Thermoplastic elastomer composition

A thermoplastic elastomer composition with propylene polymer, ethylene polymer, ethylene/α-olefin/non-conjugated diene copolymer, layered silicate, and phenolic resin addresses the lack of scratch resistance in existing compositions, ensuring rubber elasticity and durability in high-temperature applications.

JP7574641B2Active Publication Date: 2024-10-29MITSUBISHI CHEM CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020214861
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-24
Publication Date
2024-10-29
Estimated Expiration
2040-12-24

AI Technical Summary

Technical Problem

Thermoplastic elastomer compositions lack sufficient scratch resistance, which is crucial for applications like anti-slip mats in car interiors where they come into contact with smartphones, leading to potential deterioration in appearance.

Method used

A thermoplastic elastomer composition containing propylene polymer, ethylene polymer, ethylene/α-olefin/non-conjugated diene copolymer, layered silicate, and phenolic resin, dynamically crosslinked to enhance scratch resistance and maintain rubber elasticity at high temperatures.

Benefits of technology

The composition achieves excellent scratch resistance while maintaining rubber elasticity, making it suitable for automobile parts, architectural parts, medical parts, electric wire covering materials, and miscellaneous goods, particularly anti-slip mats.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574641000001
    Figure 0007574641000001
  • Figure 0007574641000002
    Figure 0007574641000002
  • Figure 0007574641000003
    Figure 0007574641000003
Patent Text Reader

Abstract

To provide a thermoplastic elastomer composition having excellent scratch resistance while maintaining rubber elasticity at a high temperature, and a molded article thereof.SOLUTION: The thermoplastic elastomer composition contains the following components (A)-(D), is obtained by dynamic crosslinking in the presence of the following component (E), and may further contain the following component (F): (A) a propylene-based polymer; (B) an ethylenic polymer; (C) an ethylene / α-olefin / nonconjugated diene copolymer rubber; (D) a layered silicate; (E) a phenolic resin; and (F) a hydrocarbon-based rubber softener. The molded article is obtained by molding the thermoplastic elastomer composition.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermoplastic elastomer composition that maintains rubber elasticity at high temperatures and has excellent scratch resistance, and to a molded article thereof. [Background technology]

[0002] Thermoplastic elastomers are materials that soften and become fluid when heated, and have rubber elasticity when cooled. Specifically, when molded, they melt at the processing temperature, and can be easily molded in the same way as known thermoplastic resins, but after molding, at the temperature at which they are actually used as various materials, they have physical properties similar to those of crosslinked rubber. As such, thermoplastic elastomers have the same moldability as thermoplastic resins, a rubbery feel and unique rubber elasticity, and are recyclable, and therefore are widely used in applications such as automobile parts, building parts, medical parts, electric wire coating materials, and miscellaneous goods.

[0003] Such components that take advantage of rubber-like properties are widely used in places where they come into contact with different components through fitting, joining, etc., and are used under conditions where external forces are applied from the different components. In this case, it is important that they have rubber elasticity in the temperature range in which they are used. For example, in the field of automobile parts, rubber elasticity is required in the high temperature range of around 70 degrees due to the environment inside the car. In response to such requirements, crosslinking technology, particularly phenol crosslinking technology, is used as a means of imparting rubber elasticity to thermoplastic elastomer compositions in applications requiring oil and chemical resistance.

[0004] For example, a thermoplastic elastomer composition is known which is obtained by dynamically heat treating a composition containing an olefin copolymer rubber, a hydrogenated diene polymer, a crystalline α-olefin polymer, an ethylene polymer, and a mineral oil-based softener in the presence of a phenolic resin crosslinking agent (see Patent Document 1). Also known is a thermoplastic elastomer composition that contains an ethylene copolymer rubber, an ethylene resin having a specific density polymerized with a single-site catalyst, a phenol resin as a crosslinking agent, and a crosslinking accelerator (see Patent Document 2). Patent Document 2 describes that by blending an ethylene resin polymerized with a single-site catalyst, the compression set of the thermoplastic elastomer composition at high temperatures is improved. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 9-302156 [Patent Document 2] JP 2005-2304 A Summary of the Invention [Problem to be solved by the invention]

[0006] With the recent spread of smartphones, many car interiors are equipped with anti-slip mats to prevent smartphones from dropping while charging, and thermoplastic elastomers with excellent moldability and a rubber-like feel are used as the material for these mats. In such applications, scratch resistance is required to prevent deterioration of the appearance due to contact with the edges of smartphones or charging connectors or scratches caused by human fingernails.

