Phenolic foam and method for producing same
The phenolic foam's asymmetric structure with varying closed cell ratios addresses the challenge of maintaining uniform properties and preventing damage, ensuring superior insulation and strength throughout its lifespan.
Patent Information
- Application Number
- JP2023526006
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-11-09
- Filing Date
- 2021-11-08
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2041-11-08
AI Technical Summary
Existing insulation foams face challenges in maintaining uniform physical properties and preventing damage during installation and long-term use, especially with increased thickness, leading to issues like warping, reduced thermal conductivity, and poor insulation performance.
A phenolic foam is divided into odd-numbered sections along its thickness, with varying closed cell ratios to create an asymmetric structure, ensuring uniform physical properties and reducing impact variation, thereby preventing warping and maintaining insulation and compressive strength.
The foam maintains excellent insulation and compressive strength, preventing deflection and ensuring long-term durability with improved production efficiency and cost-effectiveness.
Smart Images

Figure 0007573109000003 
Figure 0007573109000004 
Figure 0007573109000005
Abstract
Description
[Technical field]
[0001] The present invention relates to phenolic foams and methods for their production. [Background technology]
[0002] Insulation is an essential item used in buildings to prevent energy loss. With global warming emphasizing the importance of green growth in the world, insulation is becoming even more important to minimize energy loss.
[0003] Normally, increasing the thickness of the insulation material makes it easy to ensure insulation, but once the thickness of the insulation material exceeds a certain level, the physical properties change depending on the position in the thickness direction, making the foam more susceptible to damage and bending, resulting in a decrease in appearance and physical properties, and even a decrease in thermal conductivity.
[0004] As a result, in the past, in order to ensure the physical properties of thick products, there was a tendency to produce foams that exhibit uniform physical properties throughout the foam and have symmetrical physical properties with respect to the middle part (center) of the foam in the thickness direction.
[0005] However, in reality, it is not easy to achieve a symmetrical structure while reducing the deviation in physical properties throughout the thickness, and this is uneconomical in terms of cost and production efficiency. Summary of the Invention [Problem to be solved by the invention]
[0006] The object of the present invention is to provide a thick phenolic foam that exhibits excellent physical properties and is more economical by controlling the distribution of the closed cell ratio of the thick foam to increase production efficiency. Another object of the present invention is to provide a phenolic foam that can prevent the foam from being damaged during installation and can maintain excellent physical properties such as thermal insulation and compressive strength at a certain level not only during foam production but also during long-term use, and can prevent the occurrence of deflection.
[0007] It is also an object of the present invention to provide a method for producing said phenolic foam.
[0008] The object of the present invention is not limited to the object mentioned above, and other objects and advantages of the present invention not mentioned can be understood from the following description and can be more clearly understood from the embodiments of the present invention. Also, it is easy to understand that the object and advantages of the present invention can be realized by the means and combinations thereof as set forth in the claims. [Means for solving the problem]
[0009] The present invention provides a phenolic foam having a thickness of 90 mm or more, wherein when the foam is divided into N (N≧7 odd number) pieces from any surface in the thickness direction along the surface, the closed cell rate of the first surface layer (N1) is greater than or equal to the closed cell rate of the second surface layer (N N ) and the N pieces of the slice having the smallest closed cell ratio (N min ) is the first surface layer portion (N1) and the intermediate section (N c ) a phenolic foam positioned between the
[0010] The present invention can also provide a method for producing a phenolic foam, comprising the steps of: discharging a foaming composition containing a phenolic resin, a foaming agent, and a curing agent onto a surface material using a nozzle; and foaming and curing the discharged foaming composition, wherein the nozzle has an outlet having a shape in which the length (L) / width (W) is 1 or more and 2 or less. Effect of the Invention
[0011] The phenolic foam according to the present invention is a thick foam, which is more economical and prevents damage during the installation process of the foam. It exhibits excellent physical properties such as excellent thermal insulation and compressive strength to a certain level not only during the production of the foam but also during long-term use, and can prevent the occurrence of deflection.
[0012] Furthermore, the method for producing a phenolic foam according to the present invention can improve production efficiency and provide a phenolic foam having the above physical properties more economically.
[0013] The above-mentioned effects and specific effects of the present invention will be described in conjunction with the following description of the preferred embodiment of the invention. [Brief description of the drawings]
[0014] [Figure 1] 1 is a schematic diagram showing a phenolic foam according to an embodiment of the present invention being uniformly cut into N pieces (N=9) in the thickness direction. FIG. [Diagram 2] 1 is a schematic view of a nozzle outlet for discharging a foam composition according to an embodiment of the present invention. [Diagram 3] FIG. 13 is a schematic diagram showing a plurality of outlets arranged on a lower surface of a conveyor according to another embodiment of the present invention. [Figure 4] FIG. 4 is a schematic diagram illustrating a method for measuring the degree of deflection of a phenolic foam according to another embodiment of the present invention. [Diagram 5] FIG. 2 is a schematic diagram illustrating a method for measuring the dimensional stability of a phenolic foam according to another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The above-mentioned objects, features and advantages will be described in detail below with reference to the accompanying drawings, so that a person having ordinary skill in the art to which the present invention pertains can easily implement the technical idea of the present invention. In describing the present invention, if a detailed description of a known technology according to the present invention is deemed to obscure the gist of the present invention, the detailed description will be omitted. Hereinafter, a preferred embodiment according to the present invention will be described in detail with reference to the accompanying drawings. The same reference numerals in the drawings are used to indicate the same or similar components.
