Method for producing polyamide resin composition, pellets and molded article
A polyamide resin composition with semi-aromatic polyamide, modified ethylene/α-olefin copolymer, and lubricant addresses the issue of discolored lumps in semi-aromatic polyamide extrusion, enhancing impact resistance and product appearance by improving fluidity and reducing adhesion.
Patent Information
- Application Number
- JP2020060616
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-30
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2040-03-30
AI Technical Summary
Semi-aromatic polyamide resins used in resin moldings for heat resistance often suffer from poor impact resistance and form discolored lumps called die drool during extrusion, which can impair the appearance of molded products.
A polyamide resin composition comprising 60 to 85 parts by mass of a semi-aromatic polyamide with a melting point of 280°C or higher, 10 to 35 parts by mass of a modified ethylene/α-olefin copolymer with 0.01 to 5% grafting, and 0.1 to 1 part by mass of a lubricant, which enhances fluidity and reduces adhesion to metal members to prevent the formation of discolored resin lumps.
The composition effectively suppresses the formation of discolored resin lumps during pellet production, ensuring improved impact resistance and maintaining the appearance of molded products.
Smart Images

Figure 0007572791000001 
Figure 0007572791000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a polyamide resin composition, pellets, and a molded article. [Background technology]
[0002] Polyamide resins have been widely used as materials for various parts in automobiles, electrical and electronic equipment, industrial applications, etc. because of their excellent moldability, mechanical properties, and chemical resistance.
[0003] Among these, semi-aromatic polyamides with a melting point of 280° C. or higher are used as materials for resin moldings that require heat resistance.
[0004] On the other hand, such semi-aromatic polyamides tend to have poor impact resistance. Therefore, in order to improve the impact resistance of semi-aromatic polyamide resins, they are generally alloyed with polyolefins. For example, a resin composition containing a semi-aromatic polyamide containing a component unit derived from terephthalic acid and a component unit derived from an aliphatic diamine, and an acid-modified ethylene-α-olefin copolymer (as a polyolefin) is known (for example, Patent Document 1). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 4-270761 Summary of the Invention [Problem to be solved by the invention]
[0006] Such a resin composition is usually melt-kneaded in an extruder or the like, extruded into a strand shape from a die, and cut to a predetermined size while cooling to form pellets. The pellets are usually used as a raw material for producing a molded article.
[0007] However, when a resin composition containing a semi-aromatic polyamide is melt-kneaded in an extruder and extruded through a die, discolored resin lumps called die rools may be generated at the outlet of the die holes. The lumps tend to be mixed into the strands and may be mixed into the resulting pellets. If such lumps are mixed in, the appearance of the resulting molded product is likely to be impaired.
[0008] The present invention has been made in consideration of the above circumstances, and has an object to provide a method for producing a polyamide resin composition, pellets, and molded articles, which can suppress the generation of discolored resin lumps known as "eye gunk," for example, when a polyamide resin composition is melt-kneaded to produce pellets. [Means for solving the problem]
[0009] The present invention relates to the following polyamide resin composition, pellets, and methods for producing a molded article.
[0010] The polyamide resin composition of the present invention contains 60 to 85 parts by mass of a semi-aromatic polyamide (A) which contains component units (a1) derived from a dicarboxylic acid including component units derived from terephthalic acid and component units (a2) derived from a diamine including at least one of component units derived from an aliphatic diamine and a component unit derived from an alicyclic diamine, and has a melting point of 280°C or higher, 10 to 35 parts by mass of a modified ethylene-α-olefin copolymer (B) having a graft amount of 0.01 to 5 mass%, which is obtained by modifying an ethylene-α-olefin copolymer with an unsaturated carboxylic acid or a derivative thereof, and 0.1 to 1 part by mass of a lubricant (C) (the total of (A), (B) and (C) is 100 parts by mass).
[0011] The pellets of the present invention contain the polyamide resin composition of the present invention.
[0012] The method for producing a molded article of the present invention includes a step of melt molding the pellets of the present invention to obtain a molded article. Effect of the Invention
[0013] According to the present invention, it is possible to provide a polyamide resin composition that can suppress the formation of discolored resin lumps known as "eye gunk," for example, when the polyamide resin composition is melt-kneaded to produce pellets, and a method for producing a molded article using the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The present inventors have found that by adding a predetermined amount of lubricant (C), it is possible to suppress the generation of die discharge near the die outlet when preparing pellets of a resin composition.
[0015] The reason for this is not clear, but is presumed to be as follows. A polyamide resin composition containing a predetermined amount of lubricant (C) not only has high fluidity when molten, but also has low adhesion to metal members, and therefore has low mold release resistance (from metal members). As a result, it is believed that the molten resin is less likely to remain, adhere and grow near the outlet of the die, for example, and therefore the growth of resin at the outlet of the die can be suppressed. The configuration of the present invention will be described in detail below.
[0016] 1. Polyamide resin composition The polyamide resin composition of the present invention contains a semi-aromatic polyamide (A), a modified ethylene-α-olefin copolymer (B), and a lubricant (C).
[0017] 1-1. Semi-aromatic polyamide (A) The semi-aromatic polyamide (A) contains a component unit (a1) derived from a dicarboxylic acid and a component unit (a2) derived from a diamine.
[0018] [Component unit (a1) derived from dicarboxylic acid] The component unit (a1) derived from a dicarboxylic acid is not particularly limited, but from the viewpoint of improving the mechanical strength and heat resistance of the resulting molded article, it is preferable for it to contain a component unit derived from terephthalic acid.
[0019] The content of the component unit derived from terephthalic acid is not particularly limited, but is preferably 20 to 100 mol% based on the total number of moles of the component unit (a1) derived from dicarboxylic acid. If the content of the component unit is 20 mol% or more, the crystallinity and mechanical strength of the polyamide resin are easily improved. From the same viewpoint, the content of the component unit is more preferably 50 to 100 mol%.
[0020] The component unit (a1) derived from a dicarboxylic acid may further contain a component unit derived from a dicarboxylic acid other than the above, within a range that does not impair the effects of the present invention. Examples of the other dicarboxylic acid include aromatic dicarboxylic acids other than terephthalic acid and aliphatic dicarboxylic acids having 4 to 20 carbon atoms.
[0021] Examples of aromatic dicarboxylic acids other than terephthalic acid include 2-methylterephthalic acid, isophthalic acid, and naphthalenedicarboxylic acid. The aliphatic dicarboxylic acid having 4 to 20 carbon atoms is preferably an aliphatic dicarboxylic acid having 6 to 12 carbon atoms, and examples thereof include succinic acid, adipic acid, azelaic acid, and sebacic acid, and preferably adipic acid and sebacic acid.
[0022] The total content of component units derived from other dicarboxylic acids is preferably from 0 to 80 mol %, and more preferably from 0 to 50 mol %.
