Dummy sheet for twin-roll continuous casting and method for manufacturing thin-walled cast strip

The dummy sheet with a heat-generating reinforcing member addresses the instability in twin-roll continuous casting by enhancing molten steel temperature and connecting the dummy sheet and thin slab, preventing hot band formation and ensuring stable casting.

JP7572601B2Active Publication Date: 2024-10-24NIPPON STEEL CORPORATION
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020071034
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-04-10
Publication Date
2024-10-24
Estimated Expiration
2040-04-10

AI Technical Summary

Technical Problem

Existing twin-roll continuous casting methods face issues with unstable casting conditions at the start, leading to insufficient thin slab strength, breakage due to hot bands, and metal formation on side weirs, which are not adequately addressed by prior techniques such as preheating side weirs or using high steam pressure metal members.

Method used

A dummy sheet for twin-roll continuous casting with a reinforcing member containing a heat-generating material, such as Si-containing alloys, is used to increase the temperature of the molten steel near the width ends, suppressing metal formation and growth, and ensuring stable casting by connecting the dummy sheet and thin slab.

Benefits of technology

The dummy sheet effectively suppresses hot band formation and ensures stable casting by maintaining the strength of the thin slab, preventing breakage and ensuring uniform temperature distribution in the molten steel pool.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572601000001
    Figure 0007572601000001
  • Figure 0007572601000002
    Figure 0007572601000002
  • Figure 0007572601000003
    Figure 0007572601000003
Patent Text Reader

Abstract

To provide a twin roll type continuous casting dummy sheet which enables suppression of generation of a bullion on a surface of a side weir at the time of starting casting, suppression of breaking of a thin slab caused by a hot band, and stable starting of casting.SOLUTION: A twin roll type continuous casting dummy sheet 30 is used for a twin roll type continuous casting device that manufactures a thin slab by supplying molten steel to a molten steel storage part 16 formed by a pair of rotating cooling rolls 11, 11 and a pair of side weirs and forming / growing a solidified shell on the circumferential surface of each of the cooling rolls 11. The dummy sheet comprises: a sheet body 31 that is held between the pair of cooling rolls 11, 11; and a reinforcing member 32 that extends from one end of the sheet body 31 in the longitudinal direction, and is inserted along each cooling roll 11 into the molten steel. Exothermic materials 35 that exothermically react when added to the molten steel are arranged at both ends of the reinforcing member 32 in a width direction.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a twin-roll continuous casting dummy sheet used at the start of casting in a twin-roll continuous casting apparatus that produces thin slabs by supplying molten steel to a molten steel reservoir formed by a pair of cooling rolls and a pair of side weirs, and to a method for producing thin slabs. [Background technology]

[0002] As a method for producing a thin-walled cast slab of steel, a twin-roll continuous casting apparatus is provided which is equipped with chill rolls having an internal water-cooling structure, in which molten steel is supplied to a molten steel reservoir formed between a pair of rotating chill rolls, a solidified shell is formed and grown on the peripheral surface of the chill rolls, and the solidified shells formed on the peripheral surfaces of the pair of chill rolls are joined at a roll kiss point and pressed down to produce a thin-walled cast slab of a predetermined thickness.

[0003] When starting casting in the above-mentioned twin-roll continuous casting method, as shown in Patent Documents 1 and 2, for example, a dummy sheet is sandwiched between the chill rolls, and the chill rolls are rotated while molten steel is supplied to a molten steel reservoir formed by a pair of chill rolls and a pair of side weirs, to form a thin cast strip connected to the dummy sheet, and the dummy sheet and the thin cast strip connected to this dummy sheet are pulled out from between the chill rolls.

[0004] At the start of casting, since the casting conditions such as the amount of molten steel supplied to the molten steel reservoir and the temperature of the cooling rolls are not stable, the strength of the thin billet formed to be connected to the dummy sheet is insufficient, and a trouble occurs in which the thin billet breaks when the dummy sheet is pulled out, making it impossible to start casting. For this reason, the above-mentioned Patent Documents 1 and 2 propose a technique for ensuring the strength of the thin billet at the start of casting by arranging a reinforcing member to be connected to the dummy sheet and casting the reinforcing member with molten metal.

