Method for producing expandable polyvinyl chloride resin particles

A simplified method for producing expandable vinyl chloride resin particles by melt-kneading and extruding with controlled conditions addresses complexity and environmental issues, achieving high expansion ratios and flame retardancy.

JP7572825B2Active Publication Date: 2024-10-24KANEKA CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020162883
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-29
Publication Date
2024-10-24
Estimated Expiration
2040-09-29

AI Technical Summary

Technical Problem

Existing methods for producing expandable vinyl chloride resin particles are complex, environmentally harmful due to solvent use, time-consuming, and require large amounts of blowing agents, affecting productivity and cost.

Method used

A method involving melt-kneading a blowing agent with vinyl chloride resin, extruding through a die into pressurized water, and immediately cutting and cooling to form particles with controlled conditions, achieving high expansion ratios and improved flame retardancy.

Benefits of technology

The method simplifies production, reduces environmental impact, lowers viscosity, and enables high expansion ratios with enhanced flame retardancy, suitable for fire-resistant materials.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide a new production method for producing expandable vinyl chloride-based resin particles exhibiting a high expansion ratio.SOLUTION: A method for producing expandable vinyl chloride-based resin particles satisfying the following (a) and (b), (a) the method includes a step of extruding a melt-kneaded product of a vinyl chloride-based resin having a resin temperature of 150-250°C and contains an expanding agent into pressurized water at a temperature of 60-100°C from a die having a plurality of holes, and cutting the melt-kneaded product by a rotary cutter immediately after extrusion, and (b) a particle weight of the expandable vinyl chloride-based resin particles is 2.5-7.0 mg / granule.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing expandable vinyl chloride resin particles. [Background technology]

[0002] Resin foams have light weight, heat insulation, and shock-absorbing properties, and have been widely used as insulation materials for houses and the like, and heat-retaining materials for pipes and the like. Among them, styrene resin foam molded products obtained using expandable styrene resin particles containing a foaming agent have a high degree of freedom in shape, and are widely used as insulation materials that can be applied to areas where it is difficult to apply foams of simple shapes such as board shapes obtained by extrusion foaming methods and the like. Since styrene resins are flammable resins, flame retardants are added to styrene resin foam molded products to ensure a certain degree of flame retardancy. However, due to recent fire accidents at construction sites and fire cases in high-rise apartment buildings, higher flame retardancy than before is being required for insulation materials for construction.

[0003] Examples of foams having excellent flame retardant performance include resin foam molded products using vinyl chloride resin as a base resin.

[0004] For example, Patent Documents 1 and 2 disclose pre-expanded chlorinated polyvinyl chloride resin particles obtained by kneading a chlorinated polyvinyl chloride resin and a solvent compatible with the chlorinated polyvinyl chloride resin, pelletizing the mixture, impregnating the mixture with an evaporative blowing agent in the liquid phase, and then pre-expanding the mixture. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP-A-64-132 [Patent Document 2] Japanese Patent Publication No. 2-182735 Summary of the Invention [Problem to be solved by the invention]

[0006] However, the above-mentioned manufacturing method has a problem that the process is complicated because the pellets containing the solvent are impregnated with the foaming agent by liquid phase impregnation, and the solvent dissolves into the liquid phase, which requires an additional waste liquid treatment process, and that measures to reduce the impact on the environment are necessary. In addition, it takes a long time to impregnate the pellets with the foaming agent by liquid phase impregnation, and in particular, in order to achieve a high expansion ratio, it is necessary to impregnate the pre-expanded particles with the foaming agent. Furthermore, in order to achieve a desired expansion ratio, it is necessary to impregnate the pellets and pre-expanded particles with a large amount of foaming agent, so that a large amount of foaming agent must be used. As such, the above-mentioned manufacturing method has room for improvement in terms of productivity and cost.

[0007] Therefore, an object of the present invention is to provide a new production method capable of obtaining expandable vinyl chloride resin particles exhibiting a high expansion ratio. [Means for solving the problem]

[0008] In order to solve the above-mentioned problems, the present inventors have conducted extensive investigations into a method for producing expandable resin particles using a vinyl chloride resin, in which a blowing agent is melt-kneaded into a molten resin to dissolve and disperse the blowing agent, and the resulting resin melt containing the blowing agent is extruded through a die having a plurality of fine holes into pressurized circulating water, and then cut and cooled to solidify immediately after extrusion. As a result, they have succeeded in producing expandable resin particles with high expandability by controlling specific conditions for pelletizing the blowing agent-containing resin melt, thereby completing the present invention.

[0009] That is, the present invention relates to a method for producing expandable polyvinyl chloride resin particles that satisfies the following (a) and (b) (hereinafter sometimes abbreviated as "the method according to the present invention"). (a) a step of extruding a molten mixture of a polyvinyl chloride resin containing a foaming agent, the mixture having a resin temperature of 150 to 250°C, from a die having multiple holes into pressurized water having a temperature of 60 to 100°C, and cutting the mixture with a rotary cutter immediately after extrusion; (b) The particle weight of the expandable polyvinyl chloride resin particles is 2.5 to 7.0 mg / particle.

[0010] In the method according to the present invention, the water pressure in the pressurized water is preferably 1.0 to 1.5 MPa.

[0011] In the method according to the present invention, the plurality of holes preferably have a hole diameter of 0.7 to 1.2 mm.

[0012] In the method according to the present invention, the vinyl chloride resin preferably contains a chlorinated vinyl chloride polymer.

[0013] In the method according to the present invention, the vinyl chloride resin preferably contains a chlorinated vinyl chloride polymer having a chlorine content of 60% by weight or more and 75% by weight or less.

[0014] In the process according to the present invention, the foaming agent preferably contains a saturated hydrocarbon having 4 to 6 carbon atoms, and more preferably, at least one of the saturated hydrocarbons having 4 to 6 carbon atoms is pentane.

[0015] In the process according to the invention, it is preferred that the blowing agent comprises a ketone.

[0016] In the method according to the present invention, the expandable vinyl chloride resin particles preferably contain a vinyl chloride polymer and / or a chlorinated vinyl chloride polymer having an average degree of polymerization of 300 or more and 3,000 or less.

