Resin Emulsion
By integrating a polymerizable hindered amine-based monomer with a triazine-based ultraviolet absorber, the resin emulsion addresses the durability issues of triazine-based absorbers, resulting in a coating film with enhanced UV transmission and appearance retention.
Patent Information
- Application Number
- JP2021126480
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-08-02
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2037-03-31
AI Technical Summary
Existing resin emulsions containing triazine-based ultraviolet absorbers suffer from poor durability, leading to inferior UV appearance retention and UV transmission resistance in coating films.
Incorporating a polymerizable hindered amine-based photostable monomer into the resin emulsion, along with a triazine-based ultraviolet absorber, to enhance the durability and stability of the coating film.
The resulting resin emulsion forms a coating film with excellent UV transmission resistance and UV appearance retention, demonstrating improved durability and stability.
Smart Images

Figure 0007572333000001 
Figure 0007572333000002 
Figure 0007572333000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin emulsion. More specifically, the present invention relates to a topcoat paint, which is applied to, for example, ceramic building materials, automobiles, buildings, civil engineering structures, and the like, particularly to the exterior of buildings and the surfaces of ceramic building materials, and to a resin emulsion suitable for use in the topcoat paint and a method for producing the same. [Background technology]
[0002] As an aqueous coating composition having good storage stability and capable of forming a coating film with low gloss and excellent water repellency, water resistance, weather resistance, gloss retention and stain resistance even when a small amount of an aqueous silicone resin dispersion is used, there has been proposed an aqueous coating composition comprising: a (meth)acrylic polymer emulsion (A) obtained by polymerizing a (meth)acrylic monomer containing 2 to 15 mass % of a hydroxyl group-containing polymerizable monomer; an aqueous silicone resin dispersion (B); and a high HLB surfactant (C) having an HLB of 16 to 20, the high HLB surfactant (C) being contained in an amount of 0.2 to 2 parts by mass per 100 parts by mass of the (meth)acrylic polymer emulsion (A) (see, for example, claim 1 in Patent Document 1).
[0003] In the water-based coating composition, a triazine-based ultraviolet absorber is used for the purpose of improving weather resistance (see paragraph
[0054] of Patent Document 1). However, since the triazine-based ultraviolet absorber has poor durability in a resin emulsion, a coating film formed using the resin emulsion has the disadvantages of being poor not only in ultraviolet appearance retention but also in ultraviolet transmission resistance (see Comparative Example 1 in this specification). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2011-213941 A Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention has been made in consideration of the above-mentioned conventional technology, and an object of the present invention is to provide a resin emulsion containing a triazine-based ultraviolet absorber, which forms a coating film excellent in ultraviolet transmission resistance and ultraviolet appearance retention, a method for producing the same, and a topcoat paint containing the resin emulsion. [Means for solving the problem]
[0006] The present invention relates to (1) A resin emulsion containing a triazine-based ultraviolet absorber, characterized in that a polymerizable hindered amine-based light-stable monomer is used as a monomer component used as a resin raw material of the resin emulsion. (2) The resin emulsion according to (1), which is a resin emulsion containing emulsion particles containing a triazine-based ultraviolet absorber. (3) A topcoat paint containing the resin emulsion according to (1) or (2) above. (4) A method for producing a resin emulsion containing a triazine-based ultraviolet absorber, the method being characterized in that, when a monomer component is polymerized in the presence of the triazine-based ultraviolet absorber, a monomer component containing a polymerizable hindered amine-based light-stable monomer is used as the monomer component; and (5) The method for producing a resin emulsion according to (4) above, wherein the monomer component contains a triazine-based ultraviolet absorber. Regarding. Effect of the Invention
[0007] According to the present invention, there are provided a resin emulsion containing a triazine-based ultraviolet absorber, which forms a coating film excellent in resistance to ultraviolet transmission and ultraviolet appearance retention, a method for producing the same, and a topcoat paint containing the resin emulsion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] As described above, the resin emulsion of the present invention is characterized in that it contains a triazine-based ultraviolet absorber and that a polymerizable hindered amine-based light-stable monomer is used as a monomer component used as a resin raw material for the resin emulsion.
[0009] The resin emulsion of the present invention contains a triazine-based ultraviolet absorber, but since a polymerizable hindered amine-based light-stable monomer is used as the monomer component used as the resin raw material of the resin emulsion, a coating film excellent in ultraviolet transmission resistance and ultraviolet appearance retention is formed.
[0010] The present invention is characterized in that among various kinds of ultraviolet absorbers, a triazine-based ultraviolet absorber is used in the resin emulsion, and a polymerizable hindered amine-based light-stable monomer is used in the monomer component used as the resin raw material of the resin emulsion. As described above, in the present invention, a triazine-based ultraviolet absorber is used in the resin emulsion, and a polymerizable hindered amine-based light-stable monomer is used in the monomer component, and the resin emulsion of the present invention has both of these constitutions, and therefore not only is it excellent in ultraviolet transmission resistance, but it also forms a coating film that is excellent in ultraviolet appearance retention, which is an exceptionally outstanding effect that cannot be expected from the conventional technology.
[0011] The resin emulsion of the present invention can be obtained, for example, by a method of polymerizing a monomer component in the presence of a triazine-based ultraviolet absorber, a method of emulsion-polymerizing a monomer component and mixing the obtained resin emulsion with a triazine-based ultraviolet absorber, etc. Among these methods, the method of polymerizing a monomer component in the presence of a triazine-based ultraviolet absorber is preferred from the viewpoint of forming a coating film excellent in ultraviolet transmission resistance and ultraviolet appearance retention, water resistance, repeated freezing and thawing stability, and transparency.
[0012] Examples of the method of polymerizing a monomer component in the presence of a triazine-based ultraviolet absorber include a method of polymerizing a monomer component containing a triazine-based ultraviolet absorber, and a method of emulsion-polymerizing a monomer component in the presence of an aqueous medium containing a triazine-based ultraviolet absorber, but the present invention is not limited to these examples. Among these methods, the method of polymerizing a monomer component containing a triazine-based ultraviolet absorber is preferred from the viewpoint of forming a coating film that is excellent in ultraviolet transmission resistance and ultraviolet appearance retention, water resistance, freeze-thaw repeated stability, and transparency.
[0013] Hereinafter, as a method for polymerizing a monomer component in the presence of a triazine-based ultraviolet absorber, a method for preparing a resin emulsion by using a monomer component containing a polymerizable hindered amine-based light-stable monomer as the monomer component when polymerizing a monomer component in the presence of a triazine-based ultraviolet absorber will be described.
[0014] Examples of triazine-based ultraviolet absorbers include 2-[4-[(2-hydroxy-3-dodecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-tridecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, and 2-[4-[(2-hydroxy-3-(2'-ethyl)hexyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine. Examples of the hydroxyphenyl triazine-based ultraviolet absorbers include hydroxyphenyl triazine, 2,4-bis(2-hydroxy-4-butyloxyphenyl)-6-(2,4-bis-butyloxyphenyl)-1,3,5-triazine, hydroxyphenyl triazine, 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine, and 2,4,6-tris(2-hydroxy-4-hexyloxy-3-methylphenyl)-1,3,5-triazine, but the present invention is not limited to these examples. These triazine-based ultraviolet absorbers may be used alone or in combination of two or more kinds. Of these triazine-based ultraviolet absorbers, from the viewpoint of forming a coating film that is excellent in ultraviolet transmission resistance and ultraviolet appearance retention, and is excellent in water resistance, repeated freezing and thawing stability and transparency, hydroxyphenyltriazine-based ultraviolet absorbers such as 2-[4-[(2-hydroxy-3-dodecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine and 2-[4-[(2-hydroxy-3-tridecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine are preferred.
[0015] Triazine-based ultraviolet absorbers are commercially available and can be easily obtained. Examples of such absorbers include TINUVIN (registered trademark, the same applies below) 400 (a mixture of 2-[4-[(2-hydroxy-3-dodecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine and 2-[4-[(2-hydroxy-3-tridecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine), TINUVIN 405 (2-[4-[(2-hydroxy-3-(2'-ethyl)hexyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine), TINUVI Examples of hydroxyphenyl triazine-based ultraviolet absorbents include N460 [2,4-bis(2-hydroxy-4-butyloxyphenyl)-6-(2,4-bis-butyloxyphenyl)-1,3,5-triazine], TINUVIN477 [hydroxyphenyl triazine], TINUVIN479 [2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine], and ADEKA Corporation, trade name: Adeka STAB (registered trademark) F70 [2,4,6-tris(2-hydroxy-4-hexyloxy-3-methylphenyl)-1,3,5-triazine], but the present invention is not limited to these examples. These triazine-based ultraviolet absorbents may be used alone or in combination of two or more kinds.
[0016] The amount of triazine-based ultraviolet absorber per 100 parts by mass of the monomer component used as the resin raw material for the resin emulsion of the present invention is, from the viewpoint of forming a coating film excellent in ultraviolet transmission resistance and ultraviolet appearance retention, preferably 0.1 part by mass or more, more preferably 0.2 parts by mass or more, even more preferably 0.3 parts by mass or more, and even more preferably 0.5 parts by mass or more, and from the viewpoint of forming a coating film excellent in water resistance, repeated freeze-thaw stability and transparency, it is preferably 5 parts by mass or less, more preferably 4.5 parts by mass or less, even more preferably 4 parts by mass or less, and even more preferably 3.5 parts by mass or less.
