Copper alloy wire, plated wire, electric wire, and cable
A copper alloy wire with 0.3% to 0.45% indium and optional 0.1% tin, combined with a specific manufacturing process, achieves high tensile strength and conductivity, addressing the trade-off in existing technologies and enabling advanced applications in electronics and medicine.
Patent Information
- Application Number
- JP2020205438
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-02-06
- Filing Date
- 2020-12-11
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-12-11
AI Technical Summary
Existing copper alloy wires face a trade-off between improving tensile strength and electrical conductivity, particularly in thin wires used for conductors and cables in electronic devices, where both properties are crucial for performance.
A copper alloy wire composition containing 0.3% to 0.45% indium by mass, with optional tin up to 0.1% by mass, achieving a tensile strength of 800 MPa or more and electrical conductivity of 80% IACS or more, combined with a manufacturing process that includes controlled heat treatment and multiple drawing steps to maintain these properties.
The solution simultaneously enhances both tensile strength and electrical conductivity, enabling the production of ultra-fine copper alloy wires suitable for demanding applications in electronic devices and medical instruments.
Smart Images

Figure 0007574633000003 
Figure 0007574633000004 
Figure 0007574633000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a copper alloy wire, a plated wire, and an electric wire and a cable using the same. [Background technology]
[0002] Patent Document 1 (JP Patent Publication No. 5-311285) describes a copper alloy wire containing In and Sn in addition to Cu. Patent Document 2 (JP Patent Publication No. 2014-159609) describes a copper alloy body containing 0.01 atomic % or more of at least one element selected from the group consisting of Ag, In, Mg, and Sn as a copper alloy body before wire drawing. Patent Document 3 (WO 2014 / 007259) describes performing intermediate heat treatment between multiple cold working processes in the manufacturing process of a copper alloy material. Patent Document 4 (JP Patent Publication No. 2015-4118) describes performing annealing after drawing and then finish drawing in the manufacturing process of a drawn copper wire. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 5-311285 [Patent Document 2] JP 2014-159609 A [Patent Document 3] International Publication No. 2014 / 007259 [Patent Document 4] JP 2015-4118 A Summary of the Invention [Problem to be solved by the invention]
[0004] Metal wires made of copper alloys are used in a variety of applications. For example, there is a demand for thinner metal wires that make up conductors and cables used in wiring components of electronic devices. For such applications, the strength and electrical conductivity of the thinner metal wires are required to be improved.
[0005] An object of the present invention is to provide a technique for improving both the strength and electrical conductivity of a metal wire. [Means for solving the problem]
[0006] The copper alloy wire according to one embodiment is made of a copper alloy containing 0.3% by mass to 0.45% by mass of indium. The copper alloy wire has a tensile strength of 800 MPa or more and a conductivity of 80% IACS or more.
[0007] For example, the copper alloy contains 0.02 mass % or more and less than 0.1 mass % of tin, and the total content of the indium and the tin is 0.45 mass % or less.
[0008] Another embodiment of the electric wire includes a conductor made of a copper alloy wire and an insulator covering the conductor. The copper alloy wire is made of a copper alloy containing 0.3% by mass to 0.45% by mass of indium. The tensile strength of the copper alloy wire is 800 MPa or more, and the electrical conductivity of the copper alloy wire is 80% IACS or more.
[0009] For example, the copper alloy in the electric wire contains 0.02 mass % or more and less than 0.1 mass % of tin, and the total content of the indium and the tin is 0.45 mass % or less.
[0010] For example, the conductor is made of a plurality of the copper alloy wires twisted together.
[0011] Another embodiment of the plated wire includes a copper alloy wire and a plating layer provided around the copper alloy wire, the copper alloy wire being made of a copper alloy containing 0.3 mass % or more and 0.45 mass % or less of indium, and having a tensile strength of 750 MPa or more, an electrical conductivity of 78% IACS or more, and an elongation of 3% or less.
[0012] Another embodiment of the cable includes a conductor made of a copper alloy wire, a plurality of core wires each having an insulator covering the conductor, and a sheath covering the plurality of core wires together. The copper alloy wire is made of a copper alloy containing 0.3% to 0.45% by mass of indium. The tensile strength of the copper alloy wire is 800 MPa or more, and the electrical conductivity of the copper alloy wire is 80% IACS or more.
