Silicone rubber composition with excellent fire resistance

A silicone rubber composition using organopolysiloxane, silica, and specific refractory agents addresses the limitations of conventional compositions by enabling varied coloration and improved mechanical properties, enhancing flame retardancy and fire resistance for diverse industrial applications.

JP7573765B2Active Publication Date: 2024-10-25KCC SILICONE CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023569621
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-05-20
Filing Date
2022-05-03
Publication Date
2024-10-25
Estimated Expiration
2042-05-03

AI Technical Summary

Technical Problem

Conventional fire-resistant silicone rubber compositions using graphite as a flame retardant suffer from insufficient color toning properties and mechanical properties due to the use of dark-colored fillers, leading to limitations in application across various industrial fields.

Method used

A silicone rubber composition comprising organopolysiloxane, silica, a plasticizer, a flame retardant with a platinum catalyst, refractory agents like quartz and wollastonite, and flame retardant adjuvants such as cerium oxide and titanium dioxide, which do not include dark-colored materials, allowing for varied coloration and improved mechanical properties.

Benefits of technology

The composition achieves excellent flame retardancy and fire resistance with adjustable color and enhanced mechanical properties, suitable for applications in automobiles, electronics, architecture, ships, and railways.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573765000001
    Figure 0007573765000001
  • Figure 0007573765000002
    Figure 0007573765000002
  • Figure 0007573765000003
    Figure 0007573765000003
Patent Text Reader

Abstract

The present invention relates to a fire resistant silicone rubber composition comprising a silicone rubber comprising an organopolysiloxane, silica, and a plasticizer; a flame retardant comprising a platinum catalyst; a fire resistant agent comprising quartz and wollastonite; and a flame retardant aid comprising cerium oxide and titanium dioxide.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a silicone rubber composition which can be mixed in a variety of hues and which has excellent flame retardancy and fire resistance. [Background technology]

[0002] Silicone rubber has a strong basic structure of polymer chains even at high temperatures of over 300℃, and unlike carbon-based polymers, it does not decompose due to heat. It is flexible and has excellent thermal stability and flame retardancy, so it is widely used in many application industrial fields such as transportation, aviation, space, architecture, civil engineering, electricity, textiles, and cosmetics. In addition, these characteristics of silicone rubber remain as silica without crystalline SiO2 even under conditions of over 1000℃ such as fire, so silicone rubber is used as the basic binder for fire-resistant materials. However, silicone rubber breaks down after extinguishing a fire despite its excellent thermal stability, so it is usually used with the addition of inorganic fillers that can improve fire resistance.

[0003] For example, conventional fire-resistant compositions containing silicone rubber generally contain silicone rubber, graphite or vermiculite as a fire-resistant agent, iron oxide as a fire-resistant auxiliary, and inorganic fibers as a fire-retardant. Specifically, Korean Patent No. 1896898 (Patent Document 1) discloses a fire-resistant silicone rubber composition containing silicone rubber, a curing agent, a fire-resistant agent made of natural minerals and fire-resistant materials, a flame retardant, and a fire-resistant auxiliary. However, conventional fire-resistant compositions such as those in Patent Document 1 have problems in that they contain graphite as a fire-resistant agent, so that they have insufficient color matching, or the mechanical properties of the cured product produced by using a large amount of filler are insufficient.

[0004] Therefore, there is a need for research and development into silicone rubber compositions that do not contain dark-hued fire retardants such as graphite, can be mixed in a variety of hues, and have excellent mechanical properties after curing, as well as excellent flame retardancy and fire resistance. Summary of the Invention [Problem to be solved by the invention]

[0005] Therefore, an object of the present invention is to provide a silicone rubber composition which does not contain flame retardants or fire resistant agents with dark hues such as graphite, and therefore can be mixed in a variety of hues; it also has excellent mechanical properties when cured, and excellent flame and fire resistance; and it can be used as a material in a variety of industrial fields, such as automobiles, electronics / electrical, construction, ships, and railways. [Means for solving the problem]

[0006] The present invention relates to a silicone rubber comprising an organopolysiloxane, silica, and a plasticizer; and a flame retardant containing a platinum catalyst; a refractory material including quartz and wollastonite; A fire-resistant silicone rubber composition is provided, comprising: a flame retardant adjuvant comprising cerium oxide and titanium dioxide. Effect of the Invention

[0007] The silicone rubber composition of the present invention does not use dark flame retardants or expanding agents such as graphite or iron oxide, so it can be mixed in a variety of colors. It also has excellent mechanical properties, flame retardancy and fire resistance after curing, making it useful as a material in a variety of industrial fields such as automobiles, electronics / electrical, construction, ships, and railways. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The present invention will be described in detail below.

