METHACRYLIC COPOLYMER AND PROCESS FOR PRODUCING SAME - Patent application
A methacrylic copolymer with specific compositional and molecular weight control through continuous bulk polymerization and adiabatic flash evaporation addresses inefficiencies in existing methods, achieving high heat resistance, low water absorption, and reduced birefringence for optical applications.
Patent Information
- Application Number
- JP2021564078
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-09-30
- Filing Date
- 2020-12-11
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-12-11
AI Technical Summary
Existing methacrylic copolymers containing methyl methacrylate and α-methylstyrene units do not achieve optimal balance of properties such as heat resistance, low water absorption, and low birefringence, and their production methods are inefficient in terms of productivity and flexibility.
A methacrylic copolymer composed of 70 to 93% methyl methacrylate, 7 to 30% α-methylstyrene, and optionally other copolymerizable monomers, produced through continuous bulk polymerization in a tank reactor with controlled polymerization conditions to achieve a specific molecular weight distribution and high conversion rates, followed by adiabatic flash evaporation to remove unreacted monomers.
The resulting copolymer exhibits high heat resistance, low water absorption, and minimal birefringence, suitable for optical applications with improved productivity and flexibility in production processes.
Smart Images

Figure 0007572377000001 
Figure 0007572377000002 
Figure 0007572377000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a methacrylic copolymer essentially containing methyl methacrylate units and α-methylstyrene units, and a method suitable for producing the same. [Background technology]
[0002] Methacrylic copolymers essentially containing methyl methacrylate units and α-methylstyrene units are known as resin materials having excellent transparency.
[0003] For example, Patent Document 1 discloses a resin material for optical prisms or lenses, which is composed of a copolymer composed of 10 to 65% by weight of α-methylstyrene units, 10 to 40% by weight of methyl methacrylate units, and 10 to 80% by weight of styrene units, and which has a weight average molecular weight in the range of 50,000 to 400,000, a Vicat softening temperature of 105° C. or higher, a refractive index of 1.550 to 1.580, a water absorption rate of 0.13% or lower, and a birefringence value of 300 nm or lower when made into a prism with a thickness of 10 mm.
[0004] Patent Document 2 discloses a molding material comprising a copolymer having a weight-average molecular weight in the range of 50,000 to 200,000, a ratio of α-methylstyrene units in the range of 10 to 30% by weight, a ratio of methyl methacrylate units in the range of 40 to 70% by weight, and a ratio of styrene units in the range of 10 to 30% by weight, the copolymer having an MFR value in the range of 4 to 18 g / 10 min at 220°C under a load of 10 kg, and the copolymer having a Vicat softening temperature of 130°C or higher.
[0005] Patent Document 3 discloses a resin molded article in which the surface of a transparent thermoplastic plastic is coated with an α-methylstyrene copolymer having a weight-average molecular weight in the range of 50,000 to 200,000, and containing 10 to 40% by weight of α-methylstyrene units, 40 to 90% by weight of methyl methacrylate units, and 0 to 30% by weight of monomer units copolymerizable therewith.
[0006] α-Methylstyrene-based copolymers having a ring structure in the main chain, such as a copolymer consisting of α-methylstyrene-methyl methacrylate-maleic anhydride, are known as molding materials having excellent transparency, heat resistance, etc. (Patent Document 4, Patent Document 5, etc.) Various methods for producing a copolymer consisting of α-methylstyrene-methyl methacrylate-maleic anhydride have been proposed.
[0007] For example, Patent Document 6 discloses a method for producing a methyl methacrylate-α-methylstyrene-maleic anhydride copolymer, which comprises adding 5 to 15% (based on the weight of the monomer mixture) of maleic anhydride to a monomer mixture consisting of a predominant amount of methyl methacrylate and a minor amount of α-methylstyrene, and copolymerizing the mixture in the presence of a free radical generating catalyst by a bulk or solution polymerization method, or a combination of these.
[0008] Patent Document 7 discloses a method for producing an α-methylstyrene copolymer, which is characterized by using α-methylstyrene, methyl methacrylate, and maleic anhydride as monomers, adding a polyfunctional organic peroxide having a 10-hour half-life temperature of 60 to 110°C as a polymerization initiator in an amount of 0.05 to 1.0% by weight based on the total amount of monomers, and carrying out bulk polymerization at 100 to 150°C.
[0009] Patent Document 8 discloses a method for producing a heat-resistant methacrylic resin plate, which comprises supplying a polymerization raw material consisting of a polymerizable mixture of 40 to 89% by weight of methyl methacrylate monomer, 1 to 20% by weight of α-methylstyrene, 5 to 20% by weight of styrene, and 5 to 20% by weight of maleic anhydride from an upstream end of a molding space formed by the opposing surfaces of two endless belts running opposite to each other with a certain gap therebetween and a gasket running following the running of the belts while being sandwiched between the belts, 0.01 to 0.5 parts by weight of an acidic phosphoric acid ester per 100 parts by weight of the mixture, and a polymerization initiator, continuously polymerizing the mixture inside the molding space to a polymerization rate of 98.5% or more, and continuously taking out a heat-resistant methacrylic resin plate from the downstream end.
[0010] Patent Document 9 discloses a monomer mixture containing 70 to 95% by mass of methyl methacrylate, 0 to 15% by mass of α-methylstyrene, 0 to 20% by mass of styrene, and 2 to 15% by mass of maleic anhydride, in which the total amount of α-methylstyrene and styrene is in a molar ratio relative to maleic anhydride within a range of 1.0 to 2.5, and which has an oxygen permeability of 1.5×10 -13 (mol m -2 ·s -1 ·Pa -1 ) or less in a polymerization vessel containing at least one polymer membrane layer, which is then sealed and polymerized by heating in the gas phase. In this production method, Reference 9 states that it is preferable to add a terpenoid compound to the monomer mixture and polymerize it.
[0011] Patent Document 10 discloses a method for producing a heat-resistant methacrylic resin, which comprises supplying a monomer mixture consisting of methyl methacrylate, maleic anhydride and at least one aromatic vinyl compound to a polymerization reactor and carrying out solution polymerization or bulk polymerization at a temperature of 100 to 180°C to obtain a resin consisting of a copolymer consisting of 35 to 98% by weight of methyl methacrylate units, 1 to 40% by weight of maleic anhydride units and 1 to 35% by weight in total of aromatic vinyl compound units and having an intrinsic viscosity of 0.35 to 3.5 dl / g.
[0012] As a method for producing a methyl methacrylate copolymer, which conceptually includes an α-methylstyrene-methyl methacrylate copolymer, for example, Patent Document 11 discloses a method for continuously producing a methyl methacrylate-based syrup, which is characterized in that a monomer mainly composed of methyl methacrylate is continuously supplied to a first reaction zone of a reaction zone in which two or more reaction zones in which substantially complete mixing is achieved are arranged in series, a radical polymerization initiator is continuously supplied to at least two reaction zones including the first reaction zone, and conditions in each reaction zone are maintained so that the residual initiator concentration in at least each reaction zone to which the polymerization initiator is supplied is 1 / 2 to 1 / 1000 times the concentration of the supplied initiator, and a polymer is produced while the reaction mixture passes through each reaction zone in sequence to obtain a syrup. Patent Document 11 states that other monomers such as α-methylstyrene can be used within the range of 20% by weight or less in the monomer mainly composed of methyl methacrylate.
[0013] Patent Document 12 discloses a process for continuously supplying methyl methacrylate (1), a chain transfer agent (3), and a radical polymerization initiator (4) to a tank reactor while controlling the respective amounts thereof, a process for obtaining a reaction product by bulk polymerization in the tank reactor at a polymerization conversion rate of 40 to 70% by mass, a process for recovering a mixture (A) containing methyl methacrylate (1') and the chain transfer agent (3') from the reaction product, and a process for continuously supplying the mixture (A) to the tank reactor, in which the control of the respective amounts of methyl methacrylate (1) and the chain transfer agent (3) supplied to the tank reactor is performed based on information including the amount of mixture (A) supplied to the tank reactor and the respective proportions of methyl methacrylate (1') and the chain transfer agent (3') in the mixture (A), and the complete mixing time (θ M [hr]), and the half-life of the radical polymerization initiator at the temperature in the tank reactor (τ 1 / 2 [hr]), stirring power of tank reactor (PV [kW / m 3 ]), the average residence time of the reactants in the tank reactor (θ [hr]) and the radical polymerization initiator concentration in the reactants (I [ppm]) θ M >τ 1 / 2 , and PV × θ × I × τ 1 / 2 <4 The present invention discloses a method for producing a (meth)acrylic resin composition that satisfies the above requirements.
[0014] Patent Document 13 discloses a method for continuously bulk polymerizing a monomer mixture containing methyl methacrylate as a main component in a single complete mixing reactor without using a solvent. In the method, an inert gas is introduced into the monomer to reduce the dissolved oxygen in the monomer to 1 ppm or less, and then a radical initiator having a half-life of 0.5 to 120 seconds at the polymerization temperature is used to polymerize the monomer mixture in a continuous manner without using a solvent. 3 The present invention discloses a method for producing a colorless and transparent methacrylic polymer with excellent moldability, which is characterized by setting the average residence time so that the ratio of the half-life of the radical initiator at the polymerization temperature to the average residence time is 1 / 200 to 1 / 10,000 while stirring with a stirrer having a stirring power consumption of 0.5 to 20 kW per unit time, and polymerizing at 130 to 160°C so that the monomer conversion rate is 45 to 70%.
[0015] Patent Document 14 describes a method for producing a methacrylic polymer in which a monomer mainly composed of methyl methacrylate is bulk polymerized in a complete mixing type reaction tank to give a polymer content of 40 to 70% by weight. The reaction tank is filled with liquid with substantially no gas phase, and is in an adiabatic state with substantially no heat coming in or out from the outside of the reaction tank. The polymerization temperature is 120 to 180°C, the average residence time is 15 minutes to 2 hours, a radical initiator with a half-life of 1 minute or less at the polymerization temperature is used, and the concentration C (mol / 100 g monomer) of the radical initiator is 4×10 -5 ·exp(0.019T) <C·θ<3×10 -8 ·exp(0.079T) (wherein θ represents the average residence time (min), and T represents the polymerization temperature (°C).) Patent Document 14 states that in the monomers mainly composed of methyl methacrylate, other vinyl monomers such as α-methylstyrene can be used within the range of 20% by weight or less.
[0016] Patent Document 15 discloses a method for producing an α-methylstyrene copolymer comprising 6 to 34% by weight of α-methylstyrene units, 0 to 50% by weight of styrene units, and 94 to 16% by weight of methyl methacrylate units, characterized in that, when producing the α-methylstyrene copolymer, 0.05 to 1.0 part by weight of a polyfunctional organic peroxide having a 10-hour half-life temperature in the range of 60 to 110°C is added as a polymerization initiator to 100 parts by weight of a monomer comprising 6 to 40% by weight of α-methylstyrene, 0 to 50% by weight of styrene, and 94 to 16% by weight of methyl methacrylate, and bulk polymerization is carried out at 100 to 150°C.
[0017] Patent Document 16 discloses a method for producing an α-methylstyrene copolymer containing 10 to 35% by weight of α-methylstyrene units, 94 to 15% by weight of methyl methacrylate units, and 0 to 50% by weight of vinyl monomers copolymerizable with these monomers as constituent units, by adding 0.05 to 1.0 part by weight of an organic peroxide as a polymerization initiator and 0.01 to 0.15 part by weight of divinylbenzene to 100 parts by weight of the monomers, and polymerizing at 100 to 150° C. Patent Document 16 states that this production method enables continuous production of an α-methylstyrene copolymer by bulk polymerization. [Prior art documents] [Patent documents]
[0018] [Patent Document 1] WO2005 / 070978A [Patent Document 2] Japanese Patent Application Publication No. 4-300908 [Patent Document 3] Japanese Patent Application Publication No. 5-59321 [Patent Document 4] Japanese Patent Publication No. 152758 / 1983 [Patent Document 5] Japanese Patent Publication No. 155443 / 1983 [Patent Document 6] Special Publication No. 49-10156 [Patent Document 7] Japanese Patent Application Publication No. 4-300907 [Patent Document 8] Japanese Patent Application Publication No. 61-271313 [Patent Document 9] JP 2001-270905 A [Patent Document 10] Japanese Patent Application Laid-open No. 60-147417 [Patent Document 11] Japanese Patent Application Publication No. 54-54189 [Patent Document 12] WO2015 / 099118A1 [Patent Document 13] Japanese Patent Application Publication No. 3-111408 [Patent Document 14] Japanese Patent Application Publication No. 7-126308 [Patent Document 15] Japanese Patent Application Publication No. 4-218515 [Patent Document 16] Japanese Patent Application Publication No. 4-328111 Summary of the Invention [Problem to be solved by the invention]
[0019] An object of the present invention is to provide a novel copolymer essentially containing methyl methacrylate units and α-methylstyrene units, and a method for producing the copolymer suitable for producing the copolymer. [Means for solving the problem]
[0020] The copolymer of the present invention includes the following embodiments.
