Method for producing ferritic stainless steel powder and ferritic stainless steel powder

By adding La and Zr separately to molten ferritic stainless steel after melting, the method stabilizes production and enhances oxidation resistance, addressing yield loss and embrittlement issues in existing methods.

JP7574557B2Active Publication Date: 2024-10-29PROTERIAL LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2020117110
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-07
Publication Date
2024-10-29
Estimated Expiration
2040-07-07

AI Technical Summary

Technical Problem

Existing methods for producing ferritic stainless steel powder containing La and Zr result in reduced yield due to the formation of La and Zr oxides during atomization, which affects the oxidation resistance and stability of the final product.

Method used

The method involves adding La and Zr separately to the molten metal after the melting process, minimizing contact with refractories to maintain high addition yields and ensuring a Zr-enriched phase at the grain boundaries, which enhances oxidation resistance.

Benefits of technology

Stable production of ferritic stainless steel powder with improved oxidation resistance and reduced embrittlement, maintaining a Zr-enriched phase at grain boundaries to prevent Cr evaporation and improve high-temperature performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574557000003
    Figure 0007574557000003
  • Figure 0007574557000001
    Figure 0007574557000001
  • Figure 0007574557000002
    Figure 0007574557000002
Patent Text Reader

Abstract

To provide a method for producing ferritic stainless steel powder containing La and Zr, and ferritic stainless steel powder having excellent oxidation resistance.SOLUTION: A method for producing ferritic stainless steel powder includes: a dissolution step of dissolving an alloy base material, and obtaining molten metal of ferritic stainless steel powder containing, by mass%, C:0.1% or less, Al:0.2% or less, Si:0.2% or less, Mn:1.0% or less, Cr:26.0% or less, Ni:1.0% or less, Cu:4.0% or less, and W:3.0% or less; an addition step of adding an La raw material and a Zr material to the molten metal; and a pulverization step of obtaining ferritic stainless steel powder from the molten metal after the addition step. Ferritic stainless steel powder can be obtained by the above production method.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing ferritic stainless steel powder and to ferritic stainless steel powder. [Background technology]

[0002] Ferritic stainless steel, known as an alloy with excellent oxidation resistance, also has properties such as good electrical conductivity and a low coefficient of thermal expansion. For this reason, it is used, for example, in components such as separators, interconnectors, and current collectors for solid oxide fuel cells. The excellent oxidation resistance of this ferritic stainless steel is generally achieved by the formation of a dense oxide film mainly composed of Cr2O3 at temperatures of about 600°C to 900°C. However, at the same time, Cr evaporates from the Cr2O3 surface oxide layer. Therefore, when used at high temperatures for a long period of time, Cr decreases and oxidation resistance tends to decrease.

[0003] The applicant of the present application has proposed in Patent Documents 1 and 2 ferritic stainless steels that contain La and Zr to have better oxidation resistance, with the aim of improving the oxidation resistance even when used at high temperatures for long periods of time. Ferritic stainless steels that contain La and Zr form spinel oxides on the outside (surface side) of the Cr2O3 oxide layer at temperatures of about 600°C to 900°C. This spinel oxide layer has the effect of preventing Cr evaporation, so that excellent oxidation resistance can be achieved.

[0004] Ferritic stainless steel is used in various shapes, such as nets, thin wires, thin plates, rods, and porous bodies, depending on the application. In particular, metal porous bodies have characteristics such as air permeability and a large surface area in addition to the above-mentioned characteristics of ferritic stainless steel, and are therefore suitably used, for example, as air electrodes in solid oxide fuel cells. On the other hand, metal porous bodies have a larger surface area than other shapes and are prone to Cr evaporation, so it is effective to apply ferritic stainless steel containing La and Zr, as described in Patent Documents 1 and 2, to suppress Cr evaporation. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2007-16297 A [Patent Document 2] International Publication No. 2012 / 144600 Summary of the Invention [Problem to be solved by the invention]

