Resin composition

A resin composition combining polyphenylene ether, hydrogenated block copolymers, and specific additives achieves enhanced impact and chemical resistance, along with self-tapping strength and rigidity, addressing the limitations of previous PPE-based materials.

JP7573447B2Active Publication Date: 2024-10-25ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2021003083
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-12
Publication Date
2024-10-25
Estimated Expiration
2041-01-12

AI Technical Summary

Technical Problem

Existing resin compositions based on polyphenylene ether (PPE) lack sufficient impact resistance, chemical resistance, and self-tapping strength, making them unsuitable for mechanical parts and structures, and previous attempts to improve these properties often result in reduced stiffness or require large amounts of thermoplastic elastomers.

Method used

A resin composition comprising polyphenylene ether, a hydrogenated block copolymer with specific vinyl aromatic and conjugated diene compounds, an olefin polymer excluding propylene, and a polypropylene resin, along with additives like phosphinates and phosphate ester compounds, formulated to achieve a balanced combination of impact resistance, chemical resistance, and rigidity.

Benefits of technology

The composition exhibits excellent impact resistance, chemical resistance, and self-tapping strength, with sufficient rigidity for mechanical parts and structures, while maintaining flame retardancy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573447000001
    Figure 0007573447000001
  • Figure 0007573447000002
    Figure 0007573447000002
  • Figure 0007573447000003
    Figure 0007573447000003
Patent Text Reader

Abstract

To provide a resin composition which is excellent in impact resistance, chemical resistance, and self-tapping strength and which has rigidity applicable to a mechanical component and a structural body.SOLUTION: A resin composition of this invention contains: a polyphenylene ether-based resin (a); a hydrogenated block copolymer and / or a modified substance of the hydrogenated block copolymer (b); an olefinic polymer composed of olefins except for propylene (c); a polypropylene-based resin (d); and an admixture (e), and is characterized as having: 50-80 pts.mass component (a); 5-30 pts.mass component (b); 1-20 pts.mass component (c); and 1-20 pts.mass component (e), and a mass ratio of the component (c) to the component (d) of 1-5, in which the component (a) forms a continuous phase, a glass-transition temperature of a polymer block B in the component (b) is -65°C or less, and a brittleness temperature of the component (c) is -50°C or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition. [Background technology]

[0002] Polyphenylene ether (hereinafter sometimes simply referred to as "PPE") has advantages such as heat resistance, low specific gravity, and flame retardancy, and is used in a wide variety of applications including office equipment and automobiles. However, because polyphenylene ether is an amorphous resin, it has insufficient resistance to oils and organic solvents, and there is an issue that there are certain limitations on the applications and environments in which it can be used.

[0003] For this reason, in some applications, attempts have been made to improve chemical resistance by alloying crystalline resins with PPE resins; however, this has the problem that impact resistance rapidly deteriorates in the temperature range below the glass transition temperature of the crystalline resin.

[0004] In response to this, studies have been conducted on increasing impact resistance by adding a thermoplastic elastomer having a low glass transition temperature to polyphenylene ether or an alloy of polypropylene and polyphenylene ether (eg, Patent Documents 1 to 5). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] WO 2015 / 50060 [Patent Document 2] JP 2004-161929 A [Patent Document 3] Patent No. 5422561 [Patent Document 4] JP 2007-519782 A [Patent Document 5] International Publication No. 2017 / 208945 Summary of the Invention [Problem to be solved by the invention]

[0006] However, even if the technology of Patent Document 1 is used, it is not possible to obtain a composition having a self-tapping strength sufficient for practical use in addition to impact resistance and chemical resistance. Even if the technologies of Patent Documents 2 to 4 are used, a relatively large amount of thermoplastic elastomer needs to be added to impart a certain level of impact resistance, so the rigidity of the obtained composition is low, its applications are limited, and it is difficult to apply it to mechanical parts and structures. Furthermore, the technology of Patent Document 5 also has further problems with self-tapping strength.

[0007] Therefore, an object of the present invention is to provide a resin composition which is excellent in impact resistance, chemical resistance and self-tapping strength, and has rigidity which allows its application to mechanical parts and structures. [Means for solving the problem]

[0008] That is, the present invention is as follows. [1] (a) a polyphenylene ether resin; (b) a hydrogenated block copolymer obtained by hydrogenating at least a portion of a block copolymer including at least one polymer block A mainly made of a vinyl aromatic compound and at least one polymer block B mainly made of a conjugated diene compound, and / or a modified product of the hydrogenated block copolymer; (c) an olefin polymer comprising an olefin other than propylene; (d) a polypropylene-based resin; (e) an admixture which is a compound different from the (b) component; Contains the component (e) is a hydrogenated block copolymer obtained by hydrogenating at least a portion of a block copolymer including at least one polymer block I mainly made of a vinyl aromatic compound and at least one polymer block II mainly made of a conjugated diene compound, and / or a modified product of the hydrogenated block copolymer; the total content of 1,2-vinyl bonds and 3,4-vinyl bonds relative to the ethylenic double bonds in the conjugated diene compound units contained in the polymer block II is 65% or more and 90% or less; the mass ratio of the component (a) is 50 to 80 parts by mass, the mass ratio of the component (b) is 5 to 30 parts by mass, the mass ratio of the component (c) is 1 to 20 parts by mass, and the mass ratio of the component (e) is 1 to 20 parts by mass, relative to a total of 100 parts by mass of the component (a), the component (b), the component (c), the component (d), and the component (e); the mass ratio (c) / (d) of the component (c) to the component (d) is 1 to 5; The component (a) forms a continuous phase, the glass transition temperature of the polymer block B in the component (b) is −65° C. or lower, The brittle temperature of the component (c) is −50° C. or lower. A resin composition comprising: [2] The resin composition according to [1], further comprising (f) a phosphate ester compound. [3] Further, (g) a phosphinate is contained, The component (g) is a phosphinate represented by the following general formula (1): [ka] [In the formula, R 11 and R 12 are each independently a linear or branched alkyl group having 1 to 6 carbon atoms and / or an aryl group having 6 to 10 carbon atoms; M 1 is at least one selected from the group consisting of calcium ion, magnesium ion, aluminum ion, zinc ion, bismuth ion, manganese ion, sodium ion, potassium ion, and protonated nitrogen base; a is an integer of 1 to 3; m is an integer of 1 to 3; and a=m, A diphosphinate represented by the following formula (2): [ka] [In the formula, R 21 and R 22 are each independently a linear or branched alkyl group having 1 to 6 carbon atoms and / or an aryl group having 6 to 10 carbon atoms; R23 is a linear or branched alkylene group having 1 to 10 carbon atoms, an arylene group having 6 to 10 carbon atoms, an alkylarylene group having 6 to 10 carbon atoms, or an arylalkylene group having 6 to 10 carbon atoms; M 2 is at least one selected from the group consisting of calcium ion, magnesium ion, aluminum ion, zinc ion, bismuth ion, manganese ion, sodium ion, potassium ion, and protonated nitrogen base; b is an integer of 1 to 3; n is an integer of 1 to 3; j is an integer of 1 or 2; and b·j=2n. The resin composition according to [1] or [2], comprising at least one kind of phosphinate selected from the group consisting of: [4] The resin composition according to any one of [1] to [3], wherein the component (c) is an ethylene-1-butene copolymer. [5] The density of the component (c) is 0.87 g / cm 3 The resin composition according to any one of [1] to [4] above. [6] The density of the component (c) is 0.90 g / cm 3 The resin composition according to any one of [1] to [5] above. [7] The resin composition according to any one of [1] to [6], wherein the component (d) is a propylene homopolymer. [8] the component (e) is a hydrogenated block copolymer obtained by hydrogenating at least a portion of a block copolymer including at least one polymer block I mainly made of a vinyl aromatic compound and at least one polymer block II mainly made of a conjugated diene compound, and / or a modified product of the hydrogenated block copolymer; the total content of 1,2-vinyl bonds and 3,4-vinyl bonds relative to the double bonds in the conjugated diene compound units contained in the component (e) is more than 50% and not more than 90%, the content of vinyl aromatic compound units in the component (e) before hydrogenation is 30 to 50 mass %, The glass transition temperature of the polymer block II in the component (e) is higher than -50°C, The resin composition according to any one of [1] to [7], wherein the hydrogenation rate of the double bonds in the conjugated diene compound units contained in the component (e) is 80 to 100%. [9] The resin composition according to any one of [1] to [8], which has a flexural modulus measured in accordance with ISO 178 of 1600 MPa or more. Effect of the Invention

[0009] According to the present invention, it is possible to obtain a resin composition which is excellent in impact resistance, chemical resistance and self-tapping strength, and has sufficient rigidity to be applicable to mechanical parts and structures. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, the embodiment of the present invention (hereinafter, also referred to as the "present embodiment") will be described in detail. Note that the present invention is not limited to the following embodiment, and can be modified in various ways within the scope of the gist of the present invention.

[0011] [Resin composition] The resin composition of the present embodiment comprises: (a) a polyphenylene ether resin; (b) a hydrogenated block copolymer obtained by hydrogenating at least a portion of a block copolymer including at least one polymer block A mainly made of a vinyl aromatic compound and at least one polymer block B mainly made of a conjugated diene compound, and / or a modified product of the hydrogenated block copolymer; (c) an olefin polymer comprising an olefin other than propylene; (d) a polypropylene-based resin; (e) an admixture which is a compound different from the above (b) component; Contains the mass ratio of the component (a) is 50 to 80 parts by mass, the mass ratio of the component (b) is 5 to 30 parts by mass, the mass ratio of the component (c) is 1 to 20 parts by mass, and the mass ratio of the component (e) is 1 to 20 parts by mass, relative to a total of 100 parts by mass of the components (a), (b), (c), (d), and (e); the mass ratio (c) / (d) of the component (c) to the component (d) is 1 to 5; The component (a) forms a continuous phase, the glass transition temperature of the polymer block B in the component (b) is −65° C. or lower; The brittle temperature of the above component (c) is -50°C or lower. The resin composition of the present embodiment has excellent impact resistance, chemical resistance, and self-tapping properties, and has a rigidity that allows it to be applied to mechanical parts and structures. It is also preferable that the resin composition has excellent flame retardancy. In this embodiment, excellent flame retardancy refers to a flame retardancy level of V-1 or higher in the UL94 vertical flame test described in the examples below.

