Resin composition, electronic device member, resin additive, and organopolysiloxane composition for use as an additive to resin

A low viscosity, uniformly dispersible organopolysiloxane composition with controlled molecular weight distribution and stable components addresses dispersion and safety issues, resulting in high-quality resin products.

JP7574543B2Active Publication Date: 2024-10-29MITSUBISHI CHEM CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020064193
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-31
Publication Date
2024-10-29
Estimated Expiration
2040-03-31

AI Technical Summary

Technical Problem

Existing organopolysiloxane compositions face challenges in uniform dispersion and low viscosity, leading to issues such as precipitation, high viscosity, and volatile components that cause safety hazards and poor curing, especially when mixed with resins.

Method used

A specific organopolysiloxane composition with a narrow molecular weight distribution (Mw/Mn of 1.01 to 1.4) and controlled content of substances with coefficients T2, M2, and E2, ensuring low viscosity and excellent dispersibility, using a substance with a Si-C bond that remains stable at high temperatures, avoiding volatile components.

Benefits of technology

The composition achieves low viscosity and uniform dispersion in resins, preventing volatile hazards and ensuring stable, high-quality molded products with improved safety and reduced environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574543000001
    Figure 0007574543000001
  • Figure 0007574543000002
    Figure 0007574543000002
  • Figure 0007574543000003
    Figure 0007574543000003
Patent Text Reader

Abstract

To provide an organopolysiloxane composition which has low viscosity and is excellent in dispersibility to various resins, and a method for producing organopolysiloxane.SOLUTION: An organopolysiloxane composition contains organopolysiloxane represented by the following general formula [1], and having molecular weight distribution (Mw / Mn) of 1.01 to 1.4 and a number average molecular weight of 700<Mn<2,000 as component A, and a substance represented by the following general formula [2] as component B, in which the component A and the component B satisfy a relation of 0.1≤{(weight of component B)×100} / {(weight of component A)+(weight of component B)}≤9, a content of a substance in which coefficients T2, M2 and E2 in the expression [2] satisfy an expression of T2+2-M2+E2=0 relative to component A is 0.01 wt.% or more and 9 wt.% or less, and a content of a substance in which the coefficients T2, M2 and E2 in the expression [2] do not satisfy the expression of T2+2-M2+E2=0 is 3 wt.% or less. Expression [1]: (R1R2R3SiO1 / 2)M1(R4SiO3 / 2)T1(SiO4 / 2)Q(O1 / 2R5)E1. Expression [2]: (R6R7R8SiO1 / 2)M2(R9SiO3 / 2)T2(O1 / 2R10)E2.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an organopolysiloxane, and more particularly to an organopolysiloxane composition which is used in combination with other resins. [Background technology]

[0002] In recent years, organic-inorganic composite materials have been attracting attention, and development has been carried out with the aim of improving properties by mixing silicon materials into resins.For example, Patent Document 1 discloses an organopolysiloxane that has a narrow molecular weight distribution and is in a low-viscosity liquid state at room temperature, making it easy to mix with other resins, does not contain volatile low-molecular weight components, making it easy to handle, and has excellent properties when cured.By devising the functional groups of this liquid organopolysiloxane with a low molecular weight and narrow molecular weight distribution, various functions have been imparted to various resins. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2018 / 110613 Summary of the Invention [Problem to be solved by the invention]

[0004] In order to effectively exert the functions of the organopolysiloxane in the resin, it is important to uniformly mix and disperse the resin and the organopolysiloxane, and it is necessary to prepare a composition in a form that allows the organopolysiloxane to be easily mixed and dispersed in the resin prior to molding. However, problems arise due to the difficulty in uniformly dispersing the organopolysiloxane, such as the precipitation of certain components when the organopolysiloxane is mixed with a resin that has already been mixed with various additives, and the difficulty in diffusing the organopolysiloxane when the organopolysiloxane is mixed with a resin that has been increased in molecular weight due to the high viscosity of the resin, resulting in a concentration gradient of the organopolysiloxane in the composition and resulting in uneven physical properties of the molded product. In such cases, it is possible to improve the dispersibility of the organopolysiloxane by using a liquid organopolysiloxane composition that has a narrow molecular weight distribution and is free of volatile low molecular weight components, diluting it with an organic solvent, and mixing it; however, some of the advantages that were present before the addition of the organopolysiloxane are lost, for example, due to the danger of flammable vapor volatilizing when the mold is released during molding, the condensed organic solvent redissolving the molded product, whitening it and causing a poor appearance, poor curing due to a decrease in temperature caused by the evaporation of the organic solvent, a decrease in the melting point of the resin due to the organic solvent remaining in the molded product, shrinkage over time caused by the gradual evaporation of the organic solvent from the molded product, a decrease in strength due to the generation of voids as the organic solvent volatilizes, and coloring due to the oxidation of the organic solvent, etc. Furthermore, when an organopolysiloxane having a high viscosity is used to prepare a composition containing the same, the flowability during molding may be poor, leading to insufficient filling of the resin into a mold or the resin may harden in a state in which air is trapped within the resin. In some applications, the high viscosity of the organopolysiloxane may cause various adverse effects. For example, when used in cosmetics such as hair wax or lip gloss, the viscosity of the organopolysiloxane is an important factor since it greatly affects the texture.

[0005] Therefore, an object of the present invention is to provide an organopolysiloxane composition that has a low viscosity and excellent dispersibility in various resins, and a method for producing the organopolysiloxane. [Means for solving the problem]

[0006] Therefore, as a result of intensive studies, the present inventors have found that the viscosity can be adjusted by incorporating specific components into organopolysiloxane, and that this specific substance is difficult to volatilize even when heated, so it does not cause generation of odors, shrinkage of resins, appearance defects of molded products, reduction of transparency, insufficient curing, etc., and has stability equivalent to that of organopolysiloxane, so that in a desired use environment, it does not cause pollution of the surrounding environment or coloring due to decomposition. Further, by kneading the raw materials in the temperature range where this specific substance vaporizes and uniformly dispersing this specific substance in the resin, it has been found that there are also effects of reducing the viscosity of the resin and promoting the dispersibility of organopolysiloxane. Furthermore, as a merit of the reduction in the viscosity of organopolysiloxane, the adhesion amount to the kettle, filter, and extraction line after production is reduced, improving the recovery rate, and the dispersibility in the organic solvent is also improved, so that the cleaning labor can be reduced, and when made into a composition, it is less likely to remain in the container, reducing the cleaning load of the container after use, or when the container is discarded, since the specific substance in the organopolysiloxane composition adhering to the container has a structure similar to that of other components, there is no need to newly secure a storage place in view of the danger of the specific component as a storage place until the disposal process, and the disposal process also does not require detoxification treatment or separation treatment, and since there is no use of chemicals and energy associated therewith, it has been found that a surprising effect of contributing to environmental load reduction can be obtained, and the present invention has been achieved.

[0007] That is, the gist of the present invention is as follows. [1] Containing, as component A, an organopolysiloxane represented by the following general formula [1], having a molecular weight distribution (Mw / Mn) of 1.01 to 1.4, and a number average molecular weight of 700 < Mn < 2000, and, as component B, a substance represented by the following general formula [2], wherein the component A and the component B satisfy the relationship of 0.1 ≦ {(weight of component B) × 100} / {(weight of component A) + (weight of component B)} ≦ 9, and The content of the substance for which the coefficients T2, M2, and E2 in the formula [2] satisfy T2 + 2 - M2 + E2 = 0 with respect to the component A is 0.01% by weight or more and 9% by weight or less, and the content of the substance for which the coefficients T2, M2, and E2 in the formula [2] do not satisfy T2 + 2 - M2 + E2 = 0 is 3% by weight or less. It is an organopolysiloxane composition characterized by this. (R 1 R 2 R 3 SiO 1 / 2 ) M1 (R 4 SiO 3 / 2 ) T1 (SiO 4 / 2 ) Q (O 1 / 2 R 5 ) E1 ···[1] (R 6 R 7 R 8 SiO 1 / 2 ) M2 (R 9 SiO 3 / 2 ) T2 (O 1 / 2 R 10 ) E2 ···[2] Here, in the above formula [1], R 1 ~R 4 are each independently selected from the group consisting of an organic group containing a carbon atom and a hydrogen atom, and may be the same or different; R 5 is selected from the group consisting of an organic group having 1 to 20 carbon atoms and a hydrogen atom, and may be the same or different; The coefficients M1, T1, and Q are each independently 0 or more and less than 0.65, and satisfy M1 + T1 + Q = 1; The coefficients M1, T1, Q, and E1 satisfy 0 < T1 + Q < 0.65, 0.25 < T1, and 0 < E1 / (M1 + E1) < 1. Here, in the above formula [2], R 6 ~R 8are each independently selected from the group consisting of an organic group containing carbon atoms and a hydrogen atom, and may be the same or different; R 9 are selected from the group consisting of organic groups having 1 to 20 carbon atoms and hydrogen atoms, and may be the same or different; R 10 are selected from the group consisting of organic groups having 1 to 20 carbon atoms and hydrogen atoms, and may be the same or different; M2 is a positive integer between 1 and 5, coefficient T2 is a positive integer between 1 and 3, and coefficient E2 is 0 An integer between 0 and 5. [2] In the general formula [1], 4 The organopolysiloxane composition according to [1], wherein the organic group represented by the formula: is a phenyl group. [3] The organopolysiloxane composition according to [1] or [2], wherein the coefficient M1 is 0.40 or more and 0.55 or less, and the coefficient T1 is 0.45 or more and 0.58 or less. [4] The organopolysiloxane composition according to any one of [1] to [3], wherein the coefficient E1 is 0.01 or more and 0.1 or less. [5] R 1 ~R 3 The organopolysiloxane composition according to any one of [1] to [4], wherein is a methyl group. [6] The organopolysiloxane composition according to any one of [1] to [5], characterized in that when 200 g of the organopolysiloxane composition is placed in a 1 L eggplant-shaped flask and heated for 2 hours at an internal temperature of 110°C under reduced pressure using a vacuum pump having an evacuation capacity of a vacuum pressure of 0.15 torr, the organopolysiloxane loses a mass of 10 g or less. [7] The organopolysiloxane composition according to any one of [1] to [6], wherein the coefficient Q is 0. [8] In the general formula [2], R 9 The organopolysiloxane composition according to any one of [1] to [7], wherein is a phenyl group. [9] In the general formula [2], R6 ~R 8 The organopolysiloxane composition according to any one of [1] to [8], wherein ~R is a methyl group.

[10] The organopolysiloxane composition according to any one of [1] to [9], wherein the substance represented by the general formula [2] includes a substance in which the coefficient T2 is 1.

[11] The organopolysiloxane composition according to any one of [1] to

[10] , wherein the substance represented by the general formula [2] includes a substance in which the coefficient M2 is 3.

[12] The organopolysiloxane composition according to any one of [1] to

[11] , wherein the content of the substance represented by the general formula [2] in the organopolysiloxane composition is 0.5 to 3% by weight.

[13] A resin composition comprising the organopolysiloxane composition according to any one of [1] to

[12] .

[14] An organic solvent dilution comprising the organopolysiloxane composition according to any one of [1] to

[12] .

[15] A member for electronic equipment, comprising the organopolysiloxane composition according to any one of [1] to

[12] or a cured product thereof.

[16] A member for electronic equipment, comprising the resin composition according to

[13] or a cured product thereof.

[17] A method for producing an organopolysiloxane represented by the following general formula [1], having a heating step, wherein the heating temperature in the heating step is 100 °C or higher, and the content of alkali in the raw material mixture in the heating step is less than 100 ppm, The molecular weight distribution (Mw / Mn) of the organopolysiloxane is 1.01 to 1.4, and the number average molecular weight is 700 < Mn < 2000. A method for producing an organopolysiloxane, characterized by the above. (R 1 R 2 R 3 SiO 1 / 2 ) M1 (R 4 SiO 3 / 2 ) T1 (SiO 4 / 2 )Q (O 1 / 2 R 5 ) E1 ···[1] Here, in the above formula [1], R 1 ~R 4 are each independently selected from the group consisting of an organic group containing a carbon atom and a hydrogen atom, and may be the same or different; R 5 is selected from the group consisting of an organic group having 1 to 20 carbon atoms and a hydrogen atom, and may be the same or different; The coefficients M1, T1, and Q are each independently 0 or more and less than 0.65, and satisfy M1 + T1 + Q = 1; Also, the coefficients M1, T1, Q, and E1 satisfy 0 < T1 + Q < 0.65, 0.25 < T1, and 0 < E1 / (M1 + E1) < 1. The method for producing an organopolysiloxane according to

[17] , which produces the organopolysiloxane contained in the organopolysiloxane composition according to any one of

[18] [1] to

[12] . The method for producing an organopolysiloxane according to

[17] , which produces the organopolysiloxane contained in the resin composition according to

[19]

[13] . The method for producing an organopolysiloxane according to

[17] , which produces the organopolysiloxane contained in the organic solvent diluent according to

[20]

[14] . The method for producing an organopolysiloxane according to

[17] , which produces the organopolysiloxane contained in the organopolysiloxane composition for electronic device members according to

[21]

[15] or a cured product thereof.

