Resin composition, electronic device member, resin additive, and organopolysiloxane composition for use as an additive in resin
The formulation of a low-volatility organopolysiloxane composition addresses dispersion and viscosity issues, ensuring uniform mixing and safety in resin applications, enhancing product quality and reducing environmental impact.
Patent Information
- Application Number
- JP2020065041
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-31
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-03-31
AI Technical Summary
Existing organopolysiloxane compositions face challenges in uniform dispersion and high viscosity, leading to uneven physical properties, flammability, and environmental hazards due to solvent volatilization, which affect the quality and safety of molded products.
A specific organopolysiloxane composition is formulated with a substance that has low volatility and adjusts viscosity, ensuring uniform dispersion and stability, reducing environmental impact and improving safety.
The composition achieves low viscosity and excellent dispersibility in various resins, maintaining product quality and safety without environmental hazards, facilitating easier handling and reduced waste treatment efforts.
Smart Images

Figure 0007574544000001 
Figure 0007574544000002 
Figure 0007574544000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an organopolysiloxane, and more particularly to an organopolysiloxane composition which is used in combination with other resins. [Background technology]
[0002] In recent years, organic-inorganic composite materials have been attracting attention, and development has been carried out with the aim of improving properties by mixing silicon materials into resins.For example, Patent Document 1 discloses an organopolysiloxane that has a narrow molecular weight distribution and is in a low-viscosity liquid state at room temperature, making it easy to mix with other resins, does not contain volatile low-molecular weight components, making it easy to handle, and has excellent properties when cured.By devising the functional groups of this liquid organopolysiloxane with a low molecular weight and narrow molecular weight distribution, various functions have been imparted to various resins. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2018 / 110613 Summary of the Invention [Problem to be solved by the invention]
[0004] In order to effectively exert the functions of the organopolysiloxane in the resin, it is important to uniformly mix and disperse the resin and the organopolysiloxane, and it is necessary to prepare a composition in a form that allows the organopolysiloxane to be easily mixed and dispersed in the resin prior to molding. However, problems arise due to the difficulty in uniformly dispersing the organopolysiloxane, such as the precipitation of certain components when the organopolysiloxane is mixed with a resin that has already been mixed with various additives, and the difficulty in diffusing the organopolysiloxane when the organopolysiloxane is mixed with a resin that has been increased in molecular weight due to the high viscosity of the resin, resulting in a concentration gradient of the organopolysiloxane in the composition and resulting in uneven physical properties of the molded product. In such cases, it is possible to improve the dispersibility of the organopolysiloxane by using a liquid organopolysiloxane composition that has a narrow molecular weight distribution and is free of volatile low molecular weight components, diluting it with an organic solvent, and mixing it; however, some of the advantages that were present before the addition of the organopolysiloxane are lost, for example, due to the danger of flammable vapor volatilizing when the mold is released during molding, the condensed organic solvent redissolving the molded product, whitening it and causing a poor appearance, poor curing due to a decrease in temperature caused by the evaporation of the organic solvent, a decrease in the melting point of the resin due to the organic solvent remaining in the molded product, shrinkage over time caused by the gradual evaporation of the organic solvent from the molded product, a decrease in strength due to the generation of voids as the organic solvent volatilizes, and coloring due to the oxidation of the organic solvent, etc. Furthermore, when an organopolysiloxane having a high viscosity is used to prepare a composition containing the same, the flowability during molding may be poor, leading to insufficient filling of the resin into a mold or the resin may harden in a state in which air is trapped within the resin. In some applications, the high viscosity of the organopolysiloxane may cause various adverse effects. When used in cosmetics such as hair wax and lip gloss, the viscosity of the organopolysiloxane is an important factor since it greatly affects the texture.
[0005] Therefore, an object of the present invention is to provide an organopolysiloxane composition that has a low viscosity and excellent dispersibility in various resins. [Means for solving the problem]
[0006] Therefore, the present inventors have found, as a result of intensive research, that the viscosity can be adjusted by adding a specific component to the organopolysiloxane, that this specific substance is not easily volatilized even when heated, so it does not cause odor generation, resin shrinkage, poor appearance of molded products, reduced transparency, insufficient curing, etc., and that since it has the same stability as organopolysiloxane, it does not cause pollution of the surrounding environment or coloring due to decomposition in a desired usage environment. In addition, it has been found that by kneading the raw materials in a temperature range where the specific substance vaporizes and uniformly dispersing the specific substance in the resin, it is possible to reduce the viscosity of the resin and also to promote the dispersibility of the organopolysiloxane.
[0013] Furthermore, the inventors have discovered that as benefits of a decrease in the viscosity of the organo polysiloxane, the amount of adhesion to kettles, filters, and withdrawal lines after production is reduced, improving the recovery rate, and the improved dispersibility in organic solvents reduces the effort required for cleaning, and when made into a composition, it is less likely to remain in the container, reducing the burden of cleaning the container after use. Furthermore, when the container is disposed of, since a specific substance in the organo polysiloxane composition that has adhered to the container has a similar structure to the other components, it is not necessary to secure a new storage space until disposal, in view of the danger of the specific component, and further, no detoxification or separation treatment is required for disposal, and since no chemicals or energy are used in the disposal, it is possible to contribute to a reduction in the environmental load.
[0007] That is, the gist of the present invention is as follows. [1] A composition comprising, as component A, an organopolysiloxane generally represented by the formula [1], and as component B, a substance represented by the following formula [2], and wherein component A and component B satisfy the relationship 0.1≦{(weight of component B)×100} / {(weight of component A)+(weight of component B)}≦9; and The content of the substance that satisfies T2 + 2 - M2 + E2 = 0 for the coefficients T2, M2, and E2 in the formula [2] with respect to Component A is 0.01% by weight or more and 9% by weight or less, and the content of the substance that does not satisfy T2 + 2 - M2 + E2 = 0 for the coefficients T2, M2, and E2 in the formula [2] is 3% by weight or less. An organopolysiloxane composition characterized by this. R X SiO (4-X) / 2 ···[1] (R 1 R 2 R 3 SiO 1 / 2 ) M2 (R 4 SiO 3 / 2 ) T2 (O 1 / 2 R 5 ) E2 ···[2] Here, in the above formula [1], R is each independently selected from the group consisting of an organic group and a hydrogen atom, and may be the same or different. The coefficient X each independently satisfies 0 < X ≤ 4. Here, in the above formula [2], R 1 ~R 3 are each independently selected from the group consisting of an organic group containing a carbon atom and a hydrogen atom, and may be the same or different. R 4 is selected from the group consisting of an organic group having 1 to 20 carbon atoms and a hydrogen atom, and may be the same or different. R 5 is selected from the group consisting of an organic group having 1 to 20 carbon atoms and a hydrogen atom, and may be the same or different; The coefficient M2 is a positive integer from 1 to 5, the coefficient T2 is a positive integer from 1 to 3, and the coefficient E2 is an integer from 0 to 5. [2] The organopolysiloxane composition according to [1], characterized in that the organopolysiloxane represented by the general formula [1] contains dimethylpolysiloxane or an MQ resin. [3] The organopolysiloxane according to [1] or [2], characterized in that the organopolysiloxane represented by the general formula [1] has a group selected from the group consisting of a trimethylsiloxy group, a dimethylvinyltrimethylsiloxy group, and a dimethylsiloxy group. Composition. [4] The organopolysiloxane composition according to any one of [1] to [3], wherein the organopolysiloxane represented by the general formula [1] has a phenyl group. [5] The organopolysiloxane composition according to any one of [1] to [4], characterized in that when 200 g of the organopolysiloxane composition is placed in a 1 L eggplant-shaped flask and heated for 2 hours at an internal temperature of 110°C under reduced pressure using a vacuum pump having an evacuation capacity of a vacuum pressure of 0.15 torr, the organopolysiloxane loses a mass of 10 g or less. [6] The organopolysiloxane composition according to any one of [1] to [5], wherein the organopolysiloxane represented by the general formula [1] is liquid at 40°C. [7] In the general formula [2], R 4 The organopolysiloxane composition according to any one of [1] to [6], wherein is a phenyl group. [8] In the general formula [2], R 1 ~R 3 The organopolysiloxane composition according to any one of [1] to [7], wherein is a methyl group. [9] The organopolysiloxane composition according to any one of [1] to [8], characterized in that the substance represented by the general formula [2] contains a substance having the coefficient T2 of 1.
[10] The organopolysiloxane composition according to any one of [1] to [9], characterized in that the substance represented by the general formula [2] contains a substance having the coefficient M2 of 3.
[11] The organopolysiloxane composition according to any one of [1] to
[10] , wherein the content of the substance represented by the general formula [2] in the organopolysiloxane composition is 0.5 to 3% by weight.
[12] A resin composition comprising the organopolysiloxane composition according to any one of [1] to
[11] .
[13] An organic solvent dilution solution comprising the organopolysiloxane composition according to any one of [1] to
[11] .
[14] A member for an electronic device, comprising the organopolysiloxane composition according to any one of [1] to
[11] or a cured product thereof. Effect of the Invention
[0008] The present invention can provide an organopolysiloxane composition that has a low viscosity and excellent dispersibility in various resins. The organopolysiloxane composition also has the effect of being excellent in odor resistance and colorability, and capable of maintaining a relatively high flash point. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The following describes in detail the embodiments of the present invention, but these descriptions are merely examples (representative examples) of the embodiments of the present invention, and the present invention is not limited to these contents as long as they do not depart from the gist of the present invention. In this specification, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the lower and upper limits, and "A to B" means A or more and B or less. In addition, in this specification, the term "independently" used when describing two or more objects together means that the two or more objects may be the same or different.
[0010] 1. Organopolysiloxane Composition The organopolysiloxane composition according to one embodiment of the present invention (hereinafter, also simply referred to as "organopolysiloxane composition") generally comprises, as component A, ModeThe present invention relates to an organopolysiloxane having the general formula [1] (hereinafter, simply referred to as "organopolysiloxane") and a substance having the general formula [2] as component B, wherein component A and component B satisfy the relationship 0.1≦{(weight of component B)×100} / {(weight of component A)+(weight of component B)}≦9, and The organopolysiloxane composition is characterized in that, relative to component A, the content of substances in which the coefficients T2, M2, and E2 in formula [2] satisfy T2+2-M2+E2=0 is 0.01 part by weight or more and 9 parts by weight or less, and the content of substances in which the coefficients T2, M2, and E2 in formula [2] do not satisfy T2+2-M2+E2=0 is 3 parts by weight or less. R X SiO (4-X) / 2 [1] (R 1 R 2 R 3 SiO 1 / 2 ) M2 (R 4 SiO 3 / 2 ) T2 (O 1 / 2 R 5 ) E2 [2] Here, in the above formula [1], Each R is independently selected from the group consisting of an organic group and a hydrogen atom, and may be the same or different. Each coefficient X is independently 0≦X≦3 Meet the following. Here, in the above formula [2], R 1 ~R 3 are each independently selected from the group consisting of an organic group containing carbon atoms and a hydrogen atom, and may be the same or different. R 4 are selected from the group consisting of organic groups having 1 to 20 carbon atoms and hydrogen atoms, and may be the same or different. R 5 are selected from the group consisting of organic groups having 1 to 20 carbon atoms and hydrogen atoms, and may be the same or different; coefficient M2 is a positive integer from 1 to 5, coefficient T2 is a positive integer from 1 to 3, and coefficient E2 is an integer from 0 to 5.
