Fiber-reinforced resin molding and method for producing same
A fiber-reinforced resin molded article with brominated bisphenol A type vinyl ester resin and organic peroxide achieves flame retardancy and moldability by controlling curing conditions, addressing the moldability issues of inorganic flame retardants.
Patent Information
- Application Number
- JP2021044617
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-18
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2041-03-18
AI Technical Summary
Fiber-reinforced resin molded articles with inorganic flame retardants suffer from increased viscosity and decreased moldability, limiting their practical application.
A fiber-reinforced resin molded article using a resin composition containing brominated bisphenol A type vinyl ester resin, a curing agent, and 0.5 to 4 parts by mass of organic peroxide, with a bromine content of 5.0% by volume or more, cured at a mold temperature of 65 to 300°C within 15 minutes.
The solution provides a fiber-reinforced resin molded article with flame retardancy and improved moldability, meeting V-0 UL94 standard performance and avoiding curing failures or defects.
Smart Images

Figure 0007572884000001 
Figure 0007572884000002 
Figure 0007572884000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a fiber-reinforced resin molded product, and more particularly to a fiber-reinforced resin molded product having flame retardancy and excellent moldability, and a method for producing the fiber-reinforced resin molded product. [Background technology]
[0002] Fiber-reinforced resin composite materials are lightweight and have high strength and rigidity, and therefore have a wide range of applications, from sports and leisure applications to industrial applications such as vehicles, aircraft, construction, civil engineering, etc. Some molded articles of such fiber-reinforced resin composite materials (hereinafter also referred to as "fiber-reinforced resin molded articles") are molded using a mold and have flame retardancy imparted by blending an inorganic flame retardant such as aluminum hydroxide into the resin composition (e.g., Patent Documents 1 to 3).
[0003] When an inorganic flame retardant is blended into a resin composition, the viscosity of the resin composition increases, and the moldability of a fiber-reinforced resin molded body using a mold decreases. In response to this problem, Patent Documents 1 to 3 disclose that the range of the thickness of the molded body is specified according to the blending amount of the inorganic flame retardant, inorganic flame retardant powders with different average particle sizes are blended, and an organic compound having flame retardancy is blended in a predetermined ratio with respect to the inorganic flame retardant. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2019-6852 A [Patent Document 2] Japanese Patent Application Publication No. 8-27355 [Patent Document 3] Japanese Patent Application Publication No. 6-270276 Summary of the Invention [Problem to be solved by the invention]
[0005] However, the inventors of the present invention have found through their investigations that the fiber-reinforced resin moldings disclosed in Patent Documents 1 to 3 have insufficient moldability because they contain an inorganic flame retardant.
[0006] The present invention has been made in consideration of such problems, and aims to provide a fiber-reinforced resin molding that has flame retardancy and good moldability, and a method for manufacturing such a fiber-reinforced resin molding. [Means for solving the problem]
[0007] As a result of extensive investigation, the present inventors have found that the above object can be achieved by the following configuration.
[0008] A fiber-reinforced resin molding according to one aspect of the present invention is a fiber-reinforced resin molding obtained by impregnating reinforcing fibers with a resin composition containing a brominated bisphenol A type vinyl ester resin and a curing agent, and curing the resin composition, which contains 0.5 to 4 parts by mass of an organic peroxide as the curing agent per 100 parts by mass of the brominated bisphenol A type vinyl ester resin, has a bromine content of 5.0 volume% or more in the fiber-reinforced resin molding, and has flame retardancy of V-0 according to the UL94 standard.
[0009] A method for producing a fiber-reinforced resin molded product according to another aspect of the present invention includes curing the resin composition impregnated into the reinforcing fibers at a mold temperature of 65 to 300°C within 15 minutes to obtain a molded product. Effect of the Invention
[0010] According to the present invention, it is possible to provide a fiber-reinforced resin molded article having flame retardancy and good moldability, and a method for producing such a fiber-reinforced resin molded article. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, a fiber reinforced resin molding according to one embodiment of the present invention will be described.