[0005] Here, at the start of casting, the temperatures of the chill rolls and side gates are low, so that molten steel solidifies near the side gates, and ingots tend to form and grow on the surfaces of the side gates. In addition, since the flow of molten steel tends to stagnate near the width ends of the molten steel reservoir, if, for example, solidified pieces formed on the surface of the cooling roll are peeled off by the poured molten steel flow and float in the molten steel, these solidified pieces will agglomerate near the width ends of the molten steel reservoir and accumulate on the surface of the side weir, promoting the growth of the ingot.

[0006] When this ingot grows and fuses with the solidified shell on the circumferential surface of the rotating chill roll at the end of the chill roll, the ingot is peeled off from the side gate surface and is caught in the roll kiss point together with the solidified shell and sent out to the bottom of the casting machine. At this time, the roll gap temporarily expands beyond the original thickness of the slab in order to pass the thick ingot, and the part not wrapped with the ingot (for example, the center in the width direction) contains a large amount of unsolidified molten steel. This is called a hot band. This hot band is fragile at high temperatures and can break under the weight of the thin slab.

[0007] In order to prevent breakage caused by hot bands and ensure stable casting, it is important to prevent the formation of ingots on the side gates. Hot bands are likely to occur when the metal formed on the side gate peels off when the molten metal level is unstable. They are also likely to occur during the rise of the molten metal level in the early stages of casting. This is because the molten steel comes into contact with the side gate surface, which has not been in contact with molten steel until then, and is cooled, which makes it easy for metal to form.

[0008] As a method for preventing breakage of thin-walled cast strips due to hot bands, for example, Patent Document 3 proposes a means for suppressing the generation of metal on the surface of the side dam at the start of casting by sufficiently preheating the side dam. Furthermore, Patent Document 4 proposes a technology in which high vapor pressure metal members are disposed at both widthwise ends of a reinforcing member of a dummy sheet, and the molten steel at the widthwise ends of a molten steel reservoir is stirred by vaporized gas, thereby suppressing the generation of metal. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Japanese Patent Application Publication No. 57-058957 [Patent Document 2] Japanese Patent Application Publication No. 63-224847 [Patent Document 3] Japanese Patent Application Publication No. 62-124051 [Patent Document 4] JP 2018-114540 A Summary of the Invention [Problem to be solved by the invention]

[0010] Even if the side dam is preheated as in Patent Document 3, the temperature of the side dam inevitably drops because the side dam is brought into close contact with the end face of the chill roll to form a molten steel reservoir. When the molten steel level rises to a steady level in the early stages of casting, the molten steel first comes into contact with the side dam, whose temperature has been reduced by being pressed against the end face of the chill roll, and this makes it more likely that ingots will be produced, and there is a very high risk of breakage due to hot bands. Note that the higher the melting point of the steel, the more the side dam needs to be preheated to a high temperature. Therefore, in the case of carbon steel, which has a relatively high melting point compared to stainless steel, the side dam is preheated insufficiently, and hot bands tend to occur more easily.

[0011] Furthermore, as in Patent Document 4, it is possible to suppress the generation of metal by disposing high vapor pressure metal members at both widthwise ends of the reinforcing member of the dummy sheet and stirring the molten steel at the widthwise ends of the molten steel basin with vaporized gas; however, for example, if solidified pieces formed on the surface of the chill roll are peeled off by the poured molten steel flow and float in the molten steel, it is not possible to melt these solidified pieces.

[0012] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide a dummy sheet for twin-roll continuous casting that can sufficiently suppress the formation and growth of metal on the surface of a side dam at the start of casting, suppress breakage of a thin-walled cast strip caused by hot bands, and enable a stable start of casting, and a method for manufacturing a thin-walled cast strip using this dummy sheet for twin-roll continuous casting. [Means for solving the problem]

[0013] In order to solve the above problems, the present invention provides a twin-roll continuous casting dummy sheet for use in a twin-roll continuous casting apparatus which supplies molten steel to a molten steel reservoir formed by a pair of rotating chill rolls and a pair of side gates, and produces a thin-walled cast strip by forming and growing a solidified shell on the peripheral surface of the chill rolls, the dummy sheet comprising a sheet body held between the pair of chill rolls, and a reinforcing member extending from one longitudinal end of the sheet body and inserted into the molten steel along the chill rolls, and the reinforcing member has a reinforcing member at each of both widthwise ends which reacts exothermically when added to the molten steel. to increase the temperature of the molten steel. A heat generating material is provided, the heat generating material comprising: Silicon-containing material containing 76%mass% or more of silicon The present invention is characterized in that:

[0014] According to the twin-roll continuous casting dummy sheet having the above-mentioned configuration, a heat generating material that reacts exothermically when added to the molten steel is disposed at both widthwise ends of the reinforcing member extending from one longitudinal end of the sheet body. Therefore, when the reinforcing member is immersed in the molten steel at the start of casting, the heat generating material disposed at both widthwise ends of the reinforcing member reacts exothermically with the molten steel, thereby raising the temperature of the molten steel near the widthwise ends of the molten steel reservoir. This makes it possible to suppress the generation and growth of metal near the widthwise ends of the molten steel reservoir. It is also possible to melt floating solidified pieces. This makes it possible to suppress the generation of hot bands, suppress breakage of thin-walled cast pieces caused by hot bands, and start casting stably.

[0016] Furthermore, in the twin-roll continuous casting dummy sheet of the present invention, it is preferable that the boundary position on the widthwise central side of the area in which the heat generating material is arranged is within a range of 20 mm to 200 mm from the widthwise end of the reinforcing member. In this case, at the start of casting, heat generating material can be accurately supplied to the widthwise ends of the molten steel reservoir, making it possible to sufficiently suppress the generation and growth of metal in the vicinity of the widthwise ends of the molten steel reservoir.

[0017] In the twin-roll continuous casting dummy sheet of the present invention, the reinforcing member is preferably made of a high melting point material having a melting point of 1510° C. or higher. The reinforcing member acts as a cooling material to promote the formation of a solidified shell on the circumferential surface of the chill roll, increasing the strength of the thin-walled cast piece in the early stages of casting, and also connects the dummy sheet and the thin-walled cast piece with its own strength. By making the reinforcing member from a high-melting-point material having a melting point of 1510°C or higher, the strength of the reinforcing member can be ensured even when the temperature of the molten steel rises due to the reaction between the heat-generating material and the molten steel, and the dummy sheet and the thin-walled cast piece can be reliably connected, making it possible to start casting stably.

[0018] The method for producing a thin cast slab according to the present invention is a method for producing a thin cast slab by supplying molten steel to a molten steel pool formed by a pair of rotating chill rolls and a pair of side gates, and forming and growing a solidified shell on the peripheral surface of the chill rolls to produce a thin cast slab, and at the start of casting, the above-mentioned twin-roll continuous casting dummy sheet is used to supply molten steel to a molten steel pool formed by a pair of rotating chill rolls and a pair of side gates to produce a thin cast slab. To the department The heating material is supplied.

[0019] According to this method for producing a thin slab, the above-mentioned twin-roll continuous casting dummy sheet is used at the start of casting, so that the heat generating material can be supplied to the widthwise end of the molten steel reservoir at the start of casting, and the heat generating material and the molten steel react with each other to raise the temperature of the molten steel near the widthwise end of the molten steel reservoir. This makes it possible to suppress the occurrence of hot bands and to suppress breakage of the thin slab due to hot bands. This makes it possible to stably cast the thin slab.

[0020] In the method for producing a thin-walled cast slab according to the present invention, a cold material may be supplied to the widthwise center of the molten steel reservoir in accordance with the pouring conditions at the start of casting. In this case, the temperature of the molten steel at the widthwise center of the molten steel reservoir can be prevented from becoming too high due to the exothermic reaction between the heat-generating material and the molten steel, and the temperature distribution in the width direction of the molten steel reservoir can be made uniform, thereby enabling stable casting of thin-walled cast strips. Effect of the Invention

[0021] As described above, according to the present invention, it is possible to provide a dummy sheet for twin-roll continuous casting that can sufficiently suppress the generation and growth of metal on the surface of the side dam at the start of casting, suppress breakage of the thin billet due to hot bands, and enable a stable start of casting, and a method for manufacturing a thin billet using this dummy sheet for twin-roll continuous casting. [Brief description of the drawings]