[0017] Examples of the polymerizable hindered amine-based light-stable monomer include 4-(meth)acryloyloxy-2,2,6,6-tetramethylpiperidine, 4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 4-(meth)acryloyloxy-1,2,2,6,6-pentamethylpiperidine, 4-(meth)acryloyl-1-methoxy-2,2,6,6-tetramethylpiperidine, 4-cyano-4-(meth)acryloyloxy-2,2,6,6-tetramethylpiperidine, 1-(meth)acryloyl-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 4- Examples of the polymerizable hindered amine-based light-stable monomer include crotonoylamino-2,2,6,6-tetramethylpiperidine, 4-(meth)acryloylamino-1,2,2,6,6-pentamethylpiperidine, 4-cyano-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 4-crotonoyloxy-2,2,6,6-tetramethylpiperidine, 1-(meth)acryloyl-4-cyano-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, and 1-crotonoyl-4-crotonoyloxy-2,2,6,6-tetramethylpiperidine, but the present invention is not limited to these examples. Each of these polymerizable hindered amine-based light-stable monomers may be used alone, or two or more of them may be used in combination. Among these polymerizable hindered amine-based light-stable monomers, from the viewpoint of forming a coating film excellent in ultraviolet light transmission resistance and ultraviolet light appearance retention, water resistance, stability against repeated freezing and thawing, and transparency, 4-(meth)acryloyloxy-2,2,6,6-tetramethylpiperidine and 4-(meth)acryloyloxy-1,2,2,6,6-pentamethylpiperidine are preferred, and 4-methacryloyloxy-2,2,6,6-tetramethylpiperidine and 4-methacryloyloxy-1,2,2,6,6-pentamethylpiperidine are more preferred.
[0018] As used herein, "(meth)acryloyl" means "acryloyl" or "methacryloyl", "(meth)acrylate" means "acrylate" or "methacrylate", and "(meth)acrylic" means "acrylic" or "methacrylic".
[0019] The content of the polymerizable hindered amine-based photostable monomer in the monomer component is preferably 0.1 mass % or more, more preferably 0.3 mass % or more, and even more preferably 0.5 mass % or more, from the viewpoint of forming a coating film excellent in UV transmission resistance and UV appearance retention, and is preferably 25 mass % or less, more preferably 20 mass % or less, and even more preferably 15 mass % or less, from the viewpoint of forming a coating film excellent in water resistance and repeated freeze-thaw stability.
[0020] As the monomer component, monomers other than the polymerizable hindered amine-based light-stable monomers (hereinafter simply referred to as "other monomers") can be used.
[0021] Examples of the other monomers include alkyl (meth)acrylates, cycloalkyl (meth)acrylates having a cycloalkyl group with 3 to 12 carbon atoms, hydroxyl group-containing (meth)acrylates, silane group-containing monomers, aromatic monomers, carboxyl group-containing monomers, nitrogen atom-containing monomers, oxo group-containing monomers, fluorine atom-containing monomers, epoxy group-containing monomers, ultraviolet absorbing monomers, and light-stable monomers other than polymerizable hindered amine-based light-stable monomers, but the present invention is not limited to these examples. These other monomers may be used alone or in combination of two or more. Among these other monomers, from the viewpoint of forming a coating film excellent in UV resistance, UV appearance retention, water resistance, stability against repeated freezing and thawing, and transparency, preferred are alkyl (meth)acrylates, cycloalkyl (meth)acrylates having a cycloalkyl group with 3 to 12 carbon atoms, hydroxyl group-containing (meth)acrylates, silane group-containing monomers, and aromatic monomers, more preferred are alkyl (meth)acrylates, cycloalkyl (meth)acrylates having a cycloalkyl group with 3 to 12 carbon atoms, hydroxyl group-containing (meth)acrylates, and silane group-containing monomers, and even more preferred are alkyl (meth)acrylates, cycloalkyl (meth)acrylates having a cycloalkyl group with 3 to 12 carbon atoms, and hydroxyl group-containing (meth)acrylates.
[0022] Examples of alkyl (meth)acrylates include alkyl (meth)acrylates having an alkyl group carbon number of 1 to 18, such as methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, sec-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, tridecyl (meth)acrylate, and n-lauryl (meth)acrylate, but the present invention is not limited to these examples. These alkyl (meth)acrylates may be used alone or in combination of two or more. Among these alkyl (meth)acrylates, from the viewpoint of forming a coating film excellent in UV resistance, UV appearance retention, water resistance, stability against repeated freezing and thawing, and transparency, alkyl (meth)acrylates having an alkyl group of 1 to 8 carbon atoms are preferred, and methyl (meth)acrylate, n-butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate are more preferred.
[0023] The content of alkyl (meth)acrylate in the monomer component is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more, from the viewpoint of forming a coating film having excellent water resistance, stability against repeated freeze-thaw cycles, and transparency, and is preferably 85% by mass or less, more preferably 80% by mass or less, and even more preferably 75% by mass or less, from the viewpoint of forming a coating film having excellent resistance to ultraviolet light transmission and ultraviolet appearance retention, water resistance, stability against repeated freeze-thaw cycles, and transparency.
[0024] Examples of cycloalkyl (meth)acrylates having a cycloalkyl group with 3 to 12 carbon atoms include cyclopropyl (meth)acrylate, cyclobutyl (meth)acrylate, cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, and isobornyl (meth)acrylate, but the present invention is not limited to these examples. These cycloalkyl (meth)acrylates having a cycloalkyl group with 3 to 12 carbon atoms may be used alone or in combination of two or more. Among these cycloalkyl (meth)acrylates having a cycloalkyl group with 3 to 12 carbon atoms, from the viewpoint of forming a coating film having excellent ultraviolet transmission resistance and ultraviolet appearance retention, water resistance, freeze-thaw repeat stability, and transparency, cycloalkyl (meth)acrylates having a cycloalkyl group with 3 to 10 carbon atoms are preferred, cycloalkyl (meth)acrylates having a cycloalkyl group with 4 to 8 carbon atoms are more preferred, and cyclohexyl (meth)acrylate is even more preferred.
[0025] The content of cycloalkyl (meth)acrylate having a cycloalkyl group having 3 to 12 carbon atoms in the monomer component is, from the viewpoint of forming a coating film which is excellent in UV resistance, UV appearance retention, water resistance, repeated freeze-thaw stability and transparency, preferably at least 0 mass%, more preferably at least 10 mass%, more preferably at least 15 mass%, and even more preferably at least 20 mass%, and from the viewpoint of forming a coating film which is excellent in repeated freeze-thaw stability, preferably at most 80 mass%, more preferably at most 70 mass%, and even more preferably at most 60 mass%.
[0026] Examples of hydroxyl group-containing (meth)acrylates include hydroxyl group-containing (meth)acrylates having 1 to 18 carbon atoms in the ester group, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and glycerin mono(meth)acrylate, but the present invention is not limited to these examples. These hydroxyl group-containing (meth)acrylates may be used alone or in combination of two or more. Among these hydroxyl group-containing (meth)acrylates, 2-hydroxyethyl (meth)acrylate and glycerin mono(meth)acrylate are preferred, and 2-hydroxyethyl methacrylate is more preferred, from the viewpoint of forming a coating film that is excellent in UV resistance and UV appearance retention, water resistance, stability against repeated freezing and thawing, and transparency.
[0027] The content of the hydroxyl group-containing (meth)acrylate in the monomer component is, from the viewpoint of forming a coating film that is excellent in UV resistance, UV appearance retention, water resistance, repeated freeze-thaw stability and transparency, 0 mass % or more, preferably 0.1 mass % or more, more preferably 0.3 mass % or more, and even more preferably 0.5 mass % or more, and from the viewpoint of forming a coating film that is excellent in UV resistance, UV appearance retention, water resistance, repeated freeze-thaw stability and transparency, the content is preferably 10 mass % or less, more preferably 5 mass % or less, and even more preferably 3 mass % or less.
[0028] Examples of silane group-containing monomers include vinyltrimethoxysilane, vinyltriethoxysilane, vinyltri(methoxyethoxy)silane, γ-(meth)acryloyloxypropyltrimethoxysilane, 2-styrylethyltrimethoxysilane, vinyltrichlorosilane, γ-(meth)acryloyloxypropylhydroxysilane, γ-(meth)acryloyloxypropylmethylhydroxysilane, but the present invention is not limited to these examples. These silane group-containing monomers may be used alone or in combination of two or more. Among these silane group-containing monomers, γ-(meth)acryloyloxypropyltrimethoxysilane is preferred, and γ-methacryloyloxypropyltrimethoxysilane is more preferred, from the viewpoint of forming a coating film that is excellent in UV resistance and UV appearance retention, water resistance, stability against repeated freezing and thawing, and transparency.
[0029] The content of the silane group-containing monomer in the monomer component is, from the viewpoint of forming a coating film which is excellent in UV resistance, UV appearance retention, water resistance, repeated freeze-thaw stability and transparency, preferably at least 0.5% by mass, more preferably at least 1% by mass, and even more preferably at least 1.5% by mass, and from the viewpoint of forming a coating film which is excellent in UV resistance, UV appearance retention, water resistance, repeated freeze-thaw stability and transparency, preferably at most 5% by mass, more preferably at most 4% by mass, and even more preferably at most 3% by mass.
[0030] Examples of aromatic monomers include styrene, α-methylstyrene, p-methylstyrene, tert-methylstyrene, chlorostyrene, aralkyl (meth)acrylate, vinyltoluene, etc., but the present invention is not limited to these examples. Examples of aralkyl (meth)acrylates include aralkyl (meth)acrylates having an aralkyl group with a carbon number of 7 to 18, such as benzyl (meth)acrylate, phenylethyl (meth)acrylate, methylbenzyl (meth)acrylate, and naphthylmethyl (meth)acrylate, but the present invention is not limited to these examples. These aromatic monomers may be used alone or in combination of two or more.
[0031] Examples of the carboxyl group-containing monomer include carboxyl group-containing aliphatic monomers such as (meth)acrylic acid, maleic acid, fumaric acid, crotonic acid, itaconic acid, and maleic anhydride, but the present invention is not limited to these examples. These carboxyl group-containing monomers may be used alone or in combination of two or more kinds.
[0032] Examples of the nitrogen atom-containing monomer include (meth)acrylamide, diacetone (meth)acrylamide, N-monomethyl (meth)acrylamide, N-monoethyl (meth)acrylamide, N,N-dimethyl (meth)acrylamide, Nn-propyl (meth)acrylamide, N-isopropyl (meth)acrylamide, methylene bis (meth)acrylamide, N-methylol (meth)acrylamide, N-butoxymethyl (meth)acrylamide, dimethylaminoethyl (meth)acrylamide, N,N-dimethylaminopropyl (meth)acrylamide, and diacetone (meth)acrylamide (meth)acrylamide and other (meth)acrylamide compounds, dimethylaminoethyl (meth)acrylate, and diethylaminoethyl (meth)acrylate (meth)acrylamide and other nitrogen atom-containing (meth)acrylate compounds, N-vinylpyrrolidone, and (meth)acrylonitrile, but the present invention is not limited to these examples. These nitrogen atom-containing monomers may be used alone or in combination of two or more.