[0016] Phenolic foams according to some embodiments of the present invention will now be described.
[0017] In one embodiment of the present invention, a phenolic foam having a thickness of 90 mm or more is provided, and when the foam is divided into N pieces (N≧7 odd number) from any surface in the thickness direction along the surface, the closed cell rate of a first surface layer (N1) is greater than or equal to the closed cell rate of a second surface layer (N N ) and the N pieces of the slice having the smallest closed cell ratio (N min ) is the first surface layer portion (N1) and the intermediate section (N c ) and a phenolic foam positioned therebetween.
[0018] Generally, the thicker the foam, the easier it is to ensure thermal insulation. However, when the thickness of the foam exceeds a certain level, the curing reaction at the center of the foam in the thickness direction increases internal heat generation, and the heat is difficult to dissipate to the outside, causing the internal temperature of the foam composition to rise excessively. As a result, the physical properties of the foam may change significantly depending on the position in the thickness direction of the foam, such as bubbles near the center of the foam bursting, and the foam may be easily damaged and warped. When the foam warps, there is a high possibility of apparent defects and poor construction, and problems such as product shrinkage over a long period of time occur. In addition, even if the thickness is increased, the thermal conductivity may decrease. Therefore, in the past, in order to ensure the physical properties of a high-thickness product and prevent warping, there was a tendency to make the physical properties of the entire foam uniform and to manufacture a foam whose physical properties are symmetrical with respect to the middle part in the thickness direction of the foam. However, in reality, it is not easy to make the physical properties uniform throughout the thickness of a high-thickness foam and form a symmetric structure, which is uneconomical in terms of cost and production efficiency.
[0019] In addition, although it is possible to separate the upper and lower surface layers of a foam during manufacturing, it is difficult to separate the upper and lower parts of the foam during construction. As a result, the impact on the weaker part of the foam may vary greatly depending on which part of the upper or lower surface layer receives the impact. In particular, insulation materials, such as insulation materials for ceilings or floors, are arbitrarily positioned by workers during the installation process, stepped on, and cement is poured in and then matured for a certain period of time. Therefore, even if a foam shows excellent physical properties during manufacturing, the weaker part of the foam may be significantly damaged during the installation process, and physical properties such as insulation and compressive strength may be significantly reduced during use of the foam, and deflection may occur, which may result in a decrease in thermal conductivity.
[0020] The phenolic foam has a thickness of about 90 mm or more, and has an asymmetric structure based on the middle part in the thickness direction of the foam, and the position of the foam having the minimum closed cell ratio is adjusted to exhibit excellent physical properties such as heat insulation and compressive strength throughout the foam, and to prevent bending. Even if an impact is applied to either of the two surfaces of the phenolic foam during the installation process, the impact received by the weak part of the foam can be reduced to the same or similar extent. As a result, the phenolic foam can exhibit excellent physical properties for a long period of time even after the construction process. The phenolic foam can have a thickness of about 110 mm or more, about 150 mm or more, or about 180 mm or more to 300 mm.
[0021] When the phenol foam is divided into N (N≧7 odd number) pieces in the thickness direction along the surface of the foam, the closed cell rate of the first surface layer (N1) is greater than that of the second surface layer (N N ) and the N pieces of the slice having the smallest closed cell ratio (N min ) is the first surface layer portion (N1) and the intermediate section (N c ) located between
[0022] In the present invention, in order to measure the distribution of the closed cell ratio according to the thickness of a foam, the foam is cut evenly into N pieces (N is an odd number of 7 or more) along the surface in the thickness direction from the surface. In this case, the thickness means the direction (Z direction) in which the foaming composition on the facing material grows, and the surface perpendicular to the thickness direction is the surface, which means the surface to which the facing material is attached during the production of the foam. If the foam has a facing material, the facing material is removed, and in order to accurately measure the closed cell ratio, both surfaces of the foam where the facing material was attached are cut by 5 mm each.
[0023] Then, the foam is divided into N (N≧7 odd number) equal pieces in the thickness direction along the surface. The closed cell ratio of each piece is measured. N may be a constant number including an even number, but it is preferable that N is an odd number in order to more clearly confirm whether the physical properties are symmetrical with respect to the center of the foam in the thickness direction. Each piece may have a thickness of about 10 mm to about 30 mm.