Advantages of the Invention

[0008] According to the present invention, it is possible to provide an organopolysiloxane composition having a low viscosity and excellent dispersibility in various resins, and a method for producing the organopolysiloxane. In addition, the above organopolysiloxane composition also has the effect of being excellent in odor and colorability and being able to maintain a relatively high flash point.

Embodiments for Carrying Out the Invention

[0009] The embodiments of the present invention will be described in detail below. However, these descriptions are examples (representative examples) of the embodiments of the present invention, and the present invention is not limited to these contents unless it exceeds the gist thereof. In this specification, a numerical range represented by "~" means a range including the numerical values described before and after "~" as the lower limit value and the upper limit value, and "A~B" means A or more and B or less. In addition, in this specification, "independently" used when explaining two or more objects together means that these two or more objects may be the same or different.

[0010] <1. Organopolysiloxane Composition> An organopolysiloxane composition (hereinafter, also simply referred to as "organopolysiloxane composition"), which is an embodiment of the present invention, contains, as component A, an organopolysiloxane represented by the following general formula [1], having a molecular weight distribution (Mw / Mn) of 1.01 to 1.4, and a number average molecular weight of 700 < Mn < 2000 (hereinafter, also simply referred to as "organopolysiloxane"), and, as component B, a substance represented by the following general formula [2], the component A and the component B satisfy the relationship of 0.1 ≦ {(weight of component B) × 100} / {(weight of component A) + (weight of component B)} ≦ 9, and with respect to component A (when component A is 100% by weight), the content of the substance in which the coefficients T2, M2, and E2 in the formula [2] satisfy T2 + 2 - M2 + E2 = 0 is 0.01% by weight or more and 9% by weight or less, and the content of the substance in which the coefficients T2, M2, and E2 in the formula [2] do not satisfy T2 + 2 - M2 + E2 = 0 is 3% by weight or less. It is an organopolysiloxane composition characterized by this. (R 1 R 2 R 3 SiO 1 / 2 ) M1 (R 4 SiO 3 / 2 )T1 (SiO 4 / 2 ) Q (O 1 / 2 R 5 ) E1 ···[1] (R 6 R 7 R 8 SiO 1 / 2 ) M2 (R 9 SiO 3 / 2 ) T2 (O 1 / 2 R 10 ) E2 ···[2] Here, in the above formula [1], R 1 ~R 4 are each independently selected from the group consisting of an organic group containing a carbon atom and a hydrogen atom, and may be the same or different. R 5 is selected from the group consisting of an organic group having 1 to 20 carbon atoms and a hydrogen atom, and may be the same or different. The coefficients M1, T1, and Q are each independently 0 or more and less than 0.65, and satisfy M1 + T1 + Q = 1. Also, the coefficients M1, T1, Q, and E1 satisfy 0 < T1 + Q < 0.65, 0.25 < T1, and 0 < E1 / (M1 + E1) < 1. Here, in the above formula [2], R 6 ~R 8 are each independently selected from the group consisting of an organic group containing a carbon atom and a hydrogen atom, and may be the same or different. R 9 is selected from the group consisting of an organic group having 1 to 20 carbon atoms and a hydrogen atom, and may be the same or different. R 10 is selected from the group consisting of an organic group having 1 to 20 carbon atoms and a hydrogen atom, and may be the same or different; M2 is a positive integer from 1 to 5, the coefficient T2 is a positive integer from 1 to 3, and the coefficient E2 is an integer from 0 to 5.

[0011] In this specification, the organopolysiloxane is a general term for all components that satisfy the above general formula [1], and in this case, the content of the organopolysiloxane is a value calculated based on the combined value of the multiple types of organopolysiloxane (combined). Similarly, in the present invention, the substance represented by the above general formula [2] is a general term for all components that satisfy the above general formula [2], and in this case, the content of the substance is a value calculated based on the combined value of the multiple types of the substance (combined).

[0012] The substance represented by the above general formula [2] has a low viscosity due to its small molecular weight, and has good dispersibility in the organopolysiloxane composition represented by the general formula [1] and other resins. 9 The compatibility can be ensured by selecting the functional group type according to the organopolysiloxane composition and resin to which it is to be applied. In addition, the substance represented by the general formula [2] has Si-C bonds and Si-O-Si-C bonds that are unlikely to undergo dehydration condensation reactions with catalysts such as acids and bases used in synthesizing the organopolysiloxane, and water, and can maintain its structure even in the organopolysiloxane composition and resin, and maintains its structure even at high temperatures exceeding 200°C during molding, so it does not affect the quality of the molded product. In addition, when an organic solvent is used in the organopolysiloxane composition or resin, it volatilizes at high temperatures exceeding 200°C during molding, which can pose a risk due to the generation of flammable vapor or cause a defective appearance due to local dissolution of the molded product. However, the substance represented by the general formula [2] has excellent compatibility with the organopolysiloxane composition, so it does not volatilize even when temperatures and pressure conditions exceed the boiling point of the substance occur, and a molded product that is safe and does not have a defective appearance can be obtained.

[0013] <1.1. Organopolysiloxane represented by general formula [1]> The organopolysiloxane composition contains, as component A, an organopolysiloxane represented by the above general formula [1]. (R 1 R2 R 3 SiO 1 / 2 ) M1 (R 4 SiO 3 / 2 ) T1 (SiO 2 / 2 ) Q (O 1 / 2 R 5 ) E1 ···[1]

[0014] In general formula [1], the coefficient M1 represents the proportion of the so-called M unit in which there is one oxygen atom bonded to a silicon atom. Similarly, the coefficient T1 represents the proportion of the T unit in which there are three oxygen atoms bonded to a silicon atom, and the coefficient Q represents the proportion of the Q unit in which four oxygen atoms are bonded to a silicon atom. The coefficient E represents the proportion of the molecules in which R 5 is bonded through the oxygen bonded to the silicon atom, indicating the proportion of the alkoxy group and the proportion of the silanol group. For example, when M1 > 0, it means that the M unit is essential. Therefore, T1 + Q > 0 means that the T unit or the Q unit is essential. In addition, in the present invention, since the sum of the M unit, the T unit, and the Q unit is represented as 1 (M1 + T1 + Q = 1), T1 + Q < 0.65 means that the sum of the T unit and the Q unit is less than 65 mol% with respect to the sum of the M unit, the T unit, and the Q unit. 0.25 < T1 means that the T unit is more than 25 mol% with respect to the sum of the M unit, the T unit, and the Q unit. Also, for example, 0 ≦ E1 / (M1 + E1) means that the coefficient E may not be included or may be included. Also, when 0 < E1 / (M1 + E1), the coefficient E must be included. E1 / (M1 + E1) < 1 means that when the oxygen of the T unit and the Q unit is called a bond, as a result of the consumption of the bonds by the bonding between the T units, the bonding between the Q units, and the bonding between the T unit and the Q unit, what bonds to the unconsumed bonds is the M unit, and / or the alkoxy group and / or the silanol group, including the bond between the bond and the M unit, and indicating that the M unit is essential. It is not necessary that the units constituting the M unit, T unit, and E unit are all the same.

[0015] In the present specification, an organic group refers to a functional group that includes carbon atoms, hydrogen atoms, oxygen atoms, nitrogen atoms, phosphorus atoms, sulfur atoms, and halogen atoms, and is composed of any combination of these atoms, and does not include groups that are composed of only one hydrogen atom. Also, an organic group that includes a carbon atom refers to a functional group that satisfies the above organic group aspects and includes at least one carbon atom.

[0016] R 1 ~R 4 are each independently selected from the group consisting of an organic group containing a carbon atom and a hydrogen atom. 1 ~R 4 The atom bonded to the silicon atom is not particularly limited as long as it is not an oxygen atom, in order to avoid changing the classification of the M unit and the T unit. 1 ~R 4is selected in consideration of compatibility and reactivity from the viewpoint of mixing or reacting with a resin to be mixed or an additive used for any purpose, and for example, a combination of functional groups including a vinyl group, an allyl group, a (meth)acrylic group, a carboxyl group, a nitrile group, a formyl group, a carbonyl group, a carbinol group, an amino group, an imino group, a nitro group, a cyano group, a sulfo group, a mercapto group, a thiol bond, an ether bond, an ester bond, an amide bond, an alkyl group having 1 to 20 carbon atoms, an aromatic functional group, or the like is preferred. Specifically, a combination of functional groups including a hydrogen atom, a methyl group, an ethyl group, a propyl group, a hexyl group, a decyl group, an octadecyl group, a cyclopentyl group, a cyclohexyl group, an ethylene glycol monoethylene ether group, an acryloxypropyl group, an acryloxyoctyl group, a methacryloxypropyl group, a methacryloxyoctyl group, a glycidyl group, a glycidoxypropyl group, a glycidoxyoctyl group, a 1,2-epoxycyclohexyl-3 In the case where the polarity of the components to be mixed is low, a hydrogen atom, a methyl group, an ethyl group, a cyclopentyl group, a cyclohexyl group, a 1,2-epoxycyclohexyl-3-propyl group, a 1,2-epoxycyclohexyl-3-octyl group, a 1,2-epoxycyclohexyl-3-octyl group, a 1,2-epoxycyclohexyl-3-octyl group, a allyl group is more preferable. In the case where the polarity of the components to be mixed is high, an ethylene glycol monoethylene ether group, an acryloxypropyl group, an acryloxyoctyl group, a methacryloxypropyl group, a methacryloxyoctyl group, a glycidyl group, a glycidoxypropyl group, a glycidoxyoctyl group, a phenyl group, a phenethylene group, a styryl group, a vinyl group is more preferable. It is preferable to combine them in any ratio according to the resin composition to be mixed.

[0017] Considering the case where organopolysiloxane is mixed with other resins, R 1 ~R 4 Suitable examples of is shown below.

[0018] <When the resin to be mixed is mainly dimethylpolysiloxane> In this case, the resin is a resin with low polarity, R 1 ~R 4 are each independently preferably a hydrogen atom, a methyl group, or a vinyl group. In particular, R 1 ~R 3 When one of the groups is a hydrogen atom or a vinyl group and the other two are methyl groups, R 1 ~R 3 is a methyl group, and any combination thereof is more preferred, 4 is more preferably a hydrogen atom, a methyl group, or a vinyl group, and when a reaction such as hydrosilylation is involved, a hydrogen atom or a vinyl group is even more preferable, and when no reaction is desired, a methyl group is preferable from the viewpoint of stability.

[0019] <When the resin to be mixed is mainly composed of dimethyldiphenylpolysiloxane and methylphenylpolysiloxane> In this case, the resin corresponds to both low polarity resin and high polarity resin, and R 1 ~R 4 is preferably used in combination with a methyl group and a phenyl group, and particularly preferably 1 ~R 3 One of them is a hydrogen atom or a vinyl group, the other two are methyl groups, R 1 ~R 3 is preferably a methyl group, or a combination thereof, and R 4 is more preferably a phenyl group.

[0020] <When the resin to be mixed contains a (meth)acryloyl group> In this case, the resin is a highly polar resin, R 1 ~R 4 are preferably used in combination with an acryloxypropyl group, a methacryloxypropyl group, a methacryloxyoctyl group, a glycidoxypropyl group, a glycidoxyoctyl group, or a methyl group. 1 ~R 3 One of them is a hydrogen atom or a vinyl group, the other two are methyl groups, R1 ~R 3 is preferably a methyl group, or a combination thereof, and R 4 More preferred are an acryloxypropyl group, a methacryloxypropyl group, a methacryloxyoctyl group, a glycidoxypropyl group, a glycidoxyoctyl group, a phenyl group, and combinations thereof. From the viewpoint of increasing hardness such as pencil hardness and Shore hardness, an acryloxypropyl group, a methacryloxypropyl group, and a glycidoxypropyl group are preferred, and from the viewpoint of flexibility and brittleness, a methacryloxyoctyl group and a glycidoxyoctyl group are preferred.

[0021] <When the resin to be mixed is polycarbonate> In this case, the resin is a highly polar resin, R 1 ~R 4 are preferably used in combination with an ethylene glycol monoethylene ether group, a glycidoxypropyl group, a glycidoxyoctyl group, a phenyl group, a phenethylene group, a styryl group, a vinyl group, or a methyl group. 1 ~R 3 One of them is a hydrogen atom, a vinyl group, an ethylene glycol monoethylene ether group, or a glycidoxypropyl group, and the other two are a methyl group, R 1 ~R 3 is preferably a methyl group, or a combination thereof, and R 4 Phenyl groups are more preferable, and in terms of compatibility and heat resistance to temperatures exceeding 200°C when mixed with polycarbonate, R 1 ~R 3 is a methyl group, R 4 It is preferred that is a phenyl group.

[0022] R 5is a group selected from the group consisting of organic groups having 1 to 20 carbon atoms and a hydrogen atom. From the viewpoint of compatibility with the resin, a hydrogen atom, a methyl group, an ethyl group, a butyl group, an octyl group, or an octadecyl group is preferable. From the viewpoint of weight change or volume change due to dehydration condensation upon heating or changes over time, a hydrogen atom or a methyl group is preferable, and a hydrogen atom is particularly preferable. From the viewpoint of stability, a methyl group is preferable, and a combination of a methyl group and a hydrogen atom is also preferable.

