Elastic hot melt composition
A hot melt composition with a thermoplastic elastomer, plasticizer, and wax with specific properties addresses stretching and tackiness issues, providing enhanced flexibility and reduced stickiness for stretchable materials in absorbent articles and wearable devices.
Patent Information
- Application Number
- JP2020128384
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-07-30
- Filing Date
- 2020-07-29
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2040-07-29
AI Technical Summary
Existing hot melt compositions used in stretchable materials exhibit insufficient stretching performance and surface tackiness, which affects their workability and usability in applications requiring flexibility and reduced stickiness.
A hot melt composition comprising a thermoplastic elastomer, a plasticizer, and a wax with specific melt viscosity and melting point ranges, which enhances elongation, stretch recovery, and suppresses surface tackiness.
The composition achieves good elongation and stretch recovery, allowing for easy application with a hot melt coater and minimizing surface tackiness after cooling, making it suitable for stretchable materials in absorbent articles and wearable devices.
Smart Images

Figure 0007573388000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a hot melt composition. [Background technology]
[0002] Stretchable materials are widely used in absorbent articles, including sanitary materials such as disposable diapers, and in stretchable sensors mounted on wearable devices that are attached to the human body or clothing.
[0003] As the stretchable material, a stretchable film having a stretch recovery rate and a film-like flat appearance is used. The stretchable film is produced, for example, by an extruder and wound into a roll, so that the user either transports the rolled stretchable film in the production process and adds a step of joining it to another adherend, or cuts the stretchable film to a desired shape and size and then joins it to an adherend for use.
[0004] Meanwhile, in recent years, hot melt stretchable adhesive compositions have been proposed as stretchable materials that can be used in hot melt adhesive applicators (see Patent Document 1). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] WO2018 / 151190 [Patent Document 2] Patent Publication 2017-149850 [Patent Document 3] Patent Publication No. 2017-165895 Summary of the Invention [Problem to be solved by the invention]
[0006] When the elastic material is of the hot melt type, the elastic material can be produced using a hot melt coater, and therefore the elastic material can be formed at a desired position in various shapes, for example, a film shape, a spiral shape in which continuous hot melt fibers are applied in a circular shape, a curtain spray shape in which short fibers are made into short fibers and applied so as to overlap, and further intermittent application, etc. However, for example, for applications in which the elastic material is exposed on the surface, a material with a more suppressed tackiness (stickiness) is suitable, and the use of such a material further improves the workability of the worker.
[0007] Patent Document 2 discloses a hot melt composition containing an ethylene-unsaturated ester copolymer, a polyethylene wax grafted with a styrene monomer, and a wax having a melting point of 40°C or more and less than 80°C and a Saybolt universal viscosity at 120°C of 20 to 300 seconds, the total wax content being 50 to 80% by weight. This invention can provide a hot melt composition with excellent blocking resistance. However, the hot melt composition described in Patent Document 2 has a problem that the hot melt composition becomes hard and does not have sufficient stretchability as a stretchable material because the wax content is high relative to the total amount of the hot melt composition.
[0008] Patent Document 3 discloses a hot melt adhesive composition comprising a main component of a hot melt adhesive and a coating material that coats the surface of the main component, the coating material being a mixture of an anionic surfactant and at least one of an ethylene-vinyl acetate copolymer and a polyethylene wax. According to this invention, blocking between hot melt adhesives during transportation of the hot melt adhesive composition is suppressed, but there is a problem in that a texture remains on the surface of the hot melt adhesive composition after it is applied with a hot melt applicator and cooled.
[0009] In view of the above circumstances, the present invention has an object to provide a hot melt composition which exhibits good elongation and stretch recovery rate as a stretch material, can be applied by a hot melt applicator, and suppresses tackiness on the surface of the hot melt composition when the hot melt composition after application is cooled to room temperature. [Means for solving the problem]
[0010] As a result of intensive investigations conducted by the present inventors in order to achieve the above-mentioned object, it was found that the above-mentioned object can be achieved by a hot-melt composition comprising a thermoplastic elastomer (A), a plasticizer (B), and a wax (C), wherein the melt viscosity at 180°C is 4,000 mPa s or more and 30,000 mPa s or less, and the melting point of the wax (C) is 40°C or more and 65°C or less, and thus the present invention has been completed.
[0011] That is, the present invention relates to the following hot melt composition. 1. A hot melt composition comprising a thermoplastic elastomer (A), a plasticizer (B), and a wax (C), the hot melt composition having a melt viscosity at 180°C of 4,000 mPa·s or more and 30,000 mPa·s or less, and the melting point of the wax (C) being 40°C or more and 65°C or less. 2. The hot melt composition according to item 1, wherein the thermoplastic elastomer (A) is a styrene-based block copolymer. 3. The hot melt composition according to item 1 or 2, wherein the content of the thermoplastic elastomer (A) is 40 mass% or more, based on 100 mass% of the total content of the thermoplastic elastomer (A), the plasticizer (B), and the wax (C). 4. The hot melt composition according to any one of items 1 to 3, wherein the content of the wax (C) is 5 to 40 parts by mass per 100 parts by mass of the thermoplastic elastomer (A). 5. The hot melt composition according to any one of items 1 to 4, wherein the thermoplastic elastomer (A) is at least one selected from the group consisting of a styrene-butadiene-butylene-styrene copolymer, a styrene-ethylene-butylene-styrene copolymer, a styrene-ethylene-butylene / styrene-styrene copolymer, a styrene-ethylene-propylene-styrene copolymer, and a styrene-ethylene-ethylene-propylene-styrene copolymer. 6. A stretchable material comprising the hot melt composition according to any one of items 1 to 5. Effect of the Invention
[0012] The hot melt composition of the present invention can exhibit good elongation and stretch recovery as an elastic material, can be applied by a hot melt coater, and when the hot melt composition of the present invention is cooled to room temperature after application, the tackiness of the surface of the hot melt composition is suppressed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] 1. Hot melt composition The hot melt composition of the present invention is a hot melt composition containing a thermoplastic elastomer (A), a plasticizer (B), and a wax (C), and has a melt viscosity at 180°C of 4,000 mPa·s to 30,000 mPa·s, and the melting point of the wax (C) is 40°C to 65°C. The hot melt composition of the present invention contains the above components (A) to (C), exhibits a specific melt viscosity, and the melting point of the wax (C) is in a specific range, so that the hot melt composition can exhibit good elongation and stretch recovery as a stretch material, and can be applied with a hot melt coater. The hot melt composition of the present invention particularly exhibits a melt viscosity in a specific range, and the melting point of the wax (C) is 40°C to 65°C, so that when the hot melt composition of the present invention is applied and cooled to room temperature, the tackiness of the surface of the hot melt composition is suppressed.