[0024] The phenol foam includes a first surface and a second surface, and the first surface portion includes the first surface, and the second surface portion includes the second surface. Of the two slices at both ends including both surfaces of the foam, the slice with the lower closed cell ratio is designated N1 (first surface portion), and the other slice is designated N2 (second surface portion). N (Second surface layer), N1, N2, N3, N4, N5, ... and N N The individual slices are indicated as follows. Among the slices, the slice located in the middle is called the intermediate slice (N c ) is the mid-intercept (N c ) is the first surface layer portion (N1) and the second surface layer portion (N N For example, FIG. 1 is a schematic diagram showing nine (N=9) uniformly cut pieces of a phenolic foam according to an embodiment of the present invention in the thickness direction. Of the two pieces at both ends including both surfaces of the foam, the piece with the lowest closed cell ratio is N1 (first surface layer), the other piece is N9 (second surface layer), and the middle piece (N c ) is N5. And the section with the smallest closed cell ratio (N min) was located at the fourth segment, i.e., N4.
[0025] The phenol foam has a first surface layer (N1) having a closed cell rate that is greater than that of a second surface layer (N N ) and forms an asymmetric structure. In this case, the piece (N min ) is the first surface layer portion (N1) and the intermediate section (N c ) is located between the first surface layer portion and the second surface layer portion. Even if an impact is applied to either the first surface layer portion or the second surface layer portion, the piece having the minimum closed cell ratio (N min ) is subjected to the same or similar impact, and the foam as a whole has excellent physical properties such as heat insulation and is prevented from bending.
[0026] In general, in the case of a thick foam, it is attempted to improve the physical properties of the entire foam by making the physical properties have a symmetric distribution in the thickness direction, but this is uneconomical since it is too costly and reduces production efficiency. Moreover, as the thickness of the foam increases, it is practically impossible to make the physical properties have a symmetric distribution.
[0027] Therefore, the phenol foam has a closed cell rate of the first surface layer (N1) that is higher than that of the second surface layer (N N ) and have an asymmetric structure, making it more economical to produce a foam while still obtaining a section with a minimum closed cell content (N min ) is the second surface layer (N N The first surface layer portion (N1) and the intermediate section (N c ) to achieve the desired effect. For example, the section with the smallest closed cell ratio (N min ) is the mid-intercept (N c ) and the second surface layer with a high closed cell ratio (N N In the case where an impact is applied to the first surface layer (N1) of the foam located between the first surface layer (N2) and the second surface layer (N3), it is not a problem. N ) is impacted, the section with the smallest closed cell ratio (N minIn the thickness direction, the foam may be significantly damaged, and the physical properties may be significantly reduced during use. Since the phenolic foam has the above structure, it is economical because it can achieve the same or similar effects as a foam whose physical properties are completely symmetrical in the thickness direction.
[0028] The closed cell rate of the first surface layer portion (N1) and the closed cell rate of the second surface layer portion (N N ) and the closed cell ratio of the second surface layer (N N The closed cell content of the first surface layer portion (N1) minus the closed cell content of the first surface layer portion (N2) may be about 0.05% to about 5%. For example, it may be about 0.1% to about 5% or about 0.1% to about 3%. N If the difference in the closed cell ratio between the first and second foams is less than the above range, the cost will increase and the production efficiency will decrease, making it uneconomical. If the difference in the closed cell ratio between the first and second foams is more than the above range, there will be a limit to how excellent the physical properties of the foam as a whole will be.
[0029] The closed cell rate of the first surface layer portion (N1) and the closed cell rate of the second surface layer portion (N N The closed cell ratio of each of the first surface layer portion (N1) and the second surface layer portion (N N ) has a closed cell ratio within the above range, and thus has excellent initial thermal conductivity, prevents replacement of the foam with air, reduces the amount of change in heat insulating performance over time, and exhibits excellent heat insulating properties.
[0030] The phenol foam is the second surface layer (N N ) has the maximum closed cell ratio, and the second surface layer portion (N N ) and the section having the minimum closed cell ratio (N min ) and the closed cell ratio (△C2 = | the second surface layer (N N ) closed cell ratio - intercept (N min The closed cell ratio |) of the slice (N ) may be about 1 to about 20%. For example, it may be about 1 to about 15% or about 1% to about 7%. In this case, the slice (N min ) and the second surface layer portion (N NIf the difference in the closed cell ratio between the first surface layer portion (N1) and the slice (N2) having the minimum closed cell ratio exceeds the above range, not only will the replacement speed of the foaming agent in the bubbles with air increase, causing a large change in thermal conductivity over time, but the mechanical strength capable of withstanding shrinkage stress in a high-temperature environment will be damaged, causing a significant deterioration in the rate of dimensional change. As a result, the foam will easily and significantly exhibit a bending phenomenon. min ) and the closed cell ratio (△C1 = | closed cell ratio of the first surface layer (N1) - intercept (N min The closed cell ratio |) of the foam may be about 0.1 to about 20%, for example, about 0.1 to about 10%.
[0031] The section having the minimum closed cell ratio (N min The phenol foam may have a closed cell ratio of about 70% or more. For example, it may be about 70% to about 89%. min By adjusting the closed cell ratio of the foam to the above range, it is possible to maintain low thermal conductivity for a long period of time, prevent warping, and improve dimensional stability. For example, if it is below the above range, the replacement rate of the foaming agent in the cells with air increases, and the change in thermal conductivity over time may become large.
