Method and apparatus for manufacturing aluminum alloy cast plate
The twin-roll continuous casting method with controlled injection angles and flow velocities effectively prevents surface cracking in high Mg content aluminum alloy sheets, ensuring high-speed and stable production of high-quality cast plates.
Patent Information
- Application Number
- JP2020189738
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-13
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2040-11-13
AI Technical Summary
High Mg content aluminum alloy sheets tend to develop surface cracks during high-speed casting using twin-roll casters, leading to unstable quality and potential defects in the cast plates.
A twin-roll continuous casting method is employed with specific parameters: setting the molten metal injection angle between 0 to 20 degrees, controlling the distance from the injection point to the molten metal pool, and ensuring the molten metal flow velocity is parallel to the roll surface, while using a second rotating roll positioned at an angle between 0 to 90 degrees relative to the first roll.
This method suppresses surface cracking in high Mg content aluminum alloy sheets, enabling high-speed casting without requiring large-scale equipment, resulting in stable and high-quality cast plates.
Smart Images

Figure 0007573265000003 
Figure 0007573265000004 
Figure 0007573265000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a method and an apparatus for producing an aluminum alloy cast plate. [Background technology]
[0002] DC casting is widely used in the production of alloy plates. In the case of DC casting, a multi-stage rolling process is required after casting to obtain a metal plate of a desired thickness. Repeated rolling is expected to eliminate defects such as segregation, but there are problems such as the need for large-scale production facilities. In recent years, a manufacturing method has been proposed that reduces the number of rolling stages in the rolling process by ejecting molten alloy onto the circumferential surface of a rapidly rotating cooling roll and rapidly solidifying it.
[0003] For example, Non-Patent Document 1 discloses a twin roll caster method in which casting is performed between two rotating rolls, and a method for continuously casting a magnesium alloy is disclosed in which two rolls are arranged above and below in a horizontal format. [Prior art documents] [Non-patent literature]
[0004] [Non-Patent Document 1] Continuous casting of AZ31B magnesium alloy thin plate using semi-solid slurry, Hirokazu Shimada et al., Light Metals, Vol. 58, No. 7 (2008) Summary of the Invention [Problem to be solved by the invention]
[0005] Al-Mg alloy sheets with a high Mg content of 2% by mass or more, especially 4% by mass or more, are excellent in ductility and durability, and are lightweight, so their practical use as automobile panels and the like is desirable. However, when Al-Mg alloy sheets with a high Mg content are cast at high speed using a twin roll caster, surface cracks tend to occur, making it difficult to obtain aluminum alloy cast sheets with stable quality. In particular, there was a problem that surface cracks tend to occur when the roll peripheral speed was increased to 10 to 120 m / min. If the surface quality of aluminum alloy cast sheets is poor, defects are likely to occur during sheet forming.
[0006] The present invention has been made in view of the above circumstances, and has an object to provide a method for producing an aluminum alloy cast plate in which the occurrence of the above-mentioned surface cracks, etc. is suppressed even when the Mg content is high, by a twin-roll continuous casting method at high speed without requiring large-scale equipment, and an apparatus for producing the aluminum alloy cast plate. [Means for solving the problem]
[0007] A first aspect of the present invention is a method for producing an aluminum alloy cast plate containing 2% by mass or more of Mg by a twin-roll continuous casting method, comprising pouring a molten aluminum alloy containing 2% by mass or more of Mg into a molten metal pouring point on the surface of a first rotating roll, and pressing, cooling and solidifying the molten aluminum alloy between the first rotating roll and the second rotating roll, a melt pouring tool for pouring the melt into the melt pouring point, the angle θ1 between the pouring direction of the melt into the melt pouring point and the tangent of the surface of the first rotating roll at the melt pouring point is set to be 0 degrees or more and 20 degrees or less; forming a molten metal puddle for holding the molten metal between the first rotating roll and the second rotating roll; The distance L from the molten metal pouring point to the molten metal pool is set to more than 0 mm and (roll peripheral speed (mm / sec) × 0.2 sec) mm or less, This is a method for producing an aluminum alloy cast plate, characterized in that the flow velocity of the molten metal is set to be equal to or higher than the roll peripheral speeds of the first rotating roll and the second rotating roll.
