CURABLE COMPOSITION AND CURED PRODUCT OF CURABLE COMPOSITION

A curable composition with specific monomers and a radical polymerization initiator addresses the issue of insufficient bending strength and cracking in epoxy resin compositions, providing a robust encapsulation for optical semiconductor devices.

JP7572284B2Active Publication Date: 2024-10-23SANYO CHEM IND LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021052058
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-30
Filing Date
2021-03-25
Publication Date
2024-10-23
Estimated Expiration
2041-03-25

AI Technical Summary

Technical Problem

Existing epoxy resin compositions for encapsulating optical semiconductor devices suffer from insufficient bending strength and cracking during heat cycle tests, particularly in thick films.

Method used

A curable composition comprising a radically polymerizable monomer, a bifunctional (meth)acrylate monomer with a ring structure, and a monofunctional (meth)acrylate monomer with a ring structure, in specific ratios, along with a radical polymerization initiator, to enhance bending strength and prevent cracking.

Benefits of technology

The cured product exhibits excellent bending strength and flexibility without cracking, even in thick films, making it suitable for electronic component encapsulation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572284000001
    Figure 0007572284000001
  • Figure 0007572284000002
    Figure 0007572284000002
  • Figure 0007572284000003
    Figure 0007572284000003
Patent Text Reader

Abstract

To provide a cured product that can be cured without cracking even when it is thick, and has excellent bending strength.SOLUTION: A curable composition contains an α-(unsaturated alkoxyalkyl) acrylate (A) represented by a specific general formula, a bifunctional (meth)acrylate monomer (B) having a ring structure, a monofunctional (meth)acrylate monomer having a ring structure (C), and a radical polymerization initiator (D). The ratio [(B+C) / A] between the total weight of the (B) and the (C) and the weight of the (A) is 3-19.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a curable composition and a cured product of the curable composition. [Background technology]

[0002] In epoxy resin compositions for sealing optical semiconductor elements, liquid epoxy compounds having an alicyclic skeleton with good transparency and heat resistance are often used. However, alicyclic epoxy compounds have a problem with toughness, and cracks occur in heat cycle tests, which reduces the reliability of electronic components. As a proposal to improve such problems, for example, a resin composition that imparts toughness by combining an alicyclic epoxy resin with a specific acrylic monomer (or polymer) having an alicyclic epoxy group is known (see, for example, Patent Document 1). Furthermore, as a means of imparting toughness to epoxy resins, an acrylic polymer-dispersed alicyclic epoxy resin composition is known in which a polymer of a (meth)acrylic acid ester monomer is dispersed in an epoxy resin solvent having an alicyclic skeleton by a polymer of a (meth)acrylic acid ester monomer having an alicyclic epoxy skeleton (see, for example, Patent Document 2).

[0003] However, the bending strength of the cured product of the epoxy resin composition for sealing optical semiconductors described in Patent Document 1 is not sufficiently high. Also, the bending strength of the alicyclic epoxy resin composition described in Patent Document 2 is not sufficiently high. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2007-320974 A [Patent Document 2] Japanese Patent Application Publication No. 7-188385 Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a cured product which can be cured without cracking even in the case of a thick film and which has excellent bending strength. [Means for solving the problem]

[0006] The present inventors conducted research aimed at achieving the above object and arrived at the present invention. That is, the present invention relates to a curable composition containing a radical polymerizable monomer (A) represented by the following general formula (1), a bifunctional (meth)acrylate monomer (B) having a ring structure, a monofunctional (meth)acrylate monomer (C) having a ring structure, and a radical polymerization initiator (D), wherein the ratio of the total weight of (B) and (C) to the weight of (A) [(B+C) / A] is 3 to 19. [ka] [In formula (1), R 1 R represents a hydrogen atom or an organic group having 1 to 30 carbon atoms. 2 , R 3 , R 4 , R 5 and R 6 are each independently a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.] Effect of the Invention

[0007] The curable composition of the present invention can be cured to a thick film without cracking, and has excellent bending strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The curable composition of the present invention contains a radical polymerizable monomer (A) represented by the following general formula (1), a bifunctional (meth)acrylate having a ring structure (B), a monofunctional (meth)acrylate having a ring structure (C), and a radical polymerization initiator.

[0009] (A) is a radically polymerizable α-(unsaturated alkoxyalkyl) acrylate represented by the following general formula (1).

[0010] [ka]

[0011] In formula (1), R 1 R represents a hydrogen atom or an organic group having 1 to 30 carbon atoms. 2 , R 3 , R 4 , R 5 and R 6 are each independently a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.

