Styrenic resin composition and molded article
Optimizing the styrene resin and cellulose polysaccharide composition with specific refractive index and MFR, along with a dispersant, addresses compatibility issues, enhancing light transmittance and heat resistance in molded articles.
Patent Information
- Application Number
- JP2021058003
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-04-01
- Filing Date
- 2021-03-30
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-03-30
AI Technical Summary
Existing styrenic resin compositions with cellulose materials suffer from poor light transmittance, heat resistance, and appearance due to inadequate consideration of cellulose material length and compatibility with styrene resin, leading to colored and deteriorated products.
A styrene resin composition with a specific refractive index and MFR, combined with cellulose polysaccharides of defined size and aspect ratio, and optionally including a dispersant, to enhance compatibility and dispersion, resulting in improved light transmittance and heat resistance.
The composition achieves excellent light transmittance, heat resistance, and appearance in molded articles by optimizing the styrene resin and cellulose polysaccharide ratio and properties.
Smart Images

Figure 0007573472000004 
Figure 0007573472000001 
Figure 0007573472000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a styrene-based resin composition and a molded article. [Background technology]
[0002] Styrene-based resins are used in a wide range of applications due to their excellent moldability, dimensional stability, and transparency. Biomass materials have also been attracting attention from the perspective of environmental protection, and composite materials made from resin materials and naturally derived organic fillers or biopolymers are being investigated. For example, Patent Documents 1 and 2 disclose a styrene-based composite resin composition consisting of a styrene-based resin and a cellulose-based material. Patent Document 3 discloses a composition consisting of a styrene-based resin and modified nanocellulose (hereinafter also referred to as CNF). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 7-173352 [Patent Document 2] Japanese Patent Application Publication No. 8-231795 [Patent Document 3] JP 2016-176052 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, the techniques of Patent Documents 1 and 2 do not consider the average length of the cellulose-based material used or the compatibility of the styrene-based resin with the cellulose-based material. More specifically, Patent Documents 1 and 2 use wood flour or pulp with an average minor or major axis length of more than 50 μm, and do not consider the dispersibility or compatibility of the cellulose-based material with the styrene-based resin, so that the desired light transmittance cannot be obtained, the molded appearance is significantly deteriorated, and the products are limited. Furthermore, the technique of Patent Document 2 uses wood flour as the cellulose-based material, so there is a problem that the composition itself is colored and the appearance is deteriorated. In addition, the technology of Patent Document 3 uses modified CNF, which is costly to modify and leaves unreacted modifier remaining in the composition, resulting in problems such as reduced light transmittance, heat resistance, and appearance.
[0005] Accordingly, an object of the present invention is to provide a styrene-based resin composition excellent in light transmittance, heat resistance and appearance, and a molded article containing the styrene-based resin composition. [Means for solving the problem]
[0006] In view of the above problems, the present inventors have conducted intensive research and repeated experiments, and as a result, have found that the above problems can be solved by using a resin composition in which a styrene-based resin (a) having a refractive index of 1.545 to 1.600 and an MFR of 3 or more is mixed with a cellulose-based polysaccharide (b) of a specific size in a specific ratio, thereby completing the present invention. That is, the present invention is as follows.
[0007] [1] The present invention provides a styrene-based resin composition comprising: (a) a styrene-based resin having a refractive index of 1.545 to 1.600 and an MFR of 3 or more; and (b) a cellulose-based polysaccharide having an average minor axis length d1 and an average major axis length d2 that is equal to or greater than d1, wherein either d1 or d2 is 0.03 to 50 μm, the content of the styrene-based resin (a) is 45.0 to 99.5 parts by mass relative to the total amount (100 parts by mass) of the styrene-based resin (a) and the cellulose-based polysaccharide (b); The styrene-based resin composition is characterized in that the content of the cellulose-based polysaccharide (b) is 0.5 to 55.0 parts by mass. [2] In the present invention, the styrene-based resin (a) preferably contains an unsaturated carboxylic acid-based monomer unit. [3] In the present invention, it is preferable to further contain 0.5 to 2.0 parts by mass of a dispersing agent (c) based on the total amount (100 parts by mass) of the styrene-based resin (a) and the cellulose-based polysaccharide (b). [4] In the present invention, the dispersant (c) is preferably one or more compounds selected from the group consisting of fatty acid ester compounds, polyethylene glycol compounds, terpene compounds, and rosin compounds. [5] The present invention relates to a molded article comprising the styrene-based resin composition according to any one of the above [1] to [4]. Effect of the Invention
[0008] According to the present invention, it is possible to provide a styrene-based resin composition excellent in light transmittance, heat resistance and appearance, and a molded article using the styrene-based resin composition. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a cross-sectional view of a mold used to manufacture the container of this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The following describes in detail an embodiment of the present invention (hereinafter referred to as the "present embodiment"); however, the present invention is not limited to the following description and can be implemented in various modified forms within the scope of its gist.
[0011] [Styrene-based resin composition] The styrene-based resin composition of the present embodiment contains a styrene-based resin (a) and a cellulose-based polysaccharide (b), and contains 45.0 to 99.5 parts by mass of the styrene-based resin (a) and 0.5 to 55.0 parts by mass of the cellulose-based polysaccharide (b) relative to the total amount (100 parts by mass) of the styrene-based resin (a) and the cellulose-based polysaccharide (b). The refractive index of the styrene-based resin (a) is 1.545 to 1.600, and the MFR of the styrene-based resin (a) is 3 or more. In addition, when the average length of the minor axis of the cellulose-based polysaccharide (b) is d1 and the average length of the major axis of the cellulose is d2, the relationship d1≦d2 is established, and at least one of d1 and d2 is 0.03 to 50 μm.
[0012] <Styrene-based resin (a) (hereinafter also referred to as component (a))> In this embodiment, the content of the styrene-based resin (a) having a refractive index of 1.545 to 1.600 and an MFR of 3 or more is 45.0 to 99.5 parts by mass, preferably 50.0 to 97.0 parts by mass, and more preferably 60.0 to 95.0 parts by mass, relative to the total amount (100 parts by mass) of the styrene-based resin (a) and the cellulose-based polysaccharide (b). By setting the content to 45.0 parts by mass or more, light transmittance and appearance can be improved. On the other hand, by setting the content to 99.5 parts by mass or less, the total content of the cellulose-based polysaccharide (b) can be secured, and rigidity, heat resistance, etc. can be improved.
[0013] The refractive index of the styrene-based resin (a) in the present invention is 1.545 to 1.600, preferably 1.560 to 1.590, and more preferably 1.570 to 1.580. If the refractive index is lower than 1.545 or higher than 1.600, the light transmittance or appearance of the entire styrene-based resin composition is reduced. The refractive index is a value measured at 25°C using an Abbe refractometer. In addition, the MFR (200°C, 5 kg) of the styrene-based resin (a) in the present invention is 3 or more. It is necessary that the MFR is 5 or more, more preferably 8 or more and 30 or less, and further preferably 10 or more and 25 or less. In order to prevent coloration and discoloration of the cellulose (b), melt mixing at 240°C or less is necessary, but if the MFR is lower than 3, the cellulose polysaccharide (b) is difficult to disperse in the styrene resin (a), and diffuse reflection occurs at the interface between the cellulose polysaccharide (b) and the styrene resin (a), resulting in a decrease in light transmittance and appearance. In particular, if the cellulose (b) is in the form of a rod, the styrene resin (a) cannot sufficiently impregnate the bundles of the rod-shaped cellulose polysaccharide (b), causing diffuse reflection at the interface, resulting in a decrease in light transmittance and appearance. On the other hand, if the MFR of the styrene resin (a) is 3 or more, the cellulose polysaccharide (b) is easily impregnated into the aggregates of the cellulose polysaccharide (b), making it easy to disperse the cellulose polysaccharide (b), and it is also impregnated into the unevenness of the interface, resulting in the advantages of improved light transmittance and appearance. Furthermore, in order to improve the adhesion with the cellulose polysaccharide (b) and further prevent diffuse reflection, the styrene resin (a) preferably contains an unsaturated carboxylic acid monomer unit. The content of the unsaturated carboxylic acid monomer unit is preferably 2.0 to 16.0% by mass, more preferably 4 to 14% by mass, and even more preferably 8 to 13% by mass, based on the total amount of the styrene resin (a). The styrene resin to be used may be one type, or a blend of two or more types. In the case of a blend, the refractive index and MFR are the values of the blend. In this specification, the refractive index is a value measured at 25° C. using an Abbe refractometer. In this specification, the MFR is a value measured in accordance with ISO 1133.
[0014] The styrene-based resin (a) that can be used in this embodiment is preferably a polymer having a styrene-based monomer unit, and more preferably a copolymer having a styrene-based monomer unit. The styrene-based resin (a) is more preferably a styrene-based copolymer resin obtained by polymerizing a styrene-based monomer and one or more monomers selected from other vinyl monomers and rubber polymers that are copolymerizable with the styrene-based monomer. The styrene-based resin (a) in the present invention is not particularly limited, and examples thereof include polystyrene, a rubber-modified styrene-based resin in which particles of a rubber-like polymer (A) are dispersed in a matrix, a styrene-based copolymer resin having a styrene-based monomer unit, or a mixture thereof.
[0015] <<polystyrene> In this embodiment, polystyrene is a homopolymer obtained by polymerizing a styrene-based monomer, and generally available ones can be appropriately selected and used. In addition to styrene, the styrene-based monomer constituting polystyrene includes α-methylstyrene, α-methyl-p-methylstyrene, ο-methylstyrene, m-methylstyrene, p-methylstyrene, vinyltoluene, ethylstyrene, isobutylstyrene, and t-butylstyrene, or styrene derivatives such as bromostyrene and indene. Styrene is particularly preferred from an industrial viewpoint. One or more of these styrene-based monomers can be used. Polystyrene typically consists of styrene-based monomer units, although it is not excluded that polystyrene further contains monomer units other than the above-mentioned styrene-based monomer units within a range that does not impair the effects of the present invention.
