Fiber-reinforced resin molding and method for producing same

A resin composition with brominated bisphenol A epoxy resin and controlled acid anhydride content addresses moldability issues in fiber-reinforced resin molded articles, ensuring flame retardancy and effective fiber reinforcement.

JP7572898B2Active Publication Date: 2024-10-24FUKUBI KAGAKU IND
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021062947
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-04-01
Publication Date
2024-10-24
Estimated Expiration
2041-04-01

AI Technical Summary

Technical Problem

Fiber-reinforced resin molded articles with inorganic flame retardants suffer from increased viscosity, leading to decreased moldability.

Method used

A resin composition containing brominated bisphenol A epoxy resin, epoxy diluent, and a curing agent, with a specific ratio of acid anhydride and controlled viscosity, is used to impregnate reinforcing fibers, achieving a bromine content of 1.7% by volume and V-0 flame retardancy within 15 minutes at 65 to 300°C.

Benefits of technology

The solution results in a fiber-reinforced resin molded article with excellent flame retardancy and moldability, maintaining the integrity of the resin composition and fiber reinforcement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572898000001
    Figure 0007572898000001
  • Figure 0007572898000002
    Figure 0007572898000002
  • Figure 0007572898000003
    Figure 0007572898000003
Patent Text Reader

Abstract

To provide a fiber-reinforced resin molding which has flame retardancy and good moldability.SOLUTION: A fiber-reinforced resin molding is obtained by impregnating a reinforced fiber with a resin composition containing a brominated bisphenol A type epoxy resin, an epoxy diluent and a curing agent, and curing the resin composition, wherein the resin composition contains 50-90 pts.mass of an acid anhydride as the curing agent with respect to 100 pts.mass of the total of the brominated bisphenol A type epoxy resin and the epoxy diluent, and has viscosity of 10 dP s (25°C) or less, and a percentage content of bromine of the fiber-reinforced resin molding is 1.7 vol.% or more, and the fiber-reinforced resin molding has a V-0 flame-retardant performance in UL-94 standard.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fiber-reinforced resin molded product, and more particularly to a fiber-reinforced resin molded product having flame retardancy and excellent moldability, and a method for producing the fiber-reinforced resin molded product. [Background technology]

[0002] Fiber-reinforced resin composite materials are lightweight and have high strength and rigidity, and therefore have a wide range of applications, from sports and leisure applications to industrial applications such as vehicles, aircraft, construction, civil engineering, etc. Some molded articles of such fiber-reinforced resin composite materials (hereinafter also referred to as "fiber-reinforced resin molded articles") are molded using a mold and have flame retardancy imparted by blending an inorganic flame retardant such as aluminum hydroxide into the resin composition (e.g., Patent Documents 1 to 3).

[0003] When an inorganic flame retardant is blended into a resin composition, the viscosity of the resin composition increases, and the moldability of a fiber-reinforced resin molded body using a mold decreases. In response to this problem, Patent Documents 1 to 3 disclose that the range of the thickness of the molded body is specified according to the blending amount of the inorganic flame retardant, inorganic flame retardant powders with different average particle sizes are blended, and an organic compound having flame retardancy is blended in a predetermined ratio with respect to the inorganic flame retardant. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2019-6852 A [Patent Document 2] Japanese Patent Application Publication No. 8-27355 [Patent Document 3] Japanese Patent Application Publication No. 6-270276 Summary of the Invention [Problem to be solved by the invention]

[0005] However, the inventors of the present invention have found through their investigations that the fiber-reinforced resin moldings disclosed in Patent Documents 1 to 3 have insufficient moldability because they contain an inorganic flame retardant.

[0006] The present invention has been made in consideration of such problems, and aims to provide a fiber-reinforced resin molding that has flame retardancy and good moldability, and a method for manufacturing such a fiber-reinforced resin molding. [Means for solving the problem]

[0007] As a result of extensive investigation, the present inventors have found that the above object can be achieved by the following configuration.