[0021] [1] A methacrylic copolymer comprising 70 to 93 mass% of methyl methacrylate units, 7 to 30 mass% of α-methylstyrene units, and 0 to 23 mass% of other monomer units copolymerizable therewith, and satisfying the relationship of formula (1). (|A B |) / B < 0.05 (1) Here, A is the molecular weight at the peak top in the differential molecular weight distribution curve obtained by gel permeation chromatography measurement using a differential refractive index detector, and B is the molecular weight at the peak top in the differential molecular weight distribution curve obtained by gel permeation chromatography measurement using an absorbance detector with a detection wavelength of 254 nm.
[0022] [2] A methacrylic copolymer comprising 70 to 93 mass% of methyl methacrylate units, 7 to 30 mass% of α-methylstyrene units, and 0 to 10 mass% of other monomer units copolymerizable therewith, and satisfying the relationship of formula (1). (|A B |) / B < 0.05 (1) Here, A is the molecular weight at the peak top in the differential molecular weight distribution curve obtained by gel permeation chromatography measurement using a differential refractive index detector, and B is the molecular weight at the peak top in the differential molecular weight distribution curve obtained by gel permeation chromatography measurement using an absorbance detector with a detection wavelength of 254 nm.
[0023] [3] The methacrylic copolymer according to [1] or [2], wherein the other copolymerizable monomer unit is a monomer unit having a ring structure. [4] The methacrylic copolymer according to any one of [1] to [3], which has a glass transition temperature of 125° C. or higher. [5] Photoelastic coefficient is -4.3×10 -12 / Pa~+4.3×10 -12 / Pa. [6] A 20 mm x 40 mm x 1.0 mm thick sheet made of a methacrylic copolymer is stretched 100% in one direction at a speed of 3 mm / min at a temperature 10°C higher than the glass transition temperature, and the birefringence of the stretched film obtained (sometimes called the orientation birefringence Δn) is -10×10 -4 ~+10×10 -4 The methacrylic copolymer according to any one of [1] to [5],
[0024] Uses of the copolymer of the present invention include the following aspects. [7] A resin composition comprising the methacrylic copolymer according to any one of [1] to [6]. [8] A resin composition comprising an antioxidant and the methacrylic copolymer according to any one of [1] to [6].
[0025] [9] A molded article comprising the methacrylic copolymer according to any one of [1] to [6] or the resin composition according to [7] or [8].
[10] A film comprising the methacrylic copolymer according to any one of [1] to [6] or the resin composition according to [7] or [8].
[11] An optical film comprising the methacrylic copolymer according to any one of [1] to [6] or the resin composition according to [7] or [8].
[12] A laminate having a layer containing the methacrylic copolymer according to any one of [1] to [6] and a layer containing another thermoplastic resin.
[0026] The method for producing a methacrylic copolymer of the present invention includes the following aspects.
[0027]
[13] A reaction raw material including a monomer mixture containing 70 to 93 mass% of methyl methacrylate, 7 to 30 mass% of α-methylstyrene, and 0 to 23 mass% of other monomers copolymerizable therewith, and a radical polymerization initiator, is continuously supplied to a tank-type reactor; The monomer mixture is bulk polymerized in a tank reactor at a polymerization conversion rate of 30 to 60% by mass to obtain a reaction product; The reaction product is continuously withdrawn from the tank reactor; and removing from the reaction product any monomer mixture remaining in the withdrawn reaction product; A method for producing the methacrylic copolymer according to any one of [1] to [6].
[0028] The production method suitable for producing the methacrylic copolymer of the present invention includes the following embodiments.
[0029]
[14] A reaction raw material including a monomer mixture containing 70 to 93 mass% of methyl methacrylate, 7 to 30 mass% of α-methylstyrene, and 0 to 10 mass% of other monomers copolymerizable therewith, and a radical polymerization initiator, is continuously supplied to a tank-type reactor; The monomer mixture is bulk polymerized in a tank reactor at a polymerization conversion rate of 30 to 60% by mass to obtain a reaction product; The reaction product is continuously withdrawn from the tank reactor; and removing from the reaction product any monomer mixture remaining in the withdrawn reaction product; When the average concentration of the radical polymerization initiator in the liquid in the tank reactor is I mol / L and the average residence time of the reactants in the tank reactor is θ hr, the product I×θ is 1×10 -4 mol hr / L and over 1×10 -3 Less than mol hr / L Method for producing copolymers.
[0030]
[15] A reaction raw material comprising 100 parts by mass of a monomer mixture consisting of 40 to 92 mass% of methyl methacrylate, 7 to 25 mass% of α-methylstyrene, 1 to 25 mass% of a monomer capable of introducing a ring structure into the main chain by a polymerization reaction, and 0 to 10 mass% of other monomers copolymerizable therewith, 0 to 30 parts by mass of an organic solvent, and a radical polymerization initiator, is continuously supplied to a tank-type reactor; subjecting the monomer mixture to a polymerization reaction in a tank-type reactor to obtain a reaction product; The reaction product is continuously withdrawn from the tank reactor; and removing from the reaction product any monomer mixture remaining in the withdrawn reaction product; When the average concentration of the radical polymerization initiator in the liquid in the tank reactor is I mol / L and the average residence time of the reactants in the tank reactor is θ hr, the product I×θ is 1.0×10 -5 mol hr / L and over 1.5×10 -4mol hr / L or less, the polymerization conversion rate is 30 to 65 mass%. Method for producing copolymers.
[0031]
[16] The production method according to any one of
[13] to
[15] , wherein the temperature inside the tank reactor is 110°C or higher and 140°C or lower, and the average residence time θ of the reaction raw materials in the tank reactor is 1.5 to 5 hours.
[17] The production method according to any one of
[13] to
[16] , wherein the step of removing the monomer mixture remaining in the withdrawn reaction product from the reaction product is carried out by an adiabatic flash evaporation method.
[18] The method according to any one of
[13] to
[17] , further comprising a step of adding an antioxidant to the extracted reaction product.
[19] The production method according to any one of
[13] to
[18] , wherein the reaction raw materials further contain a chain transfer agent. Effect of the Invention
[0032] The methacrylic copolymer of the present invention has high heat resistance, low saturated water absorption, and low absolute values of orientation birefringence and photoelastic coefficient.The molded article of the present invention is suitable for use as an optical member such as a polarizing plate protective film.
[0033] According to the production method of the present invention, it is possible to carry out continuous bulk polymerization of methyl methacrylate, α-methylstyrene, and, if necessary, other monomers copolymerizable therewith at a high polymerization conversion rate in a short average residence time, so that the above-mentioned copolymers and the like can be produced with high productivity, high flexibility, or high responsiveness. The production method of the α-methylstyrene copolymer of the present invention is suitable for producing the methacrylic copolymer of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0034] The methacrylic copolymer of the present invention comprises structural units derived from methyl methacrylate (sometimes referred to as "methyl methacrylate units" in the present application), structural units derived from α-methylstyrene (sometimes referred to as "α-methylstyrene units" in the present application), and structural units derived from other copolymerizable monomers (sometimes referred to as "other copolymerizable monomer units" in the present application).
[0035] The total content of structural units derived from methyl methacrylate is usually from 70 to 93 mass %, preferably from 73 to 93 mass %, and more preferably from 75 to 92 mass %. The total content of structural units derived from α-methylstyrene is usually from 7 to 30% by mass, preferably from 7 to 27% by mass, and more preferably from 8 to 25% by mass. The total content of structural units derived from other copolymerizable monomers is usually 0 to 23 mass%, preferably 0 to 20 mass%, more preferably 0 to 17 mass%, even more preferably 0 to 10 mass%, and still more preferably 0 to 5 mass%. The total amount of the methyl methacrylate units, the α-methylstyrene units, and other monomer units copolymerizable therewith is 100% by mass.
[0036] Examples of other copolymerizable monomers include alkyl methacrylates having an alkyl group having two or more carbon atoms, such as ethyl methacrylate and butyl methacrylate; aryl methacrylates such as phenyl methacrylate; cycloalkyl methacrylates such as cyclohexyl methacrylate and norbornenyl methacrylate; alkyl acrylates such as methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, and 2-ethylhexyl acrylate; aryl acrylates such as phenyl acrylate; cycloalkyl acrylates such as cyclohexyl acrylate and norbornenyl acrylate; styrene, p-methylstyrene, m-methylstyrene; acrylamide; methacrylamide; acrylonitrile; methacrylonitrile; methacrylic acid; and vinyl monomers having only one polymerizable carbon-carbon double bond in one molecule, such as acrylic acid.
[0037] In the methacrylic copolymer of the present invention, the other copolymerizable monomer unit may be a structural unit derived from a monomer that can introduce a ring structure into the main chain by a radical polymerization reaction (sometimes referred to as a "monomer unit having a ring structure" in the present application). Examples of monomers capable of introducing a ring structure into the main chain by radical polymerization reaction include N-alkylmaleimide monomers such as N-methylmaleimide, N-ethylmaleimide, N-butylmaleimide, and N-cyclohexylmaleimide; N-arylmaleimide monomers such as N-phenylmaleimide, N-methylphenylmaleimide, and N-chlorophenylmaleimide; maleic anhydride, itaconic anhydride; and cycloolefins such as norbornene, ethylidenenorbornene, dicyclopentadiene, and tetracyclododecene. The monomers capable of introducing a ring structure into the main chain by radical polymerization reaction can be used alone or in combination of two or more. Among these, maleic anhydride is preferred. The total content of monomer units having a ring structure is preferably from 1 to 23% by mass, more preferably from 2 to 20% by mass.
[0038] The methacrylic copolymer of the present invention has a value of the formula |AB| / B generally less than 0.05, preferably less than 0.04, more preferably less than 0.03. This suggests that the methacrylic copolymer of the present invention contains structural units that absorb light at a wavelength of 254 nm in equal proportions regardless of the molecular weight, and that the degree of molecular chain growth has almost no effect on the copolymerization composition ratio. A is the molecular weight at the peak top in the differential molecular weight distribution curve obtained by gel permeation chromatography measurement using a differential refractive index detector, and B is the molecular weight at the peak top in the differential molecular weight distribution curve obtained by gel permeation chromatography measurement using an absorbance detector with a detection wavelength of 254 nm. |AB| is the absolute value of the difference between A and B. The molecular weight of the methacrylic copolymer is calculated from the elution time of the methacrylic copolymer using a calibration curve showing the relationship between the molecular weight of standard polystyrene and the elution time (retention time). The peak top molecular weight in the differential molecular weight distribution curve is the molecular weight at the inflection point or maximum slope point in the integrated molecular weight distribution curve.
[0039] The methacrylic copolymer of the present invention has a weight average molecular weight Mw of preferably 30,000 to 200,000, more preferably 40,000 to 180,000, and even more preferably 50,000 to 160,000. Mw is calculated using formula (2) from the molecular weight distribution obtained by gel permeation chromatography measurement using a differential refractive index detector. Mw = Σ(M i 2 ×N i ) / Σ(M i ×N i )=Σ(C i ×M i ) / Σ(C i ) (2) N is the number of polymer molecules, M is the molecular weight, and C is the concentration, with the relationship C=M×N. The smaller the Mw, the more brittle the molded product tends to be. The larger the Mw of a methacrylic copolymer, the lower the productivity tends to be. The number average molecular weight Mn is calculated from the molecular weight distribution obtained by gel permeation chromatography measurement using a differential refractive index detector using formula (3). Mn = Σ(M i ×N i ) / Σ(N i )=Σ(C i ) / Σ(N i ) (3) N is the number of polymer molecules, M is the molecular weight, and C is the concentration, with the relationship C=M×N.