[0032] The phenol foam may have a ratio of d1 to d2 with respect to the total thickness of the foam of about 0.2:0.8 to about 0.45:0.55. The d1 is the ratio of the thickness of the section (N1) having the smallest closed cell ratio from the first surface layer portion (N2) to the total thickness of the foam. min ) from the top surface of the first surface layer (N1) to the section (N min ) / total thickness of the foam body), and d2 is the thickness of the second surface layer portion (N N ) to the section with the minimum closed cell ratio (N min ) from the lower surface of the second surface layer (N1) to the section having the minimum independent bubble ratio (N min) / total thickness of foam). In this case, the total thickness of the foam refers to the thickness of the foam after cutting both surfaces of the foam to which the facing material was attached by 5 mm each. And, d1 and d2 are the distances between the cut pieces (N min ) means the ratio of the vertical distance to the 1 / 2 point in the thickness direction.
[0033] The section having the minimum closed cell ratio (N min ) is the first surface layer portion (N1) and the second surface layer portion (N N ), even if an impact is applied to either the first surface layer portion or the second surface layer portion, the piece (N min ) can be made to receive the same or similar impact, and the entire foam can have excellent physical properties such as thermal insulation and can prevent bending. For example, min If the fraction (N1) is outside the above range and is located closer to the first surface layer (N1), the physical properties of the first surface layer (N1) side will be significantly reduced, making it difficult to make the physical properties of the entire foam more uniform than a certain level, and shrinkage of the first surface layer (N1) including the facing material will be apparent, causing a large deflection of the product in the direction of the first surface layer (N1), resulting in a decrease in compressive strength. min ) is the second surface layer (N N ), the second surface layer (N N When an impact is applied to the section with the smallest closed cell ratio (N min ) is subject to a rapid increase in the degree of impact, making it susceptible to damage, and the second surface layer (N N ) There may be problems such as the product bending significantly in the direction.
[0034] The phenol foam has surface layers (N1, N N ) and the section with the smallest closed cell ratio (N min) by the ratio (d1, d2) of the distance between each surface layer and the slice having the smallest closed cell ratio, the value (Y) may be (|(ΔC2 / d2)-(ΔC1 / d1)|)=about 0.1 to about 9. For example, it may be about 0.1 to about 6.5 or about 0.1 to about 5. If the Y value exceeds the above range, the impact received at a specific position in the thickness direction may become large, or the physical properties of the entire foam may decrease, causing a problem of deflection.
[0035] The phenol foam has the above-mentioned closed cell ratio distribution, so that the foam as a whole exhibits excellent physical properties and can maintain excellent thermal conductivity even after long-term use.
[0036] Specifically, the phenol foam may have a compressive strength according to KS M ISO 844 of about 100 kPa to about 200 kPa. For example, it may be about 115 kPa to about 200 kPa. The compressive strength means the pressure at which the foam breaks. By having a compressive strength in the above range, the phenol foam can maintain an excellent balance between physical properties and exhibit excellent long-term durability even after distribution and application.
[0037] The phenol foam may have a dimensional change rate of about 0% to about 2.0%. For example, the phenol foam may have a dimensional change rate of about 0% to about 1.0% or about 0% to about 0.7%. In this case, the dimensional change rate can be measured by the method described in Experimental Example 4.
[0038] As shown in FIG. 4, when the foam is left at 25°C and 60% relative humidity for 7 days, the surface of the foam may bend concavely toward the floor (I) or convexly toward the ceiling (II). In this case, the change in the corners (P1 to P4) in the case of (I) and the maximum separation distance (R1, R2) between the two longitudinal sides of the foam and the floor surface in the case of (II) may affect the damage the foam receives from external impact and the overall deformation of the foam. The phenol foam may have an average deflection of about 0 cm to about 1.5 cm in the case of (I) and / or (II), respectively. Alternatively, the average deflection may be about 0.1 cm to about 0.7 cm or about 0.1 cm to about 0.5 cm, respectively.
[0039] The phenolic foam may have a thermal conductivity of about 0.017 W / m·K to about 0.020 W / m·K, measured at an average temperature of 20° C. according to KS L 9016.
[0040] The phenolic foam may have a thermal conductivity of about 0.018 W / m·K to about 0.022 W / m·K measured at an average temperature of 20°C in accordance with EN13823 after being dried at 70°C for 7 days and then at 110°C for 14 days.
[0041] The phenolic foam contains the closed cell ratio in the above-mentioned distribution, exhibits excellent physical properties such as compressive strength, is resistant to deflection, and exhibits a change in thermal conductivity over time of about 10% or less.
[0042] Another embodiment of the present invention provides a method for producing a phenolic foam, comprising the steps of: discharging a foaming composition including a phenolic resin, a foaming agent, and a curing agent onto a facing material using a nozzle; and foaming and curing the discharged foaming composition, wherein the nozzle has an outlet having a length (L) / width (W) ratio of 1 to 2.
