Method for producing chemically modified microfibril cellulose fibers
Treating chemically modified cellulose with hydrogen peroxide and defibrating it produces microfibrillar cellulose fibers with low viscosity dispersions, addressing the challenge of achieving low viscosity in existing methods.
Patent Information
- Application Number
- JP2020113440
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-06-30
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-06-30
AI Technical Summary
Existing methods struggle to produce chemically modified microfibrillar cellulose fibers that provide a low-viscosity dispersion.
A method involving the treatment of chemically modified cellulose with hydrogen peroxide, followed by defibration, to produce chemically modified microfibrillar cellulose fibers.
The method results in chemically modified microfibrillar cellulose fibers that yield low-viscosity dispersions.
Smart Images

Figure 0007574553000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing chemically modified microfibrillated cellulose fibers, and more particularly to a method for producing fibrillated chemically modified cellulose fibers that provide a low viscosity aqueous dispersion. [Background technology]
[0002] Chemically modified microfibrillated cellulose fibers are obtained by modifying cellulose raw materials such as pulp and then defibrating or pulverizing them, and are expected to be used as additives to improve paper strength and water retention, as well as additives for foods and cosmetics.
[0003] For example, Patent Document 1 describes a fine fibrous cellulose-containing material having a viscosity of 2800 mPa·s or more measured at 3 rpm and 25°C using a B-type viscometer and a haze value of 10% to 50%. Patent Document 2 describes oxidized microfibril cellulose having a Canadian standard freeness of less than 200 ml and an average fiber diameter of 500 nm or more. Patent Document 3 describes carboxymethylated microfibril cellulose fiber paper having a Canadian standard freeness of 200 ml or more and an average fiber diameter of 500 nm or more. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-57390 A [Patent Document 2] International Publication No. 2019 / 189588 [Patent Document 3] International Publication No. 2019 / 189595 Summary of the Invention [Problem to be solved by the invention]
[0005] However, it is difficult to produce chemically modified microfibril cellulose fibers that give a dispersion liquid with low viscosity using the methods described in Patent Documents 1 to 3. In view of the above, an object of the present invention is to provide a method for producing chemically modified microfibril cellulose fibers that give a dispersion liquid with low viscosity. [Means for solving the problem]
[0006] The present inventors have found that the above problems can be solved by treating chemically modified cellulose with hydrogen peroxide. The present invention includes, but is not limited to, the following aspects. (1) A method for producing chemically modified microfibril cellulose fibers, comprising the following steps (A) to (C): (A) Preparation of chemically modified cellulose (B) treating the chemically modified cellulose with peroxide. (C) A step of defibrating the chemically modified cellulose after the treatment to obtain chemically modified microfibril cellulose fibers. (2) The method according to (1), wherein the amount of the peroxide added is 0.1 to 100% by mass based on the bone dry weight of the chemically modified cellulose. (3) The method according to any one of (1) to (2), wherein the step (B) is carried out in a mixture containing a peroxide, a chemically modified cellulose, and a medium, and the concentration of the chemically modified cellulose in the mixture is 0.1 to 50% by mass. (4) The method according to any one of (1) to (3), wherein the chemically modified cellulose is a cellulose having a carboxyl group. (5) The method according to any one of (1) to (3), wherein the chemically modified cellulose is carboxymethylated cellulose. Effect of the Invention
[0007] The chemically modified microfibril cellulose fibers produced according to the present invention have the characteristic of providing a dispersion having a low viscosity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The present invention will be described in detail. In the present invention, "X to Y" includes the extreme values X and Y. nothing.
[0009] The method for producing chemically modified microfibril cellulose fibers of the present invention essentially comprises the steps of (A) preparing chemically modified cellulose, (B) treating the chemically modified cellulose with peroxide, and (C) defibrating the treated chemically modified cellulose to obtain chemically modified microfibril cellulose fibers.
[0010] (1) Process A <Chemically modified cellulose> The chemically modified cellulose used in the chemically modified microfibril cellulose fiber of the present invention is one in which the cellulose chains constituting the fiber have been chemically modified. The types of chemically modified cellulose are not limited to these, but examples include carboxylated cellulose in which a carboxyl group has been introduced, carboxyalkylated cellulose in which a carboxyalkyl group such as a carboxymethyl group has been ether-bonded, and phosphoric acid esterified cellulose in which a phosphoric acid group has been introduced. Among these, oxidation (carboxylation), etherification (e.g., carboxyalkylation), cationization, and esterification are preferred, and oxidation (carboxylation) and carboxyalkylation are more preferred. The production methods of these will be described later.
[0011] Chemically modified cellulose may take the form of a salt, and the term "chemically modified cellulose" as used herein includes salt-type chemically modified cellulose. Examples of salt-type chemically modified cellulose include those that form metal salts such as sodium salts.
[0012] The chemically modified cellulose used in the chemically modified microfibril cellulose fiber of the present invention maintains at least a part of its fibrous shape even when dispersed in water, i.e., when an aqueous dispersion of the chemically modified cellulose fiber is observed with an electron microscope or the like, a fibrous substance can be observed, and when measured by X-ray diffraction, a peak of cellulose type I crystals can be observed.
[0013] <Chemically modified microfibril cellulose fiber> The chemically modified microfibrillated cellulose fiber of the present invention is obtained by moderately beating or defibrating (fibrillating) a chemically modified cellulose raw material using a refiner or the like. Compared to chemically modified cellulose fibers that have not been beaten or defibrated, the chemically modified microfibrillated cellulose fiber has cellulose microfibril fluff on the fiber surface. In addition, compared to chemically modified cellulose nanofibers, the fiber diameter is larger and the fiber surface is efficiently fuzzed (external fibrillation) while minimizing the fiber itself (internal fibrillation).
[0014] Furthermore, the chemically modified microfibril cellulose fiber of the present invention has characteristics such as high water retention and high thixotropy due to the chemical modification, compared to microfibril cellulose fiber that is not chemically modified.
[0015] In addition, the chemically modified microfibrillated cellulose fibers obtained by fibrillating the chemically modified cellulose raw material of the present invention have the characteristic that, compared to cellulose raw material that is not chemically modified and then chemically modified, the cellulose fibers are chemically modified during fibrillation, weakening the strong hydrogen bonds between the fibers, making it easier for the fibers to come apart during fibrillation and resulting in less damage to the fibers.
[0016] The chemically modified microfibrillated cellulose fiber of the present invention has an average fiber diameter of 500 nm or more, preferably 1 μm or more, and more preferably 10 μm or more. The upper limit of the average fiber diameter is preferably 60 μm or less, more preferably 40 μm or less, even more preferably 30 μm or less, and even more preferably 20 μm or less. By performing moderate fibrillation to an extent that the average fiber diameter falls within this range, the fiber exhibits higher water retention than undefibrated cellulose fibers, and even in small amounts, a higher strength imparting effect and a higher yield improvement effect can be obtained compared to finely defibrated cellulose nanofibers.
[0017] The average fiber length of the chemically modified microfibrillated cellulose fiber is preferably 200 μm or more, more preferably 250 μm or more, and more preferably 300 μm or more. The upper limit of the average fiber length is not particularly limited, but is preferably 3000 μm or less, more preferably 2500 μm or less, more preferably 2000 μm or less, and even more preferably 1500 μm or less. According to the present invention, since a chemically modified cellulose raw material is used for beating or defibration, fibrillation can be promoted without extremely shortening the fibers. In addition, since the affinity with water is improved by the chemical modification, water retention can be increased even when the fiber length is long.
[0018] The average fiber diameter and average fiber length can be determined by an image analysis type fiber analyzer such as an L&W Fiber Tester Plus manufactured by ABB Corp. or a Fractionator manufactured by Valmet Corp. Specifically, when a fractionator is used, the average fiber diameter and average fiber length can be determined as the length-weighted fiber width and the length-weighted average fiber length, respectively.