[0012] R 2 ~R 6 When the alkyl group is an alkyl group, the alkyl group may be linear or branched. Specific examples thereof include a methyl group, an ethyl group, a propyl group, a butyl group, an amyl group, a neopentyl group, and a hexyl group.

[0013] A preferred embodiment of the α-(unsaturated alkoxyalkyl)acrylate represented by the general formula (1) is R 5 and R 6 is a hydrogen atom, and a more preferred embodiment is a compound represented by the following general formula (2): 2 ~R 6 In the case of α-(allyloxymethyl)acrylate, all of the above are hydrogen atoms.

[0014] [ka]

[0015] Above R 1 When is an organic group having 1 to 30 carbon atoms, the organic group may be linear, branched, or cyclic. From the viewpoint of bending strength, the organic group preferably has 1 to 18 carbon atoms, more preferably 1 to 12, and even more preferably 1 to 8. Examples of the organic group include organic groups having a hydrocarbon skeleton or a hydrocarbon skeleton containing an ether bond. The hydrocarbon skeleton may have a substituent.

[0016] Examples of the hydrocarbon skeleton include linear saturated hydrocarbon groups (e.g., methyl, ethyl, propyl, butyl, amyl, neopentyl, hexyl, octyl, 2-ethylhexyl, etc.), alicyclic hydrocarbon groups (e.g., cyclohexyl, cyclohexylmethyl, isobornyl, adamantyl, dicyclopentanyl, dicyclopentenyl, etc.), and aromatic hydrocarbon groups (e.g., phenyl, benzyl, naphthyl, anthranyl, etc.). These groups may have a substituent. A linear saturated hydrocarbon group that may have a substituent is preferred.

[0017] Examples of the organic group having a hydrocarbon skeleton containing an ether bond include those having a structure in which an oxygen atom is inserted into at least one carbon-carbon bond constituting the chain saturated hydrocarbon group (e.g., methyl group, ethyl group, propyl group, butyl group, amyl group, neopentyl group, hexyl group, octyl group, 2-ethylhexyl group, etc.), alicyclic hydrocarbon group (e.g., cyclohexyl group, cyclohexylmethyl group, isobornyl group, adamantyl group, dicyclopentanyl group, dicyclopentenyl group, etc.), and aromatic hydrocarbon group (e.g., phenyl group, benzyl group, naphthyl group, anthranyl group, etc.).

[0018] Examples of the substituent include halogen atoms such as a fluorine atom, a chlorine atom, a bromine atom and an iodine atom, a cyano group, a trimethylsilyl group and a hydroxyl group.

[0019] Suitable examples of such organic groups include linear saturated hydrocarbon groups having an ether bond, such as a methoxyethyl group, a methoxyethoxyethyl group, and an ethoxyethyl group; linear alicyclic hydrocarbon groups having an ether bond, such as a cyclohexyloxyethyl group and a dicyclopentenyloxyethyl group; linear aromatic aliphatic hydrocarbon groups having an ether bond, such as a phenoxyethyl group and a phenoxyethoxyethyl group; and cyclic ether groups, such as a glycidyl group, a 3,4-epoxycyclohexylmethyl group, a tetrahydrofuranyl group, and a tetrahydrofurfuryl group, but are not limited to these.

[0020] Therefore, specific examples of the α-(allyloxymethyl)acrylate compound include the following compounds: α-allyloxymethylacrylic acid, methyl α-allyloxymethylacrylate, ethyl α-allyloxymethylacrylate, n-propyl α-allyloxymethylacrylate, i-propyl α-allyloxymethylacrylate, n-butyl α-allyloxymethylacrylate, s-butyl α-allyloxymethylacrylate, t-butyl α-allyloxymethylacrylate, n-pentyl α-allyloxymethylacrylate, s-pentyl α-allyloxymethylacrylate, t-pentyl α-allyloxymethylacrylate, neopentyl α-allyloxymethylacrylate, n-hexyl α-allyloxymethylacrylate, s-hexyl α-allyloxymethylacrylate, n-heptyl α-allyloxymethylacrylate, n-octyl α-allyloxymethylacrylate, s-octyl α-allyloxymethylacrylate, α- Examples of α-(allyloxymethyl)acrylates containing a chain saturated hydrocarbon group include t-octyl allyloxymethylacrylate, 2-ethylhexyl α-allyloxymethylacrylate, nonyl α-allyloxymethylacrylate, decyl α-allyloxymethylacrylate, undecyl α-allyloxymethylacrylate, lauryl α-allyloxymethylacrylate, tridecyl α-allyloxymethylacrylate, myristyl α-allyloxymethylacrylate, pentadecyl α-allyloxymethylacrylate, cetyl α-allyloxymethylacrylate, heptadecyl α-allyloxymethylacrylate, stearyl α-allyloxymethylacrylate, nonadecyl α-allyloxymethylacrylate, eicosyl α-allyloxymethylacrylate, ceryl α-allyloxymethylacrylate, and melissyl α-allyloxymethylacrylate.