[0016] <<Rubber-modified styrene resin>> In this embodiment, the rubber-modified styrene-based resin is a resin in which particles of a rubber-like polymer (A) are dispersed in a styrene resin matrix, and can be produced by polymerizing a styrene-based monomer in the presence of the rubber-like polymer (A). Examples of the styrene monomer constituting the rubber-modified styrene resin of the present embodiment include, in addition to styrene, α-methylstyrene, α-methyl p-methylstyrene, ο-methylstyrene, m-methylstyrene, p-methylstyrene, vinyltoluene, ethylstyrene, isobutylstyrene, and t-butylstyrene, or styrene derivatives such as bromostyrene and indene. Styrene is particularly preferred. These styrene monomers can be used alone or in combination.
[0017] The rubber-like polymer (A) contained in the rubber-modified styrene-based resin of this embodiment may, for example, encapsulate a styrene monomer unit-containing resin obtained from the above-mentioned styrene-based monomer on the inside and / or may have a styrene monomer unit-containing resin grafted on the outside.
[0018] As the rubber-like polymer (A), for example, polybutadiene, polybutadiene containing polystyrene, polyisoprene, natural rubber, polychloroprene, styrene-butadiene copolymer, acrylonitrile-butadiene copolymer, etc. can be used, but polybutadiene or styrene-butadiene copolymer is preferred. As the polybutadiene, both high-cis polybutadiene having a high cis content and low-cis polybutadiene having a low cis content can be used. In addition, as the structure of the styrene-butadiene copolymer, both a random structure and a block structure can be used. These rubber-like polymers (A) can be used alone or in combination. In addition, saturated rubber obtained by hydrogenating butadiene rubber can also be used. Examples of such rubber-modified styrene-based resins include HIPS (high impact polystyrene), ABS resin (acrylonitrile-butadiene-styrene copolymer), AAS resin (acrylonitrile-acrylic rubber-styrene copolymer), and AES resin (acrylonitrile-ethylene propylene rubber-styrene copolymer). In addition, when the moldability of the entire styrene-based resin composition is important, it is preferable that the styrene-based resin composition of this embodiment does not substantially contain vinyl cyanide monomer units such as acrylonitrile monomer units, methacrylonitrile monomer units, etc. Specifically, the vinyl cyanide monomer is preferably contained in an amount of 10 mass% or less, more preferably 5 mass% or less, and even more preferably 2 mass% or less, based on the total amount of the styrene-based resin composition.
[0019] In this embodiment, when the rubber-modified styrene-based resin is a HIPS-based resin, the particularly preferred rubber-like polymer (A) is a high-cis polybutadiene having 90 mol % or more of cis-1,4 bonds. In the high-cis polybutadiene, the vinyl 1,2 bonds are preferably 6 mol % or less, and more preferably 3 mol % or less. The content of isomers having a cis-1,4, trans-1,4, or vinyl-1,2 structure as a constituent unit of the high-cis polybutadiene can be measured using an infrared spectrophotometer and calculated by processing the data according to the Morello method. Moreover, the high-cis polybutadiene can be easily obtained by a known production method, for example, by polymerizing 1,3-butadiene using a catalyst containing an organoaluminum compound and a cobalt or nickel compound.
[0020] In this embodiment, the content of the rubber-like polymer (A) contained in the rubber-modified styrene-based resin is preferably 2 to 10 mass %, more preferably 3 to 8 mass %, based on 100 mass % of the rubber-modified styrene-based resin. If the content of the rubber-like polymer (A) is less than 2 mass %, the impact resistance of the styrene-based resin may decrease. If the content of the rubber-like polymer (A) is more than 10 mass %, the light transmittance may decrease. In the present disclosure, the content of the rubber-like polymer (A) contained in the rubber-modified styrene-based resin is a value calculated using pyrolysis gas chromatography.
[0021] In this embodiment, the average particle size of the rubber-like polymer (A) contained in the rubber-modified styrene-based resin is preferably 0.5 to 2.5 μm, and more preferably 0.8 to 2.0 μm, from the viewpoint of light transmittance. In the present disclosure, the average particle size of the rubber-like polymer (A) contained in the rubber-modified styrene-based resin can be measured by the following method. A 75 nm thick ultrathin section is prepared from a rubber-modified styrene-based resin stained with osmium tetroxide, and a photograph is taken at a magnification of 10,000 times using an electron microscope. In the photograph, the black-stained particles are rubber-like polymers. From the photograph, the following formula (N1): Average particle size=ΣniDri 3 / ΣniDri 2 (N1) (In the above formula (N1), ni is the number of rubber polymer (a) particles having a particle diameter Dri, and the particle diameter Dri is the particle diameter calculated as a circle-equivalent diameter from the area of the particle in the photograph.) The area-average particle size is calculated by the above formula, and is regarded as the average particle size of the rubber-like polymer (A). In this measurement, a photograph is scanned at a resolution of 200 dpi, and the measurement is performed using particle analysis software of an image analyzer IP-1000 (manufactured by Asahi Kasei Corporation).
[0022] In this embodiment, the reduced viscosity of the rubber-modified styrene-based resin (which is an index of the molecular weight of the rubber-modified styrene-based resin) is preferably in the range of 0.50 to 0.85 dL / g, more preferably in the range of 0.55 to 0.80 dL / g. If it is less than 0.50 dL / g, there is a risk that the impact strength will decrease, and if it exceeds 0.85 dL / g, there is a risk that the moldability will decrease due to a decrease in fluidity. In this disclosure, the reduced viscosity of the rubber-modified styrene-based resin is a value measured in a toluene solution at 30° C. and a concentration of 0.5 g / dL.
[0023] In this embodiment, the method for producing the rubber-modified styrene-based resin is not particularly limited, but it can be produced by bulk polymerization (or solution polymerization) in which a styrene-based monomer (and a solvent) is polymerized in the presence of the rubber-like polymer (A), or bulk-suspension polymerization in which the reaction is changed to suspension polymerization during the course of the reaction, or emulsion graft polymerization in which a styrene-based monomer is polymerized in the presence of the rubber-like polymer (A) latex. In bulk polymerization, the rubber-like polymer (a) can be produced by continuously supplying a mixed solution containing the rubber-like polymer (a) and the styrene-based monomer, and optionally an organic solvent, an organic peroxide, and / or a chain transfer agent, to a polymerization apparatus consisting of a complete mixing reactor or a tank reactor and a plurality of tank reactors connected in series.
[0024] Styrene-based copolymer resin In this embodiment, the styrene-based copolymer resin is a resin that contains a styrene-based monomer unit, an unsaturated carboxylic acid-based monomer unit, and an unsaturated carboxylic acid ester-based monomer unit. In the styrene-based copolymer resin of the present invention, when the total content of the styrene-based monomer unit, the unsaturated carboxylic acid-based monomer unit, and the unsaturated carboxylic acid ester-based monomer unit is taken as 100 mass%, the content of the styrene-based monomer unit is preferably 69 to 98 mass%, more preferably 74 to 96 mass%, and further preferably in the range of 77 to 92 mass%. By making the content 69 mass% or more, the refractive index of the styrene-based resin (a) can be improved. On the other hand, by making the content 98 mass% or less, it becomes difficult to make the unsaturated carboxylic acid-based monomer unit and the unsaturated carboxylic acid ester-based monomer unit, which is an optional component, present in a desired amount, and it becomes difficult to obtain the effects described below due to these monomer units.
[0025] In the styrene-based copolymer resin of the present embodiment, the unsaturated carboxylic acid-based monomer unit plays a role in improving heat resistance. When the total content of the styrene-based monomer unit, the unsaturated carboxylic acid-based monomer unit, and the unsaturated carboxylic acid ester-based monomer unit in the styrene-based copolymer resin is taken as 100% by mass, the content of the unsaturated carboxylic acid-based monomer unit is preferably 2 to 16% by mass, more preferably 4 to 14% by mass, and even more preferably 8 to 13% by mass. By making the content 2% by mass or more, the dispersibility of cellulose can be improved, and the light transmittance, appearance, and heat resistance can be further improved. On the other hand, by making the content 16% by mass or less, the fluidity and mechanical properties of the resin can be improved.
[0026] Generally, styrene-methacrylic acid-methacrylic acid, which is an example of a styrene-based copolymer resin, is used. Styrene-methacrylic acid-based resins including methyl copolymer resins are mostly produced on an industrial scale by radical polymerization. In the present embodiment, however, in order to suppress the gelling reaction in the devolatilization step, various alcohols can be added to the polymerization system to carry out the polymerization.
[0027] The unsaturated carboxylic acid ester monomer can be used to suppress the dehydration reaction of the unsaturated carboxylic acid monomer through intermolecular interaction with the unsaturated carboxylic acid monomer and to improve the mechanical strength of the resin. Furthermore, the unsaturated carboxylic acid ester monomer also contributes to improving the resin properties such as weather resistance and surface hardness.
[0028] In the styrene copolymer resin of the present embodiment, when the total content of the styrene monomer unit, the unsaturated carboxylic acid monomer unit, and the unsaturated carboxylic acid ester monomer unit is 100% by mass, the content of the unsaturated carboxylic acid ester monomer unit is preferably 0 to 15% by mass, more preferably 1 to 12% by mass, and even more preferably 2 to 10% by mass. By making the content 15% by mass or less, the light transmittance and fluidity of the resin can be improved. In addition, by making the content of the unsaturated carboxylic acid ester monomer unit 0% by mass, the heat resistance can be improved and the cost can be reduced, but from the above viewpoint, the content of the unsaturated carboxylic acid ester monomer unit can also be made to exceed 0% by mass.
[0029] In addition, when an unsaturated carboxylic acid monomer and an unsaturated carboxylic acid ester monomer unit are bonded side by side, if a high-temperature, high-vacuum devolatilizer is used, a dealcoholization reaction may occur under certain conditions, resulting in the formation of a six-membered cyclic acid anhydride. The copolymer resin of this embodiment may contain this six-membered cyclic acid anhydride, but since this reduces the fluidity, it is preferable that the amount of the six-membered cyclic acid anhydride produced is as small as possible.
