Manufacturing method of glass paper prepreg and fiber reinforced plastic

The use of glass paper prepreg with a resin blend provides a smooth surface for FRP vessels, addressing unevenness issues and enabling direct design application, enhancing mechanical properties and preventing defects in high-pressure operations.

JP7574042B2Active Publication Date: 2024-10-28ARISAWA MFG CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020173510
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-14
Publication Date
2024-10-28
Estimated Expiration
2040-10-14

AI Technical Summary

Technical Problem

Existing methods for manufacturing fiber-reinforced plastic (FRP) pressure vessels require complex surface treatments to address uneven surfaces caused by fiber intersections, which can lead to reduced strength and potential water leakage or vessel failure during high-pressure operations.

Method used

A manufacturing method involving glass paper prepreg impregnated with a specific resin blend, allowing for a smooth surface finish without adjusting unevenness, using a combination of thermoplastic and thermosetting resins to form a transparent protective layer that adheres well and maintains structural integrity.

Benefits of technology

Enables direct application of designs and coatings without additional surface treatments, enhancing the mechanical properties and durability of FRP vessels by eliminating the need for surface adjustments, thus preventing defects and improving water treatment efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574042000001
    Figure 0007574042000001
  • Figure 0007574042000002
    Figure 0007574042000002
  • Figure 0007574042000003
    Figure 0007574042000003
Patent Text Reader

Abstract

To provide an unconventional, highly practical glass paper prepreg and a method for producing the same.SOLUTION: The present invention discloses a glass paper prepreg that is laminated on glass unidirectional prepreg or carbon unidirectional prepreg, or glass cloth prepreg or carbon cloth prepreg 30 to form fiber-reinforced plastic. The glass paper prepreg 1 has glass paper 2 impregnated with resin 3. The content of the resin 3 is set to 60 wt.% or more and the resin flow is set to 40% or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a glass paper prepreg and Fiber Reinforced Plastic The present invention relates to a method for producing the above-mentioned product. [Background technology]

[0002] The effect of fiber cutting on the mechanical properties of surface coating of fiber reinforced plastics (FRP) is explained below using a pressure vessel.

[0003] Conventionally, there are two technologies: reverse osmosis (RO) for desalinating seawater, and ultrafiltration (UF) for converting groundwater into sterile water for drinking or medical use.

[0004] In both methods, water treatment is carried out by applying water pressure to a membrane. The reverse osmosis membrane method requires a pressure vessel with an operating pressure of 2 to 8 MPa, while the ultrafiltration membrane method requires a pressure vessel with an operating pressure of 0.2 to 0.9 MPa. In both methods, a pressure vessel will be used that will not be destroyed by the water pressure during water treatment operation. For example, for a pressure vessel with an operating pressure of 8 MPa, a pressure vessel will be used that will not be destroyed even at a safety factor of 48 MPa, which is six times the operating pressure.

[0005] However, since thermoplastic resins such as polypropylene resin do not have sufficient pressure resistance as materials for these pressure vessels, fiber reinforced plastics (FRP), which is a composite of glass fiber or carbon fiber and epoxy resin, are used.

[0006] For example, to improve the aesthetic appearance of a water treatment plant, the surface of the product after FRP molding (FRP molded product) is painted with a design in a pale color such as white or light blue to match the image of water treatment, and a transparent top coat is applied on top of this design paint as a protective layer, or a transparent top coat is applied directly to the surface of the FRP molded product without a design paint in order to make the most of the raw surface design (crossing fiber pattern) of the FRP molded product. Various types of processing are applied to the surface of the FRP molded product, but there is a demand to make the surface processing of FRP molded products easier than it is now. In particular, when the base material of the FRP is woven carbon fiber (carbon cloth), a transparent top coat is often applied to make the most of the crossing fiber pattern.

[0007] These FRP pressure vessels are cylindrical in shape, and two methods are used to manufacture them: the filament winding method, in which fibers are impregnated with epoxy resin, crossed, wound around a mandrel that serves as a core metal, and heated to harden; and the sheet winding method, in which a woven fabric is first impregnated with epoxy resin to create a semi-hardened prepreg, which is then wound like a sushi roll around a mandrel that serves as a core metal, and heated to harden.

[0008] The filament winding method can appropriately combine two types of fiber orientations, namely fiber bundles in a helical (spiral) direction of ±40 to 60 degrees and fiber bundles in a hoop (circular) direction of ±85 to 89 degrees with the long axis of the mandrel in the 0 degree direction, and the thickness of the layers, and is therefore widely used for a variety of applications, from low-pressure vessels in the ultrafiltration membrane process to high-pressure vessels in the reverse osmosis membrane process.

[0009] On the other hand, in the sheet winding method, the long axis of the mandrel is set to the 0 degree direction, the fibers in the width direction of the woven fabric are the fibers in the 0 degree direction of the pressure vessel, and the fibers in the length direction of the woven fabric are the fibers in the 90 degree direction. In the FRP molded product by this sheet winding method, the width of the woven fabric is the length of the pressure vessel (for example, 1250 mm). In this sheet winding method, the woven fabric is the fiber base material, so the fiber orientation is 0 degrees in the length direction of the pressure vessel and 90 degrees in the circumferential direction. In addition, the pressure vessel made by this sheet winding method is a cylinder with an even thickness over the entire length, and the parts that abut against the lids at the openings at both ends cannot be made thick like a clay pipe, so from the standpoint of pressure resistance, it is not suitable for pressure vessels for high-pressure reverse osmosis membrane methods and is used for pressure vessels for low-pressure ultrafiltration membrane methods.

[0010] Incidentally, when the thermosetting resin 31 such as epoxy resin used in the manufacture of FRP is heated and cured, a 10 to 30 μm inactive layer 31' that is unsuitable for bonding to other materials or painting is formed on the surface of the FRP molded product X. This inactive layer 31' becomes an obstacle when carrying out design processing (design painting or topcoat painting) later (because paint does not adhere well to the surface of the FRP molded product X), so when bonding other materials to the surface of the cured resin 31, it is necessary to remove the inactive layer 31' by surface cutting processing such as sanding or sandblasting (see Figures 6 and 7).

[0011] Also, with the filament winding method, the fibers are dense where the helical fibers overlap (for example, the intersection where fibers at +50° and -50° overlap), and the fibers are sparse in the gaps between one intersection and the next. On the other hand, with the sheet winding method, the fibers are dense where the warp and weft threads of the woven fabric intersect, and the fibers are sparse in the gaps between one intersection and the next. Therefore, with both the filament winding method and the sheet winding method, the surface of the FRP molded product is convex in the areas where the fibers overlap, and concave in the gaps between the overlapping fibers and the adjacent overlapping fibers.

