Ferroelectric Composition
A ferroelectric composition of ferroelectric polymers and anion-modified cellulose nanofibers enhances spontaneous polarization, addressing the limitations of polymer materials by improving pyroelectricity and piezoelectricity without mechanical stretching, suitable for piezoelectric sensors and ferroelectric memories.
Patent Information
- Application Number
- JP2020024496
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-02-17
- Publication Date
- 2024-10-28
- Estimated Expiration
- 2040-02-17
AI Technical Summary
Polymer materials exhibit lower pyroelectricity and piezoelectricity, lower specific heat, and higher coercive electric field, and require mechanical stretching to align dipoles for ferroelectricity, which increases processing costs and restricts material shape.
A ferroelectric composition combining a ferroelectric polymer with anion-modified cellulose nanofibers, such as oxidized cellulose nanofibers, to enhance spontaneous polarization without mechanical stretching.
The composition improves spontaneous polarization, enabling applications in pyroelectric and piezoelectric materials like piezoelectric sensors and ferroelectric memories.
Smart Images

Figure 0007573806000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a ferroelectric composition. [Background technology]
[0002] Known ferroelectric materials to date include metal oxide-based materials such as PbTiO3, LiTaO3, BaTiO3, and PbZrTiO3 (PZT), vinylidene fluoride-based polymers such as polyvinylidene fluoride and copolymers of vinylidene fluoride and trifluoroethylene, and polymer-based materials such as copolymers of vinylidene cyanide and vinyl acetate.
[0003] Of these, polymer-based materials have lower pyroelectricity and piezoelectricity than metal oxide-based materials, but the coercive field required to reverse polarization is high. On the other hand, polymer-based materials have a low specific heat and a low dielectric constant, so they also have a good figure of merit. In addition, the coercive field is stable. For this reason, polymer-based materials are being considered for use in actuators, memory materials, etc.
[0004] In general, in order to make polymeric materials exhibit ferroelectricity, it is necessary to mechanically uniaxially or biaxially stretch the dipoles in the polymer to be aligned in one direction. This dipole orientation creates remnant polarization, which causes ferroelectricity. However, the stretching process has the disadvantages of increasing costs due to the additional processing steps and imposing limitations on the shape of the material.
[0005] It is known that polyvinylidene fluoride, a polymer material, can exhibit ferroelectricity without stretching (see Non-Patent Document 1). [Prior art documents] [Non-patent literature]
[0006] [Non-Patent Document 1] E. Yamada, A. Nishioka, H. Suzuki, T. Koda, and S. Ikeda, “Test of Ferroelectricity in Non-stretched Poly(vinylidene fluoride) / Clay Nanocomposites”, Japanese Journal of Applied Physics, 2007, Vol.46, No.11, pp.7371-7374 Summary of the Invention [Problem to be solved by the invention]
[0007] According to Non-Patent Document 1, even when using polyvinylidene fluoride, which is a polymer material, ferroelectricity can be exhibited without stretching treatment. However, the spontaneous polarization decreases.
[0008] An object of the present invention is to provide a ferroelectric composition capable of improving spontaneous polarization. [Means for solving the problem]
[0009] As a result of extensive investigations into the above problems, the inventors discovered that the above problems could be solved by using a ferroelectric polymer in combination with anion-modified cellulose nanofibers, and thus completed the present invention. That is, the present inventors provide the following [1] to [4]. [1] A ferroelectric composition comprising: component (A): a ferroelectric polymer; and component (B): anion-modified cellulose nanofibers. [2] The ferroelectric composition according to [1] above, wherein the component (A) is at least one selected from the group consisting of polyvinylidene fluoride, a nanocomposite of polyvinylidene fluoride and organoclay, polyvinylidene fluoride-trifluoroethylene copolymer, nylon 11, and nylon 7. [3] The ferroelectric composition according to [1] or [2] above, wherein the component (B) is at least one selected from the group consisting of oxidized cellulose nanofibers, carboxymethylated cellulose nanofibers, and esterified cellulose nanofibers. [4] The ferroelectric composition according to any one of the above [1] to [3], wherein the content of the component (B) is 0.1 to 50 mass % relative to the mass of the component (A). Effect of the Invention
[0010] According to the present invention, a ferroelectric composition capable of improving spontaneous polarization can be provided. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a chart showing the results of DE hysteresis measurement of the test pieces for DE measurement made using the ferroelectric compositions produced in Examples 1 and 2 and the Comparative Example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, the present invention will be described in detail based on preferred embodiments thereof. In this specification, the notation "AA to BB" means from AA to BB.
[0013] The ferroelectric composition of the present invention contains component (A): a ferroelectric polymer, and component (B): anion-modified cellulose nanofibers. The reason why the ferroelectric composition of the present invention can improve the spontaneous polarization by containing component (B) is presumed to be as follows: When component (B) is contained, the interplanar spacing between the crystals of component (A) is increased. Therefore, it is presumed that the interaction between the crystals of component (A) is weakened, and the spontaneous polarization can be improved.