[0030] In the present embodiment, the contents of the styrene monomer unit (for example, styrene monomer unit), the unsaturated carboxylic acid monomer unit (for example, methacrylic acid monomer unit), and the unsaturated carboxylic acid ester monomer unit (for example, methyl methacrylate monomer unit) in the styrene copolymer resin are respectively measured by proton nuclear magnetic resonance ( 1 It can be calculated from the integral ratio of the spectrum measured by a H-NMR spectrometer.
[0031] In the present embodiment, the styrene-based copolymer resin may further contain monomer units other than the styrene-based monomer unit, the unsaturated carboxylic acid-based monomer unit, and the unsaturated carboxylic acid ester-based monomer unit as an optional component, within a range that does not impair the effects of the present invention. However, the copolymer resin in the present invention is preferably typically composed of a styrene-based monomer unit, an unsaturated carboxylic acid-based monomer unit, and an unsaturated carboxylic acid ester-based monomer unit.
[0032] The styrene-based monomer constituting the styrene-based copolymer resin of the present embodiment is not particularly limited, but examples thereof include styrene, α-methylstyrene, α-methyl-p-methylstyrene, ο-methylstyrene, m-methylstyrene, p-methylstyrene, vinyltoluene, ethylstyrene, isobutylstyrene, t-butylstyrene, bromostyrene, indene and other styrene derivatives. From an industrial viewpoint, styrene is preferred as the styrene-based monomer. These styrene-based monomers can be used alone or in combination of two or more.
[0033] The unsaturated carboxylic acid monomer constituting the styrene copolymer resin of the present embodiment is not particularly limited, but examples thereof include methacrylic acid, acrylic acid, maleic anhydride, maleic acid, fumaric acid, itaconic acid, etc. As the unsaturated carboxylic acid monomer, methacrylic acid is preferred because it has a large effect of improving heat resistance, is liquid at room temperature, and has excellent handleability. These unsaturated carboxylic acid monomers may be used alone or in combination of two or more. It is possible.
[0034] The unsaturated carboxylate monomer constituting the styrene copolymer resin of the present embodiment is not particularly limited, but may be, for example, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, cyclohexyl (meth)acrylate, etc. As the (meth)acrylate monomer, methyl (meth)acrylate is preferred because it has little effect on the decrease in heat resistance. These unsaturated carboxylate monomers may be used alone or in combination of two or more. As the styrene-based copolymer resin of the present embodiment, a styrene-methyl (meth)acrylate copolymer, a styrene-ethyl (meth)acrylate copolymer, a styrene-propane (meth)acrylate copolymer, or a styrene-butyl (meth)acrylate copolymer, a styrene-methyl (meth)acrylate-butyl (meth)acrylate copolymer, or a styrene-methyl (meth)acrylate-methacrylic acid copolymer is preferred.
[0035] In this embodiment, the weight average molecular weight (Mw) of the styrene copolymer resin is preferably 100,000 to 350,000, more preferably 120,000 to 300,000, and further preferably 140,000 to 240,000. When the weight average molecular weight (Mw) is 100,000 to 350,000, a resin having a better balance between mechanical strength and fluidity is obtained, and the amount of gel contamination is small. The weight average molecular weight (Mw) is a value obtained by using gel permeation chromatography and converting it into a standard polystyrene equivalent. As the styrene-based resin (a) of this embodiment, a mixture of one or more of the above rubber-modified styrene-based resins and one or more of the styrene-based copolymer resins may be used. In this case, the mixing ratio of the rubber-modified styrene-based resin and the styrene-based copolymer resin can be appropriately changed depending on the purpose of use. For example, in a system in which the amount of the rubber-modified styrene-based resin is less than that of the styrene-based copolymer resin, it is preferable to contain 0.1 to 30 mass% of the styrene-based copolymer resin with respect to the total amount (100 mass%) of the styrene-based resin (a). On the other hand, in a system in which the amount of the rubber-modified styrene-based resin is more than that of the styrene-based copolymer resin, it is preferable to contain 70 to 99.9 mass% of the styrene-based copolymer resin with respect to the total amount (100 mass%) of the styrene-based resin (a). As the styrene-based resin (a) of this embodiment, a mixture of one or more homopolymers (polystyrene) polymerized from a styrene-based monomer and one or more styrene-based copolymer resins may be used. In this case, the mixing ratio of the homopolymer and the styrene-based copolymer resin can be appropriately changed depending on the purpose of use. For example, in a system in which the amount of the homopolymer is less than that of the styrene-based copolymer resin, it is preferable to contain 0.1 to 30 mass% of the styrene-based copolymer resin relative to the total amount (100 mass%) of the styrene-based resin (a). On the other hand, in a system in which the amount of the homopolymer is more than that of the styrene-based copolymer resin, it is preferable to contain 70 to 99.9 mass% of the styrene-based copolymer resin relative to the total amount (100 mass%) of the styrene-based resin (a). As described above, when a specific amount (about 60% by mass of the entire composition) of a blend of a homopolymer (polystyrene) and a styrene copolymer resin, or a blend of a rubber-modified styrene resin and a styrene copolymer resin is used as the styrene resin (a), the moldability, particularly the spreadability, of the entire composition is improved. In addition, when a specific amount of liquid paraffin is added as an additive, the moldability, particularly the spreadability, of the entire composition is further improved.
[0036] In the present embodiment, the polymerization method for the styrene-based copolymer resin is not particularly limited, but for example, a bulk polymerization method or a solution polymerization method can be suitably adopted as a radical polymerization method. The polymerization method mainly includes a polymerization step of polymerizing the polymerization raw materials (monomer components) and a devolatilization step of removing volatile matters such as unreacted monomers and polymerization solvent from the polymerization product.
[0037] Hereinafter, an example of a polymerization method for the styrene-based copolymer resin that can be used in the present embodiment will be described. When the polymerization raw materials are polymerized to obtain the styrene-based copolymer resin, a polymerization initiator and a chain transfer agent are typically contained in the polymerization raw material composition. Examples of the polymerization initiator used in the polymerization of the styrene-based copolymer resin include organic peroxides, such as peroxyketals such as 2,2-bis(t-butylperoxy)butane, 1,1-bis(t-butylperoxy)cyclohexane, and n-butyl-4,4-bis(t-butylperoxy)valerate, dialkyl peroxides such as di-t-butyl peroxide, t-butylcumyl peroxide, and dicumyl peroxide, diacyl peroxides such as acetyl peroxide and isobutyryl peroxide, peroxydicarbonates such as diisopropyl peroxydicarbonate, peroxyesters such as t-butyl peroxyacetate, ketone peroxides such as acetylacetone peroxide, and hydroperoxides such as t-butyl hydroperoxide. Among them, 1,1-bis(t-butylperoxy)cyclohexane is preferred from the viewpoint of decomposition rate and polymerization rate. Examples of the chain transfer agent used in the polymerization of the styrene-based copolymer resin include α-methylstyrene linear dimer, n-dodecyl mercaptan, t-dodecyl mercaptan, and n-octyl mercaptan.
[0038] As a polymerization method for the styrene-based copolymer resin, solution polymerization using a polymerization solvent can be adopted as necessary. Examples of the polymerization solvent used include aromatic hydrocarbons, such as ethylbenzene, and dialkyl ketones, such as methyl ethyl ketone, and each of them may be used alone or in combination of two or more. Other polymerization solvents, such as aliphatic hydrocarbons, can be further mixed with aromatic hydrocarbons as long as the solubility of the polymerization product is not reduced. These polymerization solvents are preferably used in an amount not exceeding 25 parts by mass relative to 100 parts by mass of the total monomers. If the amount of the polymerization solvent exceeds 25 parts by mass relative to 100 parts by mass of the total monomers, the polymerization rate is significantly reduced and the mechanical strength of the obtained resin tends to be significantly reduced. It is preferable to add the polymerization solvent at a ratio of 5 to 20 parts by mass relative to 100 parts by mass of the total monomers before polymerization, as this makes it easier to uniformize the quality and is also preferable in terms of polymerization temperature control.
[0039] In this embodiment, the apparatus used in the polymerization step for obtaining a styrene-based copolymer resin is not particularly limited, and may be appropriately selected according to the polymerization method of the styrene-based resin. For example, when bulk polymerization is adopted, a polymerization apparatus having one or more completely mixed reactors connected together can be used. There is also no particular limit to the devolatilization step. For example, when bulk polymerization is adopted, polymerization is continued until the unreacted monomer is finally reduced to preferably 50% by mass or less, more preferably 40% by mass or less, and devolatilization is performed by a known method in order to remove volatile matters such as the unreacted monomer. More specifically, for example, a normal devolatilization apparatus such as a flash drum, a twin-screw devolatilizer, a thin film evaporator, or an extruder can be used, but a devolatilization apparatus with a small retention portion is preferred. The temperature of the devolatilization treatment is usually about 190 to 280°C, and from the viewpoint of suppressing the formation of a six-membered cyclic acid anhydride due to the adjacency of methacrylic acid and methyl methacrylate, 190 to 260°C is more preferred. The pressure in the devolatilization treatment is usually about 0.13 to 4.0 kPa, preferably 0.13 to 3.0 kPa, and more preferably 0.13 to 2.0 kPa. Desirable devolatilization methods include, for example, a method of removing volatile matters by reducing pressure under heating, and a method of removing volatile matters through an extruder or the like designed for the purpose of removing volatile matters.