[0011] In this specification, the organopolysiloxane is a general term for all components that satisfy the above general formula [1], and in this case, the content of the organopolysiloxane is a value calculated based on the combined value of the multiple types of organopolysiloxane (combined). Similarly, in the present invention, the substance represented by the above general formula [2] is a general term for all components that satisfy the above general formula [], and in this case, the content of the substance is a value calculated based on the combined value of the multiple types of the substance (combined).
[0012] The substance represented by the above general formula [2] has a low viscosity due to its small molecular weight, and has good dispersibility in the organopolysiloxane composition represented by the general formula [1] and other resins. 4 The compatibility can be ensured by selecting the functional group type according to the organopolysiloxane composition and resin to which it is to be applied. In addition, the substance represented by the general formula [2] has Si-C bonds and Si-O-Si-C bonds that are unlikely to undergo dehydration condensation reactions with catalysts such as acids and bases used in synthesizing the organopolysiloxane, and water, and can maintain its structure even in the organopolysiloxane composition and resin, and maintains its structure even at high temperatures exceeding 200°C during molding, so it does not affect the quality of the molded product. In addition, when an organic solvent is used in the organopolysiloxane composition or resin, it volatilizes at high temperatures exceeding 200°C during molding, which can pose a risk due to the generation of flammable vapor or cause a defective appearance due to local dissolution of the molded product. However, the substance represented by the general formula [2] has excellent compatibility with the organopolysiloxane composition, so it does not volatilize even when temperatures and pressure conditions exceed the boiling point of the substance occur, and a molded product that is safe and does not have a defective appearance can be obtained.
[0013] <1.1. Organopolysiloxane represented by general formula [1]> The organopolysiloxane composition contains, as component A, an organopolysiloxane represented by the above general formula [1]. R X SiO (4-x) / 2 [1]
[0014] In the general formula [1], each coefficient X is independently greater than 0 and is bonded to silicon. It represents the content of each component of the organic group or the organic group bonded to oxygen bonded to silicon, and represents the content of each component of the silicon unit of M unit, D unit, T unit, and Q unit, and represents an organopolysiloxane composed of each component of the organopolysiloxane. R is an organic group. Regarding the wording "independently" in the coefficient X, since the organopolysiloxane represented by the general formula [1] can be an organopolysiloxane having multiple structures that satisfy the general formula [1], this wording indicates that the multiple structures may be the same or different.
[0015] In the present specification, an organic group refers to a functional group that includes carbon atoms, hydrogen atoms, oxygen atoms, nitrogen atoms, phosphorus atoms, sulfur atoms, and halogen atoms, and is composed of any combination of these atoms, and does not include groups that are composed of only one hydrogen atom. Also, an organic group that includes a carbon atom refers to a functional group that satisfies the above organic group aspects and includes at least one carbon atom.
[0016] R is independently selected from the group consisting of an organic group and a hydrogen atom, and the type thereof is not particularly limited and is selected in consideration of compatibility and reactivity from the viewpoint of mixing or reacting with a resin to be mixed or an additive used for any purpose. For example, a combination of functional groups including a vinyl group, an allyl group, a (meth)acrylic group, a carboxyl group, a nitrile group, a formyl group, a carbonyl group, a carbinol group, an amino group, an imino group, a nitro group, a cyano group, a sulfo group, a mercapto group, a thiol bond, an ether bond, an ester bond, an amide bond, an alkyl group having 1 to 20 carbon atoms, an aromatic functional group, and the like is preferable. Specifically, a hydrogen atom, a methyl group, an ethyl group, a propyl group, a hexyl group, a decyl group, an octadecyl group, a cyclopentyl group, a cyclohexyl group, an ethylene glycol monoethylene ether group, an acryloxypropyl group, an acryloxyoctyl group, a methacryloxypropyl group, a methacryloxyoctyl group, a glycidyl group, a glycidoxypropyl ... Preferably, the epoxy group is a hydrogen atom, a methyl group, an ethyl group, a cyclopentyl group, a cyclohexyl group, a 1,2-epoxycyclohexyl-3-propyl group, a 1,2-epoxycyclohexyl-3-octyl group, a phenyl group, a phenethylene group, a styryl group, a vinyl group, or an allyl group. When the polarity of the components to be mixed is low, the epoxy group is preferably a hydrogen atom, a methyl group, an ethyl group, a cyclopentyl group, a cyclohexyl group, a 1,2-epoxycyclohexyl-3-propyl group, a 1,2-epoxycyclohexyl-3-octyl ...phenyl group, a phenethylene group, a styryl group, a vinyl group, or an allyl group.
[0043] When the components to be mixed have high polarity, an ethylene glycol monoethylene ether group, an acryloxypropyl group, an acryloxyoctyl group, a methacryloxypropyl group, a methacryloxyoctyl group, a glycidyl group, a glycidoxypropyl group, a glycidoxyoctyl group, a phenyl group, a phenethylene group, a styryl group, or a vinyl group is even more preferable, and it is preferable to combine them in any ratio according to the resin or resin composition to be mixed.
[0017] Considering the case where the organopolysiloxane is mixed with other resins, suitable examples of R are shown below.
[0018] <When the resin to be mixed is mainly dimethylpolysiloxane> In this case, the resin corresponds to a resin having low polarity, and each R can be preferably independently a hydrogen atom, a methyl group, or a vinyl group.
[0019] <When the resin to be mixed is mainly composed of dimethyldiphenylpolysiloxane and methylphenylpolysiloxane> In this case, the resin corresponds to both a resin with low polarity and a resin with high polarity, and each R preferably independently has a phenyl group, and it is particularly preferable to use a combination of a methyl group and a phenyl group.
[0020] <When the resin to be mixed contains a (meth)acryloyl group> In this case, the resin corresponds to a resin having high polarity, and R is preferably a combination of an acryloxypropyl group, a methacryloxypropyl group, a methacryloxyoctyl group, a glycidoxypropyl group, a glycidoxyoctyl group, and a methyl group, each of which is independently selected.
[0021] <When the resin to be mixed is polycarbonate> In this case, the resin corresponds to a resin with high polarity, and R is preferably a combination of an ethylene glycol monoethylene ether group, a glycidoxypropyl group, a glycidoxyoctyl group, a phenyl group, a phenethylene group, a styryl group, a vinyl group, or a methyl group, and from the viewpoints of compatibility and heat resistance to heat exceeding 200°C when mixed with polycarbonate, it is preferable that R contains a methyl group or a phenyl group.
[0022] R is a terminal atom of R, and the atom bonded to the silicon atom may be oxygen, in which case, for example, an oxygen atom may be linked between the terminal atom bonded to silicon in the above-mentioned various functional groups exemplified by R. In this case, R may be a group selected from the group consisting of an organic group having 1 to 20 carbon atoms and a hydrogen atom, and from the viewpoint of compatibility with the resin, it is preferable that it is a hydrogen atom, a methyl group, an ethyl group, a butyl group, an octyl group, or an octadecyl group, and from the viewpoint of weight change or volume change due to dehydration condensation during heating or aging, a hydrogen atom or a methyl group is preferable, and a hydrogen atom is particularly preferable, and from the viewpoint of stability, a methyl group is preferable, and a combination of a methyl group and a hydrogen atom is also preferable.
[0023] In order to handle the organopolysiloxane represented by the general formula [1] as a reactive or non-reactive material with excellent stability, it is preferable that the organopolysiloxane has a group selected from the group consisting of a trimethylsiloxy group, a dimethylvinyltrimethylsiloxy group, and a dimethylsiloxy group.
[0024] The organopolysiloxane represented by the general formula [1] may be any of M units, D units, T units, and Q units, and the combination of each unit may be dimethylsiloxane consisting of M units and D units, MT resin consisting of M units and T units, MQ resin consisting of M units and Q units, and organosiloxane consisting of silicon units as shown below, but it is preferable that the organopolysiloxane represented by the general formula [1] contains dimethylsiloxane or MQ resin, particularly MDT units, MDQ units, MDTQ units, DT units, DQ units, DTQ units, and TQ units, from the viewpoint of ease of handling at room temperature. M units are R 1 'R 2 'R 3 'SiO 1 / 2 The D unit is a structural unit represented by R 4 'R 5 'SiO 2 / 2 The T unit is a structural unit represented by R 1 'SiO 1 / 2Q units are structural units represented by the formula: 4 / 2 The structural units are represented by the formula: 1 '~R 1 The conditions for R′ can be the same as those for R. Organopolysiloxanes that can have these structural units can be represented by the following general formula [A]. (R 1 'R 2 'R 3 'SiO 1 / 2 ) M1’ (R 4 'R 5 'SiO 2 / 2 ) D1’ (R 1 'SiO 1 / 2 ) T1’ (SiO 4 / 2 ) Q’ [A] Here, in the above general formula [A], the coefficients M1', D1', T1', and Q' are each equal to or greater than 0 and equal to or less than 1, and it is possible to satisfy M1'+D1'+T1'+Q'=1.
[0025] The number average molecular weight Mn of the organopolysiloxane composed of each component of the organopolysiloxane represented by the general formula [1] is, from the viewpoint of exhibiting the function of the organopolysiloxane in the resin to be mixed and ensuring compatibility with the resin, usually more than 100 and less than 200,000, but is usually 750 or more, preferably 1,000 or more, and more preferably 6,000 or more, and is usually 100,000 or less, and preferably 20,000 or less. It is preferable that the number of nuclei is 10,000 or less. The number average molecular weight Mn is measured by the method described below.
[0026] The molecular weight distribution (Mw / Mn) of the organopolysiloxane represented by general formula [1] is usually 1.01 or more and 10 or less. From the viewpoint of expressing the function of the organopolysiloxane in the resin to be mixed and ensuring compatibility with the resin, it is preferably 1.01 or more, more preferably 1.07 or more, even more preferably 1.2 or more, and particularly preferably 1.4 or more, and is preferably 5 or less, more preferably 4 or less, even more preferably 3 or less, and particularly preferably 2 or less. The weight average molecular weight Mw is measured by the method described below.
[0027] From the viewpoint of ensuring the effect of the organopolysiloxane on the resin to which it is added, the content of the organopolysiloxane represented by general formula [1] in the organopolysiloxane composition is usually 90% by weight or more, preferably 91% by weight or more, more preferably 93% by weight or more, and even more preferably 97% by weight or more, and is usually less than 100% by weight, preferably 99.5% by weight or less, more preferably 99.4% by weight or less, and even more preferably 98.7% by weight or less.
