Flame retardant polysiloxane composition
Incorporating nano-sized ZnO particles into polysiloxane compositions addresses the challenge of achieving a V0 rating without high concentrations of traditional flame retardants, demonstrating effective flame retardancy and composition stability.
Patent Information
- Application Number
- JP2022527771
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-11-25
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2039-11-25
AI Technical Summary
Existing polysiloxane compositions struggle to achieve a V0 rating in the UL94 test without the need for high concentrations of halogenated flame retardants, metal hydrates, or intumescent components.
Incorporating 0.15 weight percent or more of zinc oxide (ZnO) particles with an average particle size less than 1 micrometer into the polysiloxane polymer composition provides sufficient flame retardant properties, enabling a V0 rating without the need for these additives.
The inclusion of nano-sized ZnO particles achieves a V0 rating in the UL94 test, reducing the reliance on traditional flame retardants and maintaining composition integrity.
Smart Images

Figure 0007573028000001 
Figure 0007573028000002 
Figure 0007573028000003
Abstract
Description
[Background technology]
[0001] FIELD OF THEINVENTION The present invention relates to polysiloxane compositions containing nano-sized zinc oxide particles that achieve a V0 rating in the UL94 test.
[0002] Introduction It is desirable to improve the flame retardant properties of polysiloxane compositions. In particular, it is desirable to have polysiloxane compositions that achieve a V0 rating in the UL94 test. Efforts to improve the flame retardant properties of polysiloxane compositions include the incorporation of intumescent components into the polysiloxane polymer composition, including halogenated flame retardants at loadings of 10 weight percent or more, metal hydrates at concentrations greater than 30 volume percent, transition metal complexes at loadings of at least 1 weight percent, or blends of binders, blowing agents, and acid sources (see, for example, Timpe, David C., Rubber and Plastics News, presentation at the 2007 Hose Manufacturers Conference, Cleveland, Ohio, June 11-12, 2007).
[0003] However, it would be an advancement in the art to identify an additive that can improve the flame retardant properties of a polysiloxane polymer composition sufficiently to achieve a V0 rating in UL94 testing without the need to add intumescent components or additives at the aforementioned concentrations. Summary of the Invention
[0004] The present invention provides a solution for achieving a V0 rating in UL94 testing of polysiloxane compositions without the need to add intumescent components, 10 weight percent (wt%) or more of halogenated flame retardants, 30 volume percent (vol%) or more of metal hydrates, or 1 wt% or more of transition metal complexes.
[0005] It has been surprisingly discovered that the inclusion of 0.15 weight percent or more of zinc oxide (ZnO) powder having an average particle size of less than 1 micrometer in a polysiloxane polymer composition provides sufficient flame retardant properties to the composition to enable it to achieve a V0 rating in UL94 testing without the need for intumescent compositions, 10 wt. % or more of halogenated flame retardants, 30 vol. % or more of metal hydrates, or 1 wt. % or more of transition metal complexes. In particular, it has been shown that other metal oxide powders cannot achieve the same effect as ZnO powder.
[0006] In a first aspect, the invention is a composition comprising: (a) a polysiloxane; and (b) zinc oxide particles dispersed in the polysiloxane, having an average particle size of less than 1 micrometer and greater than 1 nanometer, as determined as the volume weighted median of the particle size distribution using a laser diffraction particle size analyzer, greater than 0.15 weight percent and less than 85 weight percent, based on the weight of the composition.
[0007] The invention is useful, for example, in polysiloxane sealant and coating formulations, as well as encapsulants or gap fillers in electronic devices. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Test methods refer to the most recent test method as of the priority date of this document unless a date is given with the test method number. Reference to a test method includes both a reference to the testing society and the test method number. The following test method abbreviations and designations apply herein: ASTM refers to the American Society for Testing and Materials, EN refers to European Norm, DIN refers to the Deutsches Institut fur Normung, ISO refers to the International Organization for Standards, and UL refers to the Underwriters Laboratory.
[0009] Products identified by trade names refer to compositions available under those trade names as of October 1, 2019.