[0040] <Cellulosic polysaccharide (b) (hereinafter also referred to as component (b))> The cellulose polysaccharide (b) in this embodiment has an average minor axis length represented by d1 and an average major axis length represented by d2, and the average major axis length d2 is equal to or greater than the average minor axis length d1, and either the average minor axis length d1 or the average major axis length d2 is The condition that the particle size is within the range of 0.03 to 50 μm is satisfied. The content of the cellulose polysaccharide (b) in the present invention is 5 to 55.0 parts by mass, preferably 10 to 50 parts by mass, and more preferably 15 to 40.0 parts by mass, based on the total amount (100 parts by mass) of the styrene resin (a) and the cellulose polysaccharide (b). By making the content of the (b) component 5 parts by mass or more, the mechanical strength can be improved. On the other hand, if the content is too high, the light transmittance is reduced, and the moldability is significantly reduced due to the reduced fluidity. The content of the cellulose polysaccharide (b) in the composition can be calculated by dissolving the styrene resin composition in a solvent that dissolves the styrene resin (a), removing the undissolved matter, and drying the mixture at 120° C. for 4 hours, as described in the Examples section below.
[0041] In this embodiment, at least one of the average length d1 of the minor axis and the average length d2 of the major axis of the cellulose polysaccharide (b) is 0.03 to 50 μm, preferably 0.05 to 30 μm, preferably 0.1 to 30 μm, and more preferably 0.2 to 20 μm. If the average lengths of the minor axis and the major axis are outside the above range, the light transmittance or rigidity may not be fully exhibited, or the impact resistance and the molded appearance may be deteriorated. On the other hand, if the average lengths of the minor axis and the major axis are within the above range, the aggregation of cellulose can be reduced, and the dispersibility in the styrene-based resin (a) is improved, thereby improving the light transmittance. In addition, in the cellulose polysaccharide (b) of this embodiment, it is preferable that the average length d1 of the minor axis is equal to or less than the average length d2 of the major axis, and the average length d1 of the minor axis is less than the average length d2 of the major axis. In the present invention, the average length d1 of the minor axis of the cellulose polysaccharide (b) is obtained by measuring the minor axis length (minimum length) of 100 cellulose polysaccharides (b) by observation with a transmission electron microscope (magnified 5000 times) and taking the arithmetic average. On the other hand, the average length of the major axis of cellulose is obtained by measuring the major axis length (maximum length) of 100 cellulose polysaccharides (b) by observation with a transmission electron microscope (magnified 5000 times) and taking the arithmetic average. In addition, the average length d1 of the minor axis of the cellulose polysaccharide (b) is obtained by measuring the minor axis length (minimum length) of the cellulose polysaccharide (b) in the same manner as the average length of the major axis. The minor axis length (minimum length) of the cellulose polysaccharide (b) refers to the length of the thinnest (or shortest) point on the image, and the major axis length (maximum length) of the cellulose polysaccharide (b) refers to the length of the longest point on the image. The light transmittance is affected by the shape of the cellulose; in the case of fibers, it is affected by the short axis, while in the case of scale-like or granular cellulose, it is affected by the average diameter of the long axis. The shape of the cellulose polysaccharide (b) in the present invention is not particularly limited, and examples thereof include spherical, irregular, powdery, scaly, fibrous, and rod-like shapes. The aspect ratio (d1 / d2) of the average minor axis length d1 to the average major axis length d2 of the cellulose polysaccharide (b) in the present invention is preferably 1 to 500, more preferably 1.2 to 300, even more preferably 1.5 to 200, and particularly preferably 2 to 100.
[0042] The cellulose polysaccharide (b) in the present invention refers to a polysaccharide having a β-1,4-glucan structure, and includes cellulose and hemicellulose. The material of the cellulose polysaccharide (b) is not particularly limited as long as the fibers constituting the cellulose polysaccharide (b) are formed from polysaccharides having a β-1,4-glucan structure, and examples of the cellulose polysaccharide (b) include natural cellulose fibers (pulps) such as cellulose fibers derived from higher plants [e.g., wood fibers (wood pulp of conifers, broad-leaved trees, etc.), bamboo fibers, sugarcane fibers, seed hair fibers (cotton linters, bombax cotton, kapok, etc.), ginseng bark fibers (e.g., hemp, paper mulberry, mitsumata, etc.), and leaf fibers (e.g., Manila hemp, New Zealand hemp, etc.)]. Cellulose fibers derived from animals (such as sea squirt cellulose), cellulose fibers derived from bacteria, chemically synthesized cellulose fibers (organic acid esters such as cellulose acetate, cellulose propionate, cellulose butyrate, cellulose acetate propionate, cellulose acetate butyrate, etc.; inorganic acid esters such as cellulose nitrate, cellulose sulfate, cellulose phosphate, etc.; mixed acid esters such as cellulose acetate nitrate; hydroxyalkyl cellulose (e.g., hydroxyethyl cellulose (HEC, hydroxypropyl cellulose, etc.); carboxyalkyl cellulose (carboxymethyl cellulose (CMC, carboxyethyl cellulose, etc.); alkyl cellulose (methyl cellulose, ethyl cellulose, etc.); regenerated cellulose (rayon, cellophane, etc.), and other cellulose derivative fibers. These fibers constituting the cellulose polysaccharide (b) may be used alone or in combination of two or more kinds.
[0043] Among the fibers constituting the above-mentioned cellulose polysaccharide (b), preferred are plant-derived cellulose fibers, for example, cellulose fibers derived from pulp such as wood fibers (wood pulp of coniferous trees, broad-leaved trees, bamboo, etc.) and seed hair fibers (cotton linter pulp, etc.), because they have high production efficiency in terms of dispersibility, rigidity, and impact resistance when the cellulose polysaccharide (b) is produced, and have appropriate fiber diameter and length. In this embodiment, the lignin content in 100% by mass of the cellulose polysaccharide (b) is preferably 10% by mass or less, and more preferably 5% by mass or less. If the lignin content is more than 10% by mass relative to the total amount of the cellulose polysaccharide (b), odor and coloring will increase during thermal processing, and the lignin degradation products will turn into charcoal-like black spots, reducing the product value, and in the case of food containers, it will cause holes during microwave heating. Furthermore, in this embodiment, it is preferable that hemicellulose is contained in an amount of 1% by mass or more relative to 100% by mass of the cellulose polysaccharide (b). By containing hemicellulose, dispersibility with the styrene resin (a) is improved, and light transmittance, rigidity, and molded appearance can be improved. In the present invention, it is preferable that these components are not completely removed in the cellulose production process, but are allowed to remain in a content within a suitable range. Hemicellulose is a polysaccharide composed of sugars such as mannan and xylan, and plays a role in connecting microfibrils by hydrogen bonding with cellulose. In addition, since the solubility parameter (SP value) of hemicellulose is on the hydrophobic side compared to cellulose, it is considered that hemicellulose has an effect of reducing the SP value difference between the styrene resin (a) and the cellulose polysaccharide (b). The amount of hemicellulose can be adjusted by reducing it to a desired amount by subjecting a natural wood raw material with a high hemicellulose content to a purification treatment, or when a raw material with a low hemicellulose content is used, the amount can be adjusted to a desired amount by adding hemicellulose obtained by extraction treatment from another raw material. In this case, it does not matter if the structure of the terminals of hemicellulose, etc., is partially different from that of the natural product due to purification or extraction treatment. In this embodiment, for the purpose of reducing the SP value difference between the styrene-based resin (a) and the cellulose-based polysaccharide (b), it is more preferable that hemicellulose is contained in an amount of 1% by mass or more and 25% by mass or less, even more preferable that it is contained in an amount of 2% by mass or more and 20% by mass or less, even more preferable that it is contained in an amount of 3% by mass or more and 20% by mass or less, even more preferable that it is contained in an amount of 5% by mass or more and 19.5% by mass or less, and especially preferable that it is contained in an amount of 7% by mass or more and 19.3% by mass or less, relative to the cellulose-based polysaccharide (b) (100% by mass). The crystallinity of the cellulose polysaccharide (b) in this embodiment is preferably 50 to 100%, more preferably 60 to 90%, and further preferably 70 to 85%. The crystallinity of the cellulose polysaccharide (b) in this specification can be calculated by X-ray diffraction. Specifically, the cellulose polysaccharide (b) or a sample containing the cellulose polysaccharide (b) is placed on a glass cell, and then the crystallinity is measured by the Segal method (see, for example, "L. Segal, JJ Creely, A.E. Martin, Jr., and C.M. Conrad, Text. Res. J., 29, 786 (1959)") using an X-ray diffraction measurement device. In the obtained X-ray diffraction results, the diffraction intensity at 2θ=10° to 30° was set as the baseline, and then the diffraction intensity of the (200) plane at 2θ=22.6° and the diffraction intensity of the amorphous phase at 2θ=18.5° were used to calculate the diffraction intensity using the following formula (1). Crystallinity (%)=[(I (200) -I) / I (200) ]×100 Formula (1) (In the above formula (1), I (200) represents the diffraction intensity of the (200) plane (2θ=22.6°), and I represents the diffraction intensity of the amorphous phase (2θ=18.5°).
[0044] <Dispersant (c) (hereinafter also referred to as component (c))> In this embodiment, for the purpose of improving the dispersibility of cellulose, the dispersant (c) may be contained in an amount of 0.5 to 20 parts by mass, more preferably 0.8 to 17 parts by mass, and even more preferably 0.8 to 11 parts by mass, based on the total amount (100 parts by mass) of the styrene-based resin (a) and the cellulose-based polysaccharide (b). From another perspective, the dispersant (c) may be contained in an amount of 0.5 to 2 parts by mass, more preferably 0.8 to 18 parts by mass, and even more preferably 0.8 to 10 parts by mass, based on the total amount (100 parts by mass) of the styrene-based resin (a) and the cellulose-based polysaccharide (b). By adding the dispersant (c) to the styrene-based resin composition, it is possible to prevent scorching or eye discharge (so-called molten resin residue) of the extruder used when compounding the cellulose fiber (b) and the styrene-based resin (a), and to further improve the molded appearance. If the amount of the dispersant is less than the specified amount, a large effect cannot be expected, and if the amount is more than the specified amount, it is difficult to obtain a large heat resistance. A dispersant having excellent affinity with the styrene-based resin (a) tends to exhibit a greater effect.