[0028] The form of the organopolysiloxane represented by general formula [1] is not particularly limited, but it is preferably a liquid, and in particular, from the viewpoint of miscibility with component [2], it is preferably a liquid at 40°C.
[0029] <1.2. Method for producing organopolysiloxane> The method for producing an organopolysiloxane according to another embodiment of the present invention (hereinafter also simply referred to as the "method for producing an organopolysiloxane") can be produced using a known method for producing an organopolysiloxane, and can be easily produced by a person skilled in the art.
[0030] <1.3. Substance represented by general formula [2]> The organopolysiloxane composition contains a substance represented by the following general formula [2] as a viscosity modifier. (R1 R 2 R 3 SiO 1 / 2 ) M2 (R 4 SiO 3 / 2 ) T2 (O 1 / 2 R 5 ) E2 [2] In the above formula [2], R 1 ~R 3 are each independently selected from the group consisting of an organic group containing carbon atoms and a hydrogen atom, and may be the same or different. R 4 are selected from the group consisting of organic groups having 1 to 20 carbon atoms and hydrogen atoms, and may be the same or different. R 5 are selected from the group consisting of organic groups having 1 to 20 carbon atoms and hydrogen atoms, and may be the same or different; coefficient M2 is a positive integer from 1 to 5, coefficient T2 is a positive integer from 1 to 3, and coefficient E2 is an integer from 0 to 5.
[0031] The coefficients T2 and M2 are both greater than or equal to 1, i.e., the T2 and M2 units are required. T2+2-M2+E2=0 means that no cyclic compounds are included in the siloxane bond. Cyclic compounds exist at T3 or higher, and even cyclic compounds have a viscosity reducing effect, and can be used in fields where the shelf life of the product is not an issue after mixing with a resin. In addition, the viscosity reducing effect of cyclic compounds may change due to ring opening, and from the viewpoint of product stability, it is desirable not to include them, but a small amount may be included. For organopolysiloxane (component A) represented by general formula [1] (when component A is 100% by weight), T2, M2, and E2 From the above viewpoints, the content of substances for which T2, M2, and E2 do not satisfy T2+2-M2+E2=0 is 0.01% by weight or more and 9% by weight or less, preferably 0.5% by weight or more, more preferably 0.6% by weight or more, even more preferably 1% by weight or more, and preferably 7% by weight or less, more preferably 5% by weight or less, and even more preferably 4% by weight or less. From the above viewpoints, the content of substances for which T2, M2, and E2 do not satisfy T2+2-M2+E2=0 in the organopolysiloxane (component A) represented by the general formula [1] is 3% by weight or less, more preferably 0.1% by weight or less, even more preferably 0.01% by weight or less, and most preferably not contained (0 ppm), but is usually 0% by weight or more, and may be 0.001% by weight or more.
[0032] R 1 ~R 4 are each independently selected from the group consisting of an organic group containing carbon atoms and a hydrogen atom; R 1 ~R 4 The atom bonded to the silicon atom is not particularly limited as long as it is not an oxygen atom, in order to avoid changing the classification of the M unit and the T unit. 1 ~R 4is selected in consideration of compatibility and reactivity from the viewpoint of mixing and reacting with the organopolysiloxane to be used as a composition, or with a resin to be mixed, or with an additive to be used for any purpose. For example, a combination of functional groups including a vinyl group, an allyl group, a (meth)acrylic group, a carboxyl group, a nitrile group, a formyl group, a carbonyl group, a carbinol group, an amino group, an imino group, a nitro group, a cyano group, a sulfo group, a mercapto group, a thiol bond, an ether bond, an ester bond, an amide bond, an alkyl group having 1 to 20 carbon atoms, an aromatic functional group, or the like is preferred. Specific examples of the functional groups include a hydrogen atom, a methyl group, an ethyl group, a propyl group, a hexyl group, a decyl group, an octadecyl group, a cyclopentyl group, a cyclohexyl group, an ethylene glycol monoethylene ether group, an acryloxypropyl group, an acryloxyoctyl group, a methacryloxypropyl group, a methacryloxyoctyl group, a glycidyl group, a glycidoxypropyl group, a glycidoxyoctyl group, a 1,2 In the case where the polarity of the components to be mixed is low, a hydrogen atom, a methyl group, an ethyl group, a cyclopentyl group, a cyclohexyl group, a 1,2-epoxycyclohexyl-3-propyl group, a 1,2-epoxycyclohexyl-3-octyl group, a 1,2-epoxycyclohexyl-3-octyl group, a phenyl group, a phenethylene group, a styryl group, a vinyl group, or an allyl group is more preferable. In the case where the polarity of the components to be mixed is high, an ethylene glycol monoethylene ether group, an acryloxypropyl group, an acryloxyoctyl group, a methacryloxypropyl group, a methacryloxyoctyl group, a glycidyl group, a glycidoxypropyl group, a glycidoxyoctyl group, a phenyl group, a phenethylene group, a styryl group, or a vinyl group is more preferable. It is preferable to combine them in any ratio according to the resin to be mixed.
[0033] R 5is a group selected from the group consisting of organic groups having 1 to 20 carbon atoms and a hydrogen atom. From the viewpoint of compatibility with the resin, a hydrogen atom, a methyl group, an ethyl group, a butyl group, an octyl group, or an octadecyl group is preferable. From the viewpoint of weight change or volume change due to dehydration condensation upon heating or changes over time, a hydrogen atom or a methyl group is preferable, and a hydrogen atom is particularly preferable. From the viewpoint of stability, a methyl group is preferable, and a combination of a methyl group and a hydrogen atom is also preferable.
[0034] Considering the case where organopolysiloxane is mixed with other resins, R 1 ~R 4 A suitable example is shown below.
[0035] <When the resin to be mixed is mainly dimethylpolysiloxane> In this case, the resin is a resin with low polarity, R 1 ~R 4 are each independently preferably a hydrogen atom, a methyl group, or a vinyl group. In particular, R 1 ~R 3 When one of the groups is a hydrogen atom or a vinyl group and the other two are methyl groups, R 1 ~R 3 are all methyl groups, and any combination thereof is more preferred. 4 is preferably a hydrogen atom, a methyl group, or a vinyl group, and is preferably accompanied by a reaction such as hydrosilylation. In this case, hydrogen atom and vinyl group are preferable. In this case, methyl group is preferable from the viewpoint of stability. 1 ~R 4 More preferably, all of are methyl groups.
[0036] <When the resin to be mixed is mainly composed of dimethyldiphenylpolysiloxane and methylphenylpolysiloxane> In this case, the resin corresponds to both the resin with low polarity and the resin with high polarity among the above-mentioned mixed components, and R 1 ~R 4 It is preferable to use a combination of a methyl group and a phenyl group for R.1 ~R 3 One of them is a hydrogen atom or a vinyl group, the other two are methyl groups, R 1 ~R 3 is preferably a methyl group, or a combination thereof, and R 4 R is more preferably a phenyl group. 1 ~R 3 are all methyl groups, and R 4 It is most preferred that is a phenyl group.
[0037] <When the resin to be mixed contains a (meth)acryloyl group> In this case, the resin is one with a high polarity among the above-mentioned mixed components, R 1 ~R 4 is preferably used in combination with an acryloxypropyl group, a methacryloxypropyl group, a methacryloxyoctyl group, a glycidoxypropyl group, a glycidoxyoctyl group, or a methyl group. In particular, R 1 ~R 3 One of them is a hydrogen atom or a vinyl group, the other two are methyl groups, R 1 ~R 3 is preferably a methyl group, or a combination thereof, and R 4 More preferred are an acryloxypropyl group, a methacryloxypropyl group, a methacryloxyoctyl group, a glycidoxypropyl group, a glycidoxyoctyl group, a phenyl group, and combinations thereof. From the viewpoint of increasing hardness such as pencil hardness and Shore hardness, an acryloxypropyl group, a methacryloxypropyl group, and a glycidoxypropyl group are preferred, and from the viewpoint of flexibility and brittleness, a methacryloxyoctyl group and a glycidoxyoctyl group are preferred.
[0038] <When the resin to be mixed is polycarbonate> In this case, the resin is one with a high polarity among the above-mentioned mixed components, R 1 ~R 4is preferably used in combination with an ethylene glycol monoethylene ether group, a glycidoxypropyl group, a glycidoxyoctyl group, a phenyl group, a phenethylene group, a styryl group, a vinyl group, or a methyl group. In particular, R 1 ~R 3 One of them is a hydrogen atom, a vinyl group, an ethylene glycol monoethylene ether group, or a glycidoxypropyl group, and the other two are a methyl group, R 1 ~R 3 is preferably a methyl group, or a combination thereof, and R 3 Phenyl groups are more preferable, and in terms of compatibility and heat resistance to temperatures exceeding 200°C when mixed with polycarbonate, R 1 ~R 3 are all methyl groups, R 4 It is preferred that is a phenyl group.
[0039] The substance represented by the general formula [2] may be used alone or in combination with two or more substances, particularly those having different values of the coefficients M2 and T2. 1 ~R 4 A plurality of compounds having different functional groups may be used.
[0040] M2 is 1 or more and 5 or less. In the modification of the bonds of the T units, the alkoxy group and silanol group represented by E2 are likely to change by dehydration condensation, but the M units are less likely to undergo silanolization and dehydration condensation associated with elimination. Therefore, from the viewpoint of stability, it is preferable that M2 is larger. Since the maximum value of T2 is 3, when T2 is 3, M2 is preferably 5, when T2 is 2, M2 is preferably 4, and when T2 is 1, M2 is preferably 3, that is, it is preferable that M2=T2+2. In addition, in the modification of the bonds of the T units, the M units are unlikely to undergo silanol formation and dehydration condensation due to elimination, but the alkoxy group and silanol group represented by E2 are easily reacted by dehydration condensation. Therefore, from the viewpoint of reactivity, it is preferable that M2 is small. Since the maximum value of T2 is 3, when T2 is 3, M2 is preferably 4 or less, more preferably 2 or less, and even more preferably 1. When it is 0, hydrolysis condensation is very unlikely. When T2 is 1, M2 is preferably 3 or less, more preferably 2 or less, and even more preferably 1. When T2 is 0, the viscosity is very susceptible to change and the viscosity change over time is large, and from the viewpoint of storage stability, M2 is 1 or more. When T2 is 1, M2 is preferably 3 or less, more preferably 2 or less, and even more preferably 1. When T2 is 0, the viscosity is very susceptible to change and the viscosity change over time is large, and from the viewpoint of storage stability, M2 is 1 or more.