[0014] (Component (A)) Component (A) is a ferroelectric polymer. Examples of the ferroelectric polymer include polymers having fluorine atoms such as polyvinylidene fluoride (PVDF), polyvinylidene fluoride-trifluoroethylene copolymer (P(VDF-TrFE)), vinylidene fluoride-tetrafluoroethylene copolymer, etc.; vinylidene cyanide-vinyl acetate copolymer, cyanoethyl cellulose, cyanoethyl hydroxysaccharose, cyanoethyl hydroxycellulose, cyanoethyl hydroxypullulan, cyanoethyl methacrylate polymer, cyanoethyl acrylate polymer, cyanoethyl hydroxyethyl cellulose, cyanoethyl amylose ... Examples of the polymers include polymers having a cyano group or a cyanoethyl group, such as cyanoethyl hydroxypropyl cellulose, cyanoethyl dihydroxypropyl cellulose, cyanoethyl hydroxypropyl amylose, cyanoethyl polyacrylamide, cyanoethyl polyacrylate, cyanoethyl pullulan, cyanoethyl polyhydroxymethylene, cyanoethyl glycidol pullulan, cyanoethyl saccharose, and cyanoethyl sorbitol; odd-numbered nylons, such as nylon 11 and nylon 7; and nanocomposites of these polymers or nylons with inorganic materials, such as organized clay and mica. An example of the organoclay in the nanocomposite of PVDF and organoclay is Clolisite (registered trademark) 20A (manufactured by Southern Clay Industries).
[0015] The ferroelectric polymer is preferably at least one selected from the group consisting of PVDF, a nanocomposite of PVDF and organized clay, PVDF-TrFE, nylon 11, and nylon 7, and more preferably a nanocomposite of PVDF and organized clay or PVDF-TrFE. Incidentally, the component (A) may be a commercially available product.
[0016] (Component (B)) Component (B) is an anion-modified cellulose nanofiber. "Anion-modified cellulose nanofiber" refers to fine fibers obtained by defibrating anion-modified cellulose fibers, in which anionic groups have been introduced into the cellulose molecular chain, to nanoscale fiber diameters. Hereinafter, "cellulose nanofiber" may be abbreviated as "CNF." Examples of anion-modified cellulose fibers include carboxylated (oxidized) cellulose fibers, carboxymethylated cellulose fibers, phosphated cellulose fibers, and phosphite cellulose fibers. By defibrating these, oxidized cellulose nanofibers, carboxymethylated cellulose nanofibers, phosphated cellulose nanofibers, and phosphite cellulose nanofibers can be obtained, respectively. Among these, carboxylated (oxidized) cellulose nanofibers and carboxymethylated cellulose nanofibers are preferred, and carboxylated (oxidized) cellulose nanofibers are more preferred.
[0017] In this specification, "CNF" refers to fine fibers with a fiber diameter of about 3 to 500 nm, which are made by pulp, a cellulose raw material, being refined to the nanometer level. The average fiber diameter and average fiber length of cellulose nanofibers can be obtained by averaging the fiber diameters and fiber lengths obtained from the results of observing each fiber using an atomic force microscope (AFM) or a transmission electron microscope (TEM). Cellulose nanofibers can be obtained by applying a mechanical force to pulp to refine it, or by defibrating anion-modified cellulose fibers such as carboxylated cellulose fibers (hereinafter also referred to as "oxidized cellulose fibers"), carboxymethylated cellulose fibers, phosphate esterified cellulose fibers, and phosphite esterified cellulose fibers. The average fiber length and average fiber diameter of fine fibers can be adjusted by oxidation treatment and defibration treatment. The anion-modified cellulose nanofibers have an average fiber length of preferably 50 μm or less, more preferably 10 μm or less, and even more preferably 1 μm or less, and an average fiber diameter of preferably 2 to 500 nm, more preferably 2 to 250 nm, and even more preferably 2 to 50 nm.
[0018] The average aspect ratio of the anion-modified cellulose nanofiber is usually 50 or more. There is no particular upper limit, but it is usually 1000 or less. The average aspect ratio can be calculated by the following formula: Aspect ratio = average fiber length / average fiber diameter
[0019] The type of cellulose (hereinafter also referred to as "cellulose raw material") used as the raw material for anion-modified cellulose nanofibers is not particularly limited, and cellulose originating from, for example, plants (e.g., wood, bamboo, hemp, jute, kenaf, agricultural waste, cloth, pulp (softwood unbleached kraft pulp (NUKP), softwood bleached kraft pulp (NBKP), hardwood unbleached kraft pulp (LUKP), hardwood bleached kraft pulp (LBKP), softwood unbleached sulfite pulp (NUSP), softwood bleached sulfite pulp (NBSP), thermomechanical pulp (TMP), recycled pulp, dissolving pulp (DKP), waste paper, etc.), animals (e.g., ascidians), algae, microorganisms (e.g., acetic acid bacteria (Acetobacter)), microbial products, etc. can be used. Cellulose fibers derived from plants or microorganisms are preferred, and cellulose fibers derived from plants are more preferred.