[0021] Hydroxy-substituted linear saturated hydrocarbon group-containing α-(allyloxymethyl)acrylates such as hydroxyethyl α-allyloxymethylacrylate, hydroxypropyl α-allyloxymethylacrylate, and hydroxybutyl α-allyloxymethylacrylate; halogen-substituted linear saturated hydrocarbon group-containing α-(allyloxymethyl)acrylates such as fluoroethyl α-allyloxymethylacrylate, difluoroethyl α-allyloxymethylacrylate, chloroethyl α-allyloxymethylacrylate, dichloroethyl α-allyloxymethylacrylate, bromoethyl α-allyloxymethylacrylate, and dibromoethyl α-allyloxymethylacrylate.

[0022] Alicyclic hydrocarbon group-containing α-(allyloxy)methylacrylates such as cyclopentyl α-allyloxymethylacrylate, cyclopentylmethyl α-allyloxymethylacrylate, cyclohexyl α-allyloxymethylacrylate, cyclohexylmethyl α-allyloxymethylacrylate, 4-methylcyclohexyl α-allyloxymethylacrylate, 4-t-butylcyclohexyl α-allyloxymethylacrylate, tricyclodecanyl α-allyloxymethylacrylate, isobornyl α-allyloxymethylacrylate, adamantyl α-allyloxymethylacrylate, dicyclopentanyl α-allyloxymethylacrylate, and dicyclopentenyl α-allyloxymethylacrylate. methyl)acrylates; aromatic hydrocarbon group-containing α-(allyloxymethyl)acrylates such as phenyl α-allyloxymethylacrylate, methylphenyl α-allyloxymethylacrylate, dimethylphenyl α-allyloxymethylacrylate, trimethylphenyl α-allyloxymethylacrylate, 4-t-butylphenyl α-allyloxymethylacrylate, benzyl α-allyloxymethylacrylate, diphenylmethyl α-allyloxymethylacrylate, diphenylethyl α-allyloxymethylacrylate, triphenylmethyl α-allyloxymethylacrylate, naphthyl α-allyloxymethylacrylate, and anthranyl α-allyloxymethylacrylate.

[0023] α-(allyloxymethyl)acrylates containing a chain-like saturated hydrocarbon group having a chain-like ether bond, such as methoxyethyl α-allyloxymethylacrylate, methoxyethoxyethyl α-allyloxymethylacrylate, methoxyethoxyethoxyethyl α-allyloxymethylacrylate, 3-methoxybutyl α-allyloxymethylacrylate, ethoxyethyl α-allyloxymethylacrylate, and ethoxyethoxyethyl α-allyloxymethylacrylate; α-(allyloxymethyl)acrylates containing an alicyclic hydrocarbon group having a chain-like ether bond, such as cyclopentoxyethyl α-allyloxymethylacrylate, cyclohexyloxyethyl α-allyloxymethylacrylate, cyclopentoxyethoxyethyl α-allyloxymethylacrylate, cyclohexyloxyethoxyethyl α-allyloxymethylacrylate, and dicyclopentenyloxyethyl α-allyloxymethylacrylate; phenoxyethyl α-allyloxymethylacrylate, α-allyloxymethylacrylate, aromatic aliphatic hydrocarbon group-containing α-(allyloxymethyl)acrylates having a chain ether bond, such as phenoxyethoxyethyl dimethylacrylate; and cyclic ether group-based saturated hydrocarbon group-containing α-(allyloxymethyl)acrylates, such as glycidyl α-allyloxymethylacrylate, β-methylglycidyl α-allyloxymethylacrylate, β-ethylglycidyl α-allyloxymethylacrylate, 3,4-epoxycyclohexylmethyl α-allyloxymethylacrylate, 2-oxetanemethyl α-allyloxymethylacrylate, 3-methyl-3-oxetanemethyl α-allyloxymethylacrylate, 3-ethyl-3-oxetanemethyl α-allyloxymethylacrylate, tetrahydrofuranyl α-allyloxymethylacrylate, tetrahydrofurfuryl α-allyloxymethylacrylate, tetrahydropyranyl α-allyloxymethylacrylate, dioxazolyl α-allyloxymethylacrylate, and dioxanyl α-allyloxymethylacrylate.

