Resin composition

The resin composition with a blend of liquid rubber resin, polyphenylene ether resin, and crosslinking agent, combined with high inorganic filler content, addresses conductivity limitations, achieving effective thermal conductivity and physical property enhancements for high-frequency transmission.

JP7573660B2Active Publication Date: 2024-10-25NANYA PLASTICS CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023006908
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-09-22
Filing Date
2023-01-20
Publication Date
2024-10-25
Estimated Expiration
2043-01-20

AI Technical Summary

Technical Problem

Current resin compositions face limitations in effectively increasing the additive ratio of thermally conductive powder (inorganic filler), resulting in insufficient conductivity improvement, especially for high-frequency transmission requirements.

Method used

A resin composition comprising a resin blend of liquid rubber resin, polyphenylene ether resin, and crosslinking agent, combined with an inorganic filler amount of at least 40 parts by weight, which includes silicon dioxide, aluminum oxide, or other compatible fillers, enhances thermal conductivity while maintaining physical properties.

Benefits of technology

The resin composition achieves improved thermal conductivity of 1.2 W/mK or more, supporting high-frequency transmission with enhanced peel strength, heat resistance, and low dielectricity, addressing issues of poor water absorption and heat resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573660000001
    Figure 0007573660000001
  • Figure 0007573660000002
    Figure 0007573660000002
  • Figure 0007573660000003
    Figure 0007573660000003
Patent Text Reader

Abstract

To provide a resin composition which effectively improves thermal conductivity of a material of a resin composition, and thereby can satisfy a severe high frequency transmission requirement.SOLUTION: A resin composition contains a resin containing a liquid rubber resin, a polyphenylene ether resin and a crosslinking agent, and an inorganic filler, wherein a used amount of the inorganic filler is at least 40 pts.mass or more with respect to 100 pts.mass of the total amount of the resin.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to compositions, particularly resin compositions. [Background technology]

[0002] 2. Description of Related Art With the rapid development of wireless networks, satellite radars and fifth-generation (5G) communications, the power output of 5G electronic products is continuously improving, and the related application frequencies are also increasing significantly. Correspondingly, the heat dissipation requirements of materials are also increasing significantly. Summary of the Invention

[0003] Problem to be solved by the invention However, the current addition ratio of thermally conductive powder (inorganic filler) cannot be effectively increased, and the usage amount only reaches about 10%, so the thermal conductivity cannot be effectively improved to meet the strict requirements of high-frequency transmissions.

[0004] Means for solving the problem The present disclosure provides a resin composition that can effectively improve the thermal conductivity of the material of the resin composition, thereby meeting stringent high-frequency transmission requirements.

[0005] The resin composition of the present disclosure includes a resin and an inorganic filler. The resin includes a liquid rubber resin, a polyphenylene ether resin, and a crosslinking agent. Compared to a total of 100 parts by mass of the resin, the amount of the inorganic filler used is at least 40 parts by mass or more.

[0006] In one embodiment of the present disclosure, the amount of inorganic filler used is between 40 parts by weight and 75 parts by weight based on 100 parts by weight of the total amount of the above resins.

[0007] In one embodiment of the present disclosure, the inorganic filler comprises silicon dioxide, aluminum oxide, silicon nitride, aluminum nitride, aluminum silicate, calcium silicate, boron nitride, silicon carbide, titanium dioxide, strontium titanate, or calcium titanate.

[0008] In one embodiment of the present disclosure, the inorganic filler comprises at least a first inorganic filler and a second inorganic filler that are different.

[0009] In one embodiment of the present disclosure, the resin contains a liquid rubber resin having a usage rate of 5 to 25% in the resin, a polyphenylene ether resin having a usage rate of 5 to 20% in the resin, and a crosslinking agent having a usage rate of 5 to 20% in the resin.

[0010] In one embodiment of the present disclosure, the liquid rubber resin has 10% to 90% of 1,2-vinyl groups, 0% to 50% of styrene groups, and a molecular weight between 1000 and 5000.

[0011] In one embodiment of the present disclosure, the above-mentioned resin composition further comprises at least one selected from the group consisting of a flame retardant, a siloxane coupling agent, and an accelerator.

[0012] In one embodiment of the present disclosure, the amount of the siloxane coupling agent used is 0.1 parts by mass to 5 parts by mass, relative to 100 parts by mass of the total amount of the above resins.

[0013] In an embodiment of the present disclosure, the amount of the accelerator used is 0.1 parts by mass to 5 parts by mass, relative to 100 parts by mass of the total amount of the above resins.

[0014] In an embodiment of the present disclosure, the thermal conductivity of the resin composition is 1.2 W / mK or more.

