Recycled slag and refining method using recycled slag

By controlling mineral phases and cooling rates, the recycled slag addresses the powdering issue of ladle slag, ensuring stable reuse as a refining agent in steelmaking, enhancing handling and reducing costs.

JP7572624B2Active Publication Date: 2024-10-24NIPPON STEEL CORPORATION
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2021012187
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-28
Publication Date
2024-10-24
Estimated Expiration
2041-01-28

AI Technical Summary

Technical Problem

Ladle slag from the steelmaking process, rich in CaO and Al2O3, is difficult to reuse due to its tendency to powder during cooling, leading to handling issues and environmental pollution, and existing methods to prevent powdering either increase costs or are not effective for ladle slag composition.

Method used

Recycled slag with controlled mineral phases and adjusted cooling rates, specifically CaO:20-60%, SiO2:2-20%, Al2O3:10% or more, basicity ≥3.0, and controlled γ-2CaO·SiO2 to CaO-Al2O3 mineral phase ratio <0.16, is used as a refining agent, suppressing powdering and maintaining shape stability.

Benefits of technology

The recycled slag exhibits excellent powder resistance and handling properties, enabling its reuse as a slag additive in steelmaking, reducing costs and environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572624000003
    Figure 0007572624000003
  • Figure 0007572624000001
    Figure 0007572624000001
  • Figure 0007572624000002
    Figure 0007572624000002
Patent Text Reader

Abstract

To provide recycled slag that has excellent handling properties and may be used in a steelmaking and refining process.SOLUTION: Recycled slag according to the present invention is slag discharged from a steelmaking and refining process, the slag consisting of CaO: 20-60%, SiO2: 2-20%, Al2O3: 10% or more, t.Fe: 0.1-1%, and MgO: 20% or less. The basicity (CaO / SiO2: mass fraction) of the slag is 3.0 or more, and the main constituent minerals of the slag are CaO-Al2O3 mineral phases, MgO, γ-2CaO-SiO2 and β-2CaO-SiO2. The CaO-Al2O3 mineral phases are Ca3Al2O6, Ca9(Al2O6)3, and Ca12Al14O32. A mass ratio of γ-2CaO-SiO2 (mass%) to the CaO-Al2O3 mineral phases (mass%) is less than 0.16.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to recycled slag produced from molten slag discharged in a steel refining process and a refining method using the recycled slag, and in particular to recycled slag having pulverization resistance and a refining method using the recycled slag. [Background technology]

[0002] Slag discharged from the steelmaking process is sometimes used for civil engineering and roadbed materials, etc., in order to reduce waste and to address the problem of depletion of natural resources. However, ladle slag discharged from the ladle refining process contains a lot of CaO and Al2O3. If ladle slag could be reused in the steelmaking process as a refining agent, it would be possible to reduce the purchase costs of expensive auxiliary materials, etc., which is favorable for the steel industry. The steelmaking process will be explained step by step below.

[0003] In steelworks, molten iron tapped from a blast furnace is generally subjected to molten iron pretreatment, including desulfurization, desiliconization, and dephosphorization. After molten iron pretreatment is completed, the process centered on decarburization is carried out in a converter. The process from tapping from the blast furnace to decarburization is called primary refining, and the molten steel that has been primarily refined is transferred to a ladle. The molten steel contained in the ladle is purified by ladle refining (secondary refining), and then it is continuously cast via a tundish to produce slabs.

[0004] Ladle refining, which refines molten steel in a ladle, can be performed in a variety of ways, including injecting a powder (refining agent) into the molten steel and stirring it to refine it, vacuum degassing, which degassses the steel in a vacuum tank, and the ladle furnace (LF) method, which forms slag on the surface of the molten steel in the ladle and stirs the molten steel while heating it with a slag arc.