[0033] Examples of oxo group-containing monomers include (di)ethylene glycol (methoxy) (meth) acrylates such as ethylene glycol (meth) acrylate, ethylene glycol methoxy (meth) acrylate, diethylene glycol (meth) acrylate, and diethylene glycol methoxy (meth) acrylate, but the present invention is not limited to these examples. These oxo group-containing monomers may be used alone or in combination of two or more kinds.
[0034] Examples of the fluorine atom-containing monomer include fluorine atom-containing alkyl (meth)acrylates having an ester group with 2 to 6 carbon atoms, such as trifluoroethyl (meth)acrylate, tetrafluoropropyl (meth)acrylate, and octafluoropentyl (meth)acrylate, but the present invention is not limited to these examples. These fluorine atom-containing monomers may be used alone or in combination of two or more kinds.
[0035] Examples of epoxy group-containing monomers include epoxy group-containing (meth)acrylates such as glycidyl (meth)acrylate, but the present invention is not limited to these examples. These epoxy group-containing monomers may be used alone or in combination of two or more kinds.
[0036] Examples of ultraviolet absorbing monomers include benzotriazole-based ultraviolet absorbing monomers, benzophenone-based ultraviolet absorbing monomers, etc., but the present invention is not limited to these examples. These ultraviolet absorbing monomers may be used alone or in combination of two or more kinds.
[0037] Examples of the benzotriazole-based ultraviolet absorbing monomer include 2-[2'-hydroxy-5'-(meth)acryloyloxymethylphenyl]-2H-benzotriazole, 2-[2'-hydroxy-5'-(meth)acryloyloxyethylphenyl]-2H-benzotriazole, 2-[2'-hydroxy-5'-(meth)acryloyloxymethylphenyl]-5-tert-butyl-2H-benzotriazole, and 2-[2'-hydroxy-5'-(meth)acryloyloxymethylphenyl]-5-tert-butyl-2H-benzotriazole. ) Acryloylaminomethyl-5'-tert-octylphenyl]-2H-benzotriazole, 2-[2'-hydroxy-5'-(meth)acryloyloxypropylphenyl]-2H-benzotriazole, 2-[2'-hydroxy-5'-(meth)acryloyloxyhexylphenyl]-2H-benzotriazole, 2-[2'-hydroxy-3'-tert-butyl-5'-(meth)acryloyloxyethylphenyl]-2H-benzotriazole , 2-[2'-hydroxy-3'-tert-butyl-5'-(meth)acryloyloxyethylphenyl]-5-chloro-2H-benzotriazole, 2-[2'-hydroxy-5'-tert-butyl-3'-(meth)acryloyloxyethylphenyl]-2H-benzotriazole, 2-[2'-hydroxy-5'-(meth)acryloyloxyethylphenyl]-5-chloro-2H-benzotriazole, 2-[2'-hydroxy-5'-(meth)acryloyloxyethylphenyl]-5-chloro-2H-benzotriazole, Examples of the benzotriazole-based ultraviolet absorbing monomer include 2-[2'-hydroxy-5'-(β-(meth)acryloyloxyethoxy)-3'-tert-butylphenyl]-5-cyano-2H-benzotriazole, 2-[2'-hydroxy-5'-(β-(meth)acryloyloxyethoxy)-3'-tert-butylphenyl]-4-tert-butyl-2H-benzotriazole, but the present invention is not limited to these examples. These benzotriazole-based ultraviolet absorbing monomers may be used alone or in combination of two or more kinds.
[0038] Benzophenone-based ultraviolet absorbing monomers include, for example, 2-hydroxy-4-(meth)acryloyloxybenzophenone, 2-hydroxy-4-[2-hydroxy-3-(meth)acryloyloxy]propoxybenzophenone, 2-hydroxy-4-[2-(meth)acryloyloxy]ethoxybenzophenone, 2-hydroxy-4-[3-(meth)acryloyloxy-2-hydroxypropoxy]benzophenone, 2-hydroxy-3-tert-butyl-4-[2-(meth)acryloyloxy]butoxybenzophenone, but the present invention is not limited to these examples. These benzophenone-based ultraviolet absorbing monomers may be used alone or in combination of two or more kinds.
[0039] Examples of light-stable monomers other than the polymerizable hindered amine-based light-stable monomer include a reaction product of decanedioic acid bis(2,2,6,6-tetramethyl-1-(octyloxy)-4-piperidinyl) ester, 1,1-dimethylethyl hydroperoxide, and octane, bis(1,2,2,6,6-pentamethyl-4-piperidyl)[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]butyl malonate, and a mixture of bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate and methyl 1,2,2,6,6-pentamethyl-4-piperidylsebacate, but the present invention is not limited to these examples. These light-stable monomers other than the polymerizable hindered amine-based light-stable monomers may be used alone or in combination of two or more kinds.
[0040] The content of other monomers in the monomer component is preferably 75% by mass or more, more preferably 80% by mass or more, and even more preferably 85% by mass or more, from the viewpoint of forming a coating film that is excellent in UV resistance, UV appearance retention, water resistance, repeated freeze-thaw stability and transparency, and is preferably 99.9% by mass or less, more preferably 99.7% by mass or less, and even more preferably 99.5% by mass or less, from the viewpoint of forming a coating film that is excellent in UV resistance, UV appearance retention, water resistance, repeated freeze-thaw stability and transparency.
[0041] Examples of the method for emulsion-polymerizing the monomer component include a method of dissolving an emulsifier in an aqueous medium containing a water-soluble organic solvent such as a lower alcohol such as methanol and water, or a medium such as water, and dropping the monomer component and a polymerization initiator under heating and stirring, and a method of dropping a monomer component that has been emulsified in advance using an emulsifier and water into water or an aqueous medium, but the present invention is not limited to such a method. The amount of the medium may be appropriately set in consideration of the amount of non-volatile matter contained in the resulting resin emulsion.
[0042] Examples of the emulsifier include anionic emulsifiers, nonionic emulsifiers, cationic emulsifiers, amphoteric emulsifiers, and polymeric emulsifiers. These emulsifiers may be used alone or in combination of two or more kinds.
[0043] Examples of the anionic emulsifier include alkyl sulfate salts such as ammonium dodecyl sulfate and sodium dodecyl sulfate; alkyl sulfonate salts such as ammonium dodecyl sulfonate and sodium dodecyl sulfonate; alkyl aryl sulfonate salts such as ammonium dodecyl benzene sulfonate and sodium dodecyl naphthalene sulfonate; polyoxyethylene alkyl sulfate salts; polyoxyethylene alkyl aryl sulfate salts; dialkyl sulfosuccinates; aryl sulfonic acid-formalin condensates; and fatty acid salts such as ammonium laurate and sodium stearate, but the present invention is not limited to these examples.
[0044] Examples of nonionic emulsifiers include polyoxyethylene alkyl ethers, polyoxyethylene alkylaryl ethers, condensates of polyethylene glycol and polypropylene glycol, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, fatty acid monoglycerides, and condensates of ethylene oxide and aliphatic amines; however, the present invention is not limited to these examples.
[0045] Examples of cationic emulsifiers include alkyl ammonium salts such as dodecyl ammonium chloride, but the present invention is not limited to these examples.
[0046] Examples of amphoteric emulsifiers include betaine ester emulsifiers, but the present invention is not limited to these examples.
[0047] Examples of polymeric emulsifiers include poly(meth)acrylates such as sodium polyacrylate; polyvinyl alcohol; polyvinylpyrrolidone; polyhydroxyalkyl(meth)acrylates such as polyhydroxyethyl acrylate; and polymers containing one or more of the monomers constituting these polymers as copolymerization components, but the present invention is not limited to these examples.
[0048] Furthermore, from the viewpoint of forming a coating film that is excellent in resistance to ultraviolet light transmission and ultraviolet appearance retention, as well as in water resistance, stability against repeated freezing and thawing, and transparency, an emulsifier having a polymerizable group, i.e., a so-called reactive emulsifier, is preferred as the emulsifier, and from the viewpoint of environmental protection, a non-nonylphenyl type emulsifier is preferred.
[0049] Examples of the reactive emulsifier include propenyl-alkyl sulfosuccinate salts, (meth)acrylic acid polyoxyethylene sulfonate salts, polyoxyethylene alkylpropenylphenyl ether ammonium sulfate (e.g., manufactured by Daiichi Kogyo Seiyaku Co., Ltd., trade names: Aqualon HS-10, Aqualon BC-10, etc.), sulfonate salts of allyloxymethyl alkyloxy polyoxyethylene (e.g., manufactured by Daiichi Kogyo Seiyaku Co., Ltd., trade name: Aqualon KH-10, etc.), sulfonate salts of allyloxymethyl nonylphenoxyethyl hydroxy polyoxyethylene (e.g., manufactured by ADEKA Corporation, trade name: Adeka Reasoap SE-10, etc.), allyloxymethyl alkoxyethyl hydroxy polyoxyethylene sulfate ester salts (e.g., manufactured by Adeka Corporation, trade name: Adeka Reasoap SE-10, etc.), and the like. Examples of such reactive emulsifiers include ADEKA Reasoap SR-10, SR-30, etc., bis(polyoxyethylene polycyclic phenyl ether) methacrylated sulfonate salts (e.g., Nippon Nyukazai Co., Ltd., trade name: Antox MS-60, etc.), allyloxymethylalkoxyethylhydroxypolyoxyethylene (e.g., ADEKA Reasoap ER-20, etc.), polyoxyethylene alkylpropenylphenyl ether (e.g., Daiichi Kogyo Seiyaku Co., Ltd., trade name: Aqualon RN-20, etc.), and allyloxymethylnonylphenoxyethylhydroxypolyoxyethylene (e.g., ADEKA Reasoap NE-10, etc.), but the present invention is not limited to these examples. Each of these reactive emulsifiers may be used alone, or two or more of them may be used in combination.