[0015] As described above, the resin of the resin composition of the present disclosure includes a liquid rubber resin, a polyphenylene ether resin, and a crosslinking agent. By combining the above-mentioned resin with an inorganic filler, the amount of the inorganic filler used can be at least 40 parts by mass or more, and the inorganic filler has good compatibility with the resin.

[0016] Effect of the Invention A substrate manufactured using the resin composition of the present disclosure can effectively improve thermal conductivity while maintaining good physical properties such as peel strength, heat resistance, water absorption, and low dielectric properties, and as a result, can meet strict high-frequency transmission requirements. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] In this embodiment, the resin composition includes at least a resin and an inorganic filler, and the resin includes a liquid rubber resin, a polyphenylene ether resin, and a crosslinking agent. In addition, by combining the resin and the inorganic filler, the amount of the inorganic filler used can be at least 40 parts by mass or more, and the inorganic filler has good compatibility with the resin. Therefore, the substrate manufactured by the resin composition of the embodiment can effectively improve the thermal conductivity while maintaining good physical properties such as peel strength, heat resistance, water absorption, and low dielectric property, and can meet strict high frequency transmission requirements. For example, the thermal conductivity of the resin composition is 1.2 W / mK or more, but the thermal conductivity of the resin composition may be determined according to actual design requirements, so it is not limited thereto.

[0018] Furthermore, the amount of inorganic filler used relative to 100 parts by mass of the total resin can be between 40 and 75 parts by mass (for example, 40 parts by mass, 45 parts by mass, 50 parts by mass, 55 parts by mass, 60 parts by mass, 65 parts by mass, 70 parts by mass, 75 parts by mass, or any value from 40 parts by mass to 75 parts by mass mentioned above), but the amount of inorganic filler used is not limited to this and can be adjusted according to actual design requirements.

[0019] In some embodiments, inorganic fillers include, but are not limited to, silicon dioxide, aluminum oxide, silicon nitride, aluminum nitride, aluminum silicate, calcium silicate, boron nitride, silicon carbide, titanium dioxide, strontium titanate, or calcium titanate.

[0020] Currently, two or more types of inorganic fillers are often used to improve the thermal conductivity in the resin composition. However, after mixing multiple types of inorganic fillers, problems of poor water absorption and poor heat resistance are likely to occur, and a follow-up problem of insufficient strength occurs between the copper foil and the substrate. However, in an embodiment, the inorganic filler may contain at least a different first inorganic filler and a second inorganic filler. By designing the resin containing the liquid rubber resin, the polyphenylene ether resin, and the crosslinker, the probability of occurrence of problems of poor water absorption and poor heat resistance after adding at least two types of inorganic fillers to the resin composition can be reduced and the thermal conductivity can be further improved, thereby improving the reliability of the follow-up substrate. It should be noted that the present disclosure does not limit the number of types of inorganic fillers used. As long as at least one type of inorganic filler is used, all of them are within the protection scope of the disclosure.

[0021] In some embodiments, the resin includes a liquid rubber resin at a usage rate of 5% to 25% in the resin, a polyphenylene ether resin at a usage rate of 5% to 20% in the resin, and a crosslinker at a usage rate of 5% to 20% in the resin, but the disclosure is not limited thereto.

[0022] In some embodiments, the liquid rubber resin may be polybutadiene and has the following structure: [ka] (wherein n=15 to 25, preferably n=16 to 22).

[0023] In some embodiments, the liquid rubber resin may be a polyolefin, including, but not limited to, styrene-butadiene-divinylbenzene terpolymer (terpolymer), styrene-butadiene-maleic anhydride terpolymer, vinyl-polybutadiene-urethane oligomer, styrene-butadiene copolymer, hydrogenated styrene-butadiene copolymer, styrene-isoprene copolymer, hydrogenated styrene-isoprene ethylene copolymer, hydrogenated styrene-butadiene-divinylbenzene copolymer, polybutadiene (homopolymer of butadiene), maleic anhydride-styrene-butadiene copolymer, methylstyrene copolymer, or combinations thereof.

[0024] In some embodiments, the liquid rubber resin has 10%-90% 1,2-vinyl, 0%-50% styrene and a molecular weight of 1000-5000, and can be effectively crosslinked with other resins to improve compatibility, although the present disclosure is not limited thereto.

[0025] In some embodiments, the polyphenylene ether resin is a thermosetting polyphenylene ether resin having a styrene-type polyphenylene ether and an acrylic-type polyphenylene ether as terminal groups. For example, the structure of the styrene-type polyphenylene ether is represented by the structural formula (A): [ka] As shown in.