[0041] T2 is 1 or more and 3 or less, but from the viewpoint of an increase in the number of T units increasing the molecular weight and decreasing the viscosity-lowering effect due to an increase in viscosity, or from the viewpoint of a decrease in dispersibility in the organopolysiloxane to be mixed due to an increase in molecular size, it is preferable that T2 is small, preferably 3 or less, preferably 2 or less, and more preferably 1. Furthermore, since an increase in the number of T units decreases volatility, low volatility is preferable when process temperatures such as molding temperature and curing temperature are high, and from the viewpoint of volatility, it is preferable that T2 is large, preferably 1 or more, more preferably 2 or more, and even more preferably 3 or more.
[0042] The content of the substance represented by general formula [2] in the organopolysiloxane composition is 0.01% by weight or more and 9% by weight or less; from the viewpoint of the viscosity-reducing effect, it is usually 0.1% by weight or more, preferably 0.5% by weight or more, more preferably 1% by weight or more, and even more preferably 2% by weight or more; and from the viewpoint of volatilization during molding or curing or volatilization over time, it is usually 9% by weight or less, preferably 7% by weight or less, more preferably 5% by weight or less, and even more preferably 3% by weight or less. Furthermore, in the organopolysiloxane composition, the ratio of the weight of component B to the sum of the weight of component A (organopolysiloxane represented by the above general formula [1]) and the weight of component B (substance represented by the above general formula [2]) per 100 ({(weight of component B) × 100} / {(weight of component A) + (weight of component B)}) is, from the viewpoint of reducing the viscosity of the organopolysiloxane and the volatility of component B, 0.1 or more and 9 or less, but is usually 0.5 or more, preferably 0.6 or more, and more preferably 1.3 or more, and is usually 7 or less, preferably 5 or less, and more preferably 3 or less. In addition, a component that can be considered as both component A and component B will be considered as component B in this specification.
[0043] By improving the compatibility between the substance represented by general formula [2] and the organopolysiloxane represented by general formula [1] above, the substance represented by general formula [2] is dispersed evenly and the viscosity of the organopolysiloxane composition containing said substance is reduced. On the other hand, if compatibility is poor, the substance represented by general formula [2] will accumulate or emulsify locally, so that the effect of reducing the viscosity of the organopolysiloxane composition containing said substance is not very noticeable and, furthermore, when emulsified, the viscosity may increase.
[0044] <1.4. Method for producing the substance represented by general formula [2]> The method of producing the substance represented by the general formula [2] is not particularly limited, and it can be produced by a known method, or a commercially available product such as tris(trimethylsiloxy)phenylsilane (PTTSS) can be used. The substance represented by the general formula [2] is a substance that can be contained at the manufacturing stage not only when it is intentionally added, but also when it is produced using a material containing M units and T units as a raw material, and it is possible that it may be contained even without being intentionally added during the production of organopolysiloxane. However, the substance represented by the general formula [2] is hated by the relevant industry as a substance that causes electrode contact problems (commonly known as low volatile problems) when producing a specific organopolysiloxane other than the organopolysiloxane of the general formula [1], and has been removed to less than 0.1% by weight by distillation such as thin film distillation. In addition, When producing an organopolysiloxane of general formula [1], the substance of general formula [2] can be produced, making it possible to include the substance without intentionally adding it. In such a case, it is possible to adjust the viscosity by adjusting the content of the substance of general formula [2] according to the purpose. It is also possible to achieve the purpose by analyzing the organopolysiloxane composition by gas chromatography to quantify the content of the substance of general formula [2], and controlling the content of the substance by distillation such as thin-film distillation.
[0045] <1.5. Other ingredients> The organopolysiloxane composition may contain components other than the organopolysiloxane represented by the above-mentioned general formula [1] and the substance represented by the general formula [2]. Examples of the other components include a curing catalyst, a chain polymerization initiator, an antioxidant, a filler, a curing agent, and a curing regulator. There are no particular limitations on the amount of other components contained in the organopolysiloxane composition, and they may be added as desired depending on the purpose, as long as the effects of the present invention are achieved.
[0046] (curing catalyst) The type of the curing catalyst is not particularly limited, and examples thereof include addition polymerization catalysts and condensation polymerization catalysts. Examples of the addition polymerization catalyst include platinum-based catalysts such as platinum black, platinic chloride, chloroplatinic acid, reaction products of chloroplatinic acid and monohydric alcohols, complexes of chloroplatinic acid and olefins, platinum bisacetoacetate, platinum (0) complexes with 1,3-divinyl-1,1,3,3-tetramethyldisiloxane, platinum (0) complexes with 1,3,5,7-tetravinyl-1,3,5,7-tetramethylcyclosiloxane, palladium catalysts, and rhodium catalysts. The amount of the addition polymerization catalyst is usually 1 ppm or more, preferably 2 ppm or more, and usually 100 ppm or less, preferably 50 ppm or less, and more preferably 20 ppm or less, based on the total weight of the organopolysiloxane. This allows the catalyst to have high catalytic activity and high transparency of the cured product. The addition polymerization catalyst may be used alone or in combination of two or more.
[0047] As the condensation polymerization catalyst, acids such as hydrochloric acid, nitric acid, sulfuric acid, organic acids, bases such as ammonia, amines, metal chelate compounds, etc. can be used, and a metal chelate compound containing one or more of Ti, Ta, Zr, Al, Hf, Zn, Sn, Pt, and In can be preferably used. Among them, the metal chelate compound is preferably one or more of Ti, Al, Zn, Zr, Pt, and In, and more preferably one containing Zr or Pt is used.
[0048] The amount of the condensation polymerization catalyst is usually 1 ppm or more, preferably 2 ppm or more, and usually 300 ppm or less, preferably 200 ppm or less, more preferably 150 ppm or less, based on the total weight of the organopolysiloxane as metal. This makes it possible to achieve high catalytic activity and small weight loss when the cured product is heated. The condensation polymerization catalyst may be used alone or in combination of two or more.
[0049] (Chain polymerization initiator) Examples of the chain polymerization initiator include a radical polymerization initiator, a cationic polymerization initiator, and an anionic polymerization initiator. Generally, a radical polymerization initiator is used.
[0050] As the radical polymerization initiator, a photopolymerization initiator and a thermal polymerization initiator can be used. As the photopolymerization initiator, an alkylphenone-based photopolymerization initiator, an acylphosphine oxide-based photopolymerization initiator, an intramolecular hydrogen abstraction type photopolymerization initiator, an oxime ester photopolymerization initiator, etc. can be used. As a preferable example, an alkylphenone-based photopolymerization initiator is used. It is possible.
[0051] As the thermal polymerization initiator, a conventionally known peroxide or azo compound can be used. Examples of organic peroxides include diacyl peroxides, peroxydicarbonates, peroxyesters, peroxyketals, dialkyl peroxides, hydroperoxides, and silyl peroxides. More specifically, cumyl peroxyneodecanoate, 1,1,3,3-tetramethylbutyl peroxyneodecanoate, 1-cyclohexyl-1-methylethyl peroxyneodecanoate, t-hexyl peroxyneodecanoate, and t-butyl peroxyneodecanoate. peroxypivalate, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane, t-hexylperoxy-2-ethylhexanoate, t-butylperoxy-2-ethylhexanoate, t-butylperoxyneoheptanoate, t-amylperoxy-2-ethylhexanoate, di-t-butylperoxyhexahydroterephthalate, t-amylperoxy -3,5,5-trimethylhexanoate, 3-hydroxy-1,1-dimethylbutylperoxyneodecanoate, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, t-amylperoxyneodecanoate, t-amylperoxy-2-ethylhexanoate, t-hexylperoxyisopropyl monocarbonate, t-butylperoxymaleic acid, t-butylperoxy-3,5,5-trimethylhexanoate, t-butylperoxylaurate, 2,5- Examples of the peroxyalkylene oxide include dimethyl-2,5-di(3-methylbenzoylperoxy)hexane, t-butylperoxy-2-ethylhexyl monocarbonate, t-hexyl peroxybenzoate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, t-butyl peroxybenzoate, dibutyl peroxytrimethyladipate, t-amyl peroxy normal octoate, t-amyl peroxy isononanoate, t-amyl peroxybenzoate, and lauroyl peroxide.
[0052] Examples of azo compounds include 2,2'-azobis-2,4-dimethylvaleronitrile, 1,1'-azobis(1-acetoxy-1-phenylethane), 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), dimethyl-2,2'-azobisisobutyronitrile, 4,4'-azobis(4-cyanovaleric acid), and 1,1'-azobis(1-cyclohexanecarbonitrile).
[0053] The radical polymerization initiator may be used alone or in combination of two or more kinds.
[0054] (Antioxidants) The curable composition preferably further contains an antioxidant, which can suppress discoloration of the cured product due to heat, such as solder reflow. Specific examples of antioxidants include 2,6-di-t-butylphenol, 2,6-di-t-butyl-p-cresol, n-octadecyl-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate, tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane, triethylene glycol bis[3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate], 1,6-hexanediol bis[ phenol-based antioxidants such as 3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate; phosphorus-based antioxidants such as triphenyl phosphite, trisisodecyl phosphite, tristridecyl phosphite, tris(2,4-di-t-butylphenyl)phosphite, and tetra(C12-15 alkyl)-4,4'-isopropylidenediphenyl diphosphite; dilauryl-3,3'-thiodipropionate, ditridecyl-3,3'-thiodipropionate, dimyris Examples of the antioxidant include sulfur-based antioxidants such as distearate-3,3'-thiodipropionate, distearate-3,3'-thiodipropionate, and pentaerythritol tetrakis(β-laurylthiopropionate). These antioxidants may be used alone or in combination of two or more.
[0055] <2. Method for producing organopolysiloxane composition> The method for producing the organopolysiloxane composition is not particularly limited, and the composition can be produced by mixing the organopolysiloxane represented by the above-mentioned general formula [1], the substance represented by general formula [2], and other optional components. In addition, when the substance represented by general formula [2] is produced in the organopolysiloxane production stage, it is not necessary to add the substance from the outside, and since the substance is contained in the composition obtained in the final stage of organopolysiloxane production, this can be used as the organopolysiloxane composition.
[0056] <3. Characteristics of the organopolysiloxane composition> The properties of the organopolysiloxane composition will now be described.
[0057] (1) 1 H-NMR 1 The amount of functional groups in an organopolysiloxane can be measured by using H-NMR. The measurement method is as follows. Approximately 50 mg of organopolysiloxane or a composition containing the same is weighed out and dissolved in approximately 1 g of deuterated acetone or deuterated dichloromethane; 1 A sample for H-NMR measurement is prepared. Using this sample for measurement, 1 The relaxation delay is measured at 20 seconds using H-NMR (e.g., AL-400 manufactured by JEOL Ltd.), and the ratio of the signal intensity of each component to the signal intensity of the internal standard and the proportion of functional groups (e.g., phenyl groups, methyl groups, and organoxy groups) are calculated from the weighed values. In the above measurements, impurities such as organic matter, water, and metals that are not bonded to organopolysiloxane must be removed to less than 0.1% by weight so as not to affect the measurement results. If the impurity content exceeds 0.1% by weight, it must be removed by distillation, filtration, or other purification methods before preparing the sample. 1 Measure H-NMR. If removal is difficult, 1 The content of impurities is calculated by H-NMR measurement or other analytical methods, and the weight of the impurities is subtracted from the weighed sample weight to avoid calculating it as part of the organopolysiloxane, and this value is used in the calculation as the true sample amount. Note that, in addition to toluene, any substance that does not react with organopolysiloxane, such as N,N-dimethylformamide or tetrabromoethane, can be used as the internal standard.