[0050] The amount of emulsifier per 100 parts by mass of the monomer component is, from the viewpoint of improving polymerization stability, preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, and even more preferably 2 parts by mass or more, and from the viewpoint of forming a coating film that is excellent in UV resistance and UV appearance retention, water resistance, repeated freeze-thaw stability, and transparency, is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, and even more preferably 5 parts by mass or less.
[0051] A polymerization initiator can be used when polymerizing the monomer components. Examples of the polymerization initiator include azo compounds such as azobisisobutyronitrile, 2,2-azobis(2-methylbutyronitrile), 2,2-azobis(2,4-dimethylvaleronitrile), 2,2-azobis(2-diaminopropane) hydrochloride, 4,4-azobis(4-cyanovaleric acid), and 2,2-azobis(2-methylpropionamidine); persulfates such as potassium persulfate and ammonium persulfate; and peroxides such as hydrogen peroxide, benzoyl peroxide, parachlorobenzoyl peroxide, lauroyl peroxide, and ammonium peroxide, but the present invention is not limited to these examples. These polymerization initiators may be used alone or in combination of two or more.
[0052] The amount of polymerization initiator per 100 parts by mass of the monomer component is preferably 0.01 parts by mass or more, more preferably 0.03 parts by mass or more, from the viewpoint of increasing the polymerization rate and reducing the amount of remaining unreacted monomer component, and is preferably 5 parts by mass or less, more preferably 3 parts by mass or less, from the viewpoint of forming a coating film that is excellent in UV resistance and UV appearance retention, water resistance, repeated freeze-thaw stability, and transparency.
[0053] The method of adding the polymerization initiator is not particularly limited. Examples of the addition method include batch charging, divided charging, continuous dropwise addition, etc. In order to hasten the end of the polymerization reaction, a part of the polymerization initiator may be added to the flask before or after the addition of the monomer components to the reaction system.
[0054] In order to promote the decomposition of the polymerization initiator, a suitable amount of a decomposer for the polymerization initiator, for example, a reducing agent such as sodium hydrogen sulfite or a transition metal salt such as ferrous sulfate, may be added to the reaction system.
[0055] In addition, if necessary, an appropriate amount of additives such as a chain transfer agent, a compound having a thiol group such as tert-dodecyl mercaptan, a pH buffer, a chelating agent, etc. may be added to the reaction system in the flask. The amount of the additive varies depending on the type and cannot be determined in general, but is usually preferably 0.01 to 5 parts by mass, more preferably 0.1 to 3 parts by mass, per 100 parts by mass of the monomer component.
[0056] The atmosphere in which the monomer components are emulsion-polymerized is not particularly limited, but from the viewpoint of increasing the efficiency of the polymerization initiator, it is preferable that the atmosphere be an inert gas such as nitrogen gas.
[0057] The polymerization temperature when emulsion-polymerizing the monomer components is not particularly limited, but is usually preferably 50 to 100° C., more preferably 60 to 95° C. The polymerization temperature may be constant or may be changed during the polymerization reaction.
[0058] The polymerization time for emulsion-polymerizing the monomer components is not particularly limited and may be appropriately set depending on the progress of the polymerization reaction, but is usually about 2 to 9 hours.
[0059] By emulsion-polymerizing the monomer components (hereinafter referred to as "the monomer components") as described above, a resin emulsion containing emulsion particles is obtained.
[0060] The polymer constituting the emulsion particles may have a crosslinked structure. The weight average molecular weight of the polymer is preferably 100,000 or more, more preferably 300,000 or more, even more preferably 550,000 or more, and particularly preferably 600,000 or more, from the viewpoint of forming a coating film excellent in UV resistance, UV appearance retention, water resistance, freeze-thaw repeat stability, and transparency. The upper limit of the weight average molecular weight of the polymer is not particularly limited when it has a crosslinked structure, since it is difficult to measure the weight average molecular weight, but when it does not have a crosslinked structure, it is preferably 5 million or less from the viewpoint of improving film-forming properties.
[0061] In this specification, the weight average molecular weight of a polymer means the weight average molecular weight (polystyrene equivalent) measured using gel permeation chromatography (manufactured by Tosoh Corporation, product number: HLC-8120GPC, columns: TSKgel G-5000HXL and TSKgel GMHXL-L in series).
[0062] The emulsion particles contained in the resin emulsion of the present invention may have a single resin layer prepared by one-stage emulsion polymerization, or may have multiple resin layers prepared by multiple-stage emulsion polymerization. Among these emulsion particles, those having multiple resin layers are preferred from the viewpoint of forming a coating film that is excellent in UV resistance and UV appearance retention, water resistance, freeze-thaw repeat stability, and transparency. In addition, when the emulsion particles have multiple resin layers, the boundaries of each resin layer do not necessarily need to be clear, and adjacent resin layers may be mixed with each other.
[0063] The number of resin layers constituting the emulsion particles is preferably 1 to 5 layers, more preferably 1 to 3 layers, and even more preferably 2 or 3 layers, from the viewpoint of forming a coating film that is excellent in UV resistance, UV appearance retention, water resistance, repeated freezing and thawing stability, and transparency.
[0064] Furthermore, among emulsion particles having multiple resin layers, from the viewpoint of forming a coating film excellent in UV-ray transmission resistance and UV-ray appearance retention, as well as excellent water resistance, freeze-thaw repeat stability and transparency, emulsion particles having a resin layer with the highest glass transition temperature as a layer located inside the outermost layer among the resin layers constituting the emulsion particles are preferred.
[0065] Emulsion particles having a single resin layer can be prepared by emulsion polymerization of the monomer component, while emulsion particles having multiple resin layers can be prepared by multi-stage emulsion polymerization of the monomer components using the same polymerization method and conditions as those for emulsion polymerization of the monomer components.
[0066] When the emulsion particles have multiple resin layers, it is preferable that the monomer components forming each layer each contain a triazine-based ultraviolet absorber, from the viewpoint of forming a coating film that is excellent in ultraviolet transmission resistance and ultraviolet appearance retention, and is excellent in water resistance, stability against repeated freezing and thawing, and transparency.
[0067] The emulsion particles having two resin layers, an inner layer and an outer layer, can be prepared by emulsion-polymerizing the monomer component forming the inner layer, and emulsion-polymerizing the monomer component forming the outer layer in the presence of the obtained emulsion particles. In this case, the monomer component is preferably used in the monomer component forming the inner layer and the outer layer from the viewpoint of forming a coating film excellent in ultraviolet transmission resistance and ultraviolet appearance retention, water resistance, freeze-thaw repeated stability and transparency. The mass ratio of the resin layer constituting the inner layer to the resin layer constituting the outer layer (resin layer constituting the inner layer / resin layer constituting the outer layer) is preferably 10 / 90 or more, more preferably 20 / 80 or more, and even more preferably 30 / 70 or more from the viewpoint of forming a coating film excellent in ultraviolet transmission resistance and ultraviolet appearance retention, water resistance, freeze-thaw repeated stability and transparency, and is preferably 80 / 20 or less, more preferably 70 / 30 or less from the viewpoint of improving film-forming properties, adhesion and blocking resistance.
[0068] The emulsion particles having three resin layers, an inner layer, an intermediate layer, and an outer layer, can be prepared by emulsion-polymerizing the monomer component forming the inner layer, emulsion-polymerizing the monomer component forming the intermediate layer in the presence of the obtained emulsion particles, and emulsion-polymerizing the monomer component forming the outer layer in the presence of the obtained emulsion particles. In this case, the monomer component is preferably used as the monomer component forming the inner layer, the intermediate layer, and the outer layer from the viewpoint of forming a coating film excellent in ultraviolet transmission resistance and ultraviolet appearance retention, water resistance, freeze-thaw repeated stability, and transparency. In addition, from the viewpoint of forming a coating film excellent in ultraviolet transmission resistance and ultraviolet appearance retention, water resistance, freeze-thaw repeated stability, and transparency, it is preferable that the content of the resin layer constituting the inner layer is 10 to 40 mass%, the content of the resin layer constituting the intermediate layer is 20 to 60 mass%, and the content of the resin layer constituting the outer layer is 20 to 60 mass%.
[0069] In emulsion particles having a single resin layer, the glass transition temperature of the resin layer is preferably -10°C or higher, more preferably -5°C or higher, and even more preferably 0°C or higher, from the viewpoint of forming a coating film that is excellent in UV resistance, UV appearance retention, water resistance, freeze-thaw repeat stability, and transparency, and is preferably 50°C or lower, more preferably 40°C or lower, and even more preferably 30°C or lower.
[0070] In emulsion particles having two resin layers, an inner layer and an outer layer, from the viewpoint of forming a coating film excellent in UV resistance, UV appearance retention, water resistance, freeze-thaw repeat stability and transparency, the glass transition temperature of the resin layer constituting the inner layer is preferably -20 to 150°C, more preferably -10 to 110°C, and the glass transition temperature of the resin layer constituting the outer layer is preferably -50 to 70°C, more preferably -40 to 60°C.
[0071] In emulsion particles having three resin layers, i.e., an inner layer, an intermediate layer, and an outer layer, from the viewpoint of forming a coating film excellent in UV resistance, UV appearance retention, water resistance, stability against repeated freezing and thawing, and transparency, the glass transition temperature of the resin layer constituting the inner layer is preferably 50 to 150°C, more preferably 80 to 110°C, the glass transition temperature of the resin layer constituting the intermediate layer is preferably -50 to 0°C, more preferably -30 to -10°C, and the glass transition temperature of the resin layer constituting the outer layer is preferably 0 to 50°C, more preferably 10 to 40°C.
[0072] In addition, the glass transition temperature of the entire emulsion particle having multiple resin layers is, from the viewpoint of forming a coating film that is excellent in UV resistance, UV appearance retention, water resistance, repeated freeze-thaw stability and transparency, preferably -10°C or higher, more preferably -5°C or higher, even more preferably 0°C or higher, and is preferably 50°C or lower, more preferably 45°C or lower, even more preferably 40°C or lower.
[0073] The glass transition temperature of the resin layer constituting the emulsion particle can be easily adjusted by adjusting the type and amount of the monomer used in the monomer component.