[0012] In this specification, a hydrogenated block copolymer obtained by hydrogenating at least a portion of a block copolymer containing at least one polymer block mainly made of a vinyl aromatic compound and at least one polymer block mainly made of a conjugated diene compound, and / or a modified product of the hydrogenated block copolymer may be simply referred to as a "hydrogenated block copolymer". Furthermore, an unmodified hydrogenated block copolymer may be referred to as an "unmodified hydrogenated block copolymer", and a modified product of the hydrogenated block copolymer may be referred to as a "modified hydrogenated block copolymer". The sum of the 1,2-vinyl bonds and the 3,4-vinyl bonds in the conjugated diene compound units may be referred to as "total vinyl bonds."

[0013] The components of the resin composition of this embodiment will be described below.

[0014] (a) Polyphenylene ether resin The polyphenylene ether resin (a) is not particularly limited, and examples thereof include polyphenylene ether, modified polyphenylene ether, and a mixture of both. The component (a) may be used alone or in combination of two or more.

[0015] From the viewpoint of further improving the flame retardancy of the resin composition, the reduced viscosity of the above-mentioned (a) component is preferably 0.25 dL / g or more, more preferably 0.28 dL / g or more, and is preferably 0.60 dL / g or less, more preferably 0.57 dL / g or less, and particularly preferably 0.55 dL / g or less. The reduced viscosity can be controlled by the polymerization time and the amount of catalyst. The reduced viscosity is η sp / c: Using a 0.5 g / dL chloroform solution, it can be measured at 30°C using an Ubbelohde type viscometer.

[0016] -Polyphenylene ether- The polyphenylene ether is not particularly limited, and examples thereof include a homopolymer having a repeating unit structure represented by the following formula (3) and / or a copolymer having a repeating unit structure represented by the following formula (3). [ka] [In the formula, R 31 , R 32 , R 33 , and R 34 are each independently a monovalent group selected from the group consisting of a hydrogen atom, a halogen atom, a primary alkyl group having 1 to 7 carbon atoms, a secondary alkyl group having 1 to 7 carbon atoms, a phenyl group, a haloalkyl group, an aminoalkyl group, a hydrocarbyloxy group, and a halohydrocarbyloxy group in which at least two carbon atoms separate the halogen atom from the oxygen atom.

[0017] The polyphenylene ether is not particularly limited, and known ones can be used.Specific examples of the polyphenylene ether include homopolymers such as poly(2,6-dimethyl-1,4-phenylene ether), poly(2-methyl-6-ethyl-1,4-phenylene ether), poly(2-methyl-6-phenyl-1,4-phenylene ether), and poly(2,6-dichloro-1,4-phenylene ether); copolymers such as copolymers of 2,6-dimethylphenol and other phenols such as 2,3,6-trimethylphenol and 2-methyl-6-butylphenol; and the like.Poly(2,6-dimethyl-1,4-phenylene ether) and copolymers of 2,6-dimethylphenol and 2,3,6-trimethylphenol are preferred, and poly(2,6-dimethyl-1,4-phenylene ether) is more preferred.

[0018] The method for producing the polyphenylene ether is not particularly limited, and can be a conventionally known method.Specific examples of the method for producing the polyphenylene ether include the method described in U.S. Pat. No. 3,306,874, etc., which uses a complex of cuprous salt and amine as a catalyst to oxidatively polymerize 2,6-xylenol, and the methods described in U.S. Pat. No. 3,306,875, U.S. Pat. No. 3,257,357, U.S. Pat. No. 3,257,358, JP-B-17880, JP-A-50-51197, JP-A-63-152628, etc.

[0019] -Modified polyphenylene ether- The modified polyphenylene ether is not particularly limited, and examples thereof include those obtained by grafting and / or adding a styrene-based polymer and / or a derivative thereof to the polyphenylene ether. The ratio of mass increase due to grafting and / or addition is not particularly limited, and is preferably 0.01% by mass or more, and preferably 10% by mass or less, more preferably 7% by mass or less, and particularly preferably 5% by mass or less, relative to 100% by mass of the modified polyphenylene ether.

[0020] The method for producing the modified polyphenylene ether is not particularly limited, and examples thereof include a method in which the polyphenylene ether is reacted with a styrene-based polymer and / or a derivative thereof in the presence or absence of a radical generator in a molten state, solution state or slurry state at a temperature of 80 to 350°C.

[0021] When the component (a) is a mixture of polyphenylene ether and modified polyphenylene ether, the mixing ratio of the polyphenylene ether and the modified polyphenylene ether is not particularly limited and may be any ratio.

[0022] ((b) Hydrogenated block copolymer) The hydrogenated block copolymer as the component (b) is a hydrogenated block copolymer obtained by hydrogenating at least a portion of a block copolymer including at least one polymer block A mainly made of a vinyl aromatic compound and at least one polymer block B mainly made of a conjugated diene compound, and / or a modified product of the hydrogenated block copolymer. The above component (b) may contain blocks other than polymer block A and polymer block B, but it is preferable that the component (b) consists of only polymer block A and polymer block B, and it is more preferable that the component (b) consists of only one type of polymer block A and one type of polymer block B. The component (b) may be used alone or in combination of two or more kinds.

[0023] --Polymer block A-- Examples of the polymer block A mainly composed of a vinyl aromatic compound include a homopolymer block of a vinyl aromatic compound, a copolymer block of a vinyl aromatic compound and a conjugated diene compound, etc. Among these, a homopolymer block of a vinyl aromatic compound and a copolymer block of a vinyl aromatic compound and a conjugated diene compound containing more than 50 mass % (preferably 70 mass % or more) of a vinyl aromatic compound unit are preferred. Here, in the polymer block A, "mainly composed of a vinyl aromatic compound" means that the polymer block A before hydrogenation contains more than 50 mass% of vinyl aromatic compound units, and preferably contains 70 mass% or more of vinyl aromatic compound units.

[0024] The vinyl aromatic compound is not particularly limited, but examples thereof include styrene, α-methylstyrene, vinyltoluene, p-tert-butylstyrene, diphenylethylene, etc. Among these, styrene is preferable. The conjugated diene compound includes the conjugated diene compounds described below, and butadiene, isoprene, and combinations thereof are preferred. These may be used alone or in combination of two or more.

[0025] In the polymer block A, the distribution of the vinyl aromatic compound, the conjugated diene compound, etc. in the molecular chain of the polymer block may be random, tapered (where the monomer component increases or decreases along the molecular chain), partially block-like, or any combination thereof.

[0026] When the component (b) contains two or more polymer blocks A, the polymer blocks A may have the same structure or different structures.

[0027] The number average molecular weight (Mn) of the polymer block A is preferably from 5,000 to 25,000, and more preferably from 10,000 to 25,000, from the viewpoint of obtaining even better rigidity, impact resistance, chemical resistance, and self-tapping strength.

[0028] --Polymer block B-- Examples of the polymer block B mainly composed of a conjugated diene compound include a homopolymer block of a conjugated diene compound, a random copolymer block of a conjugated diene compound and a vinyl aromatic compound, etc. Among these, a homopolymer block of a conjugated diene compound and a copolymer block of a conjugated diene compound and a vinyl aromatic compound containing more than 50 mass % (preferably 70 mass % or more) of a conjugated diene compound unit are preferred. Here, in the polymer block B, "mainly composed of a conjugated diene compound" means that the polymer block B before hydrogenation contains more than 50 mass% of conjugated diene compound units, and preferably contains 70 mass% or more of conjugated diene compound units.

[0029] The conjugated diene compound is not particularly limited, but examples thereof include butadiene, isoprene, 1,3-pentadiene, 2,3-dimethyl-1,3-butadiene, etc. Among them, butadiene, isoprene, and combinations thereof are preferred. The vinyl aromatic compound may be any of the vinyl aromatic compounds described above, with styrene being preferred. These may be used alone or in combination of two or more.

[0030] In the polymer block B, the distribution of the conjugated diene compound, the vinyl aromatic compound, etc. in the molecular chain of the polymer block may be random, tapered (where the monomer component increases or decreases along the molecular chain), partially block-shaped, or any combination thereof.

[0031] When the component (b) contains two or more polymer blocks B, the polymer blocks B may have the same structure or different structures.

[0032] The hydrogenation rate of the ethylenic double bonds in the conjugated diene compound units in the polymer block B is preferably 20% or more and less than 80%, more preferably 20% or more and less than 70%, from the viewpoint of obtaining even better rigidity, chemical resistance, impact resistance, and tracking resistance. When the hydrogenation rate is within the above range, the impact resistance of the resin composition is improved, which is preferable.

[0033] The total ratio of 1,2-vinyl bonds and 3,4-vinyl bonds to the ethylenic double bonds in the conjugated diene compound units in the polymer block B is preferably 25% or more and less than 60%, more preferably 25 to 55%, even more preferably 25 to 50%, and particularly preferably 35 to 48%, from the viewpoint of obtaining even better rigidity, impact resistance, chemical resistance, and self-tapping strength. In this specification, the sum of the 1,2-vinyl bond amount and the 3,4-vinyl bond amount (total vinyl bond amount) refers to the ratio of the sum of the 1,2-vinyl bond amount and the 3,4-vinyl bond amount to the sum of the 1,2-vinyl bond amount, the 3,4-vinyl bond amount and the 1,4-conjugated bond amount in the conjugated diene compound unit in the conjugated diene compound-containing polymer block before hydrogenation. The total vinyl bond amount can be measured using an infrared spectrophotometer and calculated according to the method described in Analytical Chemistry, Volume 21, No. 8, August 1949.

[0034] The number average molecular weight (Mn) of the polymer block B is preferably from 20,000 to 100,000, and more preferably from 20,000 to 80,000, from the viewpoint of obtaining even better rigidity, impact resistance, chemical resistance, and self-tapping strength.

[0035] The glass transition temperature of the polymer block B after hydrogenation is −65° C. or lower, and from the viewpoint of obtaining even better rigidity, impact resistance, chemical resistance, and self-tapping strength, it is preferably −70° C. or lower, and more preferably −75° C. or lower. In this specification, the glass transition temperature of a block copolymer and the glass transition temperature of a polymer block in the block copolymer can be measured, for example, using a dynamic viscoelasticity measuring device using a sample in a film state in a tensile mode at a temperature scan rate of 3° C. / min and a frequency of 1 Hz in a nitrogen atmosphere.