[0007] However, in the thermoplastic elastomer compositions described in Patent Documents 1 and 2, no consideration has been given to scratch resistance, and there is room for improvement in terms of scratch resistance.

[0008] The present invention has been made in consideration of such conventional problems, and an object of the present invention is to provide a thermoplastic elastomer composition that maintains rubber elasticity at high temperatures and also has excellent scratch resistance, and a molded article thereof. [Means for solving the problem]

[0009] As a result of investigations conducted by the present inventors to solve the above-mentioned problems, it was found that the above-mentioned problems can be solved by a thermoplastic elastomer composition comprising component (A): a propylene-based polymer, component (B): an ethylene-based polymer, component (C): an ethylene-α-olefin-non-conjugated diene copolymer rubber, and component (D): a layered silicate, and which is dynamically crosslinked in the presence of component (E): a phenolic resin.

[0010] That is, the gist of the present invention is as follows.

[0011] [1] A thermoplastic elastomer composition comprising the following components (A) to (D) and dynamically crosslinked in the presence of the following component (E): Component (A): Propylene-based polymer Component (B): Ethylene-based polymer Component (C): Ethylene / α-olefin / non-conjugated diene copolymer rubber Component (D): Layered silicate Component (E): Phenolic resin

[0012] [2] The thermoplastic elastomer composition according to [1], wherein the component (B) is contained in an amount of 1 to 99 parts by mass per 100 parts by mass of the total of the components (A) and (B).

[0013] [3] The thermoplastic elastomer composition according to [1] or [2], wherein the component (D) is contained in an amount of 1 to 200 parts by mass per 100 parts by mass of the total of the components (A) and (B).

[0014] [4] The density of the component (B) measured according to JIS K7112 is 0.935 g / cm 3 More than 1.00g / cm 3 The thermoplastic elastomer composition according to any one of the following [1] to [3].

[0015] [5] The thermoplastic elastomer composition according to any one of [1] to [4], further comprising the following component (F): Component (F): Hydrocarbon-based rubber softener

[0016] [6] A molded article obtained by molding the thermoplastic elastomer composition according to any one of [1] to [5]. Effect of the Invention

[0017] The thermoplastic elastomer composition of the present invention has excellent scratch resistance while maintaining rubber elasticity at high temperatures, and is therefore expected to be used in automobile parts, building parts, medical parts, electric wire coating materials, and miscellaneous goods, and is particularly suitable for automobile interior parts. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] The following describes in detail the embodiments of the present invention, but the following description is a representative example of the embodiment of the present invention, and the present invention is not limited to these contents. Note that in the present invention, the symbol "to" is used to mean that the numerical values ​​before and after it are included as the lower limit and upper limit.

[0019] [Thermoplastic elastomer composition] The thermoplastic elastomer composition of the present invention is a thermoplastic elastomer composition which contains the following components (A) to (D) and is dynamically crosslinked in the presence of the following component (E). Component (A): Propylene-based polymer Component (B): Ethylene-based polymer Component (C): Ethylene / α-olefin / non-conjugated diene copolymer rubber Component (D): Layered silicate Component (E): Phenolic resin

[0020] [mechanism] The mechanism by which the thermoplastic elastomer composition of the present invention has scratch resistance while maintaining rubber elasticity at high temperatures is as follows. In the thermoplastic elastomer composition of the present invention, the highly symmetric ethylene-based polymer and the highly rigid layered silicate tend to precipitate on the surface, which is believed to facilitate slipping when in contact with a counter material and to prevent the formation of scratching points. In addition, it is believed that the use of a high-density ethylene-based polymer enhances the rigidity of the thermoplastic elastomer matrix having an island-in-sea structure, and a part of the polymer penetrates into the rubber phase to form a pseudo-crosslinked structure of rubber, thereby exhibiting good rubber elasticity.