[0008] A fiber-reinforced resin molding according to one aspect of the present invention is a fiber-reinforced resin molding obtained by impregnating reinforcing fibers with a resin composition containing a brominated bisphenol A type epoxy resin, an epoxy diluent, and a curing agent, and curing the resin composition, the resin composition containing 50 to 90 parts by mass of an acid anhydride as the curing agent per 100 parts by mass in total of the brominated bisphenol A type epoxy resin and the epoxy diluent, having a viscosity of 10 dPa s (25°C) or less, a bromine content of the fiber-reinforced resin molding of 1.7% by volume or more, and having a flame retardancy of V-0 according to the UL94 standard.

[0009] A method for producing a fiber-reinforced resin molded product according to another aspect of the present invention includes curing the resin composition impregnated into the reinforcing fibers at a mold temperature of 65 to 300°C within 15 minutes to obtain a molded product. Effect of the Invention

[0010] According to the present invention, it is possible to provide a fiber-reinforced resin molded article having flame retardancy and good moldability, and a method for producing such a fiber-reinforced resin molded article. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, a fiber reinforced resin molding according to one embodiment of the present invention will be described.

[0012] The fiber-reinforced resin molding according to this embodiment is a fiber-reinforced resin molding obtained by impregnating reinforcing fibers with a resin composition containing a brominated bisphenol A type epoxy resin, an epoxy diluent, and a curing agent, and curing the resin composition. The resin composition contains 50 to 90 parts by mass of an acid anhydride as the curing agent per 100 parts by mass of the total of the brominated bisphenol A type epoxy resin and the epoxy diluent, has a viscosity of 10 dPa s (25°C) or less, has a bromine content of 1.7% by volume or more, and has flame retardancy of V-0 according to the UL94 standard.

[0013] Each component of the fiber-reinforced resin molding will be described below.

[0014] (Resin composition) The resin composition constituting the fiber-reinforced resin molded article according to this embodiment contains a brominated bisphenol A type epoxy resin, an epoxy diluent, and a curing agent.

[0015] (Brominated bisphenol A epoxy resin) As the brominated bisphenol A type epoxy resin, for example, tetrabromobisphenol A and the like can be used.

[0016] (Epoxy Diluent) The epoxy diluent is added to the resin composition to dilute the brominated bisphenol A type epoxy resin and to give the resin composition an appropriate viscosity. In the resin composition, the ratio of the brominated bisphenol A type epoxy resin to the epoxy diluent is preferably 50:50 to 80:20. By setting the ratio of the brominated bisphenol A type epoxy resin to the epoxy diluent within the above range, a resin composition having good moldability can be obtained. If the ratio of the brominated bisphenol A type epoxy resin is less than the above range, the amount of bromine contained in the fiber-reinforced resin molding is small, and sufficient flame retardancy may not be exhibited. On the other hand, if the ratio of the brominated bisphenol A type epoxy resin is more than the above range, the viscosity of the resin composition becomes too high, making it difficult to impregnate the fiber substrate with the resin composition. The ratio of the brominated bisphenol A type epoxy resin to the epoxy diluent is more preferably 60:40 to 70:30.

[0017] The epoxy diluent is not particularly limited, but for example, a glycidyl ether compound, a glycidyl ester compound, etc. can be used, and a glycidyl ether compound is preferred. The glycidyl ether compound may be monofunctional, bifunctional, or trifunctional or more polyfunctional. The glycidyl ether compound may be neopentyl glycol diglycidyl ether, ethylene glycol diglycidyl ether, etc., and a neopentyl glycol diglycidyl ether is preferred.

[0018] (hardening agent) The curing agent is contained in the resin composition in order to cure the brominated bisphenol A type epoxy resin. The curing agent in this embodiment contains an acid anhydride.

[0019] In the resin composition, the content of the acid anhydride relative to 100 parts by mass of the brominated bisphenol A type epoxy resin (hereinafter also simply referred to as "acid anhydride content") is 50 to 90 parts by mass. By making the acid anhydride content 50 parts by mass or more, it is possible to suppress the occurrence of poor curing of the resin composition. Furthermore, by making the acid anhydride content 90 parts by mass or less, it is possible to suppress the occurrence of molding defects such as cracks in a fiber reinforced resin molded product. The acid anhydride content is preferably 55 parts by mass or more. Furthermore, the acid anhydride content is preferably 85 parts by mass or less.