[0023] In the organopolysiloxane represented by the general formula [1], M units and T units are essential, and Q units are optional. The combination of each unit may be MT resin consisting of M units and T units, or MTQ resin consisting of M units, T units, and Q units. may be also possible. Furthermore, from the viewpoint of low molecular weight and high compatibility with resins, MT resin is preferable, and from the viewpoint of high silicon content and high molecular weight, MTQ resin is preferable.

[0024] The M units are greater than 0 and less than 0.65, but since the M units are bonded to oxygen atoms which are bonds of the T units and the Q units and reduce the number of bonds, it is possible to control the degree of polymerization by the content of the M units, and from the viewpoint of narrowing the range of the molecular weight distribution (Mw / Mn), it is usually greater than 0, preferably 0.10 or more, more preferably 0.25 or more, even more preferably 0.40 or more, and particularly preferably 0.44 or more, and is usually 0.65 or less, preferably 0.60 or less, more preferably 0.55 or less, and even more preferably 0.50 or less.

[0025] Regarding the M unit, from the viewpoint of storage stability of the organopolysiloxane, it is preferable that at least one of the M units is a trimethylsiloxy group. If the number of trimethylsiloxy groups is too small, the number of M units other than trimethylsiloxy groups, i.e., M units containing reactive groups, tends to increase automatically, so from the viewpoint of storage stability of the organopolysiloxane, it is preferable that a trimethylsiloxy group is present. On the other hand, from the viewpoint of reactivity of the organopolysiloxane, it is preferable that the amount of trimethylsiloxy groups in the organopolysiloxane or in the M units is small, and it is more preferable that no trimethylsiloxy groups are contained. If there are too many trimethylsiloxy groups, the number of reactive groups will decrease, so when the function (such as curability) that the reactive group has is important, it is preferable that the number of trimethylsiloxy groups is one or less.

[0026] The T unit is a crosslinkable silicon unit that forms organopolysiloxane microparticles, and from the viewpoint of ensuring dispersibility in the resin to be mixed by narrowing the range of the molecular weight distribution (Mw / Mn) and controlling the occurrence of a decrease in storage stability due to hydrolysis and condensation, the T unit is greater than 0.25 and less than 0.65, but is preferably 0.3 or more, more preferably 0.45 or more, and even more preferably 0.5 or more, and is usually 0.65 or less, preferably 0.62 or less, more preferably 0.60 or less, even more preferably 0.58 or less, and particularly preferably 0.57 or less.

[0027] The Q unit is the most oxidized form of silicon. By being included in the structure of organopolysiloxane, the heat resistance can be enhanced. Also, the number of oxygen atoms capable of participating in polymerization is larger than that of the D unit and the T unit, and the degree of polymerization can be increased. Therefore, from this perspective, an MTQ resin having a Q unit in its structure is preferred. Q may be 0, but is preferably greater than 0, more preferably 0.02 or more, still more preferably 0.04 or more. Also, it is usually less than 0.6. When there are many Q units, the solid or viscosity increases, and the handleability deteriorates. Therefore, it is preferably 0.4 or less, more preferably 0.1 or less, and even more preferably 0.08 or less.

[0028] The T unit and the Q unit are crosslinking components and are units that increase the degree of polymerization respectively. In addition to existing within the above-described range as the general formula [1], in the organopolysiloxane represented by the general formula [1], 0 < T1 + Q < 0.65. 0 < T1 + Q < 0.65 is a specified value regarding the degree of polymerization. When this value is small, the amount of the monomer composed of the MT unit or the monomer composed of the MQ unit increases, and the effects that the organopolysiloxane should originally impart may not be obtained. When this value is large, the solid or viscosity increases, and the handleability deteriorates. Therefore, it is greater than 0 and less than 0.65, preferably 0.10 or more, more preferably 0.50 or more, still more preferably 0.52 or more. Also, it is usually 0.65 or less, preferably 0.62 or less, more preferably 0.60 or less, and even more preferably 0.57 or less. When T1 + Q is small, M1 becomes large and converges to the monomer of the T unit modified with the M unit or the MQ monomer, so the amount of the monomer composed of the MT unit or the monomer composed of the MQ unit increases. Similarly, 0.25 < T1 / (M1 + T1 + Q) is the content of the T unit in the organopolysiloxane represented by the general formula [1]. Specifically, it indicates that the content of the T unit relative to the sum of the M unit, the T unit, and the Q unit is more than 25%.

[0029] ​E1 is a coefficient that defines the content of alkoxy groups and silanol groups. By having an organopolysiloxane component containing alkoxy groups and silanol groups in the structure, it can be treated as an organopolysiloxane with a lower viscosity than in the non-containing state. On the other hand, when a large amount of alkoxy groups and silanol groups are contained, due to the dehydration condensation reaction caused by catalysts such as acids and alkalis remaining in the organopolysiloxane and moisture in the air, the storage stability of the organopolysiloxane may decrease. Therefore, E1 is greater than 0, and may be 0.01 or more, 0.02 or more, 0.05 or more, and preferably 0.5 or less, more preferably 0.1 or less. Also, 0 < E1 / (M1 + E1) < 1 is the ratio of alkoxy groups and silanol groups with M units and E1 as coefficients in the organopolysiloxane represented by the general formula [1], indicating that it contains an organopolysiloxane component having alkoxy groups and / or silanol groups and does not exist in an amount equal to or more than the M units. Usually, it is greater than 0, preferably 0.002 or more, more preferably 0.04 or more, even more preferably 0.08 or more, usually less than 1, preferably 0.3 or less, more preferably 0.2 or less, and even more preferably 0.15 or less.

[0030] The number average molecular weight Mn of the organopolysiloxane composed of each component of the organopolysiloxane represented by the general formula [1] is greater than 700 and less than 2000 from the viewpoint of expressing the function of the organopolysiloxane in the resin to be mixed and ensuring compatibility with the resin. Usually, it is 750 or more, preferably 800 or more, more preferably 830 or more. Also, usually it is 1800 or less, preferably 1500 or less, more preferably 1200 or less, and even more preferably 1000 or less. The number average molecular weight Mn is measured by the method described later.

[0031] The molecular weight distribution (Mw / Mn) of the organopolysiloxane represented by general formula [1] is 1.01 or more and 1.4 or less. From the viewpoint of expressing the function of the organopolysiloxane in the resin to be mixed and ensuring compatibility with the resin, it is preferably 1.03 or more, more preferably 1.05 or more, and even more preferably 1.07 or more, and is preferably 1.2 or less, more preferably 1.1 or less, and even more preferably 1.09 or less. The weight average molecular weight Mw is measured by the method described below.

[0032] From the viewpoint of ensuring the effect of the organopolysiloxane on the resin to which it is added, the content of the organopolysiloxane represented by general formula [1] in the organopolysiloxane composition is usually 90% by weight or more, preferably 91% by weight or more, more preferably 93% by weight or more, and even more preferably 97% by weight or more, and is usually less than 100% by weight, preferably 99.5% by weight or less, more preferably 99.4% by weight or less, and even more preferably 98.7% by weight or less.

[0033] <1.2. Method for producing organopolysiloxane> The method for producing an organopolysiloxane according to another embodiment of the present invention (hereinafter also simply referred to as the "method for producing an organopolysiloxane") is a method for producing an organopolysiloxane according to the above embodiment, and a known method for producing an organopolysiloxane can be used. For example, any of the manufacturing methods may be used, such as a method of simultaneously condensing one or more disiloxane compounds, disilazane compounds, and their hydrolysates, alkoxysilane compounds, and their hydrolysates, and partial hydrolysis condensates, a method of condensing disiloxane compounds, disilazane compounds, and their hydrolysates, chlorosilane compounds, and their hydrolysates, and partial hydrolysis condensates, a method of ring-opening polymerization of cyclic siloxane compounds, and chain polymerization including anionic polymerization, and a combination of a plurality of manufacturing methods may be used. In addition, an organic functional group may be converted into another organic functional group by a chemical method and used. Examples of the method of converting an organic functional group into another organic functional group include a method of reacting a group in which a hydrogen atom is directly bonded to a silicon atom with an alkenyl group (hydrosilylation method). The obtained organopolysiloxane may be fractionated to obtain organopolysiloxanes having the desired molecular weight or molecular weight distribution by column chromatography, GPC, extraction with a solvent, distillation of unnecessary components, etc. Low-boiling point components may be removed by treatment such as reduced pressure or heating.

[0034] When producing organopolysiloxane, a solvent may or may not be used. When using a solvent, water and an organic solvent can be used, but organic solvents are particularly preferred, and tetrahydrofuran, toluene, hexane, heptane, acetone, ethyl acetate, methanol, ethanol, isopropanol, chloroform, and dichloromethane are more preferred, and tetrahydrofuran, toluene, and methanol are even more preferred from the viewpoints of solubility, ease of removal, and low environmental toxicity. In addition, these water and organic solvents may be used in combination of two or more types, and the solvent type may be different depending on the reaction process. In addition, when forming an organopolysiloxane skeleton by hydrolysis and condensation of an alkoxysilane compound or a chlorosilane compound, an appropriate amount of water can be added to promote hydrolysis.

[0035] The reaction temperature in producing the organopolysiloxane is not particularly limited as long as it is 0° C. or higher, from the viewpoints of the melting point of the water used in the reaction and the boiling points of the alcohol used as the solvent or the alcohol and siloxane compound produced, and is preferably 5° C. or higher and usually 120° C. or lower, more preferably 100° C. or lower, even more preferably 60° C. or lower, and preferably 40° C. or lower. The heating temperature during post-treatment heating (heating step or distillation step), such as removing the mixture of raw materials or the reactant solvent obtained in the above steps, is not particularly limited as long as the target is removed from the viewpoint of removing the solvent boiling point, unreacted raw materials, and hydrolyzates derived from the raw materials, and is preferably 60°C or higher, more preferably 100°C or higher, even more preferably 110°C or higher, and particularly preferably 120°C or higher. In addition, for the purpose of condensing unreacted silanols and increasing stability, it is preferably 100°C or higher, more preferably 110°C or higher, and even more preferably 120°C, and from the viewpoint of not changing the modified functional group by heat, it is preferably 180°C or lower, more preferably 150°C or lower, and even more preferably 140°C or lower. The above heating step is particularly preferred when no reaction occurs or when the reaction rate of the functional group to be reacted is less than 5% compared to the unreacted state.

[0036] When producing organopolysiloxane, the pressure for carrying out the reaction is not particularly limited, and is usually 0.6 atm or more, preferably 0.8 atm or more, and more preferably 0.9 atm or more. By setting the pressure in this range, the boiling point of the solvent can be kept in an appropriate range, and the reaction temperature in the reaction system can be set to an appropriate reaction temperature. In addition, the reaction is usually carried out at 1.4 atm or less, preferably 1.2 atm or less, and more preferably 1.1 atm or less. By setting the pressure in this range, the boiling point of the solvent increases, and the reaction is not accelerated more than necessary, and as a result, the risk of damage to the device or explosion can be reduced.

[0037] In the process of heating the raw material mixture or the reactants, when the heating temperature in the heating process is 100°C or higher, the organopolysiloxane undergoes hydrolysis and condensation due to the alkaline substance. Therefore, the alkali content in the raw material mixture (including the reactants) in the heating process is 100 It is less than ppm, preferably 2 ppm or less, more preferably 0.2 ppm or less, and is preferably free (0 ppm), but is usually 0 or more, and may include 0.001 ppm or more.

[0038] <1.3. Substance represented by general formula [2]> The organopolysiloxane composition contains a substance represented by the following general formula [2] as a viscosity modifier. (R 6 R 7 R 8 SiO 1 / 2 ) M2 (R 9 SiO 3 / 2 ) T2 (O 1 / 2 R 10 ) E2 [2] R 6 ~R 8 are each independently selected from the group consisting of an organic group containing carbon atoms and a hydrogen atom, and may be the same or different. R 9 are selected from the group consisting of organic groups having 1 to 20 carbon atoms and hydrogen atoms, and may be the same or different. R 10 are selected from the group consisting of organic groups having 1 to 20 carbon atoms and hydrogen atoms, and may be the same or different. M2 is a positive integer from 1 to 5; coefficient T2 is a positive integer from 1 to 3; and coefficient E2 is an integer from 0 to 5.