[0009] Fire-resistant silicone rubber composition The fire-resistant silicone rubber composition according to the present invention comprises a silicone rubber, a flame retardant, a fire-resistant agent, and a flame-retardant auxiliary.

[0010] Silicone rubber The silicone rubber includes an organopolysiloxane, silica, and a plasticizer.

[0011] Silicone rubber is a main component of the fire-resistant silicone rubber composition and plays a role in realizing mechanical properties such as hardness, tensile strength, and elongation of the fire-resistant silicone rubber produced from the silicone rubber.

[0012] <Organopolysiloxane> Organopolysiloxane is the main polymer of silicone rubber and plays a role in controlling the hardness, tensile strength, elongation, etc. of the produced rubber.

[0013] The organopolysiloxane may contain at least one alkenyl group in one molecule. For example, the organopolysiloxane may contain two or more organopolysiloxanes with different alkenyl group contents, specifically, a first organopolysiloxane with a relatively low alkenyl group content and a second organopolysiloxane with a relatively high alkenyl group content. As described above, when using two or more organopolysiloxanes with different alkenyl group contents, the crosslink density of the silicone rubber can be adjusted to adjust the physical properties of the silicone rubber, thereby improving hardness, tensile strength, elongation, etc.

[0014] The first organopolysiloxane serves to improve the tensile strength and elongation of the cured product.

[0015] The first organopolysiloxane contains at least one alkenyl group in one molecule, and can be specifically represented by the following Chemical Formula 1.

[0016] [ka]

[0017] In Chemical Formula 1, R 1 ~R 8 are each independently an alkyl group having 1 to 10 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, or an aryl group having 6 to 15 carbon atoms; R 2 and R 4 At least one of the groups is a vinyl group, a is an integer from 1 to 10,000; b is an integer from 1 to 10,000.

[0018] In this case, the alkyl group may be, for example, a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a cyclopentyl group, a cyclohexyl group, etc., and specifically, a methyl group, an ethyl group, or a propyl group.

[0019] The alkenyl group may be, for example, a vinyl group, an allyl group, a butenyl group, a pentenyl group, a hexenyl group, or the like, and specifically may be a vinyl group or an allyl group.

[0020] The aryl group (aryl) may be, for example, a phenyl group, a tolyl group, a xylyl group, a naphthyl group, a biphenylene group, or the like, and specifically, may be a phenyl group.

[0021] The alkyl and alkenyl groups may be linear or branched.

[0022] The first organopolysiloxane may have a vinyl group content of 0.03 to 0.08 mol % or 0.04 to 0.05 mol %. When the vinyl group content of the first organopolysiloxane is within the above range, the strength of the prepared cured silicone rubber can be improved. In addition, when the vinyl group content of the first organopolysiloxane is less than the above range, the vinyl group content is insufficient, resulting in a problem of reduced curing performance. When the vinyl group content of the first organopolysiloxane is more than the above range, the crosslink density of the silicone rubber composition increases more than necessary, resulting in improved curing performance, but the high crosslink density of the prepared cured product may result in reduced tensile strength and elongation.

[0023] The first organopolysiloxane may have a viscosity of 5,000,000 to 100,000,000 cst or 10,000,000 to 100,000,000 cst at 25° C. When the viscosity of the first organopolysiloxane at 25° C. is within the above range, it has the effect of adjusting the viscosity of the composition to be suitable for compression and injection molding. In addition, when the viscosity of the first organopolysiloxane at 25° C. is less than the above range, the strength of the rubber material produced is weakened, and the workability is reduced. When the viscosity exceeds the above range, the physical properties of the rubber and the dispersion of silica are difficult when the silicone rubber is produced, and the strength of the material is very hard, and the workability is poor.