[0012] In particular, in the sheet winding method, for example, carbon cloth prepreg 30 is wound around a mandrel in a sushi roll shape to produce a tubular FRP molded product X, and the inner and outer layers of this sushi roll are bonded by being cured with resin 31 that wells up from the semi-cured prepreg due to the heating and pressure of a hot roll adjacent to the mandrel, but because the resin 31 that wells up from the prepreg due to the heating and pressure of the hot roll is a viscous syrup-like substance that does not flow easily, concave depressions are likely to form in areas where the fibers 32 become coarse. Because the warp and weft threads of carbon cloth are regularly arranged, the surface of the FRP molded product X molded by the sheet winding method will have checkerboard-like depressions 33 where the open spaces between the warp and weft threads are regularly depressed.

[0013] The depth of the recesses 33 of the checkerboard pattern is 50 to 60 μm from the surface of the FRP molded product X, and can reach 70 to 80 μm in some cases, and can reach 80 μm or more depending on the molding conditions of the sheet winding method (for example, when rotating at high temperature and high speed to shorten working time) or when the resin 31 of the carbon cross prepreg 30 does not flow easily. Since paint does not adhere well to the surface of the FRP molded product X with the recesses 33 formed, similar to the inactive layer 31' described above, it is necessary to perform surface cutting processing such as sanding or sandblasting on the surface of the FRP molded product X until the recesses 33 disappear.

[0014] However, when the recesses 33 are deep, such as 80 μm, if the surface of the FRP molded product X is subjected to surface cutting processing such as sanding or sandblasting until the recesses 33 disappear in order to obtain a good paint base, the fibers 32 near the surface layer will be cut, reducing the strength and elasticity of the FRP molded product X. In the case of an FRP pressure vessel, if a surface cutting process such as sanding or blasting that cuts the fibers 32 is performed, problems such as cracks appearing in the pressure vessel during water treatment operation will occur, causing water leakage from there, making it impossible to maintain the internal pressure in the pressure vessel, reducing the water production efficiency, and in some cases causing the pressure vessel to burst and break, making it impossible to produce water using the water treatment facility.

[0015] However, if the surface cutting process such as sanding or sandblasting is limited to a level that does not cut the fibers 32 of the FRP molded product X, recesses 33 will remain on the surface of the FRP molded product X. In order to apply a design paint, for example, these recesses 33 must be removed.

[0016] Therefore, conventionally, before applying a design to the surface of this FRP molded product X, the surface of the FRP molded product X is subjected to surface cutting processing such as sanding and sandblasting to the extent that the fibers 32 are not cut, and then degreasing processing is performed (see FIG. 7), the recesses 33 are filled with a polyester resin-based putty 34, and the areas filled with this putty 34 are again surface cut to smooth out the surface of the FRP molded product X (see FIG. 8), and a design is imparted to the surface of the FRP molded product X after this unevenness adjustment.

[0017] Here, we will explain in detail the conventional surface treatment (conventional example) of FRP molded product X (cylindrical (curved surface of a cylinder) carbon cloth FRP: CFRP with a width of 1000 mm and a length of 1500 mm) from preparation of the surface base to application of a design (design painting and top coat painting).

[0018] First, a carbon cloth prepreg 30 cut into a rectangle having a width of 1000 mm and a length of 1500 mm is prepared.

[0019] The carbon cloth prepreg 30 is a cloth (woven fabric) prepreg made of 3000 carbon fiber filaments, with 3000 carbon fiber filaments, warp threads 32 and weft threads 32 both having a weave density of 12.5 threads / 25 mm and a basis weight of 198 to 200 g / m 2 The prepreg is made of a resin 31 (epoxy resin) that is heat-cured at 130 to 150°C for 1 hour using carbon cloth.

[0020] Eight sheets of this carbon cloth prepreg 30 are laminated and set in a cylindrical lower mold, the upper mold is fitted, and the mixture is heated and compressed at a temperature of 150°C and a pressure of 3 MPa. The heating and pressure are maintained for 60 minutes, and slow cooling is started after 60 minutes. The mold is opened 90 minutes after heating and compressing to obtain FRP molded product X.

[0021] Since this FRP molded product X uses carbon cloth, as described above, regular checkerboard-like recesses 33 are generated on the surface along the crossing pattern of the fibers (see FIG. 6).

[0022] Therefore, when a design is applied to the surface of this FRP molded product X (by painting the design and applying a top coat), the process proceeds as follows. Figure 9 shows a cross section of the conventional coating.

[0023] First, the surface of the FRP molded product X is cut (sanded or sandblasted) to a depth that does not cut the fibers 32, and then degreased (step 1, see FIG. 7).

[0024] Next, the recesses 33 remaining on the surface of the FRP molded product X even after the surface cutting process are filled with a putty 34 (for example, a black polyester resin-based putty). This putty 34 is hardened under the recommended hardening conditions (temperature, time) of the putty 34 used. For example, it is hardened with hot air at 40 to 60°C for 3 to 6 hours or at room temperature for one day, and after hardening, the convex parts on the surface of the FRP molded product X are sanded with, for example, #240 sandpaper, and unevenness is adjusted so that the surface to be painted with the design is roughly flat without extreme protrusions (step 2, see FIG. 8). Note that in this step 2, when hardening the putty 34 and drying and hardening the paint, if the temperature is, for example, 80°C or higher, the drying and hardening time will be shortened, but microcracks will occur in the putty 34 and paint, and peeling will occur from the surface of the FRP molded product X, so it is desirable to harden the putty 34 and dry and harden the paint at a low temperature, for example, 60°C or lower. If the temperature is lowered, the drying and curing time will be longer.

[0025] Next, a clear paint for forming an undercoat layer 41 is applied to the surface of the FRP molded product X after unevenness adjustment with a spray gun to a thickness of 25 to 30 μm, and the paint is dried and hardened, for example, at 40° C. for half a day to a day (step 3).

[0026] The undercoat layer 41 is formed to a thickness of 25 to 30 μm for the purpose of obtaining adhesion to the base material of the surface of the FRP molded product X after unevenness adjustment and corrosion resistance to alkali and acid of the surface of the FRP molded product X. At the same time, adhesion to the intermediate coat layer 42 described below is obtained.