[0024] Such α-(unsaturated alkoxyalkyl)acrylates can be produced, for example, by the method disclosed in WO 2010 / 114077.

[0025] The bifunctional (meth)acrylate monomer (B) having a ring structure may be a bifunctional (meth)acrylate monomer having an alicyclic structure and / or an aromatic ring structure in a portion other than the (meth)acryloyl group. The alicyclic structure may be an alicyclic hydrocarbon group (e.g., a cyclohexyl group, a cyclohexylmethyl group, an isobornyl group, an adamantyl group, a dicyclopentanyl group, a dicyclopentenyl group, etc.). The aromatic ring structure may be an aromatic hydrocarbon group (e.g., a phenyl group, a benzyl group, a naphthyl group, an anthranyl group, etc.). These groups may have a substituent. From the viewpoint of bending strength, the aromatic hydrocarbon group is preferably an aromatic ring structure.

[0026] Specific examples of the bifunctional (meth)acrylate monomer (B) having a ring structure include di(meth)acrylate of an alkylene oxide adduct of bisphenol A, di(meth)acrylate of an alkylene oxide adduct of 9,9-bis(4-hydroxyphenyl)fluorene, dimethyloltricyclodecane di(meth)acrylate, di(meth)acrylate of an alkylene oxide adduct of bisphenol F, di(meth)acrylic acid adduct of diglycidyl ether of bisphenol A, di(meth)acrylic acid adduct of diglycidyl ether of bisphenol F, and di(meth)acrylic acid adduct of diglycidyl ether of 9,9-bis(4-hydroxyphenyl)fluorene. Examples of the alkylene oxide in the alkylene oxide adduct include ethylene oxide (hereinafter also referred to as EO), propylene oxide (hereinafter also referred to as PO), butylene oxide, etc. Among these alkylene oxides, EO and PO are preferred from the viewpoint of the bending strength and bending modulus of the cured product. The number of moles of alkylene oxide added in the alkylene oxide adduct is, from the viewpoint of the bending strength and bending modulus of the cured product, 2 to 10 moles, more preferably 2 to 6 moles, and particularly preferably 2 to 4 moles per molecule.

[0027] The monofunctional (meth)acrylate monomer (C) having a ring structure may be a monofunctional (meth)acrylate monomer having an alicyclic structure and / or an aromatic ring structure in a portion other than the (meth)acryloyl group. The alicyclic structure may be an alicyclic hydrocarbon group (e.g., a cyclohexyl group, a cyclohexylmethyl group, an isobornyl group, an adamantyl group, a dicyclopentanyl group, a dicyclopentenyl group, etc.). The aromatic ring structure may be an aromatic hydrocarbon group (e.g., a phenyl group, a benzyl group, a naphthyl group, an anthranyl group, etc.). These groups may have a substituent. From the viewpoint of bending strength, the aromatic hydrocarbon group is preferably an aromatic ring structure.

[0028] Specific examples of the monofunctional (meth)acrylate monomer (C) having a ring structure include phenyl (meth)acrylate, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxy 2-methylethyl (meth)acrylate, phenoxyethoxyethyl (meth)acrylate, o-phenylphenyloxymethyl (meth)acrylate, p-phenylphenyloxymethyl (meth)acrylate, o-phenylphenyloxyethyl (meth)acrylate, p-phenylphenyloxyethyl (meth)acrylate, acrylate, biphenyl methyl (meth)acrylate, naphthyl methyl (meth)acrylate, para-cumyl phenoxyethyl (meth)acrylate, phenoxybenzyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, phenylbenzyl (meth)acrylate, phenylphenoxyethyl (meth)acrylate, 2-(meth)acryloyloxyethyl hexahydrophthalate, and mono(meth)acrylate compounds such as fluorene skeleton-containing mono(meth)acrylate compounds.

[0029] Examples of the radical polymerization initiator (D) include benzoin compounds (D1), acetophenone compounds (D2), anthraquinone compounds (D3), thioxanthone compounds (D4), ketal compounds (D5), benzophenone compounds (D6), phosphine oxides (D7), ketal compounds (D8), α-aminoalkylphenone compounds (D9), oxime ester compounds (D10), organic peroxides (D11), and azo initiators (D12). (D) may be used alone or in combination of two or more kinds. Generally, (D1) to (D10) are called photopolymerization initiators, and (D11) to (D12) are called thermal polymerization initiators.

[0030] Examples of the benzoin compound (D1) include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzoin isobutyl ether, 2-hydroxy-2-methyl-1-phenylpropan-1-one, and 1-hydroxycyclohexyl phenyl ketone.