[0023] [Diamine-derived component unit (a2)] The diamine-derived component unit (a2) is not particularly limited, but preferably contains at least one of an aliphatic diamine-derived component unit and an alicyclic diamine-derived component unit.
[0024] The aliphatic diamine may be a straight-chain aliphatic diamine or a branched aliphatic diamine.
[0025] The linear aliphatic diamine is a linear aliphatic diamine having 4 to 18 carbon atoms, preferably 4 to 8 carbon atoms. Examples of linear aliphatic diamines include 1,4-butanediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, etc. Among them, 1,6-hexanediamine and 1,10-decanediamine are preferred, and 1,6-hexanediamine is more preferred. These aliphatic diamines may be used alone or in combination of two or more kinds.
[0026] The branched aliphatic diamine is a branched aliphatic diamine having 4 to 18 carbon atoms, preferably 4 to 8 carbon atoms. Examples of the branched aliphatic diamine include 2-methyl-1,5-pentanediamine, 2-methyl-1,8-octanediamine, 2-methyl-1,6-hexanediamine, 2-methyl-1,7-heptanediamine, 2-methyl-1,9-nonanediamine, and 2-methyl-1,10-decanediamine. Among them, a branched aliphatic diamine having 4 to 10 carbon atoms in the main chain and a side chain alkyl group having 1 to 2 carbon atoms is preferred, 2-methyl-1,8-octanediamine and 2-methyl-1,5-pentanediamine are more preferred, and 2-methyl-1,5-pentanediamine is even more preferred. These aliphatic diamines may be one type or two or more types. For example, the diamine-derived component units (a2) preferably include at least one of component units derived from 2-methyl-1,8-octanediamine and component units derived from 2-methyl-1,5-pentanediamine.
[0027] The alicyclic diamine is a diamine having an alicyclic hydrocarbon ring having 3 to 25 carbon atoms, preferably 6 to 18 carbon atoms. Examples of the alicyclic diamine include 1,3-bis(aminomethyl)cyclohexane, bis(4-aminocyclohexyl)methane, 1,3-bis(aminocyclohexyl)methane, 1,3-bis(aminomethyl)cyclohexane, and 4,4'-diamino-3,3'-dimethyldicyclohexylmethane, and include bis(4-aminocyclohexyl)methane, 1,3-bis(aminocyclohexyl)methane, and 1,3-bis(aminomethyl)cyclohexane. These alicyclic diamines may be one type or two or more types.
[0028] Among these, the diamine-derived component unit (a2) preferably contains an aliphatic diamine-derived component unit from the viewpoint of ensuring flowability during molding, etc. The aliphatic diamine-derived component unit preferably contains a linear aliphatic diamine-derived component unit, and may further contain a branched aliphatic diamine-derived component unit.
[0029] The total content of the component units derived from an aliphatic diamine and the component units derived from an alicyclic diamine (preferably the content of the component units derived from an aliphatic diamine) is preferably 50 to 100 mol % relative to the total number of moles of the component units (a2) derived from diamine, and may be 100 mol %.
[0030] Furthermore, the content of the component units derived from branched aliphatic diamines in the component units derived from aliphatic diamines is preferably 0 to 50 mol %, and more preferably 7 to 50 mol %, based on the total content of the component units derived from linear aliphatic diamines and the component units derived from branched aliphatic diamines.
[0031] [Physical Properties] The melting point (Tm) of the semi-aromatic polyamide (A) is preferably 280° C. or higher. When the melting point (Tm) of the semi-aromatic polyamide (A) is 280° C. or higher, the mechanical strength and heat resistance of the obtained molded article are unlikely to be impaired. From the same viewpoint, the melting point (Tm) of the semi-aromatic polyamide (A) is preferably 290 to 340° C.
[0032] The glass transition temperature (Tg) of the semi-aromatic polyamide (A) is preferably 70° C. or higher, and more preferably 80 to 150° C. When the glass transition temperature (Tg) of the semi-aromatic polyamide (A) is within the above range, heat resistance is less likely to be impaired.
[0033] The melting point (Tm) and the glass transition temperature (Tg) can be measured using a differential scanning calorimeter (DSC220C, manufactured by Seiko Instruments Inc.). Specifically, about 5 mg of semi-aromatic polyamide (A) is sealed in a measuring aluminum pan and heated from room temperature to 350°C at 10°C / min. In order to completely melt the resin, it is held at 350°C for 1 minute and then cooled to 30°C at 10°C / min. After leaving it at 30°C for 1 minute, it is heated a second time to 360°C at 10°C / min. The temperature (°C) of the endothermic peak in this second heating is taken as the melting point (Tm) of the semi-aromatic polyamide (A), and the transition point corresponding to the glass transition is taken as the glass transition temperature (Tg).
[0034] The melting point (Tm) and glass transition temperature (Tg) of the semi-aromatic polyamide (A) can be adjusted by the composition of the dicarboxylic acid and diamine.
[0035] The semi-aromatic polyamide (A) preferably has an intrinsic viscosity [η] of 0.5 to 3.0 dl / g as measured in 96.5% sulfuric acid at a temperature of 25°C. When the semi-aromatic polyamide (A) has an intrinsic viscosity [η] of 0.5 dl / g or more, the mechanical strength (toughness, etc.) of the resulting molded article is easily increased, and when the intrinsic viscosity [η] is 3.0 dl / g or less, the fluidity during molding is not easily impaired. From the same viewpoint, the semi-aromatic polyamide (A) more preferably has an intrinsic viscosity [η] of 0.6 to 2.5 dl / g. The intrinsic viscosity [η] can be adjusted by the amount of terminal blocking of the semi-aromatic polyamide (A), etc.
[0036] The intrinsic viscosity can be measured in accordance with JIS K6810-1977. Specifically, 0.5 g of polyamide resin is dissolved in 50 ml of 96.5% sulfuric acid solution to prepare a sample solution. The number of seconds it takes for this sample solution to flow down is measured using an Ubbelohde viscometer under conditions of 25±0.05°C, and the obtained value can be applied to the following formula to calculate the viscosity. [η]=ηSP / [C(1+0.205ηSP)]
[0037] In the above formula, each algebra or variable represents the following: [η]: Intrinsic viscosity (dl / g) ηSP: Specific viscosity C: Sample concentration (g / dl)
[0038] ηSP is calculated by the following formula: ηSP=(t-t0) / t0 t: Time required for sample solution to flow (seconds) t0: Number of seconds that blank sulfuric acid flows (seconds)
[0039] From the viewpoint of increasing the thermal stability during molding, the terminal groups of the molecule of the semi-aromatic polyamide (A) may be blocked with a terminal blocking agent.
[0040] The end-capping agent is preferably a monoamine when the molecular terminal is a carboxyl group, and is preferably a monocarboxylic acid when the molecular terminal is an amino group.