[0045] In this embodiment, the dispersant (c) may be a fatty acid ester compound, a polyethylene glycol compound, a terpene compound, a rosin compound, a fatty acid amide, a fatty acid compound, or a fatty acid metal salt compound, etc. In particular, the dispersant (c) is preferably one or more compounds selected from the group consisting of fatty acid ester compounds, polyethylene glycol compounds, terpene compounds, and rosin compounds. Examples of the aliphatic ester compounds include methyl laurate, methyl myristate, methyl palmitate, methyl stearate, methyl oleate, methyl erucate, methyl behenate, butyl laurate, butyl stearate, isopropyl myristate, isopropyl palmitate, octyl palmitate, coconut fatty acid octyl ester, octyl stearate, tallow fatty acid octyl ester, lauryl laurate, stearyl stearate, behenyl behenate, cetyl myristate, esters of linear, unbranched, saturated monocarboxylic acid having 28 to 30 carbon atoms (hereinafter abbreviated as montanic acid) and ethylene glycol, esters of montanic acid and glycerin, ... Examples of such esters include esters of montanic acid and butylene glycol, esters of montanic acid and trimethylolethane, esters of montanic acid and trimethylolpropane, esters of montanic acid and pentaerythritol, glycerin monostearate, sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan monooleate, sorbitan sesquioleate, sorbitan trioleate, polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan monooleate, polyoxyethylene sorbitan trioleate, etc. These may be used alone or in combination of two or more. The polyethylene glycol compound is not particularly limited, and examples thereof include polyethylene glycols, polypropylene glycols, polyethylene glycol alkyl ethers, polypropylene glycol alkyl ethers, polyethylene glycol aryl ethers, polypropylene glycol aryl ethers, polyethylene glycol alkyl aryl ethers, polypropylene glycol alkyl aryl ethers, polyethylene glycol glycerin esters, polypropylene glycol glycerin esters, polyethylene sorbitol esters, polypropylene glycol sorbitol esters, polyethylene glycolized ethylenediamines, polypropylene glycolized ethylenediamines, polyethylene glycolized diethylenetriamines, and polypropylene glycolized diethylenetriamines.
[0046] The terpene resin generally refers to a resin obtained by copolymerizing a terpene monomer alone, or a terpene monomer and an aromatic monomer, or a terpene monomer and a phenol in an organic solvent in the presence of a Friedel-Crafts catalyst, but is not limited thereto. Examples of the monomer include, but are not limited to, hemiterpenes having 5 carbon atoms such as isoprene, α-pinene, β-pinene, dipentene, d-limonene, myrcene, alloocimene, ocimene, α-phellandrene, α-terpinene, γ-terpinene, terpinolene, 1,8-cineole, 1,4-cineole, α-terpineol, β-terpineol, γ-terpineol, sabinene, paramentadienes, and carenes, monoterpenes having 10 carbon atoms such as caryophyllene and longifolene, and diterpenes having 20 carbon atoms. Among these compounds, α-pinene, β-pinene, dipentene, and d-limonene are particularly preferably used. Examples of the aromatic monomer include, but are not limited to, styrene, α-methylstyrene, vinyltoluene, and isopropenyltoluene. Examples of the phenols include, but are not limited to, phenol, cresol, xylenol, bisphenol A, and the like. Also, the terpene resin may be a hydrogenated terpene resin obtained by subjecting the obtained terpene resin to a hydrogenation treatment. For example, preferred terpene resins include α-pinene resin, β-pinene resin, aromatic modified terpene resin, terpene phenol resin, and hydrogenated terpene resin. The terpene resin may be used alone or in combination of two or more kinds.
[0047] Examples of the rosin-based resin include rosins such as gum rosin, wood rosin, and tall oil rosin, as well as stabilized rosins obtained by disproportionating or hydrogenating the rosins, polymerized rosins (typically dimers) which are polymers of the rosins, and modified rosins modified with unsaturated acids such as maleic acid, fumaric acid, and (meth)acrylic acid. Examples of the rosin derivative resin include esters of the rosin-based resins, phenol-modified products, and esters thereof. The rosin-based resins may be used alone or in combination of two or more kinds. The rosin-based resins or rosin derivative resins used in the present invention are not limited to these resins.
[0048] Examples of the aliphatic amide include stearic acid amide, oleic acid amide, erucic acid amide, behenic acid amide, ethylene bisstearic acid amide, ethylene bisoleic acid amide, ethylene biserucic acid amide, ethylene bislauric acid amide, etc. These may be used alone or in combination of two or more.
[0049] Specific examples of saturated fatty acids among the above fatty acid compounds include lauric acid (dodecanoic acid), isodecanoic acid, tridecanoic acid, myristic acid (tetradecanoic acid), pentadecylic acid, palmitic acid (hexadecanoic acid), margaric acid (heptadecanoic acid), stearic acid (octadecanoic acid), isostearic acid, tuberculostearic acid (nonadecanoic acid), 2-hydroxystearic acid, arachidic acid (icosanoic acid), behenic acid (docosanoic acid), lignoceric acid (tetradocosanoic acid), cerotic acid (hexadocosanoic acid), montanic acid (octadocosanoic acid), and melissic acid, and in particular, lauric acid, palmitic acid, stearic acid, behenic acid, 12-hydroxystearic acid, and montanic acid. These may be used alone or in combination of two or more.
[0050] Specific examples of unsaturated fatty acids among the above fatty acid compounds include myristoleic acid (tetradecenoic acid), palmitoleic acid (hexadecenoic acid), oleic acid (cis-9-octadecenoic acid), elaidic acid (trans-9-octadecenoic acid), ricinoleic acid (octadecadienoic acid), vaccenic acid (cis-11-octadecenoic acid), linoleic acid (octadecadienoic acid), linolenic acid (9,11,13-octadecatrienoic acid), elestearic acid (9,11,13-octadecatrienoic acid), gadoleic acid (icosanoic acid), erucic acid (docosanoic acid), nervonic acid (tetradocosanoic acid), etc. These may be used alone or in combination of two or more.
[0051] Examples of the fatty acid metal salt include lithium salts, calcium salts, magnesium salts, zinc salts, and aluminum salts of the fatty acids of the above fatty acid compounds. These may be used alone or in combination of two or more.
[0052] <Optional addition ingredients> In addition to the above components (a) to (c), the styrene-based resin composition of the present embodiment may contain known additives, processing aids, and other additive components as necessary within the range that does not impair the effects of the present invention. Examples of such additives and processing aids include antioxidants, weathering agents, antistatic agents, fillers, and liquid paraffin.
[0053] Examples of the antioxidant include phenol-based compounds, phosphorus-based compounds, and thioether-based compounds. Examples of the phenol-based antioxidant include 2,6-di-tert-butyl-p-cresol, 2,6-diphenyl-4-octadecyloxyphenol, distearyl (3,5-di-tert-butyl-4-hydroxybenzyl)phosphonate, 1,6-hexamethylenebis[(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid amide], 4,4'-thiobis(6-tert-butyl-m-cresol), 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 2,2'-methylene Bis(4-ethyl-6-tert-butylphenol), 4,4'-butylidenebis(6-tert-butyl-m-cresol), 2,2'-ethylidenebis(4,6-di-tert-butylphenol), 2,2'-ethylidenebis(4-sec-butyl-6-tert-butylphenol), 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 1,3,5-tris(2,6-dimethyl-3-hydroxy-4-tert-butylbenzyl)isocyanurate, 1,3,5-tris(3 ,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate, 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-2,4,6-trimethylbenzene, 2-tert-butyl-4-methyl-6-(2-acryloyloxy-3-tert-butyl-5-methylbenzyl)phenol, stearyl [3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], tetrakis [3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate methyl ]methane, thiodiethylene glycol bis[(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 1,6-hexamethylene bis[(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], bis[3,3-bis(4-hydroxy-3-tert-butylphenyl)butyric acid]glycol ester, bis[2-tert-butyl-4-methyl-6-(2-hydroxy-3-tert-butyl-5-methylbenzyl)phenyl]terephthalate, 1,3,5-tris[(3,5-di-tert-butyl-4-hydroxyphenyl)propionyloxyethyl]isocyanurate, 3,9-bis[1,1-dimethyl-2-{(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy}ethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane, triethylene glycol bis[(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate], etc. These may be used alone or in combination of two or more.
[0054] Examples of the phosphorus-based antioxidant include tris(2,4-di-tert-butylphenyl)phosphite, trisnonylphenyl phosphite, tris[2-tert-butyl-4-(3-tert-butyl-4-hydroxy-5-methylphenylthio)-5-methylphenyl]phosphite, tridecyl phosphite, octyldiphenyl phosphite, di(decyl)monophenyl phosphite, di(tridecyl)pentaerythritol diphosphite, di(nonylphenyl)pentaerythritol diphosphite, bis(2,4-tert-butylphenyl)pentaerythritol diphosphite, bis(2,6- di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, bis(2,4,6-tri-tert-butylphenyl)pentaerythritol diphosphite, bis(2,4-dicumylphenyl)pentaerythritol diphosphite, tetra(tridecyl)isopropylidenediphenol diphosphite, tetra(tridecyl)-4,4'-n-butylidenebis(2-tert-butyl-5-methylphenol)diphosphite, hexa(tridecyl)-1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane triphosphite, tetrakis(2,4-di-tert-butylphenyl)biphenylene diphosphonite, 9 ,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 2,2'-methylenebis(4,6-tert-butylphenyl)-2-ethylhexyl phosphite, 2,2'-methylenebis(4,6-tert-butylphenyl)-octadecyl phosphite, 2,2'-ethylidenebis(4,6-di-tert-butylphenyl)fluorophosphite, tris(2-[(2,4,8,10-tetrakis-tert-butyldibenzo[d,f][1,3,2]dioxaphosphepin-6-yl)oxy]ethyl)amine, phosphite of 2-ethyl-2-butylpropylene glycol and 2,4,6-tri-tert-butylphenol, etc. These may be used alone or in combination of two or more.