[0006] A common method for producing a metal porous body with uniform pore size and distribution is to sinter spherical metal powder. This spherical metal powder is generally produced by the atomization method. The atomization method is a method in which molten metal in a tundish with a pouring nozzle on the bottom is made to flow down from the pouring nozzle on the bottom of the tundish, and the molten metal flow is crushed by spraying high-pressure water or high-pressure gas flow and solidified into droplets to obtain powder. The molten metal is obtained by melting in an induction heating furnace and pouring it into a tundish, or by melting it in the tundish. However, since the crucible of the induction heating furnace and the tundish and nozzle of the atomizer are made of refractory materials, contact between the molten metal and the refractory material is unavoidable. When attempting to produce the ferritic stainless steel powder containing La and Zr described in Patent Document 1 and Patent Document 2, the molten metal containing La and Zr reduces the refractory material, and La oxide and Zr oxide are generated. Therefore, there is a possibility that these La oxides and Zr oxides are removed from the molten metal during atomization, and the yield of La and Zr added in the metal powder obtained after atomization decreases. The above has been a bottleneck in the production of ferritic stainless steel powder containing the desired La and Zr. Patent Documents 1 and 2 do not consider the problems that arise during the production of these powders, and there is still room for improvement.

[0007] Based on the above, an object of the present invention is to provide a manufacturing method by which ferritic stainless steel powder containing La and Zr can be stably obtained, and a ferritic stainless steel powder having excellent oxidation resistance that can be obtained by the manufacturing method. [Means for solving the problem]

[0008] For the above-mentioned purpose, the inventors have investigated methods of adding Zr and La, and have found that ferritic stainless steel powder that ensures the desired Zr and La addition yields can be produced by separately adding Zr-based raw materials and La-based raw materials to the molten metal after the process of melting the raw material in atomization. Furthermore, it was discovered that Zr is concentrated at the grain boundaries in the metal structure of the ferritic stainless steel powder, which provides a preferable mode for suppressing embrittlement of the porous body during the manufacturing process of a metal porous body using the ferritic stainless steel powder as a raw material.

[0009] That is, one aspect of the present invention is a melting process for melting an alloy material to obtain a molten metal of a ferritic stainless steel containing, by mass%, C: 0.1% or less, Al: 0.2% or less, Si: 0.2% or less, Mn: 1.0% or less, Cr: 26.0% or less, Ni: 1.0% or less, Cu: 4.0% or less, and W: 3.0% or less; an adding step of adding a La raw material and a Zr raw material to the molten metal; and a powdering step for obtaining ferritic stainless steel powder from the molten metal after the adding step. This is a method for producing ferritic stainless steel powder, in which the ferritic stainless steel powder obtained by the powdering step contains, by mass, C: more than 0% and not more than 0.1%, Al: 0.2% or less, Si: 0.2% or less, Mn: 0.1% or more and 1.0% or less, Cr: 20.0% or more and 26.0% or less, Ni: 0.1% or more and 1.0% or less, Cu: 0.3% or more and 4.0% or less, W: 1.0% or more and 3.0% or less, La: 0.02% or more and 0.12% or less, Zr: 0.01% or more and 0.5% or less, La + Zr: 0.03% or more and 0.52% or less, with the remainder being Fe and unavoidable impurities.

[0010] In addition, another aspect of the present invention is a ferritic stainless steel powder containing, by mass%, more than 0% and 0.1% or less of C, 0.2% or less of Al, 0.2% or less of Si, 0.1% or more and 1.0% or less of Mn, 20.0% or more and 26.0% or less of Cr, 0.1% or more and 1.0% or less of Ni, 0.3% or more and 4.0% or less of Cu, 1.0% or more and 3.0% or less of W, 0.02% or more and 0.12% or less of La, 0.01% or more and 0.5% or less of Zr, and 0.03% or more and 0.52% or less of La + Zr, with the balance being Fe and unavoidable impurities, and having an average powder diameter of 100 μm or less. The metal structure of the ferritic stainless steel powder has a Zr-enriched phase at its grain boundaries, and it is a ferritic stainless steel powder.