[0074] In this specification, the glass transition temperature of the resin layer constituting the emulsion particle is expressed by the following formula, using the glass transition temperature of a homopolymer of a monomer used in the monomer component constituting the resin layer: 1 / Tg=Σ(Wm / Tgm) / 100 (In the formula, Wm represents the content (mass%) of monomer m in the monomer components constituting the polymer, and Tgm represents the glass transition temperature (absolute temperature: K) of a homopolymer of monomer m.) This refers to the temperature calculated based on the Fox formula,
[0075] In this specification, the glass transition temperature of the resin layer constituting the emulsion particle means the glass transition temperature calculated based on the Fox formula, unless otherwise specified. The glass transition temperature of the entire resin layer constituting the emulsion particle having a plurality of resin layers means the glass transition temperature calculated based on the Fox formula using the glass transition temperatures of the homopolymers of the monomers used in all the monomer components constituting all the resin layers used in the multi-stage emulsion polymerization. For monomers with unknown glass transition temperatures such as special monomers and multifunctional monomers, when the total amount of the monomers with unknown glass transition temperatures in the monomer component is 10% by mass or less in mass fraction, the glass transition temperature is calculated using only the monomers with known glass transition temperatures. When the total amount of the monomers with unknown glass transition temperatures in the monomer component exceeds 10% by mass fraction, the glass transition temperature of the polymer is calculated by differential scanning calorimetry (DSC), differential calorimetry (DTA), thermomechanical analysis (TMA), or the like.
[0076] The glass transition temperature of the resin layer can be easily adjusted by adjusting the composition of the monomer component. Taking into consideration the glass transition temperature of the resin layer constituting the emulsion particle, the composition of the monomer component used as the raw material of the resin layer constituting the emulsion particle can be determined.
[0077] The glass transition temperatures of the polymers are, for example, 105°C for a homopolymer of methyl methacrylate, 100°C for a homopolymer of styrene, 83°C for a homopolymer of cyclohexyl methacrylate, -70°C for a homopolymer of 2-ethylhexyl acrylate, -56°C for a homopolymer of n-butyl acrylate, 20°C for a homopolymer of n-butyl methacrylate, 55°C for a homopolymer of 2-hydroxyethyl methacrylate, 95°C for a homopolymer of acrylic acid, 130°C for a homopolymer of methacrylic acid, 130°C for a homopolymer of 4-methacryloyloxy-1,2,2,6,6-pentamethylpiperidine, and 70°C for a homopolymer of γ-methacryloyloxypropyltrimethoxysilane.
[0078] In addition, when the emulsion particle is composed of multiple resin layers, the solubility parameter (hereinafter also referred to as SP value) of the resin layer constituting the outer layer is preferably higher than the SP value of the resin layer constituting the inner layer from the viewpoint of improving the flexibility and film-forming property of the coating film. In addition, the difference (absolute value) between the SP value of the resin layer constituting the inner layer and the SP value of the resin layer constituting the outer layer is preferably large from the viewpoint of forming a layer-separated structure in the emulsion particle.
[0079] The SP value is a value defined by the regular solution theory introduced by Hildebrand, and is also a measure of the solubility of a two-component solution. In general, substances with similar SP values tend to mix easily with each other. Therefore, the SP value is also a measure of how easily a solute and a solvent mix.
[0080] The average particle size of the emulsion particles is preferably 30 nm or more, more preferably 50 nm or more, from the viewpoint of improving the mechanical stability of the emulsion particles themselves, and is preferably 300 nm or less, more preferably 200 nm or less, from the viewpoint of forming a coating film that is excellent in UV resistance and UV appearance retention, water resistance, repeated freeze-thaw stability, and transparency.
[0081] In this specification, the average particle size of emulsion particles means the volume average particle size measured using a particle size distribution measuring device (manufactured by Particle Sizing Systems, product name: NICOMP Model 380) using the dynamic light scattering method.
[0082] The resin emulsion of the present invention may be, for example, (1) A resin emulsion obtained by emulsion polymerization of the monomer component containing a triazine-based ultraviolet absorber, the resin emulsion containing emulsion particles containing the triazine-based ultraviolet absorber. (2) A resin emulsion obtained by mixing a resin emulsion containing emulsion particles obtained by emulsion polymerization of the monomer component with a triazine-based ultraviolet absorber. However, the present invention is not limited to these examples. Among these resin emulsions, from the viewpoint of forming a coating film excellent in resistance to ultraviolet transmission and ultraviolet appearance retention, a resin emulsion containing emulsion particles containing a triazine-based ultraviolet absorber is preferred.
[0083] The total content of the emulsion particles and the non-volatile matter of the triazine-based UV absorber in the resin emulsion of the present invention is preferably 30% by mass or more, more preferably 40% by mass or more, from the viewpoint of improving productivity, and is preferably 70% by mass or less, more preferably 60% by mass or less, from the viewpoint of improving handleability.
[0084] The total content of non-volatile matter in the resin emulsion was calculated by weighing 1 g of the resin emulsion, drying it in a hot air dryer at 110°C for 1 hour, and calculating the non-volatile matter from the resulting residue using the formula: [Total content of non-volatile matter in resin emulsion (mass%)] = ([mass of residue] ÷ [1 g of resin emulsion]) × 100 This means the value calculated based on
[0085] The minimum film-forming temperature of the resin emulsion of the present invention is preferably 100° C. or lower, more preferably 70° C. or lower, from the viewpoint of forming a coating film excellent in UV resistance, UV appearance retention, water resistance, stability against repeated freezing and thawing, and transparency. The minimum film-forming temperature of the resin emulsion can be adjusted, for example, by adjusting the glass transition temperature of the entire emulsion particle or the glass transition temperature of the outermost resin layer.
[0086] In this specification, the minimum film-forming temperature of a resin emulsion means the temperature at which cracks appear when the resin emulsion is applied with an applicator to a thickness of 0.2 mm on a glass plate placed on a thermal gradient tester.
[0087] The resin emulsion of the present invention obtained as described above may contain, for example, a crosslinking agent, if necessary. Examples of crosslinking agents include melamine-based crosslinking agents, oxazoline-based crosslinking agents, acrylamide-based crosslinking agents, polyamide-based crosslinking agents, epoxy-based crosslinking agents, isocyanate-based crosslinking agents, aziridine-based crosslinking agents, titanate-based crosslinking agents, urea-based crosslinking agents, alkyl alcohol-modified urea-based crosslinking agents, hydrazine compounds, carbodiimide compounds, zirconium compounds, zinc compounds, titanium compounds, and polyvalent metal compounds such as aluminum compounds, but the present invention is not limited to only these examples. These crosslinking agents may be used alone or in combination of two or more. The amount of the crosslinking agent is preferably set appropriately depending on the type of the crosslinking agent, etc. Among the crosslinking agents, oxazoline-based crosslinking agents and hydrazine-based crosslinking agents are preferred from the viewpoint of forming a coating film that is excellent in UV transmission resistance and UV appearance retention, and is excellent in water resistance, freeze-thaw repeat stability, and transparency.
[0088] Examples of oxazoline crosslinking agents include 2,2'-bis(2-oxazoline), 1,2-bis(2-oxazoline-2-yl)ethane, 1,4-bis(2-oxazoline-2-yl)butane, 1,8-bis(2-oxazoline-2-yl)butane, 1,4-bis(2-oxazoline-2-yl)cyclohexane, 1,2-bis(2-oxazoline-2-yl)benzene, 1,3-bis(2-oxazoline-2-yl)benzene, 2-vinyl-2-oxazoline, 2-vinyl-4-methyl-2-oxazoline, 2-vinyl-5-methyl-2-oxazoline, 2-isopropenyl-2-oxazoline, 2-isopropenyl-4-methyl-2-oxazoline, and 2-isopropenyl-5-ethyl-2-oxazoline, but the present invention is not limited to these examples. These oxazoline crosslinking agents may be used alone or in combination of two or more. Oxazoline crosslinking agents are commercially readily available, and examples of such agents include those manufactured by Nippon Shokubai Co., Ltd. under the trade names of Epocross WS-500, Epocross WS-700, Epocross K-2010, Epocross K-2020, and Epocross K-2030, but the present invention is not limited to these examples.
[0089] Examples of hydrazine crosslinking agents include adipic acid dihydrazide, polymers having dihydrazide groups, etc., but the present invention is not limited to these examples. These compounds may be used alone or in combination of two or more kinds.
[0090] The resin emulsion of the present invention forms a coating film that is excellent in resistance to ultraviolet transmission and ultraviolet appearance retention, as well as in water resistance, stability against repeated freezing and thawing, and transparency, and can therefore be suitably used, for example, in topcoat paints known as topcoats that are applied to the surfaces of building exteriors, ceramic building materials, and the like.
[0091] The topcoat paint of the present invention contains the resin emulsion of the present invention. The total content of the emulsion particles and the non-volatile content of the triazine-based ultraviolet absorber in the solid content contained in the topcoat paint of the present invention is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more, with the upper limit being 100% by mass, from the viewpoint of forming a coating film excellent in ultraviolet transmission resistance and ultraviolet appearance retention, water resistance, repeated freeze-thaw stability, and transparency.
[0092] The topcoat paint of the present invention may contain only the resin emulsion of the present invention, or may contain, if necessary, pigments, additives, etc.
[0093] Examples of the pigment include organic pigments and inorganic pigments. These pigments may be used alone or in combination of two or more kinds.
[0094] Examples of organic pigments include azo pigments, azomethine pigments, methine pigments, anthraquinone pigments, phthalocyanine pigments, perinone pigments, perylene pigments, diketopyrrolopyrrole pigments, thioindigo pigments, iminoisoindoline pigments, iminoisoindolinone pigments, quinacridone pigments such as quinacridone red and quinacridone violet, flavanthrone pigments, indanthrone pigments, anthrapyrimidine pigments, carbazole pigments, monoarylide yellow, diarylide yellow, benzimidazolone yellow, tolyl orange, naphthol orange, and quinophthalone pigments, but the present invention is not limited to these examples. These organic pigments may be used alone or in combination of two or more.