[0019] The aspect ratio of the chemically modified microfibril cellulose fiber is preferably 10 or more, more preferably 15 or more, and even more preferably 20 or more. There is no particular upper limit to the aspect ratio, but it is preferably 1000 or less, more preferably 100 or less, and even more preferably 80 or less. The aspect ratio can be calculated by the following formula: Aspect ratio = average fiber length / average fiber diameter
[0020] The fibrillation rate (Fibrillation %) of the chemically modified microfibrillated cellulose fiber measured using a fractionator manufactured by Valmet Co., Ltd. is preferably 1.0% or more, more preferably 1.2% or more, and even more preferably 1.5% or more. Although the fibrillation rate varies depending on the type of cellulose raw material used, it is considered that fibrillation has been performed within the above range. In addition, in the present invention, it is preferable to perform fibrillation so that the fibrillation rate (f0) of the chemically modified cellulose raw material before fibrillation is improved. If the fibrillation rate of the fibrillated chemically modified cellulose fiber is f, the difference in the fibrillation rates Δf=f-f0 should be more than 0, and is preferably 0.1% or more, more preferably 0.2% or more, and even more preferably 0.3% or more.
[0021] <Crystallization degree of cellulose type I> The crystallinity of the cellulose in the chemically modified microfibril cellulose fiber of the present invention is 50% or more, and more preferably 60% or more, for crystalline type I. The crystallinity of the cellulose can be controlled by the degree of chemical modification. There is no particular upper limit to the crystallinity of cellulose type I. In reality, the upper limit is thought to be about 90%.
[0022] The method for measuring the crystallinity of cellulose type I of chemically modified cellulose fibers is as follows: The sample is placed in a glass cell and measured using an X-ray diffraction measuring device (LabX XRD-6000, manufactured by Shimadzu Corporation). The degree of crystallinity is calculated using the method of Segal et al., and is calculated from the diffraction intensity of the 002 plane at 2θ = 22.6° and the diffraction intensity of the amorphous part at 2θ = 18.5° using the diffraction intensity of the X-ray diffraction pattern at 2θ = 10° to 30° as the baseline, according to the following formula.
[0023] Xc = (I002c - Ia) / I002c x 100 Xc = Crystallinity of cellulose type I (%) I002c: 2θ=22.6°, diffraction intensity of 002 plane Ia: 2θ=18.5°, diffraction intensity of the amorphous part.
[0024] <Degree of anionization> The degree of anionization (anion charge density) of the chemically modified microfibril cellulose fiber of the present invention is usually 2.50 meq / g or less, preferably 2.30 meq / g or less, more preferably 2.00 meq / g or less, and even more preferably 1.50 meq / g or less, 1.00 meq / g or less. This is considered to make the chemical modification more uniform throughout the cellulose than chemically modified cellulose fibers having a higher degree of anionization, and it is considered to make it possible to obtain the effects specific to chemically modified cellulose fibers, such as water retention, more stably. The lower limit is usually 0.08 meq / g or more, preferably 0.10 meq / g or more, more preferably 0.30 meq / g or more, but is not particularly limited. Therefore, it is preferable that the degree of anionization is 0.08 meq / g or more and 2.50 meq / g or less. The degree of anionization is the equivalent of anion per unit mass of modified cellulose microfibril, and can be calculated from the equivalent of diallyldimethylammonium chloride (DADMAC) required to neutralize the anionic groups in unit mass of modified cellulose microfibril. In the present invention, the method for measuring the degree of anionization is as follows.
[0025] Chemically modified cellulose fibers are dispersed in water to prepare an aqueous dispersion with a solid content of 10 g / L, and stirred at 1000 rpm for 10 minutes or more using a magnetic stirrer. The resulting slurry is diluted to 0.1 g / L, and 10 ml of the mixture is taken and titrated with 1 / 1000 normality diallyldimethylammonium chloride (DADMAC) using a streaming current detector (Mutek Particle Charge Detector 03). The amount of DADMAC added until the streaming current becomes zero is used to calculate the degree of anionization according to the following formula: q=(V×c) / m q: degree of anionization (meq / g) V: Amount of DADMAC added until the streaming current becomes zero (L) c: DADMAC concentration (meq / L) m: Mass (g) of chemically modified microfibrillated cellulose fibers in the measurement sample
[0026] <Water retention capacity> The chemically modified microfibrillated cellulose fibers of the present invention preferably have a water retention capacity of 15 or more as measured by the following method. The method for measuring the water retention capacity is as follows: Prepare 40 mL of a slurry (medium: water) with a solid content of 0.3% by mass of chemically modified microfibrillated cellulose fibers. Let the mass of this slurry be A. Next, centrifuge the entire amount of the slurry at 30 °C and 25000 G for 30 minutes using a high-speed cooling centrifuge to separate the aqueous phase and the sediment. Let the mass of the sediment at this time be B. Also, put the aqueous phase into an aluminum cup, dry it at 105 °C for one day and night to remove water, and measure the mass of the solid content in the aqueous phase. Let the mass of the solid content in this aqueous phase be C. Calculate the water retention capacity using the following formula. Water retention capacity = (B + C - 0.003×A) / (0.003×A - C).
[0027] As described by the above formula, the water retention capacity corresponds to the mass of water in the sediment relative to the mass of the solid content of the fibers in the sediment. The larger the value, the higher the ability of the fibers to hold water. The water retention capacity of the fibrillated chemically modified cellulose fibers of the present invention is preferably 15 or more, more preferably 20 or more, and even more preferably 30 or more. The upper limit is not particularly limited, but is considered to be about 200 or less in reality.
[0028] Note that the above method for measuring the water retention capacity is for fibrillated fibers, and it is not usually applicable to non-fibrillated or defibrated fibers or cellulose nanofibers defibrated to single microfibrils. If attempting to measure the water retention capacity of non-fibrillated or defibrated cellulose fibers by the above method, a dense sediment cannot be formed under the above centrifugation conditions, and it is difficult to separate the sediment and the aqueous phase. Also, cellulose nanofibers hardly sediment under the above centrifugation conditions.
[0029] <B-type viscosity> In the present invention, the method for measuring the Brookfield viscosity is as follows: The chemically modified microfibril cellulose fiber is weighed out into a polypropylene container and dispersed in 160 ml of ion-exchanged water to prepare an aqueous dispersion with a solid content of 1% by mass. The aqueous dispersion is adjusted to 25°C. Then, the viscosity is measured after 1 minute at a rotation speed of 60 rpm using a B-type viscometer (manufactured by Toki Sangyo Co., Ltd.) according to the method of JIS-Z-8803.
[0030] The upper limit of the Brookfield viscosity (25°C, 60 rpm) of the chemically modified microfibril cellulose fiber of the present invention is 4,000 mPa s or less, preferably 3,000 mPa s or less, more preferably 2,000 mPa s or less, and the lower limit is 40 mPa s or more, preferably 50 mPa s or more, more preferably 60 mPa s or more.
[0031] <Other> The chemically modified microfibril cellulose fiber of the present invention has an electrical conductivity of preferably 500 mS / m or less when dispersed in water at a solid content concentration of 1.0% by mass. More preferably, it is 300 mS / m or less, even more preferably 200 mS / m or less, even more preferably 100 mS / m or less, and even more preferably 70 mS / m or less. The lower limit of the electrical conductivity is preferably 5 mS / m or more, and more preferably 10 mS / m or more. The electrical conductivity can be measured by the following method: 200 g of an aqueous dispersion of chemically modified microfibril cellulose fiber with a solid content concentration of 1.0% by mass is prepared and thoroughly stirred, and then the electrical conductivity is measured using an electrical conductivity meter (HORIBA ES-71 model).