[0010] "Plurality" means two or more. "And / or" means "and, or alternatively." All ranges include endpoints unless otherwise indicated. All weight percents (wt%) are by composition weight and all volume percents (vol%) are by composition volume unless otherwise indicated. Unless otherwise indicated, molecular weights are number average molecular weights in Daltons measured by gel permeation chromatography using a tetrahydrofuran eluent at a flow rate of 1 milliliter / minute, a refractive index detector at 35°C, and 16 polystyrene narrow standards ranging in molecular weight from 580 Da to 2,300 Da, with 100 microliters of sample injected at a concentration of 15 milligrams / milliliter onto a Polymer Labs PLgel 5 micrometer guard column (50 millimeters x 7.5 millimeters) followed by two Polymer Labs PLgel 5 micrometer Mixed-C columns (300 millimeters x 7.5 millimeters). Viscosity is measured on a Brookfield DV-III cone-plate viscometer using a #CP-52 spindle at 25°C and 0.1-50 RPM.
[0011] The present invention is a composition that includes a polysiloxane and zinc oxide (ZnO) particles dispersed in the polysiloxane.
[0012] The ZnO particles are characterized by having an average particle size of less than 1 micrometer, preferably 0.90 micrometers or less, more preferably 0.80 micrometers or less, 0.70 micrometers or less, 0.60 micrometers or less, 0.50 micrometers or less, and may be 0.40 micrometers or less, 0.30 micrometers or less, 0.25 micrometers or less, 0.20 micrometers or less, 0.15 micrometers or less, and at the same time, have an average particle size of more than 1 nanometer, preferably 0.01 micrometers or more, 0.02 micrometers or more, 0.03 micrometers or more, 0.04 micrometers or more, 0.05 micrometers or more, or even 0.10 micrometers or more. The average particle size of the particles is measured herein as the volume-weighted median (D50) of the particle size distribution using a Mastersizer™ 3000 laser diffraction particle size analyzer manufactured by Malvern Instruments.
[0013] Surprisingly, it has been discovered that when ZnO particles have an average particle size of 1 micrometer or greater, they are dramatically less effective at imparting flame retardant properties to polysiloxane compositions than ZnO particles having smaller average particle sizes within the ranges specified in this invention. For practical purposes in handling and dispersion during formulation, it is desirable for the average particle size to be greater than 1 nanometer.
[0014] The ZnO particles may or may not be surface-treated. It may be desirable to use ZnO particles with a surface treatment that facilitates dispersion in the polysiloxane or polysiloxane precursor (in reactive systems). However, the flame retardant properties imparted by the ZnO particles do not require surface treatment of the ZnO particles. For example, the ZnO may be free of tetraalkoxysilanes and / or their partial hydrolysis-condensation products. Furthermore, the entire composition may be free of ZnO particles having a coating of tetraalkoxysilanes and / or their partial hydrolysis-condensation products. In fact, the composition may be free of tetraalkoxysilanes and / or their partial hydrolysis-condensation products.
[0015] The ZnO particles may be free of atoms other than zinc and oxygen, for example, the ZnO particles may be free of silicon dioxide (SiO) as is present in a ZnO2 / SiO2 composite particle.
[0016] The ZnO particles are present in the composition at a concentration of 0.15 wt% or more, and may be present at a concentration of 0.20 wt% or more, 0.25 wt% or more, 0.30 wt% or more, 0.40 wt% or more, 0.50 wt% or more, 0.60 wt% or more, 0.75 wt% or more, 1.0 wt% or more, 1.25 wt% or more, 1.50 wt% or more, 1.75 wt% or more, 2.0 wt% or more, 2.5 wt% or more, 3.0 wt% or more, 3.5 wt% or more, 4.0 wt% or more, or even 4.5 wt% or more. When the ZnO particles are present at a concentration of less than 0.15 wt%, they do not provide the silicone composition with sufficient flame retardant properties to enable the composition to achieve a rating of V0 in the UL94 test (in the absence of other flame retardants). Typically, the more ZnO present, the better the flame retardant performance, so there is no known upper limit to the amount of ZnO particles required to achieve a V0 rating in the UL94 test. In practice, the ZnO particles are present at one of the lower concentration limits described herein, while the ZnO particles are present at a concentration of 95 wt% or less, 90 wt% or less, 80 wt% or less, 70 wt% or less, 60 wt% or less, 50 wt% or less, 40 wt% or less, 30 wt% or less, 25 wt% or less, 20 wt% or less, 15 wt% or less, 10 wt% or less, 5 wt% or less, 4.5 wt% or less, 4.0 wt% or less, 3.5 wt% or less, 3.0 wt% or less, 2.5 wt% or less, 2.0 wt% or less, 1.5 wt% or less, or even 1.0 wt% or less. Wt% is by weight of the composition.