[0041] Examples of monoamines include aliphatic monoamines such as methylamine, ethylamine, propylamine, and butylamine; alicyclic monoamines such as cyclohexylamine and dicyclohexylamine; Examples of monocarboxylic acids include aliphatic monocarboxylic acids having 2 to 30 carbon atoms, such as acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, tridecylic acid, myristic acid, palmitic acid, stearic acid, oleic acid, and linoleic acid; aromatic monocarboxylic acids, such as benzoic acid, toluic acid, naphthalene carboxylic acid, methylnaphthalene carboxylic acid, and phenyl acetic acid; and alicyclic monocarboxylic acids, such as cyclohexane carboxylic acid. The aromatic monocarboxylic acid and the alicyclic monocarboxylic acid may have a substituent at the cyclic structure portion.
[0042] The semi-aromatic polyamide (A) may be one type or a combination of two or more types. For example, the polyamide resin composition may include a semi-aromatic polyamide (A1) containing, as the dicarboxylic acid-derived component units (a1), a component unit derived from terephthalic acid and a component unit derived from an aliphatic dicarboxylic acid, and a semi-aromatic polyamide (A2) containing, as the diamine-derived component units (a2), a component unit derived from a linear aliphatic diamine and a component unit derived from a branched aliphatic diamine.
[0043] The content of the semi-aromatic polyamide (A) is preferably 60 to 89 parts by mass relative to 100 parts by mass of the total of the semi-aromatic polyamide (A), the modified ethylene-α-olefin copolymer (B) and the lubricant (C). When the content of the semi-aromatic polyamide (A) is 60 parts by mass or more, the properties of the semi-aromatic polyamide (A) are easily obtained, and when the content is 89 parts by mass or less, the content of the modified ethylene-α-olefin copolymer (B) can be secured, so that impact resistance and the like can be easily improved. From the same viewpoint, the content of the semi-aromatic polyamide (A) is more preferably 65 to 85 parts by mass relative to 100 parts by mass of the total of the modified ethylene-α-olefin copolymer (B) and the lubricant (C).
[0044] 1-2. Modified ethylene-α-olefin copolymer (B) The modified ethylene-α-olefin copolymer (B) is an ethylene-α-olefin copolymer graft-modified with an unsaturated carboxylic acid or its derivative.
[0045] (Ethylene-α-olefin copolymer) The raw material, ethylene-α-olefin copolymer, contains component units derived from ethylene and component units derived from α-olefin.
[0046] The content of component units derived from ethylene is 70 mol % or more, and preferably 80 to 98 mol %, based on all component units constituting the ethylene-α-olefin copolymer.
[0047] The α-olefin is preferably an α-olefin having 3 to 20 carbon atoms. Examples of the α-olefin include propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, and 1-decene. Among them, 1-butene, 1-hexene, 4-methyl-1-pentene, and 1-octene are preferably used. These α-olefins may be used alone or in combination of two or more.
[0048] The content of component units derived from α-olefin is 30 mol % or less, and preferably 7 to 20 mol %, based on the total component units constituting the ethylene-α-olefin copolymer.
[0049] The density of the ethylene-α-olefin copolymer is not particularly limited, but is preferably 0.85 to 0.95 g / cm. 3 and preferably 0.89 to 0.95 g / cm 3 More preferably, it is 0.9 to 0.94 g / cm 3 It is even more preferred that the density is 23° C. in accordance with ASTM D792.
[0050] The melting point (Tm) of the ethylene-α-olefin copolymer is not particularly limited, but is preferably, for example, 90 to 127° C., and more preferably 95 to 125° C. The melting point can be measured as the temperature at the maximum peak position of the endothermic curve when the temperature is raised at 10° C. / min using a differential scanning calorimeter (DSC). Note that it is also possible to use an amorphous ethylene-α-olefin copolymer that does not exhibit a melting point.
[0051] The ethylene-α-olefin copolymer preferably has a crystallinity of 20 to 60%, more preferably 25 to 55%, as measured by X-ray diffraction. Alternatively, amorphous ethylene-α-olefin copolymers may also be used.
[0052] The melt flow rate (MFR: ASTM D 1238, 190°C, 2.16 kg load) of the ethylene-α-olefin copolymer is not particularly limited, but is preferably 0.01 to 100 g / 10 min, more preferably 0.1 to 50 g / 10 min, and even more preferably 0.2 to 20 g / 10 min.
[0053] (Unsaturated Carboxylic Acid) Examples of unsaturated carboxylic acids include acrylic acid, methacrylic acid, maleic acid, fumaric acid, and itaconic acid. Examples of derivatives of unsaturated carboxylic acids include acid anhydrides such as maleic anhydride, itaconic anhydride, and citraconic anhydride; esters such as methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, glycidyl acrylate, monoethyl maleate, diethyl maleate, monomethyl fumarate, dimethyl fumarate, monomethyl itaconic acid, and diethyl itaconic acid; Amides such as acrylamide, methacrylamide, maleic acid monoamide, maleic acid diamide, maleic acid-N-monoethylamide, maleic acid-N,N-diethylamide, maleic acid-N-monobutylamide, maleic acid-N,N-dibutylamide, fumaric acid monoamide, fumaric acid diamide, fumaric acid-N-monobutylamide, fumaric acid-N,N-dibutylamide; imides such as maleimide, N-butylmaleimide, N-phenylmaleimide; metal salts such as sodium acrylate, sodium methacrylate, potassium acrylate, potassium methacrylate, etc. Among them, it is preferable to use maleic anhydride.
[0054] Graft modification of ethylene-α-olefin copolymers using unsaturated carboxylic acids or their derivatives (graft monomers) can be carried out by known methods. For example, there is a melt modification method in which an ethylene-α-olefin copolymer is melted using an extruder and a graft monomer is added to perform graft copolymerization, and a solution modification method in which an ethylene-α-olefin copolymer is dissolved in a solvent and a graft monomer is added to perform graft copolymerization. In either case, it is preferable to start the reaction in the presence of a radical initiator in order to efficiently graft copolymerize the graft monomer.
[0055] The radical initiator can be an organic peroxide such as a dialkyl peroxide such as dicumyl peroxide, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di(peroxybenzoate)hexyne-3, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 1,4-bis(tert-butylperoxyisopropyl)benzene, and the like.
[0056] (Modified ethylene-α-olefin copolymer (B)) The graft sites (sites derived from unsaturated carboxylic acids or their derivatives) of the modified ethylene-α-olefin copolymer (B) easily interact with the molecular end groups (e.g., amino groups) of the semi-aromatic polyamide (A), so the two have good compatibility.