[0013] For example, the copper alloy in the cable contains 0.02 mass % or more and less than 0.1 mass % tin, and the total content of the indium and the tin is 0.45 mass % or less. Effect of the Invention
[0014] According to a representative embodiment of the present invention, it is possible to improve both the strength and the electrical conductivity of a metal wire. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a perspective cross-sectional view of a metal wire according to an embodiment. [Diagram 2] 2 is a flow chart showing an example of a manufacturing process of the metal wire shown in FIG. [Diagram 3] 2 is a cross-sectional view of a cable including the metal wire shown in FIG. 1. [Figure 4] 4 is a cross-sectional view of one of a plurality of electric wires included in the cable shown in FIG. 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In the following description, a metal wire made of a copper alloy and having a wire diameter (outer diameter) of 100 μm or less is called a copper alloy wire. Also, a wire before being drawn into a copper alloy wire is called a roughly drawn wire. Also, a copper alloy wire having a plating layer around it is called a plated wire.
[0017] In the following description, an index called "IACS (International Annealed Copper Standard)" is used as an evaluation index for electrical conductivity. The electrical conductivity using IACS is calculated based on the volume resistivity of annealed standard soft copper (volume resistivity: 1.7241×10 -2 The electrical conductivity of the specimen is defined as 100% IACS, and the percentage of the electrical conductivity of this annealed standard soft copper is expressed as "XX% IACS." The electrical conductivity described below is calculated based on the results of measuring the electrical resistance and diameter of the test piece in accordance with the test method for electrical copper wire specified in the Japanese Industrial Standards (JIS C 3002:1992).
[0018] In the following description, when the "tensile strength" and "elongation" of a metal wire are described, a tensile test is performed on a test piece in accordance with the test method for electrical copper wire specified in the Japanese Industrial Standards (JIS C 3002:1992), and the values calculated from the measurement results are taken as the "tensile strength" and "elongation".
[0019] <Metal wire structure> Fig. 1 is a perspective cross-sectional view of a metal wire according to the present embodiment. The copper alloy wire 10 shown in Fig. 1 is a copper alloy wire made of a copper alloy 11, which contains 0.3 mass% or more and 0.45 mass% or less of indium (In). The copper alloy 11 contains inevitable impurities as the remainder. The tensile strength of the copper alloy wire 10 is 800 MPa or more (preferably, 800 MPa or more and 900 MPa or less), and the electrical conductivity of the copper alloy wire 10 is 80% IACS or more (preferably, 80% IACS or more and 85% IACS or less).
[0020] Examples of the inevitable impurities contained in the copper alloy 11 include aluminum (Al), silicon (Si), phosphorus (P), sulfur (S), chromium (Cr), iron (Fe), nickel (Ni), arsenic (As), selenium (Se), silver (Ag), antimony (Sb), lead (Pb), and bismuth (Bi). The inevitable impurities contained in the copper alloy 11 are contained in a range of, for example, 20 ppm by mass to 30 ppm by mass.
[0021] The copper alloy wire 10 having the above-mentioned copper alloy 11 can achieve both high levels of tensile strength and electrical conductivity. Details will be described later as an example, but as a result of confirmation by the present inventor, the copper alloy wire 10 having the copper alloy 11 containing 0.3 mass% or more and 0.45 mass% or less of indium (In) and the remainder consisting of copper (Cu) and unavoidable impurities has electrical conductivity of 80% IACS or more. In addition, the tensile strength of the copper alloy wire 10 was 872 MPa or more. The value of the tensile strength of the copper alloy wire 10 may vary depending on the manufacturing conditions, but even if the variation due to the manufacturing conditions is taken into consideration, a value of at least 800 MPa or more can be obtained.
[0022] Conductive wires that transmit electricity (hereinafter simply referred to as electric wires) are components that constitute power transmission paths or electric signal transmission paths, and are widely used in various fields. Conductive materials such as various kinds of pure metals, alloys, and composite materials are used as conductors in electric wires. In this embodiment, a copper alloy wire 10 made of a copper alloy 11 having high conductivity will be described as a conductor in an electric wire.
[0023] Copper wires used as conductors in electric wires are used in various fields as described above, but depending on the field of use, copper wires with a small wire diameter may be required. For example, in electronic devices such as portable terminals, electric wires with conductors made of copper wires are used as internal wiring components. In this case, the wire diameter of one copper wire may be required to be 100 μm or less. In addition, in the case of probe cables used in the medical field, they may be used for applications in which they are inserted into the body of a patient, and copper wires with even smaller wire diameters are required. In this embodiment, a copper alloy wire 10 with a wire diameter 10D of 80 μm will be described as an example of an ultra-fine wire.