[0020] The acid anhydride is not particularly limited, but for example, a phthalic anhydride compound, a maleic anhydride compound, etc. can be used, and a phthalic anhydride compound is preferable. For example, a phthalic anhydride compound can be used, such as methyltetrahydrophthalic anhydride, tetrahydrophthalic anhydride, endomethylenetetrahydrophthalic anhydride, hexahydrophthalic anhydride, etc., and a methyltetrahydrophthalic anhydride is preferable.

[0021] The resin composition according to the present embodiment may contain a curing agent other than the acid anhydride.

[0022] (Other Ingredients) The resin composition according to the present embodiment may contain additives such as a curing accelerator, a mold release agent, etc., in addition to the brominated bisphenol A type epoxy resin, the epoxy diluent, and the curing agent, and it is particularly preferable that the resin composition contains a curing accelerator.

[0023] As the curing accelerator, 1-cyanoethyl-2-ethyl-4-methylimidazole, 2-ethyl-4-methylimidazole, 2-phenyl-4-methylimidazole, etc. can be used. As the curing accelerator, a commercially available product may be used, for example, Curesol (registered trademark) 2E4MZ-CN (manufactured by Shikoku Chemical Industry Co., Ltd.), 2E4MZ (manufactured by Shikoku Chemical Industry Co., Ltd.), 2P4MZ (manufactured by Shikoku Chemical Industry Co., Ltd.), etc. may be used.

[0024] The release agent is not particularly limited, and examples thereof include known internal release agents such as fatty acid esters, for example, phosphoric acid ester derivatives, fatty acid metal salts such as zinc stearate, and surfactants such as sodium dialkyl sulfosuccinate. These release agents may be used alone or in combination. Commercially available release agents may be used, such as MoldWiz (registered trademark) INT-PUL-24, INT-PUL34, INT-1846N2, INT-524M, INT-542WT, and INT-PS125 (manufactured by Axel Plastics Research Laboratories). The content of the release agent relative to a total of 100 parts by mass of the brominated bisphenol A type epoxy resin and the epoxy diluent is preferably 0.1 parts by mass or more, and more preferably 0.5 parts by mass or more. The content of the release agent is preferably 5.0 parts by mass or less, and more preferably 4.0 parts by mass or less.

[0025] As additives other than the hardening accelerator and the mold release agent, a filler, a pigment, a hardening accelerator, an ultraviolet absorbing agent, an antioxidant, etc. can be used.

[0026] (viscosity) The resin composition according to the present embodiment has a viscosity of 10 dPa·s (25°C) or less. This allows a fiber-reinforced resin molded body to be reliably molded. The "(25°C)" added after the viscosity means that the viscosity is the viscosity of the resin composition at 25°C. Hereinafter, unless a temperature is specifically described for the viscosity of the resin composition, the viscosity at 25°C is meant. The viscosity of the resin composition is preferably 8 dPa·s or less. The viscosity of the resin composition is preferably 1 dPa·s or more, more preferably 3 dPa·s or more. If the viscosity of the resin composition exceeds 10 dPa·s, the resin composition cannot be impregnated into the reinforcing fibers, and a fiber-reinforced resin molded body may not be obtained. If the viscosity is less than 1 dPa·s, the resin composition impregnated into the reinforcing fibers may not be retained by the reinforcing fibers and may pass through the reinforcing fibers, and a fiber-reinforced resin molded body may not be obtained.