[0021] [Component (A)] The propylene polymer of component (A) is a polymer in which the content of monomer units based on propylene (propylene units) relative to all monomer units is more than 50 mass %.

[0022] The type of propylene polymer is not particularly limited, and any of propylene homopolymers, propylene random copolymers, propylene block copolymers, and the like can be used.

[0023] When the propylene-based polymer is a propylene random copolymer, examples of the monomer copolymerized with propylene include ethylene, 1-butene, 2-methylpropylene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, and 1-octene. When the propylene-based polymer is a propylene block copolymer, examples include propylene block copolymers obtained by multi-stage polymerization, more specifically, propylene block copolymers obtained by polymerizing polypropylene in the first stage and polymerizing a propylene-ethylene copolymer in the second stage.

[0024] The content of the propylene unit in the propylene-based polymer is preferably 60% by mass or more, more preferably 75% by mass or more, and even more preferably 90% by mass or more. When the content of the propylene unit is equal to or more than the above lower limit, the heat resistance and rigidity tend to be good. On the other hand, the upper limit of the content of the propylene unit in the propylene-based polymer is not particularly limited, and is usually 100% by mass. The content of the propylene unit in the propylene-based polymer can be determined by infrared spectroscopy.

[0025] The melt flow rate of the propylene polymer (measurement temperature: 230° C., measurement load: 21.18 N) is not limited, but is usually 0.1 g / 10 min or more, and from the viewpoint of moldability, preferably 0.5 g / 10 min or more. The upper limit is usually 100 g / 10 min or less, and from the viewpoint of heat resistance, preferably 30 g / 10 min or less, more preferably 10 g / 10 min or less.

[0026] The melt flow rate (MFR) of the propylene polymer of component (A) is measured in accordance with JIS K7210 (1999) at a measurement temperature of 230° C. and a measurement load of 21.18 N.

[0027] The propylene polymer can be produced by a polymerization method using a known olefin polymerization catalyst. For example, a multi-stage polymerization method using a Ziegler-Natta catalyst can be used. For this multi-stage polymerization method, a slurry polymerization method, a solution polymerization method, a bulk polymerization method, a gas phase polymerization method, etc. can be used, and two or more of these methods can be combined to produce the polymer.

[0028] In addition, the propylene polymer may be a commercially available product. The commercially available propylene polymer may be procured from the manufacturers listed below, and may be appropriately selected. Available commercial products include Novatec® PP from Japan Polypropylene, Prime Polypro® from Prime Polymer, Sumitomo Noblen® from Sumitomo Chemical, polypropylene block copolymer from SunAllomer, Moplen® from LyondellBasell, ExxonMobil PP from ExxonMobil, Formolene® from Formosa Plastics, Borealis PP from Borealis, SEETEC PP from LG Chemical, ASI POLYPROPYLENE from A. Schulman, INEOS PP from INEOS Olefins & Polymers, Braskem PP from Braskem, Samsung Total from SAMSUNG TOTAL PETROCHEMICALS, Sabic® PP from Sabic, TOTAL PETROCHEMICALS Polypropylene from TOTAL PETROCHEMICALS, and YUPLENE® from SK.

[0029] The thermoplastic elastomer composition of the present invention may contain only one type of propylene-based polymer such as a propylene homopolymer, or may contain two or more types of monomer units differing in type, content, physical properties, etc.

[0030] [Component (B)] The ethylene-based polymer of component (B) is a polymer having the highest content of ethylene-based monomer units (ethylene units) among all monomer units. The ethylene-based polymer of component (B) preferably has an ethylene unit content of more than 50 mass%. The ethylene unit content of the ethylene-based polymer can be determined by infrared spectroscopy.