[0058] (2) 29 Si-NMR 29 By using Si-NMR, the values of M, D, T, and Q in the organopolysiloxane represented by the above general formula [1] can be calculated. The calculation method is as follows. Tris(2,4-pentanedionate)chromiumIII was added to deuterated chloroform to make the concentration 0.5% by mass. 29 A solvent for Si-NMR measurement is obtained. Next, about 1.5 g of the organopolysiloxane to be measured or a composition containing the same is weighed out, and the above 29 2.5 mL of a solvent for Si-NMR measurement was added to dissolve the sample, and the sample was placed in a 10 mmΦ Teflon (registered trademark) NMR sample tube. 29 Measurement is performed using Si-NMR (e.g., JNM-ECS400, TUNABLE(10), Si-free, AT10 probe manufactured by JEOL Ltd.) under the following measurement conditions, and the values of M, D, T, and Q in the organopolysiloxane represented by the above general formula [1] are calculated from the signal intensity ratio. Measurement conditions: Relaxation Delay / 15 seconds, Scan count / 1024 times, Measurement mode / Non-gated decoupled pulse method (NNE), Spin / None, Measurement temperature / 25℃
[0059] (3) Gel permeation chromatography (GPC) The number average molecular weight (Mn) and weight average molecular weight (Mw) of the organopolysiloxane can be calculated by gel permeation chromatography (GPC) according to the following method. Organopolysiloxane or a composition containing it is measured under the following conditions using GPC (for example, the apparatus is TOSOH HLC-8420GPC manufactured by Tosoh Corporation, and the columns are KF-G, KF-402.5HQ, KF-402HQ, and KF-401HQ manufactured by Showa Denko K.K.), and the values are calculated in terms of standard polystyrene. The sample used is a tetrahydrofuran solution of about 10% by weight, which is filtered through a 0.45 μm filter before measurement. Column temperature: 40℃ Eluent: tetrahydrofuran, flow rate 0.3 mL / min
[0060] (4) Gas chromatography (GC) The amount of organic solvent remaining in an organopolysiloxane or a composition containing the same, and the content of the substance represented by general formula [2] can be measured by gas chromatography (GC). The measurement method is as follows. Organopolysiloxane or a composition containing it is measured under the following conditions using GC (for example, the apparatus is a 7820A gas chromatograph manufactured by Agilent Technologies, Inc., and the column is a DB-17ht, 0.25 mm x 30 m x 0.15 μm, manufactured by Agilent Technologies, Inc.). The sample is a tetrahydrofuran solution of about 50% by mass, and the internal standard substance is selected according to the purpose, such as methylcyclopentane, toluene, or tridecane. <Setting conditions> ·Inlet: 290℃ Pressure: 21.76 psi (constant pressure) Oven program: 65℃(2minHold)→20℃ / min→325℃(40minHold) (Total 55min) Split ratio: 1 / 70 ·Injection volume: 0.5μL Detector: 290℃ <Carrier gas> Air flow rate: 350mL / min H 2 Flow rate: 35ml / mi He flow rate:
[0061] (5) Solvent turbidity test The method for evaluating the mixing and dispersibility of the organopolysiloxane or the composition containing it with the resin is as follows. As the organic solvent, 11 g of tetraglyme with added water so that the water content was 10.5% by weight was prepared. This organic solvent and 1 g of organopolysiloxane were mixed and stirred at 25°C. If the organic solvent became transparent, it was judged that it had good mixing and dispersibility in the resin, and if the organic solvent became cloudy, it was judged that it had poor mixing and dispersibility in the resin. The purity of the tetraglyme used is confirmed to be 99.8% or more by gas chromatography, and the water content is confirmed by a Karl Fischer water content analyzer.
[0062] (6) Low boiling point component confirmation test The amount of organopolysiloxane in the organopolysiloxane composition is constant; In other words, it is preferable that the organopolysiloxane composition is stable. In the case where the stability of the organopolysiloxane is evaluated by placing 200 g of the organopolysiloxane composition in a 1 L eggplant flask, heating the flask at an internal temperature of 110° C. for 2 hours under reduced pressure using a vacuum pump having an exhaust capacity of a vacuum pressure of 0.15 torr, and evaluating the mass loss of the organopolysiloxane, the mass loss is preferably 10 g or less, more preferably 5 g or less, and even more preferably 2 g or less, and it is particularly preferable that no loss is observed (below the detection limit). By making the weight loss amount under the above conditions equal to or less than the upper limit, the amount of volatilization of the substance represented by the general formula [2] during heat kneading with the resin is small, so that the resin and the desired organopolysiloxane composition can be uniformly dispersed, and the fluctuation in the content of the substance represented by the general formula [2] for each product lot can be suppressed. In addition, the flash point of the components contained in the organopolysiloxane can be kept relatively high, and the risk of a low flash point, which is difficult to handle safely under normal conditions, can be avoided. In addition, since the Fire Service Act hazard classification is classified as a lower or higher hazard, the cost of storage and transportation can be reduced. In addition, since the weight loss amount of the cured product during curing is also small, the temperature dependency of the storage elastic modulus of the cured product is small, the usable temperature range is wide, and embrittlement due to thinning is unlikely to occur. In addition, since the smaller the weight loss amount, the easier it is to obtain the above advantages, there is no preferable lower limit for the weight loss amount, but it is usually 0.0001g or more.
[0063] The weight loss upon heating under reduced pressure can be measured as follows. Organopolysiloxane composition as the measurement subject 1H-NMR is measured, and the weight of components other than the organopolysiloxane and the substance represented by general formula [2], such as the organic solvent, is calculated. Specifically, a rotor is placed in the eggplant flask, and their weights are measured. Then, the organopolysiloxane composition is placed in the eggplant flask, and the weight of the organopolysiloxane composition is measured. The eggplant flask is heated in an oil bath, the rotor is rotated with a magnetic stirrer to stir the liquid surface to the extent that it moves, and the pressure is reduced with an oil-type vacuum pump. After 2 hours, the flask is cooled to room temperature, the pressure is returned to normal, the oil adhering to the eggplant flask is thoroughly wiped off, and the weight of the organopolysiloxane composition in the eggplant flask is measured, and the weight of the eggplant flask and the rotor that were previously measured are subtracted to calculate the weight that has evaporated as a result of this operation. The weight of the organopolysiloxane composition after this operation is 1 1H-NMR was measured, and the weight of the organic solvent and other components other than the organopolysiloxane was calculated. 1 From the results of H-NMR and gas chromatography, the amount of components other than organopolysiloxane and the amount of volatilized organopolysiloxane are calculated from the weight of the volatilized matter. In addition, the volatilized distillate is entirely recovered using a cold trap or the like, and the weight and 1 H-NMR and gas chromatography may also be measured.
[0064] (7) Coloring when heated to 250℃ The coloring property was evaluated by adding 10 mg of a composition containing an organopolysiloxane to a hot plate heated to 250° C., and visually checking the coloring property after 10 minutes.
[0065] (8) Viscosity The viscosity is measured at a temperature of 25° C. using a viscometer (for example, RV-type viscometer RVDV-2+Pro manufactured by Brookfield) with the organopolysiloxane composition as the measurement object.
[0066] <4.Applications> The applications of the above-mentioned organopolysiloxane composition and the above-mentioned organopolysiloxane represented by the general formula [1] are not particularly limited, and they can be used, for example, in the applications shown below.
[0067] [Resin composition] The organopolysiloxane composition can be used as a resin composition in combination with other resins. The resin composition may contain the above-mentioned organopolysiloxane composition, and may be, for example, an embodiment in which the organopolysiloxane composition is added to a composition containing a resin, or an embodiment in which a resin is added to an organopolysiloxane composition. The manner of use of the resin composition is not particularly limited, and the resin composition may be used in the form of a composition itself, or may be used in the form of a cured product obtained by curing the composition.
[0068] The type of resin contained in the resin composition containing the organopolysiloxane composition is not particularly limited, and examples thereof include organopolysiloxane compositions, acrylic resins, polyolefin resins, polyvinyl chloride resins, polyester resins, polypropylene resins, polyethylene resins, polycarbonate resins, polybutylene terephthalate resins, polyethylene terephthalate resins, polyamide resins, PEEK resins, polyacetal resins, polyvinyl alcohol resins, and epoxy resins. In LED lighting applications requiring colorless transparency, heat resistance, light resistance, and low volatile components over time, the resin composition may be selected from the group consisting of organopolysiloxane compositions, acrylic resins, polyolefin resins, polyvinyl chloride resins, polyester resins, polypropylene resins, polyethylene resins, polycarbonate resins, polybutylene terephthalate resins, polyethylene terephthalate resins, polyamide resins, PEEK resins, polyacetal resins, polyvinyl alcohol resins, and epoxy resins. can be incorporated without impairing performance, and therefore is suitable for use in organopolysiloxane compositions and epoxy resins; for camera lens applications requiring colorless transparency, high Abbe and high refractive index, high glass transition temperature, heat resistance, and light resistance, it is suitable for use in acrylic resins, since it can be incorporated without impairing performance; for polycarbonate resins requiring colorless transparency, heat resistance during kneading, and flame retardancy due to the promotion of char formation, it is suitable for use in epoxy resins for 3D applications requiring colorless transparency, low viscosity, and short-term effectiveness.
[0069] The content of the organopolysiloxane composition in the resin composition is not particularly limited, but from the viewpoint of not changing the basic physical properties of the resin and imparting a certain function, it is preferable to add a very small amount, usually 0.01% by weight or more, preferably 0.1% by weight or more, more preferably 0.5% by weight or more, and usually 5% by weight or less, preferably 3% by weight or less, and more preferably 1% by weight or less. On the other hand, from the viewpoint of slightly changing the basic physical properties of the resin, it is preferable to add a small amount, usually 5% by weight or more, preferably 7% by weight or more, more preferably 10% by weight or more, and usually 20% by weight or less, preferably 17% by weight or less, and more preferably 15% by weight or less, and from the viewpoint of significantly changing the basic physical properties of the resin, it is 20% by weight or more, preferably 25% by weight or more, more preferably 30% by weight or more, and even more preferably 50% by weight or more, and usually 99% by weight or less, preferably 75% by weight or less, and more preferably 60% by weight or less.