[0014] The hot melt composition of the present invention can be suitably used as a stretchable material and a stretchable laminate containing the stretchable material.
[0015] (Thermoplastic elastomer (A)) The thermoplastic elastomer (A) is not particularly limited as long as it has elasticity, and examples thereof include styrene-based block copolymers, olefin-based block copolymers, polyurethane-based block copolymers, polyester-based block copolymers, etc. Among these, styrene-based block copolymers are preferred because they have better coatability in a hot melt coater and better elastic recovery.
[0016] The styrene-based block copolymer is a block copolymer obtained by block copolymerizing a vinyl aromatic hydrocarbon with a conjugated diene compound.
[0017] Vinyl aromatic hydrocarbons are aromatic hydrocarbon compounds having vinyl groups.Specific examples of vinyl aromatic hydrocarbons include styrene, o-methylstyrene, p-methylstyrene, p-tert-butylstyrene, 1,3-dimethylstyrene, α-methylstyrene, vinylnaphthalene, vinylanthracene, etc., and among these, styrene is preferred.Vinyl aromatic hydrocarbons may be used alone or in combination of two or more.
[0018] The conjugated diene compound is a diolefin compound having at least one pair of conjugated double bonds.Specific examples of the conjugated diene compound include 1,3-butadiene, 2-methyl-1,3-butadiene (or isoprene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, and 1,3-hexadiene, and among these, 1,3-butadiene and 2-methyl-1,3-butadiene are preferred.The conjugated diene compound may be used alone or in combination of two or more.
[0019] In the styrene-based block copolymer, all or a part of the block based on the conjugated diene compound may be hydrogenated, or may not be hydrogenated. From the viewpoint of further improving the heat stability of the hot melt composition, a hydrogenated styrene-based block copolymer is preferred.
[0020] In this specification, the hydrogenation ratio in a hydrogenated thermoplastic block copolymer, such as a hydrogenated product of a styrene-based block copolymer, is indicated by the "hydrogenation ratio". The "hydrogenation ratio" of a hydrogenated thermoplastic block copolymer refers to the ratio of ethylenically unsaturated double bonds that have been hydrogenated and converted to saturated hydrocarbon bonds, based on the total ethylenically unsaturated double bonds contained in the block based on a conjugated diene compound. The hydrogenation ratio can be measured by an infrared spectrophotometer, a nuclear magnetic resonance apparatus, or the like.
[0021] The hydrogenated styrene block copolymer is preferably fully hydrogenated. The hydrogenated styrene block copolymer is fully hydrogenated, which further improves the heat stability of the hot melt composition. The hydrogenated styrene block copolymer preferably has a hydrogenation rate of about 100%.
[0022] The hydrogenated product of the styrene-based block copolymer is not particularly limited, and examples thereof include styrene-butadiene-butylene-styrene copolymer (SBBS), styrene-ethylene-butylene-styrene copolymer (SEBS), styrene-ethylene-butylene / styrene-styrene copolymer (SEB / SS), styrene-ethylene-propylene-styrene copolymer (SEPS), styrene-ethylene-ethylene-propylene-styrene copolymer (SEEPS), styrene-ethylene-butylene-olefin crystalline copolymer (SEBC), etc. By using the above-mentioned styrene-based block copolymer as the thermoplastic elastomer (A), the hot melt composition of the present invention has good elongation and stretch recovery rate as a stretch material, and can be applied by a hot melt coater. Among these, from the viewpoint of achieving both good elongation and high stretch recovery rate, styrene-butadiene-butylene-styrene copolymer (SBBS), styrene-ethylene-butylene-styrene copolymer (SEBS), styrene-ethylene-butylene / styrene-styrene copolymer (SEB / SS), styrene-ethylene-propylene-styrene copolymer (SEPS), and styrene-ethylene-ethylene-propylene-styrene copolymer (SEEPS) are preferred, and styrene-ethylene-butylene-styrene copolymer and styrene-ethylene-butylene / styrene-styrene copolymer are more preferred. The thermoplastic elastomer (A) preferably contains a styrene-ethylene-butylene / styrene-styrene copolymer.
[0023] The hydrogenated styrene block copolymers may be used alone or in combination of two or more.