[0005] In the ladle refining process using the LF method (hereinafter referred to as LF refining), slag with a high CaO / SiO2 mass ratio (hereinafter referred to as "basicity") is generally formed on the surface of molten steel, and this slag is used to perform slag refining of the molten steel. When the molten steel is transferred from the converter to the ladle, a small amount of slag is also carried over to the ladle along with the molten steel. In LF refining, a CaO source and an Al2O3 source are added to this small amount of slag (hereinafter, the CaO source and the Al2O3 source added in the ladle refining process are referred to as "slag additives") to adjust the slag composition and amount. The slag thus formed is heated by immersing an electrode from above and passing electricity through it, and gas is stirred in a reducing atmosphere, whereby the molten steel is heated by heat exchange between the slag and the molten steel, and the molten steel is desulfurized and deoxidized by the slag-metal reaction.

[0006] After the LF refining is completed, the molten steel in the ladle is transferred to a tundish through vacuum refining, but the slag on the surface of the molten steel remains in the ladle. The molten slag remaining in the ladle and the solidified slag are hereinafter referred to as "ladle slag". Ladle slag is mainly composed of oxides such as CaO, Al2O3, SiO2, and MgO. Ladle slag contains a large amount of CaO and Al2O3 due to the addition of the above-mentioned slag additives, for example, 20 to 60 mass% CaO and 10 to 45 mass% Al2O3. The basicity of ladle slag is, for example, 3 to 14. The basicity is adjusted to a value suitable for the type of steel to be cast by adjusting the amount of CaO added.

[0007] In LF refining, a certain volume of ladle slag is required because the slag thickness is sufficient to immerse the electrode. The amount of slag is about 15 to 20 kg / t-steel in LF refining with a processing capacity of 300 t. In order to make such a large amount of slag into a high basicity composition and to make it molten, a large amount of CaO source and Al2O3 source must be added, and the cost of slag production is very high. The inventors thought that if ladle slag with high CaO and Al2O3 concentrations could be reused and used as a substitute for the auxiliary materials newly added in the LF method, the cost could be significantly reduced, but in order to achieve this, the following problems must be solved.

[0008] The ladle slag remaining in the ladle is discharged into a slag transport vessel (slag pan or slag pot). The slag transport vessel stores ladle slag after multiple slag refining processes. When a certain amount of ladle slag has accumulated in the slag transport vessel, it is transported to the yard by the slag transport vessel and returned to the yard. The ladle slag solidifies by cooling through contact with the yard and by being left to cool.

[0009] During this cooling process, the solidified ladle slag is prone to pulverization. Not only is the pulverized slag difficult to handle, but it also becomes dust when recycled in the refining process, resulting in poor yield. It also scatters and causes environmental pollution. The pulverization of ladle slag is thought to be caused by 2CaO·SiO2 (hereinafter also referred to as C2S), which crystallizes when the molten ladle slag is cooled. The crystallized C2S crystals undergo a phase transition from the α' phase to the β phase and from the β phase to the γ phase during the cooling process, increasing in volume and expanding, which destroys the solidified structure of the ladle slag, making the solidified ladle slag prone to pulverization. If this pulverization occurs, it becomes difficult not only to recycle the slag into the steelmaking process, but also to use it for other purposes such as roadbed material. For this reason, several technologies have been disclosed as a method of suppressing this pulverization.

[0010] Patent Document 1 discloses a technology in which slag formed on the surface of molten steel in a ladle that contains molten steel and having a basicity of 2 or more is mixed with an additive containing B (B2O3) to prevent the slag from powdering and to recycle it as a civil engineering material. Patent Document 2 discloses a molten slag treatment facility having a cooling treatment device equipped with a rotatable cooling roll for cooling and solidifying molten slag supplied to the outer peripheral surface of the rotating cooling roll, a slag supplying device for supplying molten slag to the cooling treatment device, and a recovery and transporting device for recovering and transporting the slag peeled off from the cooling roll after being cooled and solidified in the cooling treatment device. Patent Document 3 discloses a technology for reducing the expansiveness of steelmaking slag by controlling the mineral phase, although this is not for the purpose of suppressing powdering of steelmaking slag. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] JP 2012-41229 A [Patent Document 2] JP 2012-1417 A [Patent Document 3] JP 2018-24897 A Summary of the Invention [Problem to be solved by the invention]