[0040] Gel permeation chromatography measurements can be performed as follows. Tetrahydrofuran is used as the eluent, and two TSKgel SuperMultipore HZMM columns manufactured by Tosoh Corporation and a SuperHZ4000 column connected in series are used as the column. An HLC-8320 (product number) manufactured by Tosoh Corporation equipped with a differential refractive index detector (RI detector) and an absorbance detector (detection wavelength 254 nm) is used as the analytical device. 4 mg of resin material is dissolved in 5 ml of tetrahydrofuran, and then filtered through a 0.1 μm filter to prepare a test solution. The temperature of the column oven is set to 40°C, and 20 μl of the test solution is injected at an eluent flow rate of 0.35 ml / min to obtain a chromatogram. There are two types of chromatograms: a chart in which the electric signal value (intensity Y) derived from the refractive index difference between the test solution and the reference solution is plotted against the retention time X, and a chart in which the electric signal value (intensity Y) derived from the absorbance at a wavelength of 254 nm is plotted against the retention time X. Standard polystyrene with molecular weights in the range of 400 to 5,000,000 is measured by gel permeation chromatography, and a calibration curve showing the relationship between retention time and molecular weight is created. The line connecting the point where the slope of the high molecular weight side of the peak changes from zero to positive and the point where the slope of the low molecular weight side of the peak changes from negative to zero is taken as the baseline.
[0041] The methacrylic copolymer of the present invention has a glass transition temperature Tg of preferably 125° C. or higher, more preferably 126° C. or higher, and further preferably 128° C. or higher. There is no particular upper limit to the glass transition temperature of the methacrylic copolymer of the present invention, but it is preferably 140° C.
[0042] The glass transition temperature is the midpoint glass transition temperature obtained from the DSC curve. The DSC curve is obtained by differential scanning calorimetry at the second temperature rise when the resin to be measured is heated to 230°C using a differential scanning calorimeter in accordance with JIS K7121, cooled to room temperature, and then heated from room temperature to 230°C at a rate of 10°C / min. The higher the glass transition temperature of the methacrylic copolymer, the less likely a molded article made of it is to deform or shrink due to heat, i.e., the higher the heat resistance.
[0043] The methacrylic copolymer of the present invention preferably has a photoelastic coefficient K of −4.3×10 -12 / Pa~+4.3×10 -12 / Pa, more preferably -4.0×10 -12 / Pa~+4.0×10 -12 / Pa, and more preferably -3.0×10 -12 / Pa~+3.0×10 -12 / Pa. A methacrylic copolymer having a photoelastic coefficient within the above range is likely to provide a molded article with small stress birefringence. The photoelastic coefficient was measured by applying tension to a press-molded sheet of methacrylic copolymer, 15 mm wide x 60 mm long x 1.0 mm thick, at a chuck distance of 45 mm and a temperature of 23°C, increasing the tension from 0 N to 100 N in increments of 10 N. Each time the tension was increased, the birefringence of the central part of the sheet was measured at a temperature of 23°C and the D-line wavelength of Na, and the slope was calculated by approximating the relationship between the measured stress and birefringence to a linear function using the least squares method. The stress is the value obtained by dividing the tension by the cross-sectional area of the sheet. The cross-sectional area of the sheet was calculated as the product of the sheet width of 15 mm and the thickness at the measurement point in the central part of the sheet. Birefringence is the refractive index n p and the refractive index n of light with a polarization plane perpendicular to the tensile direction oDifference from (Δn=n p -n o )
[0044] The methacrylic copolymer of the present invention has an orientation birefringence Δn of preferably −10×10 -4 ~+10×10 -4 , more preferably -2.5 x 10 -4 ~+2.5×10 -4 , and more preferably −2.4×10 -4 ~+2.4×10 -4 , and even more preferably -2.3 x 10 -4 ~+2.3×10 -4 , most preferably -2.2 x 10 -4 ~+2.2×10 -4 Here, the orientation birefringence is the birefringence measured at the center of a stretched film obtained by stretching a press-molded sheet of a methacrylic copolymer, 20 mm wide × 40 mm long × 1.0 mm thick, in one direction by 100% at a temperature 10°C higher than the glass transition temperature at a speed of 3 mm / min, at a temperature of 23°C, at a D-line wavelength of Na, without applying tension.
[0045] The methacrylic copolymer of the present invention has a saturated water absorption As of preferably less than 1.9%, more preferably less than 1.8%. The saturated water absorption is determined as follows: A press-molded sheet of 50 mm × 50 mm × 1.0 mm thickness made of a methacrylic copolymer is placed in a dryer at 80 ° C. and dried for 16 hours or more. The dried sheet is returned to room temperature and the initial weight W O Then, soak it in distilled water at 23°C for 24 hours, drain it, wipe off the water with a dry cloth, etc., and weigh it to the nearest 0.1 mg within 1 minute after wiping it off. Repeat this process again, soak it in distilled water at 23°C for 24 hours, drain it, wipe off the water with a dry cloth, etc., and weigh it to the nearest 0.1 mg within 1 minute after wiping it off. If the weight change is less than the initial weight W O The weight when it becomes smaller than 0.02% of the saturated weight W S Then, the saturated water absorption rate As is calculated using the following formula. Saturated water absorption As = ((WS - W O ) / W O ) x 100
[0046] The methacrylic copolymer of the present invention is not particularly limited by its production method as long as it satisfies the above-mentioned characteristic values. The methacrylic copolymer of the present invention can be obtained, for example, by the production method of the methacrylic copolymer of the present invention.
[0047] The method for producing a methacrylic copolymer of the present invention comprises continuously supplying reaction raw materials to a tank reactor, polymerizing a monomer mixture in the tank reactor to obtain a reaction product, continuously withdrawing the reaction product from the tank reactor, and removing the monomer mixture remaining in the withdrawn reaction product from the reaction product.
[0048] (Manufacturing method I) One embodiment of the method for producing the methacrylic copolymer of the present invention (production method I) comprises continuously supplying a reaction raw material comprising a monomer mixture containing 70 to 93 mass % of methyl methacrylate, 7 to 30 mass % of α-methylstyrene, and 0 to 23 mass % of other monomers copolymerizable therewith, and a radical polymerization initiator, to a tank-type reactor, bulk polymerizing the monomer mixture in the tank-type reactor at a polymerization conversion rate of 30 to 60 mass % to obtain a reaction product, continuously withdrawing the reaction product from the tank-type reactor, and removing the monomer mixture remaining in the withdrawn reaction product from the reaction product.
[0049] The reaction raw materials used in Production Method I of the present invention contain a monomer mixture and a radical polymerization initiator, and preferably contain a monomer mixture, a chain transfer agent, and a radical polymerization initiator.
[0050] The monomer mixture includes methyl methacrylate and α-methylstyrene, and optionally other monomers copolymerizable therewith.
[0051] The amount of methyl methacrylate contained in the monomer mixture is usually from 67 to 93 mass %, preferably from 69 to 92 mass %, and more preferably from 70 to 90 mass %. The amount of α-methylstyrene contained in the monomer mixture is usually 7 to 33 mass%, preferably 7 to 31 mass%, more preferably 7 to 30 mass%, even more preferably 8 to 30 mass%, and still more preferably 10 to 30 mass%. The amount of other copolymerizable monomers contained in the monomer mixture is usually 0 to 23 mass%, preferably 0 to 20 mass%, more preferably 0 to 17 mass%, even more preferably 0 to 10 mass%, and still more preferably 0 to 5 mass%. The monomer mixture was 100% by mass in total of methyl methacrylate, α-methylstyrene, and other monomers copolymerizable therewith. The amount of the monomer capable of introducing a ring structure into the main chain by radical polymerization reaction as the other copolymerizable monomer contained in the monomer mixture is preferably 1 to 23 mass%, preferably 2 to 20 mass%. By including such an amount of the monomer in the monomer mixture, the polymerization rate of α-methylstyrene, which has low copolymerization reactivity with methyl methacrylate, is easily increased, and in a continuous polymerization system, the polymerization conversion rate can be easily increased with a short average residence time and a moderate amount of initiator. The other copolymerizable monomer and the monomer capable of introducing a ring structure into the main chain by polymerization reaction are as described above.
[0052] The monomer mixture is b * is preferably -1 to 2, and more preferably -0.5 to 1.5. * When b is within this range, when the resulting α-methylstyrene-methyl methacrylate copolymer is molded, it is advantageous in that a molded product with almost no coloring can be obtained with high productivity. * is a value measured in accordance with the International Commission on Illumination (CIE) standard (1976) or JIS Z-8722.
[0053] In the step of removing the monomer mixture remaining in the reaction product discharged from the tank reactor from the reaction product, the monomer mixture removed from the reaction product can be recovered and reused in the present invention. * If the heat applied during recovery or other processes increases the * is preferably within the above range.
[0054] A chain transfer agent can be included in the reaction raw materials in order to adjust the molecular weight of the copolymer. Examples of chain transfer agents that can be used in the present invention include alkyl mercaptans such as n-octyl mercaptan, n-dodecyl mercaptan, t-dodecyl mercaptan, 1,4-butanedithiol, 1,6-hexanedithiol, ethylene glycol bisthiopropionate, butanediol bisthioglycolate, butanediol bisthiopropionate, hexanediol bisthioglycolate, hexanediol bisthiopropionate, trimethylolpropane tris-(β-thiopropionate), and pentaerythritol tetrakisthiopropionate; α-methylstyrene dimer; and terpinolene. Among these, monofunctional alkyl mercaptans such as n-octyl mercaptan and n-dodecyl mercaptan are preferred. These chain transfer agents can be used alone or in combination of two or more. The amount of the chain transfer agent used is preferably 0 to 1 part by mass relative to 100 parts by mass of the monomer mixture, with the lower limit being more preferably 0.0001 parts by mass, even more preferably 0.01 parts by mass, and even more preferably 0.02 parts by mass, and the upper limit being more preferably 0.8 parts by mass, even more preferably 0.6 parts by mass, and still more preferably 0.4 parts by mass.
[0055] The radical polymerization initiator used in the present invention generates reactive radicals. As the radical polymerization initiator, for example, t-hexylperoxyisopropyl monocarbonate, t-hexylperoxy2-ethylhexanoate, 1,1,3,3-tetramethylbutylperoxy2-ethylhexanoate, t-butylperoxypivalate, t-hexylperoxypivalate, t-butylperoxyneodecanoate, t-hexylperoxyneodecanoate, 1,1,3,3-tetramethylbutylperoxyneodecanoate, 1,1-bis(t-hexylperoxy)cyclohexane, benzoyl peroxide, 3,5,5-trimethylhexanoyl peroxide, lauroyl peroxide, 2,2'-azobis(2-methylpropionitrile), 2,2'-azobis(2-methylbutyronitrile), and dimethyl 2,2'-azobis(2-methylpropionate) are preferable; Examples of the radical polymerization initiator include t-hexylperoxy 2-ethylhexanoate, 1,1-bis(t-hexylperoxy)cyclohexane, and dimethyl 2,2'-azobis(2-methylpropionate). These radical polymerization initiators can be used alone or in combination of two or more. The amount of the radical polymerization initiator used is preferably set so as to satisfy the average concentration of the radical polymerization initiator present in the liquid in the tank-type reactor, which will be described later.
[0056] The method of preparing the reaction raw materials is not particularly limited. The reaction raw materials are preferably prepared immediately before being supplied to the tank-type reactor. The reaction raw materials are also preferably prepared in an inert atmosphere such as nitrogen gas. For example, it is preferable to continuously supply each component constituting the reaction raw materials from a tank storing the components to a mixer through a pipe, and mix the components in the mixer to obtain the reaction raw materials. The radical polymerization initiator can be prepared as a solution by dissolving it in methyl methacrylate. The mixer can be equipped with a dynamic stirrer or a static stirrer. The obtained reaction raw materials are then continuously supplied to the tank-type reactor.
[0057] The monomer mixture can be prepared before mixing with the chain transfer agent and / or the radical polymerization initiator. The radical polymerization initiator is preferably dissolved in methyl methacrylate to form a polymerization initiator solution, which is then mixed with the monomer or with a mixture of the monomer and the chain transfer agent in a predetermined ratio. The polymerization initiator solution may have a dissolved oxygen content of preferably more than 3 ppm, more preferably more than 5 ppm, and even more preferably more than 10 ppm. The monomer mixture or the reaction raw material may be prepared in the presence of oxygen. The monomer mixture or the reaction raw material immediately after preparation may have a dissolved oxygen content of preferably more than 3 ppm, more preferably more than 5 ppm, and even more preferably more than 10 ppm.