[0024] The tensile strength of the copper alloy wire 10 made of the copper alloy 11 can be improved by causing strain in the copper alloy 11. Methods for causing strain in the copper alloy 11 include a method for increasing the content of metal elements other than copper contained in the copper alloy 11, and a method for performing wire drawing. However, when strain is caused in the copper alloy wire 10 by these methods, the resistivity of the copper alloy 11 as a conductive member increases, and therefore the conductivity of the copper alloy wire 10 decreases. In other words, there is a trade-off between increasing the tensile strength of the copper alloy wire 10 and increasing the conductivity of the copper alloy wire 10.
[0025] Therefore, in order to find a configuration that improves the electrical conductivity and tensile strength of the solid-solution strengthened copper alloy 11, the inventors of the present application focused on the effect of a plurality of metal elements on the decrease in electrical conductivity of the copper alloy 11 when they are solid-solved in the copper alloy 11, and the degree to which they contribute to strengthening the tensile strength. That is, the degree of contribution to strengthening the tensile strength of the copper alloy wire 10 varies depending on the type of metal element, and the tensile strength increases in proportion to the content of the element that is solid-solved in copper. Tin (Sn) and indium (In) are effective additive elements because they have a large effect on increasing the tensile strength when they are solid-solved in copper, compared to metals such as aluminum (Al), nickel (Ni), or magnesium (Mg).
[0026] On the other hand, the degree of influence on the decrease in electrical conductivity varies greatly depending on the type of metal element. In detail, in the case of silver (Ag), indium (In), or magnesium (Mg), the decrease in electrical conductivity can be suppressed even if the concentration of the metal elements dissolved in copper is large, compared to metals such as nickel (Ni), tin (Sn), and aluminum (Al). For example, when the concentration (mass concentration) of the above metal elements dissolved in oxygen-free copper is 900 ppm, the electrical conductivity of tin (Sn) decreases to about 92% of that of pure copper (percentage), while the electrical conductivity of indium (In) decreases to about 98%. In addition, in the case of silver (Ag), the electrical conductivity of pure copper decreases to about 99% of that of pure copper (percentage).
[0027] From the above-mentioned characteristics, the copper alloy 11 obtained by dissolving indium in copper has high levels of electrical conductivity and tensile strength. In the case of a copper alloy in which silver (Ag) is dissolved in copper, an even higher electrical conductivity can be obtained than the copper alloy wire 10 of the present embodiment. However, since silver has a smaller effect of increasing tensile strength than indium at the same concentration, increasing the silver content increases the raw material cost of the copper alloy wire 10, so it is preferable to dissolve indium.
[0028] In addition, in order to improve the tensile strength of the copper alloy 11, it is preferable that the content of oxygen contained in the copper alloy is small. In the case of the present embodiment, the oxygen content of the copper alloy 11 is 0.002 mass% or less. If the oxygen content of the copper alloy 11 is 0.002 mass% or less, it is possible to suppress a decrease in the tensile strength of the copper alloy 11 caused by oxygen.
[0029] As a modification of the copper alloy wire 10 shown in Fig. 1, the copper alloy 11 may contain 0.3 mass% or more and less than 0.43 mass% indium (In), 0.02 mass% or more and less than 0.1 mass% tin (Sn), and the balance may be copper (Cu) and unavoidable impurities. However, the total content of indium and tin contained in the copper alloy 11 is 0.45 mass% or less.
[0030] In the case of the modified copper alloy wire 10, the copper alloy 11 contains tin in a solid solution, so that the electrical conductivity is relatively low compared to the above-mentioned copper alloy wire 10 that does not contain tin. However, by making the tin content less than 0.1 mass% and making the indium content 0.3 mass% or more, the electrical conductivity of 80% IACS or more can be maintained. However, the total content of indium and tin contained in the copper alloy 11 is preferably 0.45 mass% or less. According to the experimental results described later, within the range of the above-mentioned conditions, the tensile strength of the modified copper alloy wire 10 was 872 MPa or more. Thus, in the case of the modified copper alloy wire 10, by making the tin in a solid solution, the electrical conductivity of 80% IACS or more can be maintained and the raw material cost of the copper alloy wire 10 can be reduced.
[0031] <Metal Wire Manufacturing Method> Next, a method for manufacturing the copper alloy wire 10 shown in Fig. 1 will be described. The above-mentioned copper alloy wire 10 may or may not contain tin in the copper alloy, but the manufacturing method is the same. Fig. 2 is a flow chart showing an example of a manufacturing process of the metal wire shown in Fig. 1.
[0032] In the following, as a method for manufacturing a metal wire, a method will be described in which a wire rod having a certain wire diameter (for example, about 8 mm to 12 mm) is manufactured by a continuous casting and rolling method, and then the wire rod is subjected to a wire drawing process to manufacture a metal wire. As the continuous casting and rolling method, for example, a continuous casting and rolling method called the SCR method (Southwire Continuous Rod system) can be used.