[0057] The content of the component unit derived from an unsaturated carboxylic acid or its derivative in the modified ethylene-α-olefin copolymer (B) (graft amount of the unsaturated carboxylic acid or its derivative) is preferably 0.01 to 5 mass% based on the modified ethylene-α-olefin copolymer (B). When the graft amount is 0.01 mass% or more, sufficient interaction with the semi-aromatic polyamide (A) can be achieved, making it easy to obtain good compatibility, while when it is 5 mass% or less, an increase in melt viscosity due to excessive interaction can be suppressed. From the same viewpoint, the graft amount is more preferably 0.1 to 3 mass% based on the modified ethylene-α-olefin copolymer (B).
[0058] The graft amount of the unsaturated carboxylic acid or its derivative can be calculated from the charge ratio in the preparation of the modified ethylene-α-olefin copolymer (B1-1), or can be measured by a combination of the NMR method and the IR method.
[0059] Specifically, the graft amount of the unsaturated carboxylic acid or its derivative can be measured by the following procedure. 1) Prepare several samples of modified ethylene-α-olefin copolymer (B) with different graft amounts, and measure their graft amounts by NMR. In addition, measure these samples by infrared spectroscopy (IR). Then, create a calibration curve of the graft amount obtained by NMR measurement and the intensity ratio of a specific peak in the infrared spectroscopy (IR) spectrum. 2) Next, the modified ethylene-α-olefin copolymer (B) to be measured is subjected to IR measurement, and the intensity ratio of specific peaks in the infrared spectroscopy (IR) spectrum is measured. 3) The measurement results obtained in 2) above are compared with the calibration curve obtained in 1) above to determine the graft amount of the modified ethylene-α-olefin copolymer (B) to be measured. In this method, it is necessary to prepare a calibration curve according to the type of resin and functional group.
[0060] The measurement conditions for the NMR method in 1) above may be as follows. 1For H-NMR measurements, a nuclear magnetic resonance apparatus of the ECX400 model manufactured by JEOL Ltd. was used, the solvent was deuterated orthodichlorobenzene, the sample concentration was 20 mg / 0.6 mL, the measurement temperature was 120 °C, and the observation nucleus was 1 The conditions were: H (400 MHz), sequence was single pulse, pulse width was 5.12 μsec (45° pulse), repetition time was 7.0 sec, and the number of integrations was 500 or more. The reference chemical shift was set to 0 ppm for hydrogen in tetramethylsilane, but similar results can also be obtained by setting the peak derived from residual hydrogen in deuterated orthodichlorobenzene at 7.10 ppm as the reference value for the chemical shift. 1 Peaks such as H can be assigned by conventional methods.
[0061] 13 In the case of C-NMR measurement, the measurement device was a JEOL ECP500 type nuclear magnetic resonance device, the solvent was a mixed solvent of ortho-dichlorobenzene / heavy benzene (80 / 20% by volume), the measurement temperature was 120°C, and the observation nucleus was 13 The conditions are: C (125 MHz), single pulse proton decoupling, 45° pulse, repetition time 5.5 seconds, number of integrations 10,000 or more, and chemical shift reference value 27.50 ppm. Assignment of various signals is performed based on the usual method, and quantification can be performed based on the integration value of signal intensity.
[0062] The density, melting point (Tm) and MFR range of the modified ethylene-α-olefin copolymer (B) may be similar to the density, melting point (Tm) and MFR range of the raw material ethylene-α-olefin copolymer, respectively.
[0063] The content of the modified ethylene-α-olefin copolymer (B) is preferably 10 to 35 parts by mass per 100 parts by mass of the semi-aromatic polyamide (A), the modified ethylene-α-olefin copolymer (B) and the lubricant (C). When the content of the modified ethylene-α-olefin copolymer (B) is 10 parts by mass or more, the impact resistance of the obtained molded article is easily increased, and when it is 35 parts by mass or less, the mechanical strength of the obtained molded article is not easily impaired. From the same viewpoint, the content of the modified ethylene-α-olefin copolymer (B) is more preferably 10 to 25 parts by mass per 100 parts by mass of the semi-aromatic polyamide (A), the modified ethylene-α-olefin copolymer (B) and the lubricant (C).
[0064] The content of the modified ethylene-α-olefin copolymer (B) is preferably 10 to 35 parts by mass, more preferably 10 to 25 parts by mass, per 100 parts by mass of the total of the semi-aromatic polyamide (A) and the modified ethylene-α-olefin copolymer (B). Thus, when the content of the modified ethylene-α-olefin copolymer (B) is high, the impact resistance of the molded body can be increased when melted, but the fluidity is easily impaired and the die buildup is easily generated. Even in such cases, the inclusion of the lubricant (C) of the present invention can provide good fluidity and suppress the die buildup.
[0065] 1-3.Lubricant (C) The lubricant (C) can increase the fluidity of the polyamide resin composition during melt-kneading and reduce the mold release resistance, thereby suppressing the generation of die buildup.
[0066] The lubricant (C) may be a higher fatty acid or its metal salt, ester or amide.
[0067] The higher fatty acid may be a fatty acid having 8 or more carbon atoms, preferably 8 to 40. The fatty acid is preferably a monocarboxylic acid. Examples of the higher fatty acid include saturated fatty acids such as octanoic acid, lauric acid, myristic acid, palmitic acid, stearic acid, 12-hydroxystearic acid, behenic acid, montanic acid, and sebacic acid, and unsaturated fatty acids such as erucic acid, oleic acid, and ricinoleic acid, and are preferably montanic acid, 12-hydroxystearic acid, and behenic acid.
[0068] The higher fatty acid metal salt is a metal salt of the above higher fatty acid. Examples of metal elements forming the metal salt include Group 1 elements (alkali metals) such as sodium and potassium, Group 2 elements (alkaline earth metals) such as calcium, magnesium and barium, and Group 3 elements such as zinc and aluminum, and preferably calcium salt, magnesium salt, zinc salt and aluminum salt. Examples of such metal salts of higher fatty acids include calcium 12-hydroxystearate, zinc 12-hydroxystearate, magnesium 12-hydroxystearate, aluminum 12-hydroxystearate, calcium behenate, zinc behenate, magnesium behenate, calcium montanate, zinc montanate, magnesium montanate, and aluminum montanate, and metal montanate and 12-hydroxystearate may be preferred.
[0069] The higher fatty acid ester is an ester of the above higher fatty acid and an alcohol (preferably an aliphatic alcohol having 8 to 40 carbon atoms). Examples of the aliphatic alcohol include stearyl alcohol, behenyl alcohol, and lauryl alcohol. Examples of the higher fatty acid ester include stearyl stearate and behenyl behenate.
[0070] The higher fatty acid amide is an amidation product of the above higher fatty acid. Examples of the higher fatty acid amide include stearic acid amide, oleic acid amide, erucic acid amide, ethylene bisstearylamide, ethylene bisoleylamide, N-stearylstearylamide, and N-stearylerucamide.