[0095] Examples of inorganic pigments include titanium dioxide, red iron oxide, black iron oxide, iron oxide, chromium oxide green, carbon black, ferric ferrocyanide (Prussian blue), ultramarine, lead chromate, etc., as well as flat pigments such as mica, clay, aluminum powder, talc, and aluminum silicate, and extender pigments such as calcium carbonate, magnesium hydroxide, aluminum hydroxide, barium sulfate, and magnesium carbonate, but the present invention is not limited to these examples. These inorganic pigments may be used alone or in combination of two or more kinds.
[0096] The solids content of the pigment in the topcoat paint of the present invention is 0% by mass or more, but from the viewpoint of increasing the hardness of the coating film and improving the design or hiding power of the coating film formed, it is preferably 3% by mass or more, more preferably 5% by mass or more, and from the viewpoint of improving the film-forming properties, it is preferably 50% by mass or less, more preferably 40% by mass or less.
[0097] The solid content of the pigment in the topcoat paint of the present invention is determined by the formula: [Solid content of pigment in topcoat paint (mass%)] = [(Solid content of pigment) / (Solid content of resin emulsion + Solid content of pigment)] x 100 This means the value calculated based on
[0098] Examples of additives include aggregates, leveling agents, antioxidants, polymerization inhibitors, fillers, coupling agents, rust inhibitors, antibacterial agents, metal deactivators, wetting agents, defoamers, surfactants, reinforcing agents, plasticizers, lubricants, antifogging agents, anticorrosive agents, pigment dispersants, flow regulators, peroxide decomposers, mold decolorizers, fluorescent brighteners, organic flame retardants, inorganic flame retardants, drip prevention agents, melt flow modifiers, antistatic agents, algae inhibitors, fungicides, flame retardants, slip agents, metal chelating agents, antiblocking agents, heat stabilizers, processing stabilizers, dispersants, thickeners, rheology control agents, foaming agents, antiaging agents, preservatives, antistatic agents, silane coupling agents, and antioxidants, but the present invention is not limited to these examples. These additives may be used alone or in combination of two or more.
[0099] The amount of the additive varies depending on the type of the additive and cannot be determined in general, so it is preferable to determine it appropriately depending on the type of the additive.
[0100] The total non-volatile content in the topcoat paint of the present invention cannot be determined in general terms because it varies depending on the application of the topcoat paint of the present invention, but it is usually preferably 10 to 70 mass %.
[0101] The topcoat paint of the present invention can be easily prepared, for example, by mixing the resin emulsion of the present invention and, if necessary, a pigment, additives, water, etc.
[0102] The topcoat paint of the present invention obtained as described above contains the resin emulsion of the present invention, and therefore forms a coating film that is excellent in UV transmission resistance and UV appearance retention, and is excellent in water resistance, stability against repeated freezing and thawing, and transparency, and can be suitably used for surface finishing of substrates made of materials such as metal, glass, porcelain, concrete, siding board, resin, etc. Therefore, the topcoat paint of the present invention can be suitably used as a topcoat paint called a top coat that is applied to the exterior of buildings, ceramic building materials, etc.
[0103] Examples of ceramic building materials include roofing tiles and exterior wall materials. Ceramic building materials are obtained by adding inorganic fillers, fibrous materials, etc. to a hydraulic adhesive material that is the raw material of an inorganic hardened body, molding the resulting mixture, and curing and hardening the resulting molded body. Examples of inorganic building materials that constitute the exterior of buildings include flexible boards, calcium silicate boards, gypsum slag perlite boards, wood chip cement boards, precast concrete boards, ALC boards, gypsum boards, etc.
[0104] A topcoat paint is usually applied to the surface of such building materials to impart a desired design. The topcoat paint of the present invention can be suitably used as this topcoat paint.
[0105] The topcoat paint of the present invention may be applied in one layer by itself, or may be applied by overcoating two or more layers. When applying two or more layers, only some of the layers may be formed by the topcoat paint of the present invention, or all of the layers may be formed by the topcoat paint of the present invention. Examples of overcoating include a method in which a paint for a first layer (e.g., an undercoat layer) is applied to a substrate that has been subjected to a primer treatment or a sealer treatment, and then dried, and then a paint for a second layer (e.g., a topcoat layer) is applied and dried, but the present invention is not limited to such a method. Examples of methods for applying the topcoat paint of the present invention include application methods using a brush, a bar coater, an applicator, an air spray, an airless spray, a roll coater, a flow coater, etc., but the present invention is not limited to only such examples.
[0106] The coating film formed using the topcoat paint of the present invention may be dried, for example, at room temperature or by heating.
[0107] In addition, the thickness of the coating film formed using the topcoat paint of the present invention after drying is usually preferably about 1 to 100 μm, from the viewpoint of forming a coating film that has excellent resistance to ultraviolet light transmission and ultraviolet appearance retention, as well as excellent water resistance, stability against repeated freeze-thaw cycles, and transparency.
[0108] The amount of topcoat paint applied to a substrate varies depending on the type of substrate and cannot be determined in general. However, from the viewpoint of forming a coating film that has excellent resistance to UV transmission and UV appearance retention, water resistance, stability against repeated freeze-thawing, and transparency, the amount of topcoat paint applied is usually 10 to 200 g / m2 in non-volatile content. 2 It is preferable that the amount is about 100%. EXAMPLES
[0109] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples. In the following, "parts" means "parts by mass" unless otherwise specified.
[0110] Example 1 In a flask equipped with a dropping funnel, a stirrer, a nitrogen gas inlet tube, a thermometer, and a reflux condenser, 716 parts of deionized water were charged. In the dropping funnel, 417 parts of deionized water, 120 parts of a 25% aqueous solution of an emulsifier (manufactured by ADEKA Corporation, trade name: Adeka Reasorb SR-10), 290 parts of methyl methacrylate, 250 parts of cyclohexyl methacrylate, 200 parts of 2-ethylhexyl acrylate, 200 parts of n-butyl acrylate, 20 parts of hydroxyethyl methacrylate, and 30 parts of 4-methacryloyloxy-1,2,2,6,6-pentamethylpiperidine as monomer components, and the monomers were added. A pre-emulsion for dropping was prepared containing 10 parts of a triazine-based UV absorber (manufactured by BASF Japan Ltd., product name: TINUVIN400) so that the amount of triazine-based UV absorber per 100 parts of the components was 1 part, and 154 parts of it, which is 10% of the total amount of the monomer components and the triazine-based UV absorber, was added to the flask, and the temperature was raised to 80°C while slowly blowing in nitrogen gas, and 10 parts of a 5% ammonium persulfate aqueous solution was added to start polymerization. Thereafter, the remaining part of the pre-emulsion for dropping and 30 parts of a 5% ammonium persulfate aqueous solution were uniformly dropped into the flask over 240 minutes.
[0111] After the dropwise addition was completed, the contents of the flask were maintained at 80°C for 60 minutes, and the pH was adjusted to 8 by adding 25% aqueous ammonia to terminate the polymerization. The resulting reaction liquid was cooled to room temperature, and then filtered through a 300 mesh (JIS mesh, the same applies below) wire mesh to prepare a resin emulsion. The compositions of the monomer components and triazine-based ultraviolet absorbers used as the resin raw materials of the resulting resin emulsion are shown in Table 1.
[0112] Example 2 In a flask equipped with a dropping funnel, a stirrer, a nitrogen gas inlet tube, a thermometer, and a reflux condenser, 716 parts of deionized water were charged. In the lower funnel, 209 parts of deionized water, 60 parts of a 25% aqueous solution of an emulsifier (manufactured by ADEKA Corporation, trade name: ADEKA REASOAP SR-10), 307.5 parts of methyl methacrylate, 125 parts of cyclohexyl methacrylate, 40 parts of 2-ethylhexyl acrylate, 10 parts of hydroxyethyl methacrylate, and 15 parts of 4-methacryloyloxy-1,2,2,6,6-pentamethylpiperidine as monomer components, and 100 parts of trimethylol methacrylate per 100 parts of the total monomer components were added. A first-stage pre-emulsion was prepared containing 2.5 parts of a triazine-based UV absorber (manufactured by BASF Japan Ltd., product name: TINUVIN400) so that the amount of the triazine-based UV absorber was 0.5 parts, of which 77 parts, which corresponds to 10% of the total amount of the monomer component and the triazine-based UV absorber, was added to the flask, and the temperature was raised to 80°C while slowly blowing in nitrogen gas, and 10 parts of a 5% ammonium persulfate aqueous solution was added to start polymerization. After that, the remaining part of the pre-emulsion for dropping and 15 parts of a 5% ammonium persulfate aqueous solution were uniformly dropped into the flask over 120 minutes.
[0113] After the dropwise addition was completed, the contents of the flask were maintained at 80° C. for 60 minutes, and then 209 parts of deionized water, 60 parts of a 25% aqueous solution of an emulsifier (manufactured by ADEKA CORPORATION, trade name: ADEKA REASORB SR-10), 125 parts of cyclohexyl methacrylate, 147.5 parts of 2-ethylhexyl acrylate, 200 parts of n-butyl acrylate, 10 parts of hydroxyethyl methacrylate, and 15 parts of 4-methacryloyloxy-1,2,2,6,6-pentamethylpiperidine as monomer components, and a pre-emulsion for second-stage dropping containing 2.5 parts of a triazine-based ultraviolet absorber (manufactured by BASF Japan Ltd., trade name: TINUVIN400) such that the amount of the triazine-based ultraviolet absorber per 100 parts of the total monomer components was 0.5 parts, and 15 parts of a 5% aqueous solution of ammonium persulfate were uniformly added dropwise into the flask over a period of 120 minutes.
[0114] After the dropwise addition was completed, the contents of the flask were maintained at 80°C for 60 minutes, and the pH was adjusted to 8 by adding 25% aqueous ammonia to terminate the polymerization. The resulting reaction liquid was cooled to room temperature and then filtered through a 300-mesh wire screen to prepare a resin emulsion. The compositions of the monomer components and UV absorbers used as the resin raw materials of the resulting resin emulsion are shown in Table 1.