Advantages of the Invention

[0011] According to the present invention, a ferritic stainless steel powder containing La and Zr can be stably obtained. Further, a ferritic stainless steel powder excellent in oxidation resistance can be obtained thereby.

Brief Description of the Drawings

[0012] [Figure 1] (a) is a backscattered electron image of a cross-section of the metal structure of the ferritic stainless steel powder in the present invention. (b) is the result of surface analysis of Zr by an electron beam microanalyzer. (c) is a color bar corresponding to the result of surface analysis of Zr.

Embodiments for Carrying Out the Invention

[0013] First, in the ferritic stainless steel powder according to the present invention (hereinafter, also simply referred to as "stainless steel powder"), the reasons for prescribing the content of each element will be described. The content of each element is expressed as mass%. <C: More than 0% and 0.1% or less> C is an element that combines with Cr in a member made of stainless steel powder, reducing the amount of Cr in the base material and lowering the oxidation resistance. Therefore, in order to improve the oxidation resistance, it is effective to make C as low as possible, and in the present invention, it is limited to the range of 0.1% or less. The preferable upper limit of C is 0.04%. However, in the case of the ferritic stainless steel of the present invention containing Zr, in the sintering process of forming a sintered body using the stainless steel powder of the present invention, when C forms Zr carbide (Zr carbonitride when N also exists), if C is too low, even if Zr that does not form Zr carbide dissolves in the ferrite matrix, excess Zr may remain. The excess Zr reacts with Fe to form and precipitate intermetallic compounds such as Laves phase, reducing the oxidation resistance. Therefore, C needs to exceed 0%. The preferable lower limit of C is 0.001%.

[0014] <Al: 0.2% or less> Al forms Al2O3 in the form of particles and needles in the metal structure near the Cr2O3 oxide layer at a temperature of about 600°C to 900°C in a member made of stainless steel powder. This makes the outward diffusion of Cr non-uniform and hinders the formation of a stable Cr2O3 oxide layer, thereby deteriorating the oxidation resistance. Therefore, in the present invention, it is limited to the range of 0.2% or less (including 0%).

[0015] <Si: 0.2% or less> Si forms a SiO2 film near the interface between the chromia-based oxide layer and the base material at a temperature of about 600°C to 900°C in a member made of stainless steel powder. Similar to the formation of the above-mentioned Al2O3, the SiO2 film hinders the formation of a stable Cr2O3 oxide layer, thereby deteriorating the oxidation resistance. Therefore, in the present invention, it is limited to the range of 0.2% or less (including 0%).

[0016] <Mn: 0.1% or more and 1.0% or less> Mn is an element that forms spinel-type oxides together with Cr at a temperature of about 600 °C to 900 °C in a member manufactured using stainless steel powder. The spinel-type oxide layer containing Mn is formed on the outer side (surface side) of the Cr2O3 oxide layer. This spinel-type oxide layer has a protective effect of preventing Cr from evaporating from the Cr2O3 surface oxide layer, and suppresses the decrease in oxidation resistance due to the decrease in the Cr amount of the base material. Therefore, at least 0.1% is required. On the other hand, if added excessively, the Mn content in the spinel-type oxide layer increases, the oxide film thickens, and the oxidation resistance may deteriorate. Therefore, the upper limit of Mn is 1.0%. The preferable upper limit of Mn is 0.5%.

[0017] <Cr: 20.0% or more and 26.0% or less> Cr is an element necessary to realize excellent oxidation resistance by forming a dense Cr2O3 oxide layer at a temperature of about 600 °C to 900 °C in a member manufactured using stainless steel powder in order to maintain the ferrite structure of the base material. At least 20.0% is required to obtain good oxidation resistance and electrical conductivity. The preferable lower limit of Cr is 22.0%, and the more preferable lower limit of Cr is 23.0%. However, excessive addition not only has little effect on improving oxidation resistance but also causes deterioration of mechanical properties, so the upper limit is limited to 26.0%. The preferable upper limit of Cr is 25.0%.