[0027] Next, a clear paint for forming an intermediate coat layer 42 is applied to the surface of the undercoat layer 41 with a spray gun to a thickness of 40 to 45 μm, and the paint is dried and cured, for example, at 40° C. for half a day to a day (step 4).

[0028] The intermediate coat layer 42 is formed to a thickness of 40 to 45 μm for the purposes of maintaining the smoothness of the undercoat layer 41 and obtaining impact resistance for the entire coating. At the same time, it obtains adhesion with the topcoat layer 44 described below. When design painting (or design printing) is performed, it is applied on top of the intermediate coat layer 42. The intermediate coat layer 42 also serves the purpose of forming a smooth base for design painting or design printing.

[0029] Next, when pearlescent coating is used as a design coating, it is formed to a thickness of 15 to 20 μm on the surface of the intermediate coating layer 42 after the intermediate coating layer 42 is formed. This design coating layer (design layer 43) is also dried and hardened, for example, at 40° C. for half a day to a day, like the other layers (step 5).

[0030] In addition to painting the design, the brand name or design may be silk-screened or a sticker may be affixed to the product.

[0031] Next, a clear paint forming topcoat layer 44 is applied to the surface of design layer 43 with a spray gun to a thickness of 40 to 45 μm, and the paint is dried and cured, for example, at 40° C. for half a day to a day (step 6).

[0032] In addition, in step 6, as shown in FIG. 10, there may be a case where a topcoat layer 44 is formed on the surface of the intermediate coat layer 42 without forming a design layer 43. In this case, in order to make use of the raw surface design (crossing fiber pattern) of the FRP molded product X, a transparent top coat is directly applied to the surface of the FRP molded product X without applying a design paint.

[0033] Furthermore, if necessary, a clear paint to form a second topcoat layer (not shown) is applied to the surface of the topcoat layer 44 with a spray gun to a thickness of 40 to 45 μm, and the paint is dried and hardened, for example, at 40° C. for half a day to a day (step 7).

[0034] This overcoat layer 44 is the above-mentioned topcoat coating, and is formed to a thickness of 40 to 90 μm for the purposes of maintaining gloss, improving aesthetics, scratch resistance, weather resistance, and stain resistance.

[0035] As described above, the surface of the FRP molded product X is painted through the above-mentioned steps, and there is a demand to simplify this surface painting process, which involves many steps. Summary of the Invention [Problem to be solved by the invention]

[0036] The present invention has been invented in view of the above-mentioned conventional demands, and provides a highly practical glass paper prepreg and a method for manufacturing the same that have never been available before, such as by enabling surface treatment to be performed on the surface of an FRP molded product without adjusting the surface unevenness. Fiber Reinforced Plastic The present invention provides a method for producing the above-mentioned compound. [Means for solving the problem]

[0037] The gist of the present invention will now be described with reference to the accompanying drawings.

[0038] Laminated on a glass unidirectional prepreg or a carbon unidirectional prepreg, or a glass cloth prepreg or a carbon cloth prepreg 30 , heated and pressurizedThe glass paper prepreg is used to form fiber-reinforced plastics, and the glass paper prepreg 1 is formed by impregnating glass paper 2 with resin 3, the content of resin 3 being 60 wt% or more, and the resin flow calculated from the following formula 1 being set to 40% or more. Resin flow (%) = amount of resin 3 that flows out after pressing (g) / weight of prepreg before pressing (g) Equation 1

[0039] The glass paper prepreg described in claim 1 is characterized in that the resin impregnated into the glass unidirectional prepreg or the carbon unidirectional prepreg, or the glass cloth prepreg or the carbon cloth prepreg 30, and the resin 3 impregnated into the glass paper prepreg 1 are both thermosetting resins.

[0040] Also, claims 1st article In the above glass paper prepreg, Impregnated into glass paper prepreg 1 The present invention relates to a glass paper prepreg characterized in that the resin 3 used is a mixture of a thermoplastic resin and a thermosetting resin in a compounding ratio (mass % ratio) of 15:85 to 35:65.

[0041] The present invention also relates to a glass paper prepreg as described in claim 3, characterized in that a phenoxy resin is used as the thermoplastic resin and a urethane acrylate resin is used as the thermosetting resin.

[0042] Also, claim 1 ~4 Select one of the following In the glass paper prepreg described, the resin 3 is continuously coated by a coating machine, and the tensile strength of the glass paper 2 is 15 N / 15 mm or more in one direction and 4 N / 15 mm or more in another direction perpendicular to the one direction.

[0043] In addition, the glass paper 2 that is pulled out from the wound state is passed through a resin impregnation tank section 12 that contains resin 3 to be impregnated with the resin 3, and then the resin-impregnated glass paper 2 that has passed through the resin impregnation tank section 12 is passed through a heating section 13 to semi-cure the resin 3, and the glass paper prepreg 1 in which the content of the resin 3 is set to 60 wt% or more and the resin flow calculated from the following formula 1 is set to 40% or more is produced. Laminated on a glass unidirectional prepreg or a carbon unidirectional prepreg, or a glass cloth prepreg or a carbon cloth prepreg 30 The present invention relates to a method for producing fiber-reinforced plastic, which comprises molding the fiber-reinforced plastic by applying heat and pressure. Resin flow (%) = amount of resin 3 that flows out after pressing (g) / weight of prepreg before pressing (g) Equation 1

[0044] In addition, in the method for producing fiber-reinforced plastic described in claim 6, the resin impregnated into the unidirectional glass prepreg or the unidirectional carbon prepreg, or the glass cloth prepreg or the carbon cloth prepreg 30, and the resin 3 impregnated into the glass paper prepreg 1 are both thermosetting resins.

[0045] Also, claims Book 6 Posted Manufacturing method of fiber reinforced plastic In the above Impregnated into glass paper prepreg 1 The resin 3 is a mixture of a thermoplastic resin and a thermosetting resin in a blending ratio (mass % ratio) of 15:85 to 35:65. Manufacturing method of fiber reinforced plastic This relates to:

[0046] Also, claims 8 Described Manufacturing method of fiber reinforced plastic The thermoplastic resin is a phenoxy resin, and the thermosetting resin is a urethane acrylate resin. Manufacturing method of fiber reinforced plastic This relates to:

[0047] Also, claims Select one of items 6 to 9 Described Manufacturing method of fiber reinforced plastic The glass paper 2 has a tensile strength of 15 N / 15 mm or more in one direction and 4 N / 15 mm or more in another direction perpendicular to the one direction. Manufacturing method of fiber reinforced plastic This relates to: Effect of the Invention