[0070] [Organic solvent diluent] The organopolysiloxane composition can be used as an organic solvent dilution liquid in combination with an organic solvent. The organic solvent dilution liquid may contain the above-mentioned organopolysiloxane composition, and may be, for example, an embodiment in which the organopolysiloxane composition is added to a composition containing an organic solvent, or an embodiment in which an organic solvent is added to the organopolysiloxane composition. The type of organic solvent contained in the organic solvent dilution solution containing the organopolysiloxane composition is not particularly limited and may be selected arbitrarily. For example, a work-in-progress in which the organic solvent remains or one in which the organic solvent has been intentionally dissolved may be transferred to a container, sold, transported, or introduced into a reactor containing other substances.
[0071] [Electronic device components] The organopolysiloxane composition and its cured product, and the resin containing the organopolysiloxane composition and its cured product can be used as contained in electronic device members. Examples of electronic device members include LED lighting sealants and organopolysiloxanes. Examples of such applications include use in LED-related parts, covers for LED lighting, lens and camera parts, cover parts for smartphones, voltage resistance improvers for electrolytic capacitors, parts that express a clicking sensation under the keys of a personal computer keyboard, sealing materials for power device modules, etc. The electronic device parts may be in an embodiment consisting of only the cured product of the organopolysiloxane composition, or may be in an embodiment that partially contains the cured product of the organopolysiloxane composition. The conditions for curing the organopolysiloxane composition are not particularly limited, and the composition can be cured by a known method.
[0072] The content of the organopolysiloxane composition in electronic device components is not particularly limited, but from the viewpoint of imparting certain functions without changing the basic physical properties of the resin used in the components, it is preferable to add a very small amount, which is usually 0.01 wt % or more, preferably 0.1 wt % or more, and more preferably 0.5 wt % or more, and is usually 5 wt % or less, preferably 3 wt % or less, and more preferably 1 wt % or less, and examples of this include cover components for LED lighting and cover components for smartphones. On the other hand, from the viewpoint of slightly changing the basic physical properties of the resin used in the components, it is preferable to add a small amount, and it is usually 5 wt % or more, preferably 7 wt % or more, and more preferably 10 wt % or more, and it is usually 20 wt % or less, preferably 17 wt % or less, and more preferably 15 wt % or less, which corresponds to sealing materials for LED lighting and sealing materials for power device modules, and from the viewpoint of significantly changing the basic physical properties of the resin used in the components, it is 20 wt % or more, preferably 25 wt % or more, more preferably 30 wt % or more, and even more preferably 50 wt % or more, and it is usually 99 wt % or less, preferably 75 wt % or less, and more preferably 60 wt % or less, which corresponds to lenses and camera components.
[0073] <Other uses> In addition to the uses described above, the organopolysiloxane composition can be used for other uses, such as a non-reactive viscosity modifier, a reactive viscosity modifier, a compatibilizer, a lubricant, a dispersant, a flocculating agent, an adhesive, a pressure-sensitive adhesive, a release agent, a water repellent, an oil repellent, a coating agent, a surface modifier, a metal surface repair agent, a flame retardant, an agent for reducing squeak noise, a sealing material or substrate for semiconductor devices including inorganic or organic light-emitting elements, a coating material, and an optical component. EXAMPLES
[0074] The present invention will be described in more detail below with reference to examples, but the present invention should not be construed as being limited to the following examples. In the following description, "parts" refers to "parts by weight" based on weight unless otherwise specified.
[0075] <Method of Evaluating Organopolysiloxane Composition> The organopolysiloxane and / or organopolysiloxane composition were evaluated by the following methods.
[0076] (1) 1 H-NMR Approximately 50 mg of the resulting organopolysiloxane was weighed out and dissolved in approximately 1 g of deuterated acetone or deuterated dichloromethane. 1 A sample was prepared for H-NMR measurement. 1 The relaxation delay was measured at 20 seconds using H-NMR (AL-400, manufactured by JEOL Ltd.). The proportions of phenyl groups, methyl groups, and organoxy groups were calculated from the ratios of the signal intensity of each component to the signal intensity of the internal standard and the weighed values.
[0077] (2) 29 Si-NMR Tris (2,4-pentanedionate) chromium III was added to deuterated chloroform to make it 0.5% by mass. 29A solvent for Si-NMR measurement was obtained. Approximately 1.5 g of the organopolysiloxane to be measured was weighed out and mixed with the above solvent. 29 2.5 mL of the Si-NMR measurement solvent was added to dissolve the sample, and the solution was placed in a 10 mm diameter Teflon (registered trademark) NMR sample tube. Measurements were performed using the following equipment and conditions, and the values of M, D, T, and Q in the organopolysiloxane represented by the general formula [1] above were calculated from the signal intensity ratio. Equipment: JNM-ECS400 manufactured by JEOL Ltd., TUNABLE(10), Si-free, AT10 probe Measurement conditions: Relaxation Delay / 15 seconds, Scan count / 1024 times, Measurement mode / Non-gated decoupled pulse method (NNE), Spin / None, Measurement temperature / 25℃
[0078] (3) Gel permeation chromatography (GPC) The number average molecular weight (Mn), weight average molecular weight (Mw), and molecular weight distribution (Mw / Mn) of organopolysiloxanes were measured using gel permeation chromatography (GPC) under the following conditions, and are shown as values converted into standard polystyrene. The sample used was a 10% by weight tetrahydrofuran solution, which was filtered through a 0.45 μm filter before measurement. Equipment: TOSOH HLC-8420GPC (manufactured by Tosoh Corporation) Column: KF-G, KF-402.5HQ, KF-402HQ, KF-401HQ (all manufactured by Showa Denko K.K.), column temperature 40°C Eluent: tetrahydrofuran, flow rate 0.3 mL / min
[0079] (4) Gas chromatography (GC) To confirm the amount of organic solvent remaining in the organopolysiloxane and the content of the substance represented by the general formula [2], measurements were performed using gas chromatography (GC) under the following conditions: A tetrahydrofuran solution of approximately 50% by mass was used as the sample, and methylcyclopentane was used as the internal standard substance. Equipment: Agilent Technologies 7820A gas chromatograph Column: Agilent Technologies DB-17ht, 0.25 mm x 30 m x 0.15 μm Setting temperature etc. ·Inlet: 290℃ Pressure: 21.76 psi (constant pressure) Oven program: 65℃(2minHold)→20℃ / min→325℃(40minHold) (Total 55min) Split ratio: 1 / 70 ·Injection volume: 0.5μL Detector: 290℃ <Carrier gas> Air flow rate 350ml / min H 2 Flow rate: 35mL / min He flow rate: 20mL / min
[0080] (5) Solvent turbidity test In order to evaluate the mixing and dispersibility of organopolysiloxane with resin, a mixing test with organic solvent was carried out. As an organic solvent, 11 g of tetraglyme with water added so that the water content was 10.5 wt % was prepared, and the organic solvent and 1 g of organopolysiloxane were mixed and stirred at 25°C, and the transparent one was judged to have good mixing and dispersibility in resin, and the cloudy one was judged to have bad mixing and dispersibility in resin.
[0081] (6) Low boiling point component confirmation test 200 g of the organopolysiloxane composition was placed in a 1 L eggplant-shaped flask and heated for 2 hours at an internal temperature of 110°C under reduced pressure using a vacuum pump with an exhaust capacity of 0.15 torr, and the mass loss rate was confirmed using a balance. A mass loss rate of 5% by weight or less was determined to have no effect on moldability, and a weight loss rate of more than 5% by weight was determined to have an effect on moldability. The weight loss during heating under reduced pressure was measured by the following method. Organopolysiloxane composition as the measurement subject 1H-NMR was measured, and the weight of components other than organopolysiloxane, such as organic solvent, was calculated. Specifically, a rotor was placed in an eggplant-shaped flask, and their weights were measured. Then, the organopolysiloxane composition was placed in the eggplant-shaped flask, and the weight of the organopolysiloxane composition was measured. The eggplant-shaped flask was heated in an oil bath, the rotor was rotated with a magnetic stirrer to stir the liquid surface to a degree that it was moving, and the pressure was reduced with an oil-type vacuum pump. After 2 hours, the flask was cooled to room temperature, the pressure was returned to normal pressure, the oil adhering to the eggplant-shaped flask was thoroughly wiped off, and the weight of the organopolysiloxane composition in the eggplant-shaped flask was measured, and the weight of the eggplant-shaped flask and the rotor that had been measured earlier were subtracted to calculate the weight that had evaporated by the operation. The weight of the organopolysiloxane composition after the operation was 1 H-NMR was measured, and the weights of the organic solvent and other components other than the organopolysiloxane were calculated. 1 From the results of H-NMR measurement, the amounts of components other than organopolysiloxane and the amount of volatilized organopolysiloxane were calculated from the weight of the volatilized components.
[0082] (7) Coloring when heated to 250℃ 10 mg of organopolysiloxane was added to a hot plate heated to 250°C, and the coloring was visually confirmed after 10 minutes.
[0083] (8) Viscosity The viscosity was measured at a temperature of 25° C. using an RV-type viscometer RVDV-2+Pro manufactured by Brookfield Instruments, with the organopolysiloxane composition as the measurement subject.
[0084] <Raw materials used in the production of organopolysiloxane> The raw materials used in the production of the organopolysiloxane are shown below. Hexamethyldisiloxane (NuSil Technology) Phenyltrimethoxysilane (KBM-103, manufactured by Shin-Etsu Chemical Co., Ltd.) Toluene (Kishida Chemical Co., Ltd.) Methanol (Kishida Chemical Co., Ltd.) Heptane (Kishida Chemical Co., Ltd.) 1N hydrochloric acid (Kishida Chemical Co., Ltd.) 2N potassium hydroxide solution (Kishida Chemical Co., Ltd.)
[0085] <Production Example 1 (Production Method of Organopolysiloxane Composition 1)> Organopolysiloxane 1 was prepared by hydrolysis and condensation at 40°C for 7 hours using 32 parts of hexamethyldisiloxane, 73 parts of phenyltrimethoxysilane, 19 parts of toluene and 19 parts of methanol as the solvent, and 15 parts of 1N hydrochloric acid as the catalyst and reaction substrate. 13 parts of 2N potassium hydroxide aqueous solution was added, and the mixture was further reacted at 40°C for 2 hours. After removing the potassium component by washing with hydrochloric acid and demineralized water, low boiling point components such as the solvent were distilled off while heating to 80°C using a diaphragm pump. At this time, toluene, methanol, and water were removed to obtain an organopolysiloxane composition. It was confirmed by gas chromatography that the organopolysiloxane composition contained about 3% by weight of tris(trimethylsilyloxy)phenylsilane, which corresponds to the substance represented by the general formula [2]. Then, the mixture was further heated at 40°C for 2 hours. While heating to a high temperature of 120 to 140° C., distillation was continued under high vacuum conditions until toluene peaks were no longer detected, yielding organopolysiloxane composition 1 that is liquid at room temperature.