[0031] Examples of the ethylene-based polymer include ethylene homopolymers and ethylene-based copolymers. In the ethylene-based copolymers, examples of the monomers copolymerized with ethylene include at least one of α-olefins having 3 to 10 carbon atoms (e.g., propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, and 1-hexene) and at least one of polar monomers (e.g., vinyl acetate, acrylic esters, and methacrylic esters).

[0032] Preferred examples of the ethylene polymer include high-density polyethylene, low-density polyethylene, and linear low-density polyethylene.

[0033] High density polyethylene has a density of 0.935 g / cm3 measured according to JIS K7112. 3 The high density polyethylene can be produced by a known polymerization method using a Ziegler-Natta catalyst, a metallocene catalyst, or the like as a polymerization catalyst. Examples of the polymerization method include a solution polymerization method, a bulk polymerization method, a slurry polymerization method, and a gas phase polymerization method, and two or more of these methods may be combined.

[0034] Low-density polyethylene is a polymer produced by the high-pressure process, which is a method of radically polymerizing ethylene at high temperature and pressure, and has a density of 0.935 g / cm3 measured according to JIS K7112. 3 It is less than.

[0035] Linear low-density polyethylene is a polymer produced by a low-pressure process and has a density of 0.935 g / cm3 measured according to JIS K7112. 3 It is less than.

[0036] Among these, ethylene polymers have a density of 0.935 g / cm as measured according to JIS K7112. 3 More than 1.00g / cm 3 The following is preferred from the viewpoint of achieving both excellent rubber elasticity and scratch resistance at high temperatures.

[0037] The melt flow rate of the ethylene polymer (measurement temperature: 190° C., measurement load: 21.18 N) is not limited, but is usually 0.1 g / 10 min or more, and from the viewpoint of moldability, preferably 0.5 g / 10 min or more. The upper limit is usually 100 g / 10 min or less, and from the viewpoint of heat resistance, preferably 30 g / 10 min or less, more preferably 15 g / 10 min or less.

[0038] The melt flow rate (MFR) of the ethylene polymer of component (B) is measured in accordance with JIS K7210 (1999) at a measurement temperature of 190° C. and a measurement load of 21.18 N.

[0039] In addition, the ethylene polymer may be a commercially available product. The commercially available ethylene polymer may be procured from the manufacturers listed below, and may be appropriately selected. Commercially available products include Novatec (registered trademark) from Japan Polyethylene Corporation, Sumikathene (registered trademark) from Sumitomo Chemical Co., Ltd., Hi-Zex (registered trademark), Neo-Zex (registered trademark), and Ult-Zex (registered trademark) from Prime Polymer Corporation, UBE Polyethylene (registered trademark) from Ube Maruzen Polyethylene Co., Ltd., Suntec (registered trademark) and Creolex (registered trademark) from Asahi Kasei Corporation, and SABIC (registered trademark) from Saudi Petrochemical Company.

[0040] The thermoplastic elastomer composition of the present invention may contain only one type of ethylene-based polymer, or may contain two or more types of ethylene-based polymers differing in the type, content, physical properties, etc. of the monomer units contained therein.

[0041] [Component (C)] The ethylene-α-olefin-non-conjugated diene copolymer rubber of component (C) is a copolymer containing ethylene, α-olefin, and a non-conjugated diene compound as copolymerization components. Ethylene-α-olefin-non-conjugated diene copolymer rubber includes oil-extended type rubber, which is a mixture of ethylene-α-olefin-non-conjugated diene copolymer rubber and a hydrocarbon-based rubber softener (hereinafter, also referred to as "oil-extended ethylene-α-olefin-non-conjugated diene copolymer rubber"), and non-oil-extended type rubber, which does not contain a hydrocarbon-based rubber softener. In this embodiment, the oil-extended type copolymer rubber is intended, but low-oil-extended type rubber or non-oil-extended type rubber can also be suitably used. That is, in the present invention, the ethylene-α-olefin-non-conjugated diene copolymer rubber of component (C) may be either an oil-extended type or a non-oil-extended type, and either a non-oil-extended type or an oil-extended type may be used alone, or two or more types may be used in any combination and ratio, or one or more types of oil-extended type and one or more types of non-oil-extended type may be used in any combination and ratio. In addition, when component (C) is an oil-extended ethylene-α-olefin-non-conjugated diene copolymer rubber, the hydrocarbon-based rubber softener contained in this oil-extended ethylene-α-olefin-non-conjugated diene copolymer rubber is included in the hydrocarbon-based rubber softener as component (F).