[0024] The styrene-ethylene-butylene-styrene copolymer (SEBS) is a copolymer in which the terminal styrene units form the end block phase and the ethylene-butylene units form the midblock phase. By using a copolymer in which the midblock phase is a hydrogenated ethylene-butylene unit, the polarity difference with the styrene units in the endblock phase becomes more pronounced, and the styrene units in the endblock phase become stronger than those in a copolymer in which the midblock phase is not hydrogenated. As a result, the stretch recovery rate after elongation of the hot melt composition can be further improved. Furthermore, since the midblock phase is hydrogenated, a hot melt composition with even better heat stability can be provided.
[0025] The styrene content of the styrene-ethylene-butylene-styrene copolymer is preferably 15 to 45% by mass, and more preferably 20 to 40% by mass, based on 100% by mass of the styrene-ethylene-butylene-styrene copolymer. When the lower limit of the styrene content is within the above range, the hot melt composition can have a further improved stretch recovery after elongation. When the upper limit of the styrene content is within the above range, the hot melt composition can be made softer and can exhibit even better elongation.
[0026] In this specification, the "styrene content" of a styrene-based block copolymer refers to the content (mass %) of the styrene block in the styrene-based block copolymer.
[0027] In the present specification, the method for calculating the styrene content in the styrene-based block copolymer is not particularly limited, and examples thereof include a method using proton nuclear magnetic resonance spectroscopy or infrared spectroscopy in accordance with JIS K6239.
[0028] The styrene-ethylene-butylene-styrene copolymer may be a commercially available product, such as G1650 manufactured by Kraton Polymers, MD1648 manufactured by Kraton Polymers, or Tuftec H1041 manufactured by Asahi Kasei Corporation.
[0029] The styrene-ethylene-butylene-styrene copolymer may be used alone or in combination of two or more. For example, a styrene-ethylene-butylene-styrene copolymer having a high styrene content and a styrene-ethylene-butylene-styrene copolymer having a low styrene content may be used in combination. When two or more types are used in combination, the styrene content of the entire styrene-ethylene-butylene-styrene copolymer may be calculated as an average value based on weight.
[0030] The content of the styrene-ethylene-butylene-styrene copolymer is preferably 10 to 80% by mass, more preferably 15 to 75% by mass, and even more preferably 20 to 70% by mass, based on the total amount of the hot melt composition being 100% by mass. When the lower limit of the content of the styrene-ethylene-butylene-styrene copolymer in the hot melt composition is within the above range, the stretch recovery rate after elongation of the hot melt composition is further improved. When the upper limit of the content of the styrene-ethylene-butylene-styrene copolymer is within the above range, the melt viscosity of the hot melt composition is reduced, and the coatability in a hot melt coater is further improved.
[0031] The styrene-ethylene-butylene / styrene-styrene copolymer (SEB / SS) is a styrene-ethylene-butylene-styrene copolymer in which the terminal styrene units form an end block phase and the ethylene-butylene units form a midblock phase, and in which styrene is also dispersed in the midblock phase. By using a copolymer in which styrene is dispersed in the midblock phase, even if the total styrene content of the styrene block copolymer is high, the styrene block copolymer does not become too hard and exhibits good extensibility, so that a hot melt composition containing the styrene-ethylene-butylene / styrene-styrene copolymer can achieve both good extensibility and improved stretch recovery rate after stretching. Furthermore, by using a styrene-ethylene-butylene / styrene-styrene copolymer in which styrene is dispersed in the midblock phase for a hot melt composition, an increase in melt viscosity at low temperatures is suppressed, and the coatability of the hot melt composition can be further improved while maintaining both good extensibility and stretch recovery rate as a stretch material.
[0032] The method for preparing the styrene-ethylene-butylene / styrene-styrene copolymer is not particularly limited, and examples thereof include the method described in US Pat. No. 7,169,848.
[0033] The styrene content of the styrene-ethylene-butylene / styrene-styrene copolymer is preferably 20 to 60% by mass, more preferably 25 to 55% by mass, based on 100% by mass of the styrene-ethylene-butylene / styrene-styrene copolymer. When the lower limit of the styrene content is within the above range, the hot melt composition can have a further improved stretch recovery after elongation. When the upper limit of the styrene content is within the above range, the hot melt composition can be made softer and can exhibit even better elongation.
[0034] As the styrene-ethylene-butylene / styrene-styrene copolymer, commercially available products can be used, such as MD6951 and A1536 manufactured by Kraton Polymers.
[0035] The styrene-ethylene-butylene / styrene-styrene copolymer may be used alone or in combination of two or more. For example, a styrene-ethylene-butylene / styrene-styrene copolymer having a high styrene content and a styrene-ethylene-butylene / styrene-styrene copolymer having a low styrene content may be used in combination. When two or more types are used in combination, the styrene content of the entire styrene-ethylene-butylene / styrene-styrene copolymer may be calculated by the average value based on weight.
[0036] The content of the styrene-ethylene-butylene / styrene-styrene copolymer is preferably 10 to 80% by mass, more preferably 15 to 75% by mass, and even more preferably 20 to 70% by mass, based on the total amount of the hot melt composition being 100% by mass. When the lower limit of the content of the styrene-ethylene-butylene / styrene-styrene copolymer in the hot melt composition is within the above range, the stretch recovery rate after elongation of the hot melt composition is further improved. When the upper limit of the content of the styrene-ethylene-butylene / styrene-styrene copolymer is within the above range, the melt viscosity of the hot melt composition is reduced, and the coatability in a hot melt coater is further improved.
[0037] Specific examples of non-hydrogenated styrene-based block copolymers include styrene-butadiene-styrene copolymers, styrene-isoprene-styrene copolymers, etc. The styrene-based block copolymers may be used alone or in combination of two or more.