[0086] The molecular weight of the obtained organopolysiloxane composition 1 was measured, and it was confirmed that the polystyrene-equivalent number average molecular weight (Mn) was 890, the weight average molecular weight (Mw) was 955, and the molecular weight distribution (Mw / Mn) was 1.07. Also, 1 Analysis by H-NMR showed that the amount of phenyl groups was 5.0 mmol / g, the amount of trimethylsiloxy groups was 4.4 mmol / g, and the amount of methoxy groups was 0.3 mmol / g. 29 As a result of Si-NMR measurement, it was confirmed that the values of silicon structural units M, D, T, and Q were M=0.46, D=0, T=0.54, and Q=0, respectively. Furthermore, gas chromatography confirmed that the organopolysiloxane composition contained no traces of methanol or toluene, which were used as solvents, and contained 2.1% by weight of tris(trimethylsilyloxy)phenylsilane, which is represented by the general formula [2]: 4 is a phenyl group, and R 1 ~R 3 It was confirmed that the compound contained a substance with a methyl group and coefficients T2 = 1, M2 = 3, and E2 = 0.
[0087] <Production Example 2 (Production Method of Organopolysiloxane Composition 2)> The distillation operation was continued on organopolysiloxane composition 1 under high temperature and high vacuum conditions to obtain organopolysiloxane composition 2. Tris(trimethylsilyloxy)phenylsilane, which corresponds to the substance represented by general formula [2], was not detected in organopolysiloxane composition 2 by gas chromatography. The molecular weight of the obtained organopolysiloxane composition 2 was measured, and the polystyrene-equivalent number average molecular weight (Mn) was 901, the weight average molecular weight (Mw) was 960, and the molecular weight distribution (Mw / Mn) was 1.07. In addition, 1 Analysis by H-NMR revealed that the amount of phenyl groups was 5.1 mmol / g, the amount of trimethylsiloxy groups was 4.3 mmol / g, and the amount of methoxy groups was 0.26 mmol / g.
[0088] <Production Example 3 (Production Method of Organopolysiloxane Composition 3)> Organopolysiloxane composition 3 was produced under the same production conditions as in Production Example 1, except that the stirring efficiency during the reaction was improved. The molecular weight of the obtained organopolysiloxane composition 3 was measured, and it was confirmed that the polystyrene-equivalent number average molecular weight (Mn) was 905, the weight average molecular weight (Mw) was 976, and the molecular weight distribution (Mw / Mn) was 1.08. 1Analysis by H-NMR revealed that the amount of phenyl groups was 5.2 mmol / g, the amount of trimethylsiloxy groups was 4.2 mmol / g, and the amount of methoxy groups was 0.31 mmol / g. Gas chromatography also confirmed that neither methanol nor toluene, which were used as solvents, was detected in organopolysiloxane composition 3, and that it contained 0.6% by weight of tris(trimethylsilyloxy)phenylsilane. This is represented by the general formula [2]: 4 is a phenyl group, and R 1 From R 3 is a methyl group, and the substance contains coefficients T2 = 1 and M2 = 3.
[0089] <Production Example 4 (Production Method of Organopolysiloxane Composition 4)> Organopolysiloxane composition 4 was produced under the same production conditions as in Production Example 1, except that the reaction time was 21 hours. The molecular weight of the obtained organopolysiloxane composition 4 was measured, and it was confirmed that the polystyrene-equivalent number average molecular weight (Mn) was 926, the weight average molecular weight (Mw) was 1059, and the molecular weight distribution (Mw / Mn) was 1.14. 1 Analysis by H-NMR revealed that the amount of phenyl groups was 5.2 mmol / g, the amount of trimethylsiloxy groups was 4.1 mmol / g, and the amount of methoxy groups was 0.27 mmol / g. Gas chromatography confirmed that the organopolysiloxane composition contained no traces of methanol or toluene, which were used as solvents, and contained 1.3% by weight of tris(trimethylsilyloxy)phenylsilane. This is represented by the general formula [2]: 4 is a phenyl group, and R 1 From R 3 is a methyl group, coefficients T2 = 1, M2 = 3, This means that it contains a substance with E2=0.
[0090] The organopolysiloxanes and compositions produced by the above-mentioned production methods were evaluated and the results are shown in the following table, where tris(trimethylsilyloxy)phenylsilane is abbreviated as PTTSS.
[0091] [Table 1]
[0092] <Production Example 5 (Production Method of Organopolysiloxane Composition 5)> Organopolysiloxane composition 5 was produced under the same production conditions as in Production Example 1, except that when producing based on Production Example 1, the organopolysiloxane composition prior to the step of distilling off the solvent was designated as work-in-progress 5, and potassium hydroxide was distilled off while still adhering to the inside of the kettle in the step of distilling off the solvent from work-in-progress 5. The molecular weight of the obtained organopolysiloxane composition 5 was measured, and the polystyrene equivalent number average molecular weight (Mn) was 937, the weight average molecular weight (Mw) was 1049, and the molecular weight distribution (Mw / Mn) was 1.12. Furthermore, analysis by 1H-NMR revealed that the amount of phenyl groups was 5.1 mmol / g, the amount of trimethylsiloxy groups was 4.4 mmol / g, and the amount of methoxy groups was 0.31 mmol / g. Furthermore, gas chromatography revealed that the organopolysiloxane composition contained 1.8% by weight of tris(trimethylsilyloxy)phenylsilane, and no methanol or toluene was detected as the solvent. This is a compound represented by the general formula [2]: 4 is a phenyl group, and R 1 From R 3 is a methyl group, and the coefficients T2 = 1, M2 = 3, and E2 = 0 are satisfied.
[0093] <Production Example 6 (Production Method of Organopolysiloxane Composition 6)> To the work in progress 5, potassium hydroxide was added so that the concentration was 2 ppm, and the steps after distillation were carried out under the same production conditions as in Production Example 1, thereby producing organopolysiloxane composition 6. The molecular weight of the resulting organopolysiloxane composition 6 was measured, and the polystyrene-equivalent number average molecular weight (Mn) was 963, the weight average molecular weight (Mw) was 1118, and the molecular weight distribution (Mw / Mn) was 1.16.
[0094] <Production Example 7 (Production Method of Organopolysiloxane Composition 7)> Organopolysiloxane Composition 7 was produced under the same production conditions as in Production Example 6, except that the potassium hydroxide concentration in Work in Process 5 was 0.2 ppm. The molecular weight of the resulting organopolysiloxane composition 7 was measured, and the polystyrene-equivalent number average molecular weight (Mn) was 899, the weight average molecular weight (Mw) was 965, and the molecular weight distribution (Mw / Mn) was 1.07.
[0095] The evaluation results of the organopolysiloxane compositions used in the examples are shown in Tables 2 to 4. In the examples, PTTSS stands for tris(trimethylsiloxy)phenylsilane.
[0096] [Table 2]
[0097] From Table 2, it was suggested that the viscosity can be adjusted by adding a substance represented by general formula [2] to an organopolysiloxane composition consisting of general formula [1], or by leaving it as an organopolysiloxane composition, and that the substance has transparent mixing with resin, does not have an odor, and does not color when heated, and that even if it is contained at 7.5% by weight, the amount of low-boiling point components volatilized is small, and does not affect the process problem during molding or the deterioration of the properties of the molded product, but if it is contained at 10% by weight or more, the amount of volatilization increases and may become a problem. In addition, when toluene is used as a solvent, even at 5% by weight, the entire amount volatilizes, suggesting that even if the viscosity can be reduced, the adverse effect is large when a general organic solvent is used, and it was surprisingly found that the substance represented by general formula [2] has a very low volatilization rate from the organopolysiloxane composition consisting of general formula [1].
[0098] [Table 3]
[0099] Table 3 shows that it is possible to adjust the viscosity by adding the component represented by general formula [2] to the high-viscosity organopolysiloxane composition represented by general formula [1]. In addition, the results of the solvent clouding test suggest that it is possible to mix it with resin without affecting its mixability.
[0100] [Table 4]
[0101] [Table 5]
[0102] From Tables 4 and 5, it was found that in the method for producing organopolysiloxane, when potassium hydroxide is included during the heating operation, the molecular weight and molecular weight distribution increase and the compatibility with the resin changes depending on the content. The content of potassium hydroxide in the organopolysiloxane composition is preferably 2 ppm or less, more preferably 0.2 ppm or less. On the other hand, when it is desired to express the function by adjusting the dispersibility with the resin, it is also possible to adjust the molecular weight by increasing the potassium hydroxide content, and in that case, as shown in Table 3, it was suggested that the substance represented by the general formula [2] does not change the mixed dispersibility.
[0103] As described above, the present invention can provide an organopolysiloxane composition that has a low viscosity and excellent dispersibility in various resins.
Claims
1. A resin composition comprising an organopolysiloxane composition and another resin, The organopolysiloxane composition comprises: Component A is an organopolysiloxane represented by the following general formula [1] and having silicon units selected from the group consisting of MD units, MT units, MQ units, MDT units, MDQ units, MDTQ units, DT units, DQ units, DTQ units, and TQ units; Component B includes a substance represented by the following general formula [2], The component A and the component B are 0.1≦{(weight of component B)×100} / {(weight of component A)+(weight of component B)}≦9 and For component A, The content of the substance in which the coefficients T2, M2, and E2 in the formula [2] satisfy T2+2-M2+E2=0 is 0.01% by weight or more and 9% by weight or less, The content of substances in which the coefficients T2, M2, and E2 in the formula [2] do not satisfy T2+2-M2+E2=0 is 3% by weight or less. A resin composition comprising: R X SiO (4-X) / 2 ... [1] (R 1 R 2 R 3 SiO 1/2 ) M2 (R 4 SiO 3/2 ) T2 (O 1/2 R 5 ) E2 ・・・[2] Here, in the above formula [1], R each independently has an atom or group selected from the group consisting of a (meth)acrylic group, a carboxyl group, a nitrile group, a formyl group, a carbonyl group, a carbinol group, an amino group, an imino group, a nitro group, a cyano group, a sulfo group, a mercapto group, an alkyl group having 1 to 20 carbon atoms, a cyclopentyl group, a cyclohexyl group, an ethylene glycol monoethylene ether group, an acryloxypropyl group, an acryloxyoctyl group, a methacryloxypropyl group, a methacryloxyoctyl group, a glycidyl group, a glycidoxypropyl group, a glycidoxyoctyl group, a 1,2-epoxycyclohexyl-3-propyl group, a 1,2-epoxycyclohexyl-3-octyl group, a phenyl group, a phenethylene group, and a styryl group; and coefficients X each independently satisfy 0<X≦3; Here, in the above formula [2], R 1 ~R 4 are each independently selected from the group consisting of a (meth)acrylic group, a carboxyl group, a nitrile group, a formyl group, a carbonyl group, a carbinol group, an amino group, an imino group, a nitro group, a cyano group, a sulfo group, a mercapto group, an alkyl group having 1 to 20 carbon atoms, a cyclopentyl group, a cyclohexyl group, an ethylene glycol monoethylene ether group, an acryloxypropyl group, an acryloxyoctyl group, a methacryloxypropyl group, a methacryloxyoctyl group, a glycidyl group, a glycidoxypropyl group, a glycidoxyoctyl group, a 1,2-epoxycyclohexyl-3-propyl group, a 1,2-epoxycyclohexyl-3-octyl group, a phenyl group, a phenethylene group, and a styryl group, and may be the same or different. R 5 are selected from the group consisting of a hydrogen atom, a methyl group, an ethyl group, a butyl group, an octyl group, and an octadecyl group, and may be the same or different; The coefficient M2 is a positive integer between 1 and 5; the coefficient T2 is a positive integer between 1 and 3; and the coefficient E2 is an integer between 0 and 5.