[0024] The degree of polymerization of the first organopolysiloxane may be 1,000 to 10,000, or 3,000 to 8,000. When the degree of polymerization of the first organopolysiloxane is within the above range, the tensile strength of the produced cured silicone rubber is improved. Here, the degree of polymerization is the number of silicon atoms in one molecule of the first organopolysiloxane. When the degree of polymerization of the first organopolysiloxane is below the above range, there is a problem that the workability of the produced silicone rubber, such as two-roll milling, is reduced, and when it exceeds the above range, there is a possibility that the physical properties, such as the tensile strength and elongation, of the produced cured product are poor.

[0025] The first organopolysiloxane may be included in an amount of 45 to 75 parts by weight, or 50 to 70 parts by weight, based on 100 parts by weight of silicone rubber. When the content of the first organopolysiloxane is within the above range, not only can the plasticity of the composition be easily adjusted for compression and injection molding, but the tensile strength of the cured silicone rubber can be improved to control the hardness, making it possible to use the composition as an excellent packing material. In addition, when the content of the first organopolysiloxane is less than the above range, the tensile strength and elongation of the cured silicone rubber can be reduced, and when the content exceeds the above range, the hardness of the silicone rubber can be reduced.

[0026] The second organopolysiloxane serves to reinforce the hardness and tensile strength of the silicone rubber.

[0027] The second organopolysiloxane contains at least one alkenyl group in one molecule, and can be specifically represented by the following Chemical Formula 2.

[0028] [ka]

[0029] In Chemical Formula 2, R 10 ~R 17 are each independently an alkyl group having 1 to 10 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, or an aryl group having 6 to 15 carbon atoms; R 10 , R 11 , R 13 and R 16 At least one of the groups contains a vinyl group; n is an integer from 1 to 10,000; m is an integer from 1 to 10,000.

[0030] In this case, the alkyl group may be, for example, a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a cyclopentyl group, a cyclohexyl group, etc., and specifically, a methyl group, an ethyl group, or a propyl group.

[0031] The alkenyl group may be, for example, a vinyl group, an allyl group, a butenyl group, a pentenyl group, a hexenyl group, or the like, and specifically may be a vinyl group or an allyl group.

[0032] The aryl group (aryl) may be, for example, a phenyl group, a tolyl group, a xylyl group, a naphthyl group, a biphenylene group, or the like, and specifically, may be a phenyl group.

[0033] The alkyl and alkenyl groups may be linear or branched.

[0034] The second organopolysiloxane may have a vinyl group content of 0.1 to 0.3 mol%, or 0.15 to 0.25 mol%. When the vinyl group content of the second organopolysiloxane is within the above range, the mechanical properties such as hardness and tensile strength of the silicone rubber can be well controlled. When the vinyl group content of the second organopolysiloxane is less than the above range, the hardness and tensile strength of the cured product may be low, and when it exceeds the above range, the hardness of the cured product may be high and the elongation may be low.

[0035] The second organopolysiloxane may have a viscosity of 5,000,000 to 100,000,000 cst or 10,000,000 to 100,000,000 cst at 25° C. When the viscosity of the second organopolysiloxane at 25° C. is within the above range, it has the effect of adjusting the viscosity of the composition to be suitable for compression and injection molding. In addition, when the viscosity of the second organopolysiloxane at 25° C. is less than the above range, the strength of the rubber base material is weakened, and the workability is reduced. When the viscosity of the second organopolysiloxane is greater than the above range, the physical properties of the rubber and the dispersion of silica are difficult when producing silicone rubber, and the strength of the base material is very hard, and the workability is poor.

[0036] The second organopolysiloxane may have a degree of polymerization of 1,000 to 10,000, or 3,000 to 8,000. When the degree of polymerization of the second organopolysiloxane is within the above range, the tensile strength of the produced cured silicone rubber is improved. Here, the degree of polymerization is the number of silicon atoms in one molecule of the second organopolysiloxane. When the degree of polymerization of the second organopolysiloxane is less than the above range, the elongation of the silicone rubber is reduced, and when it exceeds the above range, the mold flow and plasticity of the silicone rubber are increased, or the tensile strength is poor.

[0037] The second organopolysiloxane may be included in an amount of 10 to 30 parts by weight, or 12 to 20 parts by weight, based on 100 parts by weight of silicone rubber. When the content of the second organopolysiloxane is within the above range, not only can the plasticity of the composition be easily adjusted for compression and injection molding, but the tensile strength of the cured silicone rubber can be improved to control the hardness, making it possible to use the composition as an excellent packing material. In addition, when the content of the second organopolysiloxane is less than the above range, the hardness of the cured product is low and the tensile strength is poor, and when the content exceeds the above range, the hardness of the cured product is increased and the elongation is poor.