[0036] The polymer block B may be a single polymer block in which the total ratio of 1,2-vinyl bonds and 3,4-vinyl bonds to the ethylenic double bonds in the conjugated diene compound units contained in the polymer block B is 25% or more and less than 60%, or may be a polymer block mainly made of a conjugated diene compound having both a polymer block B1 mainly made of a conjugated diene compound in which the total ratio of 1,2-vinyl bonds and 3,4-vinyl bonds is 25 to 45%, and a polymer block B2 mainly made of a conjugated diene compound in which the total ratio of 1,2-vinyl bonds and 3,4-vinyl bonds is 45% or more and less than 70%. The structure of the block copolymer having polymer block B1 and polymer block B2 is represented, for example, by A-B2-B1-A, A-B2-B1, etc., where the polymer block A is represented as "A", the polymer block B1 is represented as "B1", and the polymer block B2 is represented as "B2", and can be obtained by a known polymerization method in which the total vinyl bond amount is controlled based on the adjusted feed sequence of each monomer unit.

[0037] --Structure of hydrogenated block copolymer-- The structure of the hydrogenated block copolymer in the component (b) can be, for example, an AB type, an ABA type, a BABA type, an (AB-) type, where the polymer block A is "A" and the polymer block B is "B". n -X type (wherein n is an integer of 1 or more, and X is a reaction residue of a polyfunctional coupling agent such as silicon tetrachloride or tin tetrachloride, or a residue of an initiator such as a polyfunctional organolithium compound), ABABA type structure, etc. are examples. Regarding the block structure, it is preferred that polymer block B is a homopolymer block of a conjugated diene compound, or a copolymer block of a conjugated diene compound containing more than 50% by mass (preferably 70% by mass or more) of conjugated diene compound units and a vinyl aromatic compound, and that polymer block A is a homopolymer block of a vinyl aromatic compound, or a copolymer block of a vinyl aromatic compound containing more than 50% by mass (preferably 70% by mass or more) of a vinyl aromatic compound and a conjugated diene compound. The molecular structure of the hydrogenated block copolymer in the component (b) is not particularly limited, and may be, for example, linear, branched, radial, or any combination thereof.

[0038] --Vinyl aromatic compound unit content-- The content of vinyl aromatic compound units (hydrogenated block copolymer constituent units derived from vinyl aromatic compounds) in the (b) component before hydrogenation is not particularly limited, but from the viewpoint of heat resistance and mechanical strength of the composition, it is preferably 10 to 70 mass%, more preferably 20 to 70 mass%, more preferably 20 to 60 mass%, even more preferably 30 to 50 mass%, and particularly preferably 30 to 40 mass%. In addition to one type of (b) component having a vinyl aromatic compound unit content within these ranges, two or more types of (b) components having different vinyl aromatic compound unit contents can be used in combination.

[0039] --Total vinyl bond content-- The total ratio of 1,2-vinyl bonds and 3,4-vinyl bonds to the ethylenic double bonds in the conjugated diene compound units contained in the above component (b) is preferably 25% or more and less than 60%, more preferably 25% or more and 55% or less, and even more preferably 25% or more and 50% or less. When the total ratio of 1,2-vinyl bonds and 3,4-vinyl bonds is less than 60%, the impact resistance of the resin composition is improved. When it is 50% or less, the impact resistance is further improved. In addition, when the total ratio of 1,2-vinyl bonds and 3,4-vinyl bonds is 25% or more, it is preferable from the viewpoint of improving compatibility with components (c) and (d). The method for controlling the total proportion of 1,2-vinyl bonds and 3,4-vinyl bonds within the above range is not particularly limited, and examples thereof include a method of adding a 1,2-vinyl bond amount regulator in the production of component (b) and a method of adjusting the polymerization temperature. "The sum of 1,2-vinyl bonds and 3,4-vinyl bonds relative to the double bonds in the conjugated diene compound units" refers to the sum of 1,2-vinyl bonds and 3,4-vinyl bonds relative to the double bonds (ethylenic double bonds) in the conjugated diene compound units in the block copolymer before hydrogenation of the hydrogenated block copolymer. For example, the block copolymer before hydrogenation can be measured with an infrared spectrophotometer and calculated by the Hampton method. It can also be calculated from the block copolymer after hydrogenation using NMR.

[0040] --Hydrogenation rate-- In the above component (b), the hydrogenation rate of the ethylenic double bonds (double bonds in the conjugated diene compound units) in the block copolymer is preferably more than 0% and less than 80%, more preferably 10% or more and less than 80%, even more preferably 20% or more and less than 80%, even more preferably 20 to 70%, and particularly preferably 20% or more and less than 70%. If the hydrogenation rate is within the above range, the impact resistance of the resin composition is improved, which is preferable. Component (b) having such a hydrogenation rate can be easily obtained, for example, by controlling the amount of hydrogen consumed in the hydrogenation reaction of the ethylenic double bonds of the block copolymer to a desired hydrogenation rate (for example, 10% or more and less than 80%). The hydrogenation rate can be determined, for example, by quantifying the amount of remaining double bonds in the polymer block B by NMR measurement. It is more preferable that the above-mentioned (b) component has a total ratio of 1,2-vinyl bonds and 3,4-vinyl bonds to the ethylenic double bonds in the conjugated diene compound units contained in the (b) component of less than 60% and a hydrogenation rate of the ethylenic double bonds in the (b) component of less than 80%, since the impact resistance of the resin composition is further improved.

[0041] --Molecular weight peak-- The molecular weight peak of the above component (b) after hydrogenation, calculated as standard polystyrene by GPC measurement, is preferably from 10,000 to 200,000, more preferably from 30,000 to 150,000, from the viewpoints of rigidity, impact resistance, chemical resistance, and self-tapping strength. The method for controlling the molecular weight peak of the component (b) within the above range is not particularly limited, but may be, for example, a method of adjusting the amount of catalyst in the polymerization step. In this specification, the molecular weight peak can be measured under the following conditions using a gel permeation chromatography System 21 manufactured by Showa Denko K. In the measurement, a column consisting of one KG, one K-800RL, and one K-800R, all manufactured by Showa Denko K., connected in series in this order, the column temperature is 40° C., the solvent is chloroform, the solvent flow rate is 10 mL / min, and the sample concentration is 1 g hydrogenated block copolymer / 1 L chloroform solution. In addition, a calibration curve is created using standard polystyrene (molecular weights of standard polystyrene are 3,650,000, 2,170,000, 1,090,000, 681,000, 204,000, 52,000, 30,200, 13,800, 3,360, 1,300, and 550). Furthermore, the wavelength of UV (ultraviolet light) at the detection section is set to 254 nm for both the standard polystyrene and the hydrogenated block copolymer.

[0042] The molecular weight distribution (Mw / Mn) of the above component (b) before hydrogenation is preferably 1.01 to 1.50, more preferably 1.03 to 1.40, from the viewpoint of obtaining even better rigidity, impact resistance, chemical resistance, and self-tapping strength.

[0043] --Manufacturing method-- The method for producing the hydrogenated block copolymer in component (b) above is not particularly limited, and any known production method can be used. Examples of the method include those described in JP-A-47-11486, JP-A-49-66743, JP-A-50-75651, JP-A-54-126255, JP-A-56-10542, JP-A-56-62847, JP-A-56-100840, JP-A-2-300218, GB Patent No. 1,130,770, U.S. Pat. No. 3,281,383, U.S. Pat. No. 3,639,517, GB Patent No. 1,020,720, U.S. Pat. No. 3,333,024, and U.S. Pat. No. 4,501,857.

[0044] -Modified hydrogenated block copolymer- Examples of modified hydrogenated block copolymers in component (b) include modified hydrogenated block copolymers obtained by reacting the hydrogenated block copolymer (particularly, an unmodified hydrogenated block copolymer) with an α,β-unsaturated carboxylic acid or a derivative thereof (an ester compound or an acid anhydride compound) in the presence or absence of a radical generator in a molten state, solution state, or slurry state at 80 to 350° C. In this case, the α,β-unsaturated carboxylic acid or a derivative thereof is preferably grafted or added in a proportion of 0.01 to 10% by mass to the unmodified hydrogenated block copolymer. When an unmodified hydrogenated block copolymer and a modified hydrogenated block copolymer are used in combination as the component (b), the mixing ratio of the unmodified hydrogenated block copolymer and the modified hydrogenated block copolymer can be determined without any particular limitation.

[0045] ((c) Olefin-based polymer) The above-mentioned (c) component is not particularly limited, and examples thereof include homopolymers of olefin-based monomers other than propylene, and copolymers of two or more monomers including olefin-based monomers other than propylene. Among them, from the viewpoint of impact resistance, copolymers of ethylene and α-olefins other than ethylene are preferred. Here, from the viewpoints of impact resistance, chemical resistance, tracking resistance, and rigidity of the resulting resin composition, propylene units are not included as monomer units constituting the (c) component. In addition, "olefin polymer composed of olefins other than propylene" and "containing no propylene units" also include cases in which propylene is contained as a structural unit to an extent that does not impair the effects of the invention. For example, this means that the content of propylene units in all structural units constituting component (c) in component (c) is less than 0.1 mass%.

[0046] Examples of the (c) component include copolymers of ethylene and one or more C4-C20 α-olefins. Among them, copolymers of ethylene and one or more C4-C8 α-olefins are more preferred, copolymers of ethylene and one or more comonomers selected from the group consisting of 1-butene, 1-hexene, 4-methyl-1-pentene, and 1-octene are even more preferred, and copolymers of ethylene and 1-butene are particularly preferred. By using such copolymers as the (c) component, a resin composition having higher impact properties and higher chemical resistance tends to be obtained. The component (c) may be used alone or in combination of two or more kinds. Also, two or more kinds of ethylene-α-olefin copolymers may be used as the component (c).

[0047] The content of structural units derived from ethylene in the component (c) is preferably 5 to 95% by mass, more preferably 30 to 90% by mass, based on the total amount of the olefin polymer, from the viewpoints of low-temperature curing resistance and flexibility of the resin composition.

[0048] The content of the structural units derived from α-olefins other than ethylene in the component (c) is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 20% by mass or more, based on the total amount of the olefin polymer, from the viewpoint of low-temperature curing resistance and flexibility of the resin composition. Also, from the viewpoint of rigidity of the resin composition, it is preferably 50% by mass or less, more preferably 48% by mass or less.

[0049] The brittle temperature of the above component (c) is -50°C or lower, and from the viewpoint of obtaining even better impact resistance and chemical resistance, it is preferably -60°C or lower, and more preferably -70°C or lower. The brittle temperature can be measured in accordance with ASTM D746.