[0039] The coefficients T2 and M2 are both greater than or equal to 1, i.e., the T2 and M2 units are required. T2+2-M2+E2=0 means that no cyclic compounds are included in the siloxane bond. Cyclic compounds exist at T3 or more, and even cyclic compounds have a viscosity reducing effect, and can be used in fields where the shelf life of the product is not important after mixing with the resin. In addition, the viscosity reducing effect of cyclic compounds may change due to ring opening, so it is preferable not to include them from the viewpoint of product stability, but a small amount may be included. From the above viewpoint, the content of the substance whose T2, M2, and E2 satisfy T2+2-M2+E2=0 in the organopolysiloxane (component A) represented by the general formula [1] (when component A is 100% by weight) is 0.01% by weight or more and 9% by weight or less, preferably 0.5% by weight or more, more preferably 0.6% by weight or more, and even more preferably 1% by weight or more, and preferably 7% by weight or less, more preferably 5% by weight or less, and even more preferably 4% by weight or less. In the organopolysiloxane (component A) represented by the general formula [1], the content of the substance in which T2, M2, and E2 do not satisfy T2+2-M2+E2=0 is 3% by weight or less, more preferably 0.1% by weight or less, even more preferably 0.01% by weight or less, and most preferably not contained (0 ppm), but usually 0% by weight or more, and may contain 0.001% by weight or more. Furthermore, in a form derived from the present invention in which a cyclic compound is volatilized from a product over time and vapor-deposited onto an electrode surface and coated with a siloxane compound, it is desirable to contain the maximum amount that does not volatilize due to the heat during mixing, and usually 1% by weight or more, preferably 3% by weight or more, and more preferably 9% by weight or more.

[0040] R 6 ~R 9 are each independently selected from the group consisting of an organic group containing carbon atoms and a hydrogen atom; R 6 ~R 9 The atom bonded to the silicon atom is not particularly limited as long as it is not an oxygen atom, in order to avoid changing the classification of the M unit and the T unit. 6 ~R 9is selected in consideration of compatibility and reactivity from the viewpoint of mixing and reacting with the organopolysiloxane to be used as the composition, or with the resin to be mixed, or with additives to be used for any purpose, and for example, a combination of functional groups including a vinyl group, an allyl group, a (meth)acrylic group, a carboxyl group, a nitrile group, a formyl group, a carbonyl group, a carbinol group, an amino group, an imino group, a nitro group, a cyano group, a sulfo group, a mercapto group, a thiol bond, an ether bond, an ester bond, an amide bond, an alkyl group having 1 to 20 carbon atoms, an aromatic functional group, or the like is preferred, and specific examples thereof include a hydrogen atom, a methyl group, an ethyl group, a propyl group, a hexyl group, a decyl group, an octadecyl group, a cyclopentyl group, a cyclohexyl group, an ethylene glycol group, an ethylene glycol terephthalate ... Preferably, the alkyl group is a aryl monoethylene ether group, an acryloxypropyl group, an acryloxyoctyl group, a methacryloxypropyl group, a methacryloxyoctyl group, a glycidyl group, a glycidoxypropyl group, a glycidoxyoctyl group, a 1,2-epoxycyclohexyl-3-propyl group, a 1,2-epoxycyclohexyl-3-octyl group, a phenyl group, a phenethylene group, a styryl group, a vinyl group, or an allyl group, and when the polarity of the components to be mixed is low, a hydrogen atom, a methyl group, an ethyl group, a cyclopentyl group, a cyclohexyl group, a 1,2-epoxycyclohexyl-3-propyl group, or a , 1,2-epoxycyclohexyl-3-octyl group, 1,2-epoxycyclohexyl-3-octyl group, and allyl group are more preferred, and when the components to be mixed have high polarity, ethylene glycol monoethylene ether group, acryloxypropyl group, acryloxyoctyl group, methacryloxypropyl group, methacryloxyoctyl group, glycidyl group, glycidoxypropyl group, glycidoxyoctyl group, phenyl group, phenethylene group, styryl group, and vinyl group are even more preferred, and it is preferable to combine them in any ratio depending on the resin composition to be mixed.

[0041] R 10is a group selected from the group consisting of organic groups having 1 to 20 carbon atoms and a hydrogen atom. From the viewpoint of compatibility with the resin, a hydrogen atom, a methyl group, an ethyl group, a butyl group, an octyl group, or an octadecyl group is preferable. From the viewpoint of weight change or volume change due to dehydration condensation upon heating or changes over time, a hydrogen atom or a methyl group is preferable, and a hydrogen atom is particularly preferable. From the viewpoint of stability, a methyl group is preferable, and a combination of a methyl group and a hydrogen atom is also preferable.

[0042] Considering the case where organopolysiloxane is mixed with other resins, R 6 ~R 9 A suitable example is shown below.

[0043] <When the resin to be mixed is mainly dimethylpolysiloxane> In this case, the resin is a resin with low polarity, R 6 ~R 9 are each independently preferably a hydrogen atom, a methyl group, or a vinyl group. In particular, R 6 ~R 8 When one of the groups is a hydrogen atom or a vinyl group and the other two are methyl groups, R 6 ~R 8 are all methyl groups, and any combination thereof is more preferred. 9 is preferably a hydrogen atom, a methyl group, or a vinyl group. When a reaction such as hydrosilylation is involved, a hydrogen atom or a vinyl group is more preferable. When a reaction is not desired, a methyl group is more preferable from the viewpoint of stability. R 6 ~R 9 More preferably, all of are methyl groups.

[0044] <When the resin to be mixed is mainly composed of dimethyldiphenylpolysiloxane and methylphenylpolysiloxane> In this case, the resin corresponds to both low polarity resin and high polarity resin, and R 6 ~R 9 It is preferable to use a combination of a methyl group and a phenyl group for R. 6 ~R 8One of them is a hydrogen atom or a vinyl group, the other two are methyl groups, R 6 ~R 8 is preferably a methyl group, or a combination thereof, and R 9 R is more preferably a phenyl group. 6 ~R 8 are all methyl groups, and R 9 It is most preferred that is a phenyl group.

[0045] <When the resin to be mixed contains a (meth)acryloyl group> In this case, the resin is a highly polar resin, R 6 ~R 9 is preferably used in combination with an acryloxypropyl group, a methacryloxypropyl group, a methacryloxyoctyl group, a glycidoxypropyl group, a glycidoxyoctyl group, or a methyl group, and particularly preferably used in combination with R 6 ~R 8 One of them is a hydrogen atom or a vinyl group, the other two are methyl groups, R 6 ~R 8 is preferably a methyl group, or a combination thereof, and R 9 is more preferably an acryloxypropyl group, a methacryloxypropyl group, a methacryloxyoctyl group, a glycidoxypropyl group, a glycidoxyoctyl group, a phenyl group, or a combination thereof, and from the viewpoint of increasing hardness such as pencil hardness and Shore hardness, an acryloxypropyl group, a methacryloxypropyl group, or a glycidoxypropyl group is preferable, and from the viewpoint of flexibility and brittleness, Methacryloxyoctyl and glycidoxyoctyl groups are preferred.

[0046] <When the resin to be mixed is polycarbonate> In this case, the resin is a highly polar resin, R 6 ~R 9 is preferably used in combination with an ethylene glycol monoethylene ether group, a glycidoxypropyl group, a glycidoxyoctyl group, a phenyl group, a phenethylene group, a styryl group, a vinyl group, or a methyl group. In particular, R 6 ~R8 One of them is a hydrogen atom, a vinyl group, an ethylene glycol monoethylene ether group, or a glycidoxypropyl group, and the other two are a methyl group, R 1 ~R 3 is preferably a methyl group, or a combination thereof, and R 8 Phenyl groups are more preferable, and in terms of compatibility and heat resistance to temperatures exceeding 200°C when mixed with polycarbonate, R 6 ~R 8 are all methyl groups, R 9 It is preferred that is a phenyl group.

[0047] The substance represented by the general formula [2] may be used alone or in combination with two or more kinds. In particular, a plurality of substances having different values ​​of the coefficients M2 and T2 may be used. 6 ~R 9 A plurality of compounds having different functional groups may be used.

[0048] M2 is 1 or more and 5 or less. In the modification of the bonds of the T units, the alkoxy group and silanol group represented by E2 are likely to change by dehydration condensation, but the M units are less likely to undergo silanolization and dehydration condensation associated with elimination. Therefore, from the viewpoint of stability, it is preferable that M2 is larger. Since the maximum value of T2 is 3, when T2 is 3, M2 is preferably 5, when T2 is 2, M2 is preferably 4, and when T2 is 1, M2 is preferably 3, that is, it is preferable that M2=T2+2. In addition, in the modification of the bonds of the T units, the M units are unlikely to undergo silanolization and dehydration condensation associated with elimination, but the alkoxy groups and silanol groups represented by E2 are easily reacted by dehydration condensation. Therefore, from the viewpoint of reactivity, it is preferable that M2 is small. Since the maximum value of T2 is 3, when T2 is 3, M2 is preferably 4 or less, more preferably 2 or less, and even more preferably 1. When T2 is 0, hydrolysis condensation occurs very easily and the viscosity change over time is large, so from the viewpoint of storage stability, M2 is 1 or more; when T2 is 2, M2 is preferably 3 or less, more preferably 2 or less, and even more preferably 1. When T2 is 0, the viscosity change over time is large, so from the viewpoint of storage stability, M2 is 1 or more; when T2 is 1, M2 is preferably 3 or less, more preferably 2 or less, and even more preferably 1. When T2 is 0, the viscosity change over time is large, so from the viewpoint of storage stability, M2 is 1 or more.

[0049] T2 is 1 or more and 3 or less, but from the viewpoint of an increase in the number of T units increasing the molecular weight and decreasing the viscosity-lowering effect due to an increase in viscosity, or from the viewpoint of a decrease in dispersibility in the organopolysiloxane to be mixed due to an increase in molecular size, it is preferable that T2 is small, preferably 3 or less, preferably 2 or less, and more preferably 1. Furthermore, since an increase in the number of T units decreases volatility, low volatility is preferable when process temperatures such as molding temperature and curing temperature are high, and from the viewpoint of volatility, it is preferable that T2 is large, preferably 1 or more, more preferably 2 or more, and even more preferably 3 or more.

[0050] The content of the substance represented by general formula [2] in the organopolysiloxane composition is usually 0.1 weight % or more, preferably 0.5 weight % or more, more preferably 1 weight % or more, and even more preferably 2 weight % or more, from the viewpoint of obtaining the viscosity-reducing effect. Furthermore, from the viewpoint of volatilization during molding or curing or volatilization over time, it is usually 9 weight % or less, preferably 7 weight % or less, more preferably 5 weight % or less, and even more preferably 3 weight % or less. Furthermore, in the organopolysiloxane composition, component A (represented by the above general formula [1] The ratio of the weight of component B to the sum of the weight of component A (the organopolysiloxane to be used) and the weight of component B (the substance represented by the general formula [2] above) relative to 100 ({(weight of component B) × 100} / {(weight of component A) + (weight of component B)}) is, from the viewpoint of reducing the viscosity of the organopolysiloxane and the viewpoint of the volatility of component B, 0.1 or more and 9 or less, but is usually 0.5 or more, preferably 0.6 or more, and more preferably 1.3 or more, and is usually 7 or less, preferably 5 or less, and more preferably 3 or less. In addition, a component that can be considered as both component A and component B will be considered as component B in this specification.

[0051] By improving the compatibility between the substance represented by general formula [2] and the organopolysiloxane represented by general formula [1] above, the substance represented by general formula [2] is dispersed evenly and the viscosity of the organopolysiloxane composition containing said substance is reduced. On the other hand, if compatibility is poor, the substance represented by general formula [2] will accumulate or emulsify locally, so that the effect of reducing the viscosity of the organopolysiloxane composition containing said substance is not very noticeable and, furthermore, when emulsified, the viscosity may increase.

[0052] <1.4. Method for producing the substance represented by general formula [2]> The method of producing the substance represented by the general formula [2] is not particularly limited, and it can be produced by a known method, or a commercially available product such as tris(trimethylsiloxy)phenylsilane (PTTSS) can be used. The substance represented by the general formula [2] can be included not only in the case of intentional addition, but also in the case of a method of producing the substance using a material containing M units and T units as a raw material, and it is possible that the substance may be included in the organopolysiloxane even if not intentionally added during the production of the organopolysiloxane. However, the substance represented by the general formula [2] is hated by the relevant traders as a substance that causes a problem of poor electrode contacts (commonly known as the low volatile problem) when a specific organopolysiloxane other than the organopolysiloxane of the general formula [1] is produced, and the substance has been removed to less than 0.1% by weight by distillation such as thin film distillation. Furthermore, by generating the substance of general formula [2] when producing the organopolysiloxane of general formula [1], it is possible to include the substance without intentionally adding it. In such a case, it is possible to adjust the content of the substance of general formula [2] according to the purpose, thereby adjusting the viscosity. It is also possible to achieve the purpose by analyzing the organopolysiloxane composition by gas chromatography to quantify the content of the substance of general formula [2], and controlling the content of the substance by distillation such as thin-film distillation.

[0053] <1.5. Other ingredients> The organopolysiloxane composition may contain components other than the organopolysiloxane represented by the general formula [1] and the component represented by the general formula [2] described above. Examples of the other components include a curing catalyst, a chain polymerization initiator, an antioxidant, a filler, a curing agent, and a curing regulator. There are no particular limitations on the amount of other components contained in the organopolysiloxane composition, and they may be added as desired depending on the purpose, as long as the effects of the present invention are achieved.

