin-screw extruder (φ=30 mm, L / D=40) so that the mass ratio of A2 / B3 was 90 / 10, thereby obtaining resin pellets. The obtained pellets were used to produce a molded body (for example, after drying at 100°C for 12 hours or more, a molded body of 100 mm x 100 mm x 3 mm thickness was produced using an injection molding machine (NS40-5A, manufactured by Nissei Plastics Co., Ltd.) at a molding temperature of 230°C and a mold temperature of 100°C).

[0312] Example 5 Resin pellets and a molded body were produced in the same manner as in Example 4, except that the mass ratio of A2 / B3 was changed to 70 / 30.

[0313] Example 6 Resin pellets and a molded body were produced in the same manner as in Example 4, except that the mass ratio of A2 / B3 was changed to 50 / 50.

[0314] Example 7 Resin pellets and a molded product were produced in the same manner as in Example 3, except that pellets of the polycarbonate resin (A3) having an alicyclic skeleton were used.

[0315] Example 8 Resin pellets and a molded product were produced in the same manner as in Example 1, except that the pellets of the acrylic resin (B4) obtained in Production Example 4 were used.

[0316] Example 9 Resin pellets and a molded product were produced in the same manner as in Example 1, except that the pellets of the acrylic resin (B5) obtained in Production Example 5 were used.

[0317] Example 10 Resin pellets and a molded product were produced in the same manner as in Example 1, except that the pellets of the acrylic resin (B6) obtained in Production Example 6 were used.

[0318] (Reference example 1) In Example 1, a resin pellet and a molded body were prepared in the same manner as in Example 1, except that pellets of a commercially available acrylic resin (manufactured by Sumitomo Chemical Co., Ltd., Sumipex MH, weight average molecular weight 93,000, molecular weight distribution 2.0, glass transition temperature 110°C, melt flow rate 2.0, refractive index 1.4924) were used.

[0319] (Reference example 2) Pellets of polycarbonate resin (A4) having an aromatic skeleton and acrylic resin (B3) obtained in Production Example 3 were kneaded at 260°C using a twin-screw extruder (φ=30 mm, L / D=40) so that the mass ratio of A4 / B3 was 70 / 30. However, the resin pellets turned white, and it was not possible to obtain a molded product that could be evaluated.

[0320] (Reference example 3) A molded body (e.g., a molded body of 100 mm x 100 mm x 3 mm thickness) was produced using the polycarbonate resin (A2) having an alicyclic skeleton (e.g., after drying at 100°C for 12 hours or more, a molding temperature of 230°C and a mold temperature of 100°C was used in an injection molding machine (NS40-5A manufactured by Nissei Plastics Co., Ltd.) to produce a molded body).

[0321] (Reference example 4) The acrylic resin (B3) obtained in Production Example 3 was used to produce a molded body (for example, after drying at 100°C for 12 hours or more, a molded body of 100 mm x 100 mm x 3 mm thick was produced using an injection molding machine (NS40-5A, manufactured by Nissei Plastics Co., Ltd.) at a molding temperature of 230°C and a mold temperature of 100°C).

[0322] The evaluation results of each Example and Reference Example are shown in Table 3. In addition, in the following Table 3, the value in parentheses for the refractive index difference of Example 9 is R B is the refractive index of the composition with AS resin (acrylic resin composition).

[0323] [Table 3]

[0324] As is clear from the above table, in the examples, a resin composition could be obtained from polycarbonate resin and acrylic resin (and further from AS resin) without whitening, etc. Furthermore, such a resin composition, although a composition in which different resins are mixed, exhibits high transparency and low colorability, and a molded article (melt molded article) excellent in various physical properties (having high surface hardness, low photoelastic coefficient, low retardation expression, etc.) could be produced.

[0325] Example 11 Pellets of the polycarbonate resin having an alicyclic skeleton (A2) and the acrylic resin (B3) obtained in Production Example 3 were mixed in a pellet blender to give a weight ratio of A2 / B3 = 70 / 30, and then dried at 100°C for 12 hours or more. Then, using an injection molding machine (Nissei Plastics Co., Ltd., NS40-5A), a molded body of 100 mm x 100 mm x 3 mm thick was produced at a molding temperature of 230°C and a mold temperature of 100°C.

[0326] Example 12 A molded article was produced in the same manner as in Example 11, except that the pellets of the acrylic resin (B5) obtained in Production Example 5 were used.

[0327] The evaluation results of each Example are shown in Table 4. In addition, for comparison, Table 4 also shows the results of Example 5 for comparison with Example 11.

[0328] [Table 4]

[0329] As shown in the results in the above table, in Examples 11 and 12, as in the previously described Examples, molded articles were produced that were highly transparent, had low coloration, and were excellent in various physical properties without whitening, etc.