[0008] A second aspect of the present invention is a method for producing an aluminum alloy cast plate as described in the first aspect, in which the second rotating roll is positioned so that an angle θ2 formed by a line connecting the opposing positions of the first rotating roll and the second rotating roll and the center of the first rotating roll, and the vertical radius of the first rotating roll, is within a range of more than 0 degrees and less than 90 degrees.
[0009] A third aspect of the present invention is an apparatus for producing an aluminum alloy cast plate containing 2% by mass or more of Mg by a twin-roll continuous casting method, comprising: A first rotating roll having a cooling capacity; a molten metal pouring tool for pouring a molten metal of an aluminum alloy containing 2% by mass or more of Mg into a molten metal pouring point on a surface of the first rotating roll; A second rotating roll is provided for pressing, cooling and solidifying the molten metal poured at the molten metal pouring point together with the first rotating roll, This is an apparatus for manufacturing aluminum alloy cast plate, characterized in that the angle θ1 between the molten metal pouring tool and a tangent to the surface of the first rotating roll at the molten metal pouring point is greater than or equal to 0 degrees and less than or equal to 20 degrees.
[0010] A fourth aspect of the present invention is a manufacturing apparatus for aluminum alloy cast plate according to the third aspect, in which the second rotating roll is positioned so that an angle θ2 formed by a line connecting the opposing positions of the first rotating roll and the second rotating roll and the center of the first rotating roll, and the vertical radius of the first rotating roll, is within a range of more than 0 degrees and less than 90 degrees. Effect of the Invention
[0011] According to the present invention, there are provided a method for producing an aluminum alloy cast plate in which the occurrence of the above-mentioned surface cracks and the like is suppressed even when the Mg content is high, by a twin-roll continuous casting method at high speed without requiring large-scale equipment, and an apparatus for producing the aluminum alloy cast plate. [Brief description of the drawings]
[0012] [Figure 1] FIG. 2 is a schematic side view for explaining the manufacturing method of the aluminum alloy cast plate of the present embodiment. [Diagram 2] FIG. 2 is a schematic side view showing an example of a molten metal pouring tool used in the manufacturing method of the aluminum alloy cast plate of the present embodiment. [Diagram 3] 4 is a schematic diagram for explaining a distance L from a molten metal pouring point to the molten metal pool. FIG. [Figure 4] FIG. 1 is a diagram showing an embodiment of a twin-roll continuous casting method to which the manufacturing method of the aluminum alloy cast plate of the present embodiment can be applied. [Diagram 5] FIG. 2 is a schematic side view illustrating a preferred embodiment of the method for producing an aluminum alloy cast plate according to the present embodiment. [Figure 6] FIG. 4 is a schematic side view for illustrating a manufacturing method of another aluminum alloy cast plate according to the present embodiment. [Figure 7] FIG. 1 is a schematic side view showing a conventional manufacturing apparatus for an aluminum alloy cast plate. [Figure 8] 4 is a photograph showing the observation results of surface cracks in an example. [Figure 9] FIG. 1 is a diagram showing the relationship between surface cracks and the width of the molten metal to be poured in the examples. [Figure 10] 1 is a photograph of a cross-sectional structure of an aluminum alloy cast plate according to the present embodiment. [Figure 11] 1 is a photograph of a cross-sectional structure of a conventional aluminum alloy cast plate. [Figure 12] 4 is a cross-sectional structural photograph of the aluminum alloy cast plate of the present embodiment and a conventional aluminum alloy cast plate after etching with Weck's reagent. [Figure 13] 4 is a photograph showing the observation results of surface cracks after cold rolling in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Aluminum alloys used for automobiles and cans have a magnesium content of 2% or more by mass, such as A5052 with a magnesium content of about 2.5% by mass, A5182 with a magnesium content of about 5% by mass, and AC7A, which have a magnesium content of about 5% by mass. When cast using a high-speed twin-roll caster, surface cracks are likely to occur. To solve this problem, a method of using a roll with a mesh or groove formed on the roll surface is considered, but this method is difficult to process the roll and has durability problems. In addition, when casting aluminum alloys with a high magnesium content, surface cracks could not be suppressed even if a mesh or the like was formed on the roll surface.