[0027] (Reinforced Fiber) The reinforcing fiber is for strengthening the fiber-reinforced resin molded body. By impregnating the reinforcing fiber with the above-mentioned resin composition and curing it, the reinforcing fiber and the resin composition are integrated, and the fiber-reinforced resin molded body can be strengthened. The reinforcing fiber is not particularly limited, but it is known as a reinforcing fiber that constitutes a fiber-reinforced resin molded body, and when the fiber-reinforced resin molded body is constituted, the fiber may be appropriately selected according to the application, etc. As specific examples of the reinforcing fiber, various fibers such as carbon fiber, glass fiber, boron fiber, alumina fiber, silicon nitride fiber, basalt fiber, etc. can be used. Two or more of these fibers may be appropriately combined and used. Among these fibers, from the viewpoint of specific strength and specific elasticity, carbon fiber, glass fiber, boron fiber, alumina fiber, and silicon nitride fiber are preferable. Furthermore, carbon fiber is more preferable because it can further improve the strength and corrosion resistance of the fiber-reinforced resin molded body. As the carbon fiber, PAN (polyacrylonitrile)-based carbon fiber and pitch-based carbon fiber can be used, and it is preferable to use PAN-based carbon fiber, which has particularly high strength. When carbon fibers are used as the reinforcing fibers, the carbon fibers may be subjected to a surface treatment with a metal.

[0028] In the fiber-reinforced resin molded body according to the present embodiment, the volume fraction Vf of the reinforcing fibers relative to the entire fiber-reinforced resin molded body is preferably 50% or more and 80% or less. By setting the volume fraction Vf of the reinforcing fibers to 50% or more, the fiber-reinforced resin molded body is sufficiently reinforced by the reinforcing fibers, so that a fiber-reinforced resin molded body having superior strength, particularly superior tensile strength, can be obtained. On the other hand, by setting the volume fraction Vf of the reinforcing fibers to 80% or less, the molding processability of the fiber-reinforced resin molded body made of epoxy resin can be maintained better. The volume fraction Vf of the reinforcing fibers is more preferably 55% or more. Moreover, the volume fraction Vf of the reinforcing fibers is more preferably 75% or less.

[0029] The volume fraction Vf of the reinforcing fibers in the fiber-reinforced resin molded product can be adjusted within the above range by appropriately controlling not only the type and thickness of the reinforcing fibers but also the temperature and pressure applied during the production of the fiber-reinforced resin molded product. The volume fraction Vf of the reinforcing fibers can be measured by a combustion method, a nitric acid decomposition method, a sulfuric acid decomposition method, etc., but the volume fraction Vf (volume %) of the reinforcing fibers in this specification is calculated based on the following formula (1).

[0030] Vf=(Tf / ρf) / (1000×H)×100…(1) In formula (1), Tf: 1m of the base material of the reinforcing fiber used in the fiber-reinforced resin molding 2 Mass per unit (g / m 2 ), ρf: density of the fiber substrate used (g / cm 3 ), H: thickness of the fiber reinforced resin molding (mm).

[0031] (bromine content) The fiber reinforced resin molded body according to this embodiment has a bromine content of 1.7% by volume or more. This allows the fiber reinforced resin molded body to have excellent flame retardancy. The bromine volume content VBr (volume %) of the fiber reinforced resin molded body in this specification is calculated based on the following formula (2) using the bromine content of the resin constituting the fiber reinforced resin molded body.

[0032] VBr=(X / 100)×(1-Vf / 100)×(ρr / ρB)×100 …(2) In formula (2), X is the bromine content (mass%) of the resin constituting the fiber-reinforced resin molding, Vf is the reinforcing fiber content (volume%) of the fiber-reinforced resin molding, and ρr is the density of the resin (g / cm 3 ), ρB: density of bromine (g / cm 3 ).

[0033] The bromine content of the fiber reinforced resin molding is preferably 2.0% by volume or more. The bromine content of the fiber reinforced resin molding is preferably 4.5% by volume or less, more preferably 4.0% by volume or less. If the bromine content is less than 1.7% by volume, it is difficult to obtain sufficient flame retardancy. If the bromine content exceeds 4.5% by volume, the viscosity of the resin composition exceeds 10 dPa·s, which is undesirable because it may become impossible to mold the resin composition.

[0034] The bromine content of the fiber-reinforced resin molding can be adjusted to the above range by adjusting the proportion of the brominated bisphenol A type epoxy resin in the fiber-reinforced resin molding, or by adjusting the content of the brominated bisphenol A type epoxy resin in the resin composition.