[0020] The number average fiber diameter of the cellulose raw material is not particularly limited. In the case of softwood kraft pulp, which is a common pulp, the number average fiber diameter is about 30 to 60 μm, and in the case of hardwood kraft pulp, the number average fiber diameter is about 10 to 30 μm. In the case of other pulps, those that have undergone general refining have a diameter of about 50 μm. For example, in the case of refining chips or the like that are several centimeters in size, it is preferable to adjust the diameter to about 50 μm by mechanical processing using a disintegrator such as a refiner or beater.
[0021] (chemical modification) Anionic groups are introduced into the above-mentioned cellulose raw material to produce anion-modified cellulose fibers. The method for introducing the anionic groups is not particularly limited, but examples thereof include a method for introducing anionic groups into the pyranose ring of cellulose by oxidation or substitution reaction. Specifically, examples of such a method include a reaction in which a hydroxyl group in the pyranose ring is oxidized to convert it into a carboxyl group, and a reaction in which a carboxymethyl group, a phosphate ester group, or a phosphorous ester group is introduced into the pyranose ring by substitution reaction.
[0022] (Carboxylation (oxidation)) An example of anion modification is carboxylation (also called oxidation). Carboxylation refers to a reaction in which the hydroxyl groups on the pyranose rings of cellulose are oxidized to carboxy groups (-COOH (acid type) or -COOM (metal salt type) (M is a metal ion)). In this specification, anion-modified cellulose fibers obtained by carboxylation are also called carboxylated cellulose fibers or oxidized cellulose fibers. Carboxylated cellulose fibers can be obtained by carboxylating (oxidizing) the above-mentioned cellulose raw material by a known method.
[0023] The amount of carboxy groups in the carboxylated cellulose fibers is not particularly limited, but is preferably adjusted to 0.6 to 3.0 mmol / g, and more preferably 1.0 to 2.0 mmol / g, based on the bone dry mass of the carboxylated cellulose fibers. The amount of carboxy groups can be adjusted by controlling the type and amount of the oxidizing agent, the temperature and time during the oxidation reaction, etc. The amount of carboxy groups in the carboxylated cellulose fibers is the same as the amount of carboxy groups in the carboxylated cellulose nanofibers.
[0024] The amount of carboxy groups in carboxylated cellulose fibers can be measured by the following method: 60 ml of 0.5% by mass slurry (medium: water) of carboxylated cellulose fiber is prepared, and 0.1 M aqueous hydrochloric acid is added to adjust the pH to 2.5. 0.05 N aqueous sodium hydroxide is added dropwise to measure the electrical conductivity until the pH becomes 11. The electrical conductivity is calculated from the amount of sodium hydroxide (a) consumed in the neutralization stage of the weak acid, where the change in electrical conductivity is gradual, using the following formula: Amount of carboxyl groups [mmol / g carboxylated cellulose fiber] = a [ml] x 0.05 / mass of carboxylated cellulose fiber [g].
[0025] One example of the carboxylation (oxidation) method is a method in which a cellulose raw material is oxidized in water using an oxidizing agent in the presence of an N-oxyl compound and a compound selected from the group consisting of bromides, iodides, and mixtures thereof. This oxidation reaction selectively oxidizes the primary hydroxyl group at the C6 position of the glucopyranose ring on the cellulose surface, and aldehyde groups and carboxy groups (-COOH) or carboxylate groups (-COO) are formed on the surface. - The concentration of the cellulose raw material in water during the reaction is not particularly limited, but is preferably 5% by mass or less.
[0026] The N-oxyl compound refers to a compound capable of generating a nitroxy radical. Any compound can be used as the N-oxyl compound as long as it promotes the target oxidation reaction. For example, 2,2,6,6-tetramethylpiperidine-1-oxy radical (TEMPO) and its derivatives (for example, 4-hydroxyTEMPO) can be mentioned. The amount of the N-oxyl compound used is not particularly limited as long as it is a catalytic amount capable of oxidizing the cellulose raw material. For example, the amount is preferably 0.01 to 10 mmol, more preferably 0.01 to 1 mmol, and even more preferably 0.05 to 0.5 mmol, per 1 g of bone-dry cellulose raw material. The amount is preferably about 0.1 to 4 mmol / L relative to the entire reaction solution.
[0027] Bromides are compounds containing bromine, examples of which include alkali metal bromides that can be dissociated and ionized in water. Also, iodides are compounds containing iodine, examples of which include alkali metal iodides. The amount of bromide or iodide used can be selected within a range that can promote the oxidation reaction. The total amount of bromide and iodide is, for example, preferably 0.1 to 100 mmol, more preferably 0.1 to 10 mmol, per 1 g of bone-dry cellulose raw material.