[0032] The chemically modified microfibril cellulose fiber of the present invention preferably has a BET specific surface area of 30 m 2 / g or more, more preferably 50m 2 / g or more, more preferably 70m 2 / g or more. If the BET specific surface area is high, for example, when used as a papermaking additive, it is easier to bind to pulp, which has the advantage of improving yield and increasing the effect of adding strength to paper. The BET specific surface area can be measured by the following method, referring to the nitrogen gas adsorption method (JIS Z 8830): (1) Approximately 2% slurry of chemically modified microfibril cellulose fiber (dispersion medium: water) is separated and placed in a centrifuge container so that the solid content is approximately 0.1 g, and 100 ml of ethanol is added. (2) Add a stirrer and stir at 500 rpm for at least 30 minutes. (3) Remove the stirrer and sediment the chemically modified microfibril cellulose fibers in a centrifuge at 7,000 G for 30 minutes at 30°C. (4) The supernatant is removed while trying to avoid removing as much of the chemically modified microfibril cellulose fibers as possible. (5) Add 100 ml of ethanol, add a stir bar, stir under conditions (2), centrifuge under conditions (3), and remove the supernatant under conditions (4). Repeat this process three times. (6) The solvent in (5) is changed from ethanol to t-butanol, and the stirring, centrifugation, and removal of the supernatant are repeated three times in the same manner as in (5) at room temperature above the melting point of t-butanol. (7) After the final solvent removal, add 30 ml of t-butanol, mix gently, then transfer to a recovery flask and freeze in an ice bath. (8) Chill in the freezer for at least 30 minutes. (9) Place in a freeze-dryer and freeze-dry for 3 days. (10) Perform BET measurement (pretreatment conditions: 2 hours at 105°C under nitrogen flow, relative pressure 0.01 to 0.30, sample amount approximately 30 mg).
[0033] The Shopper-Riegler freeness of the chemically modified microfibril cellulose fiber of the present invention is not particularly limited, but is preferably 1°SR or more, more preferably 10°SR or more, and more preferably 25°SR or more. The method for measuring the Shopper-Riegler freeness is in accordance with JIS P 82121-1:2012, and specifically, is as follows.
[0034] Chemically modified microfibrillated cellulose fibers are dispersed in water to prepare an aqueous dispersion with a solid content of 10 g / L, which is then stirred at 1000 rpm for 10 minutes or more using a magnetic stirrer. The resulting slurry is diluted to 2 g / L. A 60 mesh screen (wire diameter 0.17 mm) is set on a Mutec DFR-04, and the amount of liquid passing through the mesh from a 1000 ml test solution is measured for 60 seconds, and the Shopper-Riegler freeness is calculated according to the method of JIS P 8121-1:2012.
[0035] The Shopper-Riegler freeness is a measure of the degree of drainage of a fiber suspension, with the lower limit being 0°SR and the upper limit being 100°SR, and the closer the Shopper-Riegler freeness is to 100°SR, the less drainage (amount of drainage) is indicated. The Shopper-Riegler freeness of the fibrillated chemically modified cellulose fiber of the present invention is not particularly limited, but the lower limit is preferably 1°SR or more, more preferably 10°SR or more, more preferably 25°SR or more, more preferably 40°SR or more, and even more preferably 50°SR or more. The upper limit is not particularly limited, and is 100°SR or less.
[0036] The chemically modified microfibrillated cellulose fiber of the present invention, when dispersed in water with a solid content of 1% by mass, preferably has a transparency (transmittance of 660 nm light) of less than 60%, more preferably 40% or less, even more preferably 30% or less, and even more preferably 20% or less. There is no particular lower limit and it may be 0% or more. When the transparency is in this range, the degree of fibrillation is appropriate and the effects of the present invention are easily obtained. The transparency can be measured by the following method: An aqueous dispersion of chemically modified microfibril cellulose fiber (solid content 1% (w / v), dispersion medium: water) is prepared, and the transmittance of light with a wavelength of 660 nm is measured using a UV-VIS spectrophotometer UV-1800 (Shimadzu Corporation) with a square cell with an optical path length of 10 mm.
[0037] When the chemically modified microfibril cellulose fiber of the present invention is dispersed in water, it becomes a translucent to white gel, cream or paste at a solids concentration of about 2% or more.
[0038] The chemically modified microfibril cellulose fibers may be in the form of a dispersion obtained after production, but may be dried or redispersed in water as necessary. The drying method is not particularly limited, and known methods such as freeze drying, spray drying, tray drying, drum drying, belt drying, thin spreading on a glass plate or the like and drying, fluidized bed drying, microwave drying, and heated fan reduced pressure drying can be used. After drying, the fibers may be pulverized using a cutter mill, hammer mill, pin mill, jet mill, or the like as necessary. The method of redispersing in water is also not particularly limited, and known dispersing devices can be used.
[0039] The chemically modified microfibril cellulose fiber of the present invention is used in various applications. Since it has excellent water retention, it is considered that it can be used particularly optimally in applications requiring shape retention and water retention. In addition, since the degree of defibration is not too strong and the fiber diameter is moderate, it is considered that it can be used particularly optimally in applications requiring fiber strength or applications requiring high fiber yield. However, it may be used for other applications. The fields in which the chemically modified microfibril cellulose fiber is used are not limited, and it is considered that it can be used as a thickener, gelling agent, paste, food additive, excipient, paint additive, adhesive additive, papermaking additive, abrasive, rubber and plastic compounding material, water retention agent, shape retention agent, muddy water regulator, filter aid, overflow prevention agent, etc. in various fields in which additives are generally used, such as food, beverage, cosmetics, medicine, papermaking, various chemical products, paint, spray, agricultural chemicals, civil engineering, construction, electronic materials, flame retardants, household goods, adhesives, cleaning agents, fragrances, lubricating compositions, etc.
[0040] <Method of manufacturing chemically modified microfibril cellulose fiber> The chemically modified microfibrillated cellulose fiber of the present invention can be produced by first preparing a chemically modified cellulose raw material and then fibrillating it. As the types of chemical modification, as described above, for example, carboxylation, carboxyalkylation, phosphorylation, etc. of cellulose can be mentioned, but are not limited to these. The chemically modified cellulose raw material to be subjected to fibrillation may be a commercially available product, or may be produced by chemically modifying the cellulose raw material described below by the method described below.
[0041] <Cellulose raw material> The cellulose that is the raw material for the chemically modified microfibril cellulose fiber of the present invention is not particularly limited, and examples thereof include those derived from plants, animals (e.g., ascidians), algae, microorganisms (e.g., acetic acid bacteria (Acetobacter)), and microbial products. Examples of those derived from plants include wood, bamboo, hemp, jute, kenaf, agricultural waste, cloth, and pulp (softwood unbleached kraft pulp (NUKP), softwood bleached kraft pulp (NBKP), hardwood unbleached kraft pulp (LUKP), hardwood bleached kraft pulp (LBKP), softwood unbleached sulfite pulp (NUSP), softwood bleached sulfite pulp (NBSP), thermomechanical pulp (TMP), softwood dissolving pulp, hardwood dissolving pulp, recycled pulp, waste paper, etc.). Cellulose powder obtained by pulverizing the above-mentioned cellulose raw material may also be used. As the cellulose raw material, any one or a combination of these may be used, but cellulose fibers derived from plants or microorganisms are preferred, cellulose fibers derived from plants are more preferred, and wood-based pulp is even more preferred.
[0042] In order to maintain a crystallinity of cellulose type I of 50% or more in the chemically modified microfibril cellulose fiber, it is preferable to use cellulose having a high crystallinity of cellulose type I as the raw material. The crystallinity of the cellulose raw material is preferably 70% or more, more preferably 80% or more. The method for measuring the crystallinity of cellulose type I is the same as that described above.