[0017] In the production method according to the present invention, the expandable polyvinyl chloride resin particles preferably contain at least one selected from the group consisting of a copolymer having an aromatic vinyl monomer and an unsaturated nitrile as structural units, an acrylic resin, and a chlorinated polyethylene, and more preferably contain a copolymer having an aromatic vinyl monomer and an unsaturated nitrile as structural units and / or an acrylic resin.

[0018] In the production method according to the present invention, it is more preferable that the expandable vinyl chloride resin particles are made of a copolymer having an aromatic vinyl monomer and an unsaturated nitrile as structural units and / or an acrylic resin in combination with chlorinated polyethylene.

[0019] The method for producing pre-expanded vinyl chloride resin particles according to the present invention includes a step of pre-expanding the expandable vinyl chloride resin particles obtained by the method according to the present invention.

[0020] The method for producing a vinyl chloride resin foam according to the present invention includes a step of in-mold foaming of the pre-expanded vinyl chloride resin particles obtained by the method for producing pre-expanded vinyl chloride resin particles according to the present invention. Effect of the Invention

[0021] According to the production method of the present invention, expandable vinyl chloride resin particles exhibiting a high expansion ratio can be easily produced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] The method for producing expandable polyvinyl chloride resin particles according to the present invention (hereinafter sometimes referred to as "the present method") includes the steps of: (a) A molten mixture of a polyvinyl chloride resin containing a foaming agent, the mixture having a resin temperature of 150 to 250°C, is extruded from a die having multiple holes into pressurized water having a temperature of 60 to 100°C, and cut with a rotary cutter immediately after extrusion; and (b) The particle weight of the expandable polyvinyl chloride resin particles is 2.5 to 7.0 mg / particle.

[0023] The present manufacturing method is a simple and environmentally friendly manufacturing method compared to the conventional manufacturing method of liquid-phase impregnation of resin particles with a foaming agent. In addition, by melt-kneading the foaming agent and the vinyl chloride resin, the viscosity of the molten resin can be reduced, making it possible to lower the molding temperature of the vinyl chloride resin, and there is an advantage in that thermal decomposition is unlikely to occur and resin scorching is suppressed, making it easy to obtain a high expansion ratio. Furthermore, the present inventors have obtained a new finding that, although the expandable resin particles manufactured using the vinyl chloride resin are sufficiently gelled, there is a tendency for volatile matter to escape from the expandable resin particles compared to the expandable resin particles manufactured using the polystyrene resin. And, in the expandable vinyl chloride resin particles manufactured by extruding a molten mixture of the vinyl chloride resin containing a foaming agent, which has a resin temperature of 150 to 250 ° C, from a die having multiple holes into pressurized water at a temperature of 60 to 100 ° C, and cutting with a rotary cutter immediately after extrusion, if the expandable vinyl chloride resin is manufactured to have a specific particle weight, a high expansion ratio can be achieved. Furthermore, it was found that the shape of the expandable resin particles can be improved by setting the water pressure of the pressurized circulating water to 1.0 to 1.5 MPa in addition to the resin temperature and the temperature of the pressurized circulating water. That is, according to this manufacturing method, the expandable polyvinyl chloride resin particles obtained can have a high expansion ratio. In addition, since the flame retardancy derived from the polyvinyl chloride resin is excellent, it is suitable for flame-retardant and fire-resistant materials that require weight reduction.

[0024] In a preferred embodiment of the present production method, a vinyl chloride resin and, if necessary, various additives are fed to an extruder and melt-kneaded, a foaming agent is dissolved / dispersed in the molten mixture by the extruder or a dispersing facility downstream of the extruder, and the molten mixture of vinyl chloride resin containing a foaming agent is extruded at a resin temperature of 150-250°C through a die having many small holes attached downstream of the extruder into a cutter chamber filled with pressurized circulating water at a temperature of 60-100°C, and immediately after extrusion, the molten mixture is cut by a rotating cutter in contact with the die and cooled and solidified by the pressurized circulating water to obtain expandable vinyl chloride resin particles having a particle weight of 2.5-7.0 mg / particle.

[0025] A preferred embodiment of this production method will now be described.

[0026] The vinyl chloride resin is not particularly limited, but examples thereof include polyvinyl chloride (vinyl chloride homopolymer); vinyl chloride-vinyl acetate copolymer, vinyl chloride-(meth)acrylic acid copolymer, vinyl chloride-methyl (meth)acrylate copolymer, vinyl chloride-ethyl (meth)acrylate copolymer, vinyl chloride-maleic acid ester copolymer, vinyl chloride-ethylene copolymer, vinyl chloride-propylene copolymer, vinyl chloride-styrene copolymer, vinyl chloride-isobutylene copolymer, vinyl chloride-vinylidene chloride copolymer, vinyl chloride-styrene-maleic anhydride terpolymer, vinyl chloride-styrene-maleic anhydride terpolymer, vinyl chloride-styrene- Examples of the vinyl chloride copolymers include acrylonitrile terpolymers, vinyl chloride-butadiene copolymers, vinyl chloride-isoprene copolymers, vinyl chloride-chlorinated propylene copolymers, vinyl chloride-vinylidene chloride-vinyl acetate terpolymers, vinyl chloride-acrylonitrile copolymers, and various vinyl ether copolymers, and vinyl chloride copolymers of vinyl chloride and other monomers copolymerizable with vinyl chloride; post-chlorinated vinyl polymers, post-chlorinated polyvinyl chloride, post-chlorinated vinyl chloride copolymers, and post-chlorinated chlorinated olefins, and other vinyl polymers that have been modified (chlorinated, etc.). Furthermore, chlorinated polyolefins, such as chlorinated polyethylene, whose chemical structure is similar to that of polyvinyl chloride, may be used. Among these, from the viewpoint of flame retardancy, it is preferable to include vinyl chloride polymers and chlorinated vinyl chloride polymers, and among these, chlorinated vinyl chloride polymers are particularly preferable from the viewpoint of excellent flame retardancy and foamability. As the vinyl chloride resin, one or a mixture of two or more of these can be used. In this specification, the term "vinyl chloride polymer" means polyvinyl chloride and / or vinyl chloride copolymers.