[0043] As described above, the above-mentioned manufacturing method makes it possible to more economically manufacture a phenolic foam having a specific distribution of closed cell ratio and excellent physical properties throughout the foam. Furthermore, the phenolic foam manufactured according to the above-mentioned manufacturing method can be easily cut into a slice having a minimum closed cell ratio (N min ) to be subjected to the same or similar impact, and the foam as a whole has excellent physical properties such as thermal insulation and compressive strength, and can prevent deflection. The above-mentioned matters such as the thickness and closed cell ratio of the phenolic foam are the same as above, except as otherwise specifically described below.
[0044] In the case of a phenolic foam having a normal thickness, when the foaming composition is continuously discharged onto the first face material using one nozzle and then molded into a plate between the conveyors in the curing oven, the foaming composition rapidly foams and cures to the set thickness, and the reaction heat generated during the reaction is easily radiated through the surface face material, so that it is not difficult to have uniform physical properties throughout the thickness. On the other hand, in the case of a phenolic foam having a thickness of 90 mm or more, internal heat generation increases due to the curing reaction in the center of the foam in the thickness direction, and the heat is difficult to dissipate to the outside, so that the internal temperature of the foaming composition rises excessively. As a result, the bubbles near the center of the foam are likely to burst. In addition, the foaming composition discharged onto the first face material (lower face material) expands in the direction of the second face material (upper face material) (Z direction), and the time required for foaming and curing becomes relatively long when the product is thick. As a result, the foaming composition remains on the first face material (lower face material) for a long time, and the foaming composition gradually accumulates on the first face material (lower face material), causing relatively excessive expansion, and the bubbles near the first face material (lower face material) tend to burst easily, and the thicker the foam, the more significant the variation in physical properties becomes, which can lead to a deterioration in the overall physical properties of the foam. To overcome this, a method has been proposed in which the foaming composition is discharged individually onto the upper and lower faces using respective nozzles, but this method requires complicated equipment and has the problem of increasing costs.
[0045] The method for producing the phenolic foam according to another embodiment of the present invention includes a step of discharging a foaming composition including a phenolic resin, a foaming agent, and a curing agent onto a facing material 3 using a nozzle. At this time, the outlet 10, which is the inlet of the nozzle, may have a shape in which the length (L) / width (W) is 1 or more and 2 or less. For example, as shown in FIG. 2, the outlet may have an elliptical shape in which the length (L) is longer than the width (W), and the length (L) / width (W) may be more than 1 and 2 or less. The outlet means an inlet through which the composition is discharged. In this case, in the ellipse, the length (L) means the length of the major axis, and the width (W) means the length of the minor axis. As shown in FIG. 3, the length (L) direction of the outlet may be parallel to the thickness direction (Z direction) of the foam, and the width (W) direction of the outlet may be parallel to the width direction (Y direction) of the foam.
[0046] The nozzle outlet may have a length (L) / width (W) (aspect ratio) of 1 or more and 2 or less. For example, the nozzle outlet may have an elliptical outlet having a length (L) / width (W) ratio of more than 1 and 2 or less. This prevents the hardened bubbles from collapsing due to the movement of the foaming composition, and prevents problems such as excessive foaming and expansion of the foaming composition near the surface material (e.g., the lower surface material) from which the foaming composition is discharged. For example, if the nozzle outlet has a rectangular structure rather than an ellipse, there may be problems such as accumulation of the hardened material near the corners of the outlet. And, if the outlet has a circular or elliptical shape but the length (L) / width (W) is less than the above range, there may be problems such as excessive foaming and expansion occurring near the lower surface material from which the foaming composition is discharged, causing bubbles to easily break. If the length (L) / width (W) ratio exceeds the above range, the amount of the foaming composition spreading in the width direction of the foam (Y direction, the direction perpendicular to the extrusion direction of the foaming composition) increases, and the bubbles that have hardened due to heating collapse due to the movement of the foaming composition, further slowing the foaming and expansion speed in the thickness direction of the foam (Z direction), which can result in problems such as an increase in the time and amount of the foaming composition remaining near the lower surface material and problems such as the bubbles breaking.
[0047] The discharge port may have a length (L) of about 10 mm to about 100 mm. If the length (L) of the major axis of the discharge port is less than the above range, the pressure generated during discharge from the nozzle may increase, and if it exceeds the above range, there may be a problem that the pressure is low and appropriate foaming is not performed.
[0048] The foaming composition can be discharged at about 30 kg / min to about 100 kg / min.
[0049] The viscosity of the foaming composition at the time of extrusion may be about 5,000 cps to about 40,000 cps at 25° C. When the foaming composition has a viscosity in the above range, it can be extruded in a slurry state suitable for foaming and curing.
[0050] The temperature of the foaming composition during the discharge may be about 0° C. to about 40° C. If the temperature range is less than the above range, the viscosity of the discharged material increases excessively, making it difficult to discharge, whereas if the temperature range is exceeded, the foaming agent easily volatilizes, decreasing the thermal conductivity.