[0043] <Carboxylation of cellulose raw materials> As an example of a chemically modified cellulose raw material, a carboxylated (introduction of a carboxyl group into cellulose, also called "oxidation") cellulose raw material can be used. The carboxylated cellulose raw material (also called "oxidized cellulose raw material") may be a commercially available product, or may be produced by carboxylating (oxidizing) the above-mentioned cellulose raw material by a known method. The amount of carboxyl groups is preferably 0.1 to 2.5 mmol / g, more preferably 0.6 mmol / g to 2.5 mmol / g, and even more preferably 1.0 mmol / g to 2.0 mmol / g, based on the bone dry mass of the carboxylated cellulose fiber.
[0044] The amount of carboxyl groups in carboxylated cellulose can be measured by the following method: 60 ml of a 0.5% by mass slurry (aqueous dispersion) of carboxylated cellulose is prepared, and a 0.1 M aqueous hydrochloric acid solution is added to adjust the pH to 2.5. After that, a 0.05 N aqueous sodium hydroxide solution is added dropwise and the electrical conductivity is measured until the pH reaches 11. The electrical conductivity is calculated using the following formula from the amount of sodium hydroxide (a) consumed in the neutralization stage of the weak acid, where the change in electrical conductivity is gradual.
[0045] Amount of carboxyl groups [mmol / g carboxylated cellulose] = a [ml] x 0.05 / mass of carboxylated cellulose [g] The amount of carboxyl groups in the carboxylated cellulose raw material before fibrillation is usually the same as the amount of carboxyl groups in the carboxylated cellulose fibers after fibrillation.
[0046] One example of a carboxylation (oxidation) method is a method in which a cellulose raw material is oxidized in water using an oxidizing agent in the presence of an N-oxyl compound and a compound selected from the group consisting of bromides, iodides, and mixtures thereof. This oxidation reaction selectively oxidizes the primary hydroxyl group at the C6 position of the glucopyranose ring on the cellulose surface, resulting in the formation of aldehyde groups and carboxyl groups (-COOH) or carboxylate groups (-COO - The concentration of the cellulose raw material during the reaction is not particularly limited, but is preferably 5% by mass or less.
[0047] The N-oxyl compound refers to a compound capable of generating nitroxy radicals. Any compound that can promote the target oxidation reaction can be used as the N-oxyl compound. For example, 2,2,6,6-tetramethylpiperidine-1-oxy radical (TEMPO) and its derivatives (e.g., 4-hydroxyTEMPO) can be mentioned. The amount of the N-oxyl compound used is not particularly limited as long as it is a catalytic amount capable of oxidizing the cellulose raw material. For example, 0.01 mmol to 10 mmol is preferable, 0.01 mmol to 1 mmol is more preferable, and 0.05 mmol to 0.5 mmol is even more preferable for 1 g of bone-dry cellulose raw material. In addition, about 0.1 mmol / L to 4 mmol / L is preferable for the reaction system.
[0048] Bromides are compounds containing bromine, examples of which include alkali metal bromides that can dissociate and ionize in water. Also, iodides are compounds containing iodine, examples of which include alkali metal iodides. The amount of bromide or iodide used can be selected within a range that can promote the oxidation reaction. The total amount of bromide and iodide is, for example, preferably 0.1 mmol to 100 mmol, more preferably 0.1 mmol to 10 mmol, and even more preferably 0.5 mmol to 5 mmol, per 1 g of bone-dry cellulose raw material.
[0049] The oxidizing agent may be a known one, such as halogen, hypohalous acid, halous acid, perhalogen acid or their salts, halogen oxide, or peroxide. Among them, sodium hypochlorite is preferable because it is inexpensive and has a low environmental impact. The appropriate amount of the oxidizing agent to be used is, for example, preferably 0.5 mmol to 500 mmol, more preferably 0.5 mmol to 50 mmol, even more preferably 1 mmol to 25 mmol, and most preferably 3 mmol to 10 mmol, per 1 g of bone-dry cellulose raw material. Also, for example, 1 mol to 40 mol is preferable per 1 mol of the N-oxyl compound.
[0050] The oxidation process of the cellulose raw material can proceed efficiently even under relatively mild conditions. Therefore, the reaction temperature is preferably 4°C to 40°C, or may be room temperature of about 15°C to 30°C. As the reaction proceeds, carboxyl groups are generated in the cellulose chain, and a decrease in the pH of the reaction solution is observed. In order to efficiently proceed with the oxidation reaction, it is preferable to add an alkaline solution such as an aqueous sodium hydroxide solution to maintain the pH of the reaction solution at about 8 to 12, preferably about 10 to 11. The reaction medium is preferably water, because it is easy to handle and does not easily cause side reactions. The reaction time in the oxidation reaction can be appropriately set according to the degree of progress of the oxidation, and is usually 0.5 hours to 6 hours, for example, about 0.5 hours to 4 hours.
[0051] The oxidation reaction may also be carried out in two stages. For example, the oxidized cellulose obtained by filtration after completion of the first-stage reaction can be oxidized again under the same or different reaction conditions, allowing efficient oxidation without reaction inhibition by table salt produced as a by-product in the first-stage reaction.
[0052] Another example of the carboxylation (oxidation) method is a method in which the cellulose raw material is oxidized by contacting it with an ozone-containing gas. This oxidation reaction oxidizes at least the 2- and 6-hydroxyl groups of the glucopyranose ring and decomposes the cellulose chain. The ozone concentration in the ozone-containing gas is 50 g / m 3~250g / m 3 It is preferable that the thickness is 50 g / m 3 ~220g / m 3 It is more preferable that the ozone is added to the cellulose raw material in an amount of 0.1 to 30 parts by mass, and more preferably 5 to 30 parts by mass, based on 100 parts by mass of the solid content of the cellulose raw material. The ozone treatment temperature is preferably 0°C to 50°C, and more preferably 20°C to 50°C. The ozone treatment time is not particularly limited, but is about 1 to 360 minutes, and is preferably about 30 to 360 minutes. When the ozone treatment conditions are within these ranges, the cellulose raw material can be prevented from being excessively oxidized and decomposed, and the yield of oxidized cellulose is good. After the ozone treatment, an oxidizing agent may be used to perform a post-oxidation treatment. The oxidizing agent used in the post-oxidation treatment is not particularly limited, but examples thereof include chlorine compounds such as chlorine dioxide and sodium chlorite, oxygen, hydrogen peroxide, persulfuric acid, and peracetic acid. For example, these oxidizing agents are dissolved in a polar organic solvent such as water or alcohol to prepare an oxidizing agent solution, and the cellulose raw material is immersed in the solution to perform the post-oxidation treatment.
[0053] The amount of carboxyl groups in the carboxylated cellulose raw material can be adjusted by controlling the reaction conditions such as the amount of the oxidizing agent added and the reaction time.
[0054] <Carboxyalkylation of cellulose raw materials> As an example of a chemically modified cellulose raw material, a cellulose raw material to which a carboxyalkyl group such as a carboxymethyl group is ether-bonded (carboxyalkylated cellulose raw material) can be used. Such raw materials may be commercially available, or may be produced by carboxyalkylating the above-mentioned cellulose raw material by a known method. The degree of carboxyalkyl substitution per anhydrous glucose unit of cellulose is preferably 0.01 to 0.50. The upper limit is preferably 0.40 or less. If the degree of carboxyalkyl substitution exceeds 0.50, dissolution in water occurs easily, and the fiber form cannot be maintained in water. In order to obtain the effect of carboxyalkylation, it is necessary to have a certain degree of substitution. For example, if the degree of substitution is less than 0.02, depending on the application, the advantage of introducing a carboxyalkyl group may not be obtained. Therefore, the degree of carboxyalkyl substitution is preferably 0.02 or more, more preferably 0.05 or more, more preferably 0.10 or more, more preferably 0.15 or more, more preferably 0.20 or more, and more preferably 0.25 or more. The degree of carboxyalkyl substitution can be adjusted by controlling the amount of the carboxyalkylating agent to be reacted, the amount of the mercerizing agent, the composition ratio of water to the organic solvent, and the like.