[0033] First, in the raw material preparation step shown in FIG. 2, a raw material is prepared. The raw material is a metal mainly composed of copper. In addition to copper, the raw material may contain impurity elements that are inevitably mixed in as described above. The raw material also contains additive elements including indium. In the manufacturing method of the metal wire described as a modified example of the copper alloy wire 10 shown in FIG. 1, the additive elements are indium and tin. These additive elements are added to the raw material mainly composed of copper within a range that satisfies the above-mentioned content condition.
[0034] Next, in the melting process shown in Fig. 2, the raw materials are melted in a melting furnace (not shown). The melting furnace is a heating furnace capable of continuously melting the raw materials, and the molten copper melted in the melting furnace is transferred sequentially to a heat-retaining furnace (not shown).
[0035] Next, in the casting process shown in FIG. 2, the molten copper in the heat-retaining furnace is poured into a mold (not shown) and then cooled to solidify. The solidified casting is removed from the mold and sequentially sent to a rolling device. The melting process to the casting process shown in FIG. 2 are performed in an inert gas atmosphere (e.g., a nitrogen atmosphere). There is almost no oxygen in the inert gas atmosphere, and at least the oxygen concentration (volume concentration) is 10 ppm or less. In this way, by manufacturing the rough wire in an inert gas atmosphere with an extremely low oxygen concentration, it is possible to suppress the inclusion of oxygen in the copper during the casting process.
[0036] Next, in the rolling step shown in Fig. 2, the cast product is rolled to form a wire rod having a wire diameter of about 8 mm to 12 mm. In the rolling step, the rolling treatment may be performed multiple times. Note that, when the cast product obtained in the casting step is used as the wire rod as it is, this rolling step may be omitted.
[0037] Next, in the winding process shown in Fig. 2, the wire is wound by a winding device (not shown) to obtain a wire rod. The wire rod wound by the winding device has a tensile strength of about 250 MPa to about 300 MPa and an electrical conductivity of more than 85% IACS and about 90% IACS or less.
[0038] Next, in the wiredrawing process shown in FIG. 2, the roughly drawn wire is drawn until the wire diameter is 100 μm or less (for example, about 50 μm to 80 μm) to obtain the copper alloy wire 10 shown in FIG. 1. The wiredrawing process is carried out at room temperature (for example, 25° C.), so-called cold working. In the wiredrawing process, the roughly drawn wire is extended in the extension direction, but the wiredrawing process is divided into a plurality of processes (a first wiredrawing process and a second wiredrawing process), and a heat treatment process (sometimes called an annealing process) is performed between the wiredrawing processes to apply heat treatment to the drawn wire material during the wiredrawing process. Note that the first wiredrawing process is preferably performed by drawing the roughly drawn wire (for example, about 8 mm to 12 mm in wire diameter) to a desired wire diameter (for example, 0.5 mm to 3.0 mm in wire diameter) in one wiredrawing process. Such wiredrawing is effective in bringing the electrical conductivity, tensile strength and elongation of the metal wire after the heat treatment step into the desired range, and in making the copper alloy wire 10 obtained through the second wiredrawing step have an electrical conductivity of 80% IACS or more and a tensile strength of 800 MPa or more.
[0039] During the wire drawing process, distortion occurs in the metal wire, which increases the tensile strength of the metal wire, but decreases the electrical conductivity of the metal wire. If heat treatment (sometimes called annealing) is performed during the wire drawing process, the distortion in the metal wire is reduced. Therefore, the tensile strength of the heat-treated metal wire decreases, but the electrical conductivity increases. According to the study by the present inventors, it has been found that the tensile strength and electrical conductivity of the finally obtained hard metal wire (copper alloy wire 10) can be maintained at a high level by performing a heat treatment process during the wire drawing process (between the first wire drawing process and the second wire drawing process) so as to satisfy the following conditions. The hard copper alloy wire referred to here is a metal wire with an elongation of 0.5% to 3%.