[0035] (Flame retardant performance) The fiber reinforced resin molding according to this embodiment has a flame retardancy of V-0 according to the UL 94 standard. The flame retardancy of the fiber reinforced resin molding can be adjusted by adjusting the proportion of the brominated bisphenol A vinyl ester resin in the fiber reinforced resin molding, or by adjusting the content of the brominated bisphenol A vinyl ester resin in the resin composition.

[0036] The flame retardancy performance of the fiber reinforced resin molding according to the present embodiment in accordance with the UL 94 standard is evaluated by a vertical combustion test in accordance with ASTM D 3801. A specific evaluation method will be described in the examples below.

[0037] (Shape, size, and use of fiber-reinforced resin molding) The fiber-reinforced resin molded product according to the present embodiment may have any shape and size, for example, a plate shape, a rod shape, etc. When it is rod-shaped, the cross-sectional shape may be rectangular, circular, hollow, L-shaped, V-shaped, H-shaped, U-shaped, etc., and may have any length. When the cross-sectional shape is rectangular, the dimensions are not particularly limited, but the thickness may be about 1 to 20 mm, and the width may be about 10 to 600 mm.

[0038] The fiber-reinforced resin molded article according to this embodiment can be used, for example, in sports and leisure equipment, vehicle and aircraft parts and structures, architectural structures, and civil engineering structures.

[0039] (Manufacturing method) The method for producing a fiber-reinforced resin molded product according to this embodiment includes curing the above-mentioned resin composition impregnated into the above-mentioned reinforcing fibers at a mold temperature of 65 to 300°C within 15 minutes to obtain a molded product.

[0040] According to the method for producing a fiber-reinforced resin molding according to this embodiment, by using the above-mentioned resin composition, the curing reaction can be completed within 15 minutes, and the fiber-reinforced resin molding can be produced quickly.

[0041] The method of impregnating the reinforcing fiber with the resin composition can be any method. For example, the bundle of reinforcing fibers may be immersed in a container containing the resin composition, or the bundle of reinforcing fibers may be coated with the resin composition. This impregnation may be repeated multiple times as necessary.

[0042] In addition, the mold that can be used is not particularly limited. For example, a die having a through hole through which a bundle of reinforcing fibers impregnated with a resin composition can pass, an injection molding die into which reinforcing fibers and resin fibers can be poured, or other molds can be used.

[0043] More specifically, the method for producing the fiber-reinforced resin molded article according to this embodiment can employ a pultrusion molding method or a VaRTM (Vacuum assisted Resin Transfer Molding) molding method.

[0044] The pultrusion molding method is a molding method in which a base material, reinforcing fiber, impregnated with a resin composition, is pulled into the inside of a mold, or reinforcing fiber is impregnated with a resin composition in the mold, the resin composition is heated and cured in the mold or when it leaves the mold, and the cured product is pulled out of the mold. When the manufacturing method according to this embodiment is applied to the pultrusion molding method, the mold temperature is set to 65 to 300°C. This allows the curing of the resin composition to be completed within 15 minutes after the reinforcing fiber impregnated with the resin composition enters the mold.

[0045] The VaRTM molding method is a molding method using a mold to which a plastic film is attached. The laminated reinforcing fibers are sealed between the mold and the plastic film, and the air between the mold and the plastic film is discharged by a vacuum pump. A resin composition is injected into the space from which the air has been discharged by utilizing negative pressure to impregnate the reinforcing fibers, and the reinforcing fibers and the resin composition are sandwiched between the mold and the plastic film and cured into a desired shape. When the manufacturing method according to this embodiment is applied to the VaRTM molding method, the mold temperature (mold temperature) is set to 65 to 300°C. In addition, the curing of the resin composition is completed within 15 minutes after the reinforcing fibers are impregnated with the resin composition.

[0046] As described above, this specification discloses various aspects of the technology, the main technologies of which are summarized below.