[0038] The content of the thermoplastic elastomer (A) is preferably 40% by mass or more, more preferably 45% by mass or more, even more preferably 50% by mass or more, and particularly preferably 55% by mass or more, based on 100% by mass of the total content of the thermoplastic elastomer (A), the plasticizer (B), and the wax (C). The content of the thermoplastic elastomer (A) is preferably 80% by mass or less, more preferably 75% by mass or less, and even more preferably 70% by mass or less. By having the content of the thermoplastic elastomer (A) in the above range, the stretch recovery rate after elongation of the hot melt composition of the present invention is further improved.
[0039] The styrene content of the thermoplastic elastomer (A) in the hot melt composition of the present invention is preferably 10 to 35 mass%, more preferably 12 to 25 mass%, based on 100 mass% of the thermoplastic elastomer (A). When the lower limit of the styrene content is within the above range, the hot melt composition can have a further improved stretch recovery after being kept at a temperature. When the upper limit of the styrene content is within the above range, the hot melt composition can be made softer and can exhibit a further improved extensibility.
[0040] The weight average molecular weight (Mw) of the thermoplastic elastomer (A) in the hot melt composition of the present invention is preferably 30,000 to 200,000, more preferably 40,000 to 150,000, and even more preferably 45,000 to 125,000. When the lower limit of the weight average molecular weight is within the above range, the hot melt composition can have a further improved stretch recovery after being kept at a temperature. When the upper limit of the weight average molecular weight is within the above range, the hot melt composition can be made softer and can exhibit a further improved extensibility.
[0041] The weight average molecular weight (Mw) of the thermoplastic elastomer is a measured value obtained by using a gel permeation chromatography measuring device and converting it into standard polystyrene.
[0042] The weight average molecular weight (Mw) in this specification can be measured, for example, using the following measuring device and under the following measuring conditions. Measurement device: Waters product name "ACQUITY APC" Measurement conditions: Column ·ACQUITY APCXT45 1.7μm×1 piece ·ACQUITY APCXT125 2.5μm×1 piece ·ACQUITY APCXT450 2.5μm×1 piece Mobile phase: Tetrahydrofuran 0.8mL / min Sample concentration: 0.2% by mass Detector: Refractive index (RI) detector Standard material: polystyrene (Waters, molecular weight: 266-1,800,000) Column temperature: 40°C RI detector temperature: 40℃
[0043] (Plasticizer (B)) The hot melt composition of the present invention contains a plasticizer (B). The plasticizer (B) is preferably liquid at 23°C. In this specification, "liquid" refers to a state exhibiting fluidity. The pour point of such a plasticizer (B) is preferably 23°C or lower, more preferably 10°C or lower.
[0044] In this specification, the pour point is a value measured by a measurement method in accordance with JIS K2269.
[0045] The plasticizer (B) is not particularly limited, and examples thereof include paraffinic process oil, naphthenic process oil, aromatic process oil, liquid paraffin oil, hydrocarbon synthetic oil, etc. Among them, paraffinic process oil, naphthenic process oil, liquid paraffin oil, and hydrocarbon synthetic oil are preferred from the viewpoint of excellent heat stability.
[0046] As the paraffin-based process oil, commercially available products can be used, such as PW-32 and PS-32 manufactured by Idemitsu Kosan Co., Ltd.
[0047] As the naphthenic process oil, commercially available products can be used, such as Diana Fresia N28 manufactured by Idemitsu Kosan Co., Ltd., Diana Fresia U46 manufactured by Idemitsu Kosan Co., Ltd., and Nyflex 222B manufactured by Nynas Corporation.
[0048] As the liquid paraffin oil, commercially available products can be used, such as P-100 manufactured by MORESCO and Kaydol manufactured by Sonneborn.
[0049] As the synthetic hydrocarbon oil, commercially available products can be used, such as LUCANT HC-10 and LUCANT HC-40 manufactured by Mitsui Chemicals.
[0050] The above plasticizers may be used alone or in combination of two or more.
[0051] The content of the plasticizer (B) in the hot melt composition of the present invention is preferably 10 to 100 parts by mass, more preferably 20 to 60 parts by mass, per 100 parts by mass of the thermoplastic elastomer (A). By setting the lower limit of the content of the plasticizer (B) within the above range, the melt viscosity of the hot melt composition is further reduced, and the coatability of the hot melt composition is further improved. By setting the upper limit of the content of the plasticizer (B) within the above range, the stretch recovery rate after elongation of the hot melt composition is further improved.
[0052] (Wax (C)) The hot melt composition of the present invention contains a wax (C). The wax (C) is preferably solid at 23° C. In this specification, the term "solid" refers to a state in which the wax does not exhibit fluidity.
[0053] The wax (C) used in the present invention is not particularly limited, and examples thereof include paraffin wax, microcrystalline wax, and synthetic hydrocarbon waxes such as polyethylene wax, polypropylene wax, Fischer-Tropsch wax, vinyl acetate copolymer wax, acrylic acid copolymer wax, and maleic anhydride modified wax. Among these, from the viewpoint of further reducing the surface tackiness of the hot melt composition after the hot melt composition is applied and cooled, paraffin wax, polyethylene wax, polypropylene wax, and Fischer-Tropsch wax are preferred, and paraffin wax is more preferred.
[0054] The melting point of the wax (C) is 40°C or more and 65°C or less. If the melting point of the wax (C) is less than 40°C, the surface of the hot melt composition will have a reduced tackiness when the hot melt composition is cooled to room temperature after application. If the melting point of the wax (C) is more than 65°C, the surface of the hot melt composition will have a tackiness. The melting point of the wax (C) is preferably 42°C to 63°C, more preferably 45°C to 55°C.