[0050] The density of the component (c) measured in accordance with JIS K7112 (density at the raw material stage before kneading) is 0.87 g / cm from the viewpoint of chemical resistance of the resin composition. 3 More preferably, it is 0.90 g / cm 3 That's all. The method for controlling the density of component (c) within the above range is not particularly limited, but may be, for example, a method in which the density is adjusted by controlling the content ratio of ethylene units.

[0051] The melt flow rate (MFR, measured in accordance with ASTM D-1238 at 190°C under a load of 2.16 kgf, density at the raw material stage before kneading) of the above-mentioned component (c) is preferably 0.1 to 5.0 g / 10 min, more preferably 0.3 to 4.0 g / 10 min, and even more preferably 0.4 to 3.5 g / 10 min, from the viewpoints of stabilization of morphology due to dispersion of component (c) in the resin composition and of the impact resistance of the resin composition. The method for controlling the melt flow rate of the component (c) within the above range is not particularly limited, but examples thereof include a method of adjusting the polymerization temperature and polymerization pressure when producing the component (c), and a method of adjusting the molar ratio of the monomer concentration of ethylene, α-olefin, etc., and the hydrogen concentration in the polymerization system.

[0052] The component (c) may be, for example, an olefin polymer rubber made of an olefin other than propylene.

[0053] The torsional rigidity of the component (c) is preferably 1 to 30 MPa, more preferably 1 to 25 MPa, from the viewpoint of imparting sufficient impact resistance to the composition. The torsional rigidity of the component (c) can be measured in accordance with ASTM D 1043.

[0054] From the viewpoint of imparting sufficient impact resistance to the composition, the Shore A of the above component (c) is preferably 40 to 110, and more preferably 50 to 100. The Shore A of the component (c) can be measured in accordance with JIS K 6253.

[0055] The method for preparing the component (c) is not particularly limited, and examples thereof include a method using a catalyst (e.g., a catalyst based on titanium, metallocene, or vanadium) that can easily obtain a high molecular weight α-olefin polymer under normal processing conditions. Among these, from the viewpoint of stability of structure control, a method using a metallocene catalyst and a titanium chloride catalyst is preferred. As a method for producing an ethylene-α-olefin copolymer, a known method described in JP-A-6-306121 and JP-T-7-500622 can be used.

[0056] ((d) Polypropylene resin) Examples of the component (d) include (d1) a polypropylene resin, (d2) a modified polypropylene resin, and a mixture thereof, which will be described later.

[0057] -(d1) Polypropylene resin- The above (d1) polypropylene resin refers to a polymer in which 50 mol % or more of the constituent monomers is propylene, and other than that, there are no particular limitations. The proportion of propylene in the monomers constituting the (d1) polypropylene resin is preferably 70 mol % or more, and more preferably 90 mol % or more.

[0058] Examples of the (d1) polypropylene resin include a crystalline propylene homopolymer; and a crystalline propylene-α-olefin block copolymer, such as a crystalline propylene-ethylene block copolymer, having a crystalline propylene homopolymer portion obtained in the first polymerization step and a propylene-α-olefin random copolymer portion obtained by copolymerizing propylene, ethylene and / or at least one other α-olefin (e.g., butene-1, hexene-1, etc.) in the second or subsequent polymerization steps. These (d1) polypropylene resins may be used alone or in combination of two or more. Examples of the combination of two or more are not particularly limited, but include, for example, a mixture of a crystalline propylene homopolymer and a crystalline propylene-ethylene block copolymer (excluding those having a Shore A hardness of 75 or less). The (d1) polypropylene resin is preferably a homopolypropylene and / or a block polypropylene, and more preferably a homopolypropylene.

[0059] The method for producing the polypropylene resin (d1) is not particularly limited, but examples thereof include a method of polymerizing a monomer containing propylene at a polymerization temperature of 0 to 100°C and a polymerization pressure of 3 to 100 atm in the presence of a titanium trichloride catalyst or a titanium halide catalyst supported on a carrier such as magnesium chloride and an alkylaluminum compound. At this time, a chain transfer agent such as hydrogen may be added to adjust the molecular weight of the resulting polymer. The polymerization method is not particularly limited, and may be either a batch method or a continuous method. In addition, solution polymerization in a solvent such as butane, pentane, hexane, heptane, or octane; slurry polymerization; bulk polymerization in a monomer without a solvent; and gas phase polymerization in a gaseous monomer may also be applied.

[0060] Furthermore, in order to increase the isotacticity and polymerization activity of the resulting polypropylene resin (d1), an electron donor compound can be used as an internal donor component or an external donor component as a third component of the catalyst in the polymerization catalyst. The type of the electron donor compound is not particularly limited, and known compounds can be used. For example, ester compounds such as ε-caprolactone, methyl methacrylate, ethyl benzoate, and methyl toluate; phosphites such as triphenyl phosphite and tributyl phosphite; phosphoric acid derivatives such as hexamethylphosphoramide; alkoxy ester compounds, aromatic monocarboxylic acid esters, aromatic alkylalkoxysilanes, aliphatic hydrocarbon alkoxysilanes, various ether compounds, various alcohols, and / or various phenols.

[0061] The melt flow rate (MFR) of the polypropylene resin (d1) (measured in accordance with JIS K7210 at 230°C under a load of 2.16 kg) is preferably 0.1 to 100 g / 10 min, more preferably 0.1 to 80 g / 10 min. By setting the MFR of the polypropylene resin (d1) within the above range, the balance between the fluidity and rigidity of the resin composition tends to be good. (d1) The method for controlling the MFR of the polypropylene resin within the above range is not particularly limited, but may be, for example, a method for controlling the ratio of the amount of hydrogen supplied to the amount of monomer.

[0062] -(d2) Modified polypropylene resin- The (d2) modified polypropylene resin may be, for example, a resin obtained by reacting the (d1) polypropylene resin with an α,β-unsaturated carboxylic acid or a derivative thereof in the presence or absence of a radical generator in a molten or solution state at 30 to 350°C. The (d2) modified polypropylene resin is not particularly limited, but may be, for example, a modified polypropylene resin obtained by grafting or adding 0.01 to 10 mass% of an α,β-unsaturated carboxylic acid or a derivative thereof to the (d1) polypropylene resin. Examples of the α,β-unsaturated carboxylic acid or a derivative thereof include, but are not particularly limited to, maleic anhydride and N-phenylmaleimide.

[0063] When the above (d1) polypropylene resin and the above (d2) modified polypropylene resin are used in combination, the mixing ratio of the (d1) polypropylene resin and the (d2) modified polypropylene resin in the (d) polypropylene-based resin is not particularly limited and can be determined arbitrarily.

[0064] The polypropylene resin (d) can be obtained by the above-mentioned method or other known methods. In addition, the polypropylene resin (a) may be used alone or in combination of two or more kinds, regardless of the crystallinity or melting point of the polypropylene resin (a).

[0065] (e) Admixtures The above-mentioned (e) admixture is not particularly limited, but is preferably a copolymer having a segment chain having high compatibility with the (a) and (b) components, and a segment chain having high compatibility with the (c) and (d) components. Examples of the segment chain having high compatibility with the (a) and (b) components include a chain mainly made of a vinyl aromatic compound such as a polystyrene chain, a polyphenylene ether chain, etc. Examples of the segment chain having high compatibility with the (c) and (d) components include a polyolefin chain, a copolymer elastomer molecular chain of ethylene and α-olefin, a chain mainly made of a conjugated diene compound, etc.

[0066] Specific examples of such copolymers include copolymers having a polystyrene chain-polyolefin chain, copolymers having a polyphenylene ether chain-polyolefin chain, copolymers having a polystyrene chain-conjugated diene chain, and hydrogenated block copolymers thereof. Among them, hydrogenated block copolymers are preferred from the viewpoint of thermal stability. These may be used alone or in combination of two or more.

[0067] Examples of the hydrogenated block copolymer as component (e) include a hydrogenated block copolymer in which at least a part of a block copolymer containing at least one polymer block I mainly made of a vinyl aromatic compound and at least one polymer block II mainly made of a conjugated diene compound is hydrogenated, and a modified product of the hydrogenated block copolymer. Among them, the hydrogenated block copolymer as component (e) is preferably a block copolymer in which at least a part of a block copolymer consisting of one type of polymer block I mainly made of a vinyl aromatic compound and one type of polymer block II mainly made of a conjugated diene compound is hydrogenated. The hydrogenated block copolymer as component (e) does not include the above-mentioned component (b).

[0068] Matters relating to the unmodified and modified hydrogenated block copolymers in component (e) are described below.

[0069] -Polymer block based on vinyl aromatic compounds I- The polymer block I mainly composed of a vinyl aromatic compound is not particularly limited, and examples thereof include a homopolymer block of a vinyl aromatic compound and a copolymer block of a vinyl aromatic compound and a conjugated diene compound. In addition, in the polymer block I, "mainly composed of a vinyl aromatic compound" means that the polymer block I before hydrogenation contains more than 50 mass% of vinyl aromatic compound units, preferably contains 70 mass% or more of vinyl aromatic compound units, more preferably contains 80 mass% or more, and may be 100 mass% or less.

[0070] Examples of the vinyl aromatic compound constituting the polymer block I include styrene, α-methylstyrene, vinyltoluene, p-tert-butylstyrene, diphenylethylene, etc., with styrene being preferred. Examples of the conjugated diene compound constituting polymer block I include butadiene, isoprene, 1,3-pentadiene, 2,3-dimethyl-1,3-butadiene, etc., with butadiene, isoprene, and combinations thereof being preferred, and butadiene being more preferred. These may be used alone or in combination of two or more.

[0071] From the viewpoint of improving dispersibility in the resin composition, the number average molecular weight (Mn) of the polymer block I is preferably 15,000 or more, more preferably 20,000 or more, even more preferably 25,000 or more, particularly preferably 26,000 or more, and is preferably 100,000 or less.

[0072] -Polymer block mainly composed of conjugated diene compounds II- The polymer block II mainly composed of a conjugated diene compound is not particularly limited, and examples thereof include a homopolymer block of a conjugated diene compound and a copolymer block of a conjugated diene compound and a vinyl aromatic compound. In addition, in the polymer block II, "mainly composed of a conjugated diene compound" means that the polymer block II before hydrogenation contains more than 50 mass% of conjugated diene compound units. From the viewpoint of increasing the fluidity of the resin composition, the polymer block II preferably contains 70 mass% or more of conjugated diene compound units, more preferably 80 mass% or more, and may contain 100 mass% or less.