[0014] The present inventors have conducted extensive research to solve the above problems. As a result, they have found that, when producing an aluminum alloy cast plate containing 2% by mass or more of Mg by a twin-roll continuous casting method, the production method of this embodiment, in which the pouring angle of the molten metal into the first rotating roll is specified, can produce an Al-Mg alloy cast plate with a high Mg content (2% by mass or more) and stable quality with suppressed surface cracking at high speed without reducing the roll peripheral speed. The production method and production apparatus of the aluminum alloy cast plate according to this embodiment will be described in order below.
[0015] [Method of manufacturing aluminum alloy cast plate] With respect to a manufacturing method of an aluminum alloy cast plate, an embodiment of the present invention will be described below with reference to the drawings. However, the embodiment is merely an example for embodying the technical idea of the present invention, and the technical idea of the present invention is not limited to the embodiment.
[0016] FIG. 1 is a side view diagrammatically illustrating a method for manufacturing an aluminum alloy cast plate according to the present embodiment. The side view is a view of the manufacturing apparatus viewed in the direction of the rotation axis of a first rotating roll and a second rotating roll. The manufacturing apparatus 1 for an aluminum alloy cast plate includes at least a first rotating roll 2 having a cooling capacity, a melt injector 3 for injecting a melt 5 of an aluminum alloy containing 2% by mass or more of Mg into a melt injecting point 6 on the surface of the first rotating roll 2, and a second rotating roll 4 arranged opposite the first rotating roll 2 and for pressing, cooling, and solidifying the melt 5 injected into the surface of the first rotating roll 2 together with the first rotating roll 2. In casting, the melt 5 of an aluminum alloy containing 2% by mass or more of Mg is injected from a crucible 8 through the melt injector 3 into the melt injecting point 6 on the surface of the first rotating roll 2. The melt 5 injected into the melt injecting point 6 on the surface of the first rotating roll 2 is held between the first rotating roll 2 and the second rotating roll 4 to form a melt pool 7. The molten metal forming the molten metal pool 7 is pressed, cooled, and solidified by the first rotating roll 2 and the second rotating roll 4, to obtain an aluminum alloy cast plate 9 containing 2 mass % or more of Mg.
[0017] The melt pouring point 6 is a position at which the melt 5 is poured onto the surface of the first rotating roll 2. In Fig. 1, the melt pouring point 6 is located closer to the second rotating roll 4 than the apex A of the first rotating roll 2, but is not limited to this. The melt pouring point 6 can be set on the surface of the first rotating roll 2 in Fig. 1, for example, within a range from position G in Fig. 1 to a position facing the second rotating roll 4 in the rotation direction.
[0018] In this embodiment, the melt 5 is poured into the melt pouring point 6 by aligning the melt 5 with the melt pouring tool 3. The melt pouring tool 3 is disposed at a position where it is almost in contact with the first rotating roll 2. The angle θ1 between the melt pouring tool 3 for pouring the melt 5 into the melt pouring point 6 and the tangent B of the first rotating roll surface at the melt pouring point 6 is set to 0 degrees (°) or more and 20 degrees (°) or less. The melt pouring tool 3 pours the melt into the melt pouring point 6, that is, the angle θ1 between the flow direction of the melt 5 at the melt pouring point 6 on a plane perpendicular to the rotation axis of the first rotating roll 2 and the tangent of the first rotating roll surface at the melt pouring point (hereinafter, the angle θ1 may be simply referred to as the "melt pouring angle θ1"), which is set to 0 degrees or more and 20 degrees or less. The arrangement of the rolls and the like constituting the manufacturing apparatus of this embodiment, including the above angles, is specified when the manufacturing apparatus is viewed in the direction of the rotation axes of the first rotating roll and the second rotating roll. By setting the molten metal injection angle θ1 to 20 degrees or less, the component perpendicular to the roll surface of the molten metal flow velocity is small, making it possible to increase the flow velocity of the molten metal; furthermore, if the speed of the molten metal parallel to the roll surface is greater than or equal to the roll peripheral speed, the actual contact area between the roll and the molten metal becomes narrower and heat transfer decreases, which is thought to result in suppression of excessive cooling by the first rotating roll and sufficient suppression of surface cracks in the cast plate. The molten metal injection angle θ1 is preferably 15 degrees or less, and more preferably 10 degrees or less. On the other hand, from the viewpoint of practical pouring, the molten metal injection angle θ1 is set to 0 degrees or more.