[0017] The ZnO particles are dispersed in a polysiloxane. A "polysiloxane" is a polymer that contains multiple siloxane units along its backbone. The siloxane units are typically (RSiO 1 / 2 ), "M-type" with the general structure (RSiO 2 / 2 ), "D-type" with the general structure (RSiO 3 / 2), and "T-type" with the general structure (SiO 4 / 2 ), the oxygen subscript indicates how many oxygen bonds are attached to the silicon atom, with the remainder of the bonds being attached to moieties other than the siloxane unit. Each "R" group is independently selected from hydrogen, and / or carbon-containing moieties, such as hydrogen, hydroxyl, hydrocarbyl groups (such as methyl and phenyl), substituted hydrocarbyl groups, alkoxy groups, and substituted alkoxy groups. Some typical R groups include hydrogen, methyl, and phenyl.
[0018] In the broadest anticipated scope of the present invention, the polysiloxane is not limited and includes any combination of siloxane units and constituents R on those siloxane units. The polysiloxane is desirably a reactive polysiloxane, meaning that the polysiloxane contains reactive groups such as silanols and / or carbon-carbon unsaturated groups (e.g., alkene or alkyne groups). For example, the polysiloxane may be a reactive polysiloxane containing any one or any combination of two or more functional groups selected from the group consisting of silanol groups, alkoxy groups, epoxy groups, groups containing carbon-carbon unsaturated bonds, and silyl hydride groups.
[0019] The polysiloxane may be part of a reactive system. Desirably, the polysiloxane is a reactive polysiloxane in a reactive system that includes a component that can react with the polysiloxane. A reactive system is a set of reactants that can undergo a chemical reaction to form a reaction product. For example, a reactive system may include a reactive polysiloxane that reacts with one or more other components to form a reaction product. Any one or more other components may also be polysiloxanes. ZnO may be dispersed in one or more polysiloxanes of a reactive system to form the composition of the present invention. The polysiloxane may also be a reaction product of the reactive system. When ZnO particles are dispersed in the polysiloxane of a reactive system, the ZnO particles are generally dispersed in the reaction product of the reactive system, which is also a polysiloxane. The present invention is particularly valuable in the form of reactive systems and reaction products of reactive systems for imparting flame retardant properties to caulkings, sealants, coatings, encapsulants, and adhesives which are polysiloxane reaction products of reactive systems, which themselves are reactive systems typically containing one or more polysiloxanes.
[0020] An example of a reactive system that can contain polysiloxanes and / or produce polysiloxane reaction products is a hydrosilylation reaction system that produces a hydrosilylation reaction product. A hydrosilylation reaction system includes a reactant (typically a reactive polysiloxane) with silyl hydride functionality and a reactant (the same or different reactive polysiloxane with silyl hydride functionality) with carbon-carbon unsaturated bonds (typically vinyl or allyl groups). The silyl hydride functionality typically reacts with the carbon-carbon unsaturated bond in the presence of a hydrosilylation catalyst to bond across the unsaturated bond. The reactant containing silyl hydride can be a polysiloxane and / or the reactant containing carbon-carbon unsaturated groups can be a polysiloxane. The ZnO particles described herein can be dispersed in either or both polysiloxane reactants to form compositions within the scope of the present invention. That is, the silyl hydride functional reactant may be a polysiloxane having ZnO particles dispersed therein as described herein at the concentrations described herein to form the compositions of the invention. Alternatively, or in addition, the reactant containing carbon-carbon unsaturated bonds may be a polysiloxane having ZnO particles dispersed therein as described herein at the concentrations described herein to form the compositions of the invention. When the hydrosilylation reaction system reacts to form a hydrosilylation reaction product that is a polysiloxane, if the reaction product has ZnO particles as described herein dispersed in the polysiloxane reaction product, it may be a composition of the invention.
