VIM furnace refining method for high temperature alloys with ultra-high N content

The VIM furnace smelting method for ultra-high N-content high-temperature alloys uses chromium iron nitride addition and high-pressure argon to control nitrogen content, addressing yield and cost issues, producing high-quality products.

JP7573126B2Active Publication Date: 2024-10-24DAYE SPECIAL STEEL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023572990
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-05-25
Publication Date
2024-10-24
Estimated Expiration
2042-05-25

AI Technical Summary

Technical Problem

Existing VIM furnace methods struggle to precisely control the nitrogen content in ultra-high N-content high-temperature alloys, leading to low yield rates and high production costs due to nitrogen volatilization under high vacuum conditions.

Method used

A VIM furnace smelting method that includes adding a nitrogen-containing substance like chromium iron nitride in the latter stage, filling with high-pressure argon gas, and controlling the addition time to maintain nitrogen content, ensuring precise control and increased yield.

Benefits of technology

The method achieves precise nitrogen content control, increasing yield rates and reducing production costs by minimizing nitrogen loss and foreign defects, resulting in high-quality products like ring parts.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention discloses a VIM furnace smelting method for ultra-high N content high temperature alloy and the ultra-high N content high temperature alloy, the VIM furnace smelting method includes a smelting step in the VIM furnace and a pouring step, and in the latter stage of the smelting, a nitrogen-containing material is added to the VIM furnace to adjust the N content. Through the comprehensive improvement of the raw materials and smelting process, the present invention improves the yield of N element in the VIM furnace smelting process and realizes accurate control of the N element content of the high temperature alloy, so that the target content of nitrogen element can be guaranteed and an ideal product can be obtained.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention belongs to the field of vacuum smelting of high temperature alloys in the metallurgical industry, specifically to a VIM furnace smelting method for ultra-high N content high temperature alloys. [Background technology]

[0002] Ultra-high N content high temperature alloy is a commonly used material in power plants, and is used to manufacture many products such as forgings, ring parts, etc. Due to the influence of the working environment and the special requirements for the cleanliness of the alloy, the smelting of this alloy must be produced using a VIM furnace. In the process of smelting ultra-high N content high temperature alloy in a VIM furnace, under high vacuum conditions, the nitrogen element is easily volatilized from the vacuum system, and the ideal target value cannot be obtained. In the high vacuum environment of the VIM, the control of ultra-high content N element cannot usually be effectively realized, and the non-defective product rate obtained by the traditional smelting process is low. Summary of the Invention [Problem to be solved by the invention]

[0003] In view of the shortages and defects existing in the prior art, one of the objectives of the present invention is to provide a method for VIM furnace smelting of ultra-high N content high temperature alloy (which can also be said to be a method for precisely controlling the N content in the VIM furnace smelting process of ultra-high N content high temperature alloy). By adopting this process method, the target content of nitrogen element can be guaranteed and the yield rate of the product can be greatly improved. [Means for solving the problem]

[0004] The technical solutions adopted to solve the technical problems of the present invention are as follows:

[0005] The VIM furnace smelting method for ultra-high N content high temperature alloy includes a smelting step in a VIM furnace and a pouring step, and in the latter stage of the smelting, a nitrogen-containing material is added to the VIM furnace to adjust the N content, where the VIM furnace is a vacuum induction smelting furnace.

[0006] In the above-mentioned VIM furnace smelting method for ultra-high N content high temperature alloy, as a preferred embodiment, the N mass% in the ultra-high N content high temperature alloy is 1500-3000ppm, preferably 2000-3000ppm, more preferably 2700-3000ppm. That is, after the pouring step, the N content in the ultra-high N content ultra-high temperature alloy obtained is 1500-3000ppm, preferably 2000-3000ppm, more preferably 2700-3000ppm.