[0026] Here, R1 to R8 may be an allyl group, a hydrogen group, a C1 to C6 alkyl group, or one or more selected from the above groups, and X is O (oxygen atom), [ka] , where P1 is styryl, [ka] and n=an integer from 1 to 99.

[0027] The structure of the terminal acrylic polyphenylene ether is represented by the following structural formula (B): [ka] As shown in.

[0028] Here, R1 to R8 may be an allyl group, a hydrogen group, a C1 to C6 alkyl group, or one or more selected from the above groups. X is O (oxygen atom), [ka] where P2 may be [ka] or [ka] where n=an integer from 1 to 99.

[0029] Specific examples of polyphenylene ether resins include, but are not limited to, dihydroxy polyphenylene ether resins (e.g., SA-90 available from Sabic Corporation), vinylbenzyl polyphenylene ether resins (e.g., OPE-2st available from Mitsubishi Gas Chemical Corporation), methacrylate polyphenylene ether resins (e.g., SA-9000 available from Sabic Corporation), vinylbenzyl-modified bisphenol A polyphenylene ether resins or vinyl chain-extended bisphenol A polyphenylene ether resins. The polyphenylene ether is preferably vinyl polyphenylene ether.

[0030] In some embodiments, the crosslinking agent is used to increase the crosslinking degree of the thermosetting resin, adjust the stiffness and toughness of the substrate, and adjust the processability, and the type used may be one or more combinations of 1,3,5-triallyl cyanurate (TAC), triallyl isocyanurate (TAIC), trimethylallyl isocyanurate (TMAIC), diallyl phthalate, divinylbenzene, or 1,2,4-triallyl trimellit.

[0031] In some embodiments, the resin composition further includes at least one selected from the group consisting of a flame retardant, a siloxane coupling agent, and an accelerator. In addition, the amount of the siloxane coupling agent used is in the range of 0.1 parts by weight to 5 parts by weight (e.g., 0.1 parts by weight, 0.5 parts by weight, 1 part by weight, 1.5 parts by weight, 2 parts by weight, 3 parts by weight, 4 parts by weight, 5 parts by weight, or 0.1 parts by weight to 5 parts by weight, or the above-mentioned 0.1 parts by weight to 5 parts by weight), and the amount of the accelerator used is 0.1 parts by weight to 5 parts by weight (e.g., 0.1 parts by weight, 0.5 parts by weight, 1 part by weight, 1.5 parts by weight, 2 parts by weight, 3 parts by weight, 4 parts by weight, 5 parts by weight, or any value of the above-mentioned 0.1 parts by weight to 5 parts by weight), but the present disclosure is not limited thereto.

[0032] In some embodiments, siloxane coupling agent can include, but is not limited to, siloxane.According to the type of functional group, siloxane can be divided into aminosilane compound, epoxide silane compound, vinyl silane compound, ester silane compound, hydroxysilane compound, isocyanate silane compound, methylsilane acryloyloxysilane compound, and acryloxysilane compound, but the present disclosure is not limited thereto.

[0033] In some embodiments, the accelerator comprises a catalyst, which can be dimethylimidazole, diphenylimidazole, diethyltetramethylimidazole, or benzyldimethylamine, although the disclosure is not limited thereto.

[0034] It should be noted that the resin composition of the present disclosure can be processed into prepreg and copper foil substrate (FCCL) according to the actual design requirements. Therefore, the prepreg and FCCL manufactured using the resin composition of the present disclosure also have better thermal conductivity. Furthermore, the specific implementations listed above are not the limitations of the present disclosure. The resin of the resin composition includes a liquid rubber resin, a polyphenylene ether resin, and a crosslinking agent, and the amount of inorganic filler used can be at least 40 parts by mass or more by the combination of the resin and the inorganic filler, all of which fall within the scope of protection of the present disclosure.

[0035] The following examples and comparative examples are given to illustrate the effects of the present disclosure, but the scope of the claims of the present disclosure is not limited to the scope of the examples.

[0036] The FCCLs produced in the respective Examples and Comparative Examples were evaluated according to the following methods.

[0037] Dielectric constant Dk: The dielectric constant Dk at a frequency of 10 GHz was measured by a dielectric analyzer (E4991A) manufactured by Agilent Technologies.

[0038] Dielectric loss Df: The dielectric loss Df at a frequency of 10 GHz was measured by a dielectric analyzer (E4991A) manufactured by Agilent Technologies.

[0039] The glass transition temperature (℃) was measured using a dynamic mechanical analyzer (DMA). Thermal conductivity analysis test: An interface material heat resistance and thermal conductivity measuring instrument conforming to the ASTM D5470 standard was used.