[0055] Although the reason why the tackiness of the surface of the hot melt composition of the present invention is suppressed by setting the melting point of the wax (C) within the above range is not clear, it is presumed that the wax (C) easily migrates to the surface of the hot melt composition when the hot melt composition is cooled and solidified after application, forming a wax coating on the surface of the hot melt composition. Also, when a wax having a melting point outside the above range is used, the migration of the wax component to the surface of the hot melt composition is insufficient or slow, so that a coating of the wax component is not sufficiently formed on the surface of the hot melt composition, and the surface tackiness remains even after cooling and solidification.
[0056] In this specification, the melting point of the wax (C) is a melting point measured by a measurement method in accordance with JIS K2235 5.3.
[0057] The penetration of the wax (C) at 25°C is preferably 10 to 50 dmm, more preferably 12 to 57 dmm, and even more preferably 15 to 55 dmm. When the lower limit of the penetration of the wax (C) is within the above range, the stretch recovery rate of the hot melt composition after elongation is further improved. When the upper limit of the penetration of the wax (C) is within the above range, the tackiness of the surface of the hot melt composition after cooling after application is further suppressed.
[0058] In this specification, the penetration of the wax (C) at 25° C. is a penetration measured by a method in accordance with JIS K2235 5.4.
[0059] The content of the wax (C) in the hot melt composition is preferably 5 to 40 parts by mass, more preferably 10 to 38 parts by mass, and even more preferably 15 to 35 parts by mass, based on 100 parts by mass of the thermoplastic elastomer (A). By setting the lower limit of the wax (C) content within the above range, the tackiness of the surface of the hot melt composition after cooling after application is further suppressed. By setting the upper limit of the wax (C) content within the above range, the stretch recovery rate of the hot melt composition after elongation is further improved, and precipitation of the wax component on the surface of the hot melt composition when the hot melt composition is elongated can be further suppressed.
[0060] As the paraffin wax, commercially available products can be used, such as Paraffin Wax-115 manufactured by Nippon Seiro Co., Ltd., Paraffin Wax-125 manufactured by Nippon Seiro Co., Ltd., and EMW-0001 manufactured by Nippon Seiro Co., Ltd.
[0061] The waxes may be used alone or in combination of two or more.
[0062] (Other additives) The hot melt composition of the present invention may contain other additives to the extent that the purpose of the present invention is not essentially hindered. Examples of the other additives include antioxidants, ultraviolet absorbers, tackifier resins, liquid rubbers, and fine particle fillers.
[0063] Antioxidants include 2,6-di-t-butyl-4-methylphenol, n-octadecyl-3-(4'-hydroxy-3',5'-di-t-butylphenyl)propionate, 2,2'-methylenebis(4-methyl-6-t-butylphenol), 2,2'-methylenebis(4-ethyl-6-t-butylphenol), 2,4-bis(octylthiomethyl)-o-cresol, 2-t-butyl-6-(3-t-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenyl acrylate, 2,4-di-t-amyl-6-[1-(3,5-di-t-amyl-2-hydroxyphenyl)ethyl ester, and 2,2'-methylenebis(4-ethyl-6-t-butylphenol). hindered phenol-based antioxidants such as 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)] acrylate, tetrakis[methylene-3-(3,5-di-t-butyl-4-hydroxyphenyl) propionate] methane; sulfur-based antioxidants such as dilauryl thiodipropionate, lauryl stearyl thiodipropionate, pentaerythritol tetrakis(3-lauryl thiopropionate); phosphorus-based antioxidants such as tris(nonylphenyl) phosphite, tris(2,4-di-t-butylphenyl) phosphite, etc. The antioxidants may be used alone or in combination of two or more.
[0064] The content of the antioxidant in the hot melt composition of the present invention is preferably 0.1 to 2.0 parts by mass, more preferably 0.3 to 1.7 parts by mass, and even more preferably 0.5 to 1.5 parts by mass, based on 100 parts by mass of the thermoplastic elastomer (A). When the content of the antioxidant is within the above range, the thermal stability of the hot melt composition is improved and the odor is reduced.
[0065] Examples of the ultraviolet absorbent include benzotriazole-based ultraviolet absorbents such as 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-t-butylphenyl)benzotriazole, and 2-(2'-hydroxy-3',5'-di-t-butylphenyl)-5-chlorobenzotriazole; benzophenone-based ultraviolet absorbents such as 2-hydroxy-4-methoxybenzophenone; salicylic acid ester-based ultraviolet absorbents; cyanoacrylate-based ultraviolet absorbents; and hindered amine-based light stabilizers. The ultraviolet absorbent may be used alone or in combination of two or more.
[0066] The content of the ultraviolet absorber in the hot melt composition of the present invention is preferably 0.01 to 2.0 parts by mass, more preferably 0.05 to 1.5 parts by mass, and even more preferably 0.1 to 1.0 parts by mass, based on 100 parts by mass of the thermoplastic elastomer (A). When the content of the ultraviolet absorber is within the above range, the weather resistance of the hot melt composition is improved and the odor is reduced.
[0067] As the tackifier resin, a tackifier resin that is conventionally used in producing hot melt adhesives can be used. For example, natural rosin, modified rosin, glycerol ester of natural rosin, glycerol ester of modified rosin, pentaerythritol ester of natural rosin, pentaerythritol ester of modified rosin, copolymer of natural terpene, three-dimensional polymer of natural terpene, hydrogenated derivative of copolymer of natural terpene, terpene resin, hydrogenated derivative of phenol-based modified terpene resin; petroleum resin such as C5-based petroleum resin, C9-based petroleum resin, C5C9-based petroleum resin, dicyclopentadiene-based petroleum resin, and also partially hydrogenated petroleum resin and fully hydrogenated petroleum resin obtained by adding hydrogen to these petroleum resins can be mentioned. As the tackifier resin, petroleum resin, partially hydrogenated petroleum resin, and fully hydrogenated petroleum resin are preferred in terms of the odor and thermal stability of the hot melt composition, and partially hydrogenated petroleum resin and fully hydrogenated petroleum resin are more preferred. These tackifier resins may be used alone or in a mixture of two or more.