[0031] Examples of the acetophenone compound (D2) include acetophenone, 2,2-diethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 2-hydroxy-2-methyl-phenylpropan-1-one, diethoxyacetophenone, 1-hydroxycyclohexyl phenyl ketone, and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one.

[0032] Examples of the anthraquinone compound (D3) include 2-ethylanthraquinone, 2-t-butylanthraquinone, 2-chloroanthraquinone, and 2-amylanthraquinone.

[0033] Examples of the thioxanthone compound (D4) include 2,4-diethylthioxanthone, 2-isopropylthioxanthone, and 2-chlorothioxanthone.

[0034] Examples of the ketal compound (D5) include acetophenone dimethyl ketal and benzyl dimethyl ketal.

[0035] Examples of the benzophenone compound (D6) include benzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, and 4,4'-bismethylaminobenzophenone.

[0036] Examples of the phosphine oxide (D7) include 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide.

[0037] The ketal compound (D8) may, for example, benzyl dimethyl ketal.

[0038] Examples of the α-aminoalkylphenone compounds (D9) include 2-methyl-1-(4-methylthiophenyl)-2-morpholinopro-butanone-1 and 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone].

[0039] Examples of the oxime ester compound (D10) include 1,2-octanedione, 1-[4-(phenylthio)-,2-(O-benzoyloxime)], and ethanone-1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-1-(O-acetyloxime).

[0040] Organic peroxides (D11) include 1,1-bis(t-butylperoxy)2-methylcyclohexane, 1,1-bis(t-hexylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(t-hexylperoxy)cyclohexane, 1,1-bis(t-butylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(t-butylperoxy)cyclohexane, 2,2-bis(4,4-dibutylperoxycyclohexyl)propane, 1,1-bis(t-butylperoxy)cyclohexane, -oxy)cyclododecane, dilauroyl peroxide, t-hexylperoxyisopropyl monocarbonate, t-butylperoxymaleic acid, t-butylperoxy-3,5,5-trimethylhexanoate, t-butylperoxylaurate, t-butylperoxypivalate, t-hexylperoxypivalate, 2,5-dimethyl-2,5-di(m-toluoylperoxy)hexane, t-butylperoxyisopropyl monocarbonate, t-butylperoxy 2-ethylhexyl Monocarbonate, t-hexyl peroxybenzoate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, t-butyl peroxyacetate, 2,2-bis(t-butylperoxy)butane, t-butyl peroxybenzoate, n-butyl-4,4-bis(t-butylperoxy)valerate, di-t-butylperoxyisophthalate, α,α'-bis(t-butylperoxy)diisopropylbenzene, dicumyl peroxide, 2,5-dimethyl-2,5-di(t-butyl Examples of suitable peroxides include 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, t-butylcumyl peroxide, di-t-butyl peroxide, p-menthane hydroperoxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3, diisopropylbenzene hydroperoxide, t-butyltrimethylsilyl peroxide, 1,1,3,3-tetramethylbutyl hydroperoxide, cumene hydroperoxide, t-hexyl hydroperoxide, and t-butyl hydroperoxide.

[0041] Examples of the azo initiator (D12) include 1,1'-azobis(cyclohexane-1-carbonitrile), 2-(carbamoylazo)isobutyronitrile, 2-phenylazo-4-methoxy-2,4-dimethylvaleronitrile, azodi-t-octane, and azodi-t-butane.

[0042] These may be used alone or in combination of two or more. The organic peroxide may be combined with a reducing agent to cause a redox reaction. Among these radical polymerization initiators (D), the thermal polymerization initiators (D11) and (D12) are preferred from the viewpoint of improving strength due to uniformity of the reaction. Of the thermal polymerization initiators (D11) to (D12), (D12) is preferred from the viewpoint of preventing a decrease in bending strength due to foaming during curing, and from the viewpoint of improving reactivity, n-butyl-4,4-bis(t-butylperoxy)valerate and 1,1,3,3-tetramethylbutyl hydroperoxide.

[0043] The content of the radical polymerizable monomer (A) of the present invention is preferably 5 to 25% by weight, more preferably 10 to 25% by weight, and particularly preferably 10 to 20% by weight, based on the total weight of (A), (B) and (C) from the viewpoint of bending strength. The content of the bifunctional (meth)acrylate monomer (B) having a ring structure of the present invention is preferably 35 to 70% by weight, more preferably 35 to 65% by weight, and particularly preferably 50 to 65% by weight, based on the total weight of (A), (B) and (C) from the viewpoint of bending strength. The content of the monofunctional (meth)acrylate monomer (C) having a ring structure of the present invention is preferably 10 to 40% by weight, more preferably 15 to 40% by weight, and particularly preferably 20 to 35% by weight, based on the total weight of (A), (B) and (C), from the viewpoint of bending strength.