[0012] The fiber-reinforced resin molding according to this embodiment is a fiber-reinforced resin molding obtained by impregnating reinforcing fibers with a resin composition containing a brominated bisphenol A vinyl ester resin and a curing agent, and curing the resin composition. The resin composition contains 0.5 to 4 parts by mass of an organic peroxide as a curing agent per 100 parts by mass of the brominated bisphenol A vinyl ester resin, the bromine content in the fiber-reinforced resin molding is 5.0% by volume or more, and the fiber-reinforced resin molding has a flame retardancy of V-0 according to the UL94 standard.
[0013] Each component of the fiber-reinforced resin molding will be described below.
[0014] (Resin composition) The resin composition constituting the fiber-reinforced resin molded article according to this embodiment contains a brominated bisphenol A type vinyl ester resin and a curing agent.
[0015] (Brominated bisphenol A vinyl ester resin) The brominated bisphenol A vinyl ester resin may be a commercially available product, such as Lipoxy S-510 (manufactured by Showa Denko K.K.), Neopol 8197 (manufactured by Nippon U-Pica Co., Ltd.), ETERSET 2967 (Etemal Materials Co., Ltd.), etc.
[0016] (hardening agent) The curing agent is contained in the resin composition in order to cure the brominated bisphenol A vinyl ester resin. The curing agent in this embodiment contains an organic peroxide.
[0017] In the resin composition, the content of the organic peroxide relative to 100 parts by mass of the brominated bisphenol A type vinyl ester resin (hereinafter simply referred to as the "content of the organic peroxide") is 0.5 to 4 parts by mass. By making the content of the organic peroxide 0.5 parts by mass or more, it is possible to suppress the occurrence of poor curing of the resin composition. Furthermore, by making the content of the organic peroxide 4 parts by mass or less, it is possible to suppress the occurrence of molding defects such as cracks in the fiber reinforced resin molding. The content of the organic peroxide is preferably 1.0 part by mass or more, more preferably 2.0 parts by mass or more. Furthermore, the content of the organic peroxide is preferably 4.0 parts by mass or less, more preferably 3.0 parts by mass or less.
[0018] As the organic peroxide, peroxy esters, peroxy carbonates, hydroperoxy esters, diacyl peroxides, peroxy ketals, peroxy dicarbonates, etc. can be used. One of these may be used, but it is preferable to use two or more of them in order to adjust the reaction time.
[0019] In this embodiment, the organic peroxide is preferably at least one selected from the group consisting of peroxyesters, peroxycarbonates, hydroperoxyesters, and diacyl peroxides. In addition, the peroxyesters and peroxycarbonates constituting the group of organic peroxides preferably have a t-amyl group or a t-butyl group.
[0020] The resin composition according to the present embodiment may contain a curing agent other than the organic peroxide.
[0021] (Other Ingredients) The resin composition according to this embodiment may contain additives such as a release agent in addition to the brominated bisphenol A type vinyl ester resin and the curing agent.
[0022] The release agent is not particularly limited, and examples thereof include known internal release agents such as fatty acid esters, for example, phosphoric acid ester derivatives, fatty acid metal salts such as zinc stearate, and surfactants such as sodium dialkylsulfosuccinate. These release agents may be used alone or in combination. Commercially available release agents may be used, such as MoldWiz (registered trademark) INT-PUL-24, INT-PUL34, INT-1846N2, INT-524M, INT-542WT, and INT-PS125 (manufactured by Axel Plastics Research Laboratories). The content of the release agent relative to 100 parts by mass of the brominated bisphenol A type vinyl ester resin is preferably 0.1 parts by mass or more, and more preferably 0.5 parts by mass or more. The content of the release agent is preferably 3.0 parts by mass or less, and more preferably 2.5 parts by mass or less.