[0028] The oxidizing agent may be a known one, such as halogen, hypohalous acid, halous acid, perhalogen acid or their salts, halogen oxide, or peroxide. Among them, sodium hypochlorite is preferable because it is inexpensive and has a low environmental impact. The appropriate amount of the oxidizing agent to be used is, for example, preferably 0.5 to 500 mmol, more preferably 0.5 to 50 mmol, even more preferably 1 to 25 mmol, and even more preferably 3 to 10 mmol, per 1 g of bone-dry cellulose raw material. Also, for example, the amount of the oxidizing agent to be used is preferably 1 to 40 mol per mol of the N-oxyl compound.
[0029] The oxidation of cellulose raw materials is likely to proceed efficiently even under relatively mild conditions. Therefore, the reaction temperature may be 4 to 40°C, or may be room temperature of about 15 to 30°C. As the reaction proceeds, carboxyl groups are generated in the cellulose chains, and a decrease in the pH of the reaction solution is observed. In order to efficiently proceed with the oxidation reaction, it is preferable to add an alkaline solution such as an aqueous sodium hydroxide solution to maintain the pH of the reaction solution at about 8 to 12, preferably 10 to 11. The medium in the reaction solution is preferably water, because it is easy to handle and does not easily cause side reactions. The reaction time in the oxidation reaction can be appropriately set depending on the degree of progress of the oxidation, and is usually from 0.5 to 6 hours, and preferably from about 0.5 to 4 hours.
[0030] The oxidation reaction may be carried out in two stages. For example, the oxidized cellulose fiber obtained by filtering after the completion of the first stage reaction is oxidized again under the same or different reaction conditions, allowing the oxidation to proceed efficiently without being inhibited by salt produced as a by-product in the first stage reaction.
[0031] Another example of the carboxylation (oxidation) method is a method in which the cellulose raw material is oxidized by contacting it with an ozone-containing gas. This oxidation reaction oxidizes at least the hydroxyl groups at positions 2 and 6 of the glucopyranose ring to carboxy groups, and decomposes the cellulose chain. The ozone concentration in the ozone-containing gas is 50 to 250 g / m 3 is preferable, and 50 to 220 g / m 3 The amount of ozone added to the cellulose raw material is preferably 0.1 to 30 parts by mass, and more preferably 5 to 30 parts by mass, based on 100 parts by mass of the solid content of the cellulose raw material. The ozone treatment temperature is preferably 0 to 50°C, and more preferably 20 to 50°C. The ozone treatment time is not particularly limited, but is about 1 to 360 minutes, and preferably about 30 to 360 minutes. When the ozone treatment conditions are within these ranges, excessive oxidation and decomposition of cellulose can be prevented, and the yield of oxidized cellulose fiber is good.
[0032] After the ozone treatment, an additional oxidation treatment may be performed using an oxidizing agent. The oxidizing agent used in the additional oxidation treatment is not particularly limited, and examples thereof include chlorine compounds such as chlorine dioxide and sodium chlorite, oxygen, hydrogen peroxide, persulfuric acid, and peracetic acid. For example, these oxidizing agents are dissolved in a polar organic solvent such as water or alcohol to prepare an oxidizing agent solution, and the additional oxidation treatment can be performed by immersing the cellulose raw material in the solution.
[0033] (Carboxymethylation) As described above, an example of anion modification is carboxymethylation. Carboxymethylated cellulose fibers, which are an example of anion-modified cellulose fibers, may be obtained by carboxymethylating the above-mentioned cellulose raw material by a known method, or may be a commercially available product. In either case, the degree of carboxymethyl substitution per anhydrous glucose unit of cellulose is 0.01 to 0.50, preferably 0.01 to 0.44, more preferably 0.02 to 0.40, and even more preferably 0.10 to 0.30. If the degree of carboxymethyl substitution exceeds 0.50, the resin becomes soluble in a medium such as water, and may not be able to maintain a fibrous shape. The degree of carboxymethyl substitution of the carboxymethyl cellulose fibers is the same as the degree of carboxymethyl substitution of the carboxymethyl cellulose nanofibers.
[0034] The degree of carboxymethyl substitution of carboxymethylated cellulose fibers can be measured by the following method: Weigh out approximately 2.0 g of carboxymethylated cellulose fiber (bone dry) and place it in a 300 mL Erlenmeyer flask with a stopper. Add 100 mL of nitric acid methanol (a solution of 100 mL of concentrated nitric acid added to 1000 mL of methanol) and shake for 3 hours to convert the salt-form carboxymethylated cellulose fiber (hereinafter also referred to as "carboxymethylated cellulose fiber") into acid-form carboxymethylated cellulose fiber. Weigh out 1.5 to 2.0 g of acid-form carboxymethylated cellulose fiber (bone dry) and place it in a 300 mL Erlenmeyer flask with a stopper. Moisten the acid-form carboxymethylated cellulose fiber with 15 mL of 80% by mass methanol, add 100 mL of 0.1 N NaOH, and shake for 3 hours at room temperature. Using phenolphthalein as an indicator, back-titrate the excess NaOH with 0.1 N H2SO4. Calculate the degree of carboxymethyl substitution (DS) using the following formula: A = [(100 × F'-(0.1N H2SO4) (mL) × F) × 0.1] / (bone-dry mass of acid-form carboxylated cellulose fiber (g)) DS = 0.162 x A / (1-0.058 x A) A: The amount of 1N NaOH required to neutralize 1 g of acid-type carboxymethylcellulose fiber (mL) F: Factor of 0.1N H2SO4 F': factor of 0.1N NaOH.