[0051] The method for producing the phenol foam may include a plurality of nozzles having the discharge ports 10 arranged along a direction (Y-axis direction, width direction of the foam) perpendicular to the flow direction of the foam composition (X-axis, i.e., the running direction of the facing material 3) as shown in Fig. 3. Specifically, the number of the nozzles may be about 4 to about 12. The nozzles may be arranged in parallel at equal intervals.
[0052] In the manufacturing method, the number of nozzles having the discharge ports 10 are arranged in parallel at uniform intervals, and uniform expansion can be induced not only in the direction in which the foaming composition grows (Z-axis direction, thickness direction of the foam), but also in the direction (Y-axis direction, width direction of the foam) perpendicular to the flow direction of the foaming composition (X-axis, i.e., running direction of the facing material). This makes it possible to appropriately adjust the growth and distribution of bubbles.
[0053] The foaming composition includes a phenolic resin, a foaming agent, and a curing agent. The phenolic resin may be obtained by reacting phenol with formaldehyde, and may include, for example, a resol-type phenolic resin (hereinafter, "resole resin"). The phenolic resin may be included in the phenolic foam in an amount of about 30% by weight to about 90% by weight, about 50% by weight to about 90% by weight, or about 55% by weight to about 90% by weight. By including the phenolic resin in the above range, the phenolic foam can stably form small foam cells and realize excellent thermal conductivity.
[0054] The phenol foam may include a blowing agent. For example, the blowing agent may include one selected from the group consisting of hydrofluoroolefin (HFO)-based compounds, hydrocarbon-based compounds, and combinations thereof. Specifically, the hydrofluoroolefin-based compounds may include at least one selected from the group consisting of monochlorotrifluoropropene, trifluoropropene, tetrafluoropropene, pentafluoropropene, hexafluorobutene, and combinations thereof. The hydrocarbon-based compounds may include hydrocarbons having 1 to 8 carbon atoms. For example, the hydrocarbon-based compounds may include at least one selected from the group consisting of dichloroethane, propyl chloride, isopropyl chloride, butyl chloride, isobutyl chloride, pentyl chloride, isopentyl chloride, n-butane, isobutane, n-pentane, isopentane, cyclopentane, hexane, heptane, cyclopentane, and combinations thereof. Alternatively, the hydrocarbon compound is a hydrocarbon having 1 to 5 carbon atoms, and includes at least one selected from the group consisting of dichloroethane, propyl chloride, isopropyl chloride, butyl chloride, isobutyl chloride, pentyl chloride, isopentyl chloride, n-butane, isobutane, n-pentane, isopentane, cyclopentane, and combinations thereof, and is environmentally friendly and exhibits excellent heat insulation. The foaming agent may be included in an amount of about 6 parts by weight to about 13 parts by weight based on about 100 parts by weight of the phenol foam.
[0055] The phenolic foam includes a curing agent, which may include an acidic curing agent selected from the group consisting of toluene sulfonic acid, xylene sulfonic acid, benzene sulfonic acid, phenol sulfonic acid, ethylbenzene sulfonic acid, styrene sulfonic acid, naphthalene sulfonic acid, and combinations thereof.
[0056] The acidic hardener may be included in an amount of about 9 parts by weight to about 20 parts by weight based on 100 parts by weight of the phenolic foam. The phenolic foam may exhibit appropriate crosslinking, hardening and foaming properties by including the hardener in the above range.
[0057] The method for producing the phenolic foam includes a step of foaming and curing the discharged foaming composition. The phenolic foam can be foamed and cured into a plate shape between conveyors in a curing oven. For example, the foaming and curing can be performed under a temperature condition of about 40°C to about 90°C. The foaming and curing can be performed for about 2 minutes to about 20 minutes, but is not limited thereto, and can be appropriately varied depending on the purpose and use of the invention.
[0058] Another embodiment of the present invention provides an insulating material including the phenolic foam, which can simultaneously satisfy excellent compressive strength, resistance to deflection, and excellent insulating properties, and can be used as an insulating material for buildings.
[0059] The insulating material for construction may further include a facing material on one or both sides of the phenolic foam, and the facing material may include aluminum to further improve flame retardancy.
[0060] (Example) Example 1: A foaming composition (25° C., 20,000 cps) containing 18 parts by weight of toluenesulfonic acid as a curing agent, 10 parts by weight of cyclopentane as a foaming agent, and a surfactant, relative to 100 parts by weight of a resol resin, was prepared.
[0061] Six nozzles with elliptical outlets (length (L) = 10 mm) with a length (L) / width (W) ratio of 1.5 were arranged in parallel at equal intervals on the lower surface material along a direction (Y-axis direction, width direction of the foam) perpendicular to the movement direction of the conveyor 7 (X-axis, i.e., the running direction of the surface material).
[0062] The foaming composition was then discharged at 40 k / min using the individual discharge ports onto a conveyor moving at a speed of 10 m / min, having a width of 1200 mm and a thickness of 190 mm, and having an ambient temperature of 70° C., whereupon the foaming composition was foamed and cured to produce a phenolic foam having a thickness of 190 mm.