2. 2. The resin composition according to claim 1, wherein the organopolysiloxane comprises dimethylpolysiloxane or MQ resin.
3. 3. The resin composition according to claim 1, wherein the organopolysiloxane has a group selected from the group consisting of a trimethylsiloxy group, a dimethylvinyltrimethylsiloxy group, and a dimethylsiloxy group.
4. 4. The resin composition according to claim 1, wherein the organopolysiloxane has a phenyl group.
5. The resin composition according to any one of claims 1 to 4, characterized in that when 200 g of the organopolysiloxane composition is placed in a 1 L eggplant-shaped flask and heated for 2 hours at an internal temperature of 110°C under reduced pressure using a vacuum pump having an exhaust capacity of a vacuum pressure of 0.15 torr, the amount of mass loss of the organopolysiloxane is 10 g or less.
6. The resin composition according to any one of claims 1 to 5, wherein the organopolysiloxane is liquid at 40°C.
7. The resin composition according to any one of claims 1 to 6, characterized in that the organopolysiloxane has a number average molecular weight Mn of 750 or more and 10,000 or less.
8. The resin composition according to any one of claims 1 to 7, characterized in that the ratio of the weight average molecular weight Mw of the organopolysiloxane to the number average molecular weight Mn (molecular weight distribution: Mw / Mn) is 1.01 or more and 5 or less.
9. In the general formula [2], R 4 The resin composition according to any one of claims 1 to 8, wherein is a phenyl group.
10. In the general formula [2], R 1 ~R 3 The resin composition according to any one of claims 1 to 9, characterized in that is a methyl group.
11. The resin composition according to any one of claims 1 to 10, characterized in that the resin composition contains a substance having a coefficient T2 of 1 as the substance represented by the general formula [2].
12. The resin composition according to any one of claims 1 to 11, characterized in that the resin composition contains a substance having a coefficient M2 of 3 as the substance represented by the general formula [2].
13. The resin composition according to any one of claims 1 to 12, characterized in that the content of the substance represented by the general formula [2] in the organopolysiloxane composition is 0.5 to 3 wt%.
14. The resin composition according to any one of claims 1 to 13, wherein the content of the organopolysiloxane composition in the resin composition is 15% by weight or less.
15. the other resin is a resin having a (meth)acryloyl group, R is selected from the group consisting of acryloxypropyl, methacryloxypropyl, methacryloxyoctyl, glycidoxypropyl, glycidoxyoctyl, and methyl; R 1 ~R 3 are all methyl groups, R 4 The resin composition according to claim 1, wherein is selected from the group consisting of an acryloxypropyl group, a methacryloxypropyl group, a methacryloxyoctyl group, a glycidoxypropyl group, a glycidoxyoctyl group, and a phenyl group.
16. the other resin is polycarbonate, R is selected from the group consisting of ethylene glycol monoethylene ether, glycidoxypropyl, glycidoxyoctyl, phenyl, phenethylene, styryl, vinyl, and methyl; R 1 ~R 3 are all methyl groups, R 4 The resin composition according to claim 1 , wherein is a phenyl group.
17. A member for electronic equipment, comprising the resin composition according to any one of claims 1 to 16 or a cured product thereof.
18. A resin additive comprising an organopolysiloxane composition, The organopolysiloxane composition comprises: Component A is an organopolysiloxane represented by the following general formula [1] and having silicon units selected from the group consisting of MD units, MT units, MQ units, MDT units, MDQ units, MDTQ units, DT units, DQ units, DTQ units, and TQ units; Component B includes a substance represented by the following general formula [2], The component A and the component B are 0.1≦{(weight of component B)×100} / {(weight of component A)+(weight of component B)}≦9 and For component A, The content of the substance in which the coefficients T2, M2, and E2 in the formula [2] satisfy T2+2-M2+E2=0 is 0.01% by weight or more and 9% by weight or less, The content of substances in which the coefficients T2, M2, and E2 in the formula [2] do not satisfy T2+2-M2+E2=0 is 3% by weight or less. A resin additive characterized by: R X SiO (4-X) / 2 ... [1] (R 1 R 2 R 3 SiO 1/2 ) M2 (R 4 SiO 3/2 ) T2 (O 1/2 R 5 ) E2 ・・・[2] Here, in the above formula [1], R each independently has an atom or group selected from the group consisting of a (meth)acrylic group, a carboxyl group, a nitrile group, a formyl group, a carbonyl group, a carbinol group, an amino group, an imino group, a nitro group, a cyano group, a sulfo group, a mercapto group, an alkyl group having 1 to 20 carbon atoms, a cyclopentyl group, a cyclohexyl group, an ethylene glycol monoethylene ether group, an acryloxypropyl group, an acryloxyoctyl group, a methacryloxypropyl group, a methacryloxyoctyl group, a glycidyl group, a glycidoxypropyl group, a glycidoxyoctyl group, a 1,2-epoxycyclohexyl-3-propyl group, a 1,2-epoxycyclohexyl-3-octyl group, a phenyl group, a phenethylene group, and a styryl group; and coefficients X each independently satisfy 0<X≦3; Here, in the above formula [2], R 1 ~R 4 are each independently selected from the group consisting of a (meth)acrylic group, a carboxyl group, a nitrile group, a formyl group, a carbonyl group, a carbinol group, an amino group, an imino group, a nitro group, a cyano group, a sulfo group, a mercapto group, an alkyl group having 1 to 20 carbon atoms, a cyclopentyl group, a cyclohexyl group, an ethylene glycol monoethylene ether group, an acryloxypropyl group, an acryloxyoctyl group, a methacryloxypropyl group, a methacryloxyoctyl group, a glycidyl group, a glycidoxypropyl group, a glycidoxyoctyl group, a 1,2-epoxycyclohexyl-3-propyl group, a 1,2-epoxycyclohexyl-3-octyl group, a phenyl group, a phenethylene group, and a styryl group, and may be the same or different. R 5 are selected from the group consisting of a hydrogen atom, a methyl group, an ethyl group, a butyl group, an octyl group, and an octadecyl group, and may be the same or different; The coefficient M2 is a positive integer between 1 and 5; the coefficient T2 is a positive integer between 1 and 3; and the coefficient E2 is an integer between 0 and 5.
19. 1. An organopolysiloxane composition for use in a resin, comprising: Component A is an organopolysiloxane represented by the following general formula [1] and having silicon units selected from the group consisting of MD units, MT units, MQ units, MDT units, MDQ units, MDTQ units, DT units, DQ units, DTQ units, and TQ units; Component B includes a substance represented by the following general formula [2], The component A and the component B are 0.1≦{(weight of component B)×100} / {(weight of component A)+(weight of component B)}≦9 and For component A, The content of the substance in which the coefficients T2, M2, and E2 in the formula [2] satisfy T2+2-M2+E2=0 is 0.01% by weight or more and 9% by weight or less, The content of substances in which the coefficients T2, M2, and E2 in the formula [2] do not satisfy T2+2-M2+E2=0 is 3% by weight or less. An organopolysiloxane composition for use as an additive to a resin, comprising: R X SiO (4-X) / 2 ... [1] (R 1 R 2 R 3 SiO 1/2 ) M2 (R 4 SiO 3/2 ) T2 (O 1/2 R 5 ) E2 ・・・[2] In the above formula [1], each R is independently an atom selected from the group consisting of a (meth)acrylic group, a carboxyl group, a nitrile group, a formyl group, a carbonyl group, a carbinol group, an amino group, an imino group, a nitro group, a cyano group, a sulfo group, a mercapto group, an alkyl group having 1 to 20 carbon atoms, a cyclopentyl group, a cyclohexyl group, an ethylene glycol monoethylene ether group, an acryloxypropyl group, an acryloxyoctyl group, a methacryloxypropyl group, a methacryloxyoctyl group, a glycidyl group, a glycidoxypropyl group, a glycidoxyoctyl group, a 1,2-epoxycyclohexyl-3-propyl group, a 1,2-epoxycyclohexyl-3-octyl group, a phenyl group, a phenethylene group, and a styryl group. or a group, and each coefficient X is independently 0<X≦3; Here, in the above formula [2], R 1 ~R 4 are each independently selected from the group consisting of a (meth)acrylic group, a carboxyl group, a nitrile group, a formyl group, a carbonyl group, a carbinol group, an amino group, an imino group, a nitro group, a cyano group, a sulfo group, a mercapto group, an alkyl group having 1 to 20 carbon atoms, a cyclopentyl group, a cyclohexyl group, an ethylene glycol monoethylene ether group, an acryloxypropyl group, an acryloxyoctyl group, a methacryloxypropyl group, a methacryloxyoctyl group, a glycidyl group, a glycidoxypropyl group, a glycidoxyoctyl group, a 1,2-epoxycyclohexyl-3-propyl group, a 1,2-epoxycyclohexyl-3-octyl group, a phenyl group, a phenethylene group, and a styryl group, and may be the same or different. R 5 are selected from the group consisting of a hydrogen atom, a methyl group, an ethyl group, a butyl group, an octyl group, and an octadecyl group, and may be the same or different; The coefficient M2 is a positive integer between 1 and 5; the coefficient T2 is a positive integer between 1 and 3; and the coefficient E2 is an integer between 0 and 5.
20. The organopolysiloxane composition for use as a resin additive is 20. The organopolysiloxane composition for use in a resin according to claim 19, which is added to any resin selected from the group consisting of resins having a (meth)acryloyl group and polycarbonates.
Citation Information
Patent Citations
Organosiloxane composition
JP1997111123A
Curable composition, cured film, polysiloxane and optical semiconductor device
JP2013028709A
Polysiloxane
JP2014074183A
Dam material composition for image display apparatus and image display apparatus using the same
JP2014218582A
Polyorganosiloxane, polyorganosiloxane composition, cured product, polyorganosiloxane-containing electrolytic solution for electrolytic capacitor, and electrolytic capacitor using same
WO2018110613A1