[0048] Since the present invention is configured as described above, it is possible to perform surface treatment on the surface of an FRP molded product without adjusting the unevenness, and thus it is possible to provide a highly practical glass paper prepreg and Fiber Reinforced Plastic This is the manufacturing method. [Brief description of the drawings]

[0049] [Figure 1] FIG. 2 is a perspective view showing a glass paper prepreg and a carbon cloth prepreg according to Example 1. [Diagram 2] FIG. 2 is an explanatory diagram for explaining the production of the glass paper prepreg according to Example 1. [Diagram 3] 1 is a table showing the measurement results confirming the performance of Example 1 and the comparative example. [Figure 4]2 is a cross-sectional view illustrating a surface-treated portion of the FRP molded product A according to Example 1. FIG. [Diagram 5] 5 is a cross-sectional view illustrating the refraction of light at a surface-treated portion of the FRP molded product A according to Example 2. FIG. [Figure 6] FIG. 1 is a cross-sectional view illustrating an FRP molded product X molded by a conventional manufacturing method. [Figure 7] FIG. 1 is a cross-sectional view illustrating an FRP molded product X molded by a conventional manufacturing method. [Figure 8] FIG. 1 is a cross-sectional view illustrating an FRP molded product X molded by a conventional manufacturing method. [Figure 9] 1 is a cross-sectional view illustrating a surface-treated portion of an FRP molded product X molded by a conventional method. [Figure 10] 1 is a cross-sectional view illustrating the refraction of light at a surface-treated portion of an FRP molded product X molded by a conventional method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0050] A preferred embodiment of the present invention will be briefly described below with reference to the drawings to illustrate the operation of the present invention.

[0051] When a sheet of glass paper prepreg 1 according to the present invention is laminated on top of a unidirectional glass prepreg or a unidirectional carbon prepreg, or a glass cloth prepreg or a carbon cloth prepreg 30, and a fiber reinforced plastic (FRP molded product A) is molded, a layer having a flat surface without any recesses is formed on the surface of this FRP molded product A.

[0052] The glass paper 2 used in the present invention is impregnated with a large amount of resin 3, and the viscosity of the resin 3 decreases when heated and pressurized during molding. The resin 3 has an appropriate resin flow that allows it to completely cover the recesses in the FRP molded product A. After the resin 3 flows, its viscosity increases and it hardens in a state where it has completely covered the recesses, forming a layer with a flat surface without any recesses.

[0053] The glass paper 2 has a tensile strength of, for example, 15 N / 15 mm or more in one direction and 4 N / 15 mm or more in the other direction perpendicular to the one direction, so that the glass paper 2 can be continuously coated with resin 3 without breaking during the coating process.In addition, when the glass paper 2 is impregnated with resin 3 to form a glass paper prepreg, the optimal resin content and resin flow can be set stably and continuously.

[0054] Therefore, without the need for conventional unevenness adjustment on the surface of the FRP molded product A obtained by the present invention, it is possible to paint a design on the flat layer formed on the surface of this FRP molded product A, and then paint this design-painted surface with a transparent top coat as a protective layer. In other words, the layer formed on the surface of this FRP molded product A when it is molded serves as an optimal base for applying a design such as painting or printing.

[0055] Furthermore, the layer formed on the surface of this FRP molded product A is a clear, colorless, transparent layer, because the glass paper 2 becomes transparent by being impregnated with the resin 3.

[0056] In other words, the unfinished surface design (crossing fiber pattern) of FRP molded product A can be seen through this transparent layer.

[0057] Therefore, this transparent layer itself functions as a protective layer, and there is no need to form a protective layer by applying multiple layers as in the conventional method. EXAMPLES

[0058] A first specific embodiment of the present invention will be described with reference to the drawings.

[0059] As shown in FIG. 1, this embodiment is a glass paper prepreg 1 for forming a fiber-reinforced plastic (FRP molded product A / FRP pressure vessel) by laminating it on a unidirectional glass prepreg or a unidirectional carbon prepreg, or a glass cloth prepreg or a carbon cloth prepreg 30. As shown in FIG. 4, this FRP molded product A has a two-phase layer structure consisting of a layer A1 composed of a carbon cloth prepreg 30 and a layer A2 (a fiber base material layer in the form of a nonwoven fabric with anisotropic fiber orientation) composed of the glass paper prepreg 1 provided on this layer A1.

[0060] The carbon cloth prepreg 30 used in this embodiment is a cloth (woven fabric) prepreg made of 3000 carbon fiber filaments, as in the conventional case described above. The carbon fiber has 3000 filaments, and both the warp threads 32 and the weft threads 32 have a weave density of 12.5 threads / 25 mm and a basis weight of 198 to 200 g / m. 2 The prepreg is made of epoxy resin 31 having the characteristic of being heat-cured at 130 to 150°C for 1 hour using carbon cloth.

[0061] In this embodiment, an FRP pressure vessel is used as the FRP molded product A, but any other product that exhibits the characteristics of this embodiment may be used as appropriate.

[0062] The glass sheet prepreg 1 according to this embodiment will be described below.

[0063] This glass sheet prepreg 1 is made by coating glass paper 2 with resin 3, and in this embodiment, a vertical coating machine is used for coating the prepreg.

[0064] 2, this vertical coating machine has a glass paper delivery section 10 that delivers the rolled glass paper 2 before prepreg processing, and a glass paper prepreg take-up section 11 that winds up the prepreg-processed glass paper prepreg 1, between which are provided a resin impregnation tank section 12 for impregnating the glass paper 2 with resin 3, and a heating section 13 (semi-curing zone) through which the resin-impregnated glass paper 2 that has passed through the resin impregnation tank section 12 passes vertically up and down to heat and semi-cure the resin 3 impregnated in the glass paper 2. Reference numeral 14 denotes a tension roller.

[0065] In this embodiment, the glass paper delivery section 10 has a unit weight of 25 g / m 2 A roll of glass paper 2 having a width of 1,040 mm and a length of 100 m is set, the glass paper 2 is then passed through a resin impregnation tank section 12 to be impregnated with resin 3, the resin-impregnated glass paper 2 which has passed through the resin impregnation tank section 12 is then passed through a heating section 13 to semi-cure the resin 3 to form a glass paper prepreg 1, and this glass paper prepreg 1 is then taken up by a glass paper prepreg take-up section 11 to perform continuous prepreg coating.

[0066] In addition, in this embodiment, the glass paper 2 used has a tensile strength of 15 N / 15 mm in the length direction (vertical direction) and 4 N / 15 mm in the width direction (horizontal direction), and is anisotropic glass paper 2 in which the strength is higher in the length direction than in the width direction.