[0018] <Ni: 0.1% or more and 1.0% or less> In the case of a member manufactured using stainless steel powder, adding a small amount of Ni is effective in improving toughness. Therefore, at least 0.1% is required. On the other hand, Ni is an austenite-forming element, and when it is contained in excess, it tends to form a two-phase structure of ferrite-austenite and increases the coefficient of thermal expansion. Also, when manufacturing a ferritic stainless steel such as the present invention, for example, when using recycled materials as melting materials, it may be inevitably mixed in. When the Ni content becomes too high, in the case of a member for a solid oxide fuel cell where ferritic stainless steel is preferably used, there is a concern that the bonding property may decrease or the ceramic parts may be damaged due to the difference in thermal expansion with ceramic parts, so a large amount of addition or mixing is not preferable. Therefore, in the present invention, the upper limit of Ni is set to 1.0%.

[0019] <Cu: 0.3% or more and 4.0% or less> In the case of a member manufactured using stainless steel powder, Cu has the effect of further suppressing the evaporation of Cr from the Cr2O3 oxide layer by densifying the spinel-type oxide containing Mn and Cr formed on the Cr2O3 oxide layer at a temperature of about 600°C to 900°C. Therefore, at least 0.3% is required. On the other hand, if Cu is added in excess, a Cu phase may precipitate in the matrix, making it difficult to form a dense Cr2O3 oxide layer at the location of the Cu phase, and there is a possibility that the oxidation resistance may decrease or the ferrite structure may become unstable. Therefore, the upper limit of Cu is set to 4.0%. The preferable upper limit of Cu is 2.0% or less.

[0020] <La: 0.02% or more and 0.12% or less> When a small amount of La is added, in the case of a member manufactured using stainless steel powder, it exhibits good oxidation resistance by densifying the oxide film mainly containing Cr or improving the adhesion at a temperature of about 600°C to 900°C, and the addition is indispensable. If the addition of La is less than 0.02%, the effect of improving the denseness and adhesion of the oxide film is small. On the other hand, if more than 0.12% is added, there is a risk of an increase in inclusions such as oxides containing La and embrittlement. Therefore, La is 0.02% or more and 0.12% or less.

[0021] <Zr: 0.01% or more and 0.5% or less> Zr also has the effect of significantly improving oxidation resistance in members manufactured using stainless steel powder by adding a small amount, by densifying the oxide film or improving the adhesion of the oxide film at a temperature of about 600°C to 900°C. If Zr is less than 0.01%, the effect of improving the denseness and adhesion of the oxide film is small. On the other hand, if more than 0.5% is added, a large number of coarse compounds containing Zr are formed, which may cause embrittlement. Also, since it reacts with Fe to form and precipitate intermetallic compounds such as Laves phase and reduces oxidation resistance, Zr is set to 0.01% or more and 0.5% or less.

[0022] <La + Zr: 0.03% or more and 0.52% or less> In the present invention, for the aforementioned La and Zr, since both have the effect of improving excellent oxidation resistance at high temperatures, composite addition is preferable. In that case, if the total of La and Zr is less than 0.03%, the effect on improving oxidation resistance is small. On the other hand, if more than 0.52% is added, embrittlement is a concern due to the formation of a large number of compounds containing La or Zr. Therefore, the total of La and Zr is set to 0.03% or more and 0.52% or less.