[0021] Examples of silylhydride functional polysiloxanes suitable for use as the reactive polysiloxane in the hydrosilylation reaction system include dimethyl, methylhydrogensiloxane, trimethylsiloxy-terminated (CAS No. 68037-59-2), hydrogen-terminated dimethylsiloxane (CAS No. 70900-21-9), hydrogen-terminated dimethylmethylhydrogensiloxane (CAS No. 690113-23-6), trimethylsiloxy-terminated polymethylhydrosiloxane (CAS No. 63148-57-2), triethylsiloxy-terminated polyethylhydrosiloxane (CAS No. 24979-95-1), and hydride-terminated methylhydrosiloxane-phenylmethylsiloxane copolymer (CAS No. 115487-49-5).
[0022] Examples of polysiloxanes containing carbon-carbon unsaturated bonds suitable for use as reactive polysiloxanes in hydrosilylation reaction systems include vinyl-terminated polydimethylsiloxane (CAS No. 68083-19-2), 2,4,6,8-tetramethyl-2,4,6,8-tetravinylcyclotetrasiloxane (CAS No. 2554-06-5), dimethylcyclics with tetrakis(vinyldimethylsiloxy)silane (CAS number 316374-82-0), vinyl-terminated diphenylsiloxane-dimethylsiloxane copolymer (CAS number 68951-96-2), vinyl-terminated trifluoropropylmethylsiloxane-dimethylsiloxane copolymer (CAS number 68951-98-4), vinylmethylsiloxane-dimethylsiloxane copolymer, trimethylsiloxy-terminated (CAS number 67762-94-1), vinylmethylsiloxane-dimethylsiloxane copolymer, vinyl-terminated (CAS number 68083-18-1), vinylmethoxysiloxane homopolymer (CAS number 131298-48-1).
[0023] Hydrosilylation reaction catalysts are known in the art, and any of them can be used in the hydrosilylation reaction system including the composition of the present invention, such as as a component in the composition of the present invention. Suitable hydrosilylation reaction catalysts include transition metal (platinum, rhodium, palladium, etc.) based catalysts. Examples of hydrosilylation catalysts include platinum-based Speier catalysts, platinum-based Karstedt catalysts, and rhodium-based Wilkinson catalysts. One particularly desirable catalyst is 1,3-diethyl-1,1,3,3-tetramethyldisiloxane platinum complex, commercially available as DOWSIL™ 4000 catalyst (DOWSIL is a trademark of Dow Chemical Company).
[0024] Another example of a reactive system that may contain reactive polysiloxanes and / or may produce a polysiloxane reaction product is a condensation reaction system that reacts to produce a condensation reaction product. A condensation reaction system includes a reactant having hydroxyl and / or alkoxy functionality and often includes a condensation reaction catalyst. The reactant may include a reactive polysiloxane. A reactive polysiloxane having hydroxyl and / or alkoxy functionality can be combined with ZnO particles as described herein to form a condensation reaction reactant that is a composition of the present invention. When the reactant of the condensation reaction system includes ZnO particles and undergoes a condensation reaction, the condensation reaction product can be a polysiloxane with ZnO particles dispersed therein, and therefore can be a composition of the present invention.
[0025] Examples of suitable hydroxyl-functional polysiloxanes that can be reactants in the condensation reaction system include dimethylsiloxane, hydroxy-terminated (CAS No. 70131-67-8), silanol-terminated polydiphenylsiloxane (CAS No. 63148-59-4), and silanol-trimethylsilyl modified Q resin (CAS No. 56275-01-5).
[0026] Examples of suitable alkoxy-functional polysiloxanes which may be reactants in the condensation reaction system include dimethylsiloxane, trimethoxysiloxy-terminated (CAS No. 142982-20-5), dimethylsiloxane, monotrimethoxysiloxy- and trimethylsiloxy-terminated (CAS No. 472976-92-4), dimethylsiloxane, trimethylsiloxy-terminated (CAS No. 63148-62-9).