[0071] Among them, from the viewpoint of making it easier to suppress the formation of eye boogers, higher fatty acid metal salts and higher fatty acid esters are preferred, from the viewpoint of further reducing the mold release resistance, metal montanic acid salts or montanic acid esters are more preferred, and from the viewpoint of further increasing the fluidity, metal stearic acid salts such as 12-hydroxystearic acid or stearic acid esters are more preferred. The lubricant (C) may be one type or a combination of two or more types.
[0072] The content of the lubricant (C) is preferably 0.01 to 1 part by mass relative to 100 parts by mass of the total of the semi-aromatic polyamide (A), the modified ethylene-α-olefin copolymer (B) and the lubricant (C). When the content of the lubricant (C) is 0.01 part by mass or more, the fluidity during melt kneading is easily increased and the mold release resistance is easily reduced. As a result, the generation of die boogers can be sufficiently suppressed, for example, during pellet production. When the content of the lubricant (C) is 1 part by mass or less, the mechanical strength of the obtained molded body is not easily impaired and poor appearance due to bleed-out is not easily caused. From the same viewpoint, the content of the lubricant (C) is more preferably 0.1 to 0.5 parts by mass relative to 100 parts by mass of the total of the semi-aromatic polyamide (A), the modified ethylene-α-olefin copolymer (B) and the lubricant (C).
[0073] 1-4.Other ingredients The polyamide resin composition of the present invention may further contain other components in addition to those described above, provided that the effects of the present invention are not impaired. Examples of the other components include aliphatic polyamides, crystal nucleating agents, organic stabilizers, heat stabilizers, inorganic fillers, pigments, dyes, weathering agents, antistatic agents, plasticizers, and other polymers.
[0074] 1-4-1. Aliphatic polyamide (D) The aliphatic polyamide (D) contains a component unit having an amide bond (-NH-C(=O)-) and no aromatic ring (an amide bond-containing component unit having no aromatic ring). The content of the component unit is preferably 80 mol % or more, more preferably 90 to 100 mol %, based on the total number of moles of the amide bond-containing component units constituting the aliphatic polyamide.
[0075] The aliphatic polyamide (D) may be a product of a polycondensation reaction between a dicarboxylic acid and a diamine, a polycondensation reaction between an aminocarboxylic acid, or a ring-opening polymerization reaction between a lactam. That is, the aliphatic polyamide (D) is composed of at least one of an amide bond-containing component unit composed of a component unit derived from a dicarboxylic acid and a component unit derived from a diamine, a component unit derived from an aminocarboxylic acid, and a component unit derived from a lactam.
[0076] (Dicarboxylic acid-derived component units / diamine-derived component units) The component unit (d1) derived from a dicarboxylic acid includes a component unit derived from an aliphatic dicarboxylic acid. The aliphatic dicarboxylic acid is preferably an aliphatic dicarboxylic acid having 2 to 14 carbon atoms, more preferably 4 to 14 carbon atoms. Examples of the aliphatic dicarboxylic acid include oxalic acid (C2), adipic acid (C6), pimelic acid (C7), suberic acid (C8), azelaic acid (C9), sebacic acid (C10), dodecanedioic acid (C12) and tetradecanedioic acid (C14), and preferably adipic acid (C6) and dodecanedioic acid (C12).
[0077] The content of component units derived from aliphatic dicarboxylic acids is preferably 80 mol % or more, and more preferably 90 to 100 mol %, based on the total number of moles of component unit (e1) positions derived from dicarboxylic acids.
[0078] The diamine-derived component unit (d2) includes an aliphatic diamine-derived component unit. The aliphatic diamine may be the same as the aliphatic diamine constituting the semi-aromatic polyamide (A) described above.
[0079] The content of the component units derived from an aliphatic diamine is preferably 80 mol % or more, and more preferably 90 to 100 mol %, based on the total number of moles of the component units (d2) derived from a diamine.
[0080] (Aminocarboxylic acid structural unit) The aminocarboxylic acid may be an aminocarboxylic acid having 6 to 12 carbon atoms, preferably 6 to 10 carbon atoms. Examples of such aminocarboxylic acids include 6-aminocaproic acid, 7-aminoheptanoic acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid.
[0081] (Lactam-derived unit) The lactam may be a lactam having 6 to 12 carbon atoms, preferably 6 to 10 carbon atoms. Examples of such lactams include α-pyrrolidone, ε-caprolactam, undecanelactam, ω-laurolactam.
[0082] Examples of the aliphatic polyamide (D) include polyamide 6, polyamide 66, polyamide 610, polyamide 12, and the like.
[0083] The melting point (Tm) of the aliphatic polyamide (D) measured by differential scanning calorimetry (DSC) is preferably 200 to 290° C., more preferably 220 to 280° C. When the melting point (Tm) of the aliphatic polyamide (D) is within the above range, the moldability can be improved without impairing the heat resistance of the obtained molded article.
[0084] The content of the aliphatic polyamide (D) is preferably 0 to 15 parts by mass, and more preferably 1 to 7 parts by mass, per 100 parts by mass of the total of the semi-aromatic polyamide (A), the modified ethylene-α-olefin copolymer (B) and the lubricant (C).
[0085] The content of the aliphatic polyamide (D) is preferably 0 to 15 parts by mass relative to 100 parts by mass of the total content of the semi-aromatic polyamide (A) and the aliphatic polyamide (D). When the content of the aliphatic polyamide (D) is a certain amount or more, the fluidity of the resin composition during melting can be further increased, and the amount of die buildup can be further reduced. When the content of the aliphatic polyamide (D) is a certain amount or less, the mechanical strength and heat resistance of the obtained molded article are less likely to be impaired. From the same viewpoint, the content of the aliphatic polyamide (D) is more preferably 1 to 7 parts by mass relative to 100 parts by mass of the total content of the semi-aromatic polyamide (A) and the aliphatic polyamide (D).
[0086] 1-4-2. Nucleating agent (E) The crystal nucleating agent (E) is not particularly limited as long as it can become a crystal nucleus of the semi-aromatic polyamide (A), and may be an inorganic compound or an organic compound.
[0087] Examples of inorganic compounds include silicate compounds such as talc, clay, kaolinite, and kaolin, titanium dioxide, and calcium oxide. Among them, silicate compounds are preferred, and talc is more preferred. The average particle size of the inorganic compound particles can be 0.1 to 6 μm, preferably 0.5 to 3 μm. Examples of organic compounds include metal salts of organic phosphates.
[0088] The content of the crystal nucleating agent (E) is not particularly limited, but is preferably 0 to 5 parts by mass, and more preferably 0.1 to 3 parts by mass, per 100 parts by mass of the semi-aromatic polyamide (A) and the modified ethylene-α-olefin copolymer (B) in total.
[0089] 1-4-3. Organic stabilizers (F) Examples of the organic stabilizer (F) include phenol-based stabilizers, amine-based stabilizers, thioether-based stabilizers, and phosphorus-based stabilizers.