[0023] <W: 1.0% or more and 3.0% or less> Generally, Mo is known as an element that exhibits the same effect as W for solid solution strengthening and the like. However, compared with Mo, when oxidized at a temperature of about 600°C to 900°C, W has the effect of moderately suppressing the outward diffusion of Cr in the base material of ferritic stainless steel, suppressing the excessive growth of a dense Cr2O3 oxide layer, and is effective for maintaining a stable protective action for a long time. Therefore, in the present invention, W is added alone as essential. By adding W, the outward diffusion of Cr in the base material of ferritic stainless steel can be moderately suppressed, thereby suppressing the decrease in the Cr content of the base material after the formation of the Cr2O3 oxide layer. As a result, a dense Cr2O3 oxide layer can be maintained for a long time, preventing abnormal oxidation of the alloy and maintaining excellent oxidation resistance for a long time. To exert this effect, at least 1.0% is required. However, if W is added in excess of 3.0%, it will become brittle, so the upper limit of W is 3.0.

[0024] In the present invention, other than the elements described above, Fe and inevitable impurities are used. Hereinafter, typical impurities and their preferable upper limits are described below. Since they are impurity elements, the preferable lower limit of each element is 0%. <N: 0.05% or less> N forms nitride-based inclusions with Zr and Cr, which greatly contribute to the improvement of oxidation resistance, reducing the Zr and Cr concentrations in the matrix phase and thus reducing the oxidation resistance. Therefore, it is preferably 0.05% or less, and more preferably 0.02% or less. <O: 0.03% or less> O forms oxide-based inclusions with Zr and La, which greatly contribute to the improvement of oxidation resistance, reducing the Zr and La concentrations in the matrix phase and thus reducing the oxidation resistance. Therefore, it is preferably 0.03% or less, and more preferably 0.02 or less. <Mo: 0.2% or less> Since Mo reduces the oxidation resistance, it is not added actively. However, a content of 0.2% or less does not significantly affect the oxidation characteristics, so it is limited to 0.2% or less. <S: 0.015% or less> S forms sulfide-based inclusions with rare earth elements, reducing the amount of La, an effective rare earth element that has an effect on oxidation resistance, and not only reducing the oxidation resistance but also deteriorating the surface finish. Therefore, it is preferably 0.015% or less. More preferably, it is 0.008% or less. <P: 0.04% or less> P is an element that is more easily oxidized than Cr which forms the oxide film, and it deteriorates the oxidation resistance, so it is preferably limited to 0.04% or less. Preferably, it is 0.03% or less, more preferably 0.02% or less, and even more preferably 0.01% or less. <B: 0.003% or less> B increases the growth rate of the oxide film at a high temperature of about 700 °C or higher and deteriorates the oxidation resistance. Therefore, B is preferably limited to 0.003% or less, and it is better to reduce it to 0% as much as possible. The preferable upper limit is 0.002% or less, and more preferably less than 0.001%. <H: 0.0003% or less> When H is excessively present in the ferrite matrix of ferritic stainless steel, it tends to gather at defect sites such as grain boundaries and may cause hydrogen embrittlement, resulting in cracks during manufacturing. Therefore, it is preferably limited to 0.0003% or less. More preferably, it is 0.0002% or less.