[0027] Examples of suitable condensation catalysts for the condensation reaction system include, in the broadest sense, any condensation catalyst commonly known for use in condensation reactions.Typically, the condensation catalyst is a tin-based catalyst, acid, or base.Examples of suitable tin-based catalysts include dibutyltin diacetate, carbomethoxyphenyltin tris-uberate, isobutyltin tricerate, dimethyltin dibutyrate, dibutyltin diacetate, dibutyltin dilaurate, divinyltin diacetate, dibutyltin dibenzoate, dibutyltin dioctoate, dibutyltin dilactate, triethyltin tartrate, tributyltin acetate, triphenyltin acetate, tricyclohexyltin acrylate, tritolyltin terephthalate, and tri-n-propyl acetate.
[0028] Surprisingly and unexpectedly, the compositions of the present invention are capable of achieving a V0 rating in UL94 testing without the need for typically known flame retardants. In contrast to polysiloxane flame retardant compositions taught in the art, the compositions of the present invention are characterized by any one or any combination of two or more of the following: (a) contains less than 10 wt. %, or even 5 wt. % or less, 2 wt. % or less, 1 wt. % or less, or even no halogenated compounds; and / or (b) contains less than 30 vol.%, even 20 vol.% or less, 10 vol.% or less, 5 vol.% or less, 2 vol.% or less, 1 vol.% or less, or even no metal hydrates; and / or (c) Contains less than 1.0 wt. %, or even 0.75 wt. %, 0.5 wt. %, 0.25 wt. %, 0.10 wt. %, or even no organic complexes of platinum, rhodium, or iridium; and / or (d) does not include an expandable silicone rubber, or even does not include any expandable package, where the expandable silicone rubber and expandable package generally include a binder, a blowing agent, and an acid source that expand when heated to a temperature at which the composition in which they are located combusts; and / or (e) does not contain red phosphorus; and / or (f) does not contain silicates; and / or (g) A rating of V0 under UL94 testing can be achieved even when the material contains no more than 10 wt%, further no more than 9 wt%, 8 wt%, 7 wt%, 5 wt%, 4.5 wt%, 4 wt%, 3.5 wt%, 3 wt%, 2 wt%, or even no more than 1 wt% of a flame retardant additive.
[0029] The compositions of the present invention may be free of particulate additives other than the ZnO particles described herein, or may include particulate additives in addition to the ZnO particles described herein ("additional particulate additives"). For example, the compositions of the present invention may be free of metal oxides other than the ZnO particles described herein, or may further include ZnO particles having a size larger than those described herein, or may further include metal oxides other than ZnO.
[0030] The composition of the present invention is desirably a thermally conductive composition, which means that it has a thermal conductivity of 0.5 watts per meter-Kelvin (W / m 2 ) as determined by the test method of ISO 22007-2:2015 Part 2 measured at 22°C. *It means that the composition has a thermal conductivity of greater than 100 K. To increase the thermal conductivity, the composition of the present invention may include additional particulate additives that are thermally conductive particles such as any one or any combination of two or more thermally conductive fillers selected from the group consisting of silicon dioxide (SiO2), aluminum, aluminum oxide (Al2O3), magnesium oxide (MgO), titanium dioxide (TiO2), zirconium dioxide (ZrO2), aluminum nitride (AlN), silicon carbide (SiC), boron nitride (BN), aluminum hydroxide (Al(OH)3), magnesium trihydroxide (Mg(OH)3), calcium carbonate (CaCO3), graphite, and clay.
[0031] When additional particulate additives such as thermally conductive fillers are present, they are typically present in a concentration of 95 wt% or less, 90 wt% or less, 85 wt% or less, 80 wt% or less, 75 wt% or less, 70 wt% or less, 65 wt% or less, 60 wt% or less, 55 wt% or less, or even 50 wt% or less by weight of the composition, while typically being present in a concentration of 10 wt% or more, 20 wt% or more, 30 wt% or more, 40 wt% or more, 50 wt% or more, or even 60 wt% or more. EXAMPLES
[0032] Hydrosilylation Examples Table 1 identifies the components used in the hydrosilylation examples of Examples 1-3 and Comparative Examples AH.