[0055] Examples of the thioether-based antioxidant include dialkyl thiodipropionates such as dilauryl thiodipropionate, dimyristyl thiodipropionate, and distearyl thiodipropionate, and pentaerythritol tetra(β-alkylmercaptopropionate)s. These may be used alone or in combination of two or more.
[0056] As the weathering agent, an ultraviolet absorbing agent, a hindered amine light stabilizer, etc., can be used. As the ultraviolet absorbing agent, for example, 2-hydroxybenzophenones such as 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-octoxybenzophenone, and 5,5'-methylenebis(2-hydroxy-4-methoxybenzophenone); 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-5' 2-(2'-hydroxyphenyl)benzotriazoles such as 2,2'-methylenebis(4-tert-octyl-6-(benzotriazolyl)phenol), 2-(2'-hydroxy-3'-tert-butyl-5'-carboxyphenyl)benzotriazole; phenyl salicylate, resorcinol monobenzoate, 2,4-di-tert-butylphenyl-3,5-di-tert-butyl-4-hydroxybenzoate, 2,4-di-tert-amylphenyl-3,5-di-tert-butyl-4-hydroxybenzoate, hexadecyl-3,5-di-tert-butyl-4-hydroxybenzoate, Benzoates such as 2-ethyl-2'-ethoxyoxanilide, 2-ethoxy-4'-dodecyloxanilide, and other substituted oxanilides; cyanoacrylates such as ethyl-α-cyano-β,β-diphenylacrylate, methyl-2-cyano-3-methyl-3-(p-methoxyphenyl)acrylate, and other cyanoacrylates; triaryltriazines such as 2-(2-hydroxy-4-octoxyphenyl)-4,6-bis(2,4-di-tert-butylphenyl)-s-triazine, 2-(2-hydroxy-4-methoxyphenyl)-4,6-diphenyl-s-triazine, 2-(2-hydroxy-4-propoxy-5-methylphenyl)-4,6-bis(2,4-di-tert-butylphenyl)-s-triazine, and other triaryltriazines. These may be used alone or in combination of two or more.
[0057] Examples of the hindered amine-based light stabilizer include 2,2,6,6-tetramethyl-4-piperidyl stearate, 1,2,2,6,6-pentamethyl-4-piperidyl stearate, 2,2,6,6-tetramethyl-4-piperidyl benzoate, bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate, bis(1,2,2,6,6-tetramethyl-4-piperidyl)sebacate, bis(1-octoxy-2,2,6,6-tetramethyl-4-piperidyl)sebacate, tetrakis(2,2,6,6-tetramethyl-4-piperidyl)-1 ,2,3,4-butane tetracarboxylate, tetrakis(1,2,2,6,6-pentamethyl-4-piperidyl)-1,2,3,4-butane tetracarboxylate, bis(2,2,6,6-tetramethyl-4-piperidyl)·di(tridecyl)-1,2,3,4-butane tetracarboxylate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)·di(tridecyl)-1,2,3,4-butane tetracarboxylate, bis(1,2,2,4,4-pentamethyl-4-piperidyl)-2-butyl-2-(3,5-ditert-butyl-4-hydro 1,6-bis(2,2,6,6-tetramethyl-4-piperidylamino)hexane / 2,4-dichloro-6-morpholino-s-triazine polycondensate, 1,6-bis(2,2,6,6-tetramethyl-4-piperidylamino)hexane / 2,4-dichloro-6-tert-octylamino-s-triazine polycondensate, 1,5,8,12-tetrakis[2,4-bis(N-butyl-N-(2,2,6,6-tetramethyl -4-piperidyl)amino)-s-triazin-6-yl]-1,5,8,12-tetraazadodecane, 1,5,8,12-tetrakis[2,4-bis(N-butyl-N-(1,2,2,6,6-pentamethyl-4-piperidyl)amino)-s-triazin-6-yl]-1,5,8-12-tetraazadodecane, 1,6,11-tris[2,4-bis(N-butyl-N-(2,2,6,6-tetramethyl-4-piperidyl)amino)-s-triazin-6-yl]aminoundecane, 1,6,11-tris[2,4-bis(N-butyl-N-(1,2,2,Examples of the hindered amine compounds include 6,6-pentamethyl-4-piperidyl)amino)-s-triazin-6-yl)aminoundecane. These may be used alone or in combination of two or more.
[0058] As the antistatic agent, cationic, anionic, nonionic, amphoteric, fatty acid partial esters such as glycerin fatty acid monoesters, and the like can be used. Specifically, alkyl trimethyl ammonium salts, dialkyl dimethyl ammonium salts, benzalkonium salts, N,N-bis(2-hydroxyethyl)-N-(3-dodecyloxy-2-hydroxypropyl)methyl ammonium methosulfate, (3-lauryl amidopropyl)trimethyl ammonium methyl sulfate, stearamidopropyl dimethyl-2-hydroxyethyl ammonium nitrate, stearamidopropyl dimethyl-2-hydroxyethyl ammonium phosphate, cationic polymers, alkyl sulfonates, alkyl benzene sulfonates, sodium alkyl diphenyl ether disulfonate, alkyl nitrate ester salts, phosphorus Examples of such esters include alkyl ester salts, alkyl phosphate amine salts, stearic acid monoglyceride, pentaerythritol fatty acid esters, sorbitan monopalmitate, sorbitan monostearate, diglycerol fatty acid esters, alkyldiethanolamines, alkyldiethanolamine fatty acid monoesters, alkyldiethanolamides, polyoxyethylene dodecyl ethers, polyoxyethylene alkylphenyl ethers, polyethylene glycol monolaurates, polyoxyethylene alkylamines, polyoxyethylene alkylamides, polyether block copolymers, cetyl betaine, and hydroxyethyl imidazoline sulfate esters. These may be used alone or in combination of two or more.
[0059] As the filler, talc, calcium carbonate, barium sulfate, carbon fiber, mica, wollastonite, whisker, etc. can be used. In addition, anti-blocking agents, colorants, anti-blooming agents, surface treatment agents, antibacterial agents, anti-eye discharge agents (anti-eye discharge agents such as silicone oil described in JP 2009-120717 A, monoamide compounds of higher aliphatic carboxylic acids, and monoester compounds obtained by reacting higher aliphatic carboxylic acids with monohydric to trihydric alcohol compounds) may be added. The liquid paraffin is also called mineral oil, and is an oligomer and polymer containing paraffinic hydrocarbons. The liquid paraffin includes paraffinic oil, naphthenic oil, and paraffin wax, and is a mixture of paraffinic hydrocarbons and alkylnaphthenic hydrocarbons. It includes those having a specific gravity of 0.8494 or less at 15°C and those having a specific gravity of more than 0.8494 at 15°C. The naphthene content of the liquid paraffin is preferably 15% by mass or more and 55% by mass or less, more preferably 20% by mass or more and 45% by mass or less, and even more preferably 19% by mass or more and 35% by mass or less, based on 100% by mass of the liquid paraffin. The content of the liquid paraffin is preferably 0.07 parts by mass or more and 5 parts by mass or less, and more preferably 0.15 parts by mass or more and 2.8 parts by mass or less, relative to the total amount (100 parts by mass) of the styrene-based resin (a) and the cellulose-based polysaccharide (b).
[0060] The total content of optional components such as additives and processing aids may be 0.05 to 5% by mass in the styrene-based resin composition.
[0061] The styrene-based resin composition of the present embodiment may consist essentially of only the components (a) to (c) and any optional additional components, or may consist of only the components (a) to (c), or only the components (a) to (c) and any optional additional components. The phrase "consisting essentially of only the components (a), (b), and (c) and any optional additional components" means that 95 to 100 mass% (preferably 98 to 100 mass%) of the styrene-based resin composition is made up of the components (a), (b), and (c) or the components (a), (b), and (c) and any optional additional components. The styrene-based resin composition of the present embodiment may contain inevitable impurities in addition to the components (a) to (c) and any optional additional components, as long as the effects of the present invention are not impaired.
[0062] [Physical properties of styrene-based resin composition] <Light transparency> The light transmittance of the molded article obtained from the styrene-based resin composition of this embodiment is preferably 60% or more, more preferably 70% or less, in terms of total light transmittance at a thickness of 1 mm. If it is less than 60%, light is less likely to pass through, resulting in poor visibility and design. In this disclosure, the light transmittance is a value measured in accordance with the measurement method for total light transmittance of JIS K7361.
[0063] <Heat shrinkage rate> The heat shrinkage rate of a molded article obtained from the styrene-based resin composition of the present embodiment is preferably 20% or less, more preferably 10% or less, in an atmosphere at 120° C. for 30 minutes. If it exceeds 20%, there is a risk that the product will deform.