[0019] The melt injector 3 may be of any shape as long as it can inject the melt 5 onto the surface of the first rotating roll 2 so that the angle θ1 between the direction of injection of the melt 5 to the melt injection point 6 and the tangent B of the surface of the first rotating roll 2 at the melt injection point 6 is 0 degrees or more and 20 degrees or less. From the viewpoint of easily forming the angle θ1, the melt injector 3 preferably has a straight portion ending at the melt injection point 6. The shape of the cross section of the melt injector 3 perpendicular to the injection direction of the melt 5 may be, for example, a semicircular, cylindrical, inverted trapezoidal, or other polygonal shape. For example, a melt injector having a trough shape and made of a fire-resistant material may be used. The melt injector 3 is not limited to a straight line shape as long as it satisfies the angle θ1 at the melt injection point 6. The melt injector may have a corner 11 as shown in FIG. 2, for example. When corner 11 is provided, the angle of corner 11 and the distance from the molten metal pouring point to corner 11 can be appropriately determined; for example, the distance from the molten metal pouring point to corner 11 can be 10 mm or more.
[0020] 1, a refractory crucible 8 is used to inject the molten metal 5 into the molten metal injection point 6, but the present invention is not limited to this. Although not shown, the molten metal 5 may be supplied to the molten metal injection tool 3 via, for example, a tundish or the like.
[0021] In the manufacturing method of the aluminum alloy cast plate according to the present embodiment, a molten metal puddle 7 for holding the molten metal is formed between the first rotating roll and the second rotating roll. The amount of the molten metal puddle depends on the roll diameter, arrangement, flow rate of the molten metal, etc. of the first rotating roll and the second rotating roll, but may be an amount that can cast a plate of a desired thickness. For example, when the diameters of the first rotating roll and the second rotating roll are 1000 mm and 300 mm, respectively, and the facing position of the first rotating roll and the second rotating roll is approximately 35 degrees with respect to the vertical radius of the first rotating roll, the length of the molten metal puddle in contact with the surface of the first roll in a side view can be formed within a range of, for example, 200 mm or less.
[0022] FIG. 3 is a schematic diagram for explaining the distance L from the molten metal injection point to the molten metal pool, where FIG. 3(a) is a top view and FIG. 3(b) is a side view. As shown in FIG. 3, the distance L is the distance from the molten metal injection point 6 to the molten metal pool 7 on the surface of the first rotating roll 2. The distance L from the molten metal injection point to the molten metal pool is set to be more than 0 mm and not more than (roll circumferential speed (mm / sec)×0.2 sec) mm. By setting the distance L to be not more than (roll circumferential speed (mm / sec)×0.2 sec) mm, an effect is obtained in which the molten metal solidifies without being excessively cooled at the roll contact surface. The distance L is preferably more than 0 mm and not more than (roll circumferential speed (mm / sec)×0.1 sec) mm.
[0023] In the manufacturing method of the aluminum alloy cast plate according to the present embodiment, the first rotating roll and the second rotating roll have the same roll circumferential speed, and the roll circumferential speed (mm / sec) refers to the roll circumferential speed of the first rotating roll and the roll circumferential speed of the second rotating roll. The range of the roll circumferential speed is not particularly limited. From the viewpoint of performing high-speed continuous casting, the roll circumferential speed may be set to a range of 10 to 120 m / min.
[0024] Furthermore, in the manufacturing method of the aluminum alloy cast plate according to the present embodiment, the flow velocity of the molten metal is set to be faster than the roll circumferential speed of the first rotating roll and the second rotating roll. By increasing the flow velocity of the molten metal so that the component perpendicular to the roll surface of the molten metal flow velocity is small and the speed of the molten metal parallel to the roll surface is equal to or greater than the roll circumferential speed, surface cracking of the cast plate can be sufficiently suppressed. The flow velocity of the molten metal can be obtained, for example, by measuring the time required for the molten metal to pass a certain distance. As long as the flow velocity of the molten metal is faster than the roll circumferential speed, there is no particular restriction on the specific means. Specific means include, for example, a method of adjusting the height of the pouring position, i.e., a method of using potential energy, and a method of pushing out the molten metal by gas pressure as in low-pressure casting.
[0025] The size and arrangement of the first and second rotating rolls used in the manufacturing method of the aluminum alloy cast plate according to the present embodiment are not particularly limited as long as they satisfy the above-mentioned requirements. The two rolls may have the same diameter or different diameters. The twin roll casting method may be a vertical continuous casting method in which the two rolls are arranged horizontally, as shown in FIG. 4, in addition to the type in which the two rolls are arranged diagonally as shown in FIG. 1.