[0023] As additives other than the mold release agent, a filler, a pigment, a curing accelerator, an ultraviolet absorber, an antioxidant, etc. can be used.
[0024] (Reinforced Fiber) The reinforcing fibers are intended to reinforce the fiber-reinforced resin molded body. By impregnating the reinforcing fibers with the above-mentioned resin composition and curing the same, the reinforcing fibers and the resin composition are integrated to reinforce the fiber-reinforced resin molded body.
[0025] The reinforcing fibers are not particularly limited, but are known as reinforcing fibers that constitute fiber-reinforced resin molded bodies, and are selected appropriately depending on the application, etc., so that when the fiber-reinforced resin molded body is formed, the resin molded body satisfies the flame retardant performance described below.
[0026] Specific examples of reinforcing fibers include various fibers such as carbon fiber, glass fiber, boron fiber, alumina fiber, silicon nitride fiber, and basalt fiber. Two or more of these fibers may be used in combination. Among these fibers, carbon fiber, glass fiber, boron fiber, alumina fiber, and silicon nitride fiber are preferred from the viewpoint of specific strength and specific elasticity. Furthermore, carbon fiber is more preferred because it can further improve the strength and corrosion resistance of the fiber-reinforced resin molded body.
[0027] As the carbon fiber, it is preferable to use PAN (polyacrylonitrile)-based carbon fiber, which has particularly high strength. When using carbon fiber as the reinforcing fiber, the carbon fiber may be subjected to a surface treatment with a metal.
[0028] In the fiber reinforced resin molded body according to the present embodiment, the volume fraction Vf of the reinforcing fibers relative to the entire fiber reinforced resin molded body is preferably 50% or more and 80% or less. By setting the volume fraction Vf of the reinforcing fibers to 50% or more, the fiber reinforced resin molded body is sufficiently reinforced by the reinforcing fibers, so that a fiber reinforced resin molded body having superior strength, particularly superior tensile strength, can be obtained. On the other hand, by setting the volume fraction Vf of the reinforcing fibers to 80% or less, the molding processability of the fiber reinforced resin molded body made of vinyl ester resin can be maintained better. The volume fraction Vf of the reinforcing fibers is more preferably 55% or more. Moreover, the volume fraction Vf of the reinforcing fibers is more preferably 75% or less.
[0029] The volume fraction Vf of the reinforcing fibers in the fiber-reinforced resin molded product can be adjusted within the above range by appropriately controlling not only the type and thickness of the reinforcing fibers but also the temperature and pressure applied during the production of the fiber-reinforced resin molded product. The volume fraction Vf of the reinforcing fibers can be measured by a combustion method, a nitric acid decomposition method, a sulfuric acid decomposition method, etc., but the volume fraction Vf (volume %) of the reinforcing fibers in this specification is calculated based on the following formula (1).
[0030] Vf=(Tf / ρf) / (1000×H)×100…(1) In formula (1), Tf: 1m of the base material of the reinforcing fiber used in the fiber-reinforced resin molding 2 Mass per unit (g / m 2 ), ρf: density of the fiber substrate used (g / cm 3 ), H: thickness of the fiber reinforced resin molding (mm).
[0031] (bromine content) The fiber reinforced resin molded body according to this embodiment has a bromine content of 5.0% by volume or more. This allows the fiber reinforced resin molded body to have excellent flame retardancy. The bromine volume content VBr (volume %) of the fiber reinforced resin molded body in this specification is calculated based on the following formula (2) using the bromine content of the resin constituting the fiber reinforced resin molded body.
[0032] VBr=(X / 100)×(1-Vf / 100)×(ρr / ρB)×100 …(2) In formula (2), X is the bromine content (mass%) of the resin constituting the fiber-reinforced resin molding, Vf is the reinforcing fiber content (volume%) of the fiber-reinforced resin molding, and ρr is the density of the resin (g / cm 3 ), ρB: density of bromine (g / cm 3 ).
