Cement admixture, expansive material, and cement composition

A cement admixture with controlled chloride ions, pH, and oxidation-reduction potential, combined with an expansive substance, addresses the lack of simultaneous strength enhancement and shrinkage compensation, enhancing concrete strength and reducing bleeding.

JP7573402B2Active Publication Date: 2024-10-25DENKA CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2020164860
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-30
Publication Date
2024-10-25
Estimated Expiration
2040-09-30

AI Technical Summary

Technical Problem

Existing cement admixtures do not simultaneously achieve significant strength enhancement and shrinkage compensation effects.

Method used

A cement admixture containing thiosulfate with controlled chloride ion content within the range of 0.04 mg/g to 2.0 mg/g, pH of 6 to 9, and oxidation-reduction potential of -50 to 0 mV, combined with an expansive substance, is used to enhance strength and compensate for shrinkage.

Benefits of technology

The cement admixture exhibits strength enhancement and shrinkage compensation effects after construction, improving workability and reducing bleeding rates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573402000001
    Figure 0007573402000001
Patent Text Reader

Abstract

To provide a cement admixture capable of exhibiting a strength promotion effect and a shrinkage compensation effect after construction work.SOLUTION: The cement admixture comprises a cement additive and a swelling substance, with the cement additive containing a thiosulphate and the amount of a chloride ion contained in the cement admixture being in a range of 0.04 to 2.0 mg / g.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cement admixture, an expansive agent, and a cement composition used, for example, in the fields of civil engineering and construction. [Background technology]

[0002] Reducing cracks in cement and concrete is important from the standpoint of the reliability, durability, and aesthetics of concrete structures, and further technological developments in cement admixtures that have the effect of improving these properties, i.e., cement-based expansive agents, are desired.

[0003] So far, concrete expanding agents that have excellent expansion properties even with small amounts added (Patent Document 1), cement expanding agents in which the surface of free lime is coated with calcium carbonate (Patent Document 2), and the like have been proposed. In recent years, the combined use of expanding agents and shrinkage reducing agents has also been proposed (Patent Document 3). Meanwhile, cement admixtures containing anhydrous gypsum, thiocyanate, thiosulfate and / or silica fine powder, cement compositions containing these and cement, and cement admixtures consisting of γ-CS and thiosulfate that exhibit effects such as early strength development and carbonation inhibition effects have also been proposed (Patent Documents 4 and 5). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2002-029792 A [Patent Document 2] Japanese Patent Application Publication No. 54-93020 [Patent Document 3] JP 2003-12352 A [Patent Document 4] Japanese Patent Application Publication No. 9-156977 [Patent Document 5] JP 2004-51420 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, although these cement admixtures have the effect of increasing strength or shrinkage compensation, they do not dramatically improve the strength and shrinkage compensation effects of cement concrete at the same time.

[0006] In view of the above, an object of the present invention is to provide a cement admixture, an expansive material, and a cement composition that can exhibit strength enhancing and shrinkage compensation effects after construction.

[0007] As a result of various investigations to solve the above problems, the present inventors have found that the above problems can be solved by adding a specific cement admixture and setting the amount of chloride ions in the cement admixture within a specific range. That is, the present invention is as follows. [Means for solving the problem]

[0008] The present invention employs the following means to solve the above problems. [1] A cement admixture comprising a cement admixture and an expansive substance, the cement admixture comprising a thiosulfate, and an amount of chloride ions contained in the cement admixture being 0.04 mg / g to 2.0 mg / g. [2] The cement admixture according to [1], wherein the cement admixture has a pH of 6 to 9, an oxidation-reduction potential of -50 to 0 mV, and a solids concentration of 20 to 60%. [3] The cement admixture according to [1] or [2], wherein the thiosulfate is sodium thiosulfate. [4] The cement admixture according to any one of [1] to [3], wherein the thiosulfate in the cement admixture is 0.3 to 8 parts by mass per 100 parts by mass of the expansion substance. [5] An expansive material comprising the cement admixture according to any one of [1] to [4]. [6] A cement composition comprising the cement admixture according to [5]. Effect of the Invention

[0009] According to the present invention, it is possible to provide a cement admixture that can exhibit strength enhancing and shrinkage compensating effects after construction. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the present invention (the present embodiment) will be described in detail. Note that parts and % used in this specification are based on mass unless otherwise specified.

[0011] [1. Cement admixture] The cement admixture of the present embodiment includes a cement admixture and an expansive substance. The cement admixture includes a thiosulfate, and the amount of chloride ions included in the cement admixture is 0.04 mg / g to 2.0 mg / g.