[0026] FIG. 5 is a schematic diagram of a manufacturing apparatus according to the manufacturing method of this embodiment. As shown in FIG. 5, it is preferable to arrange the second rotating roll 4 so that the angle θ2 formed by the facing position D of the first rotating roll 2 and the second rotating roll 4, the line F connecting the center of the first rotating roll 2, and the vertical radius C of the first rotating roll is in the range of more than 0 degrees (°) and less than 90 degrees (°). The facing position D is also the closest position of the first rotating roll 2 and the second rotating roll 4. FIG. 5(a) is a diagram illustrating a case where the first rotating roll 2 rotates in a counterclockwise direction, and FIG. 5(b) is a diagram illustrating a case where the first rotating roll 2 rotates in a clockwise direction. The angle θ2 is more preferably 10 degrees or more, even more preferably 15 degrees or more, more preferably 30 degrees or less, and even more preferably 20 degrees or less. The gap formed on the facing surfaces of the first rotating roll 2 and the second rotating roll 4 may be appropriately determined according to the plate thickness of the aluminum alloy cast plate to be manufactured.
[0027] According to the preferred embodiment as illustrated in Fig. 5, unlike the vertical continuous casting method in Fig. 4, one pouring facility can be used, which is preferable because it is easy to arrange the pouring facility. In addition, the contact pressure in the vicinity of the contact start position between the second rotating roll and the molten metal can be kept low, the actual contact area between the roll and the molten metal becomes narrow, and heat transfer is reduced. As a result, it is possible to suppress excessive cooling by the second rotating roll at a higher speed, and it is considered that surface cracks of the cast strip can be sufficiently suppressed.
[0028] In Fig. 5, a rotating roll having a smaller roll diameter than the first rotating roll is used as the second rotating roll, but this is not limited thereto. The roll diameter of the second rotating roll may be equal to or larger than the roll diameter of the first rotating roll. From the viewpoint of easier casting, it is preferable to use a second rotating roll having a smaller roll diameter than the first rotating roll, as shown in Fig. 5. The roll diameter of each of the twin rolls and the ratio of the roll diameters of the two rolls can be appropriately determined depending on the size and production volume of the aluminum alloy cast plate.
[0029] The manufacturing method and manufacturing apparatus for an aluminum cast plate according to this embodiment only need to satisfy the prescribed requirements, and there are no particular restrictions on other conditions in the manufacturing method and manufacturing apparatus. Therefore, as another embodiment, as illustrated in Fig. 6, in addition to the first rotating roll 2, the second rotating roll 4 may also inject molten metal 5A from a crucible 8A into a molten metal injection point 6A using a molten metal injector 3A and a partitioning tool 10A, so as to satisfy the requirements prescribed in the manufacturing method and manufacturing apparatus according to this embodiment, and perform casting.
[0030] (Pouring temperature) The temperature of the molten metal poured into the molten metal pouring point on the surface of the first rotating roll, ie, the pouring temperature, can be, for example, the liquidus temperature + (5 to 150°C).
[0031] (Pressing load of second rotating roll) In this embodiment, the molten metal poured onto the surface of the first rotating roll is pressed and cooled by the first rotating roll and the second rotating roll to perform casting, and the pressing load of the second rotating roll is not particularly limited as long as the casting can be performed. The pressing load depends on the size of the aluminum alloy cast plate to be cast and the type of alloy constituting the aluminum alloy cast plate. For example, the pressing load of the second rotating roll can be preferably 0.005 to 0.5 kN / mm, more preferably 0.1 to 0.3 kN / mm.
[0032] (Type of aluminum alloy) From the viewpoint of ensuring ductility and durability, the aluminum alloy cast plate according to the present embodiment is made of an aluminum alloy containing 2% by mass or more of Mg. The upper limit of the Mg content of the aluminum alloy cast plate according to the present embodiment is, for example, 10% by mass or less. The above-mentioned aluminum alloy includes the components shown in Table 1 below (units are mass%, and the lower limit of elements other than Mg may be 0% by mass), with the balance being Al and unavoidable impurities. Examples of aluminum alloy types within the range of these component compositions include alloy number 5052 specified in JIS H 4000 (2014), alloy number 5182 with a Mg content of 4.5% to 5% by mass, which is used for automobile bodies and cans, and alloy number AC7A specified in JIS H 5202 (2010). According to the manufacturing method of the aluminum alloy cast plate according to the present embodiment, even an aluminum alloy cast plate with a Mg content of 4% by mass or more and 6% by mass or less, which is more likely to cause surface cracks, can be manufactured at a high speed while suppressing surface cracks.