[0067] In this embodiment, the resin 3, which is a mixture ratio (mass %) of phenoxy resin as a thermoplastic resin and urethane acrylate resin as a thermosetting resin disclosed in Japanese Patent Application No. 2018-37390 of 15:85, or a resin containing 100% urethane acrylate resin, is stored in the resin impregnation tank 12. Note that, in addition to this, an epoxy resin having the characteristics of curing at 130 to 150°C for 1 hour, similar to the resin 31 used in the carbon cloth prepreg 30 described above, such as an epoxy resin made of an epibis-based liquid epoxy as a base agent and dicyandiamide as a curing agent, may also be used.

[0068] As a method for impregnating the glass paper 2 with the resin 3, an impregnation method in which the entire glass paper 2 is immersed in the resin impregnation bath section 12 as in this embodiment (called a dipping method) is preferable.

[0069] That is, in addition to the dipping method, there is also an impregnation method (called the hot melt method) in which heated and molten resin is forced into one side of the fiber base material using the pressure of a roll or press plate, and the temperature and pressure of the next prepreg process, the press molding process or autoclave molding process, are used to fully impregnate the fiber base material.However, in order to achieve the effect of eliminating the need for unevenness adjustment for the paint base, the dipping method, in which sufficient resin impregnation is achieved at the prepreg coating stage, is preferred.

[0070] In this embodiment, the heating temperature of the prepreg heating section 13 of the vertical coater is set to 150°C, but the temperature of the heating section 13 and the coating speed are appropriately determined according to the length and heating capacity of the heating section 13 and the gel time of the resin so that the obtained prepreg is at a desired semi-cured level. For example, the temperature of the heating section 13 may be increased from 150°C to 180°C, while keeping an eye on the residence time in the heating section 13, the gel time of the resin 3, and the semi-cured state of the resin 3 impregnated in the prepreg after passing through the heating section 13. In this embodiment, a vertical coater in which the path of the heating section 13 is vertical is described, but a horizontal coater in which the heating section 13 is horizontal may be applied to prepreg coating.

[0071] Furthermore, when coating the prepreg, the inventors tried glass paper 2 with a tensile strength of 15 N / 15 mm or less in the length direction (vertical direction) and 4 N / 15 mm or less in the width direction (horizontal direction), but the forward tension and back tension during the prepreg coating caused the glass paper to tear in the length direction and width direction, making continuous coating impossible.

[0072] Therefore, it is desirable that the tensile strength of the glass paper 2 used in this prepreg coating (continuous coating of the resin 3 by a coating machine) is 15 N / 15 mm or more in the length direction (vertical direction) and 4 N / 15 mm or more in the width direction (horizontal direction) (resulting in anisotropy). In this continuous coating, the tensile strength of the glass paper 2 may be 15 N / 15 mm in the length direction (vertical direction) and 15 N / 15 mm in the width direction (horizontal direction) (resulting in isotropy).

[0073] Incidentally, the glass paper prepreg 1 is impregnated with the resin 3 and is in a semi-cured state, and this semi-cured state is determined by the resin flow of the prepreg.

[0074] Specifically, the obtained prepreg is cut to a set size (for example, 200 mm square), and the entire prepreg is press molded in a press molding machine at a set temperature and pressure (for example, a temperature of 150°C and a pressure of 0.3 MPa, which are sufficient to cure the resin blend), and the degree of semi-curing is determined by the amount of resin that flows after molding. With this method of determination, the glass paper 2, whose fibers are intricately intertwined in the base material, does not flow with the resin and remains there.

[0075] If the degree of semi-curing is close to cured, the resin will not flow easily, and if it is close to uncured, the resin will flow easily, so the state of semi-curing can be measured by the state in which the resin flows out and spreads (resin flow).

[0076] The degree of semi-curing is determined by the percentage of the weight of this flowed-out resin to the weight of the prepreg before it flowed out, and the percentage calculated using the following formula is called the resin flow.

[0077] Resin flow FL (%) = amount of resin flowing out after pressing: F (g) / weight of prepreg before pressing: W (g) Equation 1 Amount of resin that flows out after pressing: F(g) = Weight of prepreg before pressing W1(g) - Weight of FRP board after resin flows out after pressing W2(g) Equation 2 Substitute F from Equation 2 into Equation 1 to obtain the resin flow.

[0078] In this embodiment, various prototypes were made by varying the prepreg coating conditions of the vertical coater (e.g., coating speed, viscosity of resin 3, temperature setting of heating section 13, etc.) to obtain a glass paper prepreg 1 with a resin content of 80 wt% and a resin flow of 50%, and one sheet of this glass paper prepreg 1 with a resin content of 80 wt% and a resin flow of 50% was prepared with a width of 1000 mm and a length of 1500 mm.

[0079] On the other hand, the carbon cloth prepreg 30 with the resin content of 35 wt% mentioned above (carbon fiber 3000 filament, warp and weft weaving density 12.5 threads / 25 mm, basis weight 198 to 200 g / m 2 Prepare eight pieces of prepreg (made of carbon cloth and epoxy resin that hardens at 130-150℃ for 1 hour) measuring 1000mm wide and 1500mm long.

[0080] Eight sheets of this carbon cloth prepreg 30 were laminated, and one sheet of glass paper prepreg 1 was laminated on the top layer of the eight sheets of carbon cloth prepreg 30. This laminate was set in a cylindrical lower mold having a width of 1000 mm and a length of 1500 mm, and the upper mold was fitted over it. The laminate was then heated and pressed at a temperature of 150°C and a pressure of 3 MPa. The heating and pressure application was maintained for 60 minutes, and slow cooling was started after 60 minutes. 90 minutes after heating and pressing, the mold was released to provide FRP molded product A.

[0081] This FRP molded product A had a smooth surface without any checkerboard-like recesses, and was a cylindrical molded product with a thickness of 1.9 to 1.95 mm.

[0082] When the cross section of this FRP molded product A was observed under a microscope, it was found that layer A1 composed of carbon cloth prepreg 30 and layer A2 composed of glass paper prepreg 1 provided on top of layer A1 were integrated and well bonded, with layer A1 composed of carbon cloth prepreg 30 being 1.72 to 1.8 mm thick and layer A2 composed of glass paper prepreg 1 being 0.15 to 0.18 mm thick.

[0083] Next, the surface of this cylindrical FRP molded product A (surface of layer A2) was sandblasted to a depth of 40 to 60 μm for the purposes of removing the inactive layer specific to FRP and for the purposes of providing a design for the next process.