[0115] Examples 3 to 5 A resin emulsion was prepared in the same manner as in Example 2, except that the monomer components and triazine-based ultraviolet absorbers in Example 2 were changed as shown in Table 1. The compositions of the monomer components and triazine-based ultraviolet absorbers used as the resin raw materials of the obtained resin emulsion are shown in Table 1.
[0116] Example 6 Into a flask equipped with a dropping funnel, a stirrer, a nitrogen gas inlet tube, a thermometer and a reflux condenser, 716 parts of deionized water was placed. A pre-emulsion for the first drop was prepared in a funnel containing 139 parts of deionized water, 40 parts of a 25% aqueous solution of an emulsifier (ADEKA Corporation, trade name: ADEKA REASOAP SR-10), 185 parts of methyl methacrylate, 125 parts of cyclohexyl methacrylate, 10 parts of hydroxyethyl methacrylate, and 10 parts of 4-methacryloyloxy-1,2,2,6,6-pentamethylpiperidine as monomer components, and 10 parts of a triazine-based ultraviolet absorber (BASF Japan Ltd., trade name: TINUVIN400) so that the amount of triazine-based ultraviolet absorber per 100 parts of the total monomer components was 3.1 parts. Of this pre-emulsion, 51 parts, which corresponds to 10% of the total amount of the monomer components and the triazine-based ultraviolet absorber, was added to the flask, and the temperature was raised to 80° C. while slowly blowing in nitrogen gas, and 10 parts of a 5% aqueous solution of ammonium persulfate was added to initiate polymerization. Thereafter, the remainder of the pre-emulsion for dropping and 10 parts of a 5% aqueous solution of ammonium persulfate were dropped uniformly into the flask over a period of 90 minutes.
[0117] After the dropwise addition was completed, the contents of the flask were maintained at 80° C. for 60 minutes, and then 139 parts of deionized water, 40 parts of a 25% aqueous solution of an emulsifier (manufactured by ADEKA CORPORATION, trade name: ADEKA REASOAP SR-10), 125 parts of cyclohexyl methacrylate, 175 parts of 2-ethylhexyl acrylate, 10 parts of 4-methacryloyloxy-1,2,2,6,6-pentamethylpiperidine, and 10 parts of γ-methacryloyloxypropyltrimethoxysilane as monomer components, and a pre-emulsion for second-stage dropping containing 10 parts of a triazine-based ultraviolet absorber (manufactured by BASF Japan Ltd., trade name: TINUVIN400) such that the amount of the triazine-based ultraviolet absorber per 100 parts of the total monomer components was 3.1 parts, and 10 parts of a 5% aqueous solution of ammonium persulfate were uniformly added dropwise into the flask over a period of 90 minutes.
[0118] After the dropwise addition was completed, the contents of the flask were maintained at 80° C. for 60 minutes, and then 139 parts of deionized water, 40 parts of a 25% aqueous solution of an emulsifier (manufactured by ADEKA CORPORATION, trade name: ADEKA REASOAP SR-10), 125 parts of cyclohexyl methacrylate, 140 parts of n-butyl methacrylate, 35 parts of 2-ethylhexyl acrylate, 10 parts of 4-methacryloyloxy-1,2,2,6,6-pentamethylpiperidine, and 10 parts of γ-methacryloyloxypropyltrimethoxysilane as monomer components, and a pre-emulsion for second-stage dropping containing 10 parts of a triazine-based ultraviolet absorber (manufactured by BASF Japan Ltd., trade name: TINUVIN400) such that the amount of the triazine-based ultraviolet absorber per 100 parts of the total monomer components was 3.1 parts, and 10 parts of a 5% aqueous solution of ammonium persulfate were uniformly added dropwise into the flask over a period of 90 minutes.
[0119] After the dropwise addition was completed, the contents of the flask were kept at 80°C for 60 minutes, and 25% aqueous ammonia was added. The pH was adjusted to 8 by heating, and the polymerization was terminated. After that, the mixture was filtered through a 300 mesh wire net to prepare a resin emulsion. The composition of the monomer components and triazine-based ultraviolet absorber used as the resin raw materials of the obtained resin emulsion is shown in Table 1.
[0120] Comparative Examples 1 to 4 Resin emulsions were prepared in the same manner as in Example 1, except that the monomer components and UV absorbents in Example 1 were changed as shown in Table 2. The compositions of the monomer components and UV absorbents used as the resin raw materials of the obtained resin emulsions are shown in Table 2.
[0121] The abbreviations in Tables 1 and 2 have the following meanings. MMA: Methyl methacrylate St: styrene CHMA: Cyclohexyl methacrylate 2EHA: 2-Ethylhexyl acrylate BA: n-butyl acrylate BMA: n-Butyl methacrylate HEMA: 2-hydroxyethyl methacrylate Polymerizable HALS: 4-methacryloyloxy-1,2,2,6,6-pentamethylpiperidine Non-polymerizable HALS: A mixture of bis(1,2,2,6,6-pentamethyl-4-piperidyl) sebacate and methyl 1,2,2,6,6-pentamethyl-4-piperidyl sebacate (manufactured by BASF Japan Ltd., trade name: TINUVIN 292) TMSMA: γ-methacryloyloxypropyltrimethoxysilane TIN400: Triazine-based UV absorber [manufactured by BASF Japan Ltd., product name: TINUVIN400] TIN1130: Benzotriazole-based UV absorber [manufactured by BASF Japan Ltd., product name: TINUVIN1130]
[0122] Moreover, the terms used in Tables 1 and 2 below have the following meanings. [Number of layers] The number of resin layers that make up the emulsion particles contained in the resin emulsion [Polymerizable HALS amount] Content of polymerizable HALS in all monomer components (mass%) [Amount of triazine-based ultraviolet absorber] Amount of triazine-based UV absorber per 100 parts of total monomer components (parts) [Non-volatile content] Non-volatile content in resin emulsion (mass%) [Tg of Layer 1] Glass transition temperature of the resin layer 1 constituting the emulsion particles (℃) [Tg of Layer 2] Glass transition temperature of the resin layer 2 constituting the emulsion particles (°C) [Tg of Layer 3] Glass transition temperature (°C) of the resin layer 3 constituting the emulsion particles [Total Tg] Glass transition temperature of emulsion particles themselves (℃)
[0123] In Table 1, Layers 1 to 3 indicate that the layers were formed by polymerization in that order. In Table 1, for the monomer components, "-" means that the corresponding layer was not formed.
[0124] [Table 1]
[0125] [Table 2]
[0126] Experimental Example Next, 20 parts of water, 5 parts of butyl cellosolve (manufactured by Kyowa Hakko Bio Co., Ltd.) and 5 parts of 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate (manufactured by Chisso Corporation, product number: CS-12) as a film-forming aid were added to 100 parts of the resin emulsion obtained in each Example or Comparative Example to obtain a mixed solution. The resulting mixed solution was added to a flask and rotated at a speed of 1500 min using a homodisper. -1 The mixture was stirred at 40° C. for 30 minutes, and a thickener (manufactured by Nippon Shokubai Co., Ltd., product name: Acryset WR-503A) was added to the flask so that the viscosity was 65 KU when measured at 25° C. using a Krebs unit viscometer (manufactured by Brookfield, product number: KU-1). 0.3 parts of an antifoaming agent (manufactured by San Nopco Ltd., product name: SN Defoamer 777) was added to the flask, and the mixture was stirred in this state for 30 minutes to prepare a sample for evaluation.
[0127] The evaluation paint obtained above was used to examine the physical properties of the resin emulsion, including water resistance, resistance to UV transmission, UV appearance retention, repeated freeze-thaw stability, and transparency, according to the following methods. The results are shown in Table 3.
[0128] (1)Water resistance The evaluation sample obtained above was applied to a glass plate (manufactured by Nippon Test Panel Co., Ltd., length: 70 mm, width: 150 mm, thickness: 2 mm) with an applicator so that the coating thickness after drying would be 50 μm, and then dried at a temperature of 80° C. for 2 hours.
[0129] Next, the 60° specular gloss of the surface on which the evaluation sample was applied (hereinafter referred to as gloss before immersion in hot water) was measured using a gloss meter (manufactured by Nippon Denshoku Industries Co., Ltd., product number: VG2000). The glass plate was then immersed in 50°C hot water for one day, after which it was removed from the water and the gloss of the coated surface of the glass plate (hereinafter referred to as gloss after immersion in hot water) was measured using the gloss meter. Formula: [Gloss retention (%)] = [[Gloss after immersion in hot water] ÷ [Gloss before immersion in hot water]] x 100 The water resistance was evaluated based on the following criteria.
[0130] [Evaluation Criteria] ◎: Gloss retention is 90% or more ○: Gloss retention is 75% or more and less than 90% △: Gloss retention is between 60% and 75% ×: Gloss retention is less than 60%
[0131] (2) UV transmission resistance A slate board (manufactured by Nippon Test Panel Co., Ltd., length: 70 mm, width: 150 mm, thickness: 6 mm) was coated with a sealer (manufactured by SK Chemical Co., Ltd., product name: EX Sealer) at 150 g / m using an air spray. 2 The coating was uniformly applied in an amount of 100g and dried at 23°C in the air for one week to form a coating film.
[0132] The following colored paint was applied to the coating film formed above using an applicator so that the coating thickness after drying would be 100 μm, and then dried in the atmosphere at 23° C. for one week. Then, the evaluation sample obtained above was applied to the coating film formed on the surface of the slate board using an applicator so that the coating thickness after drying would be 20 μm, and then dried in the atmosphere at 23° C. for one week to obtain a test board.
[0133] [Colored paint] Add 10 parts of water and 10 parts of 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate (manufactured by Chisso Corporation, product number: CS-12) as a film-forming aid to an acrylic resin emulsion (manufactured by Nippon Shokubai Co., Ltd., product name: Acryset EMN-210E), and mix in a homodisper at a rotation speed of 1500 min -1 The mixture was stirred at RT for 30 minutes, and 30 parts of the white paste described below and 0.5 parts of an antifoaming agent (manufactured by San Nopco Ltd., product name: SN Defoamer 777) were added. A thickener (manufactured by ADEKA Corporation, product name: Adekanol UH-420) was added so that the viscosity was 70 KU when measured at 25°C using a Krebs unit viscometer (manufactured by Brookfield Ltd., product number: KU-1). Subsequently, 5 parts of an aqueous color paste (manufactured by SK Chemical Co., Ltd., product name: SK Water-based Color (a mixture of Akasabi, Oka and Blue)) was added, and the mixture was stirred in this state for 30 minutes to prepare a colored paint.