[0090] The phenol-based stabilizer is preferably a hindered phenol-based stabilizer, examples of which include octadecyl 3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate; pentaerythryl-tetrakis [3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate]; and the like. The amine-based stabilizer is preferably a hindered amine-based stabilizer, examples of which include 1,2,2,6,6-pentamethyl-4-piperidyl stearate, 2,2,6,6-tetramethyl-4-piperidyl benzoate; and the like. Examples of thioether-based stabilizers include bis[2-methyl-4-(3-n-alkoxythiopropionyloxy)-5-t-butylphenyl]sulfide; and the like. The phosphorus-based stabilizer is not particularly limited, but is preferably, for example, a phosphite-based stabilizer, examples of which include triphenyl phosphite; diphenyl phosphite; and the like. Among them, phenol-based stabilizers are preferred. The organic stabilizer (F) may be one type, or two or more types may be combined.
[0091] The content of the organic stabilizer (F) is preferably 0 to 4 parts by mass, and more preferably 0.1 to 1.5 parts by mass, per 100 parts by mass of the total of the semi-aromatic polyamide (A) and the modified ethylene-α-olefin copolymer (B).
[0092] 1-4-4.Heat stabilizer (G) Examples of the heat stabilizer (G) include copper compounds and alkali metal halides.
[0093] Examples of the copper compound include copper halides such as cuprous chloride, cuprous bromide, cuprous iodide, cupric chloride, cupric bromide, and cupric iodide; copper salts of phosphoric acid such as cupric phosphate; copper salts of organic carboxylic acids such as cupric pyrophosphate and copper acetate; copper sulfide, and copper nitrate.
[0094] Examples of the alkali metal halide compound include lithium chloride, lithium bromide, lithium iodide, sodium fluoride, sodium chloride, sodium bromide, sodium iodide, potassium fluoride, potassium chloride, potassium bromide, and potassium iodide, and preferably potassium iodide.
[0095] These may be used alone or in combination of two or more.
[0096] The content of the heat stabilizer (G) is preferably 0 to 0.4 parts by mass, and more preferably 0.005 to 0.25 parts by mass, per 100 parts by mass of the total of the semi-aromatic polyamide (A) and the modified ethylene-α-olefin copolymer (B).
[0097] The organic stabilizer (F) and the heat resistance stabilizer (G) may be added in any form. For example, they may be added to the above components as they are, or may be added in the form of a masterbatch. It is more preferable that:
[0098] 1-4-5.Inorganic filler (H) The polyamide resin composition of the present invention may further contain an inorganic filler (H) from the viewpoint of increasing the mechanical strength of a molded product.
[0099] The shape of the inorganic filler (H) is not particularly limited, but is preferably fibrous from the viewpoint of easily increasing the mechanical strength. Examples of fibrous fillers include glass fiber, wollastonite, potassium titanate whiskers, calcium carbonate whiskers, aluminum borate whiskers, magnesium sulfate whiskers, zinc oxide whiskers, milled fiber, and cut fiber. Among them, wollastonite or glass fiber is preferred from the viewpoint of easily increasing the mechanical strength of the molded body.
[0100] 1-5. Pellets The polyamide resin composition of the present invention can be used, for example, in the form of pellets. The pellets containing the polyamide resin composition of the present invention have a continuous phase mainly composed of the semi-aromatic polyamide (A) and a dispersed phase mainly composed of the modified ethylene-α-olefin copolymer (B).
[0101] The average particle size (dispersed particle size) of the dispersed phase of the modified ethylene-α-olefin copolymer (B) is not particularly limited, but is usually 2 μm or less, and preferably 0.1 to 1.3 μm. This is preferable from the viewpoints of heat resistance, impact resistance, and blocking suppression. The average particle size of the dispersed phase can be adjusted by adjusting the content ratio of the semi-aromatic polyamide (A) and the modified ethylene-α-olefin copolymer (B), kneading conditions, etc.
[0102] The lubricant (C) may be uniformly dispersed in the pellets, or may be unevenly distributed on the surface. From the viewpoint of facilitating reduction of the mold release resistance when the pellets are melt-molded, it is preferable that the lubricant (C) is unevenly distributed on the surface of the pellets. The distribution of the lubricant (C) can be adjusted by the degree of affinity of the lubricant (C) to the semi-aromatic polyamide (A). From the viewpoint of facilitating uneven distribution on the surface of the pellets, it is preferable that the lubricant (C) is, for example, a metal salt of montanic acid.
[0103] The average particle size of the pellets is not particularly limited, but from the viewpoint of facilitating smooth supply of the resin to the molding machine and smooth melting of the resin, it is 1 to 7 mm, preferably 2 to 5 mm, in the strand direction and 1 to 5 mm, preferably 2 to 4 mm, in the cutting direction (direction perpendicular to the strand direction).
[0104] 1-6. Method for producing polyamide resin composition The polyamide resin composition of the present invention can be produced, for example, by melt-kneading the above-mentioned components, followed by granulation or pulverization to form pellets.
[0105] The melting temperature (e.g., cylinder temperature) is not particularly limited, but is preferably Tmax to (Tmax+40)°C, where Tmax is the melting point of the semi-aromatic polyamide (A) having the highest melting point among the semi-aromatic polyamides (A).
[0106] The melt kneading can be carried out by any kneading method, for example, a single screw extruder, a multi-screw extruder, a kneader, or a Banbury mixer.
[0107] Before melt-kneading, the above components may be mixed as necessary, for example, by using a Henschel mixer, a V blender, a ribbon blender, or a tumbler blender.
[0108] The polyamide resin composition of the present invention contains a lubricant (C). This not only provides excellent flowability during molding, but also reduces the resistance to release from the mold. This reduces the amount of resin mixed into the pellets, allowing a molded product with good appearance to be obtained.
[0109] 2. Manufacturing method of molded body The pellets containing the polyamide resin composition of the present invention are suitably used for producing a molded article. That is, the method for producing a molded article includes a step of melt-molding the pellets containing the polyamide resin composition to obtain a molded article.
[0110] The melt molding can be carried out by any melt molding method, such as compression molding, injection molding, or extrusion molding. For example, in the extrusion molding method, pellets are fed into a hopper, heated and dried in the hopper, and then melt-kneaded in an extruder to produce a molded body of a desired shape.
[0111] The pellets can be heated and dried in the hopper by any method, for example, by supplying heated dry air or heated dry nitrogen gas and contacting the pellets with the heated air flow for a predetermined time. The temperature of the heated dry air or heated dry nitrogen gas can be, for example, 80 to 120°C, and the contact time can be, for example, 1 to 6 hours.
[0112] The melting temperature of the pellets (e.g., cylinder temperature) is not particularly limited, but may be, for example, Tmax to (Tmax+40)° C., where Tmax is the melting point of the semi-aromatic polyamide (A) having the highest melting point among the semi-aromatic polyamides (A). For example, the melting temperature may be about 350 to 300° C.