[0068] The Ring and Ball softening point temperature of the tackifier resin is preferably 80° C. or higher, and more preferably 90° C. or higher, in order to provide a hot melt composition with even better elasticity and thermal stability. The Ring and Ball softening point temperature of the tackifier resin is preferably 125° C. or lower, and more preferably 120° C. or lower, in order to provide a hot melt composition with even better flexibility and to further suppress embrittlement. In this specification, the Ring and Ball softening point temperature of the tackifier resin is a value measured in accordance with JIS K2207.
[0069] The content of the tackifier resin in the hot melt composition of the present invention is preferably 50 parts by mass or less, more preferably 35 parts by mass or less, and even more preferably 25 parts by mass or less, based on 100 parts by mass of the thermoplastic elastomer (A). When the content of the tackifier resin is within the above range, the hot melt composition does not become too hard, and the stretch recovery rate after elongation is further improved.
[0070] Examples of the liquid rubber include liquid polybutene, liquid polybutadiene, liquid polyisoprene, and hydrogenated resins thereof. The liquid rubber may be used alone or in combination of two or more.
[0071] The content of the liquid rubber in the hot melt composition of the present invention is preferably 0.1 to 40 parts by mass, more preferably 1 to 35 parts by mass, and even more preferably 3 to 20 parts by mass, based on 100 parts by mass of the thermoplastic elastomer (A). When the content of the liquid rubber is within the above range, the melt viscosity of the hot melt additive decreases, and the coating suitability is further improved.
[0072] The particulate filler is not particularly limited, and examples thereof include calcium carbonate, kaolin, talc, titanium oxide, mica, styrene beads, etc. The particulate filler may be used alone or in combination of two or more kinds.
[0073] The hot melt composition of the present invention has a melt viscosity at 180°C of 4,000 mPa·s or more and 30,000 mPa·s or less. If the melt viscosity is less than 4,000 mPa·s, the elastic material will not exhibit a good elastic recovery rate. If the melt viscosity is more than 30,000 mPa·s, the elastic material will not exhibit a good elongation and cannot be applied with a hot melt coater. The melt viscosity is preferably 4,500 to 25,000 mPa·s, more preferably 5,000 to 20,000 mPa·s.
[0074] In this specification, the "melt viscosity" refers to the viscosity of a hot melt composition in a molten state at a certain temperature. For example, the melt viscosity at 180°C may be measured by heating and melting the hot melt composition, and measuring the viscosity of the molten composition at 180°C using a Brookfield RVT viscometer (spindle No. 29).
[0075] The hot melt composition of the present invention is produced by a known method. For example, the thermoplastic elastomer (A), the plasticizer (B), the wax (C), and various additives, if necessary, are charged into a twin-arm kneader heated to 150°C, and melt-kneaded while heating. At this time, the heating temperature of the kneader is not particularly limited, and may be any temperature at which the thermoplastic elastomer is softened.
[0076] The hot melt composition of the present invention is applied using a hot melt applicator. There is no particular limitation on the method of applying the hot melt composition using a hot melt applicator. For example, the hot melt composition is charged into a hot melt composition melting tank heated to 180°C and melted sufficiently, and then the molten hot melt composition is sent from the melting tank through a heated hose to a hot melt application nozzle. The hot melt composition is then discharged from the nozzle in a desired pattern and applied. At this time, the nozzle is also heated.
[0077] The coating pattern of the hot melt composition of the present invention is not particularly limited, but any coating pattern generally used for hot melt adhesive compositions can be used. For example, slot coating, which coats the composition in a film form, bead coating, spiral coating, which coats the composition with heated air, spray coating such as curtain fiber coating, and even intermittent coating can be used.
[0078] When the hot melt composition of the present invention is applied in the form of a film, it is possible to prepare a stretchable film without a tacky surface. When the hot melt composition of the present invention is applied by spray coating, it is possible to prepare a stretchable fiber without a tacky surface. When the hot melt composition is applied in the form of short fibers by curtain coating, it is possible to prepare a stretchable porous fibrous material without a tacky surface.
[0079] The extensibility of the hot melt composition of the present invention is preferably 350% or more, more preferably 450% or more, and even more preferably 550% or more. When the extensibility of the stretchable hot melt composition is 350% or more, breakage of the hot melt composition when stretched is suppressed.
[0080] The extensibility of the hot melt composition of the present invention is measured by preparing a coating sample of the hot melt composition by the following method, and then using the coating sample by the following measurement method.
[0081] (Method of preparing a coating sample of a hot melt composition) The hot melt composition is applied by slot coating onto a release-treated PET film at a coating temperature of 180 to 190°C. The coating amount is 50 g / m 2 The coating width is 100 mm. Next, another release-treated PET film is laminated and pressed at room temperature to create a laminate. The resulting laminate is stored for 24 hours in an atmosphere of 23°C and 50% relative humidity, and the hot melt composition is cooled to room temperature to prepare a coating sample of the hot melt composition.