[0055] In this specification, anhydroglucose unit means each anhydroglucose (glucose residue) constituting cellulose. In addition, the degree of carboxyalkyl substitution (also called the degree of etherification) indicates the ratio of hydroxyl groups in the glucose residues constituting cellulose that are substituted with carboxyalkyl ether groups (the number of carboxyalkyl ether groups per glucose residue). The degree of carboxyalkyl substitution is sometimes abbreviated as DS.
[0056] The method for determining the degree of carboxyalkyl substitution is as follows: Weigh out approximately 2.0 g of the sample and place it in a 300 mL Erlenmeyer flask with a stopper. Add 100 mL of nitric acid methanol (a solution of 100 mL of concentrated nitric acid added to 1000 mL of methanol) and shake for 3 hours to convert the salt-type carboxyalkylated cellulose to hydrogen-type carboxyalkylated cellulose. Weigh out 1.5 to 2.0 g of hydrogen-type carboxyalkylated cellulose (absolutely dry) and place it in a 300 mL Erlenmeyer flask with a stopper. Moisten with 15 mL of 80% methanol, add 100 mL of 0.1 N-NaOH, and shake at room temperature for 3 hours. Using phenolphthalein as an indicator, back-titrate the excess NaOH with 0.1 N-H2SO4, and calculate the degree of carboxyalkyl substitution (DS value) using the following formula. A = [(100 × F'-0.1N-H2SO4 (mL) × F) × 0.1] / (bone-dry mass of hydrogen-type carboxyalkylated cellulose (g)) Carboxyalkyl substitution degree = 0.162 x A / (1-0.058 x A) F': Factor of 0.1N-H2SO4 F: Factor of 0.1N NaOH.
[0057] The degree of carboxyalkyl substitution in the carboxyalkylated cellulose feedstock before fibrillation and the degree of carboxyalkyl substitution in the carboxyalkylated cellulose fibers after fibrillation are usually the same.
[0058] As an example of a method for producing a carboxyalkylated cellulose feedstock, the production of a carboxymethylated cellulose feedstock is described below.
[0059] First, the cellulose raw material is mixed with a solvent and a mercerizing agent, and the cellulose raw material is mercerized at a reaction temperature of 0 to 70° C., preferably 10 to 60° C., for a reaction time of 15 minutes to 8 hours, preferably 30 minutes to 7 hours. Next, a carboxymethylating agent is added in an amount of 0.05 to 10.0 times the amount of glucose residue by mole, and carboxymethylation is carried out at a reaction temperature of 30 to 90° C., preferably 40 to 80° C., for a reaction time of 30 minutes to 10 hours, preferably 1 hour to 4 hours.
[0060] As the solvent, 3 to 20 times by mass of water or an organic solvent or a mixture thereof can be used. Examples of the organic solvent include, but are not limited to, alcohols such as methanol, ethanol, N-propyl alcohol, isopropyl alcohol, N-butanol, isobutanol, and tertiary butanol, ketones such as acetone, diethyl ketone, and methyl ethyl ketone, as well as dioxane, diethyl ether, benzene, and dichloromethane. Among these, monohydric alcohols having 1 to 4 carbon atoms are preferred because of their excellent compatibility with water, and monohydric alcohols having 1 to 3 carbon atoms are more preferred. As the mercerizing agent, it is preferred to use 0.5 to 20 times by mole of an alkali metal hydroxide per anhydrous glucose residue of the cellulose raw material, specifically sodium hydroxide or potassium hydroxide. As the carboxymethylating agent, monochloroacetic acid, sodium monochloroacetate, methyl monochloroacetate, ethyl monochloroacetate, and isopropyl monochloroacetate can be mentioned. Among these, monochloroacetic acid or sodium monochloroacetate is preferred in terms of the ease of availability of the raw material. The amount of the carboxymethylating agent used is not particularly limited, but in one embodiment, it is preferably added in the range of 0.5 to 1.5 mol per anhydrous glucose unit of cellulose. The lower limit of the above range is more preferably 0.6 mol or more, even more preferably 0.7 mol or more, and the upper limit is more preferably 1.3 mol or less, even more preferably 1.1 mol or less. The carboxymethylating agent can be added to the reactor as, for example, a 5 to 80 mass % aqueous solution, more preferably 30 to 60 mass %, but is not limited thereto, or can be added in a powder state without dissolving.
[0061] The molar ratio of the mercerizing agent to the carboxymethylating agent (mercerizing agent / carboxymethylating agent) is generally 0.90 to 2.45 when monochloroacetic acid or sodium monochloroacetate is used as the carboxymethylating agent. The reason is that if it is less than 0.90, the carboxymethylation reaction may be insufficient, and unreacted monochloroacetic acid or sodium monochloroacetate may remain and be wasted, and if it exceeds 2.45, a side reaction between the excess mercerizing agent and monochloroacetic acid or sodium monochloroacetate may proceed, resulting in the production of an alkali metal glycolate, which may be uneconomical.
[0062] When carboxymethylating a cellulose raw material, there are usually two methods: one in which both mercerization and carboxymethylation are carried out in a solvent mainly composed of water (aqueous medium method), and the other in which both mercerization and carboxymethylation are carried out in a mixed solvent of water and an organic solvent (solvent method). In the present invention, however, a solvent mainly composed of water may be used in mercerization, and a mixed solvent of an organic solvent and water may be used in carboxymethylation. By doing so, even when the crystallinity of the cellulose is maintained at 50% or more, a carboxymethylated cellulose raw material in which carboxymethyl groups are introduced uniformly rather than locally (i.e., the absolute value of the degree of anionization is small) can be economically obtained.
[0063] A solvent that mainly uses water (a solvent that is mainly made of water) refers to a solvent that contains water at a ratio of more than 50% by mass. The amount of water in the solvent that is mainly made of water is preferably 55% by mass or more, more preferably 60% by mass or more, more preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and even more preferably 95% by mass or more. Particularly preferably, the solvent that is mainly made of water is 100% by mass (i.e., water). The higher the amount of water during mercerization, the more advantageously the carboxymethyl group is introduced more uniformly into the cellulose. As the solvent other than water in the solvent that is mainly made of water (used in a mixture with water), the organic solvent described above can be used. The amount of the organic solvent in the solvent that is mainly made of water is preferably 45% by mass or less, more preferably 40% by mass or less, more preferably 30% by mass or less, more preferably 20% by mass or less, more preferably 10% by mass or less, even more preferably 5% by mass or less, and more preferably 0% by mass.
[0064] It is preferable to add an organic solvent or an aqueous solution of an organic solvent to the reactor simultaneously with the addition of the carboxymethylating agent, or before or immediately after the addition of the carboxymethylating agent, or to appropriately reduce the organic solvent other than water used in the mercerization treatment by reducing pressure or the like to form a mixed solvent of water and an organic solvent, and to proceed with the carboxymethylation reaction in this mixed solvent of water and an organic solvent. The timing of adding or reducing the organic solvent may be any time between the end of the mercerization reaction and immediately after the addition of the carboxymethylating agent, and is not particularly limited, but is preferably within 30 minutes before or after the addition of the carboxymethylating agent, for example.
[0065] The ratio of the organic solvent in the mixed solvent during carboxymethylation is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, even more preferably 45% by mass or more, and particularly preferably 50% by mass or more, based on the total amount of water and organic solvent. The higher the ratio of the organic solvent, the more likely it is that the substitution of carboxymethyl groups will occur uniformly, and the more stable the quality of the carboxymethylated cellulose raw material obtained will be. The upper limit of the ratio of the organic solvent is not limited, and may be, for example, 99% by mass or less. Considering the cost of the organic solvent to be added, it is preferably 90% by mass or less, more preferably 85% by mass or less, even more preferably 80% by mass or less, and even more preferably 70% by mass or less.