[0042] Examples of the α-olefin in component (C) include α-olefins having 3 to 20 carbon atoms, more preferably 3 to 8 carbon atoms, such as propylene, 1-butene, 3-methyl-1-butene, 1-pentene, 4-methyl-1-pentene, 4,4-dimethyl-1-pentene, 1-hexene, 4-methyl-1-hexene, 1-heptene, 1-octene, 1-decene, and 1-octadecene, but are not particularly limited thereto. Among these, from the viewpoints of crosslinking by the crosslinking agent during dynamic crosslinking and suppression of bloomout, propylene, 1-butene, 3-methyl-1-butene, and 1-pentene are preferred, and propylene and 1-butene are more preferred. The α-olefins can be used alone, or in any combination and ratio of two or more kinds.

[0043] The non-conjugated diene compounds in component (C) include dicyclopentadiene, 1,4-hexadiene, cyclohexadiene, cyclooctadiene, dicyclooctadiene, 1,6-octadiene, 5-methyl-1,4-hexadiene, 3,7-dimethyl-1,6-octadiene, 1,3-cyclopentadiene, 1,4-cyclohexadiene, 2-methyl-1,5-hexadiene, 6-methyl-1,5-heptadiene, Examples of the non-conjugated diene include, but are not limited to, 5-isopropylidene-2-norbornene, 5-vinyl-2-norbornene, vinylidene norbornene, 5-ethylidene-2-norbornene (ENB) and other ethylidene norbornenes, and 5-methylene-2-norbornene (MNB) and other methylene norbornenes. Among these, dicyclopentadiene, ethylidene norbornene, and vinylidene norbornene are preferred, and dicyclopentadiene, 5-ethylidene-2-norbornene, and vinylidene norbornene are more preferred, from the viewpoint of crosslinking properties by the crosslinking agent during dynamic crosslinking. The non-conjugated diene may be used alone or in any combination and ratio of two or more types.

[0044] Specific examples of ethylene-α-olefin-non-conjugated diene copolymer rubber include ethylene-propylene-5-ethylidene-2-norbornene copolymer rubber, ethylene-propylene-dicyclopentadiene copolymer rubber, ethylene-propylene-1,4-hexadiene copolymer rubber, ethylene-propylene-5-vinyl-2-norbornene copolymer rubber, and other ethylene-propylene-non-conjugated diene copolymer rubbers (EPDM), and ethylene-1-butene-5-ethylidene-2-norbornene copolymer rubber, but are not limited thereto. Among these, ethylene-propylene-non-conjugated diene copolymer rubber (EPDM) is preferred from the viewpoint of crosslinking by the crosslinking agent during dynamic crosslinking and suppression of bloomout. The ethylene-α-olefin-non-conjugated diene copolymer rubber can be used alone or in any combination and ratio of two or more kinds.

[0045] The content of ethylene units in the ethylene-α-olefin-non-conjugated diene copolymer rubber is not particularly limited, but is preferably 50 to 90 mass%, more preferably 55 to 85 mass%, and even more preferably 60 to 80 mass%. When the content of ethylene units is within the above preferred range, a thermoplastic elastomer composition having excellent mechanical strength and rubber elasticity tends to be obtained.

[0046] The content of the α-olefin unit in the ethylene-α-olefin-non-conjugated diene copolymer rubber is not particularly limited, but is preferably 9.5 to 49.5 mass%, more preferably 14 to 44 mass%, and even more preferably 18 to 38 mass%. When the content of the α-olefin unit is within the above preferred range, a thermoplastic elastomer composition excellent in mechanical strength, moderate flexibility, and rubber elasticity tends to be obtained.