[0047] As described above, a fiber-reinforced resin molding according to one aspect of the present invention is a fiber-reinforced resin molding obtained by impregnating reinforcing fibers with a resin composition containing a brominated bisphenol A type epoxy resin, an epoxy diluent, and a curing agent, and curing the resin composition, the resin composition containing 50 to 90 parts by mass of an acid anhydride as the curing agent per 100 parts by mass of the total of the brominated bisphenol A type epoxy resin and the epoxy diluent, the resin composition having a viscosity of 10 dPa s (25°C) or less, the bromine content of the fiber-reinforced resin molding being 1.7% by volume or more, and the fiber-reinforced resin molding having a flame retardancy of V-0 according to the UL94 standard.

[0048] According to this configuration, it is possible to obtain a fiber-reinforced resin molding having flame retardancy and good moldability.

[0049] In the resin composition for the fiber-reinforced resin molded product having the above configuration, the ratio of the brominated bisphenol A type epoxy resin to the epoxy diluent may be 50:50 to 80:20.

[0050] According to this configuration, a fiber-reinforced resin molding having better moldability can be obtained.

[0051] In the fiber-reinforced resin molding having the above configuration, the acid anhydride may be a phthalic anhydride compound.

[0052] According to this configuration, a fiber-reinforced resin molding having even better moldability can be obtained.

[0053] In the fiber-reinforced resin molding having the above configuration, the epoxy diluent may be a glycidyl ether compound.

[0054] According to this configuration, a fiber-reinforced resin molding having even better moldability can be obtained.

[0055] The fiber-reinforced resin molding having the above configuration may further contain a curing accelerator, and the curing accelerator may be an imidazole-based compound.

[0056] According to this configuration, a fiber-reinforced resin molding having even better moldability can be obtained.

[0057] A method for producing a fiber-reinforced resin molded product according to another aspect of the present invention is the method for producing the fiber-reinforced resin molded product described above, which includes curing the resin composition impregnated into the reinforcing fibers at a mold temperature of 65 to 300°C within 15 minutes to obtain a molded product.

[0058] According to this configuration, it is possible to produce a fiber-reinforced resin molding that has flame retardancy and good moldability.

[0059] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples, and may be modified within the scope of the above and below-described aims, and all such modifications are included in the technical scope of the present invention. EXAMPLES

[0060] <Production conditions of fiber reinforced resin molded body> The fiber-reinforced resin molded articles of Examples 1 to 6 and Comparative Examples 1 and 2 were produced under the following conditions.

[0061] Example 1 To produce a fiber-reinforced resin molded body, a resin composition was prepared containing 50 parts by mass of tetrabromobisphenol A (DIC Corporation, "EPICLON (registered trademark) 153"), 50 parts by mass of neopentyl glycol diglycidyl ether, 80.1 parts by mass of methyltetrahydrophthalic anhydride, 2 parts by mass of 1-cyanoethyl-2-ethyl-4-methylimidazole (Shikoku Chemical Industry Co., Ltd., "Curesol (registered trademark) 2E4MZ-CN"), and 1 part by mass of "MoldWiz (registered trademark) INT-1846N2" ​​(Axel Plastics Research Laboratories). The viscosity of this resin composition at 25°C was 3.5 dPa·s. In Tables 1 and 2, tetrabromobisphenol A is listed as the "resin," neopentyl glycol diglycidyl ether as the "diluent," methyltetrahydrophthalic anhydride as the "curing agent," 1-cyanoethyl-2-ethyl-4-methylimidazole as the "curing accelerator," and "MoldWiz® INT-1846N2" ​​as the "mold release agent."

[0062] As the reinforcing fiber, carbon fiber (manufactured by Toray Industries, Inc., "TORAYCA (registered trademark)", grade: T-700S, fiber diameter 7 μm, fineness: 1650 tex) was used.

[0063] The prepared resin composition was impregnated into the reinforcing fibers, and the resin composition and the reinforcing fibers were filled into a mold and held for a predetermined time. The resin composition was cured and then pulled out to produce a fiber-reinforced resin molded body (pultrusion molding method). The mold temperature was 180°C, and the holding time in the mold was 5 minutes. The cross-sectional shape of the fiber-reinforced resin molded body was rectangular, and the cross-sectional dimensions were 2 mm long and 30 mm wide.