[0064] <Spreadability> The malleability of the styrene-based resin composition of this embodiment refers to the ratio of the thickness of the bottom sidewall / the thickness of the upper sidewall of a container when the container is formed with a predetermined drawing ratio. It is preferable that a container with a drawing ratio of 0.5 or more is obtained by vacuum forming a sheet body, which is a molded product formed from the styrene-based resin composition of this embodiment. In this embodiment, the malleability is preferably such that the ratio of the thickness of the bottom sidewall / the thickness of the upper sidewall is 1 to 0.3 after vacuum forming a container with a drawing ratio of 0.5. As an example of the molded article of this embodiment, molding of a container will be described with reference to Fig. 1. Fig. 1 is a cross-sectional view of a mold 1 required for molding a container. Fig. 1 also shows, as an example, a state in which a spacer 2 with a height of 80 cm is placed on the bottom of the mold 1. The height of the spacer 2 can be appropriately adjusted depending on the desired height of the container. For example, the container of this embodiment can be produced according to the following procedures (I) and (II). (I) A styrene-based resin composition prepared according to a predetermined composition is extruded to produce a sheet of the styrene-based resin composition. (II) After that, the obtained sheet of the styrene-based resin composition is preheated at 150 to 250°C for 5 to 60 seconds, and then the heated sheet is placed so as to cover the recess of the mold 1 (i.e., so as to cover the opening), and shaped by a predetermined molding method. For example, the inside of the recess can be evacuated to form a container of a desired shape. Alternatively, a sheet may be placed so as to cover the recess of the mold 1, and then heated and shaped by a predetermined molding method (for example, thermocompression molding, vacuum molding, pressure molding, plug-assist molding). As an example of a preferred aspect of this embodiment, the container can be shaped by subjecting a sheet of a heated styrene-based resin composition to thermocompression molding, vacuum molding, pressure molding, or plug-assisted molding using a mold 1. Furthermore, when manufacturing a container, the spacer 2 can be used to change the drawing ratio, which is the ratio between the diameter of the upper surface of the recess in the mold 1 (= the diameter of the opening (φ80 cm as an example in Figure 1)) and the depth of the recess in the mold 1 (40 cm as an example in Figure 1). As an example, Figure 1 shows a state in which a spacer 2 with a height of 80 cm is provided in a recess with a depth of 120 cm. The drawing ratio is expressed by the following mathematical formula (2). Squeeze ratio = container height ÷ container opening diameter Formula (2)
[0065] [Method of producing styrene-based resin composition] The styrene-based resin composition of the present embodiment can be produced by melt-kneading each component by any method. For example, a high-speed stirrer such as a Henschel mixer, a batch-type kneader such as a Banbury mixer, a single-screw or twin-screw continuous kneader, a roll mixer, etc. can be used alone or in combination. The heating temperature during kneading is usually selected in the range of 180 to 250°C.
[0066] [Molded products] The molded article of the present invention is characterized by containing the above-mentioned styrene-based resin composition. The styrene-based resin composition of the present embodiment can be used to produce a molded article by the above-mentioned melt kneading molding machine, or by using pellets of the obtained styrene-based resin composition as a raw material, through injection molding, injection compression molding, extrusion molding, blow molding, press molding, vacuum molding, foam molding, or the like.
[0067] A molded article, preferably an injection molded article (including injection compression) containing the styrene-based resin composition of the present embodiment is suitably used for office automation equipment such as copiers, fax machines, personal computers, printers, information terminals, refrigerators, vacuum cleaners, and microwave ovens, home appliances, housings and various parts of electric and electronic equipment, interior and exterior materials for automobiles, construction materials, foam insulation materials, insulating films, and the like. EXAMPLES
[0068] Hereinafter, the embodiments of the present invention will be described in more detail based on examples and comparative examples, but the present invention is not limited to these examples in any way.
[0069] <Measurement and evaluation methods> The physical properties of the resin compositions obtained in each of the Examples and Comparative Examples were measured and evaluated according to the following methods. (1) Contents of styrene monomer units, methacrylic acid monomer units, and methyl methacrylate monomer units in styrene-based resin (a) Proton nuclear magnetic resonance ( 1 The resin composition was quantified from the integral ratio of the spectrum measured by a 1 H-NMR measuring device. Sample preparation: 30 mg of resin pellets were dissolved in 0.75 mL of d6-DMSO and incubated at 60°C for 4-6 h. The mixture was heated for 1 hour to dissolve. ·Measuring equipment: JNM ECA-500 manufactured by JEOL Ltd. Measurement conditions: Measurement temperature 25℃, observation nucleus 1 H, accumulation count 64, repeat time 11 seconds.
[0070] (Spectral assignment) Regarding the assignment of the spectrum measured in dimethyl sulfoxide deuterated solvent, the peaks at 0.5 to 1.5 ppm are peaks derived from hydrogen of α-methyl group of methacrylic acid, methyl methacrylate, and six-membered cyclic acid anhydride, the peaks at 1.6 to 2.1 ppm are peaks derived from hydrogen of methylene group of polymer main chain, the peak at 3.5 ppm is peak derived from hydrogen of carboxylate ester (-COOCH3) of methyl methacrylate, and the peak at 12.4 ppm is peak derived from hydrogen of carboxylate of methacrylic acid. In addition, the peaks at 6.5 to 7.5 ppm are peaks derived from hydrogen of aromatic ring of styrene. Note that the content of six-membered cyclic acid anhydride is small in the resins of the present embodiment and the comparative example, so that quantification is usually difficult by this measurement method.
[0071] (2) Weight average molecular weight of styrene-based resin (a) The weight average molecular weight of the styrene-based resin (a) was measured under the following conditions and procedures. Sample preparation: Resin was dissolved in tetrahydrofuran at approximately 0.05% by mass. Measurement conditions Equipment: TOSOH HLC-8220GPC (Gel Permeation Chromatography) Column: super HZM-H Temperature: 40℃ Carrier: THF 0.35mL / min Detector: RI, UV: 254 nm Calibration curve: Created using standard PS manufactured by TOSOH.
[0072] (3) Melt flow rate (MFR) The melt mass flow rate (g / 10 min) of the styrene-based resin (a) was measured in accordance with ISO 1133 (200° C., load 49 N).
[0073] (4) Refractive index The refractive index was measured at 25° C. using an Abbe refractometer.
[0074] (5) Total light transmittance The total light transmittance (%) was measured in accordance with JIS K7361 using a test piece (b) prepared by the method described below.
[0075] (6) Heat shrinkage rate The heat shrinkage rate (%) was determined by using a test piece (a) prepared by the method described below, leaving it in an oven at 120° C. for 30 minutes, measuring the size in the longitudinal direction, and then determining the shrinkage rate.
[0076] (7) Surface appearance The surface appearance was evaluated by observing one surface of the test piece (b) prepared by the method described below. If there were less than 20 dents with an opening of 0.1 mm or more, the surface appearance was evaluated as "passed: ○", and if there were 20 or more dents, the surface appearance was evaluated as "poor: ×".
[0077] (8) Spreadability Using a method described later, a pellet-shaped styrene-based resin composition was used as a raw material, and a container with a drawing ratio of 0.5 was vacuum-formed using mold 1 in FIG. 1. The thickness of the container at each point was confirmed, and the ductility was evaluated according to the following criteria. Evaluation criteria: good quality (ratio of bottom sidewall thickness / upper sidewall thickness is 1 to 0.3), uneven thickness (ratio of bottom sidewall thickness / upper sidewall thickness is less than 0.3), and holes (×). The drawing ratio is expressed by the following formula (2). Squeeze ratio = container height (40 cm) ÷ container opening diameter (80 cm) Formula (2)
[0078] (9) Measurement of average length A 75 nm thick ultrathin section was prepared from the test piece (b), and a 50,000x magnification was taken using an electron microscope. The photograph was then scanned at a resolution of 200 dpi, and the minimum and maximum lengths of 100 cellulose polysaccharides (b) were measured using particle analysis software of an image analyzer IP-1000 (manufactured by Asahi Kasei Corporation), and the arithmetic averages were taken as the average minor axis length d1 and the average major axis length d2. Similarly to the above, a photograph of the cellulose polysaccharide (b) alone was taken at a magnification of 50,000x using an electron microscope, and the arithmetic averages were taken as the average minor axis length d1 and the average major axis length d2.
[0079] (10) Measurement of hemicellulose content Quantitative analysis of hemicellulose in cellulosic polysaccharide (b) is as follows. The dispersion medium was removed from the dispersion of cellulose polysaccharide (b) or from a redispersion of cellulose polysaccharide (b) obtained by dissolving and removing the resin component from a styrene-based resin composition, and the cellulose residue was recovered and dried at 105°C to obtain a dry sample, and the mass of the dry sample was measured by the following method. The dried cellulose residue was ground to obtain a ground sample, which was extracted with an alcohol (ethanol) / benzene mixed solvent in a Soxhlet extractor for 6 hours. Then, extraction was performed for another 4 hours with an alcohol (ethanol) / benzene mixed solvent to obtain a defatted sample. 150 mL of distilled water, 1.0 g of sodium chlorite, and 0.2 mL of acetic acid were added to 2.5 g of the defatted sample, and the mixture was heated at 70-80°C for 1 hour. Then, 1.0 g of sodium chlorite and 0.2 mL of acetic acid were added again, and the mixture was heated at 70-80°C for 1 hour. This operation was repeated 3-4 times until the sample was decolorized to white. The obtained sample was filtered, washed with water and acetone, and dried at 105°C to obtain a holocellulose fraction (the total amount of α-cellulose and hemicellulose). The mass of this holocellulose fraction was measured. Next, 25 mL of 17.5% by mass sodium hydroxide aqueous solution was added to 1.0 g of the holocellulose fraction, and after 3 minutes, the mixture was lightly crushed with a glass rod until it became swollen. After that, the mixture was left to stand at 20°C, and 30 minutes after the addition of the sodium hydroxide aqueous solution, 25 mL of distilled water was added, stirred for exactly 1 minute, left to stand at 20°C for 5 minutes, filtered through a glass filter, and washed until the filtrate became neutral. Further, 40 mL of 10% by mass acetic acid was suction filtered, and then 1 L of boiling water was suction filtered and the washed sample was dried at 105°C until the mass became constant, to obtain an α-cellulose fraction. The mass of this α-cellulose fraction was measured. The hemicellulose content was calculated from the masses of the holocellulose fraction and the α-cellulose fraction obtained as described above using the following formula. Holocellulose (%) = holocellulose fraction (g) / sample (anhydrous basis) (g) × 100 α-cellulose (%) = α-cellulose fraction (g) / sample (anhydrous basis) (g) × 100 Hemicellulose (%) = holocellulose (%) - (α-cellulose (%))
[0080] The materials used in the examples and comparative examples are as follows. [Styrene-based resin (a)] [GPPS-1] Polystyrene with MFR 7.8 and refractive index 1.598 (GPPS, PS Japan, HF77) was used. [GPPS-2] Polystyrene with MFR 2.2 and refractive index 1.598 (GPPS, PS Japan, G9401) was used. [HIPS-1] Polystyrene with MFR 3.0 and refractive index 1.558 (HIPS, PS Japan, HT478) was used. [HIPS-2] Polystyrene with MFR 2.0 and refractive index 1.565 (HIPS, PS Japan, 475D) was used. [Copolymerization-1] A polymerization raw material liquid consisting of 70.0 parts by mass of styrene (ST), 15.0 parts by mass of butyl methacrylate (BA), 15.0 parts by mass of ethylbenzene, and 0.025 parts by mass of 1,1-bis(t-butylperoxy)cyclohexane was continuously fed at a rate of 1.1 L / hour to a 4-liter complete mixing reactor, then to a polymerization apparatus consisting of a 2-liter laminar flow reactor, and further to a devolatilizer connected to a single-screw extruder for removing volatile matters such as unreacted monomers and polymerization solvent, to prepare a styrene-based copolymer resin, Copolymer-1. The polymerization reaction conditions in the polymerization step were a polymerization temperature of 122° C. in the complete mixing reactor and a polymerization temperature of 120 to 142° C. in the laminar flow reactor. The devolatilized unreacted gas was condensed in a condenser through which a coolant of −5° C. was passed, and recovered as an unreacted liquid. The polymer content in the final polymerization solution was measured after drying the polymerization solution at 215°C under a reduced pressure of 2.5 kPa for 30 minutes according to the formula [(mass of sample after drying / mass of sample before drying)×100%], and was found to be 65.6% by mass, with an MFR of 4.6 and a refractive index of 1.578. [Copolymerization-2] Manufactured in the same manner as [Copolymer-1], except that styrene (ST) was changed to 45.0 parts by mass and methyl methacrylate (MA) to 40.0 parts by mass. The MFR was 3.2 and the refractive index was 1.542. [Blend-1] A mixture of the above HIPS-2 (475D) and 5% by mass of SMA copolymer (XIBOND250, manufactured by POLYSCOPE) [HIPS-2 (95% by mass), SMA copolymer (5% by mass)], with an MFR of 3.2 and a refractive index of 1.572. [Blend-2] A mixture of copolymer-1 and 5% by mass of SMA copolymer (XIBOND250, manufactured by POLYSCOPE) [copolymer-1 (95% by mass), SMA copolymer (5% by mass)], with MFR of 5.0 and refractive index of 1.584. [Blend-3] A mixture of the above GPPS-1 (HF77) and the above copolymer-1 at 10% by mass [GPPS-1 (90% by mass), copolymer-1 (10% by mass)], with an MFR of 7.2 and a refractive index of 1.59.