[0027] Chlorinated vinyl chloride polymers are usually produced by using a vinyl chloride polymer as a raw material, supplying chlorine to the vinyl chloride polymer dispersed in an aqueous medium, and chlorinating the polymer in an aqueous medium by irradiating the polymer with a mercury lamp for photochlorination or by heating the polymer for chlorination, or by chlorinating the vinyl chloride polymer in a gas phase by irradiating the polymer with a mercury lamp. Examples of the vinyl chloride polymer as a raw material include the polyvinyl chloride and vinyl chloride copolymers exemplified above.

[0028] The average degree of polymerization of the vinyl chloride polymer is not particularly limited, but the lower limit is preferably 300 or more, more preferably 400 or more. On the other hand, the upper limit is preferably 3000 or less, more preferably 1500 or less. If the average degree of polymerization is within the above range, a high expansion ratio tends to be obtained. The average degree of polymerization of the chlorinated vinyl chloride polymer is regarded as the average degree of polymerization of the vinyl chloride polymer before chlorination. The average degree of polymerization is measured in accordance with JIS K6720-2.

[0029] The weight average molecular weight of the chlorinated vinyl chloride polymer is not particularly limited, but is preferably in the range of 30,000 to 400,000. If the weight average molecular weight is in the above range, a high expansion ratio tends to be obtained. The weight average molecular weight is evaluated by gel permeation chromatography in terms of polystyrene.

[0030] The chlorine content of the chlorinated vinyl chloride polymer is preferably in the range of 60% by weight to 75% by weight from the viewpoint of ensuring expandability. More preferably, it is in the range of 64% by weight to 70% by weight. The higher the chlorine content, the higher the expansion ratio tends to be obtained, but on the other hand, if the chlorine content is too high, the melt viscosity increases and the processability tends to be significantly impaired. The chlorine content of the chlorinated vinyl chloride polymer is measured in accordance with JIS K7385 B method.

[0031] In one embodiment of the present process, the chlorinated vinyl chloride polymer may be used alone or in combination of two or more kinds.

[0032] In one embodiment of the present manufacturing method, the vinyl chloride resin preferably contains a chlorinated vinyl chloride polymer as a main component from the viewpoint of foaming property. Although not particularly limited, the content of the chlorinated vinyl chloride polymer is preferably 50% by weight or more, more preferably 60% by weight or more, even more preferably 70% by weight or more, and most preferably 80% by weight or more in 100% by weight of the vinyl chloride resin. On the other hand, the upper limit is preferably 100% by weight of the chlorinated vinyl chloride polymer in 100% by weight of the vinyl chloride resin.

[0033] As a preferred embodiment of the present manufacturing method, a processing aid may be added. The processing aid may be any processing aid generally used for vinyl chloride resins. For example, copolymers having aromatic vinyl monomers and unsaturated nitrile monomers as structural units, such as styrene-acrylonitrile copolymers, acrylic resins, impact modifiers such as methyl methacrylate-butadiene-styrene polymers, chlorinated polyethylene, etc. are listed. From the viewpoint of easiness in obtaining expanded particles and foamed molded articles with a high expansion ratio, it is preferable to add at least one selected from the group consisting of copolymers having aromatic vinyl monomers and unsaturated nitrile monomers as structural units, acrylic resins, and chlorinated polyethylene. Among them, from the viewpoint of promoting gelation of vinyl chloride resins and improving mechanical properties and expandability, it is more preferable to use a copolymer having aromatic vinyl monomers and unsaturated nitrile monomers as structural units and / or an acrylic resin in combination with chlorinated polyethylene.

[0034] Examples of the aromatic vinyl monomer of the copolymer having an aromatic vinyl monomer and an unsaturated nitrile monomer as structural units include styrene derivatives such as styrene, α-methylstyrene, ethylstyrene, and halogenated styrene. Examples of the unsaturated nitrile monomer include acrylonitrile and methacrylonitrile. The copolymer having an aromatic vinyl monomer and an unsaturated nitrile monomer as structural units may have structural units derived from monomers other than the aromatic vinyl monomer and the unsaturated nitrile monomer (other copolymerizable monomers). Examples of other copolymerizable monomers include (meth)acrylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, N-butyl (meth)acrylate, isobutyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate, (meth)acrylic acid, maleic anhydride, and N-substituted maleimide.

[0035] The preferred range of the unsaturated nitrile monomer in the copolymer having an aromatic vinyl monomer and an unsaturated nitrile monomer as structural units is 5 to 45% by weight, more preferably 8 to 35% by weight, and even more preferably 10 to 30% by weight, based on 100% by weight of the entire copolymer having an aromatic vinyl monomer and an unsaturated nitrile monomer as structural units. By being in the above range, expanded beads and expanded molded products with a high expansion ratio can be easily obtained.

[0036] A preferred example of the copolymer having an aromatic vinyl monomer and an unsaturated nitrile monomer as structural units is a styrene-acrylonitrile copolymer. The copolymer having an aromatic vinyl monomer and an unsaturated nitrile monomer as structural units may be used alone or in combination of two or more kinds, and it is preferable to use a styrene-acrylonitrile copolymer as at least one kind. The copolymer having an aromatic vinyl monomer and an unsaturated nitrile monomer as structural units is preferably one having a weight average molecular weight higher than the weight average molecular weight of the vinyl chloride resin used, since it is easy to ensure a high expansion ratio. The weight average molecular weight of the copolymer having an aromatic vinyl monomer and an unsaturated nitrile monomer as structural units is evaluated by gel permeation chromatography in terms of polystyrene molecular weight. For example, Blendex 869 manufactured by Galata can be used as the copolymer having an aromatic vinyl monomer and an unsaturated nitrile monomer as structural units.