[0044] In the present invention, the ratio of the total weight of (B) and (C) to the weight of (A) [(B+C) / A] is 3 to 19, preferably 3 to 13, more preferably 3.5 to 10, and particularly preferably 4 to 6. If the ratio of the total weight of (B) and (C) to the weight of (A) is less than 3, there is a problem that the flexural modulus decreases and sufficient flexural strength cannot be obtained, whereas if it exceeds 19, there is a problem that although the flexural modulus is high, sufficient flexural strength cannot be obtained because toughness decreases.

[0045] The content of the thermal polymerization initiator (D) of the present invention is preferably 0.3 to 1.5% by weight, more preferably 0.3 to 1.0% by weight, and particularly preferably 0.3 to 0.7% by weight, based on the total weight of (A), (B) and (C) from the viewpoint of bending strength.

[0046] The curable resin composition of the present invention may contain, as necessary, at least one additive (e) selected from the group consisting of a flame retardant (e1), an antioxidant (e2), an ultraviolet absorber (e3) and an inorganic filler (e4), within a range that does not impair the effects of the present invention.

[0047] Examples of the flame retardant (e1) include phosphorus-based flame retardants, nitrogen-based flame retardants, silicone-based flame retardants, inorganic flame retardants, and organic metal salt-based flame retardants.

[0048] Antioxidants (e2) include di-t-butylhydroxytoluene (BHT), 2,4-bis-(n-octylthio)-6-(4-hydroxy-3,5-di-t-butylanilino)-1,3,5-triazine, pentaerythrityl tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 2,2-thio-diethylenebis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], triethylene glycol-bis[3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate], 1,6-hexanediol-bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], propionate], octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, N,N'-hexamethylenebis(3,5-di-t-butyl-4-hydroxy-hydrocinnamamide), 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, tris-(3,5-di-t-butyl-4-hydroxybenzyl)isocyanurate, octylated diphenylamine, 2,4,-bis[(octylthio)methyl]-O-cresol, isooctyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, and dibutylhydroxytoluene.

[0049] Examples of the ultraviolet absorber (e3) include 2-(2-hydroxy-5-methyl)benzotriazole, 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl]-2H-benzotriazole, 2-(2'-hydroxy-5'-t-butylphenyl)benzotriazole, 2-(2'-hydroxy-3'-t-butyl-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-t-butylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-t-butylphenyl)-5-chlorobenzotriazole, 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol, and 2-(2'-hydroxy-3',5'-t-pentylbenzotriazole. Examples of the benzotriazole include 2-[2'-hydroxy-5'-(1,1,3,3-tetramethylbutyl)]benzotriazole, 2-(2'-hydroxy-3'-s-butyl-5'-t-butylbenzotriazole, 2-(2'-hydroxy-3-dodecyl-5'-methylbenzotriazole, 2-(2'-hydroxy-3'-t-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2,2-methylenebis[4-(1,1,3,3-tetramethylbutyl)]-6-(2H-benzotriazol-2-yl)phenol], 3-[3-(2H-benzotriazol-2-yl)-5-t-butyl-4-hydroxyphenyl]propionate, and polyethylene glycol.

[0050] Examples of the inorganic filler (e4) include silica, alumina, glass, and compounds obtained by introducing an acryloyl group or a methacryloyl group into these to impart reactivity to active energy rays.

[0051] The curable composition of the present invention can be produced, for example, by uniformly mixing the radical polymerizable monomer (A) represented by general formula (1), the bifunctional (meth)acrylate monomer (B) having a ring structure, the monofunctional (meth)acrylate monomer (C) having a ring structure, and the radical polymerization initiator (D), as well as the other additives described above, as necessary, using a known mechanical mixing method (a method using a mechanical stirrer, a magnetic stirrer, or the like).

[0052] The curable composition of the present invention can be cured to produce a cured product. A method for producing a cured product by curing the curable composition of the present invention will be described below. A method for producing a cured product using the curable composition of the present invention is not particularly limited, but the product can be obtained by thermally curing the curable composition using a mold and releasing it from the mold.