[0012] In this embodiment, the cement admixture contains thiosulfate and an expansive substance, which improves the initial strength development, and thus high strength (particularly strength enhancement) can be obtained after construction of cement concrete. In addition, the present invention focuses on the amount of chloride ions contained in the cement admixture, and has found that the amount of chloride ions affects the strength enhancement after construction. That is, if the amount of chloride ions contained in the cement admixture is less than 0.04 mg / g, the workability of the cement admixture decreases, and the strength decreases. If the amount of chloride ions exceeds 2.0 mg / g, the strength decreases.

[0013] The amount of chloride ions contained in the cement admixture is preferably 0.05 to 2.0 mg / g, more preferably 0.1 to 1.7 mg / g, even more preferably 0.2 to 1.5 mg / g, and even more preferably 0.6 to 1.3 mg / g.

[0014] The amount of chloride ions contained in the cement admixture can be adjusted, for example, by adding an admixture containing chloride ions when preparing the cement admixture. The amount of chloride ions can be measured by the method described in the Examples below.

[0015] (Cement admixture) The cement admixture according to this embodiment contains a thiosulfate, and is added to a cement admixture to mainly reduce the bleeding rate, improve workability, and contribute to high strength expression (particularly, strength increase) after construction of concrete. The bleeding rate herein refers to the rate of material separation measured by the method described in the Examples below.

[0016] From the viewpoint of fully exerting the above-mentioned effects, the content of thiosulfate in the cement admixture is preferably 90% or more, and more preferably 95% or more. Other elements that may be contained besides thiosulfate include chlorine, fluorine, sulfur, etc. The cement admixture can be used alone, but can also be used as a mixture with cement or the like.

[0017] From the viewpoints of reducing the bleeding rate, improving the workability, and contributing to high strength development after construction of concrete, the pH of the cement admixture is preferably 5-10, and more preferably 6-9. Here, the pH of the cement admixture means the pH of the supernatant liquid after adding 100 ml of pure water to 30 g of the cement admixture and stirring to prepare a mixture, and can be measured using a pH meter. To adjust the pH to 5 to 10, an acid or alkali can be added to the mixture.

[0018] Furthermore, from the viewpoint of reducing the bleeding rate, reducing the viscosity, and contributing to high strength development after construction of concrete, the oxidation-reduction potential of the cement admixture is preferably −60 to 0 mV, and more preferably −50 to 0 mV. Here, the oxidation-reduction potential of the cement admixture means the oxidation-reduction potential of the supernatant liquid after adding 100 ml of pure water to 30 g of the cement admixture and stirring to prepare a mixture, and can be measured using an oxidation-reduction potential (ORP) meter. The oxidation-reduction potential can be adjusted to -60 to 0 mV by bubbling oxygen into the mixture.

[0019] The thiosulfate is not particularly limited, and examples thereof include sodium thiosulfate, calcium thiosulfate, potassium thiosulfate, lithium thiosulfate, ammonium thiosulfate, and hydrates thereof, and one or more of these can be used. Among these, sodium thiosulfate and calcium thiosulfate are preferable, and sodium thiosulfate is more preferable because of its easy availability. One or more of the thiosulfates can be used. Thiosulfates are deliquescent and water-soluble, so when used in the present invention, they can be added in the form of a powder or dissolved in the kneading water. In addition, the particle size is not particularly limited.

[0020] From the viewpoint of liquid stability, the solid content concentration in the cement admixture is preferably 20 to 70%, and more preferably 30 to 50%.

[0021] The amount of thiosulfate in the cement admixture is preferably 0.2 to 8 parts, more preferably 0.3 to 5 parts, even more preferably 0.4 to 2 parts, and particularly preferably 0.4 to 1 part, relative to 100 parts of the expansive substance. The amount within the above range can contribute to reducing the bleeding rate, reducing the viscosity, and achieving high strength (particularly, strength enhancement) after concrete construction.

[0022] (Expansion material) The expansion material exerts a shrinkage compensation effect by being contained in the cement admixture. The expansion material is not particularly limited, and commercially available products can be used, including ettringite-based, ettringite-lime composite, lime-based, and magnesium-based products. Among them, ettringite-based expansion materials, ettringite-lime composite expansion materials, and lime-based expansion materials are preferred from the viewpoints of better shrinkage compensation effect, strength expression, and aesthetics.

[0023] From the viewpoint of a better shrinkage compensation effect, the content of the expansive substance in the cement admixture is preferably 93 to 99.7%, and more preferably 95.5 to 99.5%.

[0024] The present invention is preferably an expansive material comprising the above-mentioned cement admixture.

[0025] (cement) Examples of cement include various types of Portland cement such as normal, early strength, super early strength, low heat, and moderate heat, various mixed cements obtained by mixing blast furnace slag, fly ash, or silica with these Portland cements, filler cements obtained by mixing limestone powder, gypsum, blast furnace slag powder, etc., and environmentally friendly Portland cements (ecocement) manufactured using municipal waste incineration ash and sewage sludge incineration ash as raw materials, as well as commercially available cement-based solidification materials used in ground improvement work, commercially available fine particle cements, etc., and one or more of these can be used. Also, cements adjusted by increasing or decreasing the amount of components used in regular cements can be used.