[0037] Specific examples of acrylic resins include polymethyl methacrylate obtained by polymerizing methyl methacrylate, methacrylic acid alkyl esters having 2 to 8 carbon atoms in the alkyl group such as n-butyl methacrylate, acrylic acid alkyl esters having 1 to 8 carbon atoms in the alkyl group such as ethyl acrylate, and copolymers of at least one monomer copolymerizable with these, such as butylene, substituted styrene, and acrylonitrile. It is preferable to use an acrylic resin having a weight average molecular weight higher than that of the vinyl chloride resin used, since it is easy to ensure a high expansion ratio. The weight average molecular weight of the acrylic resin is evaluated in terms of polystyrene molecular weight by gel permeation chromatography. As the acrylic resin, for example, Kane Ace PA-40 manufactured by Kaneka can be used.

[0038] The chlorinated polyethylene may be any type that is generally used in vinyl chloride resins. The chlorine content of the chlorinated polyethylene is measured in accordance with JIS K7385 Method B.

[0039] The amount of the processing aid added is not particularly limited, but is preferably 1 to 50 parts by weight, more preferably 5 to 50 parts by weight, and even more preferably 8 to 30 parts by weight, relative to 100 parts by weight of the vinyl chloride resin. When the amount is 1 part by weight or more, expanded beads and / or expanded molded articles having a high expansion ratio are easily obtained, and when it is 50 parts by weight or less, expanded beads and / or expanded molded articles having excellent flame retardant performance can be obtained.

[0040] If necessary, flame retardants, stabilizers, lubricants, nucleating agents, foaming assistants, antistatic agents, radiation heat transfer inhibitors, plasticizers, solvents, and colorants such as pigments and dyes may be added.

[0041] As the flame retardant, known flame retardants can be used, and examples thereof include bromine-based flame retardants, phosphorus-based flame retardants, boron-based flame retardants, intumescent flame retardants such as ammonium polyphosphate and melamine cyanurate, hydroxide compounds such as aluminum hydroxide and magnesium hydroxide, and flame retardant assistants such as antimony oxide, zinc oxide, and zinc borate.

[0042] The stabilizer may be any of those conventionally used in vinyl chloride resins. Examples include tin stabilizers, antioxidants such as phenolic compounds, phosphorus compounds, and amine compounds, epoxy stabilizers, and zeolites. The amount of each stabilizer used is not particularly limited as long as it does not impair the effects of the present invention, but is preferably 10 parts by weight or less per 100 parts by weight of vinyl chloride resin.

[0043] Examples of the lubricant include waxes such as ester wax and polyethylene wax, and fatty acid metal salts such as calcium stearate and zinc stearate.

[0044] Examples of the nucleating agent include inorganic compounds such as silica, calcium silicate, wollastonite, kaolin, clay, mica, zinc oxide, calcium carbonate, sodium hydrogen carbonate, zeolite, and talc.

[0045] Examples of the radiation heat transfer inhibitor include substances that have the property of reflecting, scattering, or absorbing light in the near infrared or infrared region, such as graphite, graphene, carbon black, expanded graphite, titanium oxide, and aluminum.

[0046] Other resins (thermoplastic resins and thermosetting resins) may be used in combination with the vinyl chloride resin as long as the effects of the present invention are not impaired. When using other resins in combination, the amount of the other resins is not particularly limited as long as the effects of the present manufacturing method are not impaired, but is preferably 0 to 99 parts by weight per 100 parts by weight of the vinyl chloride resin.

[0047] The blowing agent may be any known blowing agent, and is not particularly limited, but examples thereof include the following blowing agents: hydrocarbons such as normal butane, isobutane, normal pentane, isopentane, neopentane, cyclopentane, normal hexane, and cyclohexane; ethers such as dimethyl ether, diethyl ether, methyl ethyl ether, isopropyl ether, n-butyl ether, diisopropyl ether, furan, furfural, 2-methylfuran, tetrahydrofuran, and tetrahydropyran; ketones such as dimethyl ketone (acetone), methyl ethyl ketone, diethyl ketone, methyl n-propyl ketone, methyl-n-butyl ketone, methyl-i-butyl ketone, methyl-n-hexyl ketone, ethyl-n-propyl ketone, and ethyl-n-butyl ketone; saturated alcohols having 1 to 4 carbon atoms such as methanol, ethanol, propyl alcohol, i-propyl alcohol, butyl alcohol, i-butyl alcohol, and t-butyl alcohol; methyl formate, ethyl formate, etc. Examples of the foaming agents that can be used include carboxylic acid esters such as ter, propyl formate, butyl formate, amyl formate, methyl propionate, and ethyl propionate; alkyl halides such as methyl chloride and ethyl chloride; hydrofluoroolefins or chlorinated hydrofluoroolefins such as trans-1,3,3,3-tetrafluoropropene (trans-HFO-1234e), cis-1,3,3,3-tetrafluoropropene (cis-HFO-1234ze), 2,3,3,3-tetrafluoropropene (trans-HFO-1234yf), trans-1-chloro-3,3,3-trifluoropropene (trans-HCFO-1233zd), and cis-1-chloro-3,3,3-trifluoropropene (cis-HCFO-1233zd); physical foaming agents such as inorganic foaming agents such as water, carbon dioxide, and nitrogen; and chemical foaming agents such as azo compounds and tetrazole. These other foaming agents may be used alone or in combination of two or more.

[0048] In one embodiment of the present invention, it is preferable to use a physical foaming agent as the foaming agent, and more preferably, a saturated hydrocarbon having 4 to 6 carbon atoms (4, 5, and 6 carbon atoms) is contained. When the carbon number of the foaming agent is 4 or more, the volatility is low and the foaming agent is less likely to escape from the expandable vinyl chloride resin particles, so that the foaming agent remains sufficiently in the foaming process when actually used, and sufficient foaming power can be obtained, which is preferable because it is easy to increase the foaming ratio. In addition, when the carbon number is 6 or less, the boiling point of the foaming agent is not too high, so that sufficient foaming power can be easily obtained by heating during pre-foaming, and there is a tendency that high foaming is easy to achieve. Examples of saturated hydrocarbons having 4 to 6 carbon atoms include normal butane, isobutane, normal pentane, isopentane, neopentane, cyclopentane, normal hexane, and cyclohexane. As the saturated hydrocarbons having 4 to 6 carbon atoms, it is preferable to use at least pentane from the viewpoint of the solubility and retention of the foaming agent in the resin.