[0084] In this embodiment, since the molded surface was cylindrical, sandblasting was performed, but sanding can also be performed if the FRP molded product A is flat or cylindrical, as long as a sanding machine that can handle this is available.

[0085] Not only was there no depression on the surface of the FRP molded product A after sandblasting, but when the cross section of the FRP molded product A after sandblasting was observed under a microscope, it was found that layer A2 of the surface glass paper prepreg 1 remained, and there were no areas where the carbon fibers of layer A1 of the carbon cloth prepreg 30 had been cut.

[0086] Therefore, the surface of the FRP molded product A after the sandblasting process can be subjected to the above-mentioned process of forming the undercoat layer 41 in step 3 or the process of forming the design layer 43 in step 5 without any need for surface preparation. The adhesion of this undercoat layer 41 was excellent, scoring 10 points in the cross-cut test according to JIS K5600.

[0087] Here, as the present embodiment, a flat plate was press-molded by laminating one glass paper prepreg 1 on the top layer of an eight-ply laminate of carbon cloth prepregs 30, and the surface layer (the surface layer on the glass paper prepreg side) of the flat plate was sandblasted. As a comparative example, a flat plate was press-molded using only an eight-ply laminate of carbon cloth prepregs 30, and the surface layer of the flat plate was sandblasted until all recesses disappeared. The bending strength and bending modulus of elasticity of both plates were measured using the test method of JIS K7074 with the sandblasted surface facing up, and the respective values ​​are shown in the table in FIG. 3.

[0088] In the comparative example, when sandblasting was performed until the recesses disappeared, a 19.5% decrease in bending strength and an 8.3% decrease in bending modulus were observed.

[0089] In addition, in the comparative example, partial breaks in the carbon fibers on the surface were visible to the naked eye, whereas in this example, even though sandblasting was performed to a depth of 40 to 60 μm, layer A2 of the surface glass paper prepreg 1 remained and the carbon fibers were not cut, so it is believed that there was no decrease in the strength and elastic modulus of the FRP molded product A.

[0090] In addition, in this embodiment, one sheet of glass paper prepreg 1 is laminated, but if the storage life of the carbon cloth prepreg 30 is approaching and the resin flow of the carbon cloth prepreg 30 is lower than when it was fresh, two sheets of glass paper prepreg 1 may be laminated.

[0091] Specifically, when the glass paper 2 is one sheet (one layer), it is desirable that the glass paper prepreg 1 has a resin content of 70 wt % or more and a resin flow of 40% or more.

[0092] In the inventors' experiments, when a glass paper prepreg 1 had a resin content of 70 wt% or less and a resin flow of 40% or less, and when there was only one sheet of glass paper 2, checkerboard-shaped depressions sometimes appeared in parts of the surface of the FRP molded product A.

[0093] Furthermore, when there are two sheets (two layers) of glass paper 2, the resin content of the glass paper prepreg 1 does not need to be 70 wt% or more, and it has been confirmed that it is better to make the resin content 60 wt% or more and to laminate two sheets with a resin flow of 40% or more.

[0094] Furthermore, when there are three or more sheets (three layers) of glass paper 2, it is preferable to laminate three or more sheets of glass paper prepreg 1 having a resin content of 60 wt% or more and a resin flow of 40% or more, just as when there are two sheets (two layers) of glass paper 2.

[0095] In the present embodiment, the carbon cloth prepreg 30 uses a cloth (woven fabric) prepreg made of 3,000 carbon fiber filaments. However, if, for example, a cloth (woven fabric) made of 12,000 carbon fiber filaments is used for the carbon cloth prepreg 30, the carbon fibers will be thicker than those of 3,000 filaments, and the fibers will be denser at the intersections of the warp and weft threads of the woven fabric and the fibers will be more sparse in the gaps between one intersection and the next. Therefore, in order to eliminate recesses on the surface of the FRP molded product A after sandblasting, to leave layer A2 of the surface glass paper prepreg 1, and to avoid cutting the carbon fibers, it is sufficient to use multiple sheets of glass paper 2 (multilayers).

[0096] 4, in the FRP molded product A, a layer A2 made of glass paper prepreg 1 is used as a base, and a design paint layer (design layer 43) is formed on the surface of this layer in the above-mentioned step 5, and further, a top coat layer 44 in the above-mentioned step 6 is formed on the surface of this design layer 43. In addition to the design paint, a brand name or design may be silk-screened or a sticker may be attached to impart a design.

[0097] Therefore, the FRP molded product A produced according to this embodiment does not require steps 1 to 4.

[0098] Since this embodiment is configured as described above, surface processing of the FRP molded product A can be easily performed, such as by directly applying design painting or printing to the surface of the FRP molded product A without adjusting the surface unevenness.

[0099] In Example 1, press molding using an upper and lower mold was described, but autoclave molding using only an upper mold or only a lower mold also enables surface processing of the FRP molded product A to be easily performed, such as by directly applying design paint or printing without adjusting for unevenness.

[0100] In Example 1, the carbon cloth prepreg 30 is used for explanation, but the surface processing of the FRP molded product A can be easily performed by directly applying design painting or design printing to a glass cloth prepreg, or a unidirectional glass prepreg, or a unidirectional carbon prepreg, without adjusting for unevenness. EXAMPLES

[0101] A second specific embodiment of the present invention will be described with reference to the drawings.

[0102] In this embodiment, as shown in FIG. 5, no design layer or topcoat layer is formed on layer A2 made of glass paper prepreg 1, and this layer A2 is used as a topcoat layer (protective layer) through which the unfinished surface design (cross-fiber pattern) of FRP molded product A can be seen; the other configurations are the same as in Example 1.

[0103] Conventionally, when making the raw surface design (a design of crossed fibers) of an FRP molded product A transparently visible, after the molding process as described above, a topcoat layer is formed on the surface through steps 1 to 7 (in this case step 5 is not performed).

[0104] In the process described above, it was said that only the topcoat may be applied in two layers, but the undercoat and intermediate coat may also be applied twice, with each layer being thinner, to avoid microcracks and peeling from the lower layer due to cure shrinkage during drying and hardening, so in reality, many processes and man-hours are required to complete the painting.

[0105] Specifically, for example, if the topcoat layer is 80 μm thick, trying to apply it in one coat will result in a discrepancy in the dryness state of the surface and the interior, resulting in the surface being dry while the interior is wet, and the paint film being pulled toward the surface during drying, which can lead to cracks and fissures.