[0033] [Table 1]
[0034] (Thickness of aluminum alloy casting plate) The aluminum alloy cast plate produced by the production method of this embodiment has a plate thickness of, for example, 1 mm or more and 5 mm or less.
[0035] The manufacturing method of the aluminum alloy cast plate according to the present embodiment is not limited to any conditions other than those related to the casting. For example, known methods can be used for the preparation of the molten metal, hot rolling, cold rolling, etc. after casting. For example, the cast plate can be wound into a coil after casting, and then unwound from the coil and subjected to hot rolling and cold rolling.
[0036] [Aluminum alloy casting plate manufacturing equipment] The manufacturing apparatus for aluminum alloy cast plate according to the present embodiment includes: An apparatus for producing an aluminum alloy cast plate containing 2% by mass or more of Mg by a twin-roll continuous casting method, comprising: A first rotating roll having a cooling capacity; a molten metal pouring tool for pouring a molten metal of an aluminum alloy containing 2% by mass or more of Mg into a molten metal pouring point on a surface of the first rotating roll; A second rotating roll is provided for pressing, cooling and solidifying the molten metal poured at the molten metal pouring point together with the first rotating roll, The present embodiment is characterized in that an angle θ1 between the molten metal pouring tool and a tangent to the surface of the first rotating roll at the molten metal pouring point is 0 to 20 degrees. Detailed aspects and preferred aspects of each part in the manufacturing apparatus for an aluminum alloy cast plate of the present embodiment are as described above in the manufacturing method for an aluminum alloy cast plate. EXAMPLES
[0037] The present invention will be described in more detail below with reference to examples. The present invention is not limited to the following examples, and can be practiced with appropriate modifications within the scope of the above and below-mentioned aims, and all such modifications are included in the technical scope of the present invention.
[0038] An Al-Mg-based aluminum alloy cast plate of AC7A alloy, the composition of which is shown in Table 2 below, was produced by a twin-roll continuous casting method using the apparatus shown in FIG. 1. In detail, the molten metal of the aluminum alloy was poured into a refractory crucible of size #20 using a molten metal pouring tool at a molten metal pouring point such that the molten metal pouring angle θ1 was 0 degrees in Experiment No. 1, 20 degrees in Experiment No. 2, and 40 degrees in Experiment No. 3, and casting was performed to obtain an aluminum alloy cast plate having a plate thickness of 3.4 to 3.7 mm and a width of 100 mm. The distance L from the molten metal pouring point to the molten metal pool was 200 mm in all examples. Other detailed conditions for casting are as follows. In addition to the above examples, an aluminum alloy cast plate was also obtained by a conventional method shown in FIG. 7 as Experiment No. 4. In FIG. 7, a molten metal pouring tool was not used, and a partition tool 10 was provided to form a molten metal pool. Other than that, the roll shape, installation position, amount of molten metal, etc. were the same as in Experiments Nos. 1 to 3 above. (Casting conditions) Pouring temperature: 675℃ Roll diameter of first rotating roll: 1000mm x 100mm Roll diameter of second rotating roll: 300mm x 100mm Pressing load by the second rotating roll (initial roll load): 0.3 kN / mm Position of the first and second rotating rolls facing each other: 35 degrees to the vertical radius of the first rotating roll Shape and size of molten metal injector (length and width): 300mm x 100mm Position of molten metal pouring point: 10 degrees to the vertical radius of the first rotating roll Roll speed of the first and second rotating rolls: 30 m / min Molten metal flow rate: 35m / min Size of molten metal pool: Length 200mm
[0039] [Table 2]
[0040] The surface properties and structure of each of the aluminum alloy cast plates obtained as described above were measured as follows.