[0007] In the above-mentioned VIM furnace smelting method for ultra-high N content high temperature alloy, as a preferred embodiment, the nitrogen-containing material is a nitrogen-containing alloy with a nitrogen content of 3% or more by mass%, more preferably at least one of chromium iron nitride, manganese nitride, and aluminum nitride. Preferably, the nitrogen-containing material (e.g., chromium iron nitride) is a nitrogen-containing material after baking treatment, more preferably, the baking temperature is 750-1100°C and the baking time is 6 hours or more. Usually, the nitrogen-containing material (e.g., chromium iron nitride) is not baked, whereas the present invention innovatively bakes the nitrogen-containing material (e.g., chromium iron nitride) to remove gas in the nitrogen-containing material (mainly H here), reduce the temperature difference between the nitrogen-containing material and the steel liquid, and avoid a severe impact on the yield of N by the reaction. More preferably, the baking device is located in the same work area as the VIM furnace. Among these, if the temperature is less than 750°C, it is ineffective for removing H, and if the temperature exceeds 1100°C, a part of the N dissolved in the chromium iron nitride is decomposed. Finally, the baking time is preferably 6 hours or more in order to affect the N yield and to have an effect of removing H.

[0008] In the above-mentioned VIM furnace smelting method for ultra-high N content high temperature alloy, as a preferred embodiment, in the later stage of the smelting, before adding the nitrogen-containing material (e.g., iron chromium nitride), the VIM furnace is filled with an inert gas, preferably the inert gas is argon gas, and the pressure of the argon gas in the VIM furnace is 10000 Pa or more, and the argon gas pressure is set to be as high as possible within the range of the power that the equipment can tolerate. If the argon gas pressure is too low, the N content of the product alloy will not reach the requirement, and the N yield will be low after the nitrogen-containing material (e.g., iron chromium nitride) is added. The vacuum system of the vacuum induction furnace is a dynamic equilibrium process, and some N will be discharged from the vacuum system to the outside of the furnace, so it is necessary to replenish more nitrogen-containing materials (such as iron chromium nitride), which will increase the cost or cause the final composition to be rejected, which is the reason for being judged to be discarded. On the other hand, filling with high pressure argon gas exerts compressive stress on the steel liquid surface, and increases the resistance of N brought into the steel liquid by nitrogen-containing substances (such as iron chromium nitride) to be discharged from the liquid surface, and the increased pressure inside the furnace also slows down the progress of dynamic equilibrium in the furnace system. Preferably, the filling of the inert gas continues until the end of the pouring.

[0009] Preferably, the smelting includes a melting period and a refining period, and the later period of the smelting refers to the later period of the refining.

[0010] In the above-mentioned VIM furnace smelting method for ultra-high N content high temperature alloy, in a preferred embodiment, the time from adding the nitrogen-containing material (e.g., iron chromium nitride) to the start of pouring is 15 minutes or less. If the time from adding the nitrogen-containing material (e.g., iron chromium nitride) to the start of pouring is too long, the yield of N in the alloy decreases.

[0011] In the above-mentioned VIM furnace smelting method for an ultra-high N content high temperature alloy, as a preferred embodiment, in the smelting step, when a raw material is added to the VIM furnace before smelting, the amount of metallic chromium added is 80-85% of the total mass of the metallic chromium raw material, and the remaining 15-20% of the metallic chromium is added according to a required amount in the later stage of smelting before charging an inert gas to adjust the composition.

[0012] In the above-mentioned VIM furnace smelting method for the ultra-high N content high temperature alloy of the present invention, the ultra-high N content high temperature alloy of the present invention is a kind of metallic material based on iron and nickel that can work continuously at high temperatures of 600°C or higher, and preferably a kind of metallic material that can work for a long time under the action of stress.

[0013] In the above-mentioned VIM furnace smelting method for the ultra-high N content high temperature alloy, as a preferred embodiment, the composition of the ultra-high N content high temperature alloy is, in mass%, C: 0.02-0.10%, Cr: 23.00-27.00%, Ni: 35.00-39.00%, W: ≦0.50%, Mo: ≦1.00%, P: ≦0.04%, S: ≦0.03%, Mn: ≦1.50%, Si: ≦1.00%, B: ≦0.01%, Nb: 0.40-0.90%, Co: ≦3.00%, N: 0.15-0.30%, Al: ≦0.40%, Ti: ≦0.20%, Cu: ≦0.50%, Fe: balance.