[0040] If the tensile strength of the metal wire before the heat treatment (after the wire drawing process immediately before the heat treatment) is A, the tensile strength of the metal wire after the heat treatment (immediately after the heat treatment) is B, and C=B / A, the heat treatment is performed so that the tensile strength ratio C is 0.5 to 0.8. If the elongation of the metal wire before the heat treatment (after the wire drawing process immediately before the heat treatment) is D, the elongation of the metal wire after the heat treatment (immediately after the heat treatment) is E, and F=E / D, the heat treatment is performed so that the elongation ratio F is 10 to 50. As shown in FIG. 2, since the wire drawing process is further performed after the heat treatment process, it is preferable to perform the heat treatment in the heat treatment process so that the electrical conductivity of the metal wire immediately after the heat treatment process is 86% IACS or more (preferably 88% IACS or more). It is preferable that the tensile strength of the metal wire immediately after the heat treatment process is 200 MPa to 300 MPa, and the elongation of the metal wire immediately after the heat treatment process is 20% to 40%. This allows the electrical conductivity to be 80% IACS or more after the wire drawing process (second wire drawing process) that is performed following the heat treatment process. Note that the heat treatment process is preferably performed at a temperature of 400°C or more and 900°C or less.
[0041] In FIG. 2, the embodiment has been described in which the rough wire is drawn to a desired wire diameter (for example, a wire diameter of 0.5 mm to 3.0 mm) by a wiredrawing process (first wiredrawing process), the heat treatment process is performed to heat treat the metal wire under the above-mentioned conditions, and the wiredrawing process (second wiredrawing process) is further performed to a desired wire diameter (for example, a wire diameter of 0.1 mm or less), but various modified examples are applicable. For example, the second wiredrawing process may be divided into a plurality of wiredrawing processes, and the metal wire may be drawn stepwise to the desired wire diameter by each step in the plurality of wiredrawing processes. In the second wiredrawing process, the metal wire is drawn stepwise by a plurality of wiredrawing processes, so that the above-mentioned hard metal wire (copper alloy wire 10) can be stably obtained compared to the case where the second wiredrawing process is composed of a single wiredrawing process. In addition, when the second wiredrawing process is composed of multiple wiredrawing processes, the above-mentioned heat treatment process may be provided between the multiple wiredrawing processes as necessary. After the second wiredrawing process, the metal wire may be subjected to heat treatment so as to maintain the hard state.
[0042] <Evaluation of alloy composition and properties> Next, a description will be given of the results of an experiment on the relationship between the alloy composition and characteristics of the copper alloy wire 10 shown in Fig. 1. Table 1 shows the relationship between the alloy composition and characteristics of the metal wire.
[0043] [Table 1]
[0044] In Table 1, Samples No. 1 to 7 are examples that meet the conditions of the copper alloy wire 10 described above, and Samples No. 8 to 14 are comparative examples that do not meet the conditions of the copper alloy wire 10 described above. Each of Samples No. 1 to 14 was manufactured by the manufacturing method described with reference to FIG. 2. In addition, in Table 1, the samples used in the tensile strength test and the elongation test are metal wires processed to have a wire diameter of about 80 μm. The copper alloy wires used in Samples No. 1 to 14 are composed of a copper alloy containing indium (In) and tin (Sn) with the contents shown in Table 1, and the balance being copper (Cu) and unavoidable impurities. In addition, the tensile speed was 20 mm / min, and the gauge length when measuring the elongation was 100 mm. The tensile strength was determined by dividing the maximum breaking load value by the cross-sectional area of the sample. The cross-sectional area of the sample was calculated as the area of a perfect circle from the wire diameter measured to 1 / 1000 mm with a micrometer. The elongation value is the total elongation at break (the elastic elongation and plastic elongation of the extensometer combined) and is expressed as a percentage of the extensometer gauge length. Although not shown in Table 1, each of Samples No. 1 to 14 was prepared in an environment where oxygen was unlikely to be mixed in, and the oxygen content of the copper alloy of each sample was 0.002 mass% or less.
[0045] As can be seen by comparing samples Nos. 1, 5, 6, 8, 11, and 12 in Table 1, if the indium content is 0.30 mass% or more, the tensile strength of the sample can be 800 MPa or more and the electrical conductivity can be 80% IACS or more. Also, as can be seen by comparing samples Nos. 3, 4, and 10, if tin is not added as an additive element and the indium content is 0.45 mass% or less, the tensile strength of the sample can be 800 MPa or more and the electrical conductivity can be 80% IACS or more.
[0046] Also, as can be seen by comparing Samples Nos. 5, 8, 9, and 14 in Table 1, when indium and tin are added to a copper alloy, if the tin content is 0.02 mass% or more and less than 0.1 mass%, the tensile strength of the sample can be 800 MPa or more and the electrical conductivity can be 80% IACS or more. However, as can be seen by comparing Samples Nos. 7 and 13, it is preferable that the total content of indium and tin is 0.45 mass% or less.