[0038] The first organopolysiloxane and the second organopolysiloxane may be included in a weight ratio of 2 to 6: 1, or a weight ratio of 3 to 5: 1. If the weight ratio of the first organopolysiloxane and the second organopolysiloxane is less than the above range, i.e., if a small amount of the first organopolysiloxane is included based on the weight of the second organopolysiloxane, the hardness of the cured product increases and the elongation decreases, and if it exceeds the above range, i.e., if an excessive amount of the first organopolysiloxane is included based on the weight of the second organopolysiloxane, the hardness of the cured product decreases and the tensile strength decreases, and there is a possibility of a problem of irregularity occurring during compression and injection molding.

[0039] <Silica> Silica serves to improve the mechanical strength, flame retardancy, and fire resistance of the cured product.

[0040] The silica is not particularly limited as long as it is generally applicable to silicone rubber, and may be, for example, amorphous or crystalline.

[0041] The silica may be wet, dry, fumed or pyrogenic silica.

[0042] The silica has a BET specific surface area of ​​50 m 2 / g or more, 50~400m 2 / g, or 150-250m 2 If the BET specific surface area of ​​the silica is less than the above range, the improvement in mechanical properties such as hardness and tensile strength of the produced rubber, which is an effect of adding silica, may not be sufficient, and if it exceeds the above range, the silica may not be easily dispersed, resulting in a problem that the hardness of the produced cured product is poor.

[0043] The silica may have an average particle size (d50) of 0.001 to 1 um, or 0.01 to 0.1 um. If the average particle size (d50) of the silica is less than the above range, the silica is not easily dispersed, and if the average particle size (d50) of the silica exceeds the above range, the transparency of the composition and the mechanical properties of the produced silicone rubber may be reduced. In this case, the average particle size (d50) is the particle size value at 50% cumulative volume of the particle size distribution calculated based on the volume standard measured by laser diffraction method.

[0044] The silica may be included in an amount of 10 to 35 parts by weight, or 15 to 30 parts by weight, based on 100 parts by weight of silicone rubber. If the silica content is less than the above range, the improvement in mechanical properties such as hardness and tensile strength of the silicone rubber produced, which is an effect of adding silica, may be insufficient, and if the content exceeds the above range, the excessive amount of silica may cause a problem of poor processability of the composition.

[0045] <Plasticizer> The plasticizer functions to bind to the surface of the silica, inhibiting the occurrence of crepe hardening during processing when the silica is directly bonded to the organopolysiloxane, and to improve the dispersibility of the silica.

[0046] The plasticizer may be used without any particular limitation as long as it is a surface treatment agent for normal silica, for example, it may be hydroxyl-containing organohydroxopolysiloxane.Specifically, the plasticizer may contain hydroxyl (OH) at the end without containing alkenyl group, and more specifically, it may be represented by the following chemical formula 3.

[0047] [ka]

[0048] In Chemical Formula 3, R 20 is a substituted or unsubstituted C 1-10 is an alkyl group or a hydroxyl group, R 21 and R 22 each independently represents a substituted or unsubstituted C 1-10 is an alkyl group, l is a real number between 5 and 1,500.

[0049] Specifically, R 20 is a substituted or unsubstituted C 1-4 is an alkyl group or a hydroxyl group, R 21 and R 22 each independently represents a substituted or unsubstituted C 1-6 Alkyl group or C 1-3 In this case, the alkyl group may be linear or branched.

[0050] Furthermore, 1 may be a real number from 5 to 1,000 or from 5 to 100.

[0051] The plasticizer may have a hydroxyl content of 4-7 wt%, 4.5-6.5 wt%, or 5.0-6.0 wt% based on the total weight. If the hydroxyl content of the plasticizer is less than this range, the mechanical properties of the produced fire-resistant silicone rubber may be reduced, and if it exceeds this range, the produced silicone rubber may have oil content, which may reduce its processability.