[0041] (Observation of surface cracks) The surface properties of each aluminum alloy cast plate were checked using a color check method to confirm the state of colored surface cracks. The results are shown in Figure 8. Figure 8 is a photograph of the top surface of each aluminum alloy cast plate, with the up and down direction being the width direction of the cast plate. Figure 8(a) shows the results of experiment No. 1 (molten metal pouring angle θ1 = 0 degrees), Figure 8(b) shows the results of experiment No. 2 (molten metal pouring angle θ1 = 20 degrees), Figure 8(c) shows the results of experiment No. 3 (molten metal pouring angle θ1 = 40 degrees), and Figure 8(d) shows the results of experiment No. 4 (conventional method).
[0042] Comparing Figures 8(a) to (d) above, it can be seen that, as shown in Figures 8(a) and 8(b), the aluminum alloy cast plate manufactured by the manufacturing method of this embodiment has surface cracks that are sufficiently suppressed compared to Figure 8(c) in which the molten metal pouring angle is increased and Figure 8(d) in which the conventional method is used.
[0043] The locations of the cracks on the upper and lower parts of the plate in the photographs of Figures 8(a) and 8(b) are located in the pool of molten metal, as shown in Figure 9. From Figure 9, it is considered that the surface cracks in Figures 8(a) and 8(b) can be further suppressed by increasing the width E of the molten metal, for example, by changing the shape and size of the crucible.
[0044] (Observation of cross-sectional structure) Figure 10(a) shows a photograph of the cross section of the aluminum alloy cast plate of Experiment No. 1 in the plate thickness direction, observed with an optical microscope at a magnification of 50 times. Figure 10(b) shows a photograph of the lower end of the cross section of Figure 10(a), enlarged on a personal computer. Figure 11 shows a similar photograph of the aluminum alloy cast plate of Experiment No. 4.
[0045] Furthermore, the aluminum alloy cast plates of Experiment No. 1 and Experiment No. 4 were used to etch the plate using Weck's reagent in the same manner as described in the literature "Effect of Mg Content on the Surface Pattern of Vertical High-Speed Twin-Roll Cast Al-Mg Alloy Plates," Yohei Harada et al., J.JFS, Vol. 91, No. 1 (2019) pp. 021-027. After etching, the plate was observed with an optical microscope. Figure 12 shows the photographs. Figure 12(a) shows the cross-sectional structure of the aluminum alloy cast plate of Experiment No. 1, and Figure 12(b) shows the cross-sectional structure of the aluminum alloy cast plate of Experiment No. 4, where the boundary with the black part at the bottom of the photograph is the first roll contact surface (lower surface). In these photographs, in the aluminum alloy cast plate of Experiment No. 4 produced by the conventional method, Mg has seeped into the grain boundary, as observed as a white line by the arrow in Figure 12(b). The part where Mg has seeped out delays solidification, causing cracks. In contrast, in the aluminum alloy cast plate of Experiment No. 1 produced by the production method of this embodiment, the above-mentioned Mg exudation was not observed.
[0046] Next, the aluminum alloy cast plates of Experiments Nos. 1 to 4 were used and cold-rolled until the plate thickness became 1 mm to obtain rolled plates. Photographs of the first roll contact surface (lower surface) of the rolled plate are shown in FIG. 13. The surface cracks after cold rolling were confirmed in the photographs. FIG. 13(a) shows the results of Experiment No. 1 (molten metal pouring angle θ1=0 degrees), FIG. 13(b) shows the results of Experiment No. 2 (molten metal pouring angle θ1=20 degrees), FIG. 13(c) shows the results of Experiment No. 3 (molten metal pouring angle θ1=40 degrees), and FIG. 13(d) shows the results of Experiment No. 4 (conventional method). From these photographs, it can be seen that in FIG. 13, when the aluminum alloy cast plate manufactured by the manufacturing method of this embodiment is used, the aluminum alloy rolled plate does not have surface cracks, but when the aluminum alloy cast plate manufactured by the conventional method is used, cracks still exist.