[0047] <Application examples of copper alloy wire> Next, an application example of the copper alloy wire 10 shown in Fig. 1 will be described. Fig. 3 is a cross-sectional view of a cable including the copper alloy wire 10 shown in Fig. 1. Fig. 4 is a cross-sectional view of one of the electric wires of the cable shown in Fig. 3.
[0048] The cable 60 shown in Fig. 3 has a plurality of electric wires (core wires) 70 and a sheath 61 that collectively covers the circumference of the plurality of electric wires 70. The cable 60 is a cable used in, for example, a portable electronic device or an industrial robot. The outer diameter of the cable 60 is, for example, about 4.8 mm. The cable 60 includes a plurality of electric wires 70, and each of the plurality of electric wires 70 has a small outer diameter. For example, in the example shown in Figs. 3 and 4, the outer diameter of the electric wire 70 is, for example, about 0.86 mm (860 µm).
[0049] As shown in Fig. 4, the electric wire 70 has a central conductor 71 made of a plurality of copper alloy wires 10 twisted together, and an insulator 72 covering the central conductor 71. Each of the plurality of copper alloy wires 10 constituting the central conductor 71 is made of the copper alloy 11 described with reference to Fig. 1. The copper alloy 11 constituting this copper alloy wire 10 contains 0.3 mass % or more and 0.45 mass % or less of indium, and tin whose total content with indium is 0.45 mass % or less. The wire diameter of each of the plurality of copper alloy wires 10 is, for example, 0.08 mm (80 µm).
[0050] In this way, the electric wire 70 using a plurality of copper alloy wires 10 and the cable 60 using the same can improve the transmission characteristics of electric signals or power in portable electronic devices. Alternatively, the electric wire 70 using a large number of ultra-fine copper alloy wires 10 and the cable 60 using the same can have a small wire diameter, so that the size of the housing of the portable electronic device can be reduced and industrial robots and the like can be reduced in size.
[0051] In addition, while Fig. 4 shows the electric wire 70 as an example, there are various modified examples of the electric wire to which the copper alloy wire 10 shown in Fig. 1 is applied. For example, the present invention can be applied to an electric wire that is composed of a conductor composed of one copper alloy wire 10 and an insulator that covers the conductor. In addition, in Figs. 3 and 4, the central conductor 71 of the electric wire 70 is exemplified as being made by twisting together a plurality of copper alloy wires 10, but the present invention is not limited to this, and the central conductor 71 may be made of a plated wire, which will be described later.
[0052] <Plated wire> The plated wire is configured by having a plating layer around (on the outer surface of) the copper alloy wire 10 shown in Fig. 1. The plated wire has a tensile strength of 750 MPa or more, an electrical conductivity of 78% IACS or more, and an elongation of 3% or less. That is, in a state where the plating layer is provided around the copper alloy wire 10 shown in Fig. 1, the plated wire has a tensile strength of 750 MPa or more (preferably 750 MPa or more and 900 MPa or less), an electrical conductivity of 78% IACS or more (preferably 78% IACS or more and 85% IACS or less), and an elongation of 3% or less (preferably 0.5% or more and 3% or less). The plated wire 30 is a hard wire.
[0053] As described above, the copper alloy wire 10 is made of a copper alloy containing 0.3 mass% or more and 0.45 mass% or less of indium (In). In particular, the copper alloy wire 10 is preferably made of a copper alloy containing 0.3 mass% or more and 0.45 mass% or less of indium (In), with the remainder being copper (Cu) and unavoidable impurities.
[0054] The plating layer is provided around the copper alloy wire 10 so as to contact the outer surface of the copper alloy wire. The thickness of the plating layer is, for example, 0.1 μm or more and 1.5 μm or less. The plating layer is made of, for example, tin (Sn), silver (Ag), nickel (Ni), etc.