[0022] [Figure 1] FIG. 1 is an explanatory diagram showing an example of a twin-roll continuous casting apparatus according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a perspective view of a molten steel reservoir of the twin-roll continuous casting apparatus shown in FIG. [Diagram 3] 2 is an explanatory diagram showing a molten steel reservoir and ingots in the twin-roll continuous casting apparatus shown in Fig. 1. (a) shows the shape of the molten steel reservoir, and (b) shows the ingots formed on the surface of the side weir. [Figure 4]1A and 1B are explanatory views of a dummy seat for twin-roll continuous casting according to one embodiment of the present invention, in which (a) is a side view and (b) is a front view. [Diagram 5] FIG. 1 is an explanatory diagram of a dummy sheet for twin-roll continuous casting according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] Hereinafter, a twin-roll continuous casting dummy sheet (hereinafter, sometimes simply referred to as a dummy sheet) and a method for producing a thin-walled cast piece according to an embodiment of the present invention will be described with reference to the accompanying drawings. Note that the present invention is not limited to the following embodiment. Here, the thin-walled cast slab 1 produced in this embodiment is made of steel of various compositions, and has a width within the range of 500 mm to 2000 mm, and a thickness within the range of 1 mm to 5 mm.

[0024] Examples of steel types include 0.001-0.01% C extra low carbon steel, 0.02-0.05% C low carbon steel, 0.06-0.4% C medium carbon steel, 0.5-1.2% C high carbon steel, austenitic stainless steel such as SUS304 steel, ferritic stainless steel such as SUS430 steel, 3.0-4.0% Si oriented electrical steel, 0.1-6.5% Si non-oriented electrical steel, etc. (% is by mass).

[0025] Next, a twin-roll continuous casting apparatus 10 used in the method for producing a thin-walled cast strip according to this embodiment will be described. As shown in FIG. 1 , the twin-roll continuous casting apparatus 10 of this embodiment comprises a pair of chill rolls 11, 11, pinch rolls 12, 12 and 13, 13 supporting a thin cast strip 1, side dams 15 arranged at the widthwise ends of the pair of chill rolls 11, 11, a tundish 18 for holding molten steel 3 to be supplied to a molten steel reservoir 16 defined by the pair of chill rolls 11, 11 and the side dam 15, and an immersion nozzle 20 for supplying molten steel 3 from the tundish 18 to the molten steel reservoir 16.

[0026] In this twin-roll continuous casting apparatus 10, molten steel 3 comes into contact with the rotating chill rolls 11, 11 and is cooled, causing solidified shells 5, 5 to grow on the peripheral surfaces of the chill rolls 11, 11, and the solidified shells 5, 5 formed on the pair of chill rolls 11, 11 are pressed together at the roll kiss points, thereby casting a thin-walled cast strip 1 of a predetermined thickness.

[0027] As shown in FIGS. 2 and 3, a side dam 15 is provided on the end face of the chill roll 11 to define a molten steel reservoir 16. As shown in FIG. 3( a ), the molten steel reservoir 16 has a wedge shape surrounded by two bottom surfaces formed by the peripheral surfaces of a pair of chill rolls 11, 11, side surfaces supported by the surfaces of the side dams 15 on both sides, and a molten steel surface that is surrounded on all four sides by the peripheral surfaces of the pair of chill rolls 11, 11 and the pair of side dams 15, forming a rectangular shape. The molten steel 3 in the molten steel reservoir 16 is originally solidified on the peripheral surface of the chill roll 11 and drawn downward as a thin billet 1. However, the surface of the side dam 15 forming the side of the molten steel reservoir 16 is cooled as it comes into direct sliding contact with the end of the chill roll 11, and so ingots 7 are likely to form on the surface of the side dam 15 forming the side of the molten steel reservoir 16, as shown in Fig. 3(b). In particular, the ingots 7 near the sliding contact line with the chill roll 11 are likely to join together, and if they irregularly combine with the thin billet 1 and bite into the chill roll 11, a hot band will form, which may cause a breakage.

[0028] In the twin-roll continuous casting apparatus 10 of this embodiment, at the start of casting, a twin-roll continuous casting dummy sheet 30 of this embodiment is placed between a pair of cooling rolls 11, 11, as shown in FIG. As shown in FIG. 4, this twin-roll continuous casting dummy sheet 30 comprises a sheet body 31 arranged from below a pair of cooling rolls 11, 11 to the roll kiss point, and a reinforcing member 32 extending from one longitudinal end of the sheet body 31 and into the molten steel reservoir 16. The reinforcing member 32 is suitably a metal thin plate having a melting point at least equal to or higher than that of the steel type to be cast and having bending elasticity that allows it to be disposed along the peripheral surface of the chill roll 11. Suitable metals include ultra-low to low carbon steel, molybdenum, etc. In this embodiment, the reinforcing member 32 is preferably made of a high melting point material having a melting point of 1510° C. or higher.