[0033] The bromine content of the fiber reinforced resin molding is preferably 7.0% by volume or more. The bromine content of the fiber reinforced resin molding is preferably 15.0% by volume or less, more preferably 13.0% by volume or less. If the bromine content is less than 5.0% by volume, it is difficult to obtain sufficient flame retardancy. If the bromine content exceeds 15.0% by volume, the volume fraction Vf of the reinforcing fibers of the fiber reinforced resin molding may be 50% or less, which is not preferable.
[0034] The bromine content of the fiber-reinforced resin molding can be adjusted to the above range by adjusting the proportion of brominated bisphenol A vinyl ester resin in the fiber-reinforced resin molding, or by adjusting the content of brominated bisphenol A vinyl ester resin in the resin composition.
[0035] (Flame retardant performance) The fiber reinforced resin molding according to this embodiment has a flame retardancy of V-0 according to the UL 94 standard. The flame retardancy of the fiber reinforced resin molding can be adjusted by adjusting the proportion of the brominated bisphenol A vinyl ester resin in the fiber reinforced resin molding, or by adjusting the content of the brominated bisphenol A vinyl ester resin in the resin composition.
[0036] The flame retardancy performance of the fiber reinforced resin molding according to the present embodiment in accordance with the UL 94 standard is evaluated by a vertical combustion test in accordance with ASTM D 3801. A specific evaluation method will be described in the examples below.
[0037] (Shape, size, and use of fiber-reinforced resin molding) The fiber-reinforced resin molded product according to the present embodiment may have any shape and size, for example, a plate shape, a rod shape, etc. When it is rod-shaped, the cross-sectional shape may be rectangular, circular, hollow, L-shaped, V-shaped, H-shaped, U-shaped, etc., and may have any length. When the cross-sectional shape is rectangular, the dimensions are not particularly limited, but the thickness may be about 1 to 20 mm, and the width may be about 10 to 600 mm.
[0038] The fiber-reinforced resin molded article according to this embodiment can be used, for example, in sports and leisure equipment, vehicle and aircraft parts and structures, architectural structures, and civil engineering structures.
[0039] (Manufacturing method) The method for producing a fiber-reinforced resin molded product according to this embodiment includes curing the above-mentioned resin composition impregnated into the above-mentioned reinforcing fibers at a mold temperature of 65 to 300°C within 15 minutes to obtain a molded product.
[0040] According to the method for producing a fiber-reinforced resin molding according to this embodiment, by using the above-mentioned resin composition, the curing reaction can be completed within 15 minutes, and the fiber-reinforced resin molding can be produced quickly.
[0041] The method of impregnating the reinforcing fiber with the resin composition can be any method. For example, the bundle of reinforcing fibers may be immersed in a container containing the resin composition, or the bundle of reinforcing fibers may be coated with the resin composition. This impregnation may be repeated multiple times as necessary.
[0042] In addition, the mold that can be used is not particularly limited. For example, a die having a through hole through which a bundle of reinforcing fibers impregnated with a resin composition can pass, an injection molding die into which reinforcing fibers and resin fibers can be poured, or other molds can be used.
[0043] More specifically, the method for producing the fiber-reinforced resin molded article according to this embodiment can employ a pultrusion molding method or a VaRTM (Vacuum assisted Resin Transfer Molding) molding method.
[0044] The pultrusion molding method is a molding method in which a base material, reinforcing fiber, impregnated with a resin composition, is pulled into the inside of a mold, or reinforcing fiber is impregnated with a resin composition in the mold, the resin composition is heated and cured in the mold or when it leaves the mold, and the cured product is pulled out of the mold. When the manufacturing method according to this embodiment is applied to the pultrusion molding method, the mold temperature is set to 65 to 300°C. This allows the curing of the resin composition to be completed within 15 minutes after the reinforcing fiber impregnated with the resin composition enters the mold.