[0049] In a preferred embodiment of the present invention, a ketone is used as the foaming agent from the viewpoint of improving the solubility of the foaming agent. For example, by using a saturated hydrocarbon having 4 to 6 carbon atoms in combination with a ketone, the solubility of the saturated hydrocarbon having 4 to 6 carbon atoms in the resin can be further improved.

[0050] In one embodiment of the present invention, the amount of the foaming agent added is preferably 1 to 50 parts by weight per 100 parts by weight of the total amount of components constituting the expandable vinyl chloride resin particles other than the foaming agent. By controlling the amount of the foaming agent used within the above-mentioned predetermined range, there is an advantage that it is easy to obtain expanded particles having a high expansion ratio and foamed molded products having excellent surface beauty. A more preferred range is 4 to 33 parts by weight, and even more preferably 6 to 26 parts by weight.

[0051] In a preferred embodiment of the present method, the above components are melt-kneaded in an extruder, or a melt-kneaded product of a vinyl chloride resin containing a foaming agent is prepared by an extruder or a dispersion facility following the extruder. A general extruder can be used as the extruder, and specifically, a single-screw extruder, a twin-screw extruder, a tandem extruder, etc. can be mentioned. As the tandem extruder, a single-screw extruder connected to two single-screw extruders, a twin-screw extruder connected to a single-screw extruder, etc. can be mentioned. In addition, an extruder may be used in combination with a dispersion facility such as a static mixer or an agitator without a screw.

[0052] It is preferable to gel the vinyl chloride resin sufficiently. If the gelation is not sufficient, when the resin is made into expandable resin particles, the speed at which the foaming agent escapes from the expandable resin particles may increase, and the foaming agent may not contribute to foaming easily, which may affect the foamability or the closed cell ratio.

[0053] The conditions for melt-kneading the above components can be appropriately set depending on the types and contents of the vinyl chloride resin, additives, and foaming agent.

[0054] In a preferred embodiment of the present manufacturing method, the molten mixture of vinyl chloride resin containing a blowing agent prepared by the melt kneading is extruded from a plurality of holes in a die at a resin temperature of 150-250°C into pressurized circulating water at a temperature of 60-100°C, cut by a rotary cutter adjacent to the die immediately after extrusion, and cooled and solidified by the pressurized circulating water to obtain expandable vinyl chloride resin particles. Furthermore, the particle weight of the expandable vinyl chloride resin particles is 2.5-7.0 mg / particle. Furthermore, the water pressure of the pressurized circulating water is 1.0-1.5 MPa. By satisfying these conditions, the expandable vinyl chloride resin particles obtained can achieve a high expansion ratio and have a good shape.

[0055] The resin temperature here refers to the resin temperature of the resin melt at the tip of the extruder, and is a value measured by a temperature sensor attached to the tip of the extruder. When two or more extruders are attached upstream of the die, the tip temperature of the most downstream extruder is taken as the resin temperature of the resin melt at the tip of the extruder. The lower limit of the resin temperature is preferably 155°C, more preferably 160°C. On the other hand, the upper limit is preferably 240°C, more preferably 220°C, even more preferably 210°C, and particularly preferably 200°C. If the resin temperature is 150°C or higher, the viscosity of the extruded molten kneaded product is low, small hole clogging is unlikely to occur, and the actual small hole opening rate is not reduced, so the shape of the obtained expandable polyvinyl chloride resin particles is less likely to be distorted or irregular. On the other hand, if the resin temperature is 250°C or lower, there is no risk of decomposition of the polyvinyl chloride resin and additives, and in addition, the extruded molten resin is easily solidified, so it is unlikely to be wrapped around the rotary cutter, and can be cut stably. In this specification, the "molten resin at the tip of the extruder" is referred to as the "molten kneaded product."

[0056] The die is not particularly limited as long as it has multiple holes, but from the viewpoint of suppressing pressure rise, for example, the hole size (hereinafter sometimes referred to as diameter) is preferably 0.3 mm to 2.0 mm, more preferably 0.4 mm to 1.5 mm, and even more preferably 0.7 to 1.2 mm.

[0057] In a preferred embodiment of the present manufacturing method, the tip pressure of the extruder attached upstream of the die is preferably 4 to 20 MPa, more preferably 6 to 18 MPa, and even more preferably 7 to 15 MPa. The extruder tip pressure is a value measured by a pressure sensor attached to the tip of the extruder. When two or more extruders are attached upstream of the die, the tip pressure of the most downstream extruder is taken as the tip pressure of the extruder. If the tip pressure of the extruder is 4 MPa or more, the foaming agent is easily dissolved and dispersed in the resin during melt kneading, and expandable vinyl chloride resin particles can be stably obtained. On the other hand, if the tip pressure of the extruder is 20 MPa or less, shear heat generation during melt kneading can be suppressed, and decomposition of the vinyl chloride resin and additives is less likely to occur.

[0058] The cutting device for cutting the molten resin extruded into the pressurized circulating water in this manufacturing method is not particularly limited, but examples include a device in which the molten resin is cut into small pellets by a rotating cutter that comes into contact with a die, and then transported to a centrifugal dehydrator without foaming in the pressurized circulating water, where it is dehydrated and aggregated.

[0059] In a preferred embodiment of the present production method, the temperature of the pressurized circulating water is within the range of 60 to 100° C. In order to further improve the expandability of the expandable vinyl chloride resin particles, the lower limit is preferably 70° C., more preferably 75° C., and even more preferably 80° C. On the other hand, the upper limit is preferably 97° C., more preferably 96° C., and even more preferably 95° C.