[0082] (Method of measuring extensibility) The coated sample of the hot melt composition is cut into a strip of 50 mm width in the coating direction and 100 mm in the direction perpendicular to the coating direction to prepare a test piece. Next, the release-treated PET film on both sides is peeled off, and the test piece is fixed with a jig in a tensile tester set to a jig width of 50 mm so that the direction perpendicular to the coating direction of the hot melt composition is located at the top and bottom, and pulled at a pulling speed of 500 mm / min to the point where the test piece breaks. The displacement at which the test piece breaks is taken as the breaking elongation (%) and is used as the evaluation standard for the extensibility of the hot melt composition.
[0083] The permanent set of the hot melt composition of the present invention is preferably 65% or more, more preferably 70% or more, even more preferably 80% or more, and particularly preferably 85% or more. When the permanent set of the hot melt composition is 65% or more, the hot melt composition has better elastic recovery after elongation.
[0084] The permanent deformation of the hot melt composition of the present invention is measured by the following measurement method using a coated sample of the hot melt composition.
[0085] (Method of measuring permanent deformation) A coated sample of the hot melt composition is cut into a strip of 50 mm width in the coating direction and 100 mm in the direction perpendicular to the coating direction to prepare a test piece. Next, the release-treated PET film on both sides is peeled off, and the test piece is fixed with a jig in a tensile tester set to a jig width of 50 mm so that the direction perpendicular to the coating direction of the hot melt composition is located at the top and bottom, and pulled at a pulling speed of 500 mm / min to a point where the strain displacement of the test piece is 300%. Next, the test piece is returned to its initial position at a speed of 500 mm / min. The process of pulling to a point where the strain displacement is 300% and returning to the initial position constitutes one cycle, and two cycles are repeated for the same test piece. The horizontal axis represents the strain displacement (%), and the vertical axis represents the stress (N / mm 2 In the graph, the integral value during the first tensile stress cycle is S1, and the integral value during the second tensile stress cycle is S2, and the permanent set (%) is calculated using the following formula. Permanent set (%) = (S2 / S1) x 100
[0086] The probe tack measurement value of the hot melt composition of the present invention is preferably 30 g f or less, more preferably 20 g f or less, and even more preferably 15 g f or less. When the probe tack value of the hot melt composition is 30 g f or less, the surface tackiness after the hot melt composition is applied and then cooled is further suppressed.
[0087] The probe tack of the hot melt composition of the present invention is measured by the following measurement method using a coating sample of the hot melt composition.
[0088] (Method of measuring probe tack) A test piece is prepared by cutting a coated sample of the hot melt composition to 25 mm x 25 mm. The release-treated film of the test piece is peeled off, and the hot melt composition is exposed and set in a probe tack tester (NS PROBE TACK TESTER, manufactured by Nichiban Co., Ltd.) with a probe tack load of 10 g / cm. 2 The probe tack is measured at a speed of 1 cm / sec.
[0089] The hot melt composition of the present invention can be suitably used as an elastic material and an elastic laminate containing the elastic material. The elastic material containing the hot melt composition of the present invention can also be suitably used as an elastic laminate. Such an elastic material is also one aspect of the present invention.
[0090] The stretchable material can be suitably used in absorbent articles including sanitary materials such as disposable diapers, and in stretchable sensors mounted on wearable devices that are attached to the human body or clothing. EXAMPLES
[0091] Examples of the present invention will be described below, but the present invention is not limited to the following examples.
[0092] The raw materials used in the examples and comparative examples are as follows.
[0093] Styrenic block copolymer (A1) : Styrene-ethylene-butylene / styrene-styrene (SEB / SS) copolymer: Kraton Polymers MD6951 (styrene content 34% by mass, Mw=100,000) Styrene-based block copolymer (A2) : Styrene-ethylene-butylene-styrene (SEBS) copolymer: Kraton Polymers MD1648 (styrene content 20% by mass, Mw=54,000) Styrenic block copolymer (A3) : Styrene-ethylene-butylene-styrene (SEBS) copolymer Asahi Kasei H1041 (styrene content 30% by mass, Mw=61,000)
[0094] Plasticizer (B1) : Paraffin-based process oil: Idemitsu Kosan PS-32 Plasticizer (B2) : Naphthenic process oil Nyflex222B manufactured by Nynas
[0095] Wax (C1) : Paraffin wax EMW-0001 (melting point 49°C, 25°C penetration 40dmm) manufactured by Nippon Seiro Co., Ltd. Wax (C2) : Paraffin wax: Paraffin Wax-115 (melting point 48°C, needle penetration 29dmm at 25°C) manufactured by Nippon Seiro Co., Ltd. Wax (C3) : Paraffin wax: Paraffin Wax-125 (melting point 53°C, needle penetration 15dmm at 25°C) manufactured by Nippon Seiro Co., Ltd. Wax (C4) : Paraffin wax: Paraffin Wax-135 (melting point 59°C, needle penetration 11dmm at 25°C) manufactured by Nippon Seiro Co., Ltd. Wax (C5) : Paraffin wax: Paraffin Wax-145 (melting point 63°C, needle penetration 12dmm at 25°C) manufactured by Nippon Seiro Co., Ltd. Wax (C6): Paraffin wax: Paraffin Wax-155 (melting point 69°C, needle penetration 12dmm at 25°C) manufactured by Nippon Seiro Co., Ltd. Wax (C7) : Vinyl acetate wax Honeywell AC-400 (melting point 92°C, 25°C penetration 9.5dmm) Wax (C8) : Polyethylene wax Honeywell AC-1702 (melting point 90℃, 25℃ penetration 98dmm)
[0096] Antioxidants : Phenolic antioxidant: BASF IRGANOX1010
[0097] Examples and Comparative Examples The above-mentioned raw materials were charged into a stirring kneader equipped with a heating device in the amounts shown in Table 1. The mixture was kneaded while heating at 150° C. for 90 minutes to produce a hot melt composition.