[0054] (curing catalyst) The type of the curing catalyst is not particularly limited, and examples thereof include addition polymerization catalysts and condensation polymerization catalysts. Examples of the addition polymerization catalyst include platinum-based catalysts such as platinum black, platinic chloride, chloroplatinic acid, reaction products of chloroplatinic acid with monohydric alcohols, complexes of chloroplatinic acid with olefins, platinum bisacetoacetate, platinum group metal catalysts such as platinum(0) complexes with 1,3-divinyl-1,1,3,3-tetramethyldisiloxane, platinum(0) complexes with 1,3,5,7-tetravinyl-1,3,5,7-tetramethylcyclosiloxane, palladium-based catalysts, and rhodium-based catalysts. The amount of the addition polymerization catalyst to be used is determined based on the total weight of the organopolysiloxane as the platinum group metal. The amount of the addition polymerization catalyst is usually 1 ppm or more, preferably 2 ppm or more, and usually 100 ppm or less, preferably 50 ppm or less, and more preferably 20 ppm or less. This allows the catalyst activity to be high and the cured product to have high transparency. The addition polymerization catalyst may be used alone or in combination of two or more kinds.

[0055] As the condensation polymerization catalyst, acids such as hydrochloric acid, nitric acid, sulfuric acid, organic acids, bases such as ammonia, amines, metal chelate compounds, etc. can be used, and a metal chelate compound containing one or more of Ti, Ta, Zr, Al, Hf, Zn, Sn, Pt, and In can be preferably used. Among them, the metal chelate compound is preferably one or more of Ti, Al, Zn, Zr, Pt, and In, and more preferably one containing Zr or Pt is used.

[0056] The amount of the condensation polymerization catalyst is usually 1 ppm or more, preferably 2 ppm or more, and usually 300 ppm or less, preferably 200 ppm or less, more preferably 150 ppm or less, based on the total weight of the organopolysiloxane as metal. This makes it possible to achieve high catalytic activity and small weight loss when the cured product is heated. The condensation polymerization catalyst may be used alone or in combination of two or more.

[0057] (Chain polymerization initiator) Examples of the chain polymerization initiator include a radical polymerization initiator, a cationic polymerization initiator, and an anionic polymerization initiator. Generally, a radical polymerization initiator is used.

[0058] As the radical polymerization initiator, a photopolymerization initiator and a thermal polymerization initiator can be used. As the photopolymerization initiator, an alkylphenone-based photopolymerization initiator, an acylphosphine oxide-based photopolymerization initiator, an intramolecular hydrogen abstraction type photopolymerization initiator, an oxime ester photopolymerization initiator, or the like can be used, and an alkylphenone-based photopolymerization initiator can be preferably used.

[0059] As the thermal polymerization initiator, a conventionally known peroxide or azo compound can be used. Examples of organic peroxides include diacyl peroxides, peroxydicarbonates, peroxyesters, peroxyketals, dialkyl peroxides, hydroperoxides, and silyl peroxides. More specifically, cumyl peroxyneodecanoate, 1,1,3,3-tetramethylbutyl peroxyneodecanoate, 1-cyclohexyl-1-methylethyl peroxyneodecanoate, and t-hexyl peroxyneodecanoate. t-butyl peroxyneodecanoate, t-butyl peroxypivalate, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane, t-hexylperoxy-2-ethylhexanoate, t-butylperoxy-2-ethylhexanoate, t-butylperoxyneoheptanoate, t-amylperoxy-2-ethylhexanoate, di-t-butyl Peroxyhexahydroterephthalate, t-amylperoxy-3,5,5-trimethylhexanoate, 3-hydroxy-1,1-dimethylbutylperoxyneodecanoate, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, t-amylperoxyneodecanoate, t-amylperoxy-2-ethylhexanoate, t-hexylperoxyisopropylmonocarbonate, t-butylperoxymaleate, t-butylperoxy Oxy-3,5,5-trimethylhexanoate, t-butyl peroxylaurate, 2,5-dimethyl-2,5-di(3-methylbenzoylperoxy)hexane, t-butylperoxy-2-ethylhexylmonocarbonate, t-hexylperoxybenzoate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, t-butylperoxybenzoate, dibutylperoxytrimethyladipate, t-amylperoxynormaloctoate , t-amyl peroxyisononanoate, t-amyl peroxybenzoate, lauroyl peroxide, and the like.

[0060] Examples of azo compounds include 2,2'-azobis-2,4-dimethylvaleronitrile, 1,1'-azobis(1-acetoxy-1-phenylethane), 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), dimethyl-2,2'-azobisisobutyronitrile, 4,4'-azobis(4-cyanovaleric acid), and 1,1'-azobis(1-cyclohexanecarbonitrile).

[0061] The radical polymerization initiator may be used alone or in combination of two or more kinds.

[0062] (Antioxidants) The curable composition preferably further contains an antioxidant, which can suppress discoloration of the cured product due to heat, such as solder reflow. Specific examples of the antioxidant include phenol-based antioxidants such as 2,6-di-t-butylphenol, 2,6-di-t-butyl-p-cresol, n-octadecyl-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate, tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane, triethylene glycol bis[3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate], and 1,6-hexanediol bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate]. antioxidants; phosphorus-based antioxidants such as triphenyl phosphite, tris-isodecyl phosphite, tris-tridecyl phosphite, tris(2,4-di-t-butylphenyl) phosphite, and tetra(C12-15 alkyl)-4,4'-isopropylidenediphenyl diphosphite; and sulfur-based antioxidants such as dilauryl-3,3'-thiodipropionate, ditridecyl-3,3'-thiodipropionate, dimyristyl-3,3'-thiodipropionate, distereyl-3,3'-thiodipropionate, and pentaerythritol tetrakis(β-laurylthiopropionate). These antioxidants may be used alone or in combination of two or more.

[0063] <2. Method for producing organopolysiloxane composition> The method for producing the organopolysiloxane composition is not particularly limited, and the composition can be produced by mixing the organopolysiloxane represented by the above-mentioned general formula [1], the substance represented by general formula [2], and other optional components. In addition, when the substance represented by general formula [2] is produced in the organopolysiloxane production stage, it is not necessary to add the substance from the outside, and since the substance is contained in the composition obtained in the final stage of organopolysiloxane production, this can be used as the organopolysiloxane composition.

[0064] <3. Characteristics of organopolysiloxane composition, etc.> The properties of the organopolysiloxane composition and the like will now be described.

[0065] (1) 1 H-NMR 1 By using H-NMR, the amount of functional groups in organopolysiloxanes etc. can be measured. The measurement method is as follows. Approximately 50 mg of organopolysiloxane or a composition containing the same is weighed out and dissolved in approximately 1 g of deuterated acetone or deuterated dichloromethane; 1 A sample for H-NMR measurement is prepared. Using this sample for measurement, 1 The relaxation delay is measured in 20 seconds using H-NMR (e.g., AL-400 manufactured by JEOL Ltd.), and the ratio of the signal intensity of each component to the signal intensity of the internal standard and the weighted values ​​are used to determine the functional group (e.g., phenanthroline). The proportion of aryl groups, methyl groups, and organooxy groups is calculated. In the above measurements, impurities such as organic matter not bonded to organopolysiloxane, water, and metals must be removed to less than 0.1% by weight so as not to affect the measurement results. If the impurity content exceeds 0.1% by weight, it must be removed by distillation, filtration, or other purification methods before preparing the sample. 1Measure H-NMR. If removal is difficult, 1 The content of impurities is calculated by H-NMR measurement or other analytical methods, and the weight of the impurities is subtracted from the weighed sample weight to avoid calculating it as part of the organopolysiloxane, and this value is used as the true sample amount in the calculation. Note that, in addition to toluene, any substance that does not react with organopolysiloxane, such as N,N-dimethylformamide or tetrabromoethane, can be used as the internal standard.

[0066] (2) 29 Si-NMR 29 By using Si-NMR, the values ​​of M, D, T, and Q in the above general formula [1] can be calculated. The calculation method is as follows. Tris(2,4-pentanedionate)chromiumIII was added to deuterated chloroform to make the concentration 0.5% by mass. 29 A solvent for Si-NMR measurement is obtained. Next, about 1.5 g of the organopolysiloxane to be measured or a composition containing the same is weighed out, and the above 29 2.5 mL of a solvent for Si-NMR measurement was added to dissolve the sample, and the sample was placed in a 10 mmΦ Teflon (registered trademark) NMR sample tube. 29 Measurement is performed using Si-NMR (e.g., JNM-ECS400, TUNABLE(10), Si-free, AT10 probe manufactured by JEOL Ltd.) under the following measurement conditions, and the values ​​of M, D, T, and Q in the above general formula [1] are calculated from the signal intensity ratio. Measurement conditions: Relaxation Delay / 15 seconds, SCAN count / 1024 times, Measurement mode / Non-gated decoupled pulse method (NNE), Spin / None, Measurement temperature / 25℃

[0067] (3) Gel permeation chromatography (GPC) The number average molecular weight (Mn) and weight average molecular weight (Mw) of the organopolysiloxane can be calculated by gel permeation chromatography (GPC) according to the following method. Organopolysiloxane or a composition containing it is measured under the following conditions using GPC (for example, the apparatus is TOSOH HLC-8420GPC manufactured by Tosoh Corporation, and the columns are KF-G, KF-402.5HQ, KF-402HQ, and KF-401HQ manufactured by Showa Denko K.K.), and the values ​​are calculated in terms of standard polystyrene. The sample used is a tetrahydrofuran solution of about 10% by weight, which is filtered through a 0.45 μm filter before measurement. Column temperature: 40℃ Eluent: tetrahydrofuran, flow rate 0.3 mL / min

[0068] (4) Gas chromatography (GC) The amount of remaining organic solvent in an organopolysiloxane or a composition containing the same, and the content of the substance represented by general formula [2] can be measured by gas chromatography (GC). The measurement method is as follows. Organopolysiloxane or a composition containing it is measured under the following conditions using GC (for example, the apparatus is a 7820A gas chromatograph manufactured by Agilent Technologies, Inc., and the column is a DB-17ht, 0.25 mm x 30 m x 0.15 μm, manufactured by Agilent Technologies, Inc.). The sample is a tetrahydrofuran solution of about 50% by mass, and the internal standard substance is selected according to the purpose, such as methylcyclopentane, toluene, or tridecane. <Setting conditions> ·Inlet: 290℃ Pressure: 21.76psi (constant pressure) Oven program: 65℃(2minHold)→20℃ / min→325℃(40minHold) (Total 55min) Split ratio: 1 / 70 ·Injection volume: 0.5μL Detector: 290℃ <Carrier gas> Air flow rate: 350mL / min H2 flow rate: 35ml / min He flow rate: 20mL / min

[0069] (5) Solvent turbidity test The method for evaluating the mixing and dispersibility of the organopolysiloxane or the composition containing it with the resin is as follows. As the organic solvent, 11 g of tetraglyme with added water so that the water content was 10.5% by weight was prepared. This organic solvent and 1 g of organopolysiloxane were mixed and stirred at 25°C. If the organic solvent became transparent, it was judged that it had good mixing and dispersibility in the resin, and if the organic solvent became cloudy, it was judged that it had poor mixing and dispersibility in the resin. The purity of the tetraglyme used is confirmed to be 99.8% or more by gas chromatography, and the water content is confirmed by a Karl Fischer water content analyzer.

[0070] (6) Low boiling point component confirmation test It is preferable that the amount of organopolysiloxane in the organopolysiloxane composition is constant, that is, the organopolysiloxane composition is stable.As a method for evaluating the stability of this organopolysiloxane, when 200g of the organopolysiloxane composition is put into a 1L eggplant flask, and heated for 2 hours at an internal temperature of 110°C under reduced pressure with a vacuum pump having an exhaust capacity of a vacuum pressure of 0.15 torr, the mass loss of the organopolysiloxane is evaluated, and the mass loss is preferably 10g or less, more preferably 5g or less, and even more preferably 2g or less, and particularly preferably no loss is observed (below the detection limit). By making the weight loss amount under the above conditions equal to or less than the upper limit, the amount of volatilization of the substance represented by the general formula [2] during heat kneading with the resin is small, so that the resin and the desired organopolysiloxane composition can be uniformly dispersed, and the fluctuation in the content of the substance represented by the general formula [2] for each product lot can be suppressed. In addition, the flash point of the components contained in the organopolysiloxane can be kept relatively high, and the risk of a low flash point, which is difficult to handle safely under normal conditions, can be avoided. In addition, since the Fire Service Act hazard classification is classified as a lower or higher hazard, the cost of storage and transportation can be reduced. In addition, since the weight loss amount of the cured product during curing is also small, the temperature dependency of the storage elastic modulus of the cured product is small, the usable temperature range is wide, and embrittlement due to thinning is unlikely to occur. In addition, since the smaller the weight loss amount, the easier it is to obtain the above advantages, there is no preferable lower limit for the weight loss amount, but it is usually 0.0001g or more.