[0012] In the steelmaking refining process, quicklime and alumina (aluminum oxide) are purchased and used as slag additives to be added to molten steel, and as mentioned above, the LF process requires a large amount of them. Here, the ladle slag that remains in the ladle and is collected in the slag transport vessel contains quicklime and alumina added as slag additives during LF refining, so it contains a large amount of CaO and Al2O3. In addition, ladle slag contains a low amount of lower oxides such as FeO, MnO, P2O5, and SiO2, so molten steel is less likely to be oxidized, and it is a substance with high cleanliness for steel. Therefore, if ladle slag can be reintroduced into the ladle as a slag additive instead of quicklime and alumina to refine molten steel, the purchase cost of the slag additives can be reduced, and it is more cost-effective than recycling it as a civil engineering material such as a roadbed material.

[0013] In the technology described in Patent Document 1, a powdering prevention material containing B2O3 is added to the molten slag and stirred to prevent powdering of the ladle slag. Therefore, the B2O3 content in the solidified ladle slag is high. If ladle slag with a high B2O3 content is reused as a slag additive, the B2O3 is reduced to B by slag refining, and this B dissolves in the molten steel, resulting in a phenomenon in which the B concentration of the cast steel increases. Even a small amount of B has a significant effect on the properties of the steel, so that ladle slag with a high B2O3 content can be reused in the steelmaking process only for some steel types that can tolerate the effect.

[0014] In the technology described in Patent Document 2, the molten ladle slag is rapidly cooled to prevent the ladle slag from powdering. However, this requires large-scale equipment to rapidly cool the ladle slag, which requires huge capital investment.

[0015] On the other hand, the technology described in Patent Document 3 controls the mineral phase of steelmaking slag within a suitable range to reduce the hydration expansion of the slag. However, this technology is aimed at suppressing the hydration expansion of converter slag compositions, and the main constituent mineral phases of the ladle slag compositions used in the present invention are fundamentally different, so the technology cannot be applied to the present invention and its effectiveness in solving the problems is unclear.

[0016] The present invention has been made in consideration of the above circumstances, and has an object to provide recycled slag that is resistant to powdering and a refining method using recycled slag. [Means for solving the problem]

[0017] In order to solve the problems, the present invention provides the following technical solutions. (1) The recycled slag of the present invention is slag discharged from the steelmaking refining process, The composition of the slag is CaO: 20-60%, SiO2: 2-20%, Al2O3: 10% or more, t.Fe: 0.1-1%, MgO: 20% or less, The basicity of the slag (CaO / SiO2: mass ratio) is 3.0 or more, The main constituent minerals of the slag are CaO-Al2O3 mineral phase, MgO, γ-2CaO SiO2, and β-2CaO SiO2, The CaO-Al2O3 mineral phase consists of Ca3Al2O6, Ca9(Al2O6)3, and Ca 12 Al 14 O 32 and It is characterized by a mass ratio of γ-2CaO·SiO2 (mass%) to CaO-Al2O3 mineral phase (mass%) being less than 0.16. (2) The refining method using recycled slag of the present invention is characterized in that the recycled slag described in (1) is used as a refining agent. Effect of the Invention

[0018] The recycled slag of the present invention has a mass ratio of γ-2CaO·SiO2 to the CaO-Al2O3 mineral phase, which is its constituent mineral phase, that is equal to or less than a predetermined value, and has resistance to powdering and excellent shape stability. [Brief description of the drawings]

[0019] [Figure 1] This figure shows the relationship between the mass fraction M(-) of γ-2CaO SiO2 to the CaO-Al2O3 mineral phase and the solidification rate for solidified ladle slag. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The process by which the problem was solved is described below. In the experiments described below, the inventors investigated the relationship between the composition of ladle slag, the constituent mineral phase types and their amounts, and the solidification rate of slag. As a result, it was confirmed that the amount of γ-2CaO SiO2 and the amount of CaO-Al2O3 mineral phase that crystallize during the cooling process are dominant in the disintegration behavior of ladle slag, and that disintegration of ladle slag can be suppressed by controlling the ratio of these within an appropriate range.