[0081] [Cellulosic polysaccharides (b)] Cellulose fiber-1 (Celite, SW-10, d1: 20 μm, d2: 700 μm, hemicellulose content 11% by mass, lignin content 0.5% by mass, crystallinity 80%) Cellulose fiber-2 (Celite, SW-30, d1: 60 μm, d2: 700 μm, hemicellulose content 15% by mass, lignin content 0.5% by mass, crystallinity 80%) CNF: Cellulose nanofiber (manufactured by Chuetsu Pulp Industry Co., Ltd., CNF-10, d1: 35 nm, d2: approx. 1 μm, hemicellulose content 15% by mass, lignin content 0.2% by mass, crystallinity 75%) Cotton powder (manufactured by DTI Corporation, 100% cotton pulverized product, spherical body, d1: 25 μm, d2: 35 μm, hemicellulose content 0.5% or less by mass, lignin content 0.1% by mass, crystallinity 90%) Hemicellulose (Wako Pure Chemical Industries, xylan) Wood flour (made by Naka Wood Co., Ltd., raw material: cedar, d1: 40 μm, d2: 300 μm, hemi Cellulose content 18% by mass, lignin content 18% by mass, crystallinity 55%) (The above lignin content indicates the ratio to the total amount of each cellulosic polysaccharide (b).)
[0082] [Dispersant] Fatty acid ester: Glycerol monostearate (Riken Vitamin Co., Ltd.: S-100) Terpene: Aromatic modified terpene resin (Yasuhara Chemical Co., Ltd.: YS Resin TO-105)
[0083] [Additives] (Phenol-based antioxidant) 3-(3,5-di-tert-butyl-4-hydroxyphenyl)stearyl propionate (BASF, Irganox 1076) (Phosphorus-based antioxidant) Tris(2,4-di-tert-butylphenyl)phosphite (BASF, Irgafos168) (liquid paraffin) Liquid paraffin (Idemitsu Kosan CP-68N)
[0084] [Examples 1 to 17] Each component was added in the composition ratio shown in Table 1-1 and Table 1-2, and 0.2 parts by mass of Irganox1076 and Irgafos168 were added as antioxidants to a total of 100 parts by mass of components (a) and (b), and then premixed. The obtained premixes were mixed together and melt-extruded at 180°C to 220°C using a twin-screw extruder (Toshiba Machine Co., Ltd., TEM-26SS) to obtain pellets of a styrene-based resin composition as a kneaded product. At this time, the screw rotation speed was 150 rpm and the discharge rate was 10 kg / hr. The pellets thus obtained were molded using an injection molding machine manufactured by Japan Steel Works Co., Ltd. equipped with an ISO standard test piece type (a) mold at a cylinder temperature of 220°C, a mold temperature of 50°C, an injection pressure (gauge pressure 40-60 MPa), an injection speed (panel setting value) of 50%, and an injection time / cooling time = 5 sec / 20 sec to prepare a test piece (a). The heat shrinkage rate was evaluated using the obtained test piece (a). Similarly, a test piece (b) was prepared by molding under the same conditions as above using an injection molding machine manufactured by Japan Steel Works, Ltd., equipped with a mold (b) measuring 50 x 120 mm and 1 mm thick. The test piece (b) was then used to measure the total light transmittance and evaluate the appearance of the molded product. The evaluation results are shown in Tables 1-1 and 1-2. Further, a non-foamed extruded sheet was produced using the obtained pellet-like styrene resin composition. For the non-foamed extruded sheet, a 25 mmφ single-screw sheet extruder manufactured by Soken Co., Ltd. was used to produce a sheet having a thickness of about 0.8 mm at a resin melting zone temperature of 180 to 200°C. Then, a container was produced using the obtained sheet. For the container, a sheet container molding machine manufactured by Soken Co., Ltd. was used to vacuum mold a container with a drawing ratio of 50% at a heating zone of 200°C, and the ductility was evaluated. The results are shown in Table 1-1 and Table 1-2.
[0085] [Table 1-1]
[0086] [Table 1-2]
[0087] [Comparative Examples 1 to 5] Comparative Examples 1 to 5 were carried out in the same manner as Example 1, except that the compositions were changed as shown in Table 2. Table 2 shows the results of the measurements and evaluations of the various physical properties.
[0088] [Table 2]
[0089] As shown in Table 1, Examples 1 to 17 have high total light transmittance, good light transmittance, and excellent surface appearance of molded articles. In addition, they have low heat shrinkage and therefore excellent heat resistance. As shown in Comparative Examples 1 to 5 in Table 2, when the refractive index or MFR of the styrene resin is outside the prescribed range, the light transmittance and the surface appearance of the molded article are inferior. Also, when the average diameter of the minor axis (d1) or major axis (d2) (d1≦d2) is greater than 50 μm, the light transmittance is low and the surface appearance and heat resistance of the molded article are inferior. [Industrial Applicability]
[0090] Molded articles containing the styrene-based resin composition of the present invention can be suitably used for packaging materials, building materials, electronic and electric parts, automobiles, etc.
Claims
1. A styrene-based resin (a) having a refractive index of 1.545 to 1.600 and an MFR of 3 or more; Average minor axis length d 1 and the above d 1 The average length of the major axis is equal to or greater than d 2 d 1 Or d 2 and a cellulose polysaccharide (b) having a particle size of 0.03 to 50 μm, the styrene-based resin (a) is a rubber-modified styrene-based resin having particles of a rubber-like polymer (A) dispersed in a matrix, or a styrene-based copolymer resin having a styrene-based monomer unit and an unsaturated carboxylic acid-based monomer unit; The content of the rubber-like polymer (A) is 2 to 10% by mass based on 100% by mass of the rubber-modified styrene-based resin, The crystallinity of the cellulose polysaccharide (b) is 50 to 100%; A styrene-based resin composition, characterized in that the content of the styrene-based resin (a) is 45.0 to 99.5 parts by mass, and the content of the cellulose-based polysaccharide (b) is 0.5 to 55.0 parts by mass, relative to the total amount (100 parts by mass) of the styrene-based resin (a) and the cellulose-based polysaccharide (b).
2. A styrene-based resin composition as described in claim 1, wherein the lignin content in 100 mass% of the cellulose-based polysaccharide (b) is 10 mass% or less.
3. A styrene-based resin composition as described in claim 1 or 2, containing a rubber-modified styrene-based resin as the styrene-based resin (a), and the average particle diameter of the rubber-like polymer (A) contained in the rubber-modified styrene-based resin is 0.5 to 2.5 μm.
4. The styrene-based resin composition according to claim 1 or 2, further comprising 0.5 to 20 parts by mass of a dispersant (c) relative to the total amount (100 parts by mass) of the styrene-based resin (a) and the cellulose-based polysaccharide (b).
5. 5. The styrene-based resin composition according to claim 4, wherein the dispersant (c) is one or more compounds selected from the group consisting of fatty acid ester-based compounds, polyethylene glycol-based compounds, terpene-based compounds, and rosin-based compounds.
6. A molded article comprising the styrene-based resin composition according to any one of claims 1 to 5.
Citation Information
Patent Citations
Styrene-based composite resin composition
JP1995173352A
Styrenic composite resin composition
JP1996231795A
Resin composition
JP2011137094A
Fiber reinforced resin composition containing chemical modified cellulose nanofiber and thermoplastic resin
JP2016176052A