[0106] Also, depending on the drying conditions, the surface of the coating may become matte. Cracks, crevices, and matte surfaces in the coating will cause the coating to lose its transparency, and the cross-pattern of the fibers will no longer be clearly visible. Therefore, clear coating that allows the cross-pattern of the fibers to be seen is applied thinly once, then polished with #1000 paper to improve smoothness, and the drying and application process is repeated several times to create a thick coat. However, clear coating that allows the cross-pattern of the fibers to be seen is quite costly in terms of both materials and labor, including the drying time of the paint, and the number of days, drying equipment, painting, and management of drying conditions.

[0107] Conventionally, in order to make the cross-pattern of fibers visible through the paint, the undercoat, intermediate coat, and top coat all need to be transparent. Also, for example, if the paint dries too quickly and a hardened film (interface film) is formed at the interface between the undercoat and intermediate coat or between the intermediate coat and top coat, birefringence or double reflection occurs at the interface (for example, the interface between the top coat and intermediate coat) as shown in Figure 10, and the cross-pattern of fibers may become blurred or appear as a double image.

[0108] In particular, the surface of the above-mentioned topcoat layer 44 needs to be smooth enough that the reflection of the fluorescent light can be seen as a straight tubular fluorescent light. In steps 6 and 7 for forming this topcoat layer 44, care must be taken with how it is applied and dried so that the tubular reflection of the fluorescent light does not appear jagged.

[0109] In addition, when the painted surface of an FRP molded product has a U-shaped cross section and is both horizontal and vertical, the paint film tends to be thick on the horizontal surfaces and the paint film tends to sag on the vertical surfaces, so consideration must be given to the horizontal and vertical surfaces of the paint. If this is to be formed with a clear coat, there will be double refraction and double reflection at the paint interface in the dry state, so even more consideration must be given to the drying area and drying conditions.

[0110] In this regard, according to this embodiment, the surface layer (the transparent layer obtained by the glass paper prepreg) through which the cross fiber pattern is transparently visible is a single layer, and therefore no birefringence or double reflection occurs at the interface (for example, the interface between a top coat and an undercoat such as in painting), and the cross fiber pattern does not become blurred or appear as a double image.

[0111] Furthermore, because this protective layer is formed on the mirror surface of the upper part of the metal mold, it is smooth enough that the reflection of the fluorescent light can be seen as a straight tube. There is no need to pay attention to the painting and drying methods, as in steps 6 and 7, where the clear coating is applied, to prevent the tubular reflection of the fluorescent light from becoming jagged.

[0112] Furthermore, even if the painted surfaces of an FRP molded product have a U-shaped cross section and are both horizontal and vertical, a transparent layer is obtained using the glass paper prepreg by molding it using a mold, so there is no need to worry about the paint film becoming thicker on horizontal surfaces or the paint film becoming more prone to dripping on vertical surfaces, as occurs with painting (see Figure 5).

[0113] The surface layer through which the crossed fiber pattern can be seen transparently (referring to the transparent layer A2 obtained from the glass paper prepreg 1, which is called the top coat layer) can be obtained by omitting all of the above-mentioned steps 1 to 7.

[0114] As described above, there is a large difference between Example 2 and the conventional example in the number of days required for the process and the attention paid to each process in order to make the mesh of the carbon cloth stand out transparently.

[0115] That is, in Example 2, a transparent topcoat layer is obtained at the same time as molding the FRP molded product A. When FRP is molded in a mold, the resin of the glass paper prepreg and the resin of the carbon cloth prepreg that form the topcoat layer are both thermosetting resins, and when heated, the respective resins flow out in a liquid form and become compatible with each other and harden, resulting in good adhesion at the interface between the carbon cloth FRP layer and the glass paper FRP layer.

[0116] In addition, as explained in the method for determining resin flow, glass paper 2, whose base material fibers are intricately intertwined, has the characteristic that the fibers do not flow with the resin but remain there. Therefore, when the glass fibers of glass paper 2 are in contact with the carbon fibers of the carbon cloth, the carbon fibers are held down by the glass fibers of glass paper 2 and are not washed away by the flow of resin in the carbon cloth prepreg, so the mesh of the carbon cloth does not become misaligned and the warp and weft threads are kept neatly perpendicular to each other.

[0117] In addition, the outermost layer, which requires careful painting, is a transfer of the surface of the mold in this embodiment, so there is no need to pay attention to the painting method, drying method, or finishing method, as in the case of painting, in order to prevent the tubular reflection of the fluorescent light from becoming jagged. Also, in the embodiment of this application, the top coat layer is a single layer of a single material, prepreg made of glass paper, so birefringence and birefringence that occur with clear coating do not occur.

[0118] In the conventional example, after the molding of the FRP molded product X, the process proceeds while paying careful attention to the coating thickness, drying, and hardening, and a transparent top coat layer is finally obtained through surface preparation (unevenness adjustment), undercoating, intermediate coating, and top coating. There are significant differences between the examples of the present application and the conventional example in terms of process (e.g., the number of days required) and quality control (e.g., painting work to improve the surface condition of the coating and control of paint drying conditions).

[0119] This example has been described using the cross pattern of carbon fibers in the FRP molded product A using carbon cloth prepreg 1, but a transparent top coat layer can also be applied to an FRP molded product using glass cloth prepreg, allowing the cross pattern of the glass fibers to stand out transparently.

[0120] Similarly, a transparent topcoat layer can be applied to FRP molded products made of unidirectional glass prepregs or unidirectional carbon prepregs, allowing the unidirectional or crossed fiber patterns to stand out transparently.

[0121] In addition, the transparent topcoat layer made of the glass paper prepreg 1 in the present embodiment is hardened by the combination of resin and hardener, and is not a paint in which the contained organic solvent is dried, so that a surface layer with excellent chemical resistance and scratch resistance can be obtained.

[0122] In this embodiment, as in embodiment 1, one glass paper prepreg 1 is laminated, but if the storage life of the carbon cloth prepreg 30 is approaching and the resin flow of the carbon cloth prepreg 30 is lower than when it was fresh, two glass paper prepregs 1 may be laminated.

[0123] Specifically, when the glass paper 2 is one sheet (one layer), it is desirable that the glass paper prepreg 1 has a resin content of 70 wt % or more and a resin flow of 40% or more.

[0124] In the experiments conducted by the inventors, when a glass paper prepreg 1 having a resin content of 70 wt% or less and a resin flow of 40% or less was used with one sheet of glass paper 2, checkerboard-shaped depressions occurred in some parts of the surface of the FRP molded product A, causing the tubular reflection of the fluorescent lamp to appear jagged.