[0014] A super-high N content high temperature alloy, the super-high N content high temperature alloy being produced by using the VIM furnace smelting method for the super-high N content high temperature alloy.

[0015] The technical principle of the present invention to obtain the ideal target N content under high vacuum conditions by VIM smelting is that the fixed nitrogen content of ferrochromium nitride is much larger than that of other alloy raw materials, so ferrochromium nitride is used as the medium to carry the N element of this high-temperature alloy. However, since VIM is smelted under high vacuum conditions and the N element is discharged from the vacuum system to the outside of the furnace in the form of a free state, it is very difficult to effectively and accurately control the nitrogen content. Therefore, the present invention controls the timing of adding ferrochromium nitride (adding it at the later stage of smelting), controls the addition conditions (filling high-pressure inert gas before adding ferrochromium nitride to improve the yield of N element), and controls the time from adding ferrochromium nitride to pouring. When the yield of N element is guaranteed, it is cast into an ingot to obtain a high-temperature alloy product with the ideal target value. Effect of the Invention

[0016] The present invention has the following positive effects compared to the prior art:

[0017] (1) The method of the present invention is simple, easy to implement, and effective, and does not require additional dedicated equipment or process facilities.

[0018] (2) The present invention (high temperature alloy, the proportion of alloy is much higher than that of steel) has increased the yield of N element in the VIM furnace smelting process through the comprehensive improvement of raw materials and smelting processes, and realized the precise control of the N element content of this high temperature alloy, so as to guarantee the target content of nitrogen element and obtain ideal products.

[0019] (3) The present invention effectively solves the problem of N element yield under high vacuum conditions, increases the yield rate of products such as ring parts, and reduces production costs for manufacturing enterprises.

[0020] (4) The present invention can ensure the yield of nitrogen element by performing a rational baking process on ferrochromium nitride, and can reduce the moisture in ferrochromium nitride from bringing H into the steel liquid.

[0021] (5) In the present invention, by filling the steel with Ar gas of 10,000 Pa or more, the pressure is changed from the conventional high vacuum state to a high pressure state, causing the steel liquid surface to be subjected to dense pressure stress, thereby enhancing the solubility of N in the steel liquid and ultimately increasing the yield.

[0022] (6) The present invention controls the time from adding ferrochromium nitride to pouring after filling with argon, thereby ensuring the yield of N and preventing the occurrence of foreign metal inclusion defects due to incomplete melting of ferrochromium nitride. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] In order to prominently express the objectives, technical solutions and advantages of the present invention, the present invention will be further described below based on examples, which do not limit the present invention but are expressed by way of explanation of the present invention. The technical solutions of the present invention are not limited to the specific embodiments listed below, and also include any combination between each specific embodiment.

[0024] The iron chromium nitride of the present invention may be any iron chromium nitride having a nitrogen content of 3 wt % or more, and in the following examples, iron chromium nitride having the number FeNCr3-A will be taken as an example.

[0025] <Example 1> Example 1 of the present invention uses a VIM furnace with a nominal capacity of 6 tons to smelt this ultra-high nitrogen content high temperature alloy, and includes the following steps:

[0026] Step 1: Baking ferrochromium nitride: The ferrochromium nitride is baked in a high-temperature annealing furnace in the factory.

[0027] Here, the baking parameters of the ferrochromium nitride are an N content (mass ratio of N in the ferrochromium nitride) of 5.1%, a baking (heating) temperature of 930° C., and a baking time of 8.5 hours.

[0028] Step 2: Pre-smelting charge: Ni, Fe, Nb, Cr and other raw materials are fed into the VIM furnace one after another. Chromium nitride iron residue is 100%, no addition. Metallic chromium residue is 20%, no addition.

[0029] Step 3: Smelting process: Smelt the raw materials (including melting and refining stages, the indicators of the completion of the melting stage are monitoring the complete melting temperature of 1530°C, the refining stage temperature of 1510°C, and the time of 130 minutes), add the required amount of metallic chromium in the later stage of refining to adjust the composition, then fill the furnace with argon gas in the later stage of refining to make the pressure in the furnace 10000pa, and then add ferrochromium nitride to adjust the N content.