[0053] More specifically, the method for producing the cured product may be the following method. A frame made of silicon spacers is placed on the glass, and the obtained curable composition is cast therein. The film thickness is preferably 1 to 20 mm, more preferably 1 to 5 mm, from the viewpoints of suppressing cracks due to cure shrinkage and resin deterioration due to heat generation during cure. After leaving it for a certain period of time under nitrogen pressure (0.3 MPa) at 20 to 30°C, it can be cured by heating at 70 to 150°C while still under pressure. From the viewpoints of suppressing cure shrinkage and preventing resin deterioration due to heat generation during cure, it is preferable that the curing temperature is 70 to 120°C at the beginning of the reaction, and then 130 to 150°C. The curing time can be adjusted as needed, and can usually be 5 to 10 hours at the beginning of the reaction, and about 7 to 10 hours after the temperature rise. After curing, it is released from the mold to obtain a resin cured product. EXAMPLES

[0054] The present invention will be further described below with reference to examples and comparative examples, but the present invention is not limited to these.

[0055] <Production Example 1> In a reactor equipped with a stirrer, a cooling tube, a thermometer, and a gas inlet tube, 198.4 parts by weight of tetrahydrofurfuryl alcohol (THFOH), 100.1 parts by weight of AOMA (methyl α-allyloxymethyl acrylate, manufactured by Nippon Shokubai Co., Ltd.), 10.9 parts by weight of titanium tetrabutoxide, and 0.10 parts by weight of 4H-TEMPO (4-hydroxy-2,2,6,6-tetramethylpiperidine-1-oxyl) were charged, and while stirring, oxygen / nitrogen mixed gas (oxygen concentration 8%) was passed through, and the temperature was raised to 100°C and reacted for 14 hours. After the reaction was completed, analysis by gas chromatography showed that the area ratio of α-allyloxymethyl tetrahydrofurfuryl acrylate (THF-AMA):AOMA:tetrahydrofurfuryl alcohol was 24:11:51. In addition, α-allyloxymethyl acrylate n-butyl (nBu-AMA) was contained as an impurity derived from the catalyst at 15 area % relative to THF-AMA. The reaction liquid was diluted with n-hexane, water was added, and the titanium compound was precipitated and removed by filtration. The filtrate was separated into oil and water, and water was added to the obtained organic layer, stirred thoroughly, left to stand, and oil and water were separated, and the remaining tetrahydrofurfuryl alcohol was removed to the water layer side. 0.15 parts by weight of 4H-TEMPO was added to the obtained organic layer, and the mixture was charged into a reactor equipped with a stirrer, a temperature sensor, a gas inlet tube, a T-shaped tube, a cooling tube, and a distillate receiver, and while stirring, oxygen / nitrogen mixed gas (oxygen concentration 8%) was passed through, and the pressure in the reactor was gradually reduced until it reached 400 Pa. After reaching 400 Pa, the temperature was gradually raised, and the remaining AOMA was removed until the internal temperature reached 80°C. Then, it was cooled and decompressed. The obtained liquid was diluted with n-hexane, water was added, stirred thoroughly, left to stand, and oil and water were separated. This operation was repeated three times, and 4H-TEMPO was removed. The obtained organic layer was charged into a reactor equipped with a stirrer, a temperature sensor, a gas inlet tube, an U-shaped tube, a cooling tube, and a distillate receiver, and while stirring, oxygen / nitrogen mixed gas (oxygen concentration 8%) was passed through and heated to an internal temperature of 25-30° C., while slowly reducing the pressure to 800 Pa to remove n-hexane. After reaching 800 Pa, the pressure was maintained for 20 minutes and then released, yielding 70.0 parts by weight of the target compound, THF-AMA (A-2).0.021 parts by weight of p-methoxyphenol was added to the obtained THF-AMA (A-2) so that the concentration of p-methoxyphenol was adjusted to 300 ppm.

[0056] Examples 1 to 7 and 9 to 13, Comparative Examples 1 to 7 The ingredients were mixed together in accordance with the composition (parts by weight) shown in Table 1 and stirred with a disperser until homogenous, to obtain curable compositions (X-1) to (X-7), (X-9) to (X-13), and (Z-1) to (Z-7). Next, a frame of 20 mm length x 60 mm width x 3 mm height made of silicon spacers was placed on the glass, and each of the obtained curable compositions was cast therein. The mixture was left to stand at 30°C under nitrogen pressure (0.3 MPa) for 15 hours. After that, the mixture was heated to 110°C while still under pressure, and held for 10 hours, and further held at 130°C for 8 hours. The mixture was then removed from the mold to obtain a cured product.