[0021] Specifically, in slag with a composition range of CaO: 20-60%, SiO2: 2-20%, Al2O3: 10% or more, t.Fe: 0.1-1%, MgO: 20% or less, a basicity (CaO / SiO2: mass ratio) of 3.0 or more, and main constituent minerals being CaO-Al2O3 mineral phase, MgO, γ-2CaO·SiO2, and β-2CaO·SiO2, disintegration of ladle slag can be suppressed by the amount of CaO-Al2O3 mineral phase (A (mass %)) and the amount of γ-2CaO·SiO2 (γ (mass %)) satisfying the following formula (1). The basis for this will be shown in the examples described later. The CaO-Al2O3 mineral phase refers to Ca3Al2O6, Ca9(Al2O6)3, Ca 12Al 14 O 32 It is. M = γ / A < 0.16 (1)

[0022] Here, "composition range of CaO: 20-60%, SiO2: 2-20%, Al2O3: 10% or more, t.Fe: 0.1-1%, MgO: 20% or less" specifies the general composition range of ladle slag. "Basicity (CaO / SiO2: mass ratio) is 3.0 or more" specifies the general basicity of ladle slag. In the ladle refining process, in order to purify the molten steel, slag additives are added to adjust the slag basicity to 3 or more, and as a result, the basicity of the ladle slag remaining in the ladle is also 3 or more. "Major constituent minerals" means that the total of the constituent minerals is 60% by mass or more.

[0023] The recycled slag of the present invention is specified by the value of the parameter M (%) (hereinafter also referred to as the M value), which indicates the ratio of the amount of γ-2CaO·SiO2 (γ (mass%)) to the amount of CaO-Al2O3 mineral phase (A (mass%)), being less than 0.16, as shown in formula (1). It is not enough to simply have a small amount of γ-2CaO·SiO2, but the amount of CaO-Al2O3 mineral phase also has a relationship with the powdering phenomenon of ladle slag after solidification, and this is derived from the examples described below. It is believed that the CaO-Al2O3 mineral phase has the effect of suppressing the powdering phenomenon. In addition, in the composition of ladle slag, the higher the ratio of the amount of Al2O3 and the lower the ratio of the amount of SiO2, the lower the M value can be.

[0024] To obtain recycled slag that satisfies formula (1), the cooling rate at which ladle slag is solidified is adjusted. Here, the cooling rate of ladle slag refers to the average cooling rate at which ladle slag is cooled from 1400°C, where it is in a molten state, to 500°C. In the above-mentioned slag composition range, the content of CaO and Al2O3 is high, so the crystallization temperature of the primary crystals is generally lower than 1400°C. The lower limit of the cooling rate measurement, 500°C, is a temperature lower than the phase transition temperature (α' phase to γ ​​phase) of the crystallized 2CaO SiO2.

[0025] As described above, ladle slag is discharged from the slag transport vessel to the yard and allowed to cool. However, in ladle slag that has been allowed to cool and solidify in this way, it is difficult for the mineral phase satisfying formula (1) to be formed. It is effective to increase the cooling rate, which contributes greatly to reducing the formation of 2CaO·SiO2. A specific cooling rate of 4°C / min to 35°C / min is preferable. If the cooling rate is slower than 4°C / min, the amount of γ-2CaO·SiO2 increases (the ratio of γ phase to the total mass of the slag increases), and the powdering phenomenon cannot be suppressed. To achieve a cooling rate of 4°C / min to 35°C / min, for example, water can be poured over the ladle slag when it is discharged to the yard, or an iron plate is laid on the yard and the slag is discharged onto the iron plate to cool it.