[0045] The VaRTM molding method is a molding method using a mold to which a plastic film is attached. The laminated reinforcing fibers are sealed between the mold and the plastic film, and the air between the mold and the plastic film is discharged by a vacuum pump. A resin composition is injected into the space from which the air has been discharged by utilizing negative pressure to impregnate the reinforcing fibers, and the reinforcing fibers and the resin composition are sandwiched between the mold and the plastic film and cured into a desired shape. When the manufacturing method according to this embodiment is applied to the VaRTM molding method, the mold temperature (mold temperature) is set to 65 to 300°C. In addition, the curing of the resin composition is completed within 15 minutes after the reinforcing fibers are impregnated with the resin composition.
[0046] As described above, this specification discloses various aspects of the technology, the main technologies of which are summarized below.
[0047] As described above, a fiber-reinforced resin molding according to one aspect of the present invention is a fiber-reinforced resin molding obtained by impregnating reinforcing fibers with a resin composition containing a brominated bisphenol A type vinyl ester resin and a curing agent and curing the resin composition, the resin composition containing 0.5 to 4 parts by mass of an organic peroxide as the curing agent per 100 parts by mass of the brominated bisphenol A type vinyl ester resin, the bromine content in the fiber-reinforced resin molding being 5.0% by volume or more, and the fiber-reinforced resin molding having a flame retardancy of V-0 according to the UL94 standard.
[0048] According to this configuration, it is possible to obtain a fiber-reinforced resin molding having flame retardancy and good moldability.
[0049] In the fiber-reinforced resin molding having the above configuration, the organic peroxide may be at least one selected from the group consisting of peroxy esters, peroxy carbonates, hydroperoxy esters, and diacyl peroxides.
[0050] According to this configuration, a fiber-reinforced resin molding having better moldability can be obtained.
[0051] In the fiber-reinforced resin molding having the above configuration, the peroxy ester and the peroxy carbonate may have a t-amyl group or a t-butyl group.
[0052] According to this configuration, a fiber-reinforced resin molding having even better moldability can be obtained.
[0053] A method for producing a fiber-reinforced resin molded product according to another aspect of the present invention is the method for producing the fiber-reinforced resin molded product described above, which includes curing the resin composition impregnated into the reinforcing fibers at a mold temperature of 65 to 300°C within 15 minutes to obtain a molded product.
[0054] According to this configuration, it is possible to produce a fiber-reinforced resin molding that has flame retardancy and good moldability.
[0055] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples, and may be modified within the scope of the above and below-described aims, and all such modifications are included in the technical scope of the present invention. EXAMPLES
[0056] <Production conditions of fiber reinforced resin molded body> The fiber-reinforced resin molded articles of Examples 1 to 9 and Comparative Examples 1 and 2 were produced under the following conditions.
[0057] Example 1 In order to prepare a fiber-reinforced resin molded body, a resin composition containing 100 parts by mass of brominated bisphenol A vinyl ester (manufactured by Showa Denko K.K., "Lipoxy (registered trademark) S-510"), 0.5 parts by mass of t-amylperoxy-2-ethylhexanoate (manufactured by Kayaku Nouryon Co., Ltd., "Trigonox (registered trademark) 121-50E"), and 0.5 parts by mass of "MoldWiz (registered trademark) INT-PUL-24" (manufactured by Axel Plastics Research Laboratories) was prepared. In Tables 1 and 2, the brominated bisphenol A vinyl ester is described as "resin", the t-amylperoxy-2-ethylhexanoate as "curing agent 1", and MoldWiz (registered trademark) INT-PUL-24 as "mold release agent".
[0058] As the reinforcing fiber, carbon fiber (manufactured by Toray Industries, Inc., "TORAYCA (registered trademark)", grade: T-700S, fiber diameter 7 μm, fineness: 1650 tex) was used.