[0058] The amount of dissolved oxygen in the reaction raw material immediately before being fed to the tank reactor is preferably 10 ppm or less, more preferably 5 ppm or less, even more preferably 4 ppm or less, and most preferably 3 ppm or less. If the amount of dissolved oxygen is within such a range, the polymerization reaction proceeds smoothly, and it becomes easier to obtain a molded product without silver streaks or coloring. The amount of dissolved oxygen in the reaction raw material immediately before being fed can be adjusted by purging the reaction raw material with nitrogen immediately after preparation to expel oxygen.
[0059] The tank reactor used in the present invention is capable of simultaneously carrying out the supply of reaction raw materials, the polymerization reaction of the monomer mixture, and the withdrawal of the reaction product in parallel. The tank reactor is usually equipped with a stirring means for stirring the liquid in the tank reactor, a feed port for feeding the reaction raw materials to the tank reactor, and a withdrawal port for withdrawing the reaction product from the tank reactor. The amount of the reaction raw materials fed to the tank reactor and the amount of the reaction product withdrawn from the tank reactor are balanced so that the amount of liquid in the tank reactor is almost constant. The amount of liquid in the tank reactor (volume V) is preferably 1 / 4 or more, more preferably 1 / 4 to 3 / 4, and even more preferably 1 / 3 to 2 / 3 of the volume of the tank reactor.
[0060] The tank reactor used in the present invention preferably has a plurality of supply ports for supplying the reaction raw materials. The reaction raw materials are continuously supplied from at least two supply ports simultaneously or alternately, preferably simultaneously. The supply ports may be installed on the top surface of the tank reactor, on the side surface of the tank reactor, on the bottom surface of the tank reactor, or on at least two of the top surface, side surface, and bottom surface. In addition, it is preferable that the supply ports are arranged in symmetrical positions. The height of the supply port may be higher than the liquid level in the tank reactor, or lower than the liquid level in the tank reactor. The shape of the supply port may be the shape of the cut end of the circular tube itself, or may be a shape that allows the reaction raw materials to be widely spread on the liquid surface in the tank reactor. By providing at least two supply ports, the efficiency of the radical generation reaction is increased, and the amount of radical polymerization initiator required to achieve a desired polymerization conversion rate can be reduced.
[0061] Examples of the stirring means include a Max Blend type stirrer, a lattice blade type stirrer, a propeller type stirrer, a screw type stirrer, a helical ribbon type stirrer, a paddle type stirrer, etc. Among these, the Max Blend type stirrer is preferred from the viewpoint of uniform mixing.
[0062] The temperature inside the tank reactor, i.e., the temperature of the liquid inside the tank reactor, is preferably 110 to 140° C., more preferably 114 to 135° C. The temperature of the liquid can be controlled by an external heat exchanger control method such as a jacket or a heat transfer tube, or a self-heat exchanger control method in which a tube through which the reaction raw materials or reaction products flow is disposed inside the reaction tank.
[0063] The average residence time of the reaction raw materials in the tank reactor is preferably 1.5 to 5 hours, more preferably 2 to 4.5 hours, and further preferably 2.5 to 4 hours. The average concentration of the radical polymerization initiator present in the liquid in the tank reactor is preferably 5.1×10 -5 mol / L or more 2.4×10 -4 mol / L or less.
[0064] In bulk polymerization, a solvent is not used in principle, but when it is necessary to adjust the viscosity of the liquid in the tank reactor, a solvent can be included in the reaction raw materials. As the solvent, aromatic hydrocarbons such as benzene, toluene, and ethylbenzene are preferable. These solvents can be used alone or in combination of two or more. The amount of such a solvent to be used is preferably 30 parts by mass or less, more preferably 10 parts by mass or less, and even more preferably 0 parts by mass, based on 100 parts by mass of the monomer mixture.
[0065] In Production Method I of the present invention, the amount of water contained in the liquid in the tank reactor is preferably 1000 ppm or less, more preferably 700 ppm or less, and even more preferably 280 ppm or less. By reducing the water content, it is possible to suppress the generation of resin foreign matter of several μm to several tens of μm during the polymerization reaction, and it is possible to significantly reduce the occurrence of defects having an outer diameter of several tens of μm caused by the foreign matter when the composition containing the obtained copolymer is formed into a film or sheet by melt molding.
[0066] Examples of methods for reducing the amount of water contained in the liquid in a tank-type reactor include a method comprising pretreating the reaction raw materials in an adsorption / dehydration tower or the like, and a method comprising introducing an inert gas into the gas phase part of a tank-type reactor, entraining a part of the water vapor with the inert gas, condensing it in a brine-cooled condenser, and withdrawing it from the system.
[0067] In the tank reactor, bulk polymerization is carried out until the polymerization conversion rate is 30 to 65% by mass, preferably 35 to 60% by mass, more preferably 35 to 45% by mass, and even more preferably 35 to 40% by mass. The polymerization conversion rate can be calculated as a value based on the content of the copolymer or monomer mixture present in the reaction product discharged from the tank reactor relative to the content in the reaction raw materials. The bulk polymerization in the tank reactor is preferably carried out in an atmosphere of an inert gas such as nitrogen gas.
[0068] An additional reactor may be connected to the rear of the tank reactor. The additional reactor that can be connected to the rear may be tank type or tubular type. In the additional reactor, bulk polymerization is continued. The bulk polymerization in the additional reactor may be carried out until the polymerization conversion rate is 30 to 65 mass%, preferably 35 to 60 mass%, more preferably 35 to 45 mass%, and even more preferably 35 to 40 mass%. The polymerization conversion rate can be calculated as a value relative to the content in the reaction raw material from the content of the copolymer or monomer mixture present in the reaction product extracted from the additional reactor. The bulk polymerization in the additional reactor is preferably carried out in an atmosphere of an inert gas such as nitrogen gas.
[0069] According to Production Method I of the present invention, the ratio of the molar fraction of α-methylstyrene units in the copolymer to the molar fraction of α-methylstyrene in the monomer mixture can be preferably 0.7 to 1.0, more preferably 0.79 to 0.99. Specifically, the mass fraction of α-methylstyrene in the monomer mixture is 7 to 30 mass%, preferably 10 to 25 mass%, but according to Production Method I of the present invention, the mass fraction of α-methylstyrene units in the copolymer can be 5 to 27 mass%, preferably 8 to 24 mass%.
[0070] The manufacturing method I of the present invention has a step of removing the monomer mixture from the reaction product. In this step, the solvent is also removed at the same time, if necessary. The copolymer is isolated by this step. The removal method is not particularly limited, but a thermal devolatilization method is preferred. Examples of the thermal devolatilization method include an equilibrium flash evaporation method and an adiabatic flash evaporation method, but an adiabatic flash evaporation method is preferred. The temperature at which the adiabatic flash evaporation method is carried out is preferably 200 to 300°C, more preferably 200 to 280°C, more preferably 210 to 280°C, and even more preferably 220 to 270°C. If the temperature at which the adiabatic flash evaporation method is carried out is too low, devolatilization takes time, devolatilization becomes insufficient, and the molded product may have a poor appearance such as silver. On the other hand, if the temperature at which the adiabatic flash evaporation method is carried out is too high, the copolymer tends to be colored due to oxidation, burning, decomposition, etc., or the copolymer tends to undergo a depolymerization reaction. The adiabatic flash evaporation method may be carried out in multiple stages. In this case, the reaction product flowing through the heat transfer tube is heated with the vapor of the flash evaporated monomer mixture, and the heated reaction product is supplied to a low-pressure flash tank for flash evaporation. The reaction product can be pressurized by a pump or the like.
[0071] The copolymer obtained by removing the monomer mixture from the reaction product can be made into pellets or powder according to a known method to facilitate easy handling as a molding material. The amount of the monomer mixture contained in the copolymer after removing the monomer mixture is preferably 1 mass % or less, more preferably 0.5 mass % or less. It is preferable to use a vented extruder to remove the monomer mixture and to convert the isolated copolymer into a molding material and / or to mix the additives described below.
[0072] (Manufacturing method II) One embodiment of a production method (production method II) suitable for producing the methacrylic copolymer of the present invention comprises continuously supplying a reaction raw material comprising a monomer mixture containing 70 to 93 mass % of methyl methacrylate, 7 to 30 mass % of α-methylstyrene, and 0 to 10 mass % of other monomers copolymerizable therewith, and a radical polymerization initiator, to a tank reactor, bulk polymerizing the monomer mixture in the tank reactor at a polymerization conversion rate of 30 to 60 mass % to obtain a reaction product, continuously withdrawing the reaction product from the tank reactor, and removing the monomer mixture remaining in the withdrawn reaction product from the reaction product, wherein when the average concentration of the radical polymerization initiator present in the liquid in the tank reactor is I mol / L and the average residence time of the reaction raw materials in the tank reactor is θ hr, their product I×θ is 1×10 -4 mol hr / L and over 1×10 -3 mol·hr / L or less. By using Production Method II, not only the methacrylic copolymer of the present invention but also other copolymers can be obtained.
[0073] The amount of methyl methacrylate contained in the monomer mixture is usually from 70 to 93% by mass, and preferably from 75 to 90% by mass. The amount of α-methylstyrene contained in the monomer mixture is usually from 7 to 30% by mass, preferably from 10 to 25% by mass. The content of other copolymerizable monomers contained in the monomer mixture is usually 0 to 10% by mass, preferably 0 to 5% by mass. The monomer mixture was 100% by mass in total of methyl methacrylate, α-methylstyrene, and other monomers copolymerizable therewith.
[0074] In the production method II, the amount of reaction raw material Q m supplied to the tank reactor 3 The product I×θ of the average concentration I mol / L of the radical polymerization initiator present in the liquid in the tank reactor and the average residence time θ hr of the reactant in the tank reactor is 1×10 -4 mol hr / L and over 1×10 -3The mean residence time θ hr is the amount of reaction raw material supplied to the tank reactor Q m 3 / hr vs. volume of liquid in tank reactor V m 3 The ratio V / Q is The average concentration I of the radical polymerization initiator present in the liquid in the tank reactor is calculated by dividing the concentration I of the radical polymerization initiator in the reaction raw material supplied to the tank reactor by 0 mol / L and the half-life τ of the radical polymerization initiator at the temperature of the liquid in the tank reactor. 1 / 2 The value is calculated from the average residence time θ hr of the reaction raw materials in the tank reactor and the average residence time θ hr of the reaction raw materials in the tank reactor by the following formula. I = I0 / (1+k d ×θ×3600) k d = ln(2) / τ 1 / 2 or k d =A×exp(-ΔE / RT) In addition, A is the frequency factor, ΔE is the activation energy, R is the gas constant (8.314 J / mol / K), T is the absolute temperature (K), and τ 1 / 2 is the half-life of the radical polymerization initiator at absolute temperature T (K), k d is the decomposition rate constant (1 / sec) of the radical polymerization initiator at absolute temperature T (K).
[0075] In production method II, the average residence time θ of the reaction raw materials in the tank reactor is not particularly limited as long as the above relationship is satisfied, but is preferably 1.5 to 5 hours, more preferably 2 to 4.5 hours, and even more preferably 2.5 to 4 hours.
[0076] In the production method II, the average concentration I of the radical polymerization initiator present in the liquid in the tank reactor is not particularly limited as long as the above relationship is satisfied, but is preferably 5.1×10 -5 mol / L or more 2.4×10 -4 mol / L or less.
[0077] Other conditions in Production Method II are the same as those in Production Method I.
[0078] According to the production method II, the ratio of the molar fraction of α-methylstyrene units in the copolymer to the molar fraction of α-methylstyrene in the monomer mixture can be preferably 0.7 to 1.0, more preferably 0.79 to 0.99. Specifically, the mass fraction of α-methylstyrene in the monomer mixture is 7 to 30 mass%, preferably 10 to 25 mass%, but the mass fraction of α-methylstyrene units in the copolymer can be 5 to 27 mass%, preferably 8 to 24 mass%, by the production method of the present invention.
[0079] By the production method II, copolymers having various molecular weight distributions can be obtained. For example, the copolymer obtained by the production method II has a weight average molecular weight of preferably 35,000 to 200,000, more preferably 40,000 to 150,000, and even more preferably 45,000 to 130,000, from the viewpoints of flowability, moldability, impact resistance, toughness, and the like. In addition, the ratio of the weight average molecular weight to the number average molecular weight is preferably 1.5 to 3.0, more preferably 1.6 to 2.6, and particularly preferably 1.7 to 2.3. The weight average molecular weight and the number average molecular weight are calculated by converting the molecular weight of standard polystyrene based on a chromatogram measured by gel permeation chromatography.