[0047] According to this embodiment, in casting an Al-Mg alloy with a high Mg content (2 mass % or more), an Al-Mg alloy cast plate with reduced surface cracks could be produced without reducing the roll peripheral speed, for example, even when the roll peripheral speed was set to a high speed of 20 m / min or more and the roll load was set to the same as in the conventional case, for example, about 0.3 kN / mm. [Industrial Applicability]
[0048] The method for producing an aluminum alloy cast plate according to this embodiment is suitable for producing an aluminum alloy cast plate with a high Mg content that is used for automobile bodies and cans, which have excellent ductility and durability and are lightweight. [Explanation of symbols]
[0049] 1. Aluminum alloy casting plate manufacturing equipment 2. First rotating roll 3. 3A Molten Metal Injector 4. Second Rotating Roll 5, 5A molten metal 6, 6A Molten metal pouring point 7 Molten metal pool 8, 8A crucible 9. Aluminum alloy casting plate 10, 10A Partition 11 Corner of molten metal pouring tool A. The top of the first rotating roll B Tangent to the first rotating roll surface at the molten metal pouring point C Vertical radius of the first rotating roll D. Position of the first and second rotating rolls facing each other E Width of molten metal F: A line connecting the position where the first rotating roll 2 and the second rotating roll 4 face each other and the center of the first rotating roll
Claims
1. A method for producing an aluminum alloy cast plate containing 2% by mass or more of Mg by a twin-roll continuous casting method, comprising pouring a molten aluminum alloy containing 2% by mass or more of Mg into a molten metal pouring point on a surface of a first rotating roll, and pressing, cooling and solidifying the molten aluminum alloy between the first rotating roll and the second rotating roll, comprising the steps of: an angle θ1 between a direction of injection of the molten metal to the molten metal injection point by a molten metal injection tool for injecting the molten metal to the molten metal injection point and a tangent to the surface of the first rotating roll at the molten metal injection point is set to be 0 degrees or more and 20 degrees or less; forming a molten metal puddle for holding the molten metal between the first rotating roll and the second rotating roll; The distance L from the molten metal pouring point to the molten metal pool is more than 0 mm and 200 mm or less, 3. A method for producing an aluminum alloy cast plate, comprising: setting a flow velocity of the molten metal to be equal to or greater than a peripheral speed of the first rotating roll and the second rotating roll.
2. 2. The method for manufacturing an aluminum alloy cast plate according to claim 1, wherein the second rotating roll is arranged such that an angle θ2 formed by a line connecting the opposing positions of the first rotating roll and the second rotating roll and the center of the first rotating roll, and a vertical radius of the first rotating roll is within a range of more than 0 degrees and less than 90 degrees.
3. An apparatus for manufacturing an aluminum alloy cast plate, which is used in the method for manufacturing an aluminum alloy cast plate according to claim 1, and which is an apparatus for manufacturing an aluminum alloy cast plate containing 2% by mass or more of Mg by a twin-roll continuous casting method, A first rotating roll having a cooling capacity; a molten metal pouring tool for pouring a molten metal of an aluminum alloy containing 2% by mass or more of Mg into a molten metal pouring point on a surface of the first rotating roll; a second rotating roll for pressing, cooling and solidifying the molten metal poured at the molten metal pouring point together with the first rotating roll; An apparatus for manufacturing aluminum alloy cast plate, characterized in that an angle θ1 between the molten metal pouring tool and a tangent to the surface of the first rotating roll at the molten metal pouring point is 0 degrees or more and 20 degrees or less.
4. An apparatus for manufacturing an aluminum alloy cast plate, which is used in the method for manufacturing an aluminum alloy cast plate according to claim 2, and which is an apparatus for manufacturing an aluminum alloy cast plate containing 2% by mass or more of Mg by a twin-roll continuous casting method, A first rotating roll having a cooling capacity; a molten metal pouring tool for pouring a molten metal of an aluminum alloy containing 2% by mass or more of Mg into a molten metal pouring point on a surface of the first rotating roll; a second rotating roll for pressing, cooling and solidifying the molten metal poured at the molten metal pouring point together with the first rotating roll; The angle θ1 between the molten metal pouring tool and a tangent to the surface of the first rotating roll at the molten metal pouring point is 0 degrees or more and 20 degrees or less, an angle θ2 formed by a line connecting the opposing positions of the first and second rotating rolls and the center of the first rotating roll, and the vertical radius of the first rotating roll, is within a range of more than 0 degrees and less than 90 degrees.
Citation Information
Patent Citations
Method and apparatus for producing directly metal strip
JP1987270254A
Apparatus for continuously casting strip
JP1989241356A
Apparatus and method for manufacturing alloy plate
JP2011206787A
Molding of hypereutectic aluminum-silicon alloy rolled sheet and method for manufacturing the same
JP2013001988A
SLIDE MEMBER, AND MANUFACTURING METHOD OF Al ALLOY LAYER FOR SLIDE MEMBER
JP2020128563A