[0057] Example 8 In a reactor equipped with a stirrer, a temperature sensor, a gas inlet tube, a T-shaped tube, a cooling tube, and a distillate receiver, 30.0 parts by weight of phenoxybenzyl methacrylate and 71.4 parts by weight of a propylene glycol monomethyl ether acetate (PGMEA) solution (evaporation residue 70% by weight) of methacrylic acid adduct of 9,9-bis(4-hydroxyphenyl)fluorenediglycidyl ether (FGDA) were charged, and the temperature was raised to 70°C while stirring and passing oxygen / nitrogen mixed gas (oxygen concentration 8%). After reaching 70°C, the pressure in the reactor was gradually reduced to 10 kPa to remove the solvent PGMEA. After confirming that the concentration of PGMEA was less than 0.5% by weight by NMR analysis, 20 parts by weight of AOMA was charged to the obtained composition, homogenized, and then cooled to 30°C. After cooling, 0.5 parts by weight of n-butyl-4,4-bis(t-butylperoxy)valerate as an initiator was added at 20 to 30° C., and the mixture was stirred and homogenized to obtain the desired curable composition (X-8). Next, a 20 mm x 60 mm x 3 mm frame made of silicon spacers was placed on the glass, and the obtained curable composition was cast therein. It was left to stand at 30°C under nitrogen pressure (0.3 MPa) for 15 hours. After that, while still under pressure, it was heated to 110°C, held for 10 hours, and further held at 130°C for 8 hours. It was then removed from the mold to obtain a cured product.

[0058] <Evaluation method> [Flexural strength test (flexural modulus and flexural strength)] The test pieces for the bending strength test were prepared by processing the cured products prepared under the above preparation conditions into 5 mm x 50 mm x 3 mm pieces. The bending strength test was performed with a support distance of 30 mm and a bending speed of 10 mm / min, in accordance with JIS K 6911:2006. The bending strength and bending modulus of the obtained cured products are shown in Table 1. [Appearance (check for cracks)] A 20mm x 60mm x 5mm frame made of silicon spacers was placed on the glass, and the obtained curable composition was poured into it. The curing conditions were the same as those in the above-mentioned cured product preparation method. The appearance of the obtained cured product was checked to see if there were any cracks. ○: No cracks ×: Some cracks are present

[0059] [Table 1]

[0060] The abbreviations in Table 1 are as follows: AOMA (A-1): α-allyloxymethyl methyl acrylate [trade name "AOMA", manufactured by Nippon Shokubai Co., Ltd.] (R 1 is a methyl group, R 2 , R 3 , R 4 , R 5 and R 6 is a hydrogen atom) Bis-EMA (B-1): Dimethacrylate of EO adduct of bisphenol A (average number of moles added: 2.6) [product name: Light Ester BP-2EM, manufactured by Kyoeisha Chemical Co., Ltd.] Bis-GMA (B-2): Methacrylic acid adduct of bisphenol A diglycidyl ether [product name "Epoxy Ester 3000MK", Kyoeisha Chemical Co., Ltd.] FGDA(B-3): Methacrylic acid adduct of 9,9-bis(4-hydroxyphenyl)fluorenediglycidyl ether FDA-6EO (B-4): 9,9-bis(4-hydroxyphenyl)fluorene EO adduct diacrylate (average number of moles of EO added: 6) [product name: KONOMER-D064, manufactured by KPX Chemical Co., Ltd.] [Industrial Applicability]

[0061] The curable composition of the present invention has a high bending strength and bending modulus of elasticity, and is therefore excellent in mechanical strength, and is therefore useful as a sealant, molding material, or casting material for electronic parts. Specifically, it is useful as a semiconductor encapsulation material.

Claims

1. A curable composition containing a radical polymerizable monomer (A) represented by the following general formula (1), a bifunctional (meth)acrylate monomer (B) having a ring structure, a monofunctional (meth)acrylate monomer (C) having a ring structure, and a radical polymerization initiator (D), wherein the content of (A) is 5 to 25% by weight, the content of (B) is 35 to 70% by weight, and the content of (C) is 10 to 40% by weight, based on the total weight of (A), (B), and (C), and the ratio of the total weight of (B) and (C) to the weight of (A), [(B+C) / A], is 3 to 19. [Formula 1] [In formula (1), R 1 represents a hydrogen atom or an organic group having 1 to 30 carbon atoms. 2 , R 3 , R 4 , R 5 and R 6 are each independently a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.]

2. The curable composition according to claim 1 , wherein the ring structures of (B) and (C) are aromatic ring structures.

3. A cured product of the curable composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Alicyclic epoxy resin composition, its production and its cured product

    JP1995188385A

  • Resin composition for sealing optical semiconductor

    JP2007320974A

  • Curable composition for forming peelable resist

    JP2013091789A

  • Actinic-ray-curable ink and production method for printed matter

    JP2019002009A

  • Actinic-ray-curable ink and production method for printed matter

    JP2019002010A