[0035] An example of a method for producing carboxymethyl cellulose fibers is as follows: To the cellulose raw material, 3 to 20 times by weight of water and / or a lower alcohol (e.g., water, methanol, ethanol, N-propyl alcohol, isopropyl alcohol, N-butyl alcohol, isobutyl alcohol, tertiary butyl alcohol) is added as a solvent, either alone or as a mixed medium of two or more kinds. When a lower alcohol is mixed with the solvent, the mixing ratio of the lower alcohol is preferably 60 to 95% by mass. To this, an alkali metal hydroxide (e.g., sodium hydroxide, potassium hydroxide) is added as a mercerizing agent in an amount of 0.5 to 20 times the molar amount per anhydrous glucose residue of the cellulose raw material. The cellulose raw material, solvent, and mercerizing agent are mixed, and a mercerization treatment is carried out at a reaction temperature of 0 to 70°C (preferably, 10 to 60°C) and for a reaction time of 15 minutes to 8 hours (preferably, 30 minutes to 7 hours). Thereafter, a carboxymethylating agent (e.g., monochloroacetic acid or a salt thereof) is added in an amount of 0.05 to 10.0 times the molar amount per glucose residue, and an etherification reaction is carried out at a reaction temperature of 30 to 90°C (preferably, 40 to 80°C) and for a reaction time of 30 minutes to 10 hours (preferably, 1 to 4 hours).
[0036] "Carboxymethylated cellulose fiber," a type of anion-modified cellulose used in the preparation of anion-modified CNF, is one that maintains at least a part of its fibrous shape even when dispersed in water. Therefore, it is distinguished from carboxymethyl cellulose, a type of water-soluble polymer. When observing an aqueous dispersion of "carboxymethylated cellulose fiber" with an electron microscope, a fibrous substance can be observed. On the other hand, when observing an aqueous dispersion of carboxymethyl cellulose, a type of water-soluble polymer, no fibrous substance is observed. In addition, when "carboxymethylated cellulose fiber" is measured by X-ray diffraction, a peak of cellulose type I crystals can be observed, but cellulose type I crystals are not observed in carboxymethyl cellulose, a water-soluble polymer.
[0037] (Esterification) An example of anion modification is esterification. An example of esterification is introduction of a phosphate group or a phosphite group into a cellulose raw material. In this specification, anion modified cellulose fibers obtained by introduction of a phosphate group are called phosphate esterified cellulose fibers, and anion modified cellulose fibers obtained by introduction of a phosphite group are called phosphite esterified cellulose fibers, and both are collectively called esterified cellulose fibers.
[0038] An example of a method for producing phosphated cellulose fibers is a method in which a powder or an aqueous solution of a compound having a phosphate group is mixed with a cellulose raw material or a slurry thereof. Examples of the compound having a phosphate group include phosphoric acid, sodium dihydrogen phosphate, disodium hydrogen phosphate, trisodium phosphate, sodium pyrophosphate, sodium metaphosphate, potassium dihydrogen phosphate, dipotassium hydrogen phosphate, tripotassium phosphate, potassium pyrophosphate, potassium metaphosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, triammonium phosphate, ammonium pyrophosphate, and ammonium metaphosphate, which may be used alone or in combination of two or more.
[0039] The ratio of the compound having a phosphate group to the cellulose raw material is preferably 0.1 to 500 parts by mass, more preferably 1 to 400 parts by mass, and even more preferably 2 to 200 parts by mass, calculated as phosphorus element, per 100 parts by mass of the solid content of the cellulose raw material. The reaction temperature is preferably 0 to 95°C, more preferably 30 to 90°C. The reaction time is not particularly limited, but is about 1 to 600 minutes, more preferably 30 to 480 minutes. From the viewpoint of suppressing hydrolysis of cellulose, the obtained suspension of phosphoric acid esterified cellulose fiber is preferably heat-treated at 100 to 170°C after dehydration. The degree of phosphoric acid substitution per glucose unit of the phosphoric acid esterified cellulose fiber is preferably 0.001 or more and less than 0.40.
[0040] Examples of methods for producing phosphite-esterified cellulose fibers include a method in which an additive (A) consisting of an alkali metal ion-containing substance and at least one of phosphorous acids and metal phosphites (preferably sodium hydrogen phosphite) is added to a cellulose raw material or a slurry thereof, and then heated to introduce an ester group of phosphorous acid containing an inorganic cation into the cellulose fibers. It is more preferable to add an additive (B) consisting of at least one of urea and a urea derivative, and then heated to introduce an ester group of phosphorous acid containing an inorganic cation and a carbamate group into the cellulose fibers. Examples of the alkali metal ion-containing substance that can be used include hydroxides, metal sulfates, metal nitrates, metal chlorides, metal phosphates, metal phosphites, and metal carbonates. However, metal phosphites that also serve as additive (A) are preferred, and sodium hydrogen phosphite is more preferred.