[0055] <Method of manufacturing plated wire> The plated wire is obtained by forming a plating layer on the copper alloy wire 10 obtained by the manufacturing method of the copper alloy wire 10 shown in FIG. 2. The copper alloy wire 10 before forming the plating layer is a metal wire in a hard state having a tensile strength of 800 MPa or more and an electrical conductivity of 80% IACS or more. The copper alloy wire 10 is immersed in a plating tank in which a molten plating material (e.g., Sn) having a predetermined temperature (e.g., 250°C to 300°C) is stored. In this way, the hot-dip plating is applied to the entire outer surface of the copper alloy wire 10. Thereafter, the copper alloy wire 10 in the state in which the hot-dip plating is applied is passed through a plating die to adjust the thickness of the hot-dip plating applied to the surface of the copper alloy wire 10, and a plating layer having a predetermined thickness is formed. In particular, the conditions for applying the hot-dip plating to the surface of the copper alloy wire 10 are preferably a linear speed of 100 m / min or more and an immersion time in the hot-dip plating of 0.1 seconds to 1.0 seconds. The plated wire on which the plating layer is formed in this manner maintains a hard state, and the elongation of the plated wire is 0.5% or more and 3.0% or less. Before applying hot-dip plating to the surface of the copper alloy wire 10, the copper alloy wire 10 may be heat-treated at a predetermined temperature (e.g., 300°C or more and 500°C or less). The heat treatment time when the copper alloy wire 10 is heat-treated is, for example, 0.1 seconds or more and 1.0 seconds or less, and the copper alloy wire 10 is immersed in the hot-dip plating of the next process while maintaining the hard state. This heat treatment may be performed in the same manufacturing line as the process of forming the plating layer, or may be performed in a manufacturing line different from the process of forming the plating layer.
[0056] <Characteristics of plated wire> Next, the results of an experiment on the characteristics of the plated wire will be described. Table 2 shows the relationship between the alloy composition of the copper alloy wire constituting the plated wire and the characteristics of the plated wire.
[0057] [Table 2]
[0058] In Table 2, Samples No. 15 to 20 are examples that meet the above-mentioned conditions of the plated wire. Each of Samples No. 15 to 20 is a copper alloy wire manufactured by the manufacturing method described with reference to FIG. 2, and a plating layer is formed around it. Specifically, the copper alloy wire manufactured by the manufacturing method described with reference to FIG. 2 is immersed in a plating tank storing molten Sn (temperature: 250°C to 300°C), and then the copper alloy wire coated with the hot-dip plating is passed through a plating die to adjust the thickness of the hot-dip plating applied to the surface of the copper alloy wire, and a plating layer having a predetermined thickness is formed. In addition, in Table 2, the samples used for the tensile strength test and elongation test of the plated wire are copper alloy wires processed to have a wire diameter of about 80 μm (Samples No. 15 to 17) or about 50 μm (Samples No. 18 to 20), and a plating layer (thickness: about 0.5 μm) is provided around the copper alloy wires processed to have a wire diameter of about 80 μm (Samples No. 15 to 17) or about 50 μm (Samples No. 18 to 20). The copper alloy wires used in samples No. 15 to 20 are composed of copper alloys containing indium (In) and tin (Sn) with the contents shown in Table 2, with the remainder being copper (Cu) and unavoidable impurities. The tensile speed was 20 mm / min, and the gauge length when measuring the elongation was 100 mm. The tensile strength was determined by dividing the maximum breaking load value by the cross-sectional area of the sample. The cross-sectional area of the sample was calculated as the area of a perfect circle from the wire diameter measured to 1 / 1000 mm with a micrometer. The elongation value is the total elongation at break (the combination of the elastic elongation and plastic elongation of the extensometer) and is expressed as a percentage of the gauge length of the extensometer. Although not shown in Table 2, each of samples No. 15 to 20 was prepared in an environment where oxygen was unlikely to be mixed in, and the oxygen contained in the copper alloy wire of each sample was 0.002 mass% or less.
[0059] As can be seen by comparing samples No. 15 to No. 20 in Table 2, if the indium content is 0.30 mass% or more, the tensile strength of the sample can be 750 MPa or more and the electrical conductivity can be 78% IACS or more. Also, as can be seen by comparing samples No. 15 and No. 16, even if tin is added as an additive element, the tensile strength of the sample can be 750 MPa or more and the electrical conductivity can be 78% IACS or more, similarly to the case where tin is not added. The content of indium contained in the copper alloy constituting the copper alloy wire is preferably 0.30 mass% or more and 0.45 mass% or less. Also, when indium and tin are added to the copper alloy constituting the copper alloy wire, if the content of tin is 0.02 mass% or more and less than 0.1 mass%, the tensile strength of the sample can be 750 MPa or more and the electrical conductivity can be 78% IACS or more.
[0060] <Application examples of plated wire> As described above, the plated wire can be used as a central conductor for constituting an electric wire or cable. Specifically, the electric wire has a central conductor made of a plurality of plated wires twisted together and an insulator covering the central conductor. In addition, the electric wire may be provided with a shield layer or sheath around it to form a cable.
[0061] The present invention is not limited to the above-described embodiment and examples, and various modifications can be made without departing from the spirit and scope of the present invention.
[0062] The above embodiment includes the following aspects.