[0066] The reaction medium for carboxymethylation (a mixed solvent of water and an organic solvent, etc., not containing cellulose) preferably has a lower proportion of water (in other words, a higher proportion of organic solvent) than the reaction medium for mercerization. By satisfying this range, the crystallinity of the resulting carboxymethylated cellulose raw material is easily maintained, and the fiber of the present invention can be obtained more efficiently. In addition, when the reaction medium for carboxymethylation has a lower proportion of water (a higher proportion of organic solvent) than the reaction medium for mercerization, there is also an advantage that when transferring from the mercerization reaction to the carboxymethylation reaction, a mixed solvent for the carboxymethylation reaction can be formed by a simple means of adding a desired amount of organic solvent to the reaction system after the mercerization reaction is completed.
[0067] In carboxymethylation, the effective utilization rate of the carboxymethylating agent is preferably 15% or more. More preferably, it is 20% or more, further preferably, it is 25% or more, and particularly preferably, it is 30% or more. The effective utilization rate of the carboxymethylating agent refers to the ratio of the carboxymethyl groups introduced into cellulose among the carboxymethyl groups in the carboxymethylating agent. By using a solvent mainly composed of water during mercerization and a mixed solvent of water and an organic solvent during carboxymethylation, it is possible to obtain a carboxymethylated cellulose raw material with a high effective utilization rate of the carboxymethylating agent (i.e., economically without greatly increasing the amount of the carboxymethylating agent used). The upper limit of the effective utilization rate of the carboxymethylating agent is not particularly limited, but in reality, the upper limit is about 80%. The effective utilization rate of the carboxymethylating agent is sometimes abbreviated as AM.
[0068] The effective utilization rate of the carboxymethylating agent is calculated as follows: AM = (DS × moles of cellulose) / moles of carboxymethylating agent DS: Degree of carboxymethyl substitution (measurement method will be described later) Molar number of cellulose: Pulp mass (dry mass when dried at 100°C for 60 minutes) / 162 (162 is the molecular weight per glucose unit of cellulose).
[0069] <Phosphate esterification of cellulose raw materials> As an example of a chemically modified cellulose raw material, a phosphoric acid esterified cellulose raw material can be used. Examples of the esterification method include a method of mixing a powder or an aqueous solution of a compound having a phosphoric acid group with the cellulose raw material, and a method of adding an aqueous solution of a compound having a phosphoric acid group to a slurry of the cellulose raw material. Examples of compounds having a phosphoric acid group include phosphoric acid, sodium dihydrogen phosphate, disodium hydrogen phosphate, trisodium phosphate, sodium phosphite, potassium phosphite, sodium hypophosphite, potassium hypophosphite, sodium pyrophosphate, sodium metaphosphate, potassium dihydrogen phosphate, dipotassium hydrogen phosphate, tripotassium phosphate, potassium pyrophosphate, potassium metaphosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, triammonium phosphate, ammonium pyrophosphate, and ammonium metaphosphate. Phosphate groups can be introduced into the cellulose raw material by using one or more of these in combination. Among these, phosphoric acid, sodium salts of phosphoric acid, potassium salts of phosphoric acid, and ammonium salts of phosphoric acid are preferred from the viewpoints of high efficiency of phosphoric acid group introduction, ease of defibration in the defibration step described below, and ease of industrial application. Sodium dihydrogen phosphate and disodium hydrogen phosphate are particularly preferred. In addition, the compound having a phosphate group is preferably used in the form of an aqueous solution, since this allows the reaction to proceed uniformly and increases the efficiency of the introduction of the phosphate group. The pH of the aqueous solution of the compound having a phosphate group is preferably 7 or less, since this increases the efficiency of the introduction of the phosphate group, but is preferably 3 to 7 in terms of suppressing hydrolysis of the fibers.
[0070] The following method can be mentioned as an example of a method for producing a phosphoric acid esterified cellulose raw material. A compound having a phosphoric acid group is added to a suspension of the cellulose raw material having a solid content concentration of 0.1 to 10% by mass while stirring to introduce a phosphoric acid group into the cellulose. When the cellulose raw material is taken as 100 parts by mass, the amount of the compound having a phosphoric acid group added is preferably 0.2 to 500 parts by mass, more preferably 1 to 400 parts by mass, in terms of the amount of phosphorus element.
[0071] From the viewpoint of suppressing hydrolysis of cellulose after dehydrating the obtained suspension of phosphorylated cellulose raw material, it is preferable to heat treat it at 100 to 170° C. Furthermore, during the heat treatment, it is preferable to heat it at 130° C. or less, preferably 110° C. or less while water is contained, and after removing the water, heat treat it at 100° C. to 170° C.
[0072] The degree of phosphate substitution per glucose unit of the phosphorylated cellulose raw material is preferably 0.001 or more and less than 0.40. The degree of phosphate substitution in the phosphorylated cellulose raw material before fibrillation is usually the same as the degree of phosphate substitution in the phosphorylated cellulose fiber after fibrillation.
[0073] (2) Process B In this step, the chemically modified cellulose is treated with peroxide, which causes the chemically modified cellulose to be oxidatively decomposed, thereby obtaining chemically modified microfibril cellulose fibers that give a low-viscosity aqueous dispersion.
[0074] From the viewpoint of suppressing side reactions, it is preferable to carry out this step by stirring a mixture containing a reaction medium containing water, chemically modified cellulose fiber, and peroxide. The amount of water in the reaction medium is preferably 80 to 100% by mass, more preferably 90 to 100% by mass, and even more preferably 100% by mass. The other component is preferably a water-soluble organic solvent such as alcohol.
[0075] As the peroxide, hydrogen peroxide, peracetic acid, or persulfuric acid can be used, with hydrogen peroxide being preferred.
[0076] The pH of the reaction system is not limited, but from the viewpoint of achieving a low viscosity of the chemically modified microfibril cellulose fiber, the pH of the reaction system is preferably in the neutral to alkaline range, more preferably 7.0 to 14.0, and even more preferably 8.0 to 13.0. In particular, in the case of carboxymethylated microfibril cellulose, if the pH is less than 7.0, the damage to the carboxymethylated cellulose becomes large, and the strength of the obtained chemically modified microfibril cellulose fiber may decrease. In addition, carboxymethylated cellulose has a characteristic that the cellulose is partially swollen by mercerization before the etherification treatment. Therefore, if the pH in this step becomes high, the carboxymethylated cellulose tends to swell more easily from the part swollen by the mercerization, and the entanglement of the three-dimensional network structure becomes stronger, and the effect of reducing the viscosity tends to be difficult to obtain. On the other hand, if the pH exceeds 14.0, the strength of the obtained fibrillated chemically modified cellulose fiber may decrease. Since the reaction system contains hydrogen peroxide, the pH of the reaction system is usually acidic, but it is preferable to appropriately adjust the pH using an alkali. The pH can be measured using a known device. Since the main component of the reaction medium used in the present invention is water, even if it contains an organic solvent, the value measured using a device for measuring the pH of water (such as a pH meter) may be used as the pH of the reaction medium.
[0077] The alkali used is preferably sodium hydroxide. When sodium hydroxide is added, the amount added is preferably 1 to 10% by mass, more preferably 2 to 5% by mass, based on the absolute weight of the chemically modified cellulose fiber.
[0078] The concentration of the chemically modified cellulose fiber in the mixture is preferably 1 to 50% by mass, more preferably 1 to 10% by mass. The amount of hydrogen peroxide added is preferably 0.1 to 100% by mass, more preferably 1 to 80% by mass, based on the bone dry weight of the chemically modified cellulose fiber. The reaction temperature and time can be appropriately set, but it is preferable to carry out the reaction at 60 to 120°C for about 0.5 to 24 hours. There are no limitations on the apparatus used to carry out this step. For example, known apparatus such as an autoclave or a kneader can be used.
[0079] The carboxymethyl groups of the carboxymethyl cellulose used in this step may be in the acid form (-CH2-COOH), the salt form (-CH2-COOM: M is a monovalent metal ion), or a mixture of these forms.