[0041] The additive (A) is composed of at least one of phosphorous acids and metal phosphites. As the additive (A), for example, phosphorous acid compounds such as phosphorous acid, sodium hydrogen phosphite, ammonium hydrogen phosphite, potassium hydrogen phosphite, sodium dihydrogen phosphite, sodium phosphite, lithium phosphite, potassium phosphite, magnesium phosphite, calcium phosphite, triethyl phosphite, triphenyl phosphite, and pyrophosphorous acid can be used. These phosphorous acids or metal phosphites can be used alone or in combination. However, sodium hydrogen phosphite, which also contains an alkali metal ion, is preferred. The amount of the additive (A) added is preferably 1 to 10,000 g, more preferably 100 to 5,000 g, and even more preferably 300 to 1,500 g, per kg of the cellulose raw material.
[0042] The additive (B) is at least one of urea and a urea derivative. For example, urea, thiourea, biuret, phenylurea, benzylurea, dimethylurea, diethylurea, and tetramethylurea can be used as the additive (B). These ureas or urea derivatives can be used alone or in combination. However, it is preferable to use urea. The amount of the additive (B) added is preferably 0.01 to 100 mol, more preferably 0.2 to 20 mol, and further preferably 0.5 to 10 mol, relative to 1 mol of the additive (A).
[0043] The reaction temperature is preferably 100 to 200° C., more preferably 100 to 180° C. The reaction time is not particularly limited, but is about 10 to 180 minutes, more preferably 30 to 120 minutes. The cellulose fibers having phosphorous ester groups or the like introduced therein are preferably washed prior to defibration. The degree of substitution of phosphorous groups per glucose unit of the phosphorous esterified cellulose fibers is preferably 0.01 or more and less than 0.23.
[0044] (Defibrilization) The device for defibrating the anion-modified cellulose fibers is not particularly limited, but it is preferable to apply a strong shear force to the dispersion of the anion-modified cellulose fibers using a device such as a high-speed rotation type, a colloid mill type, a high-pressure type, a roll mill type, or an ultrasonic type. For efficient defibration, it is preferable to use a wet high-pressure or ultra-high-pressure homogenizer that can apply a pressure of 50 MPa or more and a strong shear force to the dispersion of the anion-modified cellulose fibers. The pressure is more preferably 100 MPa or more, and even more preferably 140 MPa or more. The number of passes through the defibrator may be one or two or more times, and is preferably two or more times.
[0045] In the dispersion treatment, the anion-modified cellulose fibers are usually dispersed in a solvent. The solvent is not particularly limited as long as it can disperse the anion-modified cellulose fibers, and examples of the solvent include water, organic solvents (e.g., hydrophilic organic solvents such as methanol), and mixtures thereof. Since the anion-modified cellulose fibers are hydrophilic, the solvent is preferably water.
[0046] The solid content concentration of the anion-modified cellulose fiber in the dispersion is usually 0.1% by weight or more, preferably 0.2% by weight or more, and more preferably 0.3% by weight or more. This allows the amount of liquid relative to the amount of the anion-modified cellulose fiber to be appropriate and efficient. The upper limit is usually 10% by weight or less, and preferably 6% by weight or less. This allows the fluidity to be maintained.
[0047] In addition, prior to the defibration and dispersion treatment with the high-pressure homogenizer, the anion-modified cellulose fiber can be pretreated as necessary. The pretreatment can be carried out using a mixing, stirring, emulsifying, and dispersing device such as a high-speed shear mixer.
[0048] The anion-modified cellulose fiber may be in the form of an aqueous dispersion obtained after production, or may be subjected to post-treatment as necessary. Examples of the post-treatment include, but are not limited to, drying (e.g., freeze drying, spray drying, tray drying, drum drying, belt drying, thin spreading on a glass plate or the like and drying, fluidized bed drying, microwave drying, and heated fan-type reduced pressure drying), redispersion in water (dispersion device is not limited), and pulverization (e.g., pulverization using equipment such as a cutter mill, hammer mill, pin mill, or jet mill).
[0049] The component (B) may be used alone or in combination of two or more.
[0050] (ratio) In the ferroelectric composition of the present invention, the content of component (B) is preferably 0.1 to 50 mass%, more preferably 0.1 to 20 mass%, even more preferably 0.1 to 10 mass%, and further more preferably 0.1 to 4 mass%, 0.1 to 2 mass%, or 0.1 to 1 mass%, relative to 100 mass% of component (A). When each component is in the form of an aqueous solution, the ratio of each component is calculated based on the solid content.