[0060] The pressure conditions of the pressurized circulating water can be appropriately adjusted depending on the types and contents of resin, additives, foaming agent, etc., but it is preferable to adjust the pressure so that the expansion ratio of the resulting expandable polyvinyl chloride resin particles is 1.0 to 1.25 times. The expansion ratio of the expandable polyvinyl chloride resin particles is determined based on the true density (kg / m) of the base resin. 3 ) is the true density (kg / m 3 The true density of the base resin and expandable polyvinyl chloride resin particles referred to here is calculated by dividing the weight W (kg) of polyvinyl chloride resin pellets or expandable polyvinyl chloride resin particles by the volume V (m 3 Although it depends on the type of foaming agent used, the pressure condition is preferably 0.6 to 2.0 MPa, more preferably 0.7 to 1.8 MPa, still more preferably 0.8 to 1.7 MPa, still more preferably 0.9 to 1.6 MPa, and particularly preferably 1.0 to 1.5 MPa, from the viewpoint of improving the shape of the expandable vinyl chloride resin particles, in particular reducing dents.

[0061] In this manufacturing method, the resin temperature of the molten mixture of the vinyl chloride resin containing the foaming agent and the temperature of the pressurized water are controlled, and the particle weight of the expandable vinyl chloride resin particles is controlled to 2.5 to 7.0 mg / particle, so that the expandable vinyl chloride resin obtained can achieve a high expansion ratio. The particle weight of the expandable vinyl chloride resin can be appropriately adjusted by the discharge amount per small hole of the die, the number of cutter blades, the cutter rotation speed, etc. The particle weight is preferably 2.8 to 7.0 mg / particle, more preferably 3.0 to 6.7 mg / particle, even more preferably 3.2 to 6.5 mg / particle, and particularly preferably 3.4 to 6.5 mg / particle.

[0062] The discharge rate per small hole of the die is preferably 0.4 to 5.0 kg / h. If it is 0.4 kg / h or more, clogging of the small holes due to solidification of the resin is easily prevented, and if it is 5.0 kg / h or less, there is no need to excessively increase the cutter rotation speed to adjust the grain weight, so cutter wear is reduced and productivity is excellent.

[0063] The number of cutter blades is preferably 2 to 10. By using 2 or more blades, there is no need to excessively increase the cutter rotation speed, which reduces cutter wear and provides excellent productivity, and by using 10 or less blades, the cutter rotation speed does not become too slow, which tends to make it easier to prevent problems such as the resin wrapping around the cutter.

[0064] The cutter rotation speed is preferably 600 to 5000 rpm. By setting it to 600 rpm or more, it becomes easier to prevent the resin from wrapping around the cutter and the generation of particles sticking to each other, and by setting it to 5000 rpm or less, wear on the cutter is reduced, resulting in excellent productivity.

[0065] The shape of the expandable polyvinyl chloride resin particles obtained by this manufacturing method may be a general granular object (for example, small rounded particles such as spherical, approximately spherical, convex lens, concave lens, spindle-shaped, etc.) as long as the shape of the expandable resin particles can be pre-expanded and foam-molded as described below, and may also be particles with indentations. In one embodiment of this manufacturing method, the shape of the expandable polyvinyl chloride resin particles is preferably spherical or approximately spherical. If the shape is spherical or approximately spherical, the specific surface area can be reduced and the escape of the foaming agent can be easily suppressed, and the pre-expanded particles are also likely to be spherical, which makes it easier to fill the mold during foam molding.

[0066] (Polyvinyl chloride resin foam particles and their manufacturing method) The expandable polyvinyl chloride resin particles obtained by this production method can be pre-expanded 2 to 110 times by a heating medium such as heated air or steam to become expanded polyvinyl chloride resin particles, which can then be used for a foamed molded article. The steam that can be used may be saturated steam or superheated steam.

[0067] The heating temperature during foaming should be appropriately adjusted depending on the glass transition temperature and melting point of the resin and the content of the foaming agent, but is preferably 90° C. or higher, and more preferably 100° C. or higher. On the other hand, from the viewpoint of suppressing the variation in expansion ratio among the foamed beads and preventing the shrinkage of the foamed beads, the heating temperature is preferably 150° C. or lower, and more preferably 130° C. or lower.

[0068] (Polyvinyl chloride resin foam molded product and its manufacturing method) The polyvinyl chloride resin foam particles are molded (e.g., molded in a mold) using a conventional molding machine, for example, with steam, to produce a polyvinyl chloride resin foam molded article. Depending on the shape of the mold used, a molded article with a complex shape or a block-like molded article can be obtained.

[0069] The vinyl chloride resin foam particles and the vinyl chloride resin foam molded article obtained by the present production method preferably have an average cell diameter of 70 to 1000 μm, more preferably 90 to 800 μm, and even more preferably 100 to 600 μm. By having an average cell diameter within the above-mentioned range, a vinyl chloride resin foam molded article with higher heat insulating properties can be obtained. When the average cell diameter is 70 μm or more, there is a tendency that the expansion ratio can be easily increased, and when it is 1000 μm or less, an increase in thermal conductivity, i.e., a deterioration in heat insulating performance can be avoided.

[0070] The vinyl chloride resin foamed beads and the vinyl chloride resin foamed molded articles obtained by this method preferably have a closed cell ratio of 70% or more, more preferably 80% or more, and even more preferably 90% or more. When the closed cell ratio is within the above-mentioned range, the foamed beads are easily expanded during molding, the foamed beads have good moldability, and the surface properties of the foamed molded articles obtained are improved. In addition, when the closed cell ratio is within the above-mentioned range, the strength of the foamed molded articles, such as the compressive strength, tends to be increased.

[0071] (Applications of foamed molded products) The foamed molded article made from the expandable polyvinyl chloride resin particles obtained by the present process has a high expansion ratio and excellent flame retardancy, and is therefore suitable for various applications such as building insulation, ceiling materials, core materials for metal sandwich panels, food container boxes, cold storage boxes, cushioning materials, agricultural and fishery boxes, bathroom insulation materials, and hot water tank insulation materials. EXAMPLES

[0072] Hereinafter, one embodiment of the present invention will be specifically described based on examples and comparative examples, but the present invention is not limited to these.

[0073] The measurement and evaluation methods in the following examples and comparative examples are as follows.