[0025] Next, a method for manufacturing the ferritic stainless steel powder of the present invention will be described. The ferritic stainless steel powder of the present invention can be used for members that require oxidation resistance and electrical conductivity, and is preferably used for battery members such as current collector members and separators. When used as a member, it can be processed into shapes such as powder, powder sintered body, and powder sintered porous body for use. <Melting step> In the manufacturing method of this embodiment, first, an alloy material is melted to obtain a molten metal of ferritic stainless steel containing C: 0.1% or less, Al: 0.2% or less, Si: 0.2% or less, Mn: 1.0% or less, Cr: 26.0% or less, Ni: 1.0% or less, Cu: 4.0% or less, and W: 3.0% or less. The alloy material may be scrap, cuttings, metal ingots, metal foils, metal plates, metal powders, or cast bodies obtained by melting and casting them. There is no particular limitation on the method of melting the alloy material, and the molten metal can be obtained by using a conventional method in the manufacture of alloys. For example, the molten metal melted in advance in an induction heating furnace may be poured into a tundish, or the alloy material may be melted in the tundish by high-frequency induction heating. The components of this molten metal are preferably the components of the powder finally obtained, except for La and Zr, but since the components can be adjusted in the addition process described later, it is sufficient that the components are within the range not exceeding the upper limit of each component described above. For example, when only La and Zr are added in the addition step, the components of the molten metal are preferably, in mass%, C: over 0% and not more than 0.1%, Al: 0.2% or less, Si: 0.2% or less, Mn: 0.1% or more and 1.0% or less, Cr: 20.0% or more and 26.0% or less, Ni: 0.1% or more and 1.0% or less, Cu: 0.3% or more and 4.0% or less, W: 1.0% or more and 3.0% or less, with the balance being Fe and unavoidable impurities. In addition, since it is possible to use stainless steel scrap containing La and Zr as the alloy material, La and Zr may be contained in the molten metal. In addition, the total amount of La+Zr may be 0.6% or less by using a recycled stainless steel material equivalent to the present invention. However, in the present invention, it is important to provide an "addition process" in which La and Zr are added again after melting the alloy material (i.e., after the melting process) in order to adjust the La and Zr contents to the target values ​​at the stage of the stainless steel powder after the pulverization process.

[0026] <Addition process> Next, an adding step is carried out in which the La raw material and the Zr raw material are added to the molten metal obtained in the melting step. In the present invention, the La raw material and the Zr raw material are not added to the alloy material during the melting step, or, if they are added, they are added to the molten metal after the melting step (i.e., immediately before the pulverization step described below). In order to maintain the addition yield of La and Zr in the powder after pulverization, it is considered to shorten the time that the molten metal containing La and Zr before pulverization is in contact with a refractory such as a tundish, suppress the formation of La oxides and Zr oxides, that is, to pulverize the molten metal "immediately". However, in order to melt the alloy material and make it in a state where it can be pulverized, in addition to the time until the melting is completed, it also takes time to adjust the molten metal after the melting is completed to a temperature suitable for flowing down. Therefore, in the present invention, after the melting of the alloy material is completed, and preferably after the molten metal after the melting is completed is adjusted to the flowing down temperature, the La raw material and the Zr raw material are added and adjusted to their respective target values, thereby making it possible to improve the addition yield of La and Zr. The amounts of La and Zr added are preferably such that the powder after the pulverization step contains La: 0.06% to 0.4%, Zr: 0.01% to 0.5%, and La+Zr: 0.07% to 0.9%. In this addition step, the raw materials are added in an inert gas atmosphere to suppress oxidation of La and Zr.

[0027] The La raw material and the Zr raw material can be selected from La metal, Zr metal, La-containing alloy, Zr-containing alloy, and La-Zr-containing alloy. Here, the La-containing alloy refers to an alloy containing 20% ​​or more of La by mass%, and the Zr-containing alloy refers to an alloy containing 20% ​​or more of Zr by mass%. The added raw material can be in any form, such as powder, wire, plate, crushed, or block. In addition, the La-containing alloy, the Zr-containing alloy, and the La-Zr-containing alloy may contain at least one of C, Al, Si, Mn, Cr, Ni, Cu, W, and Fe. This allows the content of elements other than La and Zr to be adjusted (added).

[0028] <Powdering process> In this embodiment, after this addition step, stirring is performed and the process proceeds to the pulverization step. In the pulverization step, the molten metal after the addition step is allowed to flow down, and high-pressure water or high-pressure inert gas is sprayed onto the molten metal flow to pulverize it, and at the same time, the molten metal is rapidly cooled and solidified, thereby obtaining a ferritic stainless steel powder. The spray medium is not particularly limited, and a conventional method may be used, for example, the water atomization method using high-pressure water or the gas atomization method using high-pressure gas as described above may be used. If necessary, the obtained powder may be subjected to a spheroidization treatment by thermal plasma or mechanical processing. Here, the time from the start of the addition step to the end of the pulverization step is preferably within 30 minutes. If this time is exceeded, the molten metal containing La and Zr will be in contact with the resistant material such as a tundish for a long time, and there is a concern that the addition yield of La and Zr will decrease due to the formation of La oxide and Zr oxide. The time is preferably within 10 minutes, more preferably within 5 minutes.