[0063] [Appendix 1] (a) preparing a raw material containing copper and an additive element other than copper; (b) melting the raw material and then casting it to form a wire rod; (c) drawing the wire into a metal wire; (d) after the step (c), a step of subjecting the drawn metal wire to a heat treatment; (e) after the step (d), further drawing the heat-treated metal wire to elongate it to a length of 0.1 mm or less; Including, The method for producing a copper alloy wire, wherein the roughly drawn wire is made of a copper alloy and contains 0.3 mass% or more and 0.45 mass% or less of indium, and tin whose total content together with the indium is 0.45 mass% or less.
[0064] [Appendix 2] In Appendix 1: The copper alloy contains 0.02 mass% or more and less than 0.1 mass% tin.
[0065] [Appendix 3] In Appendix 1 or 2, In the step (d), the tensile strength of the metal wire drawn after the step (c) is A, the tensile strength of the metal wire subjected to the heat treatment after the step (d) is B, and the ratio of the tensile strengths is C=B / A, the heat treatment is performed so that the value of C is 0.5 or more and 0.8 or less, a tensile strength of the metal wire that has been subjected to the heat treatment after the step (d) is E, and an elongation ratio F=E / D is set to be 10 or more and 50 or less.
[0066] [Appendix 4] In Appendix 3, in the (d) step, a heat treatment is performed so that the electrical conductivity of the metal wire immediately after the heat treatment in the (d) step is 86% IACS or more. [Industrial Applicability]
[0067] INDUSTRIAL APPLICABILITY The present invention can be used for copper alloy wires applied to conductors of internal wiring cables (e.g., micro coaxial cables, etc.) for small electronic devices (e.g., digital cameras, surveillance cameras, personal computers, smartphones, etc.) and flexible cables (e.g., endoscope cables, probe cables, etc.) used in industrial robots and medical devices (e.g., gastroscopes, ultrasonic diagnostic devices, etc.). [Explanation of symbols]
[0068] 10 Copper alloy wire 10D Wire diameter 11 Copper alloys 60 Cable 61,74 Sheath (insulator) 70 Electric wire (core wire, coaxial cable) 71 Center conductor 72 Insulators 73 Outer conductor
Claims
1. A copper alloy wire made of a copper alloy, The copper alloy contains 0.3 mass% or more and 0.45 mass% or less of indium and 0.02 mass% or more and less than 0.1 mass% of tin, the total content of the indium and the tin being 0.45 mass% or less, and the balance being copper and unavoidable impurities; The tensile strength is 800 MPa or more, A copper alloy wire having a conductivity of 80% IACS or more.
2. A conductor made of a copper alloy wire; and an insulator covering the conductor. The copper alloy wire is made of a copper alloy having a composition containing 0.3 mass% or more and 0.45 mass% or less of indium and 0.02 mass% or more and less than 0.1 mass% of tin, a total content of the indium and the tin being 0.45 mass% or less, and the remainder being copper and unavoidable impurities; The copper alloy wire has a tensile strength of 800 MPa or more, The electrical conductivity of the copper alloy wire is 80% IACS or more.
3. The electric wire according to claim 2, The conductor is an electric wire formed by twisting together a plurality of the copper alloy wires.
4. A plurality of core wires each including a conductor made of a copper alloy wire and an insulator covering the conductor; a sheath that collectively covers the plurality of core wires; A cable having The copper alloy wire is made of a copper alloy having a composition containing 0.3 mass% or more and 0.45 mass% or less of indium and 0.02 mass% or more and less than 0.1 mass% of tin, a total content of the indium and the tin being 0.45 mass% or less, and the remainder being copper and unavoidable impurities; The copper alloy wire has a tensile strength of 800 MPa or more, A cable, wherein the electrical conductivity of the copper alloy wire is 80% IACS or more.
5. A copper alloy wire and a plating layer provided around the copper alloy wire, The copper alloy wire is made of a copper alloy having a composition containing 0.3 mass% or more and 0.45 mass% or less of indium and 0.02 mass% or more and less than 0.1 mass% of tin, a total content of the indium and the tin being 0.45 mass% or less, and the remainder being copper and unavoidable impurities; A plated wire having a tensile strength of 750 MPa or more, a conductivity of 78% IACS or more, and an elongation of 3% or less.
Citation Information
Patent Citations
Copper alloy wire
JP1993311285A
Conductor for bending resistant cable and production method therefor
JP2002363668A
Copper alloy wire and manufacturing method therefor, copper alloy twist wire and manufacturing method therefor, insulated electric wire using these, coaxial cable and multi-core cable
JP2010018848A
Copper alloy body, its manufacturing method and conductive material
JP2014159609A
Drawn copper wire, method of producing drawn copper wire and cable