[0033] Prepare the Part A and Part B compositions as described in Tables 2 and 3 using a 10 liter Turello mixer.
[0034] For the Part A composition, place the specified amount of VFP1 in a mixer and mix for 5 minutes at 20 revolutions per minute (RPM) under a nitrogen flow of 0.4 cubic meters / hour. Add the specified amount of quartz powder, ZnO, Al2O3, and / or TiO2 and mix for an additional 15 minutes. Heat to 80 degrees Celsius (°C) under vacuum for 1 hour. Cool to 22°C and add the hydrosilylation catalyst.
[0035] For the Part B compositions, place the specified amount of VFP1 in a separate mixer pot and mix for 5 minutes at 20 RPM under a nitrogen flow of 0.4 cubic meters per hour. Add the specified quartz powder and ZnO components and mix for an additional 15 minutes. Heat to 95°C under vacuum for 1 hour. Cool to 22°C and add the specified amounts of VFP2 and SHFP1 and mix.
[0036] Equal parts by weight of Part A and Part B are blended to form a reactive mixture and cured at 70° C. for 30 minutes to obtain a hydrosilylated reaction product. Hydrosilylated reaction products of each composition are prepared at thicknesses of 125±5 millimeters and 13.0±0.5 millimeters. Ten samples of each thickness are prepared. Five samples are evaluated in the UL94 vertical burn test immediately after preparation as samples. Five samples are aged at 70° C. for 168 hours, serving as "aged samples," and then subjected to the UL94 vertical burn test. The burn test results are shown in Table 4.
[0037] The compositions and test results are shown below.
[0038] [Table 1]
[0039] [Table 2]
[0040] [Table 3]
[0041] [Table 4]
[0042] Comparative Example A shows that the composition fails to achieve a V0 rating when no ZnO is present. Comparative Examples B and C show that even with a loading of 1 wt% micro-ZnO, the composition still fails to achieve a V0 rating. Comparative Example D shows that a loading of 0.1 wt% nano-ZnO is insufficient to achieve a V0 rating. Examples 1-3 show that nano-ZnO achieves a V0 rating from as little as 0.15 wt% (Example 1) up to 1 wt%. It is clear from the values that increasing the loading of nano-ZnO continues to achieve a V0 rating.
[0043] Comparative Examples E and F show that even a 0.30 wt% loading of nano-Al2O3 does not achieve the V0 rating as well as nano-ZnO. Similarly, Comparative Examples G and H show that even a 0.30 wt% loading of nano-TiO2 does not achieve the V0 rating as well as nano-ZnO.
[0044] Aluminum oxide filled hydrosilylation system Table 5 discloses the ingredients used to prepare Comparative Example I and Example 4.
[0045] Comparative Example I and Example 4 Prepare the Part A and Part B compositions as described in Tables 6 and 7 using a 10 liter Turello mixer. Prepare Comparative Example I and Example 4 by blending the corresponding Part A and Part B compositions in a 1:1 weight ratio and curing at 120°C for 60 minutes to obtain a hydrosilylation reaction product. Prepare the hydrosilylation reaction product of each composition at a thickness of 125±5 millimeters and 13.0±0.5 millimeters. Prepare 10 samples of each thickness. Evaluate five samples in the UL94 vertical burn test immediately after preparation as samples. Age five samples at 70°C for 168 hours to serve as "aged samples" and then subject them to the UL94 vertical burn test. The burn test results are shown in Table 8 below.