[0074] <Measurement of particle weight of expandable polyvinyl chloride resin particles> Using an electronic balance capable of measuring to the nearest 0.01 mg, the weight of 100 randomly sampled expandable polyvinyl chloride resin particles was measured, and the particle weight was calculated using the following formula. Grain weight (mg) = [Weight of 100 grains (mg)] / 100 <True density measurement of polyvinyl chloride resin pellets (base resin)> After blending polyvinyl chloride resin with auxiliary materials such as processing aids, stabilizers, and lubricants to obtain a uniform mixture, it is melted and kneaded in an extruder. The weight of the polyvinyl chloride resin pellets obtained, W3 (kg), is submerged in a measuring cylinder containing ethanol, and the volume V1 (m3) is calculated from the rise in the liquid level of the measuring cylinder (submersion method). 3 ) was calculated using the following formula: True density of polyvinyl chloride resin pellets (kg / m 3 )=(W3 / V1) The true density of the polyvinyl chloride resin pellets measured based on the above method was 1430 kg / m 3 This value was determined as the density of the base resin used in the present invention.

[0075] <Measurement of expansion ratio of polyvinyl chloride resin foam particles> A polyvinyl chloride resin foam particle with a weight of W4 (kg) is submerged in a measuring cylinder containing ethanol, and the volume V2 (m 3 ) was obtained and calculated using the following formula. From the above <Measurement of true density of polyvinyl chloride resin pellets (base resin)>, the base resin density was 1430 kg / m 3 was used. Expansion ratio of polyvinyl chloride resin foam particles (times) = 1430 / (W4 / V2)

[0076] <Evaluation of foaming of expandable polyvinyl chloride resin particles> The expansion ratio of the polyvinyl chloride resin particles obtained in the examples and comparative examples and the amount of the blowing agent (volatile matter) contained in the polyvinyl chloride resin particles were measured according to the following measurement method. Note that, in order to properly evaluate the expansion of the polyvinyl chloride resin particles, the following measurements were performed on the same day.

[0077] <Measurement of expansion ratio of polyvinyl chloride resin foam particles> A part of the obtained expandable polyvinyl chloride resin particles was put into an oven (forced convection constant temperature dryer SOFW-600, manufactured by AS ONE Corporation) heated to 130°C, and expanded under a heated air atmosphere at a temperature of 130°C by changing the heating time, to obtain expanded particles for each heating time. The heating time was changed at 30 second intervals, such as 30 seconds, 60 seconds, and 90 seconds after putting into the oven, and heating was continued until shrinkage of the expanded particles due to overheating (decrease in the expansion particle expansion ratio) was confirmed. The expansion ratio of the expanded particles obtained for each heating time was measured based on (measurement of expansion ratio of expanded polyvinyl chloride resin particles described above), and the highest expansion ratio among these was determined as the maximum expansion ratio of the expanded polyvinyl chloride resin particles.

[0078] <Measurement of the amount of blowing agent (volatile matter) contained in expandable polyvinyl chloride resin particles> The resulting expandable polyvinyl chloride resin particles were weighed out as W1 (g), heated in an oven at 150°C for 30 minutes, cooled in a desiccator at room temperature for 30 minutes, and then weighed again as W2 (g). The weight difference (W1-W2) before and after heating was taken as the foaming agent content in the expandable polyvinyl chloride resin particles. The volatile content was calculated using the following formula. Volatile content (wt%) = (W1-W2) / W1 x 100

[0079] Example 1 [Preparation of expandable polyvinyl chloride resin particles] To 100 parts by weight of chlorinated vinyl chloride polymer (Kaneka Corporation, H716S, average degree of polymerization 600, chlorine content 67.6% by weight), 10 parts by weight of acrylic resin (Kaneka Corporation, Kaneace PA-40), 5 parts by weight of butyltin mercapto stabilizer, 3 parts by weight of lubricant (ester wax, polyethylene wax), and 5 parts by weight of chlorinated polyethylene with a chlorine content of 35% by weight were added, and the mixture was blended to obtain a uniform mixture, which was then melt-kneaded in a co-rotating intermeshing twin screw extruder to obtain pellets with the above-mentioned blending ratio. The obtained pellets were melt-kneaded in a φ40mm co-rotating intermeshing twin screw extruder at a feed rate of 40 kg / hr. From the middle of the φ40mm co-rotating intermeshing twin screw extruder, 8.8 parts by weight of normal pentane (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.) and 3.8 parts by weight of acetone (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.) were pressed into 100 parts by weight of the pellets. After that, through a continuation pipe attached to the tip of the twin screw extruder, a single screw extruder, a gear pump, and a diverter valve, the pellets were extruded at a discharge rate of 45 kg / hr from a die set at 250°C having 30 small holes with a diameter of 1.0 mm and a land length of 3.5 mm attached downstream of the diverter valve, into pressurized circulating water at a temperature of 70°C and 1.3 MPa. At this time, the set temperature of the single screw extruder was 165°C, the tip pressure of the single screw extruder was 15 MPa, and the resin temperature of the melt (i.e., the resin temperature of the resin melt at the tip of the extruder) was 168°C. The extruded molten resin was cut and pelletized using a rotary cutter (number of blades: 3) in contact with the die at a cutter rotation speed of 1500 rpm, and transferred to a centrifugal dehydrator to obtain expandable polyvinyl chloride resin particles with a particle weight of 6.0 mg. The obtained expandable polyvinyl chloride resin particles had small dents and were of good shape.

[0080] [Evaluation of foaming of expandable polyvinyl chloride resin particles] The obtained expandable polyvinyl chloride resin particles were stored at 10°C for 2 days, and then the volatile content and expansion ratio of the expanded particles were measured according to the above-mentioned <Expansion Evaluation of Expandable Polyvinyl Chloride Resin Particles>. The volatile content was 8.9% by weight, and the maximum expansion ratio of the expanded particles was 21.7 times.

[0081] Example 2 Expandable polyvinyl chloride resin particles having a particle weight of 5.5 mg were obtained in the same manner as in Example 1, except that the temperature of the pressurized circulating water was changed from 70° C. to 80° C. The resin temperature of the molten material was 168° C.