[0071] The weight loss upon heating under reduced pressure can be measured as follows. Organopolysiloxane composition as the measurement subject 1H-NMR is measured, and the weight of components other than the organopolysiloxane and the substance represented by general formula [2], such as the organic solvent, is calculated. Specifically, a rotor is placed in the eggplant flask, and the weights of these components are measured. The organopolysiloxane composition is then placed in the eggplant flask, and the weight of the organopolysiloxane composition is measured. The eggplant flask is heated in an oil bath, and the weight of the organopolysiloxane composition is measured using a magnetic stirrer. The rotor is rotated to stir the liquid surface until it becomes fluid, and the pressure is reduced using an oil vacuum pump. After 2 hours, the mixture is cooled to room temperature, the pressure is returned to normal, the oil adhering to the eggplant-shaped flask is thoroughly wiped off, and the weight of the organopolysiloxane composition in the eggplant-shaped flask is measured, and the weight of the eggplant-shaped flask and the rotor, which were previously measured, are subtracted to calculate the weight that has evaporated as a result of this operation. 1 1H-NMR was measured, and the weight of the organic solvent and other components other than the organopolysiloxane was calculated. 1 From the results of H-NMR and gas chromatography, the amount of components other than organopolysiloxane and the amount of volatilized organopolysiloxane are calculated from the weight of the volatilized matter. In addition, the volatilized distillate is entirely recovered using a cold trap or the like, and the weight and 1 H-NMR and gas chromatography may also be measured.

[0072] (7) Coloring when heated to 250℃ The coloring property was evaluated by adding 10 mg of a composition containing an organopolysiloxane to a hot plate heated to 250° C., and visually checking the coloring property after 10 minutes.

[0073] (8) Viscosity The viscosity is measured at a temperature of 25° C. using a viscometer (for example, RV-type viscometer RVDV-2+Pro manufactured by Brookfield) with the organopolysiloxane composition as the measurement object.

[0074] <4.Applications> The applications of the above-mentioned organopolysiloxane composition and the above-mentioned organopolysiloxane represented by the general formula [1] are not particularly limited, and they can be used, for example, in the applications shown below.

[0075] [Resin composition] The organopolysiloxane composition can be used as a resin composition in combination with other resins. The resin composition may contain the above-mentioned organopolysiloxane composition, and may be, for example, an embodiment in which the organopolysiloxane composition is added to a composition containing a resin, or an embodiment in which a resin is added to an organopolysiloxane composition. The manner of use of the resin composition is not particularly limited, and the resin composition may be used in the form of a composition itself, or may be used in the form of a cured product obtained by curing the composition.

[0076] The type of other resin contained in the resin composition containing the organopolysiloxane composition is not particularly limited, and examples thereof include organopolysiloxane resins other than the above-mentioned organopolysiloxanes, acrylic resins, polyolefin resins, polyvinyl chloride resins, polyester resins, polypropylene resins, polyethylene resins, polycarbonate resins, polybutylene terephthalate resins, polyethylene terephthalate resins, polyamide resins, PEEK resins, polyacetal resins, polyvinyl alcohol resins, and epoxy resins. However, the resins are required to be colorless and transparent, heat-resistant, light-resistant, and have low volatile components over time. For LED lighting applications, where colorless transparency, high Abbe and high refractive index, high glass transition temperature, heat resistance, and light resistance are required, it is suitable for use in organopolysiloxane compositions and epoxy resins because it can be contained without impairing performance; for camera lens applications, where colorless transparency, high Abbe and high refractive index, high glass transition temperature, heat resistance, and light resistance are required, it is suitable for use in acrylic resins because it can be contained without impairing performance; for polycarbonate resins, where colorless transparency, heat resistance during kneading, and flame retardancy due to the promotion of char formation are required; and for 3D applications, where colorless transparency, low viscosity, and short-term effectiveness are required, it is suitable for use in epoxy resins. Other suitable applications include flame retardants for thermoplastic resins, resin additives for 3D printers, additives for LED resins, and glass surface modifiers for vapor deposition.

[0077] The content of the organopolysiloxane composition in the resin composition is not particularly limited, but from the viewpoint of not changing the basic physical properties of the resin and imparting a certain function, it is preferable to add a very small amount, usually 0.01% by weight or more, preferably 0.1% by weight or more, more preferably 0.5% by weight or more, and usually 5% by weight or less, preferably 3% by weight or less, and more preferably 1% by weight or less. On the other hand, from the viewpoint of slightly changing the basic physical properties of the resin, it is preferable to add a small amount, usually 5% by weight or more, preferably 7% by weight or more, more preferably 10% by weight or more, and usually 20% by weight or less, preferably 17% by weight or less, and more preferably 15% by weight or less, and from the viewpoint of significantly changing the basic physical properties of the resin, it is 20% by weight or more, preferably 25% by weight or more, more preferably 30% by weight or more, and even more preferably 50% by weight or more, and usually 99% by weight or less, preferably 75% by weight or less, and more preferably 60% by weight or less.

[0078] [Organic solvent diluent] The organopolysiloxane composition can be used as an organic solvent dilution liquid in combination with an organic solvent. The organic solvent dilution liquid may contain the above-mentioned organopolysiloxane composition, and may be, for example, an embodiment in which the organopolysiloxane composition is added to a composition containing an organic solvent, or an embodiment in which an organic solvent is added to the organopolysiloxane composition. The type of organic solvent contained in the organic solvent dilution solution containing the organopolysiloxane composition is not particularly limited and may be selected arbitrarily. For example, a work-in-progress in which the organic solvent remains or one in which the organic solvent has been intentionally dissolved may be transferred to a container, sold, transported, or introduced into a reactor containing other substances.

[0079] [Electronic device components] The organopolysiloxane composition and its cured product, as well as the resin composition containing the organopolysiloxane composition and its cured product, can be used in electronic equipment members. Examples of electronic equipment members include LED lighting sealants and LED-related parts in which organopolysiloxane is used, covers for LED lighting, lens and camera members, smartphone cover members, voltage resistance improvers for electrolytic capacitors, members expressing a clicking sensation under the keys of a personal computer keyboard, and sealants for power device modules. The electronic equipment members may be in an embodiment consisting of only the cured product of the organopolysiloxane composition, or may be in an embodiment containing a part of the cured product of the organopolysiloxane composition. The conditions for curing the organopolysiloxane composition are not particularly limited, and the composition can be cured by a known method.

[0080] The content of the organopolysiloxane composition or its cured product in the electronic device member is not particularly limited, but from the viewpoint of not changing the basic physical properties of the resin used in the member and imparting a certain function, it is preferable to add a very small amount, usually 0.01% by weight or more, preferably 0.1% by weight or more, more preferably 0.5% by weight or more, and usually 5% by weight or less, preferably 3% by weight or less, and more preferably 1% by weight or less, which corresponds to cover members for LED lighting and cover members for smartphones. On the other hand, from the viewpoint of slightly changing the basic physical properties of the resin used in the member, it is preferable to add a small amount, usually 5% by weight or more, preferably 7% by weight or more, and more preferably 10% by weight or more, and usually 20% by weight or less, preferably 17% by weight or less, and more preferably 15% by weight or less, which corresponds to sealing materials for LED lighting and sealing materials for power device modules. From the viewpoint of significantly changing the basic physical properties of the resin used in the member, it is preferable to add 20% by weight or more, preferably 25% by weight or more, and more preferably 30% by weight or less. % or more, more preferably 50% or more by weight, and usually 99% or less by weight, preferably 75% or less by weight, more preferably 60% or less by weight, which corresponds to lenses and camera parts.

[0081] <Other uses> In addition to the uses described above, the organopolysiloxane composition can be used for other uses, such as a non-reactive viscosity modifier, a reactive viscosity modifier, a compatibilizer, a lubricant, a dispersant, a flocculating agent, an adhesive, a pressure-sensitive adhesive, a release agent, a water repellent, an oil repellent, a coating agent, a surface modifier, a metal surface repair agent, a flame retardant, an agent for reducing squeak noise, a sealing material or substrate for semiconductor devices including inorganic or organic light-emitting elements, a coating material, and an optical component. EXAMPLES

[0082] The present invention will be described in more detail below with reference to examples, but the present invention should not be construed as being limited to the following examples. In the following description, "parts" refers to "parts by weight" based on weight unless otherwise specified.

[0083] <Method of Evaluating Organopolysiloxane Composition> The organopolysiloxane and / or organopolysiloxane composition were evaluated by the following methods.

[0084] (1) 1 H-NMR Approximately 50 mg of the resulting organopolysiloxane was weighed out and dissolved in approximately 1 g of deuterated acetone or deuterated dichloromethane. 1 A sample was prepared for H-NMR measurement. 1 The relaxation delay was measured at 20 seconds using H-NMR (AL-400, manufactured by JEOL Ltd.). The proportions of phenyl groups, methyl groups, and organoxy groups were calculated from the ratios of the signal intensity of each component to the signal intensity of the internal standard and the weighed values.

[0085] (2) 29 Si-NMR Tris (2,4-pentanedionate) chromium III was added to deuterated chloroform to make it 0.5% by mass. 29 A solvent for Si-NMR measurement was obtained. Approximately 1.5 g of the organopolysiloxane to be measured was weighed out and mixed with the above solvent. 29 2.5 mL of the Si-NMR measurement solvent was added to dissolve the sample, and the sample was placed in a 10 mm diameter Teflon (registered trademark) NMR sample tube. Measurements were performed using the following equipment and conditions, and the values ​​of M, D, T, and Q in the above general formula [1] were calculated from the signal intensity ratio. Equipment: JNM-ECS400 manufactured by JEOL Ltd., TUNABLE(10), Si-free, AT10 probe Measurement conditions: Relaxation Delay / 15 seconds, SCAN count / 1024 times, Measurement mode / Non-gated decoupled pulse method (NNE), Spin / None, Measurement temperature / 25℃

[0086] (3) Gel permeation chromatography (GPC) The number average molecular weight (Mn), weight average molecular weight (Mw), and molecular weight distribution (Mw / Mn) of organopolysiloxanes were measured using gel permeation chromatography (GPC) under the following conditions, and are shown as values ​​converted into standard polystyrene. The sample used was a 10% by weight tetrahydrofuran solution, which was filtered through a 0.45 μm filter before measurement. Equipment: TOSOH HLC-8420GPC (manufactured by Tosoh Corporation) Column: KF-G, KF-402.5HQ, KF-402HQ, KF-401HQ (all manufactured by Showa Denko K.K.), column temperature 40°C Eluent: tetrahydrofuran, flow rate 0.3 mL / min

[0087] (4) Gas chromatography (GC) To confirm the amount of organic solvent remaining in the organopolysiloxane and the content of the substance represented by the general formula [2], measurements were performed using gas chromatography (GC) under the following conditions: A tetrahydrofuran solution of approximately 50% by mass was used as the sample, and methylcyclopentane was used as the internal standard substance. Equipment: Agilent Technologies 7820A gas chromatograph Column: Agilent Technologies DB-17ht, 0.25 mm x 30 m x 0.15 μm <Setting conditions> ·Inlet: 290℃ Pressure: 21.76 psi (constant pressure) Oven program: 65℃(2minHold)→20℃ / min→325℃(40minHold) (Total 55min) Split ratio: 1 / 70 ·Injection volume: 0.5μL Detector: 290℃ <Carrier gas> Air flow rate: 350ml / min H2 flow rate: 35mL / min He flow rate: 20mL / min

[0088] (5) Solvent turbidity test In order to evaluate the mixing and dispersibility of organopolysiloxane with resin, a mixing test with organic solvent was carried out. As an organic solvent, 11 g of tetraglyme with water added so that the water content was 10.5 wt % was prepared, and the organic solvent and 1 g of organopolysiloxane were mixed and stirred at 25°C, and the transparent one was judged to have good mixing and dispersibility in resin, and the cloudy one was judged to have bad mixing and dispersibility in resin.

[0089] (6) Low boiling point component confirmation test 200 g of the organopolysiloxane composition was placed in a 1 L eggplant-shaped flask and heated for 2 hours at an internal temperature of 110°C under reduced pressure using a vacuum pump with an exhaust capacity of 0.15 torr, and the mass loss rate was confirmed using a balance. A mass loss rate of 5% by weight or less was determined to have no effect on moldability, and a weight loss rate of more than 5% by weight was determined to have an effect on moldability. The weight loss during heating under reduced pressure was measured by the following method. Organopolysiloxane composition as the measurement subject 1H-NMR was measured, and the weight of components other than organopolysiloxane, such as organic solvent, was calculated. Specifically, a rotor was placed in an eggplant-shaped flask, and their weights were measured. Then, the organopolysiloxane composition was placed in the eggplant-shaped flask, and the weight of the organopolysiloxane composition was measured. The eggplant-shaped flask was heated in an oil bath, the rotor was rotated with a magnetic stirrer to stir the liquid surface to a degree that it was moving, and the pressure was reduced with an oil-type vacuum pump. After 2 hours, the flask was cooled to room temperature, the pressure was returned to normal pressure, the oil adhering to the eggplant-shaped flask was thoroughly wiped off, and the weight of the organopolysiloxane composition in the eggplant-shaped flask was measured, and the weight of the eggplant-shaped flask and the rotor that had been measured earlier were subtracted to calculate the weight that had evaporated by the operation. The weight of the organopolysiloxane composition after the operation was 1 H-NMR was measured, and the weights of the organic solvent and other components other than the organopolysiloxane were calculated. 1 From the results of H-NMR measurement, the amounts of components other than organopolysiloxane and the amount of volatilized organopolysiloxane were calculated from the weight of the volatilized components.