[0098] The properties of the obtained hot melt composition were evaluated under the following measurement conditions.
[0099] (180℃ Melt Viscosity) The hot melt composition was heated to melt, and the viscosity of the molten composition at 180° C. was measured using a Brookfield RVT viscometer (spindle No. 29).
[0100] (Coatability) The hot melt composition was charged into a melt tank heated to 180 to 190° C., and discharged from a slot nozzle heated to 180 to 190° C. to contact-coat a release-treated PET film. The coatability of the hot melt composition was visually observed and evaluated according to the following criteria. ◎: Coating can be done evenly at a coating temperature of 180°C. ◯: At a coating temperature of 180°C, some coating unevenness was observed, but this was not problematic in use, and at a coating temperature of 190°C, coating was possible without unevenness. △: At a coating temperature of 190°C, some coating unevenness was observed, but this did not cause any problems in use. ×: Significant unevenness in application was observed, or the desired amount of hot melt composition was not dispensed.
[0101] (extensibility) Preparation of test specimens The hot melt composition was applied by slot coating onto a release-treated PET film at a coating temperature of 180 to 190°C. The coating amount was 50 g / m 2 The coating width was 100 mm. Next, another release-treated PET film was laminated and pressure-bonded at room temperature to prepare a laminate. The obtained laminate was stored for 24 hours in an atmosphere of 23°C and 50% relative humidity, and the hot melt composition was cooled to room temperature to prepare a coating sample of the hot melt composition. The coating sample of the hot melt composition was cut into a strip with a width of 50 mm in the coating direction and 100 mm in the direction perpendicular to the coating direction to prepare a test piece. Measurement method The release-treated PET films on both sides were peeled off, and the test piece was fixed to a tensile tester set to a jig width of 50 mm so that the direction perpendicular to the coating direction of the hot melt composition was positioned at the top and bottom, and pulled at a pulling speed of 500 mm / min until the test piece broke. The displacement at which the test piece broke was taken as the breaking elongation (%) and was used as the evaluation standard for the extensibility of the hot melt composition.
[0102] (Recovery rate after elongation) Measurement method The coated sample of the hot melt composition was cut into a strip shape with a width of 50 mm in the coating direction and a width of 100 mm in the direction perpendicular to the coating direction to prepare a test piece. Next, the release-treated PET film on both sides was peeled off, and the test piece was fixed with a jig in a tensile tester set to a jig width of 50 mm so that the direction perpendicular to the coating direction of the hot melt composition was located up and down, and pulled at a pulling speed of 500 mm / min to a point where the strain displacement of the test piece was 300%. Then, it was returned to its initial position at a speed of 500 mm / min. The process of pulling to a point where the strain displacement was 300% and returning to the initial position was defined as one cycle, and two cycles were repeated for the same test piece. In a graph with the horizontal axis being the strain displacement (%) and the vertical axis being the test force (N), the integral value during the first cycle of pulling was S1, and the integral value during the second cycle of pulling was S2, and the permanent set (%) was calculated by the following formula and used as the evaluation standard for the stretch recovery rate. In this case, the closer the permanent deformation value is to 100%, the better the stretch recovery rate is. Permanent set (%) = (S2 / S1) x 100
[0103] (Surface tackiness) Measurement method A test piece was prepared by cutting the coated sample of the hot melt composition to 25 mm × 25 mm. The release-treated film of the test piece was peeled off, and the hot melt composition was exposed and set in a probe tack tester (NS PROBE TACK TESTER, manufactured by Nichiban Co., Ltd.) with a probe tack load of 10 g / cm. 2 The probe tack was measured at a speed of 1 cm / sec to evaluate the surface tackiness.
[0104] The results are shown in Table 1.
[0105] [Table 1]
Claims
1. A hot melt composition comprising a thermoplastic elastomer (A), a plasticizer (B), and a wax (C), the hot melt composition having a melt viscosity at 180°C of 4,000 mPa·s or more and 20,000 mPa·s or less, and a melting point of the wax (C) of 40°C or more and 65°C or less.
2. The hot melt composition according to claim 1 , wherein the thermoplastic elastomer (A) is a styrene-based block copolymer.
3. 3. The hot melt composition according to claim 1, wherein the content of the thermoplastic elastomer (A) is 40 mass% or more, based on 100 mass% of the total content of the thermoplastic elastomer (A), the plasticizer (B), and the wax (C).
4. The hot melt composition according to any one of claims 1 to 3, wherein the content of the wax (C) is 5 to 40 parts by mass per 100 parts by mass of the thermoplastic elastomer (A).
5. The hot melt composition according to any one of claims 1 to 4, wherein the thermoplastic elastomer (A) is at least one selected from the group consisting of a styrene-butadiene-butylene-styrene copolymer, a styrene-ethylene-butylene-styrene copolymer, a styrene-ethylene-butylene / styrene-styrene copolymer, a styrene-ethylene-propylene-styrene copolymer, and a styrene-ethylene-ethylene-propylene-styrene copolymer.
6. A stretchable material comprising the hot melt composition according to any one of claims 1 to 5.
Citation Information
Patent Citations
Hot-melt adhesive composition
JP1988189485A
Preparation of paper diaper
JP1990007955A
Water-swellable hot-melt presealing material for lap joint of outer wall material for building
JP1997176618A
Outdoor wall sealing agent composition and outdoor wall
JP1998204414A
Road surface indicating material and method for sticking road surface indicating material to road surface
JP2001026915A