[0082] The foaming evaluation of the expandable polyvinyl chloride resin particles was carried out in the same manner as in Example 1. The volatile content was 9.0% by weight, and the maximum expansion ratio of the expanded particles was 26.3 times. The obtained expandable polyvinyl chloride resin particles had few dents and a good shape.

[0083] Example 3 Expandable polyvinyl chloride resin particles with a particle weight of 5.3 mg were obtained in the same manner as in Example 1, except that the temperature of the pressurized circulating water was changed from 70° C. to 90° C. In accordance with the above change, however, the extruder tip pressure was 14 MPa. The resin temperature of the molten material was 167° C.

[0084] The foaming evaluation of the expandable polyvinyl chloride resin particles was carried out in the same manner as in Example 1. The volatile content was 9.0% by weight, and the maximum expansion ratio of the expanded particles was 26.7 times. The obtained expandable polyvinyl chloride resin particles had few dents and a good shape.

[0085] Example 4 In Example 1, expandable polyvinyl chloride resin particles with a particle weight of 5.3 mg were obtained in the same manner as in Example 1, except that the temperature of the pressurized circulating water was changed from 70°C to 95°C. However, due to the above change, the extruder tip pressure was 13 MPa. The resin temperature of the molten material was 167°C.

[0086] The foaming evaluation of the expandable polyvinyl chloride resin particles was carried out in the same manner as in Example 1. The volatile content was 9.0% by weight, and the maximum expansion ratio of the expanded particles was 27.1 times. The obtained expandable polyvinyl chloride resin particles had few dents and a good shape.

[0087] Example 5 In Example 1, the cutter rotation speed was changed from 1500 rpm to 2300 rpm, and the same procedure was followed to obtain expandable polyvinyl chloride resin particles with a particle weight of 3.5 mg. However, due to the above change, the extruder tip pressure was 16 MPa. The resin temperature of the molten material was 167°C.

[0088] The foaming evaluation of the expandable polyvinyl chloride resin particles was carried out in the same manner as in Example 1. The volatile content was 8.5% by weight, and the maximum expansion ratio of the expanded particles was 24.1 times. The obtained expandable polyvinyl chloride resin particles had few dents and a good shape.

[0089] Comparative Example 1 In Example 1, the temperature of the pressurized circulating water was changed from 70°C to 95°C, and the cutter rotation speed was changed from 1500 rpm to 3400 rpm, but the procedure was the same as in Example 1 to obtain expandable polyvinyl chloride resin particles with a particle weight of 2.3 mg. However, due to the above changes, the extruder tip pressure was 14 MPa. The resin temperature of the molten material was 167°C.

[0090] The foaming evaluation of the expandable polyvinyl chloride resin particles was carried out in the same manner as in Example 1. The volatile content was 7.9% by weight, and the maximum expansion ratio of the expanded particles was 18.2 times. The obtained expandable polyvinyl chloride resin particles had few dents and a good shape.

Claims

1. A method for producing expandable polyvinyl chloride resin particles that satisfy the following (a) and (b): (a) a molten mixture of a vinyl chloride resin containing a foaming agent, the mixture having a resin temperature of 150 to 250°C, is extruded from a die having a plurality of holes into pressurized water having a temperature of 60 to 100°C, and cut with a rotary cutter immediately after extrusion; (b) The particle weight of the expandable polyvinyl chloride resin particles is 2.5 to 7.0 mg / particle.

2. 2. The method for producing expandable polyvinyl chloride resin particles according to claim 1, wherein the water pressure in the pressurized water is 1.0 to 1.5 MPa.

3. 3. The method for producing expandable polyvinyl chloride resin particles according to claim 1, wherein the plurality of holes have a diameter of 0.7 to 1.2 mm.

4. The method for producing expandable vinyl chloride resin particles according to any one of claims 1 to 3, wherein the vinyl chloride resin comprises a chlorinated vinyl chloride polymer.

5. The method for producing expandable vinyl chloride resin particles according to any one of claims 1 to 4, wherein the vinyl chloride resin comprises a chlorinated vinyl chloride polymer having a chlorine content of 60% by weight or more and 75% by weight or less.

6. The method for producing expandable vinyl chloride resin particles according to any one of claims 1 to 5, wherein the foaming agent contains a saturated hydrocarbon having 4 to 6 carbon atoms.

7. 7. The method for producing expandable polyvinyl chloride resin particles according to claim 6, wherein at least one of the saturated hydrocarbons having 4 to 6 carbon atoms is pentane.

8. The method for producing expandable polyvinyl chloride resin particles according to any one of claims 1 to 7, wherein the foaming agent comprises a ketone.

9. The method for producing expandable vinyl chloride-based resin particles according to any one of claims 1 to 8, wherein the expandable vinyl chloride-based resin particles contain a vinyl chloride-based polymer and / or a chlorinated vinyl chloride-based polymer having an average degree of polymerization of 300 or more and 3,000 or less.

10. The method for producing expandable vinyl chloride-based resin particles according to any one of claims 1 to 9, wherein the expandable vinyl chloride-based resin particles contain a copolymer having an aromatic vinyl monomer and an unsaturated nitrile as structural units and / or an acrylic resin.

11. The method for producing expandable polyvinyl chloride resin particles according to any one of claims 1 to 10, wherein the expandable polyvinyl chloride resin particles contain chlorinated polyethylene.

12. A method for producing pre-expanded vinyl chloride resin particles, comprising a step of pre-expanding the expandable vinyl chloride resin particles obtained by the production method according to any one of claims 1 to 11.

13. A method for producing a polyvinyl chloride resin foam, comprising a step of in-mold foaming of the pre-expanded polyvinyl chloride resin particles obtained by the method according to claim 12.

Citation Information

Patent Citations

  • JP1972039360Y1

  • Chlorinated vinyl chloride resin composition pellet, preexpanded particle composed thereof and production thereof

    JP1990182735A

  • Production of expandable polymer particle

    JP1995196840A

  • Production of expandable thermoplastic resin particle

    JP1997221562A

  • Production method of particles of foaming thermoplastic resin

    JP2018172543A