[0080] (Manufacturing method III) One embodiment of a production method (production method III) suitable for producing the methacrylic copolymer of the present invention comprises continuously supplying reaction raw materials containing 100 parts by mass of a monomer mixture consisting of 40 to 92 mass % methyl methacrylate, 7 to 25 mass % α-methylstyrene, 1 to 25 mass % of a monomer capable of introducing a ring structure into the main chain by polymerization reaction, and 0 to 10 mass % of other monomers copolymerizable therewith, 0 to 30 parts by mass of an organic solvent, and a radical polymerization initiator to a tank reactor, polymerizing the monomer mixture in the tank reactor to obtain a reaction product, continuously withdrawing the reaction product from the tank reactor, and removing the monomer mixture remaining in the withdrawn reaction product from the reaction product, wherein when the average concentration of the radical polymerization initiator present in the liquid in the tank reactor is I mol / L and the average residence time of the reaction raw materials in the tank reactor is θ hr, their product I×θ is 1.0×10-5 mol hr / L and over 1.5×10 -4 When the conversion rate is less than mol·hr / L, the polymerization conversion rate is 30 to 65% by mass. By the production method III, not only the methacrylic copolymer of the present invention but also other copolymers can be obtained.
[0081] In the production method III, the amount of methyl methacrylate contained in the monomer mixture is usually 40 to 92% by mass, and preferably 53 to 86% by mass. In the production method III, the amount of α-methylstyrene contained in the monomer mixture is usually from 7 to 25% by mass, and preferably from 10 to 20% by mass. In the production method III, the amount of the monomer capable of introducing a ring structure into the main chain by polymerization reaction contained in the monomer mixture is usually 1 to 25 mass %, preferably 2 to 20 mass %. By including such an amount of the monomer capable of introducing a ring structure into the main chain by polymerization reaction in the monomer mixture, the polymerization rate of α-methylstyrene, which has low copolymerization reactivity with methyl methacrylate, is easily increased, and in a continuous polymerization system, the polymerization conversion rate can be easily increased with a short average residence time and an appropriate amount of initiator. In the production method III, the amount of other monomers contained in the monomer mixture is usually from 0 to 10% by mass, and preferably from 2 to 7% by mass. In addition, the monomer mixture in production method III is 100 mass % in total of methyl methacrylate, α-methylstyrene, a monomer capable of introducing a ring structure into the main chain by a polymerization reaction, and other monomers copolymerizable therewith.
[0082] Examples of the other monomer in the production method III include aromatic vinyl monomers other than α-methylstyrene, such as styrene, p-methylstyrene, and m-methylstyrene; vinyl cyanide monomers, such as acrylonitrile and methacrylonitrile; alkyl methacrylates having an alkyl group with 2 or more carbon atoms, such as ethyl methacrylate and butyl methacrylate; aryl methacrylates, such as phenyl methacrylate; cycloalkyl methacrylates, such as cyclohexyl methacrylate and norbornenyl methacrylate; alkyl acrylates, such as methyl acrylate, ethyl acrylate, and butyl acrylate; aryl acrylates, such as phenyl acrylate; cycloalkyl acrylates, such as cyclohexyl acrylate and norbornenyl acrylate; vinyl carboxylic acid monomers, such as acrylic acid and methacrylic acid. The other monomers can be used alone or in combination of two or more.
[0083] In the production method III, the amount of reaction raw material Q m supplied to the tank reactor 3 The product I×θ of the average concentration I mol / L of the radical polymerization initiator present in the liquid in the tank reactor and the average residence time θ hr of the reactant in the tank reactor is 1×10 -5 mol hr / L and over 1.5×10 -4 The mean residence time θ hr is the amount of reaction raw material supplied to the tank reactor Q m 3 / hr vs. volume of liquid in tank reactor V m 3 The ratio V / Q is The average concentration I of the radical polymerization initiator present in the liquid in the tank reactor is calculated by dividing the concentration I of the radical polymerization initiator in the reaction raw material supplied to the tank reactor by 0 mol / L and the half-life τ of the radical polymerization initiator at the temperature of the liquid in the tank reactor. 1 / 2 The value is calculated from the average residence time θ hr of the reaction raw materials in the tank reactor and the average residence time θ hr of the reaction raw materials in the tank reactor by the following formula. I = I0 / (1+k d ×θ×3600) k d = ln(2) / τ 1 / 2 =A×exp(-ΔE / RT) In addition, A is the frequency factor, ΔE is the activation energy, R is the gas constant (8.314 J / mol / K), T is the absolute temperature (K), and τ 1 / 2 is the half-life of the radical polymerization initiator at absolute temperature T (K), k d is the decomposition rate constant (1 / sec) of the radical polymerization initiator at absolute temperature T (K).
[0084] In production method III, the average residence time θ of the reaction raw materials in the tank reactor is not particularly limited as long as the above relationship is satisfied, but is preferably 1 to 6 hours, more preferably 1.5 to 5 hours, even more preferably 2 to 4.5 hours, and still more preferably 2.5 to 4 hours.
[0085] In the production method III, the average concentration I of the radical polymerization initiator present in the liquid in the tank reactor is not particularly limited as long as the above relationship is satisfied. For example, -5 mol / L or more 2.4×10 -4 mol / L or less, preferably 1.0×10 -6 mol / L or more 2.4×10 -4 mol / L or less, more preferably 5.0×10 -6 mol / L or more 8.0×10 -5 mol / L or less, more preferably 6.0×10 -6 mol / L or more 5.5×10 -5 mol / L or less.
[0086] In the production method III, an organic solvent can be included in the reaction raw materials. Examples of the organic solvent include aromatic hydrocarbons such as benzene, toluene, xylene, chlorobenzene, and ethylbenzene, ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and acetophenone, and ethers such as tetrahydrofuran and 1,4-dioxane. From the viewpoint of the solubility of the monomer and copolymer and the ease of solvent recovery, methyl ethyl ketone, methyl isobutyl ketone, and toluene are preferred. The organic solvent can be used alone or in combination of two or more. The upper limit of the amount of the organic solvent used is preferably 30 parts by mass, more preferably 25 parts by mass, and even more preferably 20 parts by mass, relative to 100 parts by mass of the monomer mixture. The lower limit of the amount of the organic solvent used is usually 0 parts by mass, and preferably 1 part by mass.
[0087] Other conditions in Production Method III are the same as those in Production Method I.
[0088] According to the production method III, the ratio of the molar fraction of α-methylstyrene units in the copolymer to the molar fraction of α-methylstyrene can be preferably 0.8 or more, more preferably 0.9 or more. For example, the mass fraction of α-methylstyrene in the monomer mixture is 7 to 25 mass%, preferably 10 to 20 mass%, but according to the production method of the present invention, the mass fraction of α-methylstyrene units in the copolymer can be 6 to 30.0 mass%, preferably 7 to 24.9 mass%, more preferably 8 to 19.9 mass%.
[0089] By the production method III, copolymers having various molecular weight distributions can be obtained. For example, the copolymer obtained by the production method III has a weight average molecular weight of preferably 35,000 to 200,000, more preferably 40,000 to 150,000, and even more preferably 45,000 to 130,000, from the viewpoints of flowability, moldability, impact resistance, toughness, and the like. In addition, the ratio of the weight average molecular weight to the number average molecular weight is preferably 1.5 to 3.0, more preferably 1.6 to 2.6, and particularly preferably 1.7 to 2.3. The weight average molecular weight and the number average molecular weight are calculated by converting the molecular weight of standard polystyrene based on a chromatogram measured by gel permeation chromatography.
[0090] The methacrylic copolymer of the present invention or the copolymer obtained by the production method I, II or III of the present invention can be subjected to a polymer reaction by a known method, such as the imidization reaction described in JP-A-2010-254742 or JP-A-2010-261025 or the grafting reaction described in JP-A-2012-201831.
[0091] The methacrylic copolymer of the present invention can be mixed with various additives as necessary to form a resin composition. The amount of the additives is preferably 0.5% by mass or less, more preferably 0.2% by mass or less, based on the resin composition. If the amount of the additives is too large, the molded product may have poor appearance such as silver streaks.
[0092] In addition, the manufacturing method I, II or III of the present invention may further include a step of adding various additives to obtain a resin composition as necessary. The amount of additives contained in the resin composition is preferably 0.5 mass% or less, more preferably 0.2 mass% or less, based on the copolymer. If the amount of additives contained in the resin composition is too large, the molded product may have poor appearance such as silver. The additives may be added to the reaction raw materials, the reaction product, or the copolymer.
[0093] Examples of the additives include antioxidants, heat deterioration inhibitors, ultraviolet absorbers, light stabilizers, lubricants, release agents, polymer processing aids, antistatic agents, flame retardants, dyes and pigments, light diffusing agents, organic dyes, matting agents, impact resistance modifiers, and fluorescent materials.
[0094] The antioxidant alone exerts an effect of preventing the oxidative deterioration of the resin in the presence of oxygen. Examples of the antioxidant include phosphorus-based antioxidants, hindered phenol-based antioxidants, and thioether-based antioxidants. These antioxidants can be used alone or in combination of two or more. Among these, from the viewpoint of the effect of preventing the deterioration of optical properties due to coloring, phosphorus-based antioxidants or hindered phenol-based antioxidants are preferred, and a combination of a phosphorus-based antioxidant and a hindered phenol-based antioxidant is more preferred. When the phosphorus-based antioxidant and the hindered phenol-based antioxidant are used in combination, their ratio is not particularly limited, but the mass ratio of the phosphorus-based antioxidant / the hindered phenol-based antioxidant is preferably 1 / 5 to 2 / 1, and more preferably 1 / 2 to 1 / 1.
[0095] As the phosphorus-based antioxidant, 2,2-methylenebis(4,6-di-t-butylphenyl)octylphosphite (manufactured by Asahi Denka Co., Ltd.; trade name: Adekastab HP-10), tris(2,4-di-t-butylphenyl)phosphite (manufactured by Ciba Specialty Chemicals Co., Ltd.; trade name: IRUGAFOS168), and the like are preferable.
[0096] Preferred examples of the hindered phenol antioxidant include pentaerythrityl-tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate] (manufactured by Ciba Specialty Chemicals; trade name IRGANOX1010) and octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate (manufactured by Ciba Specialty Chemicals; trade name IRGANOX1076).
[0097] The heat deterioration inhibitor is capable of preventing the thermal deterioration of a resin by capturing polymer radicals that are generated when the resin is exposed to high heat in a substantially oxygen-free state. Preferred examples of the heat deterioration inhibitor include 2-t-butyl-6-(3'-t-butyl-5'-methyl-hydroxybenzyl)-4-methylphenyl acrylate (manufactured by Sumitomo Chemical Co., Ltd.; product name: Sumilizer GM) and 2,4-di-t-amyl-6-(3',5'-di-t-amyl-2'-hydroxy-α-methylbenzyl)phenyl acrylate (manufactured by Sumitomo Chemical Co., Ltd.; product name: Sumilizer GS).
[0098] An ultraviolet absorber is a compound that has the ability to absorb ultraviolet rays. An ultraviolet absorber is a compound that is said to have the function of converting light energy into heat energy. Examples of the ultraviolet absorbent include benzophenones, benzotriazoles, triazines, benzoates, salicylates, cyanoacrylates, oxalic acid anilides, malonic acid esters, formamidines, etc. These may be used alone or in combination of two or more. Among these, benzotriazoles, or the maximum molar absorption coefficient ε max 1200dm 3 mol -1 cm -1 Preferred are UV absorbers which are:
[0099] Benzotriazoles are highly effective in suppressing deterioration of optical properties such as coloration due to exposure to ultraviolet light, and are therefore preferred as ultraviolet absorbents when the resin composition of the present invention is applied to applications requiring such properties.
[0100] Preferred benzotriazoles include 2-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol (manufactured by Ciba Specialty Chemicals; trade name TINUVIN 329) and 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol (manufactured by Ciba Specialty Chemicals; trade name TINUVIN 234).
[0101] In addition, the maximum molar absorption coefficient ε max 1200dm 3 mol -1 cm -1 The ultraviolet absorbents below can suppress the yellowing of the resulting molded product.