[0026] The cement admixture can be prepared, for example, by mixing a cement admixture with an expansive material. In addition, the oxidation-reduction potential at this time is preferably −100 to 25 mV, more preferably −50 to 10 mV, from the viewpoints of reducing the bleeding rate of fresh concrete, reducing the viscosity, and achieving high strength after concrete construction. The oxidation-reduction potential is measured as described above.

[0027] [2. Cement Composition] The cement composition according to the present embodiment contains the above-mentioned cement admixture. Here, examples of the cement used in the cement composition include various Portland cements such as normal, early strength, super early strength, low heat, and moderate heat, various mixed cements obtained by mixing these Portland cements with blast furnace slag, fly ash, or silica, filler cements obtained by mixing limestone powder and blast furnace slag powder, and environmentally friendly Portland cements (ecocement) manufactured using municipal waste incineration ash and sewage sludge incineration ash as raw materials. In addition, examples include geopolymer cement, sulfoaluminate cement, and limestone calcined clay cement (LC3), which emit less CO2 than conventional cements. One or two of these can be used. The cement admixture may be an expanding material according to the present embodiment.

[0028] In this embodiment, in addition to cement, cement admixtures, and fine aggregates such as sand and coarse aggregates such as gravel, it is possible to use one or more of the following admixtures in a range that does not substantially impair the object of the present invention: early strengthening agents, rapid hardening agents, water reducing agents, AE water reducing agents, high performance water reducing agents, high performance AE water reducing agents, fluidizing agents, antifoaming agents, thickening agents, rust inhibitors, antifreeze agents, shrinkage reducing agents, setting reducing agents, hydration heat inhibitors, polymer emulsions, clay minerals such as bentonite, anion exchangers such as hydrotalcite, slags such as ground granulated blast furnace slag and ground cooled blast furnace slag, limestone fine powder, siliceous fine powder, gypsum, calcium silicate, etc. In addition, it may be used in combination with fibrous materials such as vinylon fiber, acrylic fiber, and carbon fiber.

[0029] The amount (mixture amount) of the cement admixture (or expansive agent) used (mixture amount) is not particularly limited since it varies depending on the mix ratio of the concrete, but usually, in 100 parts of the cement composition containing cement and the cement admixture (or expansive agent), 3 to 12 parts is preferable, and 4 to 7 parts is more preferable. When the amount is 3 parts or more, sufficient expansion performance can be obtained. Also, when the amount is 12 parts or less, excessive expansion is not caused, and the occurrence of expansion cracks in the concrete can be prevented.

[0030] The amount (mixture amount) of the cement admixture (or expansive agent) used (mixture amount) is not particularly limited since it varies depending on the mix ratio of concrete, but is usually preferably 1 to 20 parts, more preferably 2 to 17 parts, and even more preferably 6 to 16 parts, per 100 parts of cement composition consisting of cement and cement admixture. If the amount of the cement admixture used is small, sufficient shrinkage compensation effect, bleeding suppression, improvement of workability, and strength enhancement effect after construction may not be obtained.

[0031] The water / binder ratio of the cement composition of the present invention is preferably 25-70%, more preferably 30-65%. If the amount of water is small, pumpability and workability may decrease, or shrinkage may occur, while if the amount of water is excessive, strength development may decrease. Here, the binder refers to the total amount of cement, the cement admixture (or expansive agent) of the present invention, and other admixtures.

[0032] The cement admixture and cement composition of the present invention may be prepared by mixing the respective materials at the time of application, or may be mixed in part or in whole in advance.

[0033] As the mixing device, any existing device can be used, for example, a tilting mixer, an omni mixer, a Henschel mixer, a V-type mixer, a Nauta mixer, or the like. EXAMPLES

[0034] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these.

[0035] <Materials used> The materials used in the examples and comparative examples are listed below. (Thiosulfate) Sodium thiosulfate: a first-class reagent Calcium thiosulfate: First-class reagent

[0036] (Expansion material) Ettringite-based expanding agent: Denka CSA#20 manufactured by Denka Ettringite-lime composite expansive material: Denka Power CSA Type S manufactured by Denka Corporation

[0037] Cement: Ordinary Portland cement, commercially available, Blaine specific surface area 3,200 cm 2 / g Fine aggregate: "Standard sand for cement strength testing" from the Cement Association, density 2.64g / cm 3

[0038] [Example 1] (Preparation of cement admixture) The thiosulfates shown in Table 1 were added to pure water to obtain the specified solid content concentration, and the mixture was stirred for 10 minutes to prepare a cement admixture. The pH was adjusted using an aqueous sodium hydroxide solution, and the ORP was adjusted by bubbling oxygen.