[0029] Next, the structural morphology of the ferritic stainless steel powder of the present invention will be described. The stainless steel powder produced by the above-mentioned production method has a Zr-enriched phase at the grain boundaries of the metal structure by being rapidly solidified in a state where Zr is homogeneously dissolved in the molten metal in the powdering process. This Zr-enriched phase combines with C to form Zr carbides in the sintering process for forming a sintered body using the ferritic stainless steel powder of the present invention. Since Zr is concentrated at the grain boundaries, Zr carbides are preferentially formed at the grain boundaries, which not only prevents embrittlement due to the formation of coarse Zr carbides, but also strengthens the grain boundaries and is expected to improve high-temperature strength. The Zr-enriched phase at the grain boundaries in the present invention refers to a region where the Zr count number observed on the grain boundaries of the metal structure is 3 or more when the cross section of the metal structure of the ferritic stainless steel powder is observed using a scanning electron microscope and an electron microanalyzer under conditions of a voltage of 15 kV, a current of 100 nA, and a measurement time of 0.01 seconds per point, as shown in FIG. 1, and the backscattered electron image obtained is compared with the surface analysis results of Zr. In the present invention, the grain boundary coverage of the Zr-enriched phase (the ratio of the length of the grain boundary covered by the Zr-enriched phase to the total length of the grain boundary) is preferably 50% or more, more preferably 60% or more, even more preferably 70% or more, and particularly preferably 80% or more.

[0030] In the ferritic stainless steel powder of the present invention, if the powder diameter is greater than 100 μm on average, the gaps between the powder particles will become large during the production of a sintered body, preventing sintering and resulting in embrittlement of the sintered body. Therefore, the average powder diameter of the ferritic stainless steel powder of the present invention is limited to 100 μm or less, and preferably 70 μm or less. There is no particular need to specify a lower limit, and the average powder diameter can be set to 1 μm or more, for example. When handling properties and the like are taken into consideration, the average powder diameter can be set to 5 μm or more, or 10 μm or more. EXAMPLES

[0031] The present invention will be described in more detail in the following examples, but the present invention is not limited to these examples. First, alloy materials were prepared using a vacuum induction furnace. The component analysis values ​​of the obtained alloy materials are shown in Table 1. No. 1 was 6955g, and No. 2 was 6980g.

[0032] [Table 1]

[0033] <Dissolution process> Next, the obtained alloy material was placed in a tundish of a gas atomizer, and the atmosphere was replaced with Ar. After that, melting was completed by high-frequency induction heating, and the temperature was adjusted to a suitable level for allowing the obtained molten metal to flow down. <Addition process> After adjusting the temperature, 30 g of crushed La raw material (LaNi5) and 12.3 g of crushed Zr raw material (metallic Zr) were added to the molten metal in No. 1 to prepare an example of the present invention. In contrast, the addition process was not carried out in No. 2, which was prepared as a comparative example. <Powdering process> The molten metal was then allowed to flow down and Ar gas was sprayed onto it to produce metal powders No. 1 and No. 2 through the pulverization process. The time taken from the start of the No. 1 addition process to the completion of the pulverization process was approximately 3 minutes. The component analysis values ​​of the obtained metal powders are shown in Table 2.