[0051] (optional ingredient) The ferroelectric composition of the present invention may contain any known optional components, so long as they do not impair the effects of the present invention. Examples of the optional components include ferroelectric oxides, other additive elements, sintering aids, antioxidants, lubricants, etc.
[0052] (Preparation method) The ferroelectric composition of the present invention can be prepared by mixing component (A) and component (B), and, if necessary, any optional components. The mixing may be carried out by dispersing component (B) in component (A), for example, by dissolving or dispersing components (A) and (B) in a solvent, or by melt blending without using a solvent. The solvent may be either water or an organic solvent. Examples of the organic solvent include N-N-dimethylformamide, hexamethylphosphoamide, acetone, glycerin, diethylene glycol, alcohol-based solvents, and ether-based solvents. Among these, N-N-dimethylformamide, hexamethylphosphoamide, and acetone are preferred, and N-N-dimethylformamide is more preferred.
[0053] The stirring is not particularly limited as long as it can uniformly disperse component (B). For example, stirring can be performed with a homogenizer for 30 minutes.
[0054] (Application) The ferroelectric composition of the present invention can be used after drying after preparation. The drying conditions are not particularly limited, and the composition is usually dried by heating under vacuum. After drying, the ferroelectric composition of the present invention may be subjected to a known treatment such as stretching, annealing, or poling in order to increase the crystallinity.
[0055] The ferroelectric composition of the present invention can improve spontaneous polarization, and therefore can be used as a material for pyroelectrics or piezoelectrics. For example, when the ferroelectric composition of the present invention is used as a piezoelectric or pyroelectric, it can increase the signal output caused by the change in spontaneous polarization that occurs when pressure or temperature changes. Therefore, it can be suitably used in piezoelectric sensors and pyroelectric sensors, including ferroelectric memories and touch panels. EXAMPLES
[0056] The present invention will now be described in more detail with reference to examples. The following examples are provided to suitably explain the present invention and are not intended to limit the present invention.
[0057] [Amount of carboxyl groups]: The amount of carboxyl groups was measured as follows. 60 ml of a 0.5% by mass slurry (aqueous dispersion) of oxidized cellulose fiber was prepared, and a 0.1 M aqueous hydrochloric acid solution was added to adjust the pH to 2.5. A 0.05 N aqueous sodium hydroxide solution was added dropwise, and the electrical conductivity was measured until the pH reached 11. The amount of carboxyl groups was calculated using the following formula from the amount of sodium hydroxide (a) consumed in the neutralization stage of the weak acid, where the change in electrical conductivity is gradual. Amount of carboxyl groups [mmol / g oxidized cellulose fiber] = a [ml] x 0.05 / mass of oxidized cellulose [g] As described in the specification, the amount of carboxy groups in the oxidized cellulose fibers is the same as the amount of carboxy groups in the oxidized cellulose nanofibers.
[0058] [Average fiber diameter (nm)]: An aqueous dispersion of oxidized cellulose nanofibers was prepared by diluting the oxidized cellulose nanofibers to a concentration of 0.001% by mass. This diluted dispersion was thinly spread on a mica sample stage and dried by heating at 50°C to prepare a sample for observation. The cross-sectional height of the shape image observed with an atomic force microscope (AFM) was measured, and the weighted average fiber diameter was calculated.
[0059] [Average fiber length (nm)]: Oxidized cellulose nanofibers were fixed on a mica slice, and the fiber lengths of 200 fibers were measured using an atomic force microscope (AFM) to calculate the length-weighted average fiber length. The fiber length was measured using image analysis software WinROOF (Mitani Shoji Co., Ltd.).
[0060] [Aspect ratio]: Calculated by dividing the average fiber length by the average fiber diameter.
[0061] (Production example: Production of oxidized cellulose nanofibers) 5 g (bone dry) of bleached conifer-derived DKP (Buckeye) was added to 500 ml of an aqueous solution containing 78 mg (0.5 mmol) of TEMPO (Sigma Aldrich) and 755 mg (7.4 mmol) of sodium bromide, and the mixture was stirred until the pulp was uniformly dispersed. After adding 16 ml of 2M sodium hypochlorite aqueous solution to the reaction system, the pH was adjusted to 10.3 with 0.5N hydrochloric acid aqueous solution to start the oxidation reaction (oxidation treatment). During the reaction, the pH in the system decreased, so 0.5N sodium hydroxide aqueous solution was added successively to adjust the pH to 10. After reacting for 2 hours, the mixture was filtered through a glass filter and thoroughly washed with water to obtain oxidized cellulose fibers. The amount of carboxyl groups in the obtained oxidized cellulose fibers was 1.7 mmol / g. This was adjusted to 1.0% (w / v) with water and treated 10 times with an ultra-high pressure homogenizer (20°C, 140 MPa) (defibration and dispersion treatment) to obtain a dispersion of oxidized cellulose nanofibers. The average fiber diameter was 3 nm and the average fiber length was 350 nm.