[0029] With the dummy sheet 30 disposed as described above, the molten steel 3 is poured from the tundish 18 through the submerged nozzle 20 toward the molten steel reservoir 16. When the surface of the molten steel 3 in the molten steel reservoir 16 reaches a predetermined position, the chill rolls 11, 11 are rotated. Then, the molten steel 3 moves between the chill rolls 11, 11 together with the reinforcing member 32, and as the solidification of the molten steel 3 progresses, the reinforcing member 32 and the thin billet 1 are joined together, and the thin billet 1 is pulled out following the dummy sheet 30.

[0030] Here, at the start of casting, the temperatures of the chill roll 11 and side weir 15 are low, so in the process of pouring molten steel 3 into the molten steel reservoir 16 and the molten steel level rising, ingot 7 may be formed and grow on the surface of the side weir 15. In addition, solidified pieces formed on the surface of the chill roll 11 are peeled off by the poured molten steel flow and float in the molten steel 3, and these solidified pieces aggregate and accumulate in the vicinity of the widthwise ends of the molten steel reservoir 16, promoting the growth of the ingot 7. The metal 7 thus generated generates hot bands, which can cause the thin-walled cast slab 1 to break. Therefore, in the twin-roll continuous casting dummy sheet 30 of this embodiment, in order to suppress the generation of ingot 7 at the start of casting, a heat generating material 35 that reacts exothermically when added to molten steel 3 is disposed at least on both widthwise ends of the reinforcing member 32.

[0031] In this embodiment, as shown in FIG. 4(b), it is preferable that the boundary position on the widthwise center side of the area in which the heat generating material 35 is arranged is within a range of 20 mm to 200 mm from the widthwise end of the reinforcing member 32.

[0032] Here, the heat generating material 35 contains a heat generating material that reacts exothermically when added to the molten steel 3. Examples of the heat generating material include those containing elements such as Si, Al, and V. Among these, it is most preferable to use Si because it generates a large amount of heat when added to the molten steel 3. In this embodiment, the heat generating material 35 is preferably a Si-containing material that contains more than 50 mass % of Si.

[0033] Specifically, an Fe-Si alloy (ferrosilicon) can be used as the heat generating material 35. For example, when ferrosilicon No. 2 with a Si content of 76 mass% is added to molten steel, even if the added heat generating material 35 (ferrosilicon No. 2) is at room temperature, the temperature of the molten steel can be raised by about 14°C by adding 1 mass% of the molten steel. The ferrosilicon may be that specified in the Japanese Industrial Standard JIS G 2302:1998 or that specified in the international standard ISO5445-1980.

[0034] The amount of temperature rise of the molten steel when the heat generating material 35 contains Si will be described below. The temperature rise of molten steel when 1 mass% of the molten steel is added with room temperature heat generating material 35 is ΔT a is roughly approximated by the following equation (1). (1) Formula: ΔT a =30×[1-(100-A Si ) / 60] 1.5 (50≦A Si ≦100) Here, A Si : Si content (mass%) of the heat generating material 35 to be added

[0035] Next, the amount of molten steel in the widthwise end region of the molten steel reservoir 16 is defined by the following formula (2). (2) Formula: M E =700×H×[R-(R 2 -H 2 ) 0.5 ] Here, M E : Weight of molten steel in one end width region (kg) R: Radius of cooling roll 11 (m) H: Depth of molten steel reservoir 16 (m)

[0036] The temperature rise ΔT of the molten steel 3 in the width end region of the molten steel reservoir 16 E (℃) is expressed by the following formula (3). (3) Formula: ΔT E =100×ΔT a ×(W A / M E ) Here, W A : Amount of heat generating material 35 disposed on one end

[0037] In the above formula (3), the temperature rise ΔT E The Si content A in formula (1) is set so that Si The amount of heat generating material 35 disposed on one end in formula (3) W A To determine. Here, ΔT E If ΔT is less than 5°C, sufficient heating effect cannot be obtained. E If the temperature rise amount ΔT exceeds 60° C., the cracking sensitivity of the thin-walled cast slab 1 increases, and the quality may be impaired. E The temperature is set to 10°C or higher and 50°C or lower. The total amount of heat generating material 35 installed at both ends of the width is 2W. A It becomes.