[0073] Examples of the conjugated diene compound constituting the polymer block II include butadiene, isoprene, 1,3-pentadiene, 2,3-dimethyl-1,3-butadiene, etc., with butadiene, isoprene, and combinations thereof being preferred, and butadiene being more preferred. Examples of the vinyl aromatic compound constituting the polymer block II include styrene, α-methylstyrene, vinyltoluene, p-tert-butylstyrene, diphenylethylene, etc., with styrene being preferred. These may be used alone or in combination of two or more.

[0074] The hydrogenation rate of the ethylenic double bonds in the conjugated diene compound units contained in the polymer block II is preferably 80% or more, and more preferably 90% or more, from the viewpoint of obtaining even better rigidity, chemical resistance, impact resistance, and tracking resistance. The hydrogenation rate can be measured by using a nuclear magnetic resonance (NMR) spectrometer.

[0075] In the microstructure of the polymer block II (bonding form of the conjugated diene compound), the sum of the amount of 1,2-vinyl bonds and the amount of 3,4-vinyl bonds (total vinyl bond amount) relative to the ethylenic double bonds in the conjugated diene compound units contained in the polymer block II is preferably 50% or more, more preferably 55% or more, even more preferably 65% ​​or more, and is preferably 90% or less, from the viewpoint of increasing the compatibility of the polymer block II with the components (c) and (d) and improving the impact resistance.

[0076] The number average molecular weight (Mn) of the polymer block II is preferably 30,000 to 100,000, and more preferably 40,000 to 100,000, from the viewpoint of obtaining even better rigidity, chemical resistance, impact resistance, and tracking resistance.

[0077] The glass transition temperature of the polymer block II after hydrogenation is preferably higher than -50°C, more preferably higher than -50°C and not higher than 0°C, and even more preferably from -40 to -10°C, from the viewpoint of obtaining even better rigidity, chemical resistance, impact resistance, and tracking resistance.

[0078] The distribution of the vinyl aromatic compound in the molecular chain of polymer block I and the conjugated diene compound in the molecular chain of polymer block II contained in the block copolymer as the component (e) is not particularly limited, and examples thereof include random, tapered (wherein the monomer portion increases or decreases along the molecular chain), partial block, and combinations thereof.

[0079] The block structure of the block copolymer of the unmodified and modified hydrogenated block copolymer as the component (e) is not particularly limited, and for example, when polymer block I is represented as "I" and polymer block II is represented as "II", the component (c) may have structures such as I-II, I-II-I, II-I-II-I, (I-II-)4M, and I-II-I-II-I. Here, (I-II-)4M is a reaction residue of a polyfunctional coupling agent such as silicon tetrachloride (M=Si) or tin tetrachloride (M=Sn), or a residue of an initiator such as a polyfunctional organolithium compound. The component (e) may contain a block other than polymer block I and polymer block II.

[0080] The molecular structure of the unmodified and modified hydrogenated block copolymers as component (e) above is not particularly limited, and examples thereof include linear, branched, radial, and combinations thereof.

[0081] When the block copolymer as the component (e) contains a plurality of polymer blocks I or a plurality of polymer blocks II, the plurality of polymer blocks I or the plurality of polymer blocks II may have the same structure or different structures.

[0082] From the viewpoint of improving the fluidity, impact resistance, and appearance of the component (e) and reducing the occurrence of welds, the content of vinyl aromatic compound units in the block copolymer before hydrogenation is preferably 30% by mass or more, more preferably 32% by mass or more, and even more preferably more than 40% by mass, and is preferably 50% by mass or less, more preferably 48% by mass or less. The content of the vinyl aromatic compound can be measured using an ultraviolet spectrophotometer.

[0083] The total ratio of the 1,2-vinyl bond content and the 3,4-vinyl bond content to the ethylenic double bonds in the conjugated diene compound units contained in the above component (e) is preferably more than 50% and not more than 90%, more preferably 60 to 90%.

[0084] In the above component (e), the hydrogenation rate relative to the ethylenic double bonds (double bonds in the conjugated diene compound units) in the block copolymer is preferably 80 to 100%, and more preferably 90 to 100%.

[0085] In the above component (e), the number average molecular weight (Mn) of the block copolymer before hydrogenation is preferably 5,000 or more, more preferably 10,000 or more, and even more preferably 30,000 or more, and is preferably 1,000,000 or less, more preferably 800,000 or less, and even more preferably 500,000 or less. In the component (e), the molecular weight peak of the block copolymer after hydrogenation is preferably 5,000 or more, more preferably 10,000 or more, and even more preferably 30,000 or more, and is preferably 1,000,000 or less, more preferably 800,000 or less, even more preferably 500,000 or less, and particularly preferably 100,000 or less.

[0086] In the above component (e), the molecular weight distribution (Mw / Mn) of the block copolymer before hydrogenation is preferably 10 or less, more preferably 8 or less, and even more preferably 5 or less. The molecular weight distribution (Mw / Mn) can be calculated by dividing the weight average molecular weight (Mw) determined using GPC (mobile phase: chloroform, standard substance: polystyrene) by the above-mentioned number average molecular weight (Mn).

[0087] The method for hydrogenating the block copolymer is not particularly limited, and examples thereof include a method of hydrogenating the block copolymer using a supported heterogeneous hydrogenation catalyst in which a metal such as Ni, Pt, Pd, Ru, etc. is supported on carbon, silica, alumina, diatomaceous earth, etc., a so-called Ziegler type hydrogenation catalyst which uses a transition metal salt such as an organic acid salt or an acetylacetone salt of Ni, Co, Fe, Cr, etc., and a reducing agent such as an organoaluminum, or a so-called organometallic complex of an organometallic compound such as Ti, Ru, Rh, Zr, etc., at a reaction temperature of 0 to 200° C. and a hydrogen pressure of 0.1 to 15 MPa.

[0088] The method for synthesizing the block copolymer containing polymer block I and polymer block II is not particularly limited, and examples thereof include known methods such as anionic polymerization.

[0089] The method for producing the unmodified and modified hydrogenated block copolymers is not particularly limited, and known production methods can be used. For example, the methods described in JP-A-47-11486, JP-A-49-66743, JP-A-50-75651, JP-A-54-126255, JP-A-56-10542, JP-A-56-62847, JP-A-56-100840, JP-A-2-300218, GB Patent No. 1,130,770, U.S. Pat. No. 3,281,383, U.S. Pat. No. 3,639,517, GB Patent No. 1,020,720, U.S. Pat. No. 3,333,024, and U.S. Pat. No. 4,501,857 can be mentioned.

[0090] In the following, particular attention will be given to the modified hydrogenated block copolymer in component (e).

[0091] -Modified hydrogenated block copolymer- The modified hydrogenated block copolymer is obtained by grafting or adding an α,β-unsaturated carboxylic acid or a derivative thereof (eg, an acid anhydride, an ester, etc.) to the unmodified hydrogenated block copolymer.

[0092] The proportion of mass increase due to grafting or addition is not particularly limited, and is preferably 0.01% by mass or more, and preferably 10% by mass or less, more preferably 7% by mass or less, and even more preferably 5% by mass or less, relative to 100% by mass of the unmodified hydrogenated block copolymer.

[0093] The method for producing the modified hydrogenated block copolymer is not particularly limited, and examples thereof include a method in which the unmodified hydrogenated block copolymer is reacted with an α,β-unsaturated carboxylic acid or a derivative thereof in the presence or absence of a radical generator, in a molten state, a solution state or a slurry state, at a temperature of 80 to 350° C.

[0094] (f) Phosphate ester compounds The resin composition of the present embodiment preferably further contains (f) a phosphate ester compound. The (f) phosphoric acid ester compound optionally used in this embodiment is not particularly limited and may be any phosphoric acid ester compound (such as a phosphoric acid ester compound or a condensed phosphoric acid ester compound) having the effect of improving the flame retardancy of the resin composition, and examples thereof include triphenyl phosphate, phenyl bis dodecyl phosphate, phenyl bis neopentyl phosphate, phenyl-bis (3,5,5'-trimethyl-hexyl phosphate), ethyl diphenyl phosphate, 2-ethyl-hexyl di(p-tolyl) phosphate, bis-(2-ethylhexyl)-p-tolyl phosphate, tritolyl phosphate, bis-(2-ethylhexyl)phenyl phosphate, tri-(nonylphenyl) phosphate, di(dodecyl)-p-tolyl phosphate, tricresyl phosphate, dibutylphenyl phosphate, 2-chloroethyl diphenyl phosphate, p-tolyl bis(2,5,5'-trimethylhexyl) phosphate, 2-ethylhexyl diphenyl phosphate, bisphenol A bis(diphenyl phosphate), diphenyl-(3-hydroxyphenyl) phosphate, bisphenol A bis(dicresyl phosphate), resorcinol bis(diphenyl phosphate), resorcinol bis(dixylenyl phosphate), 2-naphthyl diphenyl phosphate, 1-naphthyl diphenyl phosphate, di(2-naphthyl)phenyl phosphate, etc. Among them, condensed phosphate ester compounds are preferred.

[0095] In particular, the (f) phosphate ester compound is represented by the following formula (4): [ka] [In formula (4), Q 41 , Q 42 , Q 43 , Q 44 are each independently an alkyl group having 1 to 6 carbon atoms; R 41 , R 42 are each independently a methyl group; R 43 , R 44are each independently a hydrogen atom or a methyl group; x is an integer of 0 or more; p1, p2, p3, and p4 are each an integer of 0 to 3; and q1 and q2 are each an integer of 0 to 2, and The following formula (5) [ka] [In formula (5), Q 51 , Q 52 , Q 53 , Q 54 are each independently an alkyl group having 1 to 6 carbon atoms; R 51 is a methyl group; y is an integer of 0 or more; r1, r2, r3, and r4 are each an integer of 0 to 3; and s1 is each an integer of 0 to 2. The aromatic condensed phosphate ester compound represented by the following formula (1) is preferably used as a main component. The condensed phosphate ester compounds represented by the above formula (4) and formula (5) may each contain a plurality of types of molecules, and x and y are preferably integers of 1 to 3 for each molecule.

[0096] As a suitable (e) phosphate compound containing as a main component at least one selected from the group consisting of condensed phosphate compounds represented by the above formula (4) and formula (5), a compound in which the average values ​​of x and y are, overall, at least 1 is preferred. The above suitable (e) phosphate compound can generally be obtained as a mixture containing at least 90% of compounds in which x and y are 1 to 3, and contains, in addition to compounds in which x and y are 1 to 3, polymers in which x and y are 4 or more and other by-products.