[0064] The volume fraction Vf of the reinforcing fibers in the produced fiber-reinforced resin molding was 66%, and the volume fraction VBr of bromine was 2.0%. The volume fraction Vf of the reinforcing fibers was calculated based on the above formula (1), and the volume fraction VBr of bromine was calculated based on the above formula (2).

[0065] Example 2 In Example 2, the resin composition used was the same as that used in Example 1 except that the content of tetrabromobisphenol A (resin) was 60 parts by mass, the content of neopentyl glycol diglycidyl ether (diluent) was 40 parts by mass, and the content of methyltetrahydrophthalic anhydride (curing agent) was 72.4 parts by mass. The viscosity of this resin composition at 25°C was 4 dPa s. The volume fraction Vf of the reinforcing fibers in the produced fiber-reinforced resin molding was 66%, and the volume fraction VBr of bromine was 2.6%.

[0066] Example 3 In Example 3, the resin composition used was the same as that used in Example 1 except that the content of tetrabromobisphenol A (resin) was changed to 70 parts by mass, the content of neopentyl glycol diglycidyl ether (diluent) to 30 parts by mass, and the content of methyltetrahydrophthalic anhydride (curing agent) to 64.7 parts by mass. The viscosity of this resin composition at 25°C was 5 dPa s. The volume fraction Vf of the reinforcing fibers in the produced fiber-reinforced resin molding was 66%, and the volume fraction VBr of bromine was 3.2%.

[0067] Example 4 In Example 4, the resin composition used was the same as that used in Example 1 except that the content of tetrabromobisphenol A (resin) was 80 parts by mass, the content of neopentyl glycol diglycidyl ether (diluent) was 20 parts by mass, and the content of methyltetrahydrophthalic anhydride (curing agent) was 56.9 parts by mass. The viscosity of this resin composition at 25°C was 7 dPa s. The volume fraction Vf of the reinforcing fibers in the produced fiber-reinforced resin molding was 66%, and the volume fraction VBr of bromine was 4.0%.

[0068] (Examples 5 and 6) In Examples 5 and 6, the carbon fiber in Example 2 was replaced with glass fiber or basalt fiber as the reinforcing fiber. The glass fiber was a glass roving material "RS 440 RR-520" manufactured by Nitto Boseki Co., Ltd., with a fiber diameter of 10 to 13 μm and a fineness of 4400 tex. The basalt fiber was "BCR16-4800" manufactured by HG GBF Basalt Fiber Co., Ltd., with a fiber diameter of 16 μm and a fineness of 4800 tex.

[0069] Comparative Example 1 In Comparative Example 1, the resin composition used was the same as that used in Example 1 except that the content of tetrabromobisphenol A (resin) was 40 parts by mass, the content of neopentyl glycol diglycidyl ether (diluent) was 60 parts by mass, and the content of methyltetrahydrophthalic anhydride (curing agent) was 87.9 parts by mass. The viscosity of this resin composition at 25°C was 3 dPa s. The volume fraction Vf of the reinforcing fibers in the produced fiber-reinforced resin molding was 70%, and the volume fraction VBr of bromine was 1.3%.

[0070] Comparative Example 2 In Comparative Example 2, the resin composition used was the same as that used in Example 1 except that the content of tetrabromobisphenol A (resin) was 90 parts by mass, the content of neopentyl glycol diglycidyl ether (diluent) was 10 parts by mass, and the content of methyltetrahydrophthalic anhydride (curing agent) was 49.2 parts by mass. The viscosity of this resin composition at 25°C was 12 dPa s. The volume fraction Vf of the reinforcing fibers in the produced fiber-reinforced resin molding was 66%, and the volume fraction VBr of bromine was 5.0%.

[0071] [Table 1]

[0072] [Table 2]

[0073] Evaluation Test The flame retardancy and moldability of these fiber-reinforced resin moldings were evaluated according to the UL94 standard.

[0074] (Method of evaluating flame retardant performance) The flame retardant performance was evaluated by a vertical combustion test conforming to ASTM D3801. The samples used in the combustion test were cut out from the prepared fiber-reinforced resin moldings. The dimensions of the samples were 125±5 mm in length, 13.0±0.5 mm in width, and 2 mm in thickness. The standard thickness of the samples is 0.025 mm to 13 mm.