[0063] Example 2: A phenolic foam was produced in the same manner as in Example 1, except that a nozzle having a circular outlet (length (L) = 10 mm) with a length (L) / width (W) ratio of 1 was used.
[0064] Comparative Example 1: A phenolic foam was produced in the same manner as in Example 1, except that a nozzle having an elliptical outlet (length (L) = 10 mm) with a length (L) / width (W) ratio of 2.5 was used.
[0065] Comparative Example 2: A phenolic foam was produced in the same manner as in Example 1, except that a nozzle having an elliptical outlet (length (L) = 10 mm) with a length (L) / width (W) ratio of 0.5 was used.
[0066] evaluation Experimental Example 1: Closed cell ratio of each piece The face material attached to the phenol foam of each of the examples and comparative examples was removed, and both surfaces of the foam to which the face material had been attached were cut by 5 mm each.
[0067] The foam was then cut uniformly from the surface into nine (N=9) slices in the thickness direction along the surface, producing foam slices measuring 2.5 cm (L) x 2.5 cm (W) x 2.0 cm (T) so as to include the middle portion throughout the entire thickness direction of the foam before cutting. Of the two slices at both ends including both surfaces of the foam, the slice with the lowest closed cell rate was designated N1 (first surface layer), and the other slice was designated N9 (second surface layer), with the individual slices designated N2, N3, N4, N5, N6, N7, N8, and N9 in order from N1. As a result, the middle slice (N c ) is N5.
[0068] The closed cell ratio of each of the specimens (N1 to N9) was measured using a closed cell ratio measuring device (Quantachrome, ULTRAPYC 1200e) according to KS M ISO 4590, and the results are shown in Table 1 below.
[0069] And, d1 is the distance from the first surface layer portion (N1) to the entire thickness of the foam having the minimum independent cell ratio (N min ) thickness (=N1~N min thickness) ratio (d1=N1~N min d1 is the thickness of the second surface layer portion (N9) / total thickness of the foam body, and d2 is the thickness of the section (N min ) thickness (=N9~N min thickness) ratio (d2=N9~N min In this case, the total thickness of the foam means the thickness of the foam after cutting off 5 mm from both surfaces of the foam to which the facing material was attached. min Thickness and N9~N min As shown in FIG. 1, the thickness of the section (N min ) in the thickness direction. In other words, d1 is the vertical distance from the upper surface of the first surface layer (N1) to the section (N min ) / total thickness of the foam, d2 is the thickness from the lower surface of the second surface layer (N1) to the section (N min ) / total thickness of the foam.
[0070] [Table 1]
[0071] Experimental example 2: Compressive strength The phenolic foams of the examples and comparative examples were prepared into test pieces of 150 mm (L) x 150 mm (W) x the same thickness as the foam including the face material, and the test pieces were placed between the wide plates of the LF Plus Universal Testing Machine of Lloyd Instruments, and the UTM was set to a speed of 10% mm / min of the thickness of the test piece, and a compressive strength test was started, and the strength at the first compressive yield point shown during the thickness reduction was recorded. The compressive strength was measured according to the method of KS M ISO 844 standard, and the results are shown in Table 2 below.
[0072] Experimental Example 3: Deflection Fig. 4 is a schematic diagram showing a simplified method for measuring the degree of deflection of a phenolic foam containing a facing material according to the present invention. The phenolic foam containing the facing material of the examples and comparative examples was placed on a flat floor so that the surface of the foam was in contact with the floor. The four corners (vertices) of the surface of the phenolic foam in contact with the floor and the distances (p1, p2, p3, p4) from the floor were then measured. The maximum separation distances (r1, r2) between the two longitudinal sides of the phenolic foam and the floor were then measured. At this time, when the foam is in close contact with the floor, each distance is "0".
[0073] The phenolic foam was left for 7 days under conditions of 25°C and 60% relative humidity, and the degree of deflection of the phenolic foam was then measured. In the case where the surface of the foam was bent concavely toward the floor (I), the distances (P1, P2, P3, P4) between the four corners (vertices) and the floor were measured using the same method as above, and the degree of deflection of the phenolic foam was recorded in Table 2 using the following formula 1. In the case where the surface of the foam was bent convexly toward the ceiling (II), the maximum separation distances (R1, R2) between the two sides in the length direction of the phenolic foam and the floor were measured, and the degree of deflection of the phenolic foam was recorded in Table 2 using the following formula 2.
[0074] [Formula 1] Degree of deflection (△S) = [|P1-p1|+|P2-p2|+|P3-p3|+|P4-p4|] / 4
[0075] [Formula 2] Degree of deflection (△S') = [|R1-r1|+|R2-r2|] / 2
[0076] Example 4: Dimensional stability FIG. 4 is a schematic diagram showing a simplified method for measuring the dimensional stability of a phenolic foam of the present invention.