[0097] ((g) Phosphinates) In this embodiment, (g) a phosphinate can be used as necessary. As the (g) phosphinate, a phosphinate represented by the following formula (1) can be used. [ka] [In formula (1), R 11 and R12 are each independently a linear or branched alkyl group having 1 to 6 carbon atoms and / or an aryl group having 6 to 10 carbon atoms; M 1 is at least one selected from the group consisting of calcium ion, magnesium ion, aluminum ion, zinc ion, bismuth ion, manganese ion, sodium ion, potassium ion, and protonated nitrogen base; a is an integer of 1 to 3; m is an integer of 1 to 3; and a=m, and a diphosphinic acid salt represented by the following formula (2): [ka] [In formula (2), R 21 and R 22 are each independently a linear or branched alkyl group having 1 to 6 carbon atoms and / or an aryl group having 6 to 10 carbon atoms; R 23 is a linear or branched alkylene group having 1 to 10 carbon atoms, an arylene group having 6 to 10 carbon atoms, an alkylarylene group having 6 to 10 carbon atoms, or an arylalkylene group having 6 to 10 carbon atoms; M 2 is at least one selected from the group consisting of calcium ion, magnesium ion, aluminum ion, zinc ion, bismuth ion, manganese ion, sodium ion, potassium ion, and protonated nitrogen base; b is an integer of 1 to 3; n is an integer of 1 to 3; j is an integer of 1 or 2; and b·j=2n. At least one selected from the group consisting of: The (g) phosphinate may be a mixture of the phosphinate represented by the formula (1) and the diphosphinate represented by the formula (2).

[0098] Examples of the (g) phosphinate salts include calcium dimethylphosphinate, magnesium dimethylphosphinate, aluminum dimethylphosphinate, zinc dimethylphosphinate, calcium ethylmethylphosphinate, magnesium ethylmethylphosphinate, aluminum ethylmethylphosphinate, zinc ethylmethylphosphinate, calcium diethylphosphinate, magnesium diethylphosphinate, aluminum diethylphosphinate, zinc diethylphosphinate, calcium methyl-n-propylphosphinate, magnesium methyl-n-propylphosphinate, aluminum methyl-n-propylphosphinate, zinc methyl-n-propylphosphinate, calcium methane di(methylphosphinate), magnesium methane di(methylphosphinate), aluminum methane di(methylphosphinate), zinc methane di(methylphosphinate), calcium benzene-1,4-(dimethylphosphinate), Examples of the phosphinate include benzene-1,4-(dimethylphosphinate), magnesium benzene-1,4-(dimethylphosphinate), aluminum benzene-1,4-(dimethylphosphinate), zinc benzene-1,4-(dimethylphosphinate), calcium methylphenylphosphinate, magnesium methylphenylphosphinate, aluminum methylphenylphosphinate, zinc methylphenylphosphinate, calcium diphenylphosphinate, magnesium diphenylphosphinate, aluminum diphenylphosphinate, and zinc diphenylphosphinate. Of these, calcium dimethylphosphinate, aluminum dimethylphosphinate, zinc dimethylphosphinate, calcium ethylmethylphosphinate, aluminum ethylmethylphosphinate, zinc ethylmethylphosphinate, calcium diethylphosphinate, aluminum diethylphosphinate, and zinc diethylphosphinate are preferred, and aluminum diethylphosphinate is more preferred. (g) Commercially available phosphinates include, but are not limited to, Exolit (registered trademark) OP1230, OP1240, OP1311, OP1312, OP930, and OP935 manufactured by Clariant Japan.

[0099] ((h)Thermoplastic resin) The resin composition of the present embodiment may further contain (h) a thermoplastic resin. The (h) thermoplastic resin is a thermoplastic resin other than the above-mentioned components (a) to (g), and examples thereof include polystyrene, syndiotactic polystyrene, and high impact polystyrene.

[0100] (i) Other additives The resin composition of the present embodiment may further contain (i) other additives. The above (i) other additives are compounds other than the above-mentioned components (a) to (h), and examples thereof include block copolymers of vinyl aromatic compounds-conjugated diene compounds other than components (b) and (e), olefin-based elastomers other than components (c) and (d), antioxidants, metal deactivators, heat stabilizers, flame retardants other than components (f) and (g) (ammonium polyphosphate-based compounds, magnesium hydroxide, aromatic halogen-based flame retardants, silicone-based flame retardants, zinc borate, etc.), fluorine-based polymers, plasticizers (low molecular weight polyethylene, epoxidized soybean oil, polyethylene glycol, fatty acid esters, etc.), flame retardant assistants such as antimony trioxide, weather (light) resistance improvers, nucleating agents for polyolefins, slip agents, various colorants, release agents, etc.

[0101] The proportions of the components in the resin composition of this embodiment will be described below.

[0102] The content of each component in the resin composition of this embodiment is 50 to 80 parts by mass of the component (a), 5 to 30 parts by mass of the component (b), 1 to 20 parts by mass of the component (c), and 1 to 20 parts by mass of the component (e) relative to a total of 100 parts by mass of the components (a), (b), (c), (d), and (e), from the viewpoint of improving the impact resistance, chemical resistance, and self-tapping strength of the resin composition and imparting sufficient rigidity that can be applied to mechanical parts and structures. It is preferable that the component (a) is 55 to 75 parts by mass, the component (b) is 5 to 20 parts by mass, the component (c) is 1 to 10 parts by mass, and the component (e) is 1 to 15 parts by mass. The component (a) is preferably 55 to 75 parts by mass, more preferably 60 to 75 parts by mass. The amount of the component (b) is preferably 5 to 30 parts by mass, and more preferably 7 to 25 parts by mass. The total mass of the above-mentioned (a), (b), (c), (d) and (e) components may be 80 to 100 parts by mass, 85 to 100 parts by mass, or even 100 parts by mass, relative to 100 parts by mass of the resin composition of this embodiment.

[0103] The mass proportion of the component (d) relative to 100 parts by mass of the total mass of the components (a), (b), (c), (d) and (e) is preferably 1 to 10 parts by mass, and more preferably 2 to 8 parts by mass, from the viewpoint of improving impact resistance, chemical resistance and self-tapping strength and imparting sufficient rigidity for application to mechanical parts and structures. From the viewpoint of increasing the impact resistance, chemical resistance, and self-tapping strength of the resin composition and imparting sufficient rigidity for application to mechanical parts and structures, the mass ratio (c) / (d) of the above component (c) to the above component (d) is 1 to 5, and preferably 1 to 3.

[0104] From the viewpoint of the balance of mechanical properties of the composition, the content of the (f) phosphate compound is preferably 5 to 30 parts by mass per 100 parts by mass of the total of the (a) to (e) components.

[0105] From the viewpoints of balancing the mechanical properties and flame retardancy of the resin composition and improving the self-tapping strength, the content of the (g) phosphinic acid salt is preferably 1 to 30 parts by mass, and more preferably 2 to 20 parts by mass, per 100 parts by mass of the total of the (a) to (e) components.

[0106] The content of the (h) thermoplastic resin is not particularly limited as long as it does not impair the effects of the present invention, and may be, for example, 0 to 400 parts by mass per 100 parts by mass of the total of the (a) to (d) components.

[0107] (Flexural modulus) The resin composition of the present embodiment preferably has a flexural modulus of 1600 MPa or more, more preferably 1700 to 3000 MPa, measured in accordance with ISO 178. When the flexural modulus is within this range, the composition can have rigidity suitable for use in structural parts and structures. In order to achieve a flexural modulus of 1600 MPa or more, specific components (a) to (e), and, if necessary, specific amounts of components (f), (g), and (h) can be included to appropriately adjust the content.

[0108] (Morphology) In terms of mechanical strength and chemical resistance, the morphology of the resin composition of the present embodiment is such that (a) the polyphenylene ether resin forms a continuous phase. These morphologies can be observed, for example, using a TEM (transmission electron microscope). Specifically, they can be observed by the method described in the examples below.

[0109] (Method of producing resin composition) The resin composition of the present embodiment can be produced by melt-kneading the above-mentioned components (a) to (e), and, as necessary, components (f), (g), (h), and (i).

[0110] A preferred method for producing the resin composition of the present embodiment is a production method including the following steps (1-1) and (1-2). (1-1): A step of melt-kneading the above-mentioned (a) component and (e) component to obtain a kneaded product. (1-2): A step of adding the above-mentioned (b), (c), and (d) components to the kneaded product obtained in the above-mentioned (1-1), and melt-kneading the mixture. In the step (1-1), the component (a) may be added in its entirety or in part. The component (e) may be added in its entirety or in part. Among these, the step (1-1) is preferably a step of melt-kneading the entire amount of the component (a) and, if necessary, the entire amount or part of the component (e) to obtain a kneaded product. In the step (1-2), the components (b), (c), and (d) may be added in their entirety or in part. When a portion is added in the step (1-2), the components (b), (c), and (d) may be added in their entirety in the steps (1-1) and (1-2). The step (1-2) is preferably a step of adding the entire amounts of the components (b), (c), and (d) to the kneaded product obtained in the step (1-1) and melt-kneading the mixture. In this manufacturing method, by adding components (b), (c), and (d) in step (1-2) during melt-kneading (particularly by adding all of components (b), (c), and (d) in step (1-2)), components (b), (c), and (d) are efficiently dispersed in component (a), and a resin composition having even more excellent chemical resistance and self-tapping strength can be obtained.

[0111] The melt kneader suitably used for melt kneading each component in the method for producing the resin composition of the present embodiment is not particularly limited, and examples thereof include extruders such as multi-screw extruders such as single-screw extruders and twin-screw extruders, rolls, kneaders, Brabender plastographs, Banbury mixers, etc., and from the viewpoint of kneading properties, twin-screw extruders are particularly preferred. Specific examples of twin-screw extruders include the ZSK series manufactured by Coperion, the TEM series manufactured by Toshiba Machine Co., Ltd., and the TEX series manufactured by The Japan Steel Works, Ltd. The type, specifications, etc. of the extruder are not particularly limited and may be any known type.

[0112] A preferred embodiment in which an extruder such as a single screw extruder or a multi-screw extruder such as a twin screw extruder is used will be described below.

[0113] The L / D (effective barrel length / inner barrel diameter) of the extruder is preferably 20 or more, more preferably 30 or more, and is preferably 75 or less, more preferably 60 or less.