[0102] The maximum molar absorption coefficient ε of the ultraviolet absorber max The absorbance is measured as follows. 10.00 mg of the ultraviolet absorber is added to 1 L of cyclohexane, and dissolved until no undissolved matter is found by visual observation. This solution is poured into a quartz glass cell measuring 1 cm x 1 cm x 3 cm, and the absorbance at wavelengths of 380 to 450 nm is measured using a Hitachi U-3410 spectrophotometer. The molecular weight (Mw) of the ultraviolet absorber and the maximum absorbance (A) measured are used as the absorbance. max ) and calculate the maximum molar absorption coefficient εmax using the following formula: ε max =[A max / (10×10 -3 )]×Mw
[0103] Maximum molar absorption coefficient ε at wavelengths from 380 to 450 nm max 1200dm 3 mol -1 cm -1 Examples of the ultraviolet absorbing agent include 2-ethyl-2'-ethoxy-oxalanilide (manufactured by Clariant Japan; trade name: Sanduvoir VSU). Among these ultraviolet absorbents, benzotriazoles are preferably used from the viewpoint of suppressing resin deterioration due to exposure to ultraviolet light.
[0104] A light stabilizer is a compound that is said to have the function of capturing radicals generated mainly by oxidation due to light. Suitable light stabilizers include hindered amines such as compounds having a 2,2,6,6-tetraalkylpiperidine skeleton.
[0105] The release agent is a compound having a function of facilitating the release of a molded product from a mold. Examples of the release agent include higher alcohols such as cetyl alcohol and stearyl alcohol; and higher fatty acid esters of glycerin such as monoglyceride stearate and diglyceride stearate. In the present invention, it is preferable to use higher alcohols and glycerin fatty acid monoesters in combination as the release agent. When higher alcohols and glycerin fatty acid monoesters are used in combination, the ratio is not particularly limited, but the mass ratio of higher alcohols / glycerin fatty acid monoesters is preferably 2.5 / 1 to 3.5 / 1, more preferably 2.8 / 1 to 3.2 / 1.
[0106] The polymer processing aid is a compound that is effective in achieving thickness accuracy and thinning when molding the resin composition of the present invention. The polymer processing aid is usually a polymer particle having a particle size of 0.05 to 0.5 μm, which can be produced by emulsion polymerization. The polymer particles may be single-layer particles made of a polymer with a single composition ratio and a single intrinsic viscosity, or multi-layer particles made of two or more polymers with different composition ratios or intrinsic viscosities. Among these, preferred are particles with a two-layer structure having an inner polymer layer with a low intrinsic viscosity and an outer polymer layer with a high intrinsic viscosity of 5 dl / g or more.
[0107] The polymer processing aid preferably has an intrinsic viscosity of 3 to 6 dl / g. If the intrinsic viscosity is too low, the effect of improving moldability tends to be low. If the intrinsic viscosity is too high, the melt fluidity of the resin composition tends to decrease.
[0108] The resin composition of the present invention may contain an impact resistance modifier. Examples of the impact resistance modifier include a core-shell type modifier containing an acrylic rubber or a diene rubber as a core layer component, and a modifier containing a plurality of rubber particles.
[0109] As the organic dye, a compound having a function of converting ultraviolet rays, which are considered to be harmful to resins, into visible light is preferably used. Examples of the light diffusing agent and the matting agent include glass particles, crosslinked polysiloxane particles, crosslinked polymer particles, talc, calcium carbonate, and barium sulfate. Examples of fluorescent materials include fluorescent pigments, fluorescent dyes, fluorescent white dyes, fluorescent brighteners, fluorescent bleaches, and the like.
[0110] These additives may be added at the stage of the reaction raw materials, at the stage of the reaction product, or at the stage of the methacrylic copolymer or resin composition obtained after devolatilization.
[0111] The methacrylic copolymer of the present invention or its resin composition, or the copolymer obtained by the manufacturing method of the present invention or its resin composition can be molded (melt-heat molded) by a conventional molding method such as injection molding, compression molding, extrusion molding, vacuum molding, etc., to obtain various molded products. Examples of the molded products of the present invention include signboard parts such as advertising towers, stand signs, side signs, transom signs, and rooftop signs; display parts such as showcases, partitions, and store displays; lighting parts such as fluorescent light covers, mood lighting covers, lampshades, light ceilings, light walls, and chandeliers; interior parts such as pendants and mirrors; architectural parts such as doors, domes, safety window glass, partitions, staircase wainscots, balcony wainscots, and leisure building roofs; transport parts such as aircraft windshields, pilot visors, motorcycles, motorboats, bus shading plates, automobile side visors, rear visors, head wings, and headlight covers; electronic equipment parts such as audiovisual nameplates, stereo covers, television protective masks, and vending machines; childcare and X-ray parts; equipment-related parts such as machine covers, instrument covers, experimental equipment, rulers, dials, and observation windows; optical parts such as liquid crystal protection plates, light guide plates, light guide films, Fresnel lenses, lenticular lenses, front panels of various displays, and diffusion plates; traffic-related parts such as road signs, information boards, convex mirrors, and soundproof walls; film components such as polarizer protective films, polarizing plate protective films, retardation films, surface materials for automobile interiors, surface materials for mobile phones, and marking films; home appliance components such as washing machine canopy materials and control panels, and rice cooker top panels; and other applications include greenhouses, large aquariums, box aquariums, clock panels, bathtubs, sanitary products, desk mats, game parts, toys, and face protection masks during welding.
[0112] The present invention will be described in more detail below with reference to the following examples. Note that the present invention is not limited to the following examples. The present invention also includes all aspects that are formed by any combination of the items expressing the technical features, such as the characteristic values, forms, manufacturing methods, and uses, described above.
[0113] Measurements of physical properties were carried out by the following methods.
[0114] (Polymerization conversion rate) A gas chromatograph GC-14A manufactured by Shimadzu Corporation was connected to an INERTCAP1 (df=0.4 μm, 0.25 mm I.D.×60 m) manufactured by GL Sciences Inc. as a column, and analysis was performed under the following conditions, and calculations were made based on the results. injection temperature=250℃ detector temperature=250℃ Temperature conditions: Hold at 60°C for 5 minutes → Raise temperature to 250°C at 10°C / min → Hold at 250°C for 10 minutes
[0115] (Weight average molecular weight Mw, molecular weight distribution Mw / Mn) The molecular weight of the copolymer was determined based on the molecular weight of standard polystyrene measured by gel permeation chromatography (GPC). Equipment: Tosoh GPC equipment HLC-8320 Separation column: Tosoh Corporation's TSKguardcolum SuperHZ-H, TSKgel HZM-M, and TSKgel SuperHZ4000 connected in series Eluent: Tetrahydrofuran Eluent flow rate: 0.35 ml / min Column temperature: 40℃ Detection method: Refractive index (RI), absorbance detector (UV)
[0116] (Composition of each unit in the copolymer) For α-methylstyrene-methyl methacrylate copolymer, 1 The proton ratio of the phenyl group of the α-methylstyrene unit and the methoxy group of the methyl methacrylate unit was determined by H-NMR, and the αMS of the α-methylstyrene unit was calculated from this. For α-methylstyrene-methyl methacrylate-maleic anhydride copolymer, 13The carbon ratios of the phenyl group of the α-methylstyrene unit, the carbonyl group of the methyl methacrylate unit, and the carbonyl group of the maleic anhydride unit were determined by C-NMR, and the αMS of the α-methylstyrene unit and Mah of the maleic anhydride unit were calculated from this.
[0117] (glass transition temperature Tg) In accordance with JIS K7121, a differential scanning calorimeter (Shimadzu Corporation, DSC-50 (product number)) was used to measure a DSC curve under the conditions of heating once to 250° C., then cooling to room temperature, and then heating from room temperature to 200° C. at a rate of 10° C. / min. The midpoint glass transition temperature determined from the DSC curve measured during the second heating was taken as the glass transition temperature in the present invention.
[0118] (Photoelastic coefficient K) A 1.0 mm sheet was obtained by press molding a methacrylic copolymer. A 15 mm x 60 mm test piece was cut out from the center of the obtained press molded sheet. Both ends of the long side direction of the cut out sheet were fixed so that the distance between the chucks was 45 mm, and tension was applied to the sheet in steps of 10 N from 0 N to 100 N using an X-axis dovetail stage B05-11BM manufactured by Suruga Seiki. The tension T was monitored by a sensor separate type digital force gauge ZPS-DPU-50N manufactured by Imada Co., Ltd. The phase difference PD at each tension was measured at the D line wavelength of Na using KOBRA-WR manufactured by Oji Scientific Instruments. After the phase difference measurement, the sheet was removed from the jig and the thickness d of the phase difference measurement part was measured. From the measured values, the cross-sectional area S of the sheet (S = 15 mm × d), stress σ (= T / S), and birefringence Δn (= PD / d) were calculated, and the stress σ was plotted on the horizontal axis and the birefringence Δn on the vertical axis. The slope of the straight line obtained by the least squares method was taken as the photoelastic coefficient.
[0119] (Orientation birefringence Δn) A 1.0 mm sheet was obtained by press molding the methacrylic copolymer. A 20 mm x 40 mm test piece was cut out from the center of the obtained press molded sheet, and the test piece was placed in an autograph with a heating chamber (manufactured by SHIMADZU). The grip distance in the autograph was set to 20 mm, and the sheet was held at the glass transition temperature +10°C for 3 minutes. Then, the sheet was stretched 100% in one direction at a speed of 3 mm / min (grip distance became 40 mm). The obtained stretched film was cooled to 23°C, removed from the autograph, and the phase difference PD of the central part of the stretched film was measured at the D-line wavelength of Na using KOBRA-WR manufactured by Oji Scientific Instruments. The thickness d of the retardation measurement part was measured. From the measured value, the birefringence Δn (=PD / d) was calculated, which was taken as the orientation birefringence.
[0120] The effects of the methacrylic copolymer of the present invention are shown in the following examples. The results of Examples Ie-1 to Ie-3 and Ic-1 to Ic-4 are shown in Table 1.
[0121] Example Ie-1 The methacrylic copolymer produced and isolated in Example IIe-3 described later was extruded into strands, and the strands were cut with a pelletizer to obtain resin pellets. The resulting methacrylic copolymer had a weight average molecular weight Mw of 133,000, a number average molecular weight Mn of 66,500, a mass fraction of methyl methacrylate units MMA of 92 mass%, a mass fraction of α-methylstyrene units αMS of 8 mass%, a glass transition temperature Tg of 128°C, a saturated water absorption rate As of 1.7%, and an orientation birefringence Δn of -2.2×10 -4 , the photoelastic coefficient K is -4.0×10 -12 Pa -1 , and |AB| / B was 0.011.
[0122] Example Ie-2 Resin pellets were obtained in the same manner as in Example Ie-1, except that the copolymer produced in Example IIe-1 described later was used instead. The resulting methacrylic copolymer had a weight average molecular weight Mw of 110,000, a number average molecular weight Mn of 55,000, a mass fraction of methyl methacrylate units MMA of 88 mass%, a mass fraction of α-methylstyrene units αMS of 12 mass%, a glass transition temperature Tg of 131° C., a saturated water absorption As of 1.6%, and an orientation birefringence Δn of −2.0×10 -4 , photoelastic coefficient K is -2.5×10 -12 Pa -1 , and |AB| / B was 0.012.
[0123] Example Ie-3 Resin pellets were obtained in the same manner as in Example Ie-1, except that the copolymer produced in Example IIe-6 described later was used instead. The resulting methacrylic copolymer had a weight average molecular weight Mw of 90,000, a number average molecular weight Mn of 42900, a mass fraction of methyl methacrylate units MMA of 82 mass%, a mass fraction of α-methylstyrene units αMS of 18 mass%, a glass transition temperature Tg of 134° C., a saturated water absorption As of 1.3%, and an orientation birefringence Δn of −1.6×10 -4 , the photoelastic coefficient K is -1.0×10 -12 Pa -1 , |AB| / B was 0.025.
[0124] Example Ic-1 A monomer mixture consisting of 95% by mass of methyl methacrylate and 5% by mass of α-methylstyrene and 400 ppm of 2,2'-azobis(2-methylpropionitrile) was obtained, and a reaction raw material having a dissolved oxygen content of more than 10 ppm was obtained. This reaction raw material was used instead of the reaction raw material obtained in Example Ie-1, and a polymerization conversion rate of 42% was obtained by the same method as in Example Ie-1. The obtained methacrylic copolymer had a weight average molecular weight Mw of 141,000, a number average molecular weight Mn of 70,500, a mass fraction of methyl methacrylate units MMA of 96% by mass, a mass fraction of α-methylstyrene units αMS of 4% by mass, a glass transition temperature Tg of 122°C, a saturated water absorption coefficient As of 1.9%, and an orientation birefringence Δn of -2.5×10 -4 , photoelastic coefficient K is -4.3×10-12 Pa -1 , |AB| / B was 0.011.