[0026] The cooling rate from 1400°C to 500°C is determined by measuring the temperature of the ladle slag while it is discharged into the slag transport vessel and discharged into the dumping yard and allowed to cool, and by measuring the time it takes for the measured temperature to decrease from 1400°C to 500°C. Specifically, the temperature of the ladle slag in the slag transport vessel is measured, for example, by a radiation thermometer, and the temperature of the ladle slag discharged into the dumping yard is measured, for example, by a thermocouple. The cooling rate can be adjusted by measuring the cooling rate in advance in a prior experiment, etc., and by changing whether or not water is sprayed on the ladle slag, or by changing the amount of water sprayed on the ladle slag.

[0027] In addition, in the above-mentioned slag composition range, the higher the basicity, the better. The basicity (slag composition) of the ladle slag is adjusted by changing the amount of CaO added. CaO can be added not only in the ladle but also in the slag transport vessel, for example, at the latest just before the ladle slag transported to the processing equipment is cooled or before the ladle slag solidifies (before it drops below the crystallization temperature of the primary crystals), so that the composition of the ladle slag can be adjusted.

[0028] This recycled slag is easy to handle and contains a large amount of CaO and Al2O3, so it can be used as a slag additive in the steelmaking refining process, just like regular additives. EXAMPLES

[0029] As an example, the basis for determining the ladle slag treatment conditions is shown. In this example, a method was adopted in which the slag composition and temperature were controlled using a Tammann furnace (electric furnace) to melt and cool simulated ladle slag, reproducing the ladle slag treatment method used in an actual machine.

[0030] (Sample preparation) For the test, simulated ladle slag that imitates the ladle slag of an actual machine was used as the sample. The simulated ladle slag was prepared by mixing powder reagents of the main components (CaO, Al2O3, SiO2, MgO, T.Fe, and MnO) in the proportions (mass%) shown in Table 2. Table 2 shows the constituent mineral proportions (mass%) and M values ​​after solidification, as well as the test results (solidification rate) and their evaluation.

[0031] (Experimental Method) A Tammann furnace was used for the experiment, and the temperature inside the furnace was controlled. First, a sample (simulated ladle slag) mixed in the ratio shown in Table 2 was placed in a crucible and placed in a Tammann furnace. The temperature inside the furnace was raised to 1550°C. The simulated ladle slag was melted by maintaining it at 1550°C for 60 minutes. After melting, the temperature inside the furnace was once lowered to 1400°C, and then the crucible was removed from the Tammann furnace and cooled to 500°C to solidify. At that time, the temperature of the sample was measured by a thermocouple. Among the 13 experiments, the cooling rate from 1400°C to 500°C was set to 4 to 35°C / min in Experiments 1 to 12, and less than 4°C / min in Experiment 13.

[0032] (Measurement of solidification rate) The solidified sample in the crucible was sieved through a sieve with 0.5 mm mesh. The solidified sample was separated through the sieve, and the masses of the oversieved and undersieved parts were weighed to measure the solidification rate. The solidification rate was calculated using the following formula (2). The powder amount is the mass of the undersieved part when sieved through the sieve. Solidification rate = (Input amount - Powdering amount) / (Input amount) × 100 (%) ···(2) Charge amount: Total mass of simulated ladle slag Powder amount: Mass under the sieve (0.5 mm sieve)

[0033] A horizontal X-ray diffractometer (SmartLab) manufactured by Rigaku Corporation was used to investigate the amount of crystalline phase in the recycled slag. The measurement conditions were as follows: target: Cu, D / teX250 was used for monochromatization, target output: 45kV-200mA, measurement angle (2θ): 5-100°, measurement width: 0.02°. The RIR (Reference Intensity Ratio) method was used to quantify the crystalline phase. The RIR method is a method to simply calculate a quantitative value using the RIR value listed in the database from the integrated intensity at the strongest line of the detected component.