[0090] (7) Coloring when heated to 250℃ 10 mg of organopolysiloxane was added to a hot plate heated to 250°C, and the coloring was visually confirmed after 10 minutes.

[0091] (8) Viscosity The viscosity was measured at a temperature of 25° C. using an RV-type viscometer RVDV-2+Pro manufactured by Brookfield Instruments, with the organopolysiloxane composition as the measurement subject.

[0092] <Raw materials used in the production of organopolysiloxane> The raw materials used in the production of the organopolysiloxane are shown below. Hexamethyldisiloxane (NuSil Technology) Phenyltrimethoxysilane (KBM-103, manufactured by Shin-Etsu Chemical Co., Ltd.) Toluene (Kishida Chemical Co., Ltd.) Methanol (Kishida Chemical Co., Ltd.) Heptane (Kishida Chemical Co., Ltd.) 1N hydrochloric acid (Kishida Chemical Co., Ltd.) 2N potassium hydroxide solution (Kishida Chemical Co., Ltd.)

[0093] <Production Example 1 (Production Method of Organopolysiloxane Composition 1)> 32 parts of hexamethyldisiloxane, 73 parts of phenyltrimethoxysilane, 19 parts of toluene and 19 parts of methanol as the raw materials for organopolysiloxane 1, 15 parts of 1N hydrochloric acid as the catalyst and reaction substrate were used, and hydrolysis and condensation were carried out at 40°C for 7 hours. 13 parts of 2N potassium hydroxide aqueous solution were added, and the reaction was further carried out at 40°C for 2 hours. After removing the potassium component by washing with hydrochloric acid and demineralized water, low boiling point components such as the solvent were distilled off while heating to 80°C using a diaphragm pump. At this time, toluene, methanol, and water were removed to obtain an organopolysiloxane composition. It was confirmed by gas chromatography that the organopolysiloxane composition contained about 3% by weight of tris(trimethylsilyloxy)phenylsilane, which corresponds to the substance represented by the general formula [2]. Thereafter, while heating to a high temperature of 120° C. to 140° C., distillation was continued under high vacuum conditions until toluene peaks were no longer detected, yielding organopolysiloxane composition 1 which is liquid at room temperature.

[0094] The molecular weight of the obtained organopolysiloxane composition 1 was measured, and it was confirmed that the polystyrene-equivalent number average molecular weight (Mn) was 890, the weight average molecular weight (Mw) was 955, and the molecular weight distribution (Mw / Mn) was 1.07. Also, 1 Analysis by H-NMR showed that the amount of phenyl groups was 5.0 mmol / g, the amount of trimethylsiloxy groups was 4.4 mmol / g, and the amount of methoxy groups was 0.31 mmol / g. 29 As a result of Si-NMR measurement, it was confirmed that the values ​​of silicon structural units M, D, T, and Q were M = 0.46, D = 0, T = 0.54, and Q = 0, respectively. This is because in the general formula [1], M1 = 0.46, T1 = 0.54, E1 = 0.035, and R 4is a phenyl group, and the other R 1 ~R 3 , R 5 is a methyl group. In addition, gas chromatography confirmed that the organopolysiloxane composition contained no traces of methanol or toluene, which were used as solvents, and contained 2.1% by weight of tris(trimethylsilyloxy)phenylsilane, which is represented by the general formula [2]: 9 is a phenyl group, and R 6 ~R 8 It was confirmed that the substance contained was a methyl group with coefficients T2 = 1, M2 = 3, and E2 = 0.

[0095] <Production Example 2 (Production Method of Organopolysiloxane Composition 2)> The distillation of organopolysiloxane composition 1 was continued under high temperature and high vacuum conditions to obtain organopolysiloxane composition 2. In organopolysiloxane composition 2, tris(trimethylsilyloxy)phenylsilane, which corresponds to the substance represented by general formula [2], was not detected. The molecular weight of the obtained organopolysiloxane composition 2 was measured, and the polystyrene-equivalent number average molecular weight (Mn) was 901, the weight average molecular weight (Mw) was 960, and the molecular weight distribution (Mw / Mn) was 1.07. 1 As a result of H-NMR analysis, the amount of phenyl groups was 5.1 mmol / g, the amount of trimethylsiloxy groups was 4.3 mmol / g, and the amount of methoxy groups was 0.26 mmol / g. This corresponds to M1 = 0.45, T1 = 0.55, E1 = 0.033, and R 4 is a phenyl group, and the other R 1 From R 5 means a methyl group.

[0096] <Production Example 3 (Production Method of Organopolysiloxane Composition 3)> Organopolysiloxane composition 3 was produced under the same production conditions as in Production Example 1, except that the stirring efficiency during the reaction was improved. The molecular weight of the obtained organopolysiloxane composition 3 was measured, and it was confirmed that the polystyrene-equivalent number average molecular weight (Mn) was 905, the weight average molecular weight (Mw) was 976, and the molecular weight distribution (Mw / Mn) was 1.08. 1 As a result of H-NMR analysis, the amount of phenyl groups was 5.2 mmol / g, the amount of trimethylsiloxy groups was 4.2 mmol / g, and the amount of methoxy groups was 0.31 mmol / g. This corresponds to M1 = 0.45, T1 = 0.55, E1 = 0.033, and R 4 is a phenyl group, and the other R 1 From R 5 was confirmed to be a methyl group. Furthermore, gas chromatography confirmed that neither methanol nor toluene, which were used as solvents, was detected in organopolysiloxane composition 3, and that it contained 0.6% by weight of tris(trimethylsilyloxy)phenylsilane. This is the general formula [2], 9 is a phenyl group, and R 6 From R 8 is a methyl group, and the substance contains coefficients T2 = 1, M2 = 3, and E2 = 0.

[0097] <Production Example 4 (Production Method of Organopolysiloxane Composition 4)> Organopolysiloxane composition 4 was produced under the same production conditions as in Production Example 1, except that hydrolysis and condensation were carried out at 40°C for 7 hours, followed by aging at room temperature for 14 hours. The molecular weight of the obtained organopolysiloxane composition 4 was measured, and it was confirmed that the number average molecular weight (Mn) was 926, the weight average molecular weight (Mw) was 1059, and the molecular weight distribution (Mw / Mn) was 1.14, calculated based on polystyrene. 1 As a result of H-NMR analysis, the amount of phenyl groups was 5.2 mmol / g, the amount of trimethylsiloxy groups was 4.1 mmol / g, and the amount of methoxy groups was 0.27 mmol / g. This corresponds to M1 = 0.44, T1 = 0.56, E1 = 0.029, and R 4is a phenyl group, and the other R 1 ~R 5 is a methyl group. Furthermore, gas chromatography confirmed that the organopolysiloxane composition contained no traces of methanol or toluene, which were used as solvents, and contained 1.3% by weight of tris(trimethylsilyloxy)phenylsilane. This is the organopolysiloxane represented by the general formula [2], R 9 is a phenyl group, and R 6 From R 8 is a methyl group, and the substance contains coefficients T2 = 1, M2 = 3, and E2 = 0.

[0098] The organopolysiloxanes and compositions produced by the above-mentioned production methods were evaluated and the results are shown in the following table, where tris(trimethylsilyloxy)phenylsilane is abbreviated as PTTSS.

[0099] [Table 1]

[0100] <Production Example 5 (Production Method of Organopolysiloxane Composition 5)> Organopolysiloxane composition 5 was produced under the same production conditions as in Production Example 1, except that when produced based on Production Example 1, the organopolysiloxane composition prior to the step of distilling off the solvent was used as work-in-progress 5, and potassium hydroxide was distilled off while still adhering to the inside of the kettle in the step of distilling off the solvent from work-in-progress 5. The molecular weight of the obtained organopolysiloxane composition 5 was measured, and the polystyrene-equivalent number average molecular weight (Mn) was 937, the weight average molecular weight (Mw) was 1049, and the molecular weight distribution (Mw / Mn) was 1.12. 1 As a result of H-NMR analysis, the amount of phenyl groups was 5.1 mmol / g, the amount of trimethylsiloxy groups was 4.4 mmol / g, and the amount of methoxy groups was 0.31 mmol / g. This corresponds to M1 = 0.46, T1 = 0.54, E1 = 0.033, and R 4 is a phenyl group, and the other R 1 From R5 is a methyl group. Furthermore, by gas chromatography, the organopolysiloxane composition was found to contain no methanol or toluene, which were used as solvents, and contained 1.8% by weight of tris(trimethylsilyloxy)phenylsilane. This is the organopolysiloxane represented by the general formula [2]: R 9 is a phenyl group, and R 6 From R 8 is a methyl group, and the coefficients T2 = 1, M2 = 3, and E2 = 0 are satisfied.

[0101] <Production Example 6 (Production Method of Organopolysiloxane Composition 6)> When producing based on Production Example 1, the composition prior to the step of distilling off the solvent was designated work-in-progress 6, and potassium hydroxide was added to work-in-progress 6 so that the concentration was 2 ppm. Organopolysiloxane composition 6 was produced by applying the same production conditions as in Production Example 1 for the steps after the distillation. The molecular weight of the resulting organopolysiloxane composition 6 was measured, and the polystyrene-equivalent number average molecular weight (Mn) was 963, the weight average molecular weight (Mw) was 1118, and the molecular weight distribution (Mw / Mn) was 1.16.

[0102] <Production Example 7 (Production Method of Organopolysiloxane Composition 7)> Organopolysiloxane Composition 7 was produced under the same production conditions as in Production Example 6, except that the potassium hydroxide concentration in Work in Process 6 was 0.2 ppm. The molecular weight of the resulting organopolysiloxane composition 7 was measured, and the polystyrene-equivalent number average molecular weight (Mn) was 899, the weight average molecular weight (Mw) was 965, and the molecular weight distribution (Mw / Mn) was 1.07.

[0103] The evaluation results of the organopolysiloxane compositions used in the examples are shown in Tables 2 to 4. In the examples, PTTSS stands for tris(trimethylsiloxy)phenylsilane.

[0104] [Table 2]

[0105] From Table 2, it was suggested that the viscosity can be adjusted by adding a substance represented by general formula [2] to an organopolysiloxane composition consisting of general formula [1], or by leaving it as an organopolysiloxane composition, and that the substance has transparent mixing with resin, does not have an odor, and does not color when heated, and that even if it is contained at 7.5% by weight, the amount of low-boiling point components volatilized is small, and does not affect the process problem during molding or the deterioration of the properties of the molded product, but if it is contained at 10% by weight or more, the amount of volatilization increases and may become a problem. In addition, when toluene is used as a solvent, even at 5% by weight, the entire amount volatilizes, suggesting that even if the viscosity can be reduced, the adverse effect is large when a general organic solvent is used, and it was surprisingly found that the substance represented by general formula [2] has a very low volatilization rate from the organopolysiloxane composition consisting of general formula [1].

[0106] [Table 3]

[0107] Table 3 shows that it is possible to adjust the viscosity by adding the component represented by general formula [2] to the high-viscosity organopolysiloxane composition represented by general formula [1]. In addition, the results of the solvent clouding test suggest that it can be mixed with resin without affecting its mixability.

[0108] [Table 4]

[0109] [Table 5]

[0110] From Tables 4 and 5, it was found that in the method for producing organopolysiloxane, when potassium hydroxide is included during the heating operation, the molecular weight and molecular weight distribution increase and the compatibility with the resin changes depending on the content. The content of potassium hydroxide in the organopolysiloxane composition is preferably 2 ppm or less, more preferably 0.2 ppm or less. On the other hand, when it is desired to express the function by adjusting the dispersibility with the resin, it is also possible to adjust the molecular weight by increasing the potassium hydroxide content, and in that case, as shown in Table 3, it was suggested that the compound represented by the general formula [2] does not change the mixed dispersibility.

[0111] As described above, the present invention can provide an organopolysiloxane composition that has low viscosity and excellent dispersibility in various resins, and a method for producing the same.