[0125] Example Ic-2 A reaction raw material containing a monomer mixture of 62.5% by mass of methyl methacrylate and 37.5% by mass of α-methylstyrene and 400 ppm of 2,2'-azobis(2-methylpropionitrile) and having a dissolved oxygen content of more than 10 ppm was obtained, and bulk polymerization was carried out in the same manner as in Example Ie-1, except that this reaction raw material was used instead of the reaction raw material obtained in Example Ie-1 having a dissolved oxygen content of more than 10 ppm. The polymerization conversion rate was 3%. The reaction product withdrawn was poured into methanol, and the solid content was precipitated and dried to obtain a methacrylic copolymer. The resulting methacrylic copolymer had a weight average molecular weight Mw of 80,000, a number average molecular weight Mn of 38,100, a mass fraction of methyl methacrylate units MMA of 80 mass%, a mass fraction of α-methylstyrene units αMS of 20 mass%, a glass transition temperature Tg of 125°C, a saturated water absorption As of 1.7%, and an orientation birefringence Δn of -7.4×10 -4 , the photoelastic coefficient K is -4.7×10 -12 Pa -1 , |AB| / B was 0.052.
[0126] Example Ic-3 A reaction raw material containing a monomer mixture of 85% by mass of methyl methacrylate and 15% by mass of α-methylstyrene and 400 ppm of 2,2'-azobis(2-methylpropionitrile) and having a dissolved oxygen content of more than 10 ppm was obtained, and this was used instead of the reaction raw material obtained in Example Ie-1 having a dissolved oxygen content of more than 10 ppm, and resin pellets were obtained with a polymerization conversion rate of 50% in the same manner as in Example Ie-1, except that the temperature during bulk polymerization was changed to 150°C. The obtained methacrylic copolymer had a weight average molecular weight Mw of 92,000, a number average molecular weight Mn of 46,000, a mass fraction of methyl methacrylate units MMA of 94% by mass, a mass fraction of α-methylstyrene units αMS of 6% by mass, a glass transition temperature Tg of 123°C, a saturated water absorption coefficient As of 1.8%, and an orientation birefringence Δn of -2.7×10 -4 , photoelastic coefficient K is -4.4×10 -12 Pa -1, |AB| / B was 0.055.
[0127] Example Ic-4 Into the autoclave, 85 parts by mass of methyl methacrylate, 15 parts by mass of α-methylstyrene, 0.47 parts by mass of pentaerythritol tetrakisthiopropionate, 0.06 parts by mass of azobisisobutyronitrile, 0.01 parts by mass of 1,1-bis(1,1-dimethylperoxy)cyclohexane, 231 parts by mass of water, 1.4 parts by mass of dispersant, and 17.5 parts by mass of pH adjuster were placed. While stirring the inside of the autoclave, the inside of the autoclave was raised from room temperature to 70°C, held at 70°C for 120 minutes, and then held at 120°C for 60 minutes to perform suspension polymerization. Thereafter, the temperature was lowered to room temperature, and the reaction product was extracted from the autoclave. The solid content was removed from the reaction product by filtration, washed with water, and dried with hot air at 80°C for 24 hours. The obtained solid content was fed to the hopper of a twin-screw extruder, melt-kneaded at a cylinder temperature of 230°C, and the molten resin was extruded to obtain resin pellets. The resulting copolymer had a weight average molecular weight Mw of 19,000, a number average molecular weight Mn of 9,000, and |AB| / B of 0.122. Because polymers with different average molecular weights were simultaneously produced, no further evaluation was performed.
[0128] [Table 1]
[0129] As shown by the above results, the methacrylic copolymer of the present invention has a high glass transition temperature (an index of heat resistance), a low saturated water absorption coefficient As, and small absolute values of orientation birefringence Δn and photoelastic coefficient K. The methacrylic copolymer of the present invention is suitable for optical members requiring highly accurate control of physical properties.
[0130] The effects of Production Method II of the present invention will be shown by comparison with the following examples. Table 2 shows the production conditions of Examples IIe-1 to IIe-6 and IIc-1 to IIc-4.
[0131] [Table 2]
[0132] Example IIe-1 In an autoclave equipped with a stirrer and a sampling tube, 85 parts by mass of purified methyl methacrylate MMA and 15 parts by mass of α-methylstyrene αMS were mixed. 2,2'-azobis(2-methylpropionitrile) AIBN was mixed to a concentration of 400 ppm. The amount of dissolved oxygen was over 10 ppm. Nitrogen gas was blown into the mixture to remove the amount of dissolved oxygen to 3 ppm, and the reaction raw material was obtained. The atmosphere in a continuous flow tank reactor equipped with a brine cooling condenser was replaced with nitrogen gas. The reaction raw materials were continuously supplied to the tank reactor at a constant flow rate so that the average residence time θ was 180 minutes, and bulk polymerization was carried out at a temperature of 120°C. At the same time, the reaction product was continuously withdrawn from the tank reactor. The pressure in the tank reactor was regulated by a pressure control valve connected to the brine cooling condenser. The amount of water present in the liquid in the tank reactor was maintained at 280 ppm or less, and the average concentration I of the radical polymerization initiator was 5.2 x 10 -5 mol / L. I×θ was 1.6×10 -4 The polymerization conversion rate was 40%. The reaction product was subjected to devolatilization to remove the remaining monomer mixture, and the α-methylstyrene-methyl methacrylate copolymer of Example Ie-2 was obtained. The ratio of the molar fraction of α-methylstyrene units in the copolymer to the molar fraction of α-methylstyrene in the monomer mixture was 0.796.
[0133] Example IIe-2 An α-methylstyrene-methyl methacrylate copolymer having a weight average molecular weight of 108,000, a number average molecular weight of 54,000, and a mass fraction of α-methylstyrene units of 13 mass% was obtained in the same manner as in Example IIe-1, except that 400 ppm of 2,2'-azobis(2-methylpropionitrile) was changed to 400 ppm of 1,1-bis(t-butylperoxy)cyclohexane. The average concentration I of the radical polymerization initiator present in the liquid in the tank-type reactor was 2.3×10 -4mol / L. I×θ was 6.8×10 -4 mol hr / L. The polymerization conversion was 43%. The ratio of the molar fraction of α-methylstyrene units in the copolymer to the molar fraction of α-methylstyrene in the monomer mixture was 0.796.
[0134] Example IIe-3 90 parts by mass of purified methyl methacrylate, 10 parts by mass of α-methylstyrene, and 0.05 parts by mass of n-octyl mercaptan were mixed in an autoclave equipped with a stirrer and a sampling tube. 2,2'-azobis(2-methylpropionitrile) was mixed with this to a concentration of 300 ppm to obtain a reaction raw material. Nitrogen gas was blown into the reaction raw material to remove dissolved oxygen to 3 ppm. The atmosphere in a continuous flow tank reactor equipped with a brine cooling condenser was replaced with nitrogen gas. The reaction raw materials were continuously supplied to the tank reactor at a constant flow rate so that the average residence time θ was 180 minutes, and bulk polymerization was carried out at a temperature of 120°C. At the same time, the reaction product was continuously withdrawn from the tank reactor. The pressure in the tank reactor was regulated by a pressure control valve connected to the brine cooling condenser. The average concentration I of the radical polymerization initiator present in the liquid in the tank reactor was 3.9×10 -5 mol / L. I×θ was 1.2×10 -4 The polymerization conversion rate was 41%. The withdrawn reaction product was subjected to adiabatic flash evaporation to remove the remaining monomer mixture, thereby obtaining the α-methylstyrene-methyl methacrylate copolymer of Example Ie-1. The ratio of the molar fraction of α-methylstyrene units in the copolymer to the molar fraction of α-methylstyrene in the monomer mixture was 0.798.
[0135] Example IIe-4 An α-methylstyrene-methyl methacrylate copolymer having a weight average molecular weight of 117,000, a number average molecular weight of 59,000, and a mass fraction of α-methylstyrene units of 8 mass% was obtained in the same manner as in Example IIe-3, except that the temperature during bulk polymerization was changed from 120°C to 110°C and the concentration of 2,2'-azobis(2-methylpropionitrile) was changed to 500 ppm. The average concentration I of the radical polymerization initiator present in the liquid in the tank reactor was 1.8 x 10 -4 mol / L. I×θ was 5.4×10 -4 mol hr / L. The polymerization conversion was 41%. The ratio of the molar fraction of α-methylstyrene units in the copolymer to the molar fraction of α-methylstyrene in the monomer mixture was 0.798.
[0136] Example IIe-5 An α-methylstyrene-methyl methacrylate copolymer having a weight average molecular weight of 59,000, a number average molecular weight of 30,000, and a mass fraction of α-methylstyrene units of 13 mass% was obtained in the same manner as in Example IIe-2, except that the temperature during bulk polymerization was changed from 120°C to 130°C and the concentration of 1,1-bis(t-butylperoxy)cyclohexane was changed to 300 ppm. The average concentration I of the radical polymerization initiator present in the liquid in the tank reactor was 7.0 x 10 -5 mol / L. I×θ was 2.1×10 -4 mol hr / L. The polymerization conversion was 41%. The ratio of the molar fraction of α-methylstyrene units in the copolymer to the molar fraction of α-methylstyrene in the monomer mixture was 0.796.
[0137] Example IIe-6 The α-methylstyrene-methyl methacrylate copolymer of Example Ie-3 was obtained in the same manner as in Example IIe-1, except that the amount of methyl methacrylate was changed to 75 parts by mass and the amount of α-methylstyrene was changed to 25 parts by mass. The average concentration I of the radical polymerization initiator present in the liquid in the tank-type reactor was 5.2×10 -5 mol / L. I×θ was 1.6×10 -4 The polymerization conversion rate was 35%. The ratio of the molar fraction of α-methylstyrene units in the copolymer to the molar fraction of α-methylstyrene in the monomer mixture was 0.712.
[0138] Example IIc-1 An α-methylstyrene-methyl methacrylate copolymer having a weight average molecular weight of 102,000 and a number average molecular weight of 51,000 was obtained in the same manner as in Example IIe-1, except that the temperature during bulk polymerization was changed from 120° C. to 90° C. The average concentration I of the radical polymerization initiator present in the liquid in the tank reactor was 9.1×10 -4 mol / L. I×θ was 2.7×10 -3 mol hr / L. The polymerization conversion rate was low at 13%.
[0139] Example IIc-2 An α-methylstyrene-methyl methacrylate copolymer having a weight average molecular weight of 83,000 and a number average molecular weight of 42,000 was obtained in the same manner as in Example IIe-1, except that 400 ppm of 2,2'-azobis(2-methylpropionitrile) was replaced with 400 ppm of t-hexylperoxyneodecanoate. The average concentration I of the radical polymerization initiator present in the liquid in the tank reactor was 1.9×10 -6 mol / L. I×θ was 5.7×10 -6 mol hr / L. The polymerization conversion rate was low at 22%.
[0140] Example IIc-3 An α-methylstyrene-methyl methacrylate copolymer having a weight average molecular weight of 295,000 and a number average molecular weight of 147,000 was obtained in the same manner as in Example IIe-1, except that the concentration of 2,2'-azobis(2-methylpropionitrile) was changed to 100 ppm. The average concentration I of the radical polymerization initiator present in the liquid in the tank-type reactor was 1.3 × 10 -5 mol / L. I×θ was 3.9×10 -5 mol hr / L. The polymerization conversion rate was low at 24%.
[0141] Example IIc-4 An α-methylstyrene-methyl methacrylate copolymer having a weight average molecular weight of 398,000 and a number average molecular weight of 199,000 was obtained in the same manner as in Example IIc-3, except that the average residence time θ was changed to 600 minutes. The average concentration I of the radical polymerization initiator present in the liquid in the tank reactor was 3.9×10 -6 mol / L. I×θ was 3.9×10 -5 The polymerization conversion rate was 43%. However, the average residence time was long, so the flexibility and responsiveness of production was low. Specifically, the production process could not be rearranged immediately in response to sudden small-lot production orders or changes in delivery dates.
[0142] As can be seen from the above results, according to the production method II of the present invention, an α-methylstyrene-methyl methacrylate copolymer can be produced at an appropriately high polymerization conversion rate and an appropriately long average residence time, which are suitable for a continuous bulk polymerization method.
[0143] The effects of the production method III of the present invention will be shown by comparison with the following examples. Table 3 shows the production conditions of Examples IIIe-1, IIIe-2 and IIIc-1 to IIIc-4.