[0038] The heat generating material 35 may be in the form of a lump, granules, or powder, and there is no limitation on its shape or form. The heat generating material 35 can be disposed on the reinforcing member 32 of the dummy sheet 30 in the following manner, but the method is not particularly limited. A lump-shaped heat generating material 35 is placed on one surface of the reinforcing member 32. The granular heat generating material 35 is pressed onto one surface of the reinforcing member 32 . The heat generating material 35 in powder or granular form is wrapped in iron foil and fixed to one side of the reinforcing member 32. The granular heat generating material 35 is dropped onto one surface of the reinforcing member 32.

[0039] Here, the addition of the heat generating material 35 increases the temperature of the molten steel in the molten steel reservoir 16. However, if the width of the submerged nozzle 20 is small compared to the wide chill roll 11, there is a risk that the difference in molten steel temperature between the width ends and width center of the molten steel reservoir 16 will become large. Therefore, in order to make the molten steel temperature uniform at the widthwise ends and widthwise center of the molten steel reservoir 16, a cooling material (iron powder, thin steel sheet pieces, steel wool, etc.) may be charged into the widthwise center of the molten steel reservoir 16. The widthwise center refers to the portion in the width direction of the dummy sheet reinforcing member disposed in the molten steel reservoir 16 excluding the end regions where the heat generating material 35 is disposed.

[0040] According to the twin-roll continuous casting dummy sheet 30 and the manufacturing method of the thin billet, which are the present embodiment, and which are configured as described above, the heat generating material 35, which reacts exothermically when added to the molten steel 3, is disposed at both ends in the width direction of the reinforcing member 32 extending from one end in the longitudinal direction of the sheet body 31. Therefore, when the reinforcing member 32 is immersed in the molten steel 3 at the start of casting, the heat generating material 35 disposed at both ends in the width direction of the reinforcing member 32 reacts exothermically with the molten steel 3, and the temperature of the molten steel in the vicinity of the width end of the molten steel reservoir 16 can be increased. This makes it possible to suppress the occurrence and growth of the ingot 7 in the vicinity of the width end of the molten steel reservoir 16. In addition, it is also possible to melt floating solidified pieces. Therefore, the occurrence of hot bands can be suppressed, and the breakage of the thin billet 1 caused by the hot bands can be suppressed, and casting can be started stably.

[0041] Furthermore, in this embodiment, when the heat generating material 35 is a Si-containing material containing more than 50 mass% Si, it is possible to sufficiently increase the temperature of the molten steel in the vicinity of the width end portion of the molten steel reservoir 16 when the reinforcing member 32 is immersed in the molten steel 3.

[0042] Furthermore, in this embodiment, when the boundary position L on the widthwise central side of the area in which the heat generating material 35 is arranged is within a range of 20 mm to 200 mm from the widthwise end of the reinforcing member 32, the heat generating material 35 can be accurately supplied to the widthwise end of the molten steel reservoir 16 at the start of casting, and the generation and growth of the ingot 7 in the vicinity of the widthwise end of the molten steel reservoir 16 can be sufficiently suppressed.

[0043] Furthermore, in this embodiment, when the reinforcing member 32 is made of a high melting point material having a melting point of 1510°C or higher, even if the molten steel temperature rises due to the reaction between the heat generating material 35 and the molten steel 3, the strength of the reinforcing member 32 can be ensured, the dummy sheet 30 and the thin-walled cast piece 1 can be reliably connected, and casting can be started stably.

[0044] Furthermore, in this embodiment, when a cold material (iron powder, thin steel sheet, steel wool, etc.) is supplied to the widthwise center of the molten steel reservoir 16, the exothermic reaction between the heat-generating material 35 and the molten steel 3 can prevent the molten steel temperature in the widthwise center of the molten steel reservoir 16 from becoming too high, making it possible to homogenize the temperature distribution in the width direction of the molten steel reservoir 16. This makes it possible to stably cast the thin-walled slab 1.