[0052] The plasticizer may have a viscosity of 30 to 60 cP (centi-poise), or 35 to 50 cP at 25° C. If the viscosity of the plasticizer at 25° C. is below this range, silica is not easily dispersed, resulting in a problem of reduced mechanical properties of the cured product, while if it exceeds this range, the viscosity of the composition is low, resulting in a problem of reduced workability.

[0053] The plasticizer may be included in an amount of 1 to 8 parts by weight or 1 to 5 parts by weight based on 100 parts by weight of silicone rubber. If the plasticizer content is less than this range, silica is not easily dispersed, resulting in a problem of reduced mechanical properties of the cured product. If the plasticizer content exceeds this range, there is a possibility that an excessive amount of oil will be present in the rubber composition, resulting in reduced workability and mechanical properties.

[0054] Flame retardants The flame retardant can improve flame retardancy by increasing the crosslink density of the resin during burning in a fire and forming a resin. The flame retardant contains a platinum catalyst.

[0055] The platinum catalyst can be any catalyst that can be used normally for silicone rubber without any particular limitations. Examples of the platinum catalyst include platinum halides (e.g., reaction products containing platinum halides such as PtCl4, H2PtCl4·6H2O, and Na2PtCl4·4H2O and cyclohexane), platinum-olefin complexes, platinum-alcohol complexes, platinum-alcoholate complexes, platinum-ether complexes, platinum-aldehyde complexes, platinum-ketone complexes, platinum-vinylsiloxane complexes (e.g., platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complexes), bis-(γ-picoline)-platinum dichloride, trimethylenedipyridine-platinum dichloride, dicyclopentadiene-platinum dichloride, cyclooctadiene-platinum dichloride, cyclopentadiene-platinum dichloride, bis(alkynyl)bis(triphenylphosphine)platinum complexes, and bis(alkenyl)(cyclooctadiene)platinum complexes.

[0056] The flame retardant may be included in an amount of 0.01 to 0.5 parts by weight, or 0.05 to 0.3 parts by weight, based on 100 parts by weight of silicone rubber. If the amount of the flame retardant is less than the above range, the flame retardancy and fire resistance during burning will be poor. If the amount of the flame retardant is more than the above range, the economic efficiency will be reduced due to the use of expensive platinum catalyst, and the appearance of the cured product will be strongly yellow.

[0057] Additionally, the silicone rubber composition may further comprise a flame retardant commonly used in the silicone rubber field.

[0058] Fireproofing agent The fireproofing agent serves to improve the ceramicization performance of the composition during combustion in a fire and to improve the fire resistance of the resulting hardened product.

[0059] The fireproofing agent includes quartz and wollastonite. When the silicone rubber is burned, the fireproofing agents quartz and wollastonite combine with other inorganic fillers to form a ceramic structure, thereby exhibiting fire resistance.

[0060] The quartz may have an average diameter of 0.5 to 50 um, 1 to 10 um, or 1 to 5 um. If the average diameter of the quartz is less than the above range, problems may occur in charging the silicone rubber, and if it exceeds the above range, problems may occur in the mechanical properties and fire resistance of the silicone rubber.

[0061] The wollastonite may have an average diameter of 1 to 50 um, 5 to 20 um, or 5 to 10 um. If the average diameter of the wollastonite is less than the above range, problems may occur in charging the silicone rubber, and if it exceeds the above range, problems may occur in the mechanical properties and fire resistance of the silicone rubber.

[0062] The fire-resistant silicone rubber composition may contain quartz and wollastonite in a weight ratio of 1:0.5 to 1.5, or 1:0.7 to 1.2. If the mixing weight ratio of quartz and wollastonite is below the above range, i.e., if a small amount of wollastonite is contained relative to the quartz content, the flame retardancy and fire resistance of the cured product may be poor, and if it exceeds the above range, i.e., if an excessive amount of wollastonite is contained relative to the quartz content, the mechanical properties and workability such as two-roll milling of the cured product may be poor.

[0063] For example, the fireproofing agent may be included in the composition in an amount of 40 to 65 parts by weight or 45 to 60 parts by weight per 100 parts by weight of silicone rubber. Specifically, the fireproof silicone rubber composition may include 20 to 35 parts by weight or 22 to 30 parts by weight of quartz and 20 to 35 parts by weight or 22 to 30 parts by weight of wollastonite per 100 parts by weight of silicone rubber.