[0114] The configuration of the extruder is not particularly limited, and may be, for example, an extruder including a first raw material supply port on the upstream side in the direction in which the raw materials flow, a first vacuum vent downstream of the first raw material supply port, a second raw material supply port downstream of the first vacuum vent, a first liquid addition pump downstream of the second raw material supply port, a second vacuum vent downstream of the first liquid addition pump, and a second liquid addition pump downstream of the second vacuum vent.

[0115] The method of supplying the raw material through the second raw material supply port is not particularly limited, and may be a method of simply adding the raw material through the upper opening of the raw material supply port, or a method of adding the raw material through the side opening using a forced side feeder. In particular, from the viewpoint of stable supply, the method of adding the raw material through the side opening using a forced side feeder is preferred.

[0116] When the components are melt-kneaded, the melt-kneading temperature is not particularly limited and may be 200 to 370° C., and the screw rotation speed is not particularly limited and may be 100 to 1200 rpm.

[0117] When adding a liquid raw material, it can be added by directly feeding the liquid raw material into the cylinder system using a liquid addition pump or the like in the cylinder part of the extruder. The liquid addition pump is not particularly limited, and examples thereof include gear pumps and flange-type pumps, and gear pumps are preferred. At this time, from the viewpoint of reducing the load on the liquid addition pump and improving the operability of the raw material, it is preferred to heat the parts that serve as the flow path of the liquid raw material, such as a tank for storing the liquid raw material, a piping between the tank and the liquid addition pump, and a piping between the pump and the extruder cylinder, using a heater or the like to reduce the viscosity of the liquid raw material.

[0118] [Molded body] A molded article can be obtained from the resin composition of this embodiment. The molded article is not particularly limited, and examples thereof include automobile parts, interior and exterior parts of electric equipment, and other parts. Examples of automobile parts are not particularly limited, and examples thereof include exterior parts such as bumpers, fenders, door panels, various moldings, emblems, engine hoods, wheel caps, roofs, spoilers, and various aero parts; interior parts such as instrument panels, console boxes, and trims; secondary battery case parts mounted on automobiles, electric vehicles, hybrid electric vehicles, power-assisted bicycles, wheelchairs, and the like; lithium-ion secondary battery parts, and the like. In addition, examples of interior and exterior parts of electric equipment are not particularly limited, and examples thereof include various computers and their peripheral devices, junction boxes, various connectors, other office automation equipment, cabinets for televisions, videos, and various disc players, and chassis, and parts used in refrigerators, air conditioners, and liquid crystal projectors. Other parts include electric wires and cables obtained by applying a coating to metal conductors or optical fibers, fuel cases for solid methanol batteries, fuel cell water pipes, water cooling tanks, boiler exterior cases, ink-related parts and components for inkjet printers, furniture (chairs, etc.), chassis, water piping, joints, etc.

[0119] (Method of Manufacturing Molded Product) The molded article can be produced by molding the resin composition of the present embodiment described above. The method for producing the molded body is not particularly limited, and examples thereof include injection molding, extrusion molding, extrusion profile molding, blow molding, and compression molding. From the viewpoint of more effectively obtaining the effects of the present invention, injection molding is preferred. EXAMPLES

[0120] Hereinafter, the present invention will be described in detail with reference to examples, but the present invention is not limited to these examples.

[0121] The raw materials used for the resin compositions and molded articles in the examples and comparative examples are shown below.

[0122] -(a) Polyphenylene ether resin- (ai): The reduced viscosity (η sp / c: 0.5g / dL chloroform solution) 0.51dL / g polyphenylene ether (a-ii): The reduced viscosity (η sp / c: 0.5g / dL chloroform solution) 0.42dL / g polyphenylene ether The reduced viscosity is η sp / c: Measured using a 0.5 g / dL chloroform solution at 30°C using an Ubbelohde type viscometer.

[0123] -(b) Hydrogenated block copolymer- An unmodified block copolymer was synthesized by using polystyrene as polymer block A and polybutadiene as polymer block B. The physical properties of the obtained block copolymer are shown below. (bi): Polystyrene content in block copolymer before hydrogenation: 30 mass%, molecular weight peak of block copolymer after hydrogenation: 125,000, number average molecular weight (Mn) of polystyrene block: 18,750, number average molecular weight (Mn) of polybutadiene block: 87,500, molecular weight distribution (Mw / Mn) of block copolymer before hydrogenation: 1.10, 1,2-vinyl bond amount (total vinyl bond amount) in polybutadiene block before hydrogenation: 40%, hydrogenation rate of polybutadiene portion constituting polybutadiene block: 35%, glass transition temperature of polybutadiene block after hydrogenation: -80°C. The content of vinyl aromatic compounds was measured using an ultraviolet spectrophotometer. The number average molecular weight (Mn) and the molecular weight peak were determined using GPC (mobile phase: chloroform, standard substance: polystyrene). The molecular weight distribution (Mw / Mn) was calculated by dividing the weight average molecular weight (Mw) determined by a conventional method using GPC (mobile phase: chloroform, standard substance: polystyrene) by the number average molecular weight (Mn) described above. The total vinyl bond amount was measured using an infrared spectrophotometer and calculated according to the method described in Analytical Chemistry, Volume 21, No. 8, August 1949. The hydrogenation rate was measured using a nuclear magnetic resonance apparatus (NMR). The mixing ratio was determined from the peak area ratio during GPC measurement. (b-ii): Polystyrene content in block copolymer before hydrogenation: 30 mass%, molecular weight peak of block copolymer after hydrogenation: 53,000, number average molecular weight (Mn) of polystyrene block: 8,000, number average molecular weight (Mn) of polybutadiene block: 37,000, molecular weight distribution (Mw / Mn) of block copolymer before hydrogenation: 1.10, 1,2-vinyl bond amount (total vinyl bond amount) in polybutadiene block before hydrogenation: 40%, hydrogenation rate of polybutadiene portion constituting polybutadiene block: 35%, glass transition temperature of polybutadiene block after hydrogenation: -80°C. (b-iii): Polystyrene content in block copolymer before hydrogenation: 20 mass%, molecular weight peak of block copolymer after hydrogenation: 100,000, number average molecular weight (Mn) of polystyrene block: 10,000, number average molecular weight (Mn) of polybutadiene block: 80,000, molecular weight distribution (Mw / Mn) of block copolymer before hydrogenation: 1.10, 1,2-vinyl bond amount (total vinyl bond amount) in polybutadiene block before hydrogenation: 45%, hydrogenation rate of polybutadiene portion constituting polybutadiene block: 70%, glass transition temperature of polybutadiene block after hydrogenation: -73°C. (b-iv): Polystyrene content in block copolymer before hydrogenation: 30 mass%, molecular weight peak of block copolymer after hydrogenation: 200,000, number average molecular weight (Mn) of polystyrene block: 30,000, number average molecular weight (Mn) of polybutadiene block: 140,000, molecular weight distribution (Mw / Mn) of block copolymer before hydrogenation: 1.10, 1,2-vinyl bond amount (total vinyl bond amount) in polybutadiene block before hydrogenation: 33%, hydrogenation rate of polybutadiene portion constituting polybutadiene block: 99%, glass transition temperature of polybutadiene block after hydrogenation: -55°C.

[0124] -(c) Olefin polymer- (ci): Ethylene-butene copolymer, product name "Tafmer DF610", manufactured by Mitsui Chemicals, Inc., MFR: 1.2 g / 10 min (190°C, 2.16 kgf condition), brittle temperature: <-70°C, density: 0.862 g / cm 3 (c-ii): Ethylene-butene copolymer, trade name "Tafmer DF810", manufactured by Mitsui Chemicals, Inc., MFR: 1.2 g / 10 min (190°C, 2.16 kgf condition), brittle temperature: <-70°C, density: 0.885 g / cm 3 (c-iii): Ethylene-butene copolymer, trade name "Tafmer DF110", manufactured by Mitsui Chemicals, Inc., MFR: 1.2 g / 10 min (190°C, 2.16 kgf condition), brittle temperature: <-70°C, density: 0.905 g / cm 3 (c-iv): Low density polyethylene, MFR = 2.0 g / 10 min (190°C, 2.16 kgf condition), brittle temperature: -80°C, density: 0.918 g / cm 3 (cv): Product name "Tafmer BL3450M", manufactured by Mitsui Chemicals, Inc., MFR: 4.0g / 10min (190℃, 2.16kgf condition), Brittle temperature: -32℃

[0125] -(d) Polypropylene resin- Propylene homopolymer (melting point: 165°C, MFR: 0.4g / 10min (230°C, 2.16kgf conditions))

[0126] -(e) Admixtures- A block copolymer having a block structure of II-I-II-I was synthesized by a known method, with polymer block I being made of polystyrene and polymer block II being made of polybutadiene. The synthesized block copolymer was hydrogenated by a known method. The polymer was not modified. The physical properties of the obtained unmodified hydrogenated block copolymer are shown below. Polystyrene content in block copolymer before hydrogenation: 44 mass%, molecular weight peak of block copolymer after hydrogenation: 95,000, number average molecular weight (Mn) of polystyrene block: 41,800, number average molecular weight (Mn) of polybutadiene block: 53,200, molecular weight distribution (Mw / Mn) of block copolymer before hydrogenation: 1.06, 1,2-vinyl bond amount (total vinyl bond amount) in polybutadiene block before hydrogenation: 75%, hydrogenation rate of polybutadiene portion constituting polybutadiene block: 99%, glass transition temperature of polybutadiene block after hydrogenation: -15°C.

[0127] -(f) Phosphate ester compounds- (f): "E890" (condensed phosphate ester compound) manufactured by Daihachi Chemical Industry Co., Ltd.

[0128] -(g) Phosphinates- (g): Clariant Japan "Exolit OP930" (corresponding to formula (1))

[0129] Measurement methods (1) to (5) of physical properties in the examples and comparative examples are shown below.

[0130] (1) Morphology The obtained resin composition pellets were fed into a small injection molding machine (product name: IS-100GN, manufactured by Toshiba Machine Co., Ltd.) with a cylinder temperature set to 280°C, and molded under conditions of a mold temperature of 70°C, injection pressure of 70 MPa, injection time of 20 seconds, and cooling time of 15 seconds to produce ISO dumbbells for evaluation. Ultrathin sections were prepared from this ISO dumbbell using an ultramicrotome, and the (b) component was stained with osmium tetroxide. The stained ultrathin sections were observed using a TEM (product name "HT7700", manufactured by Hitachi High-Technologies Corporation) to obtain images at a magnification of 10,000 times. The obtained images were observed to determine whether or not the (a) component formed a continuous phase. Cases in which the (a) component formed a continuous phase (including cases in which the (a) component and other components were co-continuous) were judged as "good", and cases in which the (a) component was a dispersed phase were judged as "bad".