[0144] [Table 3]
[0145] Example IIIe-1 In an autoclave equipped with a stirrer and a sampling tube, 82.0 parts by mass of methyl methacrylate MMA, 15.0 parts by mass of α-methylstyrene αMS, 3.00 parts by mass of maleic anhydride MAh, and 0.02 parts by mass of n-octyl mercaptan were mixed. 2,2'-azobis(2-methylpropionitrile) was mixed as a radical polymerization initiator to a concentration of 300 ppm. Nitrogen gas was blown into the mixture to obtain a reaction raw material with a dissolved oxygen content of 3 ppm. The atmosphere in a continuous flow tank reactor equipped with a brine cooling condenser was replaced with nitrogen gas. The reaction raw materials were continuously fed to the tank reactor at a constant flow rate so that the average residence time θ was 2.50 hours. The temperature was 130°C, and the average concentration I of the radical polymerization initiator present in the liquid in the tank reactor was 1.75×10 -5 The bulk polymerization reaction was carried out at 1000 mol / L, and at the same time, the reaction product with a polymerization conversion rate of 40% was continuously withdrawn from the tank reactor. The pressure inside the tank reactor was adjusted by a pressure control valve connected to the brine cooling condenser. I×θ was 4.37×10 -5 It is expressed in mol hr / L.
[0146] The withdrawn reaction product was subjected to adiabatic flash evaporation to remove the remaining monomer mixture, thereby obtaining an α-methylstyrene-methyl methacrylate-maleic anhydride copolymer shown in Example IVe-1 of Table 4. The ratio of the molar fraction of α-methylstyrene units in the copolymer to the molar fraction of α-methylstyrene in the monomer mixture was 0.830.
[0147] Example IIIe-2 In an autoclave equipped with a stirrer and a sampling tube, 70.0 parts by mass of methyl methacrylate, 20.0 parts by mass of α-methylstyrene, 10.0 parts by mass of maleic anhydride, and 0.005 parts by mass of n-octyl mercaptan were mixed. 2,2'-azobis(2-methylpropionitrile) was mixed as a radical polymerization initiator to a concentration of 300 ppm. Nitrogen gas was blown into the mixture to obtain a reaction raw material with a dissolved oxygen content of 3 ppm. The atmosphere in a continuous flow tank reactor equipped with a brine cooling condenser was replaced with nitrogen gas. The reaction raw materials were continuously fed to the tank reactor at a constant flow rate so that the average residence time θ was 2.50 hours. The temperature was 130°C, and the average concentration I of the radical polymerization initiator present in the liquid in the tank reactor was 1.79×10 -5 The bulk polymerization reaction was carried out at 1000 mol / L, and at the same time, the reaction product with a polymerization conversion rate of 58% was continuously withdrawn from the tank reactor. The pressure inside the tank reactor was adjusted by a pressure control valve connected to the brine cooling condenser. I×θ was 4.48×10 -5 It is expressed in mol hr / L.
[0148] The withdrawn reaction product was subjected to adiabatic flash evaporation to remove the remaining monomer mixture, thereby obtaining an α-methylstyrene-methyl methacrylate-maleic anhydride copolymer shown in Example IVe-2 in Table 4. The ratio of the molar fraction of α-methylstyrene units in the copolymer to the molar fraction of α-methylstyrene in the monomer mixture was 1.02.
[0149] Example IIIc-1 The temperature was set to 90°C, and the average concentration I of the radical polymerization initiator in the liquid in the tank reactor was set to 7.70 x 10 -6 A reaction product with a polymerization conversion rate of 20% was obtained in the same manner as in Example IIIe-1, except that the reaction product was changed to 1.91×10 -3 The polymerization conversion rate is low, so the yield per reactor volume is low.
[0150] Example IIIc-2 The reaction raw material was obtained in the same manner as in Example IIIe-1, except that 2,2'-azobis(2-methylpropionitrile) was replaced with 400 ppm of t-hexylperoxyneodecanoate. Using this reaction raw material, the average concentration I of the radical polymerization initiator present in the liquid in the tank-type reactor was adjusted to 9.77 x 10 -7 A reaction product with a polymerization conversion rate of 28% was obtained in the same manner as in Example IIIe-1, except that the reaction product was changed to 1.0 mol / L. A copolymer was obtained in the same manner as in Example IIIe-1, except that the reaction product was used. I×θ was 2.40×10 -6 The polymerization conversion rate is low, so the yield per reactor volume is low.
[0151] Example IIIc-3 The reaction raw material was obtained in the same manner as in Example IIIe-1, except that the concentration of 2,2'-azobis(2-methylpropionitrile) was changed to 60 ppm. Using this reaction raw material, the average concentration I of the radical polymerization initiator present in the liquid in the tank-type reactor was 3.49 x 10 -6 A reaction product with a polymerization conversion rate of 23% was obtained in the same manner as in Example IIIe-1, except that the reaction product was changed to 1.0 mol / L. A copolymer was obtained in the same manner as in Example IIIe-1, except that the reaction product was used. I×θ was 8.74×10 -6 mol·hr / L. The resulting copolymer had a weight average molecular weight of 121,000 and a number average molecular weight of 60,500. The polymerization conversion rate was low, so the yield per reactor volume was low.
[0152] Example IIIc-4 The reaction raw materials were obtained in the same manner as in Example IIIc-3, and the average residence time θ was set to 10.0 hours and the average concentration I of the radical polymerization initiator in the liquid in the tank reactor was set to 8.80×10 -7 A reaction product with a polymerization conversion rate of 38% was obtained in the same manner as in Example IIIc-3, except that the reaction product was changed to . A copolymer was obtained in the same manner as in Example IIIe-1, except that the reaction product was used. I×θ was 8.80×10 -6 mol·hr / L. The resulting copolymer had a weight-average molecular weight of 130,000 and a number-average molecular weight of 65,000. A long average residence time is required to reach the desired polymerization conversion rate, resulting in low flexibility or responsiveness in production. Specifically, the production process cannot be immediately rearranged in response to sudden small-lot production orders or changes in delivery dates.
[0153] As can be seen from the above results, according to Production Method III, a copolymer having a ring structure in the main chain can be produced with an appropriately high polymerization conversion rate and an appropriately long average residence time, which are suitable for a continuous polymerization method.
[0154] [Table 4]
[0155] Example IVe-1 The copolymer obtained in Example IIIe-1 was evaluated.
[0156] Example IVe-2 The copolymer obtained in Example IIIe-2 was evaluated.
[0157] Example IVc-1 Resin pellets were obtained by the same treatment as in Example IIIe-1, except that the polymerization temperature was increased to 150° C. The resulting α-methylstyrene-methyl methacrylate-maleic anhydride copolymer had a weight average molecular weight of 85,000, a number average molecular weight of 42,500, a mass fraction of α-methylstyrene units of 10 mass%, a mass fraction of maleic anhydride units of 2 mass%, a glass transition point of 122° C., and an orientation birefringence of −6.6×10 -4 , photoelastic coefficient is -4.5×10 -12 Pa -1 , |AB| / B was 0.055.
[0158] Example IVc-2 Resin pellets were obtained by the same process as in Example IIIe-1, except that the monomer mixture was changed to 97% by mass of methyl methacrylate, 2% by mass of α-methylstyrene, and 1% by mass of maleic anhydride. The resulting α-methylstyrene-methyl methacrylate-maleic anhydride copolymer had a weight average molecular weight of 90,000, a number average molecular weight of 40,900, a mass fraction of α-methylstyrene units of 1% by mass, a mass fraction of maleic anhydride units of 0.5% by mass, a glass transition point of 124° C., and an orientation birefringence of −2.6×10 -4 , photoelastic coefficient is -4.6×10 -12 Pa -1 , |AB| / B was 0.003.
Claims
1. A methacrylic copolymer comprising 70 to 93 mass % of methyl methacrylate units, 7 to 30 mass % of α-methylstyrene units, and 0 to 23 mass % of other monomer units copolymerizable therewith, and satisfying the relationship of formula (1). |A-B| / B < 0.05 (1) In the above, A is the molecular weight at the peak top in a differential molecular weight distribution curve obtained by gel permeation chromatography measurement using a differential refractive index detector, and B is the molecular weight at the peak top in a differential molecular weight distribution curve obtained by gel permeation chromatography measurement using an absorbance detector with a detection wavelength of 254 nm.
2. The methacrylic copolymer according to claim 1, wherein the other copolymerizable monomer unit is a monomer unit having a ring structure.
3. The methacrylic copolymer according to claim 1 or 2, which has a glass transition temperature of 125° C. or higher.
4. Photoelastic coefficient is -4.3 x 10 -12 / Pa~+4.3×10 -12 The methacrylic copolymer according to any one of claims 1 to 3, wherein the viscosity is 100% or more.
5. A 20 mm x 40 mm x 1.0 mm thick sheet made of a methacrylic copolymer is stretched 100% in one direction at a speed of 3 mm / min at a temperature 10° C. higher than the glass transition temperature, and the birefringence of the stretched film obtained is −10×10 -4 ~ +10 x 10 -4 The methacrylic copolymer according to any one of claims 1 to 4.
6. A resin composition comprising the methacrylic copolymer according to any one of claims 1 to 5.
7. A resin composition comprising an antioxidant and the methacrylic copolymer according to any one of claims 1 to 5.
8. A molded article comprising the methacrylic copolymer according to any one of claims 1 to 5 or the resin composition according to claim 6 or 7.
9. A film comprising the methacrylic copolymer according to any one of claims 1 to 5 or the resin composition according to claim 6 or 7.
10. An optical film comprising the methacrylic copolymer according to any one of claims 1 to 5 or the resin composition according to claim 6 or 7.
11. A laminate comprising a layer containing the methacrylic copolymer according to any one of claims 1 to 5 and a layer containing another thermoplastic resin.
12. A reaction raw material including a monomer mixture containing 70 to 93 mass % of methyl methacrylate, 7 to 30 mass % of α-methylstyrene, and 0 to 10 mass % of other monomers copolymerizable therewith, and a radical polymerization initiator is continuously supplied to a tank-type reactor; The monomer mixture is bulk polymerized in a tank reactor at a polymerization conversion rate of 30 to 60 mass% to obtain a reaction product; The reaction product is continuously withdrawn from the tank reactor; and removing from the reaction product any monomer mixture remaining in the withdrawn reaction product; The temperature in the tank reactor is 110° C. or higher and 140° C. or lower, The average residence time θ of the reaction raw materials in the tank reactor is 1.5 to 4.5 hours, When the average concentration of the radical polymerization initiator in the liquid in the tank reactor is I mol / L and the average residence time of the reaction raw materials in the tank reactor is θ hr, the product I×θ is 1×10 -4 mol・hr / L and over 1×10 -3 Less than mol·hr / L A method for producing the methacrylic copolymer according to claim 1.
13. The process of claim 12, wherein the reactants further comprise a chain transfer agent.
14. A reaction raw material including 100 parts by mass of a monomer mixture consisting of 40 to 92% by mass of methyl methacrylate, 7 to 25% by mass of α-methylstyrene, 1 to 25% by mass of a monomer capable of introducing a ring structure into the main chain by a polymerization reaction, and 0 to 10% by mass of another monomer copolymerizable therewith, 0 to 30 parts by mass of an organic solvent, and a radical polymerization initiator is continuously supplied to a tank-type reactor; subjecting the monomer mixture to a polymerization reaction in a tank-type reactor to obtain a reaction product; The reaction product is continuously withdrawn from the tank reactor; and removing from the reaction product any monomer mixture remaining in the withdrawn reaction product; The temperature in the tank reactor is 110° C. or higher and 140° C. or lower, The average residence time θ of the reaction raw materials in the tank reactor is 1.5 to 4.5 hours, When the average concentration of the radical polymerization initiator present in the liquid in the tank reactor is I mol / L and the average residence time of the reaction raw materials in the tank reactor is θ hr, the product I×θ is 1.0×10 -5 mol hr / L and over 1.5 x 10 -4 mol hr / L or less, the polymerization conversion rate is 30 to 65% by mass; A method for producing a methacrylic copolymer.
15. The process of claim 14, wherein the reactants further comprise a chain transfer agent.
Citation Information
Patent Citations
JP1974010156A
Continuous preparation of methyl methacrylate syrup
JP1979054189A
Transfer of high-temperature polymerizable liquid composition
JP1984210910A
Production of heat-resistant methacrylic resin
JP1985147417A
Heat-resistant methacrylic resin composition
JP1986152758A