[0034] [Table 2]

[0035] From Tables 1 and 2, the amount of La and Zr contained in the alloy material in No. 2, which is a comparative example, is greatly reduced. This is believed to be because the refractory is in contact with the molten metal for a long time during the melting process, and the reduction reaction of the refractory by La and Zr in the molten metal proceeds sufficiently, and La and Zr in the molten metal are removed as La oxides and Zr oxides. On the other hand, in No. 2, which is an example of the present invention, the analytical values ​​of La and Zr in the stainless steel powder are within the composition ranges for La: 0.02% to 0.12% and Zr: 0.01% to 0.52%, which are the composition ranges for achieving excellent oxidation resistance, and the addition yield is improved. This is believed to be because the La raw material and Zr raw material are added after the melting process, which significantly shortens the time for La and Zr in the molten metal to react with the refractory from the time the amount of La and Zr in the molten metal is adjusted to the target value until it flows down. In No. 1, the components of Si, Al, and Ni are increased. The increase in Si and Al is believed to be due to the reduction of Al2O3 and SiO2 contained in the refractory by La and Zr contained in the alloy material, while the increase in Ni is believed to be due to the influence of Ni contained in the added LaNi5.

[0036] The obtained ferritic stainless steel powder 1 of No. 1 was cold embedded in embedding resin 2 and polished, and then the cross section of the metal structure at the center of the powder with a diameter of about 40 μm was observed with a scanning electron microscope and a Zr surface analysis was performed using a JEOL electron probe microanalyzer JXA-8530F at a voltage of 15 kV, a current of 100 nA, and 0.01 seconds per point. The obtained photograph is shown in Figure 1. Comparing the backscattered electron image shown in Figure 1(a) with the Zr surface analysis results shown in Figure 1(b), it was confirmed that a Zr-enriched phase with a Zr count of 3 or more was present at the crystal grain boundaries of the powder structure with a grain boundary coverage rate of 50% or more. [Explanation of symbols]

[0037] 1 Ferritic stainless steel powder 2. Mounting resin

Claims

1. a melting step of melting an alloy material to obtain a molten ferritic stainless steel containing, by mass%, C: 0.1% or less, Al: 0.2% or less, Si: 0.2% or less, Mn: 1.0% or less, Cr: 26.0% or less, Ni: 1.0% or less, Cu: 4.0% or less, and W: 3.0% or less; an adding step of adding a La raw material and a Zr raw material to the molten metal; and a powdering step for obtaining ferritic stainless steel powder from the molten metal after the adding step. A method for producing a ferritic stainless steel powder, wherein the ferritic stainless steel powder obtained by the powdering step contains, by mass%, C: more than 0% and not more than 0.1%, Al: 0.2% or less, Si: 0.2% or less, Mn: 0.1% or more and 1.0% or less, Cr: 20.0% or more and 26.0% or less, Ni: 0.1% or more and 1.0% or less, Cu: 0.3% or more and 4.0% or less, W: 1.0% or more and 3.0% or less, La: 0.02% or more and 0.12% or less, Zr: 0.01% or more and 0.5% or less, La + Zr: 0.03% or more and 0.52% or less, with the balance being Fe and unavoidable impurities.

2. A ferritic stainless steel powder containing, by mass%, C: more than 0% and 0.1% or less, Al: 0.2% or less, Si: 0.2% or less, Mn: 0.1% or more and 1.0% or less, Cr: 20.0% or more and 26.0% or less, Ni: 0.1% or more and 1.0% or less, Cu: 0.3% or more and 4.0% or less, W: 1.0% or more and 3.0% or less, La: 0.02% or more and 0.12% or less, Zr: 0.01% or more and 0.5% or less, La + Zr: 0.03% or more and 0.52% or less, the balance being Fe and unavoidable impurities, and having an average powder size of 1 μm to 100 μm, The metal structure of the ferritic stainless steel powder has a Zr-enriched phase at the grain boundaries.

Citation Information

Patent Citations

  • Steel for solid oxide fuel cell separator

    JP2003173795A

  • Steel for solid-oxide fuel cell separator

    JP2007016297A

  • Steel for solid oxide fuel cells having excellent oxidation resistance, and member for solid oxide fuel cells using same

    WO2012144600A1