[0034] The crystal phase names, chemical formulas, and RIR values ​​used for the crystal phase identification are shown in Table 1. The integrated powder X-ray diffraction software PDXL was used to identify the crystal phases, and they were classified as shown in Table 1. Specifically, the 2CaO SiO2 phase (C2S phase) was classified as γ-C2S as γ and β-C2S as β. Ca3(Al2O6), Ca9(Al2O6), and Ca 12 Al 14 O 32 is classified as CaO-Al2O3 mineral phase (A), MgO is classified as MgO mineral phase (G), and Ca 20 Al 26 Mg3Si3O 68 was classified as other mineral phases (O). The mineral phase column in Table 2 shows the proportions of A, G, O, γ, and β in mass%.

[0035] [Table 1]

[0036] [Table 2]

[0037] (Experimental Results) The experimental results are shown in the "Solidification rate" and "Evaluation" columns in Table 2. A solidification rate of over 90% was evaluated as ◯. Figure 1 shows the experimental results of Experiments 1 to 13, and is a diagram illustrating the relationship between the parameter M and the solidification rate corresponding to Experiments 1 to 13. As shown in Figure 1, the solidification rate increases sharply when the parameter M is 0.16 or less (Experiments 1 to 9: ◆ in the figure).

[0038] In summary, recycled slag, which is made by solidifying ladle slag of a specified composition so that it satisfies M=γ / A<0.16 (A: amount of CaO-Al2O3 mineral phase (mass%), γ: amount of γ-2CaO·SiO2 (mass%)), is resistant to pulverization and has excellent stability. This recycled slag is easy to handle and contains a large amount of CaO and Al2O3, so it can be used as a slag additive in the steelmaking refining process.

[0039] It should be noted that the embodiments disclosed herein are illustrative in all respects and should not be considered as limiting. In particular, in the embodiments disclosed herein, matters not expressly disclosed, such as operating conditions, operating conditions, various parameters, dimensions, weights, volumes of components, etc., do not deviate from the scope of ordinary practice by a person skilled in the art, and values ​​that can be easily assumed by a person skilled in the art are adopted.

[0040] In this embodiment, ladle slag, which is a steel by-product generated during refining in a ladle refining furnace, has been used as an example. However, the present invention can also be applied to steelmaking slag generated in various refining processes in steelworks, such as electric furnace oxidation slag, dephosphorization slag, decarburization slag, desulfurization slag, and desiliconization slag.

Claims

1. In the slag discharged from the steel refining process, The composition of the slag is CaO: 20-60%, SiO 2 : 2-20%, Al 2 O 3 :10 % or more, t.Fe: 0.1 to 1%, MgO: 5 to 20%, The basicity of the slag (CaO / SiO 2 : mass ratio) is 3.0 or more, The main constituent minerals of the slag are CaO-Al 2 O 3 Mineral phase, MgO, γ-2CaO・Si O 2 , β-2CaO・SiO 2 and CaO-Al 2 O 3 The mineral phase is Ca 3 A 2 O 6 , Ca 9 (Al 2 O 6 ) 3 , and Ca 12 A 14 O 32 and CaO-Al 2 O 3 γ-2CaO.SiO relative to mineral phase (mass%) 2 Quality (% by mass) The recycled slag is characterized in that the amount ratio is less than 0.

16.

2. A refining method, comprising using the recycled slag according to claim 1 as a refining agent.

Citation Information

Patent Citations

  • Method for controlling powdering and recycling of refining slags in steelmaking

    CN109929965A

  • JP1975080203A

  • Method for modifying smelting reduction slag

    JP1991023243A

  • Device for producing water-granulated slag

    JP1996231253A

  • Treating method of slag in reducing period

    JP2001152233A