[0039] (Preparation of cement admixture) Next, 0.5 parts of the prepared cement admixture was mixed with 100 parts of the expansive agent and a chloride ion-containing admixture (material name: sodium chloride) to obtain the chloride ion concentration shown in Table 1 to prepare a cement admixture.

[0040] (Preparation of Cement Composition) Cement was further added to the prepared cement admixture, and the mixture was mixed for 2 minutes using a mortar mixer to prepare the cement composition shown in Table 1. The blending amount of the cement admixture was as shown in Table 1.

[0041] (Mortar preparation) Mortar was prepared by mixing 100 parts of the cement composition shown in Table 1, 100 parts of fine aggregate, and 50 parts of water. The prepared mortar was observed for the presence or absence of bleeding, and the flow, the increase in compressive strength from 3 days to 28 days, and the length change rate at 7 days were measured. The results are shown in Table 1.

[0042] <Chloride ions in cement admixtures> The chloride ion content of the prepared cement admixture was measured in accordance with JIS R 5202:2010 "Methods for chemical analysis of cement." The results are shown in Table 1 below.

[0043] <Breeding> The bleeding rate was measured according to the Japan Society of Civil Engineers' Standard Specifications (JSCE-F542-2013) "Test Method for Bleeding Rate and Expansion Rate of Filling Mortar". Those without bleeding water were marked with ○, those with bleeding water but in a small amount that could not be collected were marked with △, and those with bleeding water that could be collected were marked with ×.

[0044] <Flow test> The mortar was mixed according to JIS R 5201:2015 "Physical Testing Methods for Cement" and the 15-point flow value was measured immediately after mixing. The temperature, humidity, and mortar mix were the same as those in the compressive strength test. Standard sand was used in the test. The results are shown in Table 1 below.

[0045] <Compressive strength> Test specimens measuring 4 x 4 x 16 cm were prepared in accordance with JIS R 5201:2015 "Physical Testing Methods for Cement," and the compressive strength was measured at 3 days (3d) and 28 days (28d). The increase in compressive strength from 3 days to 28 days was calculated using Equation 1. The results are shown in Table 1 below.

[0046] [Formula 1] Compressive strength increase rate (%) = (compressive strength at 28 days - compressive strength at 3 days) / compressive strength at 3 days x 100

[0047] <Rate of change in length> The length change rate after 7 days of use was measured according to JIS A 6202:2017 "Expansive additive for concrete" Appendix A "Expansive additive mortar expansion test method". The length change rate is 300 to 700μ (μ=10 -6 ) is preferred.

[0048] [Examples 2 to 12, Comparative Examples 1 and 2] A cement admixture was prepared in the same manner as in Example 1, except that the blend ratio, pH, and oxidation-reduction potential were as shown in Table 1. The amount of chloride ions was measured in the same manner as in Example 1. A cement composition was prepared in the same manner as in Example 1, except that the blend ratio of cement and cement admixture was as shown in Table 1. Flow and compressive strength were measured in the same manner as in Example 1. The results are shown in Table 1.

[0049] [Table 1]

[0050] As shown in Table 1, the present invention can provide strength enhancement and shrinkage compensation effects after construction.

Claims

1. A cement admixture comprising a cement admixture and an expansive material, the cement admixture comprising a thiosulfate salt, and an amount of chloride ions contained in the cement admixture being 0.04 mg / g to 2.0 mg / g; The cement admixture, wherein the expansive material is an ettringite-based material, an ettringite-lime composite-based material, a lime-based material, or a magnesium-based material.

2. The cement admixture according to claim 1, wherein the cement admixture has a pH of 6 to 9, an oxidation-reduction potential of -50 to 0 mV, and a solids concentration of 20 to 60%.

3. 3. The cement admixture according to claim 1, wherein the thiosulfate is sodium thiosulfate.

4. The cement admixture according to any one of claims 1 to 3, wherein the thiosulfate in the cement admixture is 0.3 to 8 parts by mass relative to 100 parts by mass of the expansion substance.

5. An expansive material comprising the cement admixture according to any one of claims 1 to 4.

6. A cement composition comprising the cement admixture according to claim 5.

Citation Information

Patent Citations

  • Lime containing particulate composition* cement composition containing same and method of making same

    JP1979093020A

  • Production of centrifugally molded material

    JP1994009256A

  • Method for dehydrating gypsum slurry of by-product from flue gas desulfurization and apparatus therefor

    JP1995330397A

  • Cement admixture and cement composition

    JP1997156977A

  • Manufacture of concrete product

    JP1999090918A