[0045] The above is a description of the dummy sheet for twin-roll continuous casting according to the present embodiment of the present invention. Although the manufacturing method of the thin-walled cast slab has been specifically described, the present invention is not limited thereto, and appropriate modifications can be made without departing from the technical concept of the invention. For example, in the present embodiment, as shown in FIG. 1, an example of a thin-walled cast strip manufacturing apparatus having pinch rolls is described, but the arrangement of these rolls is not limited, and the design may be changed as appropriate.

[0046] Further, in the present embodiment, as shown in FIG. 4, the reinforcing member 32 is described as being located above the molten steel surface in the molten steel reservoir 16, but this is not limited thereto, and the reinforcing member 32 may be located only below the molten steel surface in the molten steel reservoir 16, as shown in FIG. 5. EXAMPLES

[0047] The results of experiments carried out to confirm the effects of the present invention will be described below. A thin-walled cast slab made of carbon steel containing 0.05 mass% C, 0.6 mass% Si, 1.5 mass% Mn, and 0.03 mass% Al was produced using the twin-roll continuous casting apparatus shown in the above embodiment.

[0048] The common conditions for manufacturing thin-walled cast slabs are shown below. Cooling roll diameter: 500mm Casting width: 800mm Depth of molten steel in molten steel reservoir: 190mm Cast piece thickness: 2.0mm Casting speed: 50m / min Casting atmosphere: Ar gas

[0049] (Example 1 of the present invention) The temperature of the molten steel in the molten steel vessel (tundish) was set to 1580° C. The dummy sheet used had a sheet body and reinforcing members made of mild steel with a thickness of 0.3 mm and a width of 790 mm. The exothermic material was then pressed onto the widthwise end region of the dummy sheet on the inner surface side of the reinforcing member, which corresponds to the molten steel reservoir. Here, the widthwise end region refers to the range of 0 to 195 mm from the widthwise end of the dummy sheet (corresponding to ¼ of the roll width). The heat generating material was metal silicon with a purity of 95% or more, the shape of the heating element was granular with a particle size of 2 mm or less, and the total amount of the heating element (including the amount of the heating element on both sides) was 0.16 kg. The amount of the heating element was determined using formulas (1) to (3) so that the temperature rise of the molten steel at the width end was 20°C. As a result of casting under the above conditions, the occurrence of ingots in the early stages of casting was suppressed, and no hot bands were observed at all.

[0050] (Example 2 of the present invention) The temperature of the molten steel in the molten steel vessel (tundish) was set to 1560° C. The dummy sheet used had a sheet body and reinforcing members made of mild steel with a thickness of 0.5 mm and a width of 790 mm. Then, the heat generating material was pressed onto the widthwise end region of the dummy sheet on the inner surface side of the reinforcing member, which corresponds to the molten steel reservoir portion. Here, the widthwise end region is defined as a range of 0 to 150 mm from the widthwise end of the dummy sheet. Furthermore, before the start of casting, the preheated side gate was pressed against the chill roll, and at the same time, taking into consideration the molten steel temperature, granular metal silicon was dropped onto the reinforcing member of the dummy sheet, and the heat generating material to be placed was added. Here, the position where the heat generating material was dropped was within the range of 0 to 100 mm from the end of the roll width. The heating material was metal silicon with a purity of 95% or more, the heating element shape was granular (bonded portion) with a particle size of 2 mm or less and chunks (dropped portion) with a particle size of 5 mm or less, and the total amount of heating elements was 0.40 kg (bonded portion 0.16 kg, dropped portion 0.24 kg). The amount of heating elements was determined using formulas (1) to (3) so that the temperature rise of the molten steel at the width end was 50°C. As a result of casting under the above conditions, similar to Example 1, the occurrence of ingots in the early stages of casting was suppressed, and no hot bands occurred.