[0113] Alternatively, the pellets may be melted in an injection molding machine and then injected into a mold to produce a molded article.
[0114] The pellets containing the polyamide resin composition of the present invention can be used to manufacture various molded products. The uses of the molded products are not particularly limited, but include, for example, products molded using complex molds, such as connectors for connecting electronic circuits to each other, electric tools and general industrial parts, mechanical parts such as gears and cams, electronic parts such as printed wiring boards and housings for electronic parts, automobile interior and exterior parts, engine room parts, and automobile electrical parts. Among them, the resin is also suitable for forming automobile interior and exterior parts, engine room parts, and automobile electrical parts. EXAMPLES
[0115] The present invention will now be described with reference to examples, which should not be construed as limiting the scope of the present invention.
[0116] 1. Constituent materials (1) Semi-aromatic polyamide (A) <Preparation of Polyamide (PA-1)> 1,6-Hexanediamine 139.3 g (1.20 mol), 2-methyl-1,5-pentanediamine 139.3 (1.20 mol), terephthalic acid 365.5 g (2.2 mol), sodium hypophosphite 0.55 g (5.2 × 10 -3 mol) and 64 mL of ion-exchanged water were charged into a 1-liter reactor, and after replacing with nitrogen, the reaction mixture was heated at 250°C and 35 kg / cm 2The reaction was carried out for 1 hour under the above conditions. The molar ratio of 1,6-hexanediamine to 2-methyl-1,5-pentanediamine was 50:50. After 1 hour had passed, the reaction product produced in the reactor was transferred to a pressurized water supply system connected to the reactor and maintained at a pressure of about 10 kg / cm. 2 The mixture was withdrawn into a receiver set at a low temperature to obtain 561 g of a polyamide precursor having an intrinsic viscosity [η] of 0.15 dL / g. The polyamide precursor was then dried and melt-polymerized using a twin-screw extruder at a cylinder temperature of 330°C to obtain polyamide (PA-1).
[0117] The composition of the obtained polyamide (PA-1) was such that the content of the component units derived from terephthalic acid in the component units (a1) derived from dicarboxylic acid was 100 mol%, the content of the component units derived from 1,6-hexanediamine in the component units (a2) derived from diamine was 50 mol%, and the content of the component units derived from 2-methyl-1,5-pentanediamine was 50 mol%. The intrinsic viscosity [η] of the polyamide (PA-1) was 0.9 dL / g, and the melting point was 300°C.
[0118] <Preparation of Polyamide (PA-2)> 269.3 g (2.32 mol) of 1,6-hexanediamine, 205.6 g (1.24 mol) of terephthalic acid, 148.0 g (1.01 mol) of adipic acid, and 0.48 g (4.50 × 10) of sodium hypophosphite as a catalyst. -3 3.43 g (2.81 x 10 moles) of benzoic acid as a molecular weight regulator -2 mol) and 62 mL of ion-exchanged water were charged into a 1-liter reactor, and after replacing with nitrogen, the mixture was heated at 250°C and 35 kg / cm 2 The reaction was carried out for 1 hour under the above conditions. The molar ratio of terephthalic acid to adipic acid was 55:45. After 1 hour had passed, the reaction product produced in the reactor was transferred to a pressurized water supply system connected to the reactor and maintained at a pressure of about 10 kg / cm. 2 The mixture was withdrawn into a receiver set at a low temperature to obtain 559 g of a polyamide precursor having an intrinsic viscosity [η] of 0.15 dL / g. The polyamide precursor was then dried and melt-polymerized using a twin-screw extruder at a cylinder temperature of 330°C to obtain polyamide (PA-2).
[0119] The composition of the obtained polyamide (PA-2) is as follows: the content of the component units derived from terephthalic acid in the component units (a1) derived from dicarboxylic acid was 55 mol %, the content of the component units derived from adipic acid was 45 mol %, and the content of the component units derived from 1,6-hexanediamine in the component units (a2) derived from diamine was 100 mol %. The intrinsic viscosity [η] of the polyamide (PA-2) was 1.0 dL / g, and the melting point was 295°C.
[0120] The compositions and physical properties of the resulting polyamides (PA-1) and (PA-2) are shown in Table 1.
[0121] [Table 1]
[0122] The intrinsic viscosity [η] and the melting point (Tm) were measured by the following methods.
[0123] (Intrinsic viscosity [η]) According to JIS K6810-1977, 0.5 g of polyamide resin was dissolved in 50 ml of 96.5% sulfuric acid solution to prepare a sample solution. The flow time of the obtained sample solution was measured using an Ubbelohde viscometer under the condition of 25±0.05°C. The measurement results were applied to the following formula to calculate the intrinsic viscosity [η] of the polyamide resin. [η]=ηSP / [C(1+0.205ηSP)] ηSP=(t-t0) / t0 [η]: Intrinsic viscosity (dl / g) ηSP: Specific viscosity C: Sample concentration (g / dl) t: Time required for sample solution to flow (seconds) t0: Number of seconds that blank sulfuric acid flows (seconds)
[0124] (Melting point (Tm)) The melting point (Tm) of the polyamide resin was measured using a differential scanning calorimeter (DSC220C type, manufactured by Seiko Instruments Inc.). Specifically, about 5 mg of the polyamide resin was sealed in an aluminum pan for measurement and set in the differential scanning calorimeter. Then, it was heated from room temperature to 350°C at 10°C / min. In order to completely melt the resin, it was held at 360°C for 3 minutes, and then cooled to 30°C at 10°C / min. After leaving it at 30°C for 5 minutes, it was heated a second time to 360°C at 10°C / min. The temperature (°C) of the endothermic peak in this second heating was taken as the melting point (Tm) of the polyamide resin.
[0125] (2) Modified ethylene-α-olefin copolymer (B) <Production of modified ethylene-1-butene copolymer (MAH-PE)> Ethylene-1-butene copolymer (density = 0.920 g / cm) prepared using a Ti catalyst 3 A modified ethylene-1-butene copolymer (MAH-PE) was obtained by melting 100 parts by mass of a tertiary ethylcellulose copolymer having a melting point of 124°C, crystallinity of 48%, MFR (ASTM D 1238, 190°C, 2.16 kg load) of 1.0 g / 10 min, and ethylene content of 96 mol%), 0.8 parts by mass of maleic anhydride, and 0.07 parts by mass of a peroxide (product name: Perhexyne-25B, manufactured by Nippon Oil & Fats Co., Ltd.) in a Henschel mixer. The resulting mixture was melt-graft-modified in a 65 mmφ single-screw extruder set to 230°C, to obtain a modified ethylene-1-butene copolymer (MAH-PE).
[0126] The amount of maleic anhydride grafted into the modified ethylene-1-butene copolymer (MAH-PE) obtained was measured by IR analysis to be 0.8% by mass, and the MFR was 0.27g / 10min and the melting point was 122℃.