[0064] If the content of the fireproofing agent in the fire-resistant silicone rubber composition is less than the above range, the fire resistance and flame retardancy of the cured product may be poor, and if it exceeds the above range, the mechanical properties and workability of the cured product may be poor.

[0065] Flame Retardant Additives The flame retardant auxiliary improves heat resistance by preventing oxidation of the organic layer and scission of the main chain, and improves flame retardancy during combustion, thereby improving the heat resistance and flame retardancy of the cured product produced and exerting a synergistic effect on the ceramicization performance of the composition.

[0066] The flame retardant aid includes cerium oxide and titanium dioxide.

[0067] The cerium oxide (CeO2) may have an average diameter of 0.5 to 10 um or 1 to 5 um. If the average diameter of the cerium oxide is less than the above range, it may be difficult to disperse the cerium oxide in the composition, and if it exceeds the above range, it may cause problems such as poor heat resistance and flame retardancy of the silicone rubber.

[0068] The titanium dioxide (TiO2) has a BET specific surface area of ​​20 to 70 m 2 / g, or 35-60m 2 If the BET specific surface area of ​​titanium dioxide is less than the above range, problems such as poor heat resistance and flame retardancy may occur, and if it exceeds the above range, problems such as difficulty in dispersing titanium dioxide in the composition may occur.

[0069] The fire-resistant silicone rubber composition may contain cerium oxide and titanium dioxide in a weight ratio of 1:0.5 to 1.5, or 1:0.8 to 1.3. If the mixed weight ratio of cerium oxide and titanium dioxide is below the above range, i.e., if a small amount of titanium dioxide is contained relative to the cerium oxide content, the cured product may have poor flame retardancy, and if it exceeds the above range, i.e., if an excessive amount of titanium dioxide is contained relative to the cerium oxide content, the cured product may have poor heat resistance.

[0070] For example, the flame retardant auxiliary may be included in the composition in an amount of 0.2 to 10 parts by weight or 0.5 to 5 parts by weight per 100 parts by weight of silicone rubber. Specifically, the fire-resistant silicone rubber composition may include 0.1 to 5 parts by weight or 0.2 to 3 parts by weight of cerium oxide and 0.1 to 5 parts by weight or 0.2 to 3 parts by weight of titanium dioxide per 100 parts by weight of silicone rubber.

[0071] If the content of the flame retardant auxiliary in the fire-resistant silicone rubber composition is less than the above range, the heat resistance and flame retardancy of the silicone rubber may be poor, and if the content exceeds the above range, the mechanical properties of the silicone rubber may be deteriorated or the color may be affected.

[0072] The fire-resistant silicone rubber composition is substantially free of conventional colored flame retardants and / or fire resistant agents such as expanded graphite, expanded vermiculite, iron oxide, hydromagnesite, huntite, diatomaceous earth, kaolin, aluminum oxide, magnesium oxide, etc. Specifically, the fire-resistant silicone rubber composition may contain less than 0.1 wt % or less than 0.01 wt % of the above-mentioned colored flame retardants or fire resistant agents based on the total weight. This provides the fire-resistant silicone rubber composition according to the present invention with the advantage that it can be colored in a variety of hues.

[0073] In addition, the fire-resistant silicone rubber composition does not contain a platinum-based flame retardant such as bis(2,4-pentanedionato)platinum. Specifically, the fire-resistant silicone rubber composition may contain less than 0.1 wt % or less than 0.01 wt % of a platinum-based flame retardant based on the total weight. As a result, the fire-resistant silicone rubber composition according to the present invention has excellent flame retardancy and fire resistance.

[0074] Fire-Resistant Silicone Rubber The fire resistant silicone rubber according to the present invention is produced from the fire resistant silicone rubber composition as described above.

[0075] The fire-resistant silicone rubber may have a hardness of 55 to 65 Shore A or 57 to 62 Shore A, as measured by the method described in ASTM D2240. If the hardness of the fire-resistant silicone rubber is less than the above range, it may be very soft and have reduced elasticity, and if the hardness exceeds the above range, it may be very hard and have reduced elasticity and elongation.

[0076] The fire-resistant silicone rubber may have a tensile strength of 6.0 MPa or more or 6.0 to 7.5 MPa, as measured by the method described in ASTM D412. If the tensile strength of the fire-resistant silicone rubber is below the above range, the strength is weak and the mechanical properties may be poor.