[0080] (3) Process C In step C, the chemically modified cellulose raw material is defibrated or beaten to obtain chemically modified microfibrillated cellulose fibers. The defibration or beating in the fibrillation is preferably carried out in a wet manner (i.e., in the form of a dispersion in which water or the like is used as a dispersion medium) using a refiner such as a disk type, conical type, or cylinder type, a high-speed defibrator, a shear type mixer, a colloid mill, a high-pressure jet disperser, a beater, a PFI mill, a kneader, a disperser, or the like, but is not particularly limited to these devices and may be any device that imparts mechanical defibration force in a wet manner.
[0081] The solid content of the raw material in the dispersion of the chemically modified cellulose raw material to be fibrillated is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, more preferably 1.0% by mass or more, and even more preferably 2.0% by mass or more. The upper limit of the concentration is preferably 50% by mass or less, and even more preferably 30% by mass or less.
[0082] The pH of the aqueous dispersion of the chemically modified cellulose raw material during defibration or mechanical treatment is preferably 7 or more, more preferably 8 or more, and even more preferably 5 or less. The lower limit of the pH is not particularly limited, but is usually 2 or more, preferably 3 or more, and more preferably 3.5 or more. The pH can be adjusted, for example, by adding an acid (e.g., hydrochloric acid) to the aqueous dispersion.
[0083] Before preparing a dispersion for fibrillation, the chemically modified cellulose raw material obtained by the above method may be dried and pulverized in advance. The dry-pulverized chemically modified cellulose raw material may then be dispersed in a dispersion medium and subjected to fibrillation (wet). The apparatus used for dry pulverization of the raw material is not particularly limited, and examples thereof include impact mills such as hammer mills and pin mills, media mills such as ball mills and tower mills, and jet mills.
[0084] As described above, fibrillation is carried out so as to maintain the average fiber diameter at 500 nm or more, preferably at 1 μm or more, and more preferably at 10 μm or more. The upper limit of the average fiber diameter is preferably 60 μm or less, more preferably 40 μm or less, even more preferably 30 μm or less, and even more preferably 20 μm or less. By carrying out moderate fibrillation to such an extent that the average fiber diameter falls within this range, the cellulose fiber exhibits higher water retention than undefibrated cellulose fibers, and even in small amounts, a higher strength imparting effect and a higher yield improvement effect can be obtained compared to cellulose nanofibers that have been defibrated more finely. EXAMPLES
[0085] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited thereto. Unless otherwise specified, parts and % indicate parts by mass and % by mass.
[0086] <Procedure for measuring the physical properties of chemically modified microfibril cellulose fibers> (Chemical Properties) Carboxyl (COOH) group amount: 60 ml of a 0.5% by mass aqueous dispersion of the sample was prepared, and a 0.1 M aqueous hydrochloric acid solution was added to adjust the pH to 2.5. Then, a 0.05 N aqueous sodium hydroxide solution was added dropwise, and the electrical conductivity was measured until the pH reached 11. The amount of carboxyl (COOH) group was calculated using the following formula from the amount of sodium hydroxide (a) consumed in the neutralization stage of the weak acid, where the change in electrical conductivity is gradual: Amount of carboxyl groups [mmol / g carboxylated cellulose] = a [ml] × 0.05 / mass of carboxylated cellulose [g]. Degree of substitution: Approximately 2.0 g of sample was weighed out and placed in a 300 mL Erlenmeyer flask with a stopper. 100 mL of nitric acid methanol (a solution of 100 mL of concentrated nitric acid added to 1000 mL of methanol) was added and shaken for 3 hours to convert the salt-type carboxyl group to the acid-type. 1.5 to 2.0 g of the obtained acid-type sample (absolutely dry) was weighed out and placed in a 300 mL Erlenmeyer flask with a stopper. The sample was moistened with 15 mL of 80% methanol, 100 mL of 0.1 N-NaOH was added, and the mixture was shaken at room temperature for 3 hours. Excess NaOH was back-titrated with 0.1 N-H2SO4 using phenolphthalein as an indicator, and the degree of substitution (DS value) was calculated by the following formula.
[0087] A = [(100 x F'-0.1N-H2SO4 (mL) x F) x 0.1] / (absolute dry mass of acid sample (g)) Substitution degree=0.162×A / (1-0.058×A) F': Factor of 0.1N-H2SO4 F: Factor of 0.1N NaOH.
[0088] Crystallinity of cellulose type I: A sample is placed in a glass cell and measured using an X-ray diffraction measuring device (e.g., LabX XRD-6000, manufactured by Shimadzu Corporation). The crystallinity is calculated using the method of Segal et al. For example, the diffraction intensity at 2θ=10° to 30° in the X-ray diffraction pattern is used as the baseline, and the crystallinity is calculated from the diffraction intensity of the 002 plane at 2θ=22.6° and the diffraction intensity of the amorphous part at 2θ=18.5° using the following formula. Xc = (I 002C -Ia) / I 002C ×100 Xc: Crystallinity of cellulose type I (%) I 002C : Diffraction intensity of 002 plane at 2θ=22.6° Ia: 2θ=18.5°, diffraction intensity of amorphous part The samples for measuring the crystallinity were freeze-dried samples prepared in the same manner as in the items (1) to (9) in the measurement of the specific surface area described later, and molded into tablets.
[0089] - Method for measuring the degree of anionization: Chemically modified microfibril cellulose fibers were dispersed in water to prepare an aqueous dispersion with a solid content of 10 g / L, which was then stirred at 1000 rpm for 10 minutes or more using a magnetic stirrer. The aqueous dispersion thus obtained was diluted to 0.1 g / L, and 10 ml of the solution was taken and titrated with 1 / 1000 normality diallyldimethylammonium chloride (DADMAC) using a streaming current detector (Mutek Particle Charge Detector 03). The amount of DADMAC added until the streaming current became zero was used to calculate the degree of anionization according to the following formula: q=(V×c) / m q: degree of anionization (meq / g) V: Amount of DADMAC added until the streaming current becomes zero (L) c: DADMAC concentration (meq / L) m: mass (g) of chemically modified microfibrillated cellulose fibers in the measurement sample.
[0090] (Fiber properties) Average fiber width and average fiber length: The aqueous dispersion was diluted to a solid content concentration of 0.25% by mass and passed through a fractionator to determine the length-weighted fiber width and length-weighted average fiber length (n=2).
[0091] Aspect ratio: Calculated from the measured fiber width and fiber length using the following formula. Aspect ratio = average fiber length / average fiber diameter
[0092] Specific surface area: (1) Approximately 2% aqueous dispersion of chemically modified microfibril cellulose fiber was placed in a centrifuge container so that the solid content was approximately 0.1 g, and 100 ml of ethanol was added. (2) A stirrer was added and the mixture was stirred at 500 rpm for at least 30 minutes. (3) The stirrer was removed, and the chemically modified microfibril cellulose fibers were sedimented in a centrifuge at 7,000 G for 30 minutes at 30°C. (4) The supernatant was removed while trying to avoid removing as much of the chemically modified microfibril cellulose fibers as possible. (5) 100 ml of ethanol was added, a stir bar was added, and the mixture was stirred under the conditions of (2), centrifuged under the conditions of (3), and the supernatant was removed under the conditions of (4). This process was repeated three times. (6) The solvent in (5) was changed from ethanol to t-butanol, and the stirring, centrifugation, and removal of the supernatant were repeated three times in the same manner as in (5) at room temperature above the melting point of t-butanol. (7) After the final solvent removal, 30 ml of t-butanol was added and mixed gently, then transferred to a recovery flask and frozen in an ice bath. (8) Cool in the freezer for at least 30 minutes. (9) The mixture was attached to a freeze-dryer and freeze-dried for 3 days. (10) BET measurements were performed (pretreatment conditions: under nitrogen flow, 105°C, 2 hours, relative pressure 0.01 to 0.30, sample amount approximately 30 mg). Water retention capacity: 40 mL of an aqueous dispersion of chemically modified microfibril cellulose fiber with a solids concentration of 0.3% by mass was prepared. The mass of the aqueous dispersion at this time was designated A. Next, the entire amount of the aqueous dispersion was centrifuged at 30°C and 25,000G for 30 minutes in a high-speed refrigerated centrifuge to separate the aqueous phase and sediment. The mass of the sediment at this time was designated B. The aqueous phase was placed in an aluminum cup and dried overnight at 105°C to remove the water, and the mass of the solids in the aqueous phase was measured. The mass of the solids in this aqueous phase was designated C. The water retention capacity was calculated using the following formula.