[0059] The prepared resin composition was impregnated into the reinforcing fibers, and the resin composition and the reinforcing fibers were filled into a mold and held for a predetermined time. The resin composition was cured and then pulled out to produce a fiber-reinforced resin molded body (pultrusion molding method). The mold temperature was 180°C, and the holding time in the mold was 5 minutes. The cross-sectional shape of the fiber-reinforced resin molded body was rectangular, and the cross-sectional dimensions were 2 mm long and 30 mm wide.
[0060] The volume fraction Vf of the reinforcing fibers in the produced fiber-reinforced resin molding was 70%, and the volume fraction VBr of bromine was 8.0%. The volume fraction Vf of the reinforcing fibers was calculated based on the above formula (1), and the volume fraction VBr of bromine was calculated based on the above formula (2).
[0061] Example 2 In Example 2, the resin composition used was the same as that used in Example 1 except that the content of t-amylperoxy-2-ethylhexanoate (curing agent 1) was changed to 2 parts by mass. The volume fraction Vf of the reinforcing fibers in the produced fiber-reinforced resin molding was 60%, and the volume fraction VBr of bromine was 10.4%.
[0062] Example 3 In Example 3, the resin composition used was the same as that used in Example 1 except that the content of t-amylperoxy-2-ethylhexanoate (curing agent 1) was changed to 4 parts by mass. The volume fraction Vf of the reinforcing fibers in the produced fiber-reinforced resin molding was 55%, and the volume fraction VBr of bromine was 11.4%.
[0063] (Examples 4 to 6) In Examples 4 to 6, the resin composition used was the same as that used in Examples 1 to 3, except that t-amylperoxy-2-ethylhexanoate (curing agent 1) was replaced with t-amylperoxyisopropyl carbonate (manufactured by Nouryon Chemical Industries, Ltd., "Trigonox (registered trademark) 129-75"). In Tables 1 and 2, t-amylperoxyisopropyl carbonate is described as "curing agent 2".
[0064] Example 7 In Example 7, 2 parts by mass of t-amylperoxy-2-ethylhexanoate (curing agent 1) in the resin composition of Example 2 was replaced with 1 part by mass of t-amylperoxy-2-ethylhexanoate (curing agent 1) and 1 part by mass of t-amylperoxyisopropyl carbonate (curing agent 2).
[0065] (Examples 8 and 9) In Examples 8 and 9, the carbon fiber in Example 7 was replaced with glass fiber or basalt fiber, respectively, as the reinforcing fiber. The glass fiber was a glass roving material "RS 440 RR-520" manufactured by Nitto Boseki Co., Ltd., with a fiber diameter of 10 to 13 μm and a fineness of 4400 tex. The basalt fiber was "BCR16-4800" manufactured by HG GBF Basalt Fiber Co., Ltd., with a fiber diameter of 16 μm and a fineness of 4800 tex.
[0066] Comparative Example 1 In Comparative Example 1, the resin composition used was the same as in Example 1 except that the content of t-amylperoxy-2-ethylhexanoate (curing agent 1) was changed to 0.3 parts by mass. The volume fraction Vf of the reinforcing fibers in the fiber-reinforced resin molding was 60%, and the volume fraction VBr of bromine was 10.6%.
[0067] Comparative Example 2 In Comparative Example 2, the resin composition used was the same as that in Example 1 except that the content of t-amylperoxy-2-ethylhexanoate (curing agent 1) was changed to 5 parts by mass. The volume content Vf of the reinforcing fibers in the fiber-reinforced resin molding was 60%, and the volume content VBr of bromine was 10.0%.
[0068] [Table 1]
[0069] [Table 2]
[0070] Evaluation Test The flame retardancy and moldability of these fiber-reinforced resin moldings were evaluated according to the UL94 standard.