[0046] [Table 5]
[0047] Comparative example I For the Part A composition, place the specified amount of vinyl polysiloxane and treating agent in a mixer and mix for 5 minutes at 20 revolutions per minute (RPM) under a nitrogen flow of 0.4 cubic meters / hour. While mixing, add half of the 2 micrometer sized aluminum oxide filler and continue mixing for 10 minutes at 45 RPM under a nitrogen purge. Add the remaining 2 micrometer sized aluminum oxide filler and mix for 10 minutes at 45 RPM under a nitrogen purge. Stop mixing and scrape material off the walls and cover of the mixing vessel. Heat to 60°C. Add half of the 60 micrometer sized aluminum oxide particles and mix for 10 minutes at 45 RPM under a nitrogen purge. Add the remaining 60 micrometer sized aluminum oxide particles and mix for 10 minutes at 45 RPM under a nitrogen purge. Stop mixing and scrape material off the walls of the mixing vessel. Continue mixing under vacuum at 45 RPM for 60 minutes. Heat to 130°C and mix under vacuum at 45 RPM for 30 minutes. Cool to 40°C, stop mixing and release the vacuum. Scrape material off the walls of the vessel and the mixer blades. Add the platinum catalyst component and mix at 45 RPM for 15 minutes under nitrogen purge, then 30 minutes under vacuum. Stop mixing and release the vacuum to obtain the composition of Comparative Example I, Part A.
[0048] In Part B, add vinyl polymer, blue pigment, carbon black, and filler treatment to mixer vessel. Mix at 20 RPM under 0.4 cubic meters / hour nitrogen purge. Add half of the 2 micrometer aluminum oxide filler and mix at 45 RPM for 10 minutes under nitrogen purge. Add remaining 2 micrometer aluminum oxide filler and mix at 45 RPM for 10 minutes under nitrogen purge. Stop mixing and scrape material off sides of vessel. Heat to 60°C and add half of the 60 micrometer aluminum oxide filler and mix at 45 RPM for 10 minutes under nitrogen purge. Add remaining 60 micrometer aluminum oxide filler and mix at 45 RPM for 10 minutes under nitrogen purge. Stop mixing and scrape material off walls of vessel. Mix under vacuum at 45 RPM for 60 minutes. Heat to 130°C and mix under vacuum at 45 RPM for 30 minutes. Cool to 40°C, release the vacuum, and scrape material off the sides of the vessel. Add the cure inhibitor, chain extender, and crosslinker and mix for 15 minutes at 45 RPM under a nitrogen purge. Mix for 30 minutes at 45 RPM under vacuum. Stop mixing and release the vacuum to obtain the composition of Comparative Example I, Part B.
[0049] Example 4 For the Part A composition, the specified amount of vinyl polymer and treating agent are placed in a mixer and mixed for 5 minutes at 20 revolutions per minute (RPM) under a nitrogen flow of 0.4 cubic meters / hour. Add the nano-ZnO and half of the 2 micrometer sized aluminum oxide filler while mixing and continue mixing for 10 minutes at 45 RPM under a nitrogen purge. Add the remaining 2 micrometer aluminum oxide filler and mix for 10 minutes at 45 RPM under a nitrogen purge. Stop mixing and scrape material off the walls and cover of the mixing vessel. Add half of the 60 micrometer sized aluminum oxide particles and mix for 10 minutes at 45 RPM under a nitrogen purge. Add the remaining 60 micrometer sized aluminum oxide particles and mix for 10 minutes at 45 RPM under a nitrogen purge. Stop mixing and scrape material off the walls of the mixing vessel. Continue mixing under vacuum at 45 RPM for 60 minutes. Heat to 130° C. and mix under vacuum at 45 RPM for 30 minutes. Cool to 40°C, stop mixing and release the vacuum. Scrape material off the walls of the vessel and the mixer blades. Add the platinum catalyst component and mix at 45 RPM for 15 minutes under nitrogen purge, then 30 minutes under vacuum. Stop mixing and release the vacuum to obtain the composition of Example 4, Part A.
[0050] In Part B, add vinyl polymer and filler treatment to mixer vessel. Mix at 20 RPM under 0.4 m3 / hr nitrogen purge. Add nano-ZnO and half of the 2 micrometer aluminum oxide filler and mix at 45 RPM for 10 minutes under nitrogen purge. Add remaining 2 micrometer aluminum oxide filler and mix at 45 RPM for 10 minutes under nitrogen purge. Stop mixing and scrape material off sides of vessel. Add half of 60 micrometer aluminum oxide filler and mix at 45 RPM for 10 minutes under nitrogen purge. Add remaining 60 micrometer aluminum oxide filler and mix at 45 RPM for 10 minutes under nitrogen purge. Stop mixing and scrape material off walls of vessel. Mix under vacuum at 45 RPM for 60 minutes. Heat to 130°C and mix under vacuum at 45 RPM for 30 minutes. Cool to 40°C, release vacuum, and scrape material off sides of vessel. Add cure inhibitor, chain extender, and crosslinker and mix for 15 minutes at 45 RPM under nitrogen purge. Mix for 30 minutes at 45 RPM under vacuum. Stop mixing and release vacuum to obtain composition of Example 4, Part B.