[0127] (Melt Flow Rate (MFR)) The measurements were performed in accordance with ASTM D1238 at 190°C and a load of 2.16 kg.
[0128] (density) Measured at 23°C according to ASTM D792.
[0129] (graft amount) Specifically, the graft amount of the unsaturated carboxylic acid or its derivative can be measured by the following procedure. 1) Prepare several samples of modified ethylene-α-olefin copolymer (B) with different graft amounts, and compare the graft amounts. 13 The graft amount was measured by C-NMR. In addition, infrared spectroscopy (IR) was also performed on these samples. A calibration curve was then created between the graft amount measured by NMR and the intensity ratio of a specific peak in the infrared spectroscopy (IR) spectrum. 2) Next, the intensity ratio of specific peaks in the infrared (IR) spectrum of the modified ethylene-α-olefin copolymer (B) to be measured was measured. 3) The results of the measurement in 2) above were compared with a calibration curve to identify the graft amount of the modified ethylene-α-olefin copolymer (B) to be measured. The NMR and IR measurement conditions were as described above.
[0130] (3) Lubricant (C) Calcium montanate (CS-8CP manufactured by Nitto Kasei Kogyo Co., Ltd.) Calcium behenate (CS-7 manufactured by Nitto Kasei Kogyo Co., Ltd.) 12-Hydroxybarium stearate (BS-6 manufactured by Nitto Kasei Kogyo Co., Ltd.)
[0131] (4) Other ingredients Aliphatic polyamide (D): Polyamide 12 (PA12) (manufactured by Ube Industries, melting point 179°C) Nucleating agent (E): Talc Organic stabilizer (F): Irganox 1010 (manufactured by BASF Japan, hindered phenol stabilizer) Heat stabilizer (G): A mixture of 10% by mass of copper iodide and 90% by mass of potassium iodide
[0132] 2. Preparation and evaluation of pellets of polyamide resin composition [Examples 1 to 3 and Comparative Example 1] The semi-aromatic polyamide (A), modified ethylene-α-olefin copolymer (B), lubricant (C), aliphatic polyamide (D), crystal nucleating agent (E), organic stabilizer (F), and heat stabilizer (G) shown in Table 2 were mixed in the ratios shown in Table 2. This mixture was melt-kneaded in a TEX30α twin-screw extruder (screw diameter 30 mm, L / D=49, barrel temperature (℃) 330℃) manufactured by The Japan Steel Works, Ltd., and extruded from a die into a strand shape. The strand-shaped resin composition was then cut with a pelletizer to obtain pellets.
[0133] The presence or absence of nozzle discharge during pellet production, flowability, and mold release resistance were evaluated by the following methods.
[0134] (eye boogers) Under the above conditions, pellets of the polyamide resin composition were produced, and the length of the die resin adhering to the die outlet was measured 30 minutes after the start of production.
[0135] (Flow length) The obtained polyamide resin composition was injected into a barflow mold having a width of 10 mm and a thickness of 0.5 mm under the following conditions, and the flow length (mm) of the resin composition in the mold was measured. Injection molding machine: Sodick Plastech Co., Ltd., Tupearl TR40S3A Injection pressure setting: 2000kg / cm 2 Cylinder setting temperature: Melting point of semi-aromatic polyamide (A) + 10℃ Mold temperature: 120℃
[0136] (Mold release resistance) The obtained polyamide resin composition was injection molded under the following conditions using a connector mold having a length of 62 mm, a width of 6 mm, a thickness of 7 mm, and 50 cores, and the resistance at the time of demolding was measured. Specifically, the resistance at the time of demolding was measured by reading the resistance of the ejector pin when the molded body was demolded from the monitor of the injection molding machine. Injection molding machine: Sumitomo Heavy Industries, Ltd. SE50DU Cylinder temperature: 310℃ Mold temperature: 80℃
[0137] The evaluation results of Examples 1 to 3 and Comparative Example 1 are shown in Table 2.
[0138] [Table 2]
[0139] As shown in Table 2, the polyamide resin compositions of Examples 1 to 3 containing the lubricant (C) have shorter die length during pellet production than the polyamide resin composition of Comparative Example 1 containing no lubricant (C). They also have longer flow length and lower mold release resistance. These facts show that the polyamide resin composition of the present invention has high moldability. [Industrial Applicability]
[0140] According to the present invention, it is possible to provide a polyamide resin composition capable of suppressing the generation of lumps known as "pit deposits," for example, when a polyamide resin composition is melt-kneaded to produce pellets, and a method for producing a molded article using the same.
Claims
1. 64.9 to 89 parts by mass of a semi-aromatic polyamide (A) containing component units (a1) derived from a dicarboxylic acid including component units derived from terephthalic acid and component units (a2) derived from a diamine including at least one of component units derived from an aliphatic diamine and a component unit derived from an alicyclic diamine, and having a melting point of 280° C. or higher; 10 to 35 parts by mass of a modified ethylene / α-olefin copolymer (B) having a graft amount of 0.01 to 5% by mass, the modified ethylene / α-olefin copolymer being obtained by modifying an ethylene / α-olefin copolymer with an unsaturated carboxylic acid or a derivative thereof; 0.1 to 1 parts by mass of a lubricant (C); (wherein the total of (A), (B) and (C) is 100 parts by mass), the ethylene / α-olefin copolymer is a copolymer of ethylene and a C4 to C20 α-olefin, and has a content of ethylene-derived component units of 70 mol % or more and a content of α-olefin-derived component units of 30 mol % or less based on all component units of the copolymer; The lubricant (C) contains at least one metal salt or ester of a fatty acid selected from the group consisting of montanic acid, 12-hydroxystearic acid, and behenic acid. Polyamide resin composition.
2. The content of the component units derived from the terephthalic acid is 20 to 100 mol % based on the total number of moles of the component units (a1) derived from the dicarboxylic acid. The polyamide resin composition according to claim 1.
3. The diamine-derived component unit (a2) includes an aliphatic diamine-derived component unit. The polyamide resin composition according to claim 1 or 2.
4. The component units derived from the aliphatic diamine include component units derived from a linear aliphatic diamine having 4 to 8 carbon atoms. The polyamide resin composition according to claim 3.
5. The component unit derived from the linear aliphatic diamine having 4 to 8 carbon atoms includes a component unit derived from 1,6-hexanediamine. The polyamide resin composition according to claim 4.
6. The content of the modified ethylene / α-olefin copolymer (B) is 15 to 35 parts by mass per 100 parts by mass of the total of (A), (B) and (C). The polyamide resin composition according to any one of claims 1 to 5.
7. Further comprising an aliphatic polyamide (D), The polyamide resin composition according to any one of claims 1 to 6.
8. The polyamide resin composition according to any one of claims 1 to 7, pellet.
9. The process includes melt molding the pellet according to claim 8 to obtain a molded body. A method for producing a molded body.