[0077] The phenolic foams of the examples and comparative examples were prepared into test pieces measuring 100 mm (L) x 100 mm (W) x the thickness of the foam including the facing material. Lines were drawn at n (n=3) equal intervals in the length (L) and width (W) directions of the test pieces as shown in Figure 5, and the initial length (a) of each line was measured at 25°C.
[0078] The specimens were then left in an oven at 70°C for 48 hours, after which the length (a') at each point was measured, and the dimensional change rate (%) from the initial dimension was calculated according to the following formula 3, and the average value was recorded in Table 2. The dimensional stability was measured according to the method of KS M ISO 2796.
[0079] [Formula 3] Dimensional change rate (%) = (|Initial length (a) - Subsequent length (a')| / Initial length (a)) x 100
[0080] In the above formula 3, the initial length (a) is the length of each of n equal lines in the length (L) and width (W) directions of the foam, and the subsequent length (a') is the subsequent length (a') of each line at each point after the foam is left in an oven at 70° C. for 48 hours, where n may be 2 to 5.
[0081] Experimental Example 5: Initial Thermal Conductivity The phenolic resin foams of the examples and comparative examples were cut to 50 mm from either surface, and then cut to a size of 300 mm x 300 mm to prepare test pieces, which were then pretreated by drying at 70° C. for 12 hours. Thermal conductivity of the test pieces was measured using a thermal conductivity instrument HC-074-300 (EKO Co., Ltd.) at an average temperature of 20° C. according to the measurement conditions of KS L 9016 (plate heat flow meter measurement method), and the results are shown in Table 2 below.
[0082] Experimental Example 6: Long-term thermal conductivity The phenolic resin foams of the Examples and Comparative Examples were cut to 50 mm from either surface, and then cut into 300 mm x 300 mm pieces to prepare test pieces. The test pieces were dried at 70°C for 7 days and then at 110°C for 14 days in accordance with EN13823, and the thermal conductivity was measured at an average temperature of 20°C using a thermal conductivity instrument HC-074-300 (EKO Co., Ltd.). The results are shown in Table 2 below.
[0083] [Table 2]
[0084] As shown in Table 1 above, the phenol foam of the embodiment has excellent compressive strength, sufficiently suppresses the degree of deflection, and exhibits excellent thermal conductivity. As described above, the present invention has been described with reference to the exemplary drawings. However, the present invention is not limited to the embodiments and drawings disclosed in this specification, and it is clear that various modifications can be made by those skilled in the art within the scope of the technical concept of the present invention. It should be noted that, even if the effects of the configuration of the present invention are not explicitly described in the above description of the embodiments of the present invention, it is natural that the effects that can be predicted by the configuration should also be recognized. [Explanation of symbols]
[0085] d1 is the distance from the first surface layer (N1) to the entire thickness of the foam having the smallest closed cell ratio (N min ) thickness d2 The thickness of the second surface layer (NN ) to the section with the minimum closed cell ratio (N min ) thickness 10 Nozzle outlet L Length of outlet W outlet width 3. Surface material 7 Conveyor 100 Phenolic Foam
Claims
1. A phenolic foam having a thickness of 90 mm to 300 mm, When the foam is divided into N (N is an odd number of 7) pieces having a thickness of 10 mm to 30 mm from any surface of the foam, the first surface layer (N 1 The closed cell ratio of the second surface layer (N N ) having a smaller closed cell ratio than the N pieces of the slice (N min ) is the first surface layer portion (N 1 ) and the intermediate section (N c ) and a difference between the closed cell rate of the first surface layer portion (N 1 ) and the closed cell rate of the second surface layer portion (N N ) is 0.1% to 3%; the closed cell rate of the first surface layer portion (N 1 ) and the closed cell rate of the second surface layer portion (N N ) are each 85% or more; The closed cell ratio of the piece (N min ) having the minimum closed cell ratio is 70% or more; The second surface layer portion (N N ) has a maximum closed cell ratio; a difference in closed cell ratio between the second surface layer portion (N N ) and the piece (N min ) having the minimum closed cell ratio is 1% to 7%; Phenolic foam.
2. The ratio of d1 to d2 with respect to the total thickness of the foam is 0.2:0.8 to 0.45:0.55; The d1 is the thickness of the first surface layer portion (N 1 ) from the section with the minimum closed cell ratio (N min ) to the total thickness of the foam body, and d2 is the ratio of the thickness of the second surface layer portion (N N ) from the section with the minimum closed cell ratio (N min ) is the ratio of the thickness to the thickness of the 2. The phenolic foam of claim 1.
3. The deflection of the foam after 7 days under conditions of 25°C and 60% relative humidity is 0.1 cm to 0.7 cm. The phenolic foam of claim 1 or 2.
4. A thermal conductivity of 0.018 W / m K to 0.022 W / m K measured at an average temperature of 20° C. after drying at 70° C. for 7 days and then at 110° C. for 14 days in accordance with EN 13823. The phenolic foam of claim 1 or 2.
Citation Information
Patent Citations
Phenol resin foam plate and method for producing the same
JP2018095870A