[0051] (Example 3 of the present invention) The temperature of the molten steel in the molten steel vessel (tundish) was set to 1590°C. The dummy sheet was made of mild steel, with a thickness of 0.5 mm and a width of 790 mm, and the heat generating material was attached to the widthwise end region of the dummy sheet on the inner surface of the reinforcing member, which corresponds to the molten steel reservoir. The widthwise end region is the range from 0 to 150 mm from the widthwise end of the dummy sheet, and the heat generating material was ferrosilicon with a Si content of 76 mass%, the shape of the heating element was granular with a particle size of 3 mm or less, and the total amount of the heating element (adding the amount of heating element on both sides) was 0.24 kg. The amount of heating element was determined using formulas (1) to (3) so that the temperature rise of the molten steel at the widthwise end was 14°C. Furthermore, in order to lower the temperature of the molten steel at the width center, taking into consideration the temperature of the molten steel, steel wool was dropped onto the reinforcing members of the dummy sheet as a cooling material before the start of casting. The position where the steel wool was dropped was 100 mm or less away from the center of the roll width, i.e., within the width of 200 mm at the center. The material of the steel wool was steel containing 0.05 mass% C and having the same composition as the thin-walled cast slab to be produced. The steel wool was collected from steel cutting chips, and the amount used was 0.16 kg. As a result of casting under the above conditions, the occurrence of ingots in the early stage of casting was suppressed and no hot bands were observed, as in invention examples 1 and 2. Furthermore, the central part of the width of the thin-walled cast piece was prevented from becoming too hot and becoming brittle, and a thin-walled cast piece could be stably obtained.

[0052] (Conventional Example 1) The temperature of the molten steel in the molten steel vessel (tundish) was set to 1580° C. The dummy sheet used had a sheet body and reinforcing members made of mild steel with a thickness of 0.3 mm and a width of 790 mm. As a result of casting without using heat generating materials, the metal formed on the side gates became caught in the slab in the early stages of casting, causing hot bands. In some cases, the slab broke after several castings.

[0053] From the above results, it has been confirmed that the present invention can provide a dummy sheet for twin-roll continuous casting that can sufficiently suppress the formation and growth of metal on the surface of the side dam at the start of casting, suppress breakage of thin-walled cast strips caused by hot bands, and enable a stable start of casting, as well as a method for manufacturing thin-walled cast strips using this dummy sheet for twin-roll continuous casting. [Explanation of symbols]

[0054] 1 Thin-walled cast pieces 3. Molten Steel 10 Twin roll continuous casting equipment 11 Cooling roll 15 Side Weir 16 Molten steel reservoir 30 Dummy sheet for twin roll continuous casting 31 Seat body 32 Reinforcement members 35 Heat generating materials

Claims

1. A twin-roll continuous casting dummy seat for use in a twin-roll continuous casting apparatus which supplies molten steel to a molten steel reservoir formed by a pair of rotating chill rolls and a pair of side gates, and produces a thin-walled cast strip by forming and growing a solidified shell on a peripheral surface of the chill rolls, a sheet body sandwiched between the pair of chill rolls; and a reinforcing member extending from one end of the sheet body in a longitudinal direction and inserted into the molten steel along the chill rolls, a heat generating material that, when added to the molten steel, reacts with heat to increase the temperature of the molten steel is disposed at both ends of the reinforcing member in the width direction, The heat generating material is a Si-containing material containing 76% by mass or more of Si.

2. 2. The dummy sheet for twin-roll continuous casting according to claim 1, characterized in that the boundary position on the widthwise central side of the area in which the heat generating material is arranged is within a range of 20 mm to 200 mm from the widthwise end of the reinforcing member.

3. 3. The dummy sheet for twin-roll continuous casting according to claim 1, wherein the reinforcing member is made of a high-melting point material having a melting point of 1510° C. or higher.

4. A method for producing a thin cast slab by supplying molten steel to a molten steel reservoir formed by a pair of rotating chill rolls and a pair of side gates, and forming and growing a solidified shell on a peripheral surface of the chill rolls, comprising the steps of:

4. A method for producing a thin-walled cast strip, comprising the steps of: supplying the heat generating material to the molten steel reservoir at the start of casting by using the dummy sheet for twin-roll continuous casting according to claim 1.

5. 5. The method for producing a thin-walled cast slab according to claim 4, wherein cold material is supplied to the widthwise center of the molten steel reservoir in accordance with a pouring condition at the start of casting.

Citation Information

Patent Citations

  • Starting method for direct rolling type continuous casting machine

    JP1982058957A

  • Continuous casting apparatus for sheet

    JP1987124051A

  • Dummy bar for continuously casting metal strip

    JP1988224847A

  • Twin roll type continuous casting method

    JP1995227649A

  • Dummy sheet for twin-roll type continuous casting and method for manufacturing thin cast piece

    JP2018114540A