[0125] Furthermore, it has been confirmed that when there are two sheets (two layers) of glass paper 2, it is good to laminate two sheets of glass paper prepreg 1 having a resin content of 60 wt % or more and a resin flow of 40% or more.

[0126] When there are three or more sheets (three layers) of glass paper 2, it is preferable to laminate three or more sheets of glass paper prepreg 1 with a resin content of 60 wt% or more and a resin flow rate of 40% or more, just as in the case of two sheets (two layers) of glass paper 2. This makes it possible to obtain a smooth topcoat layer that prevents jagged reflections from the tubular shape of the fluorescent lamp.

[0127] In the present embodiment, the carbon cloth prepreg 30 uses a cloth (woven fabric) prepreg made of 3,000 carbon fiber filaments. However, if, for example, a cloth (woven fabric) made of 12,000 carbon fiber filaments is used for the carbon cloth prepreg 30, the carbon fibers will be thicker than those of 3,000 filaments, and the fibers will be denser at the intersections of the warp and weft threads of the woven fabric and the fibers will be more sparse in the gaps between one intersection and the next. Therefore, in order to obtain a smooth topcoat layer on the surface of the FRP molded product A that is free of checkerboard-like depressions and does not cause jagged tubular reflections of fluorescent lamps, it is sufficient to use multiple sheets of glass paper 2 (multilayers).

[0128] Since this embodiment is configured as described above, the unfinished surface design of the FRP molded product A (the crossing pattern of fibers) can be seen through the transparent layer formed when the FRP molded product A is molded, and this layer functions as a protective layer, eliminating the need to apply multiple layers to form a protective layer as in the past, and making it easy to process the surface of the FRP molded product A.

[0129] Since Example 2 has the same configuration as Example 1, the explanation has been given in the case of press molding using an upper and lower mold, but the same applies to autoclave molding using only an upper mold or only a lower mold. The unfinished surface design of FRP molded product A (the crossing pattern of fibers) can be seen through the transparent layer formed when FRP molded product A is molded, and this layer functions as a protective layer, making it unnecessary to apply multiple layers to form a protective layer as in the past, and thus simplifying the surface processing of FRP molded product A.

[0130] Since Example 2 has the same configuration as Example 1, it has been explained using carbon cross prepreg 30, but the same can be said for glass cross prepreg, glass unidirectional prepreg, or carbon unidirectional prepreg. The unfinished surface design of the FRP molded product A (the crossed fiber pattern, unidirectional in the case of a cross prepreg) can be seen through the transparent layer formed when the FRP molded product A is molded, and this layer functions as a protective layer, making it unnecessary to form a protective layer by applying multiple layers as in the past, and thus facilitating surface processing of the FRP molded product A. [Explanation of symbols]

[0131] 1. Glass paper prepreg 2. Glass Paper 3. Resin 12 Resin impregnation tank section 13 Heating section 30 Carbon cloth prepreg

Claims

1. A glass paper prepreg for forming a fiber reinforced plastic by layering on a unidirectional glass prepreg or a unidirectional carbon prepreg, or a glass cloth prepreg or a carbon cloth prepreg 30 and heating and pressing the same, the glass paper prepreg being made by impregnating glass paper with a resin, the resin content being 60 wt % or more, and the resin flow calculated from the following formula 1 being set to 40% or more. Resin flow (%) = amount of resin 3 flowing out after pressing (g) / weight of prepreg before pressing (g) ... Equation 1

2. A glass paper prepreg as described in claim 1, characterized in that the resin impregnated into the glass unidirectional prepreg or the carbon unidirectional prepreg, or the glass cloth prepreg or the carbon cloth prepreg, and the resin impregnated into the glass paper prepreg are both thermosetting resins.

3. The glass paper prepreg according to claim 1, characterized in that the resin impregnated into the glass paper prepreg is a resin obtained by mixing a thermoplastic resin and a thermosetting resin in a compounding ratio (mass % ratio) of 15:85 to 35:

65.

4. 4. The glass paper prepreg according to claim 3, wherein the thermoplastic resin is a phenoxy resin, and the thermosetting resin is a urethane acrylate resin.

5. The glass paper prepreg according to any one of claims 1 to 4, characterized in that the resin is continuously coated by a coating machine, and the tensile strength of the glass paper is 15 N / 15 mm or more in one direction and 4 N / 15 mm or more in another direction perpendicular to the one direction.

6. A method for producing fiber reinforced plastic, comprising: passing glass paper pulled out from a wound state through a resin impregnation tank section containing resin to impregnate the glass paper with the resin; subsequently, passing the resin-impregnated glass paper which has passed through the resin impregnation tank section through a heating section to semi-harden the resin; laminating this glass paper prepreg, the resin content of which is set to 60 wt% or more and the resin flow calculated from the following formula 1 is set to 40% or more, on top of a glass unidirectional prepreg or a carbon unidirectional prepreg, or a glass cloth prepreg or a carbon cloth prepreg, and heating and pressurizing the resulting product to form a fiber reinforced plastic. Resin flow (%) = amount of resin 3 flowing out after pressing (g) / weight of prepreg before pressing (g) ... Equation 1

7. A method for producing fiber-reinforced plastics as described in claim 6, characterized in that the resin impregnated into the unidirectional glass prepreg or the unidirectional carbon prepreg, or the glass cloth prepreg or the carbon cloth prepreg, and the resin impregnated into the glass paper prepreg are both thermosetting resins.

8. The method for producing fiber-reinforced plastics according to claim 6, wherein the resin impregnated into the glass paper prepreg is a resin obtained by mixing a thermoplastic resin and a thermosetting resin in a blending ratio (mass % ratio) of 15:85 to 35:

65.

9. 9. The method for producing fiber-reinforced plastics according to claim 8, wherein a phenoxy resin is used as the thermoplastic resin, and a urethane acrylate resin is used as the thermosetting resin.

10. The method for producing fiber-reinforced plastics according to any one of claims 6 to 9, characterized in that the tensile strength of the glass paper is 15 N / 15 mm or more in one direction and 4 N / 15 mm or more in another direction perpendicular to the one direction.

Citation Information

Patent Citations

  • Method of producing copper laminated board with land

    JP1978010864A

  • Preparation of fiber reinforced plastic product

    JP1990169231A

  • Copper clad laminated sheet

    JP1996090714A

  • Laminated substrate for high-frequency and its manufacturing method

    JP2004174992A

  • Prepreg and manufacturing method of prepreg molded article

    JP2019151730A