Claims

1. A resin composition comprising an organopolysiloxane composition and another resin, The organopolysiloxane composition comprises: Component A is an organopolysiloxane represented by the following general formula [1], having a molecular weight distribution (Mw / Mn) of 1.01 to 1.08 and a number average molecular weight of 700<Mn<2000; Component B includes a substance represented by the following general formula [2]: The component A and the component B satisfy the relationship of 0.1≦{(weight of component B)×100} / {(weight of component A)+(weight of component B)}≦9, and With respect to the component A, the content of a substance in which the coefficients T2, M2, and E2 in the formula [2] satisfy T2+2-M2+E2=0 is 0.01% by weight or more and 9% by weight or less, and the content of a substance in which the coefficients T2, M2, and E2 in the formula [2] do not satisfy T2+2-M2+E2=0 is 3% by weight or less, The other resin is a resin having a (meth)acryloyl group or a polycarbonate. (R 1 R 2 R 3 SiO 1/2 ) M1 (R 4 SiO 3/2 ) T1 (SiO 4/2 ) Q (O 1/2 R 5 ) E1 ・・・[1] (R 6 R 7 R 8 SiO 1/2 ) M2 (R 9 SiO 3/2 ) T2 (O 1/2 R 10 ) E2 ・・・[2] Here, in the above formula [1], R 1 ~R 4 are each independently selected from the group consisting of a (meth)acrylic group, a carboxyl group, a nitrile group, a formyl group, a carbonyl group, a carbinol group, an amino group, an imino group, a nitro group, a cyano group, a sulfo group, a mercapto group, an alkyl group having 1 to 20 carbon atoms, a cyclopentyl group, a cyclohexyl group, an ethylene glycol monoethylene ether group, an acryloxypropyl group, an acryloxyoctyl group, a methacryloxypropyl group, a methacryloxyoctyl group, a glycidyl group, a glycidoxypropyl group, a glycidoxyoctyl group, a 1,2-epoxycyclohexyl-3-propyl group, a 1,2-epoxycyclohexyl-3-octyl group, a phenyl group, a phenethylene group, and a styryl group, and may be the same or different. Also well; R 5 are selected from the group consisting of a hydrogen atom, a methyl group, an ethyl group, a butyl group, an octyl group, and an octadecyl group, and may be the same or different; The coefficients M1, T1, and Q are each independently equal to or greater than 0 and less than 0.65, and M1+T1+Q=1 is satisfied; The coefficients M1, T1, Q, and E1 satisfy 0<T1+Q<0.65, 0.25<T1, and 0<E1 / (M1+E1)<1. Here, in the above formula [2], R 6 ~R 9 each independently represents a (meth)acrylic group, a carboxyl group, a nitrile group, a formyl group, a carbonyl group, a carbinol group, an amino group, an imino group, a nitro group, a cyano group, a sulfo group, a mercapto group, an alkyl group having 1 to 20 carbon atoms, a cyclopentyl group, a cyclohexyl group, an ethylene glycol monoethylene ether group, an acryloxypropyl group, an acryloxyoctyl group, a methacryloxypropyl group, a methacryloxyoctyl group, a glycidyl group, a glycidoxypropyl group, a glycidoxyoctyl group, a 1,2-epoxycyclohexyl-3-propyl group, a 1,2-epoxycyclohexyl-3-octyl group, a phenyl group, are selected from the group consisting of aryl, phenethylene, and styryl groups, and may be the same or different; R 10 are selected from the group consisting of a hydrogen atom, a methyl group, an ethyl group, a butyl group, an octyl group, and an octadecyl group, and may be the same or different; M2 is a positive integer from 1 to 5; coefficient T2 is a positive integer from 1 to 3; and coefficient E2 is an integer from 0 to 5.

2. In the general formula [1], the R 4 The resin composition according to claim 1, wherein the organic group represented by the formula (I) is a phenyl group.

3. 3. The resin composition according to claim 1, wherein the coefficient M1 is 0.40 or more and 0.55 or less, and the coefficient T1 is 0.45 or more and 0.58 or less.

4. The resin composition according to any one of claims 1 to 3, wherein the coefficient E1 is 0.01 or more and 0.1 or less.

5. The R 1 ~R 3 The resin composition according to any one of claims 1 to 4, characterized in that is a methyl group.

6. The resin composition according to any one of claims 1 to 5, characterized in that when 200 g of the organopolysiloxane composition is placed in a 1 L eggplant-shaped flask and heated for 2 hours at an internal temperature of 110°C under reduced pressure using a vacuum pump having an exhaust capacity of a vacuum pressure of 0.15 torr, the amount of mass loss of the organopolysiloxane is 10 g or less.

7. The resin composition according to any one of claims 1 to 6, wherein the coefficient Q is 0.

8. In the general formula [2], R 9 The resin composition according to any one of claims 1 to 7, wherein is a phenyl group.

9. In the general formula [2], R 6 ~R 8 The resin composition according to any one of claims 1 to 8, wherein is a methyl group.

10. The resin composition according to any one of claims 1 to 9, characterized in that the resin composition contains a substance having a coefficient T2 of 1 as the substance represented by the general formula [2].

11. The resin composition according to any one of claims 1 to 10, characterized in that the resin composition contains a substance having a coefficient M2 of 3 as the substance represented by the general formula [2].

12. The resin composition according to any one of claims 1 to 11, characterized in that the content of the substance represented by the general formula [2] in the organopolysiloxane composition is 0.5 to 3 wt%.

13. 13. The resin composition according to claim 1, wherein the content of the organopolysiloxane composition in the resin composition is 15% by weight or less.

14. the other resin is the resin having a (meth)acryloyl group, The R 1 to R 3 are all methyl groups, R 4 is selected from the group consisting of acryloxypropyl, methacryloxypropyl, methacryloxyoctyl, glycidoxypropyl, glycidoxyoctyl, and phenyl groups; The R6 to R 8 are all methyl groups, R 9 The resin composition according to claim 1 , wherein is selected from the group consisting of an acryloxypropyl group, a methacryloxypropyl group, a methacryloxyoctyl group, a glycidoxypropyl group, a glycidoxyoctyl group, and a phenyl group.

15. the other resin is the polycarbonate, The R 1 to R 3 are all methyl groups, The R 4 is a phenyl group, The R6 to R 8 are all methyl groups, The R 9 The resin composition according to claim 1 , wherein is a phenyl group.

16. A member for electronic equipment, comprising the resin composition according to any one of claims 1 to 15 or a cured product thereof.

17. A resin additive comprising an organopolysiloxane composition, The organopolysiloxane composition comprises: Component A is an organopolysiloxane represented by the following general formula [1], having a molecular weight distribution (Mw / Mn) of 1.01 to 1.08 and a number average molecular weight of 700<Mn<2000; Component B includes a substance represented by the following general formula [2]: The component A and the component B satisfy the relationship of 0.1≦{(weight of component B)×100} / {(weight of component A)+(weight of component B)}≦9, and A resin additive, characterized in that, relative to component A, a content of a substance in which coefficients T2, M2, and E2 in formula [2] satisfy T2+2-M2+E2=0 is 0.01% by weight or more and 9% by weight or less, and a content of a substance in which coefficients T2, M2, and E2 in formula [2] do not satisfy T2+2-M2+E2=0 is 3% by weight or less. (R 1 R 2 R 3 SiO 1/2 ) M1 (R 4 SiO 3/2 ) T1 (SiO 4/2 ) Q (O 1/2 R 5 ) E1 ・・・[1] (R 6 R 7 R 8 SiO 1/2 ) M2 (R 9 SiO 3/2 ) T2 (O 1/2 R 10 ) E2 ・・・[2] Here, in the above formula [1], R 1 ~R 4 each independently represents a (meth)acrylic group, a carboxyl group, a nitrile group, a formyl group, a carbonyl group, a carbinol group, an amino group, an imino group, a nitro group, a cyano group, a sulfo group, a mercapto group, an alkyl group having 1 to 20 carbon atoms, a cyclopentyl group, a cyclo are selected from the group consisting of a hexyl group, an ethylene glycol monoethylene ether group, an acryloxypropyl group, an acryloxyoctyl group, a methacryloxypropyl group, a methacryloxyoctyl group, a glycidyl group, a glycidoxypropyl group, a glycidoxyoctyl group, a 1,2-epoxycyclohexyl-3-propyl group, a 1,2-epoxycyclohexyl-3-octyl group, a phenyl group, a phenethylene group, and a styryl group, and may be the same or different; R 5 are selected from the group consisting of a hydrogen atom, a methyl group, an ethyl group, a butyl group, an octyl group, and an octadecyl group, and may be the same or different; The coefficients M1, T1, and Q are each independently equal to or greater than 0 and less than 0.65, and M1+T1+Q=1 is satisfied; The coefficients M1, T1, Q, and E1 satisfy 0<T1+Q<0.65, 0.25<T1, and 0<E1 / (M1+E1)<1. Here, in the above formula [2], R 6 ~R 9 each independently represents a (meth)acrylic group, a carboxyl group, a nitrile group, a formyl group, a carbonyl group, a carbinol group, an amino group, an imino group, a nitro group, a cyano group, a sulfo group, a mercapto group, an alkyl group having 1 to 20 carbon atoms, a cyclopentyl group, a cyclohexyl group, an ethylene glycol monoethylene ether group, an acryloxypropyl group, an acryloxyoctyl group, a methacryloxypropyl group, a methacryloxyoctyl group, a glycidyl group, a glycidoxypropyl group, a glycidoxyoctyl group, a 1,2-epoxycyclohexyl-3-propyl group, a 1,2-epoxycyclohexyl-3-octyl group, a phenyl group, are selected from the group consisting of aryl, phenethylene, and styryl groups, and may be the same or different; R 10 are selected from the group consisting of a hydrogen atom, a methyl group, an ethyl group, a butyl group, an octyl group, and an octadecyl group, and may be the same or different; M2 is a positive integer from 1 to 5; coefficient T2 is a positive integer from 1 to 3; and coefficient E2 is an integer from 0 to 5.

18. 1. An organopolysiloxane composition for use in a resin, comprising: Component A is an organopolysiloxane represented by the following general formula [1], having a molecular weight distribution (Mw / Mn) of 1.01 to 1.08 and a number average molecular weight of 700<Mn<2000; Component B includes a substance represented by the following general formula [2]: The component A and the component B satisfy the relationship of 0.1≦{(weight of component B)×100} / {(weight of component A)+(weight of component B)}≦9, and an organopolysiloxane composition for use as an additive to a resin, characterized in that the content of substances in which the coefficients T2, M2, and E2 in formula [2] satisfy T2+2-M2+E2=0 is 0.01% by weight or more and 9% by weight or less, and the content of substances in which the coefficients T2, M2, and E2 in formula [2] do not satisfy T2+2-M2+E2=0 is 3% by weight or less, relative to component A: (R 1 R 2 R 3 SiO 1/2 ) M1 (R 4 SiO 3/2 ) T1 (SiO 4/2 ) Q (O 1/2 R 5 ) E1 ・・・[1] (R 6 R 7 R 8 SiO 1/2 ) M2 (R 9 SiO 3/2 ) T2 (O 1/2 R 10 ) E2 ・・・[2] Here, in the above formula [1], R 1 ~R 4 each independently represents a (meth)acrylic group, a carboxyl group, a nitrile group, a formyl group, a carbonyl group, a carbinol group, an amino group, an imino group, a nitro group, a cyano group, a sulfo group, a mercapto group, an alkyl group having 1 to 20 carbon atoms, a cyclopentyl group, a cyclohexyl group, an ethylene glycol monoethylene ether group, an acryloxypropyl group, an acryloxyoctyl group, a methacryloxypropyl group, a methacryloxyoctyl group, a glycidyl group, a glycidoxypropyl group, a glycidoxyoctyl group, a 1,2-epoxycyclohexyl group, 1,2-epoxycyclohexyl-3-propyl group, 1,2-epoxycyclohexyl-3-octyl group, phenyl group, phenethylene group, and styryl group, which may be the same or different; R 5 are selected from the group consisting of a hydrogen atom, a methyl group, an ethyl group, a butyl group, an octyl group, and an octadecyl group, and may be the same or different; The coefficients M1, T1, and Q are each independently equal to or greater than 0 and less than 0.65, and M1+T1+Q=1 is satisfied; The coefficients M1, T1, Q, and E1 satisfy 0<T1+Q<0.65, 0.25<T1, and 0<E1 / (M1+E1)<1. Here, in the above formula [2], R 6 ~R 9 each independently represents a (meth)acrylic group, a carboxyl group, a nitrile group, a formyl group, a carbonyl group, a carbinol group, an amino group, an imino group, a nitro group, a cyano group, a sulfo group, a mercapto group, an alkyl group having 1 to 20 carbon atoms, a cyclopentyl group, a cyclohexyl group, an ethylene glycol monoethylene ether group, an acryloxypropyl group, an acryloxyoctyl group, a methacryloxypropyl group, a methacryloxyoctyl group, a glycidyl group, a glycidoxypropyl group, a glycidoxyoctyl group, a 1,2-epoxycyclohexyl-3-propyl group, a 1,2-epoxycyclohexyl-3-octyl group, a phenyl group, are selected from the group consisting of aryl, phenethylene, and styryl groups, and may be the same or different; R 10 are selected from the group consisting of a hydrogen atom, a methyl group, an ethyl group, a butyl group, an octyl group, and an octadecyl group, and may be the same or different; M2 is a positive integer from 1 to 5; coefficient T2 is a positive integer from 1 to 3; and coefficient E2 is an integer from 0 to 5.

19. 19. The organopolysiloxane composition for use in a resin additive according to claim 18, which is added to any one of resins selected from the group consisting of resins having a (meth)acryloyl group and polycarbonates.

Citation Information

Patent Citations

  • Organosiloxane composition

    JP1997111123A

  • Polysiloxane

    JP2014074183A

  • Curable silicon composition, cured product thereof, and optical semiconductor device

    WO2013005858A1

  • Polyorganosiloxane, polyorganosiloxane composition, cured product, polyorganosiloxane-containing electrolytic solution for electrolytic capacitor, and electrolytic capacitor using same

    WO2018110613A1