[0077] The fire-resistant silicone rubber may have an elongation percentage of 300 to 500% or 350 to 500%. If the elongation percentage of the fire-resistant silicone rubber is less than the above range, the durability may decrease, and if it exceeds the above range, the elasticity may decrease.

[0078] In addition, the fire-resistant silicone rubber may have a flame retardancy of UL-V0 as measured by the method described in UL94-V. That is, the fire-resistant silicone rubber has excellent flame retardancy and fire resistance, and can be used as a material in various industrial fields such as automobiles, electronics / electrical, construction, ships, and railways.

[0079] The present invention will be described in more detail with reference to the following examples. However, the following examples are merely intended to specifically describe specific embodiments of the present invention, and are not intended to limit or interpret the scope of the present invention to the contents described in these examples.

[0080] Example 1. Preparation of fire-resistant silicone rubber composition 59.3 parts by weight of the first organopolysiloxane, 15 parts by weight of the second organopolysiloxane, 22.6 parts by weight of silica, and 3.1 parts by weight of plasticizer were added to a kneader reactor and stirred at 80±20°C for 20 minutes. At this time, the silica was added in 4 portions and stirred to disperse. When the stirring was completed, the temperature was raised to 160±10°C, and the mixture was stirred for 2 hours, and then cooled to 80°C to prepare a base compound, which is a silicone rubber. Then, 26.7 parts by weight of wollastonite, 26.7 parts by weight of quartz, 0.15 parts by weight of platinum catalyst, 0.8 parts by weight of cerium oxide (CeO2), and 0.8 parts by weight of titanium dioxide (TiO2) were added to 100 parts by weight of the silicone rubber, and the mixture was mixed in a kneader reactor for 30 minutes or more to prepare a fire-resistant silicone rubber composition.

[0081] Examples 2 to 21 and Comparative Examples 1 to 6 Silicone rubber compositions were produced in the same manner as in Example 1, except that the compositions shown in Tables 1 to 3 were used.

[0082] [Table 1]

[0083] [Table 2]

[0084] [Table 3]

[0085] The ingredients and product names of each component used in the following Examples and Comparative Examples are shown in Table 4 below.

[0086] [Table 4]

[0087] Test example: Physical property evaluation The physical properties of the specimens prepared from the compositions of the Examples and Comparative Examples were measured in the following manner and are shown in Table 5.

[0088] Specifically, the test specimen was prepared by uniformly mixing 100 parts by weight of the fire-resistant silicone rubber composition of the Example or Comparative Example and 1.5 parts by weight of 2,4-dichlorobenzoyl peroxide as a curing agent in a two-roll mill, curing the mixture at 120°C for 5 minutes as a first curing step, and curing the mixture at 200°C for 4 hours as a second curing step to prepare a sheet-shaped test specimen of fire-resistant silicone rubber having a thickness of 2 mm.

[0089] (1) Plasticity The measuring device used was a Plastometer, and the Williams Plasticity measuring method of JIS K6249 was used to measure the degree of spreading for 5 minutes by plasticizing (softening) the sample, followed by a 2-minute degassing process, after which a mass twice the specific gravity was taken and allowed to cool for 5 minutes, after which a load of 5 kg was applied to measure the degree of spreading for 5 minutes.

[0090] In this case, plasticity is a physical property that indicates the softness or spreadability of rubber. If the plasticity is low (i.e., very soft) when working with a two-roll mill, it is difficult to extract the rubber in a sheet form, and when it is injected into an injector, it must be injected in a long ribbon form without breaking, but it breaks easily, which can cause problems when injecting into the injector.

[0091] (2)Hardness The method was as described in ASTM D2240. After preparing a 6mm thick test piece from the fire-resistant silicone rubber, the hardness was measured 5 times at 1 / 2 inch inside from the end using a Shore A type hardness tester. The measurement position was randomly determined, and the measurement was performed while avoiding the part that had already been measured. The hardness of the test piece was determined by calculating the average of the 5 hardness values ​​measured.

[0092] (3) Tensile strength The tensile strength of the fire-resistant silicone rubber was measured according to the method described in ASTM D412, specifically, an ASTM D412 C type specimen having a thickness of 2 mm was prepared, and the specimen was pulled at a speed of 500 mm / min using a Universal Testing Machine as a measuring instrument to measure the tensile strength. The tensile strength was measured for four specimens for each composition, and the average value of the four was determined as the tensile strength.