[0093] Electrical conductivity: 200 g of an aqueous dispersion of chemically modified microfibril cellulose fiber with a solid content of 1.0% by mass was prepared and thoroughly stirred. Then, the electrical conductivity was measured using an electrical conductivity meter (HORIBA ES-71).
[0094] pH: The solids concentration of the chemically modified microfibril cellulose fiber after the fibrillation treatment was adjusted to 1.0% by mass, and the pH was measured.
[0095] [Example 1] (1) Step A <TEMPO oxidation of pulp> 5.00 g (bone-dry) of bleached unbeaten kraft pulp derived from coniferous trees (NBKP, Nippon Paper Industries Co., Ltd., brightness 85%) was added to 500 ml of an aqueous solution containing 39 mg (0.05 mmol per 1 g of bone-dry cellulose) of TEMPO (Sigma Aldrich) and 514 mg (1.0 mmol per 1 g of bone-dry cellulose) of sodium bromide, and the mixture was stirred until the pulp was uniformly dispersed. An aqueous solution of sodium hypochlorite was added to the reaction system so that the sodium hypochlorite concentration was 5.5 mmol / g, and the oxidation reaction was started at room temperature. The pH of the system decreased during the reaction, but 3 M aqueous sodium hydroxide was added successively to adjust the pH to 10. The reaction was terminated when the sodium hypochlorite was consumed and the pH of the system no longer changed. After the reaction, the mixture was adjusted to pH 2 by adding hydrochloric acid, filtered through a glass filter, and the pulp was separated. The separated pulp was thoroughly washed with water to obtain TEMPO-oxidized pulp. The pulp yield was 90%, the time required for the oxidation reaction was 90 minutes, the amount of carboxyl groups was 1.54 mmol / g, and the pH was 4.5. An aqueous dispersion of the obtained TEMPO oxidized pulp with a solid content concentration of 2.0 mass % was prepared, and a 5% NaOH aqueous solution and sodium hydrogen carbonate were added to adjust the pH to 7.5. (2) Step B <Treatment with hydrogen peroxide> To the resulting TEMPO oxidized pulp aqueous dispersion, 0.6 g of 5% sodium hydroxide solution and 0.14 g of 35% hydrogen peroxide solution were added per gram of bone-dry TEMPO oxidized pulp, and the mixture was thoroughly stirred. After stirring, the mixture was allowed to stand for 30 minutes to obtain peroxide-treated TEMPO oxidized pulp. (3) Step C <Fibrillation> The obtained hydrogen peroxide-treated TEMPO oxidized pulp was treated for 10 minutes using Top Finer (Aikawa Iron Works Co., Ltd.) to prepare oxidized cellulose microfibrils (TEMPO oxidized MFC). The physical properties of the obtained oxidized cellulose microfibrils are shown in Table 1. The methods for measuring each physical property were as described above.
[0096] [Example 2] (1) Step A <Carboxymethylation of pulp> In a twin-shaft kneader adjusted to a rotation speed of 100 rpm, 75 parts of water and 22 parts of sodium hydroxide dissolved in 100 parts of water were added, and 100 parts (dry mass when dried at 100 ° C for 60 minutes) of bleached unbeaten kraft pulp derived from hardwood (LBKP, manufactured by Nippon Paper Industries Co., Ltd.) were added. These were stirred and mixed for 90 minutes at 30 ° C to prepare a mercerized cellulose-based raw material. Further, while stirring, 200 parts of isopropanol (IPA) and 60 parts of sodium monochloroacetate were added, and after stirring for 30 minutes, the temperature was raised to 70 ° C and a carboxymethylation reaction was carried out for 90 minutes. The concentration of IPA in the reaction medium during the carboxymethylation reaction was 37%. After the reaction was completed, the mixture was neutralized with acetic acid to a pH of about 7, and a carboxymethylated pulp (sodium salt) with a carboxymethylation degree of 0.36, a carboxyl group amount of 2.11 mmol / g, and a crystallinity of cellulose I type was obtained. An aqueous dispersion of the obtained carboxymethylated pulp having a solids concentration of 2.0% by mass was prepared, and a 5% aqueous NaOH solution was added to adjust the pH to 7.5. (2) Step B <Treatment with hydrogen peroxide> To the resulting carboxymethylated pulp aqueous dispersion, 0.6 g of a 5% aqueous sodium hydroxide solution and 0.14 g of a 35% aqueous hydrogen peroxide solution were added per gram of bone-dry carboxymethylated pulp, and the mixture was thoroughly stirred. After stirring, the mixture was allowed to stand for 30 minutes to obtain a peroxide-treated carboxymethylated pulp. (3) Step C <Fibrillation> The obtained hydrogen peroxide-treated carboxymethylated pulp was treated for 10 minutes using Topfiner (manufactured by Aikawa Iron Works Co., Ltd.) to prepare carboxymethylated cellulose microfibrils (carboxymethylated MFC). The physical properties of the obtained carboxymethylated cellulose microfibrils are shown in Table 1. The methods for measuring each physical property were as described above.
[0097] [Comparative Example 1] Except for not carrying out the treatment with hydrogen peroxide, it was prepared in the same manner as in Example 1. The physical properties of the obtained oxidized cellulose microfibrils are shown in Table 1. The methods for measuring each physical property were as described above.
[0098] [Comparative Example 2] Except for not carrying out the treatment with hydrogen peroxide, the preparation was carried out in the same manner as in Example 2. The physical properties of the obtained carboxymethylated cellulose microfibrils are shown in Table 1. The methods for measuring the respective physical properties are as described above.
[0099] [Table 1]
[0100] As shown in Table 1, hydrogen peroxide treatment enabled the production of a low-viscosity aqueous dispersion of chemically modified microfibril cellulose fibers.
Claims
1. A method for producing chemically modified microfibril cellulose fibers, comprising the following steps (A) to (C): (A) Preparing chemically modified cellulose (B) treating the chemically modified cellulose with peroxide in a reaction system having a pH of 8.0 to 13.0 (C) A step of defibrating the chemically modified cellulose after the treatment to obtain chemically modified microfibril cellulose fibers having an average fiber diameter of 1 μm or more and an average fiber length of 200 μm or more.
2. The method according to claim 1, wherein the amount of the peroxide added is 0.1 to 100% by mass based on the bone dry weight of the chemically modified cellulose.
3. The method according to any one of claims 1 to 2, wherein the step (B) is carried out in a mixture containing a peroxide, a chemically modified cellulose, and a medium, and the concentration of the chemically modified cellulose in the mixture is 0.1 to 50% by mass.
4. The method according to any one of claims 1 to 3, wherein the chemically modified cellulose is a cellulose having a carboxyl group.
5. The method according to any one of claims 1 to 3, wherein the chemically modified cellulose is carboxymethylated cellulose.
Citation Information
Patent Citations
Fine fibrous cellulose-containing material
JP2017057390A
Method for producing anion-modified cellulose nanofibers
JP2017071700A
Rubber composition and process for producing same
JP2019172858A
Method for producing master batch, master batch obtained by said production method, rubber composition for tire, and pneumatic tire
WO2016136453A1
Carboxymethylated cellulose nanofibers and production method therefor
WO2018194049A1