[0030] Step 4: Pouring process: The steel liquid obtained during the smelting process is poured into the pot. The time from adding iron chromium nitride to the start of pouring (tapping) is 14 minutes.

[0031] Step 5: Verification: The casting component contents (wt%) are verified according to the standard requirements: C: 0.061%, Cr: 25.40%, Ni: 37.03%, P: 0.006%, S: 0.002%, Mn: 0.74%, Si: 0.470%, B: ≦ 0.01%, Nb: 0.63%, N: 0.2857%, Al: 0.230%, Ti: 0.05%, Cu: 0.01%, H: 0.0001%.

[0032] The nitrogen yield (ie, nitrogen yield rate: the ratio of the nitrogen content in the obtained product to the nitrogen content introduced in the raw materials used) and the non-defective product rate are 76.92% and 100%, respectively.

[0033] <Example 2> Example 2 of the present invention uses a VIM furnace with a nominal capacity of 6 tons to smelt this ultra-high nitrogen content high temperature alloy, and includes the following steps:

[0034] Step 1: Baking ferrochromium nitride: The ferrochromium nitride is baked in a high-temperature annealing furnace in the factory.

[0035] Here, the baking parameters of the iron chromium nitride are N content of 5.1%, baking (heating) temperature of 930° C., and baking time of 8.5 hours.

[0036] Step 2: Pre-smelting charge: Ni, Fe, Nb, Cr and other raw materials are fed into the VIM furnace one after another. Chromium nitride iron residue is 100%, no addition. Metallic chromium residue is 20%, no addition.

[0037] Step 3: Smelting process: The raw material is smelted (including melting and refining periods, and the indicators of the completion of the melting period are the complete melting temperature of 1530°C, the refining period temperature of 1510°C, and the time of 130 minutes), and the necessary amount of metallic chromium is added during the smelting process to adjust the composition, and then argon gas is filled in at the later stage of refining to make the pressure 10000pa, and then chromium iron nitride is added to adjust the N content.

[0038] Step 4: Pouring process: The time from pouring the steel liquid obtained during the smelting process and adding ferrochromium nitride to the start of pouring (tapping) is 15 minutes.

[0039] Step 5: Verification: The casting component contents (wt%) are verified according to the standard requirements: C: 0.060%, Cr: 25.60%, Ni: 37.00%, P: 0.005%, S: 0.001%, Mn: 0.76%, Si: 0.440%, Nb: 0.63%, N: 0.2893%, Al: 0.250%, Ti: 0.04%, Cu: 0.01%. H: 0.0001%.

[0040] The nitrogen yield and non-defective rate are 76.90% and 100%, respectively.

[0041] <Example 3> The same as in Example 1, except that the baking temperature of the iron chromium nitride was 800°C.

[0042] Step 5: Verification: The casting component contents (wt%) are verified according to the standard requirements: C: 0.061%, Cr: 25.30%, Ni: 37.05%, P: 0.005%, S: 0.002%, Mn: 0.75%, Si: 0.500%, B: ≦ 0.01%, Nb: 0.65%, N: 0.2937%, Al: 0.250%, Ti: 0.05%, Cu: 0.01%, H: 0.00015%.

[0043] The nitrogen yield and non-defective rate are 76.70% and 100%, respectively.

[0044] <Example 4> The same as in Example 1, except that the baking temperature of the iron chromium nitride was 1050°C.

[0045] Step 5: Verification: The casting component contents (wt%) are verified according to the standard requirements: C: 0.059%, Cr: 25.33%, Ni: 37.00%, P: 0.004%, S: 0.001%, Mn: 0.70%, Si: 0.480%, B: ≦ 0.01%, Nb: 0.62%, N: 0.2900%, Al: 0.250%, Ti: 0.04%, Cu: 0.01%, H: 0.00015%.

[0046] The nitrogen yield and non-defective rate are 76.80% and 100%, respectively.