[0093] (4) Elongation rate The elongation of the fire-resistant silicone rubber was measured according to the method described in ASTM D412, specifically, an ASTM D412 C type specimen with a thickness of 2 mm was prepared, and the final length increase of the specimen at the time of specimen breakage was measured using a Universal Testing Machine as a measuring instrument. The length increase was then calculated as a percentage relative to the initial horizontal length of the specimen (2 cm) to determine the elongation.

[0094] (5) Specific gravity Specific gravity was measured according to the method described in ASTM D792.

[0095] (6) Flame retardancy Flame retardancy was measured according to the method described in UL94-V.

[0096] (7) Fire resistance To measure the fire resistance of fire-resistant silicone rubber, a 2mm thick sheet-like test piece was placed on a fixable stand and then one side was heated with a butane gas torch (gas consumption 80g / h, 960kcal) with a flame length of 10cm for 10 minutes. The silicone rubber was then removed from the stand and the appearance was checked and rated as poor if there were holes or the piece was completely burned, fair if there were cracks and good if the appearance was good.

[0097] [Table 5]

[0098] As shown in Table 5, the specimens prepared from the compositions of the examples had appropriate plasticity, hardness, tensile strength, elongation, and specific gravity, and were excellent in flame retardancy and fire resistance.

[0099] On the other hand, in the case of the comparative examples, Comparative Example 1, which did not contain quartz, was poor in tensile strength, elongation, and flame retardancy, and Comparative Example 2, which did not contain wollastonite, was poor in flame retardancy and fire resistance.

[0100] In addition, Comparative Examples 3 and 4, which did not contain cerium oxide or titanium dioxide, had poor fire resistance, and Comparative Example 5, in which triazole, a conventional flame retardant auxiliary, was used instead of titanium dioxide, had poor fire resistance.

[0101] Moreover, in Comparative Example 6, in which diatomaceous earth, a conventional fireproofing agent, was used instead of wollastonite, the flame retardancy and fire resistance were poor.

Claims

1. A silicone rubber comprising a first organopolysiloxane having a vinyl group content of 0.03 to 0.08 mol%, a second organopolysiloxane having a vinyl group content of 0.1 to 0.3 mol%, silica, and a plasticizer; A flame retardant containing a platinum catalyst; a fireproofing agent comprising quartz and wollastonite; a flame retardant aid comprising cerium oxide and titanium dioxide; The first organopolysiloxane and the second organopolysiloxane are contained in a weight ratio of 2 to 6:1, The silica is contained in an amount of 10 to 35 parts by weight per 100 parts by weight of silicone rubber, The plasticizer is contained in an amount of 1 to 8 parts by weight per 100 parts by weight of silicone rubber. Fire-resistant silicone rubber composition.

2. 2. The fire resistant silicone rubber composition of claim 1, comprising quartz and wollastonite in a weight ratio of 1:0.5-1.

5.

3. 2. The fire resistant silicone rubber composition of claim 1, comprising cerium oxide and titanium dioxide in a weight ratio of 1:0.5-1.

5.

4. 2. The fire resistant silicone rubber composition of claim 1, comprising 100 parts by weight of silicone rubber, 0.01 to 0.5 parts by weight of a flame retardant, 40 to 65 parts by weight of a fire resistant agent, and 0.2 to 10 parts by weight of a flame retardant auxiliary.

5. A fire-resistant silicone rubber produced from the fire-resistant silicone rubber composition according to any one of claims 1 to 4.

6. 6. The fire-resistant silicone rubber according to claim 5, having a hardness of 55 to 65 Shore A as measured by the method described in ASTM D2240, a tensile strength of 6.0 MPa or more as measured by the method described in ASTM D412, and an elongation of 300 to 500%.

Citation Information

Patent Citations

  • Silica gel formula capable of enhancing fire resistance

    CN105838075A

  • Application of hybrid systems MgO-SiO2 / multiwalled olygomeric silsesquioxanes as promoters of ceramization in silicone composites for covers of electrical cables

    EP2740716A1

  • JP1973074553A

  • Flame-retardant silicone rubber wire and cable coating composition

    JP2002536504A

  • Room-temperature-curable organopolysiloxane composition

    JP2009167420A