[0071] (Method of evaluating flame retardant performance) The flame retardant performance was evaluated by a vertical combustion test conforming to ASTM D3801. The samples used in the combustion test were cut out from the prepared fiber-reinforced resin moldings. The dimensions of the samples were 125±5 mm in length, 13.0±0.5 mm in width, and 2 mm in thickness. The standard thickness of the samples is 0.025 mm to 13 mm.
[0072] The sample was held with a clamp so that the longitudinal direction of the sample was vertical, and cotton of a specified dimension was placed below the sample. A 20 mm long flame was applied to the bottom end of the sample for 10 seconds (first flame application), and the afterflame time t1 was measured. After the combustion stopped, the flame was applied again for 10 seconds (second flame application), and the afterflame time t2 and afterglow time (time the sample was red hot) t3 were measured. In addition, it was confirmed whether the cotton had ignited due to dripping from the sample, and whether the sample had burned up to the clamp. The above tests were carried out on five samples, and the results of each item were combined to evaluate the flame retardancy of the samples, as shown in Table 3.
[0073] [Table 3]
[0074] (Method of evaluating moldability) The surface of the produced fiber-reinforced resin molded body was visually observed to check for the occurrence of defects such as cracks. If no defects were found, the moldability of the fiber-reinforced resin molded body was evaluated as good, and if defects were found, the moldability of the fiber-reinforced resin molded body was evaluated as not good.
[0075] Evaluation Results As shown in Tables 1 and 2, the fiber reinforced resin moldings (Examples 1 to 9) that satisfied the requirements of the present invention had flame retardancy of V-0 according to the UL94 standard. In addition, the resin compositions all hardened within 15 minutes in the mold, and the surfaces of the molded fiber reinforced resin moldings were free of defects such as cracks and had good moldability.
[0076] On the other hand, as shown in Table 2, in Comparative Example 1 in which the content of the curing agent was less than that specified in the present invention, the resin composition did not harden even after 15 minutes in the mold, so that a fiber-reinforced resin molding could not be molded and the flame retardant performance could not be evaluated.
[0077] In Comparative Example 2, in which the content of the curing agent was higher than that specified in the present invention, the resin composition cured within 15 minutes in the mold, but cracks occurred on the surface of the fiber-reinforced resin molding, and the moldability was poor. The fiber-reinforced resin molding of Comparative Example 2 had a flame retardancy of V-0 according to the UL94 standard.
Claims
1. A fiber-reinforced resin molding is obtained by impregnating a reinforcing fiber with a resin composition containing a brominated bisphenol A vinyl ester resin and a curing agent, and curing the resin composition. The resin composition contains 0.5 to 4 parts by mass of an organic peroxide having a t-amyl group as the curing agent relative to 100 parts by mass of the brominated bisphenol A vinyl ester resin, The bromine content in the fiber reinforced resin molded body is 5.0% by volume or more and 13.0% by volume or less, The volume fraction Vf of the reinforcing fibers is 55% or more and 80% or less, A fiber-reinforced resin molding having flame retardancy of V-0 according to the UL94 standard.
2. The fiber-reinforced resin molding according to claim 1, wherein the organic peroxide is at least one selected from the group consisting of peroxy esters, peroxy carbonates, hydroperoxy esters, and diacyl peroxides.
3. The method for producing a fiber-reinforced resin molded body according to claim 1 or 2, comprising curing the resin composition impregnated into the reinforcing fibers at a mold temperature of 65 to 300 ° C. within 15 minutes to obtain a molded body.
4. A method for producing a fiber-reinforced resin molding as described in claim 3, applying a pultrusion molding method.
Citation Information
Patent Citations
Production of fiber reinforced synthetic resin molded object
JP1994270276A
Flame retardant fiber-reinforced plastic molding or molding composition
JP1996027355A
Electrical metallic foil-plated laminated sheet
JP2004009584A
Fiber reinforced composite molding and its manufacturing method
JP2012106460A
Resin diffusion medium and method of manufacturing the same and method of manufacturing fiber reinforced plastic molded body
JP2013216017A