[0047] <Comparative Example 1> The same as in Example 1, except that the baking temperature of the iron chromium nitride was 650°C.

[0048] Step 5: Verification: The casting component contents (wt%) are verified according to the standard requirements: C: 0.061%, Cr: 25.35%, Ni: 37.01%, P: 0.005%, S: 0.001%, Mn: 0.72%, Si: 0.500%, B: ≦ 0.01%, Nb: 0.65%, N: 0.2955%, Al: 0.250%, Ti: 0.05%, Cu: 0.01%, H: 0.00035% (the lower the H content, the better during the use of the alloy; too high H will affect the durability and fatigue life during the use of the user).

[0049] The nitrogen yield is 76.80%.

[0050] <Comparative Example 2> The same as in Example 1, except that the baking temperature of the iron chromium nitride was 1200°C.

[0051] Step 5: Verification: The casting component contents (wt%) are verified according to the standard requirements: C: 0.060%, Cr: 25.30%, Ni: 37.05%, P: 0.005%, S: 0.001%, Mn: 0.72%, Si: 0.460%, B: ≦ 0.01%, Nb: 0.60%, N: 0.2890%, Al: 0.250%, Ti: 0.05%, Cu: 0.01%, H: 0.00009%.

[0052] The nitrogen yield is 63.34%.

[0053] <Comparative Example 3> The procedure was the same as in Example 1, except that the pressure inside the furnace was set to 9000 Pa by filling the furnace with argon gas.

[0054] Step 5: Verification: The casting component contents (wt%) are verified according to the standard requirements: C: 0.059%, Cr: 25.33%, Ni: 37.10%, P: 0.005%, S: 0.001%, Mn: 0.70%, Si: 0.510%, B: ≦ 0.01%, Nb: 0.66%, N: 0.2910%, Al: 0.260%, Ti: 0.06%, Cu: 0.01%, H: 0.0001%.

[0055] The nitrogen yield and non-defective rate are 74.38% and 100%, respectively.

[0056] <Comparative Example 4> The same as in Example 1, except that the time from addition of iron chromium nitride to tapping was 17 minutes.

[0057] The casting component contents (wt%) verified according to standard requirements are C: 0.062%, Cr: 25.28%, Ni: 37.15%, P: 0.005%, S: 0.001%, Mn: 0.60%, Si: 0.500%, B: ≦ 0.01%, Nb: 0.67%, N: 0.2913%, Al: 0.250%, Ti: 0.06%, Cu: 0.01%, H: 0.0001%.

[0058] The nitrogen yield and non-defective rate are 75.80% and 100%, respectively.

[0059] <Comparative Example 5> In this comparative example, step 1 of Example 1, ie, the baking step of iron chromium nitride, is omitted, and the other steps are the same as those of Example 1.

[0060] The casting component contents (wt%) verified according to standard requirements are C: 0.059%, Cr: 25.30%, Ni: 37.20%, P: 0.005%, S: 0.001%, Mn: 0.68%, Si: 0.520%, B: ≦ 0.01%, Nb: 0.68%, N: 0.2910%, Al: 0.250%, Ti: 0.06%, Cu: 0.01%, H: 0.0005%.

[0061] If the chromium nitride is not baked, a large amount of elemental H will be carried into the alloy from the chromium nitride, and the content of elemental H will be too high, resulting in waste.

[0062] The nitrogen yield and non-defective rate are 76.15% and 0.0%, respectively.

[0063] <Comparative Example 6> In this comparative example, the step of filling the furnace with argon gas in the smelting process of Example 1 is omitted, that is, argon gas is not filled in the later stage of refining, but the other steps are the same as those of Example 1.

[0064] The casting component contents (wt%) according to the standard requirements are C: 0.059%, Cr: 25.34%, Ni: 37.15%, P: 0.005%, S: 0.001%, Mn: 0.71%, Si: 0.520%, B: ≦ 0.01%, Nb: 0.65%, N: 0.1010%, Al: 0.270%, Ti: 0.06%, Cu: 0.01%, H: 0.0001%.