[0051] [Table 6]
[0052] [Table 7]
[0053] [Table 8]
[0054] The results of Comparative Example I and Example 4 show that the Al2O3 filler alone does not achieve a V0 rating, but Example 4, where some of the Al2O3 is replaced with nano-sized zinc oxide, achieves a V0 rating.
[0055] Condensation Example Table 9 identifies the components used in the condensation examples.
[0056] Prepare Part A and Part B compositions as described in Tables 10 and 11. Blend equal parts by volume of Part A and Part B compositions for each Comparative Example and Example in a 2-part cartridge equipped with a static mixer to form a 3 millimeter thick reactive mixture on a polytetrafluoroethylene film and cure at 23°C (how long? Any particular level of humidity required?). Cut 10 specimens from each composition for UL94 vertical flame testing. Evaluate 5 specimens immediately as "as-prepared" specimens. Age 5 specimens for 168 hours at 70°C as "aged" specimens prior to UL94 testing. Flame test results are shown in Table 12.
[0057] Comparative Example J shows that in the absence of nano-ZnO, the composition fails to achieve a V0 rating. Examples 5-7 show that the inclusion of nano-ZnO in the composition enables the composition to achieve a V0 rating.
[0058] [Table 9]
[0059] [Table 10]
[0060] [Table 11]
[0061] [Table 12]
Claims
1. 1. A composition comprising: (a) a polysiloxane; (b) dispersed in said polysiloxane, zinc oxide particles having an average particle size of less than 1 micrometer and greater than 1 nanometer, as determined as the volume weighted median of the particle size distribution using a laser diffraction particle size analyzer, equal to or greater than 0.15 weight percent and equal to or less than 4.5 weight percent, based on the weight of the composition; (c) 50 to 95 weight percent of a thermally conductive filler, based on the weight of the composition. Including, A composition wherein the zinc oxide particles do not have a surface treatment.
2. 2. The composition of claim 1, wherein the polysiloxane is a reactive polysiloxane containing any combination of one or more functional groups selected from the group consisting of silanol groups, alkoxy groups, epoxy groups, silyl hydride groups, and groups containing carbon-carbon unsaturated bonds.
3. The composition of claim 1 , wherein the composition is selected from a hydrosilylation reaction system, a hydrosilylation reaction product, a polysiloxane condensation reaction system, and a polysiloxane condensation reaction product.
4. The composition of claim 2 , wherein the composition further comprises a platinum or tin catalyst.
5. The thermally conductive filler is SiO 2 , and Al 2 O 3 The composition according to any one of claims 1 to 4, which is at least one selected from the group consisting of:
6. The composition of any one of claims 1 to 5, wherein the composition contains from 0 to less than 10 weight percent of a flame retardant, based on the weight of the composition.
7. 7. The composition of claim 1, wherein the composition contains from 0 to less than 10 weight percent of halogenated compounds based on the weight of the composition, from 0 to less than 30 volume percent of metal hydrates based on the volume of the composition, from 0 to less than 1.0 weight percent of organic complexes of platinum, rhodium, and iridium based on the weight of the composition, is free of red phosphorus, and is free of an expandable silicone rubber formulation that includes a binder, a blowing agent, and an acid source that foams when heated to a temperature at which the composition combusts.
8. The composition of any one of claims 1 to 7, wherein the polysiloxane is part of a reactive system or is the reaction product of a reactive system.
Citation Information
Patent Citations
High-adhesion scratch-resistant organosilicone blade coating ink and preparation method thereof
CN107964277A
Flexible heat conduction sheet and preparation method thereof
CN108690355A
Flame-retardant silicone rubber composition
JP1993125282A
Thermoconductive silicone composition, thermoconductive material and thermoconductive silicone grease
JP1998110179A
Heat radiation member