[0131] (2) Flexural modulus (1) The flexural modulus (MPa) of ISO dumbbells injection molded under the same conditions as those used for the morphology evaluation was measured according to ISO 178. The higher the flexural modulus, the better the rigidity was judged to be. In particular, when the flexural modulus was 1600 MPa or more, it was judged that the rigidity was sufficient for application to mechanical parts and structures.

[0132] (3) Charpy impact strength (1) Using ISO dumbbells injection-molded under the same conditions as those used for the morphology evaluation, the notched Charpy impact strength was measured in a 23°C environment in accordance with ISO179 1eA.

[0133] (4) Chemical resistance The obtained pellets of the resin composition were fed into a small injection molding machine (product name: IS-100GN, manufactured by Toshiba Machine Co., Ltd.) with a cylinder temperature set to 280°C, and molded into a flat plate of 150 mm x 150 mm x 3 mm under conditions of a mold temperature of 70°C, an injection pressure of 75 MPa, an injection time of 20 seconds, and a cooling time of 15 seconds. A test piece measuring 75 mm x 12.7 mm x 3 mm was cut out from this plate and set in a bending form designed to change the strain continuously. CRC 5-56 (manufactured by CRC Industries, USA) was applied to the surface of the test piece and left for 48 hours under the conditions of 23°C x 50% RH. After 48 hours, the test piece was strained, and the stopping position of the bending form when cracks appeared on the surface of the test piece was measured to determine the critical strain amount (%) that indicates the limit of the strain amount at which cracks do not occur. As an evaluation criterion, it was determined that the greater the critical strain value, the more excellent the chemical resistance.

[0134] (5) Self-tapping strength The obtained pellets of the resin composition were fed into a small injection molding machine (product name: IS-100GN, manufactured by Toshiba Machine Co., Ltd.) with a cylinder temperature set to 280°C, and a molded product having a boss with an inner diameter of 2.55 mm and an outer diameter of 5.75 mm was molded under conditions of a mold temperature of 70°C and an injection pressure of 70 MPa. A P-tight screw (size M3 × 10) was screwed into the boss of the obtained molded product, and the maximum screwing torque (N·m) at which the resin inside the boss was broken or damaged was measured. It was determined that the higher this torque value, the better the self-tapping strength and the greater the freedom in designing and assembling the actual product.

[0135] (6) Flame retardancy The obtained resin composition pellets were fed to a small injection molding machine (product name: IS-100GN, manufactured by Toshiba Machine Co., Ltd.) set at a cylinder temperature of 280°C, and molded under conditions of a mold temperature of 70°C and an injection pressure of 60MPa to prepare five test pieces (1.6 mm thick) for measuring UL94 vertical combustion test. The flame retardancy of these five test pieces was evaluated based on the UL94 vertical combustion test method. After 10 seconds of contact with the flame, the burning time from when the flame was removed until the flame went out was defined as t1 (seconds), and after 10 seconds of contact with the flame again, the burning time from when the flame was removed until the flame went out was defined as t2 (seconds). The average of t1 and t2 was calculated as the average burning time for each of the five pieces. Meanwhile, the maximum of the 10 burning times, including t1 and t2, was calculated as the maximum burning time. Then, based on the UL94 standard, the test pieces were judged as V-0, V-1, V-2, and HB. In particular, when the flame retardancy level was judged to be V-1 or higher, the material was judged to have excellent flame retardancy.

[0136] (Examples 1 to 16, Comparative Examples 1 to 11) Each example and comparative example will be described in detail below. A twin-screw extruder (ZSK-25, manufactured by Coperion) was used as a melt kneader for producing the resin compositions of each of the Examples and Comparative Examples. The L / D of the extruder was set to 35. The twin-screw extruder was configured to include a first raw material supply port on the upstream side in the direction in which the raw materials flow, a first vacuum vent downstream of the first raw material supply port, a second raw material supply port downstream of the first vacuum vent, a liquid addition pump downstream of the second raw material supply port, and a second vacuum vent downstream of the liquid addition pump. The barrel temperature of the twin-screw extruder was set to 320°C from the first raw material supply port to the first vacuum vent, and 280°C downstream of the second raw material supply port, and pellets of the resin composition were produced under the conditions of a screw rotation speed of 300 rpm and an extrusion rate of 15 kg / h. The configuration of the twin-screw extruder is shown in Table 1.

[0137] [Table 1]

[0138] Components (a) to (g) were fed into the twin-screw extruder set up as described above as shown in Tables 2 and 3 to obtain pellets of the resin composition. For each of the Examples and Comparative Examples, physical property tests were carried out using the above-mentioned measuring methods (1) to (6). The results are shown in Tables 2 and 3.

[0139] [Table 2]

[0140] [Table 3]

[0141] As shown in Tables 2 and 3, the resin compositions of the examples were found to have superior impact resistance, chemical resistance, and tracking resistance compared to the resin compositions of the comparative examples, and to have rigidity that makes them suitable for use in mechanical parts and structures. [Industrial Applicability]

[0142] According to the present invention, it is possible to obtain a resin composition and a molded article having excellent impact resistance, chemical resistance, and tracking resistance, and having rigidity that can be applied to mechanical parts and structures. The molded article containing the resin composition of the present invention is suitably used as an automobile part, an interior / exterior part of an electric device, other parts, etc.

Claims

1. (a) a polyphenylene ether resin; (b) a hydrogenated block copolymer obtained by hydrogenating at least a portion of a block copolymer including at least one polymer block A mainly made of a vinyl aromatic compound and at least one polymer block B mainly made of a conjugated diene compound, and / or a modified product of the hydrogenated block copolymer; (c) an olefin polymer comprising an olefin other than propylene; (d) a polypropylene-based resin; (e) an admixture which is a compound different from the (b) component; Contains the component (e) is a hydrogenated block copolymer obtained by hydrogenating at least a portion of a block copolymer including at least one polymer block I mainly made of a vinyl aromatic compound and at least one polymer block II mainly made of a conjugated diene compound, and / or a modified product of the hydrogenated block copolymer; the total ratio of 1,2-vinyl bonds and 3,4-vinyl bonds to the ethylenic double bonds in the conjugated diene compound units contained in the polymer block II is 65% or more and 90% or less, the mass ratio of the component (a) is 50 to 80 parts by mass, the mass ratio of the component (b) is 5 to 30 parts by mass, the mass ratio of the component (c) is 1 to 20 parts by mass, and the mass ratio of the component (e) is 1 to 20 parts by mass, relative to a total of 100 parts by mass of the component (a), the component (b), the component (c), the component (d), and the component (e); the mass ratio (c) / (d) of the component (c) to the component (d) is 1 to 5; The component (a) forms a continuous phase, the glass transition temperature of the polymer block B in the component (b) is −65° C. or lower, The brittle temperature of the component (c) is −50° C. or lower. A resin composition comprising:

2. The resin composition according to claim 1 , further comprising (f) a phosphoric acid ester compound.

3. Further, (g) a phosphinate is contained, The component (g) is a phosphinate represented by the following general formula (1): 【Chemistry 1】 [In the formula, R 11 and R 12 are each independently a linear or branched alkyl group having 1 to 6 carbon atoms and / or an aryl group having 6 to 10 carbon atoms; M 1 is at least one selected from the group consisting of calcium ion, magnesium ion, aluminum ion, zinc ion, bismuth ion, manganese ion, sodium ion, potassium ion, and protonated nitrogen base; a is an integer of 1 to 3; m is an integer of 1 to 3; and a=m; and A diphosphinate represented by the following formula (2): 【Chemistry 2】 [In the formula, R 21 and R 22 are each independently a linear or branched alkyl group having 1 to 6 carbon atoms and / or an aryl group having 6 to 10 carbon atoms; R 23 is a linear or branched alkylene group having 1 to 10 carbon atoms, an arylene group having 6 to 10 carbon atoms, an alkylarylene group having 6 to 10 carbon atoms, or an arylalkylene group having 6 to 10 carbon atoms; M 2 is at least one selected from the group consisting of calcium ion, magnesium ion, aluminum ion, zinc ion, bismuth ion, manganese ion, sodium ion, potassium ion, and protonated nitrogen base; b is an integer of 1 to 3; n is an integer of 1 to 3; j is an integer of 1 or 2; and b·j=2n. The resin composition according to claim 1 or 2, comprising at least one phosphinate selected from the group consisting of:

4. The resin composition according to any one of claims 1 to 3, wherein the component (c) is an ethylene-1-butene copolymer.

5. The density of the component (c) is 0.87 g / cm 3 The resin composition according to any one of claims 1 to 4.

6. The density of the component (c) is 0.90 g / cm 3 The resin composition according to any one of claims 1 to 5.

7. The resin composition according to any one of claims 1 to 6, wherein the component (d) is a propylene homopolymer.

8. the component (e) is a hydrogenated block copolymer obtained by hydrogenating at least a portion of a block copolymer including at least one polymer block I mainly made of a vinyl aromatic compound and at least one polymer block II mainly made of a conjugated diene compound, and / or a modified product of the hydrogenated block copolymer; the total of 1,2-vinyl bonds and 3,4-vinyl bonds relative to the double bonds in the conjugated diene compound units contained in the component (e) is more than 50% and not more than 90%, the content of vinyl aromatic compound units in the component (e) before hydrogenation is 30 to 50 mass %, The glass transition temperature of the polymer block II in the component (e) is higher than −50° C., The resin composition according to any one of claims 1 to 7, wherein a hydrogenation rate of double bonds in the conjugated diene compound units contained in the component (e) is 80 to 100%.

9. The resin composition according to any one of claims 1 to 8, having a flexural modulus measured in accordance with ISO 178 of 1600 MPa or more.

Citation Information

Patent Citations

  • Small electromagnetic relay and method of making same

    JP1979022561A

  • Polyphenylene ether resin composition

    JP1995331057A

  • Resin composition for cladding material of wire and cable

    JP2004161929A

  • Flexible poly(arylene ether) compositions and articles thereof

    JP2007519782A

  • Flame-retardant poly(arylene ether) composition and its use as a coating material for coated wires

    JP2010540716A