[0330] It was also found that the above-mentioned molded body could be obtained without using a pre-melted mixture of acrylic resin and polycarbonate resin. In particular, it was surprising that due to this specific combination of resins, not only was it possible to produce an excellent molded body, but also that a molded body with even higher transparency (and even lower colorability) could be obtained even when the resins were subjected to molding (melt molding) without being pre-melted and mixed (mixed) by pelletizing, etc. [Industrial Applicability]

[0331] According to the present invention, a novel resin composition and the like can be provided.

Claims

1. A polycarbonate resin (A) containing a polycarbonate resin (A1) having an alicyclic skeleton, and an acrylic resin (B) having a ring structure, A composition, wherein the acrylic resin (B) has at least one ring structure selected from a cyclic imide structure, a cyclic amide structure, and a cyclic ester structure.

2. The refractive index (wavelength 589 nm) R of polycarbonate resin (A) A and the refractive index of acrylic resin (B) (wavelength 589 nm) R B The composition of claim 1, wherein the absolute value of the difference between

3. The composition according to claim 1 or 2, wherein the polycarbonate resin (A1) has a structural unit derived from an alicyclic dihydroxy compound.

4. The composition according to any one of claims 1 to 3, wherein the polycarbonate resin (A1) has a structural unit derived from an alicyclic dihydroxy compound represented by the following formula (X): 【Chemistry 1】

5. 5. The composition according to claim 1, wherein the proportion of the polycarbonate resin (A1) having an alicyclic skeleton relative to the entire polycarbonate resin (A) is 30 mass % or more.

6. The composition according to any one of claims 1 to 5, wherein the polycarbonate resin (A) has a refractive index (wavelength 589 nm) of 1.540 or less.

7. 7. The composition according to claim 1, wherein the polycarbonate resin (A) has a glass transition temperature of 90 to 140° C. and a melt flow rate of 5 to 25 g / 10 min at 230° C. under a load of 3.8 kg.

8. The composition according to any one of claims 1 to 7, wherein the acrylic resin (B) has a cyclic ester structure.

9. The composition according to any one of claims 1 to 8, wherein the acrylic resin (B) has a glass transition temperature of 115°C or higher.

10. The composition according to any one of claims 1 to 9, wherein the acrylic resin (B) has a melt flow rate of 0.5 to 8 g / 10 min at 230°C under a load of 3.8 kg and a weight average molecular weight of 50,000 to 200,000.

11. The composition according to any one of claims 1 to 10, wherein the refractive index (wavelength 589 nm) of the acrylic resin (B) is 1.492 to 1.

510.

12. The composition according to any one of claims 1 to 11, wherein the mass ratio of the polycarbonate resin (A) to the acrylic resin (B) is 30 / 70 to 97 / 3.

13. the polycarbonate resin (A) has a refractive index (wavelength 589 nm) of 1.520 or less and contains a polycarbonate resin (A1) having an alicyclic skeleton in a proportion of 30% by mass or more; The acrylic resin (B) has a refractive index (wavelength 589 nm) of 1.494 or more and a glass transition temperature of 120° C. or more, Refractive index of polycarbonate resin (A) (wavelength 589 nm) R A and the refractive index of acrylic resin (B) (wavelength 589 nm) R B The absolute value of the difference between The composition according to any one of claims 1 to 12, wherein the mass ratio of the polycarbonate resin (A) to the acrylic resin (B) is 40 / 60 to 95 / 5.

14. The composition according to any one of claims 1 to 13, which is not melt-kneaded.

15. A molded article comprising the composition according to any one of claims 1 to 14.

16. The molded article according to claim 15, which is an optical component.

17. Total light transmittance is 89% or more, haze is 20% or less, pencil hardness is H or more, and photoelastic coefficient is 26×10 -12 The composition or molded article according to any one of claims 1 to 16, wherein the viscosity is 1 / Pa or less.

18. A method for producing a molded article, comprising a step of melt molding the composition according to any one of claims 1 to 14.

19. 20. The method according to claim 18, wherein at least the polycarbonate resin (A) and the acrylic resin having a ring structure (B) are mixed without melting to obtain a composition, and the composition is subjected to melt molding.

Citation Information

Patent Citations

  • Thermoplastic resin composition excellent in transparency and antistatic properties

    JP1994100747A

  • Solar cell module

    JP2014068003A

  • Thermoplastic resin composition having scratch resistance and molded article thereof

    JP2014080525A

  • Thermoplastic resin composition and molded article using the same

    JP2017226818A

  • Automobile interior and exterior member and ship outer machine component

    JP2018095789A

Cited By

  • Resin composition

    JP2023124741A