[0075] The sample was held with a clamp so that the longitudinal direction of the sample was vertical, and cotton of a specified dimension was placed below the sample. A 20 mm long flame was applied to the bottom end of the sample for 10 seconds (first flame application), and the afterflame time t1 was measured. After the combustion stopped, the flame was applied again for 10 seconds (second flame application), and the afterflame time t2 and afterglow time (time the sample was red hot) t3 were measured. In addition, it was confirmed whether the cotton had ignited due to dripping from the sample, and whether the sample had burned up to the clamp. The above tests were carried out on five samples, and the results of each item were combined to evaluate the flame retardancy of the samples, as shown in Table 3.

[0076] [Table 3]

[0077] (Method of evaluating moldability) The surface of the produced fiber-reinforced resin molded body was visually observed to check for the occurrence of defects such as cracks. If no defects were found, the moldability of the fiber-reinforced resin molded body was evaluated as good, and if defects were found, the moldability of the fiber-reinforced resin molded body was evaluated as not good.

[0078] Evaluation Results As shown in Tables 1 and 2, the fiber reinforced resin moldings (Examples 1 to 6) that satisfied the requirements of the present invention had flame retardancy of V-0 according to the UL94 standard. In addition, the resin compositions all hardened within 15 minutes in the mold, and the surfaces of the molded fiber reinforced resin moldings were free of defects such as cracks and had good moldability.

[0079] On the other hand, as shown in Table 2, in Comparative Example 1 in which the bromine content of the fiber-reinforced resin molding was lower than the stipulated in the present invention, the flame retardancy was V-1 according to the UL94 standard, which was poor in flame retardancy.

[0080] In Comparative Example 2, in which the content of the curing agent (acid anhydride) was less than that specified in the present invention and the viscosity was lower than that specified in the present invention, the resin composition cured in a mold within 15 minutes, but the viscosity was too high to mold, and the flame retardant performance could not be evaluated.

Claims

1. A fiber-reinforced resin molding is obtained by impregnating a reinforcing fiber with a resin composition containing a brominated bisphenol A type epoxy resin, an epoxy diluent, and a curing agent, and curing the resin composition. the resin composition contains 50 to 90 parts by mass of an acid anhydride as the curing agent relative to 100 parts by mass of the total of the brominated bisphenol A type epoxy resin and the epoxy diluent, and has a viscosity of 10 dPa s (25° C.) or less; The bromine content of the fiber reinforced resin molded body is 1.7% by volume or more and 4.5% by volume or less, It has a flame retardant performance of V-0 according to the UL94 standard. In the resin composition, the ratio of the brominated bisphenol A type epoxy resin to the epoxy diluent is 50:50 to 80:20; The fiber-reinforced resin molding, wherein the epoxy diluent is a glycidyl ether compound.

2. The fiber-reinforced resin molding according to claim 1 , wherein the acid anhydride is a phthalic anhydride compound.

3. The resin composition further contains a curing accelerator, The fiber-reinforced resin molding according to claim 1 or 2, wherein the curing accelerator is an imidazole-based compound.

4. A fiber-reinforced resin molding described in any one of claims 1 to 3, wherein the volume content Vf of the reinforcing fibers relative to the entire fiber-reinforced resin molding is 50% or more and 80% or less.

5. The resin composition impregnated into the reinforcing fibers is cured at a mold temperature of 65 to 300 ° C. within 15 minutes to obtain a molded body. The method for producing a fiber-reinforced resin molded body according to any one of claims 1 to 4.

6. A method for producing a fiber-reinforced resin molding as described in claim 5, applying a pultrusion molding method.

Citation Information

Patent Citations

  • Flame-retardant liquid epoxy resin composition and manufacture of laminate sheet for electrical use therefrom

    JP1984170115A

  • Production of fiber reinforced synthetic resin molded object

    JP1994270276A

  • Flame retardant fiber-reinforced plastic molding or molding composition

    JP1996027355A

  • Fiber reinforced resin composite material

    JP2005239939A

  • Flame-retardant prepreg

    JP2006077202A