[0040] Peel strength (lb / in): Tests the peel strength between copper foil and circuit carrier. <Examples 1 to 4 and Comparative Examples 1 to 3>

[0041] Toluene was mixed with the resin composition shown in Table 1 to form a varnish of a thermosetting resin composition. The varnish was impregnated into Nanya glass fiber cloth (Nanya Plastics Co., Ltd., cloth type 1078) at room temperature, and then dried (impregnator) at 110°C for several minutes to obtain a prepreg with a resin content of 76 wt%. Finally, four prepregs were laminated between two pieces of 35 μm thick copper foil and heated to 25 kg / cm. 2 The mixture was kept at a constant pressure and temperature of 85°C for 20 minutes, heated to 185°C at a heating rate of 3°C / min, kept at a constant temperature for 120 minutes, and then slowly cooled to 130°C to obtain a 0.8 mm thick FCCL.

[0042] The physical properties of the prepared FCCL are tested, and the results are shown in Table 1. After comparing the results of Examples 1-4 and Comparative Examples 1-3 in Table 1, the following conclusions can be drawn. Compared with Comparative Example 1, Example 1 has a proportion of inorganic filler up to 40wt%, so the thermal conductivity can reach 1.2w / mk or more; compared with Comparative Example 2, Example 1 uses two kinds of inorganic fillers, so the thermal conductivity can be made good; compared with Comparative Example 3, Example 1 uses a styrene-containing liquid rubber resin, so the peel strength can be further improved. Furthermore, compared with Example 1, Example 2 can further improve the glass transition temperature and peel strength by increasing the amount of accelerator used; compared with Example 1, Example 3 can further improve the thermal conductivity by increasing the amount of filler (boron nitride) used; compared with Example 1, Example 4 can further improve the peel strength by increasing the amount of siloxane coupling agent used. In addition, compared with Comparative Examples 1 to 3, Example 1 already exhibits good technical effects, and Examples 2 to 4 are optional technical means, and in this case, the technical means are not essential.

[0043] [Table 1]

[0044] In summary, the resin of the resin composition of the present disclosure includes a liquid rubber resin, a polyphenylene ether resin, and a crosslinking agent. By combining the aforementioned resin with an inorganic filler, the amount of the inorganic filler used can be at least 40 parts by mass or more, and the inorganic filler has good compatibility with the resin.

[0045] Industrial Applicability The substrate manufactured by the disclosed resin composition can effectively improve thermal conductivity while maintaining good physical properties such as peel strength, heat resistance, water absorption, and low dielectric properties, and as a result, can meet the stringent requirements of high frequency transmission.

Claims

1. A resin composition comprising a liquid rubber resin, a polyphenylene ether resin, a crosslinking agent, an inorganic filler, a siloxane coupling agent, and an accelerator, the crosslinking agent is 1,3,5-triallyl cyanurate (TAC), triallyl isocyanurate (TAIC), trimethylallyl isocyanurate (TMAIC), diallyl phthalate, divinylbenzene, 1,2,4-triallyl trimellitate, or a combination of two or more thereof; The polyphenylene ether resin is used in an amount of 5% by mass to 20% by mass in the resin, the inorganic filler comprises boron nitride and silicon dioxide; A resin composition, wherein an amount of the inorganic filler used is in the range of 40 parts by mass to 75 parts by mass per 100 parts by mass of a total amount of the resin, and an amount of the boron nitride used is greater than an amount of the silicon dioxide used.

2. The resin is A crosslinking agent having a usage ratio of 5% to 20% in the resin; The resin composition according to claim 1 .

3. 2. The resin composition of claim 1, wherein the liquid rubber resin has 10% to 90% 1,2-vinyl groups, 0% to 50% styryl groups, and a molecular weight of 1000 to 5000.

4. The resin composition according to claim 1, wherein the amount of the siloxane coupling agent used is in the range of 0.1 to 5 parts by mass per 100 parts by mass of the total amount of the resin.

5. The resin composition according to claim 1 , wherein the amount of the accelerator used is in the range of 0.1 to 5 parts by mass per 100 parts by mass of the total amount of the resin.

6. The resin composition according to claim 1 , wherein the resin composition has a thermal conductivity of 1.2 W / mK or more.

Citation Information

Patent Citations

  • Resin composition for preparing heat-conducting high-frequency copper-clad plate adhesive and preparation method thereof

    CN114231014A

  • Prepreg and product thereof

    CN114456574A

  • Rubber composition and pneumatic tire

    WO2020100493A1

  • Resin composition, prepreg, resin-equipped film, resin-equipped metal foil, metal-cladded layered sheet, and wiring board

    WO2021059911A1