[0065] If argon gas is not filled, after the ferrochromium nitride put into the furnace is melted and decomposed, some of the nitrogen element will be discharged out of the furnace as free N2 through the vacuum system under high vacuum, which will result in a low yield of nitrogen element, and the nitrogen element in the alloy will not meet the standard requirement, and will ultimately be waste.

[0066] The nitrogen yield and non-defective rate are 33.34% and 0.0%, respectively.

Claims

1. 1. A VIM furnace smelting process for ultra-high N content high temperature alloys, comprising the steps of: The method includes a smelting step performed in the VIM furnace and a pouring step, The smelting includes a melting period and a refining period, and the latter period of the smelting refers to the later period of the refining period. In the later period of the smelting, a nitrogen-containing material is added to the VIM furnace to adjust the N content; The nitrogen-containing material is a nitrogen-containing material after baking, the baking temperature is 750 to 1100° C., and the baking time is 6 hours or more; In the latter stage of the smelting, before the nitrogen-containing material is added, the VIM furnace is filled with an inert gas, the time from the addition of the nitrogen-containing material to the start of pouring is 14 to 15 minutes, the inert gas is argon gas, and the pressure of the argon gas in the VIM furnace is 10,000 Pa or more; In the smelting step, when the raw material is added to the VIM furnace before smelting, the amount of metallic chromium added is 80 to 85% of the total mass of the metallic chromium raw material, and the remaining 15 to 20% of the metallic chromium is added in a required amount before the inert gas is charged in the later stage of smelting to adjust the composition; The composition of the ultra-high N content high temperature alloy in mass % is as follows: C: 0.02-0.10%, Cr: 23.00-27.00%, Ni: 35.00-39.00%, W: ≦0.50%, Mo: ≦1.00%, P: ≦0.04%, S: ≦0.03%, Mn: ≦1.50%, Si: ≦1.00%, B: ≦0.01%, Nb: 0.40-0.90%, Co: ≦3.00%, N: 0.15-0.30%, Al: ≦0.40%, Ti: ≦0.20%, Cu: ≦0.50%, Fe: balance. A method for smelting high temperature alloys with ultra-high N content in a VIM furnace.

2. The N mass content in the ultra-high N content high temperature alloy is 2000 to 3000 ppm; 2. The VIM furnace smelting method for ultra-high N content high temperature alloy according to claim 1.

3. The N mass content in the ultra-high N content high temperature alloy is 2700 to 3000 ppm; 3. The VIM furnace smelting method for ultra-high N content high temperature alloys according to claim 2.

4. The nitrogen-containing material is a nitrogen-containing alloy having a nitrogen content of 3% by mass or more.

2. The VIM furnace smelting method for ultra-high N content high temperature alloy according to claim 1.

5. The nitrogen-containing material is at least one of chromium iron nitride, manganese nitride, and aluminum nitride.

5. The VIM furnace smelting method for ultra-high N content high temperature alloys according to claim 4.

6. The baking equipment is located in the same work area as the VIM furnace.

6. The VIM furnace smelting method for ultra-high N content high temperature alloys according to claim 5.

7. The inert gas is introduced until the pouring is completed.

2. The VIM furnace smelting method for ultra-high N content high temperature alloy according to claim 1.

8. The ultra-high N content high temperature alloy is a type of metal material based on iron and nickel that can continue to function at high temperatures of 600°C or higher.

2. The VIM furnace smelting method for ultra-high N content high temperature alloy according to claim 1.

9. The ultra-high N content high temperature alloy is a type of metallic material that operates for a long time under stress.

9. The VIM furnace smelting method for ultra-high N content high temperature alloys according to claim 8.

Citation Information

Patent Citations

  • High-temperature alloy, alloy hood manufactured from same and manufacturing technology of alloy hood

    CN103173692A

  • High-nitrogen austenitic stainless steel for vascular stent and application thereof

    CN103233174A

  • Heat-resistant cast austenitic stainless steel with excellent high-temperature comprehensive properties

    CN104593692A

  • Production of high-strength oil well pipe of high stress corrosion cracking resistance

    JP1983006927A

  • Production of high nitrogen steel

    JP1995070691A