[0062] A five-fold amount of N,N-dimethylformamide (hereinafter referred to as "DMF") was added to the obtained oxidized cellulose nanofiber dispersion, the oxidized cellulose nanofibers were precipitated using a centrifuge, and the supernatant was removed. This process was repeated three times, after which DMF was added so that the CNF concentration became 5% by weight, and the mixture was treated with an ultra-high pressure homogenizer (140 MPa) to produce an N,N-dimethylformamide dispersion of oxidized cellulose nanofibers (hereinafter referred to as "DMF / CNF dispersion").
[0063] Example 1 Polyvinylidene fluoride-trifluoroethylene copolymer (hereinafter referred to as "P(VDF-TrFE)") was added to DMF solvent (Kanto Chemical Co., Ltd.) and stirred with a homogenizer for 30 minutes to prepare a DMF / P(VDF-TrFE) solution. The DMF / CNF dispersion prepared in Production Example 1 was added to the prepared DMF / P(VDF-TrFE) solution, and then the solution was stirred and dispersed with a homogenizer for 30 minutes to prepare a ferroelectric composition. The amount of DMF / CNF dispersion added was adjusted so that the amount of CNF added was 0.1 wt%. The prepared ferroelectric composition was dried at a temperature of 90° C. under vacuum for 24 hours to prepare a P(VDF-TrFE) film.
[0064] Example 2 A ferroelectric composition was produced in the same manner as in Example 1, except that the amount of CNF added was changed to 1.0 wt %, and a P(VDF-TrFE) film was fabricated.
[0065] (Comparative Example) A ferroelectric composition was produced in the same manner as in Example 1, except that the DMF / CNF dispersion was not added, and a P(VDF-TrFE) film was fabricated.
[0066] The P(VDF-TrFE) films prepared in Examples 1 and 2 and Comparative Example were annealed at 140°C. Gold was deposited on the top and bottom of the P(VDF-TrFE) / CNF using an ion coater to serve as electrodes to which a voltage was applied. A test piece for DE measurement was prepared by adhering aluminum foil to the gold-deposited area using silver paste and applying a voltage. DE hysteresis was measured for the prepared test piece for DE measurement under the following conditions. The measurement results are shown in Figure 1.
[0067] [DE hysteresis measurement]: For the measurement, an AC voltage was applied using a function generator WF1941 (NF Circuit Design Block). The voltage was amplified 1000 times using a high voltage amplifier 609C-6 (TREK). This was applied to the sample using a Sawyer-Tower bridge circuit. Data was recorded using a recording board CB-68LP (National Instruments). The waveform was a triangular wave, the frequency was 0.25Hz, and the voltage was 2000V.
[0068] As is clear from Fig. 1, the spontaneous polarization was improved by adding component (B). Therefore, the ferroelectric composition of the present invention containing components (A) and (B) can improve the spontaneous polarization.
Claims
1. Component (A): a ferroelectric polymer, Component (B): Anion-modified cellulose nanofiber, component (B) contains oxidized cellulose nanofibers having a carboxy group amount of 1.0 to 2.0 mmol / g; Component (A) is (a) one or more polymers selected from the group consisting of polyvinylidene fluoride (PVDF), polyvinylidene fluoride-trifluoroethylene copolymer (P(VDF-TrFE)), vinylidene fluoride-tetrafluoroethylene copolymer, vinylidene cyanide-vinyl acetate copolymer, cyanoethyl cellulose, cyanoethyl hydroxysaccharose, cyanoethyl hydroxycellulose, cyanoethyl hydroxypullulan, cyanoethyl methacrylate polymer, cyanoethyl acrylate polymer, cyanoethyl hydroxyethyl cellulose, cyanoethyl amylose, cyanoethyl hydroxypropyl cellulose, cyanoethyl dihydroxypropyl cellulose, cyanoethyl hydroxypropyl amylose, cyanoethyl pullulan, cyanoethyl polyhydroxymethylene, cyanoethyl glycidol pullulan, cyanoethyl saccharose, cyanoethyl sorbitol, nylon 11, and nylon 7; and (b) A nanocomposite of the polymer (a) and an inorganic substance. Either or both of Ferroelectric composition.
2. 2. The ferroelectric composition according to claim 1, wherein the component (A) is at least one selected from the group consisting of polyvinylidene fluoride, a nanocomposite of polyvinylidene fluoride and organoclay, polyvinylidene fluoride-trifluoroethylene copolymer, nylon 11, and nylon 7.
3. 3. The ferroelectric composition according to claim 1, wherein the content of the component (B) is 0.1 to 50 mass % based on the mass of the component (A).
Citation Information
Patent Citations
Resin composition and manufacturing method of resin composition
JP2019143113A
Coating composition for forming high dielectric film and high dielectric film
WO2009116393A1
Coating composition for forming high dielectric film and high dielectric film
WO2009116527A1
Cellulose nanofiber material and cellulose film
WO2014192634A1
Organic flexible ferroelectric polymer nanocomposites
WO2018198139A1