[0134] [White paste] 210 parts of deionized water, 60 parts of dispersant (manufactured by Kao Corporation, product name: Demol EP), 50 parts of dispersant (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., product name: Discoat N-14), 10 parts of wetting agent (manufactured by Kao Corporation, product name: Emulgen LS-106), 60 parts of propylene glycol, 1000 parts of titanium oxide (manufactured by Ishihara Sangyo Kaisha, Ltd., product number: CR-95) and 200 parts of glass beads (diameter: 1 mm) were mixed in a homodisper at a rotation speed of 3000 min. -1 The mixture was dispersed at 40° C. for 60 minutes to prepare a white paste.
[0135] The side and back of the test plate obtained above were sealed with aluminum tape, and the color difference (L0, a0, b0) of the coating surface of the test plate was measured with a color difference meter (manufactured by Nippon Denshoku Industries Co., Ltd., product name: Spectroscopic Color Difference Meter SE-2000). Next, after carrying out an ultraviolet irradiation test for 800 hours under the following ultraviolet irradiation test conditions, the color difference (L1, a1, b1) of the coating surface of the test plate was measured, and the color tone change (ΔE) before and after the test was calculated using the formula: ΔE = [(L1 - L0) 2 +(a1-a0) 2 +(b1-b0) 2 ]1 / 2 The resistance to ultraviolet light transmission was evaluated based on the following criteria.
[0136] [Ultraviolet light irradiation test conditions] Testing machine: Metal weather meter (manufactured by Daipla Wintes Co., Ltd., product number: KU-R5 type) Irradiation: Irradiation for 4 hours in an atmosphere with a temperature of 65°C and a relative humidity of 50% (irradiation intensity: 65mW / cm 2 ) Humidity: Humidify for 4 hours in an atmosphere with a temperature of 65°C and a relative humidity of 98%. Water shower: Shower for 30 seconds before and after wetting
[0137] [Evaluation Criteria] ◎: ΔE is less than 1 ○: ΔE is 1 or more and less than 3 △: ΔE is 3 or more and less than 5 ×: ΔE is 5 or more
[0138] (3) Appearance retention against UV rays The side and back of the test plate obtained above were sealed with aluminum tape, and the 60° specular gloss of the coating surface of the test plate (hereinafter referred to as gloss before irradiation test) was measured with a gloss meter (manufactured by Nippon Denshoku Industries Co., Ltd., product number: VG2000). Next, after carrying out an ultraviolet irradiation test for 1000 hours under the same conditions as the ultraviolet irradiation test conditions described above, the 60° specular gloss of the coating surface of the test plate (hereinafter referred to as gloss after irradiation test) was measured with the gloss meter, and the change in gloss before and after the test (appearance retention rate %) was calculated using the formula: [Appearance retention rate (%)] = [[Gloss after irradiation test] ÷ [Gloss before irradiation test]] × 100 The appearance retention against ultraviolet light was evaluated based on the following criteria.
[0139] [Evaluation Criteria] ◎: Appearance retention rate is 90% or more ○: Appearance retention rate is 75% or more but less than 90% △: Appearance retention rate is 60% or more but less than 75% ×: Appearance retention rate is less than 60%
[0140] (4) Stability after repeated freezing and thawing The sides of the test plate obtained above were sealed with a silicone-based bath bond (manufactured by Konishi Co., Ltd.), and then a freeze-thaw tester was used to cool the plate to -20°C in the air, freezing it for 2 hours, and then immersing it in 20°C water for 1 hour (this constitutes one cycle).The above procedure was repeated 300 times, with the condition of cracks on the coating surface of the test plate being observed using a 30x magnifying glass every 100 cycles, and the repeated freeze-thaw stability was evaluated based on the following evaluation criteria.
[0141] [Evaluation Criteria] ◎: No problems even after 300 cycles ○: No problem after 200 cycles, but cracks occurred after 300 cycles △: No problem after 100 cycles, but cracks appear after 200 cycles ×: Cracks occurred after 100 cycles
[0142] (5) Transparency The difference in transparency (haze) between the polyester film and the coating was measured using a turbidity meter (manufactured by Nippon Denshoku Industries Co., Ltd., product number: NDH300A) in accordance with JIS K7105, and the transparency of the coating was evaluated based on the following evaluation criteria.
[0143] [Evaluation Criteria] ◎: Haze difference is less than 0.5% 〇: Haze difference is 0.5% or more and less than 1% △: Haze difference is 1% or more but less than 2% ×: Haze difference is 2% or more
[0144] (6) Overall evaluation Next, for each physical property, a ◎ rating was assigned 20 points, a ○ rating 15 points, a △ rating 10 points, and an × rating 0 points, and a total score (maximum score: 100 points) was calculated, and the results are shown in the overall rating column of Table 3. Anything with even one × in the rating is considered a failure.
[0145] [Table 3]
[0146] From the results shown in Table 3, it can be seen that the resin emulsions obtained in each Example all form coating films excellent in UV resistance and UV appearance retention. It can also be seen that the resin emulsions obtained in each Example all form coating films excellent in water resistance, freeze-thaw cycle stability, and transparency. Therefore, it can be seen that the resin emulsions obtained in each Example all form coating films excellent overall in UV resistance, UV appearance retention, water resistance, freeze-thaw cycle stability, and transparency. [Industrial Applicability]
[0147] The resin emulsion of the present invention can be suitably used for surface finishing of substrates made of materials such as metal, glass, porcelain, concrete, siding board, resin, etc. Therefore, the resin emulsion of the present invention can be suitably used for applications such as ceramic building materials, automobiles, buildings, civil engineering structures, etc., particularly for topcoat paints called topcoats that are applied to the exteriors of buildings and the surfaces of ceramic building materials, etc.
Claims
1. A resin emulsion containing emulsion particles containing a triazine-based ultraviolet absorber, the emulsion particles having a plurality of resin layers, a polymerizable hindered amine-based light-stable monomer is used in a content of 0.1 to 25 mass% in a monomer component used as a raw material for the plurality of resin layers, the monomer component contains a triazine-based ultraviolet absorber, the amount of the triazine-based ultraviolet absorber is 0.1 to 5 mass parts per 100 mass parts of the monomer component, and the polymerizable hindered amine-based light-stable monomer is 4-(meth)acrylonitrile. and at least one polymerizable hindered amine-based light-stable monomer selected from the group consisting of 2-[4-[(2-hydroxy-3-dodecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-tri ... or 2-[4-[(2-hydroxy-3-tridecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine is used as the triazine-based ultraviolet absorber. )oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-(2'-ethyl)hexyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2,4-bis(2-hydroxy-4-butyloxyphenyl)-6-(2,4-bis-butyloxyphenyl)-1,3,5-triazine, hydroxyphenyl triazine, 2-(2-hydroxy-4-[1-octyloxyca and wherein at least one hydroxyphenyltriazine-based ultraviolet absorber selected from the group consisting of 2,4,6-tris(2-hydroxy-4-hexyloxy-3-methylphenyl)-1,3,5-triazine is used, and the emulsion particles are emulsion particles having, among the resin layers constituting the emulsion particles, a resin layer having the highest glass transition temperature as a layer located more inside than the outermost layer.
2. 2. The resin emulsion according to claim 1, wherein the monomer component contains a monomer other than the polymerizable hindered amine-based light-stable monomer in an amount of 75 to 99.9% by mass.
3. 3. The resin emulsion according to claim 1, wherein the monomer components constituting each of the plurality of resin layers each contain a triazine-based ultraviolet absorber.
4. The resin emulsion according to any one of claims 1 to 3, wherein the plurality of resin layers is three resin layers.
5. A method for producing a resin emulsion containing emulsion particles containing a triazine-based ultraviolet absorber, the method comprising the steps of: polymerizing a monomer component in the presence of the triazine-based ultraviolet absorber to produce a resin emulsion containing emulsion particles having a plurality of resin layers; using a monomer component containing a polymerizable hindered amine-based light-stable monomer at a content of 0.1 to 25% by mass as the monomer component; incorporating a triazine-based ultraviolet absorber into the monomer component; and adjusting the amount of the triazine-based ultraviolet absorber per 100 parts by mass of the monomer component to 0.1 to 5 parts by mass. As the polymerizable hindered amine-based light-stable monomer, at least one polymerizable hindered amine-based light-stable monomer selected from the group consisting of 4-(meth)acryloyloxy-2,2,6,6-tetramethylpiperidine and 4-(meth)acryloyloxy-1,2,2,6,6-pentamethylpiperidine is used, and as the triazine-based ultraviolet absorber, 2-[4-[(2-hydroxy-3-dodecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-[ (2-hydroxy-3-tridecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-(2'-ethyl)hexyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2,4-bis(2-hydroxy-4-butyloxyphenyl)-6-(2,4-bis-butyloxyphenyl)-1,3,5-triazine, hydroxyphenyl triazine, 2-(2-hydroxy- and adjusting the glass transition temperature of an inner layer of each resin layer constituting the emulsion particle so that the glass transition temperature of the inner layer is the highest among the resin layers constituting the emulsion particle.
6. 6. The method for producing a resin emulsion according to claim 5, wherein the content of the monomer other than the polymerizable hindered amine-based light-stable monomer in the monomer component is adjusted to 75 to 99.9 mass %.
7. 7. The method for producing a resin emulsion according to claim 5 or 6, wherein when a monomer component is polymerized in the presence of the triazine-based ultraviolet absorber, a triazine-based ultraviolet absorber is contained in each of the monomer components constituting each of the plurality of resin layers.
8. The method for producing a resin emulsion according to any one of claims 5 to 7, wherein the plurality of resin layers is three resin layers.
Citation Information
Patent Citations
Emulsion having high durability
JP1998120724A
Coating material
JP2003025521A
Aqueous coating composition, and method of manufacturing the same
JP2011213941A
Resin emulsion for coating materials
WO2017047749A1