[0047] Furthermore, the content of the non-conjugated diene unit in the ethylene-α-olefin-non-conjugated diene copolymer rubber is not particularly limited, but is preferably 0.5 to 30 mass%, more preferably 1 to 20 mass%, and even more preferably 2 to 10 mass%. When the content of the non-conjugated diene unit is within the above-mentioned preferred range, it becomes easy to adjust the crosslinkability and moldability, and a thermoplastic elastomer composition having excellent mechanical strength and rubber elasticity tends to be easily obtained.

[0048] The content of each structural unit of component (C) can be determined by infrared spectroscopy.

[0049] In the present invention, as component (C), particularly preferred is an ethylene-propylene-non-conjugated diene copolymer rubber having an ethylene unit content of 55 to 75 mass%, a propylene unit content of 15 to 40 mass%, and a content of at least one non-conjugated diene unit selected from the group consisting of dicyclopentadiene, 5-ethylidene-2-norbornene, and vinylidenenorbornene of 1 to 10 mass%.

[0050] The component (C) can be produced by a polymerization method using a known olefin polymerization catalyst, for example, a slurry polymerization method, a solution polymerization method, a bulk polymerization method, or a gas phase polymerization method using a complex catalyst such as a Ziegler-Natta catalyst, a metallocene complex, or a nonmetallocene complex.

[0051] Among the ethylene-α-olefin-non-conjugated diene copolymer rubbers of component (C) used in the present invention, the Mooney viscosity (ML 1+4 , 125°C) is usually 45 or more, preferably 50 or more. The Mooney viscosity (ML 1+4 , 125° C.) is more preferably 50 to 400, and further preferably 50 to 300. On the other hand, the Mooney viscosity (ML 1+4 , 125° C.) is not particularly limited, but is preferably 30 to 100, and more preferably 35 to 80. When the Mooney viscosity of component (C) is equal to or higher than the lower limit, the compression set is good and it is also preferable from the viewpoint of improving the appearance of the obtained molded article, while when it is equal to or lower than the upper limit, it is preferable from the viewpoint of moldability.

[0052] In the present invention, the Mooney viscosity (ML 1+4 , 125° C.) is expressed by the following formula as described in JP-A-1-103639. Calculation formula: log(ML1 / ML2)=0.0066(ΔPHR) ML1: Mooney viscosity of ethylene-α-olefin-non-conjugated diene copolymer rubber before oil extension ML2: Mooney viscosity of oil-extended ethylene-α-olefin-non-conjugated diene copolymer rubber ΔPHR: Amount of oil extension per 100 parts by mass of ethylene-α-olefin-non-conjugated diene copolymer rubber

[0053] The density of the ethylene-α-olefin-non-conjugated diene copolymer rubber of component (C) is not particularly limited, but is preferably 0.850 g / cm 3 It is preferable that the content is equal to or higher than 0.860 g / cm. 3 or more, while 0.900 g / cm 3 It is preferable that the content is 0.890 g / cm or less, and more preferable that the content is 0.890 g / cm or less. 3 When the density of the ethylene-α-olefin-non-conjugated diene copolymer rubber of component (C) is within the above-mentioned preferred range, a thermoplastic elastomer composition excellent in processability, moldability, flexibility, etc. tends to be obtained. The density can be measured based on JIS K7112:1999.

[0054] As mentioned above, an oil-extended ethylene-α-olefin-conjugated diene copolymer can also be used as component (C). In the oil-extended ethylene-α-olefin-conjugated diene copolymer, the hydrocarbon-based rubber softener is used to soften the ethylene-α-olefin-non-conjugated diene copolymer rubber, increasing its flexibility and elasticity, as well as to improve the processability and flowability of the resulting thermoplastic elastomer composition.

[0055] Examples of the hydrocarbon-based rubber softeners used in the oil-extended ethylene-α-olefin-conjugated diene copolymer rubber include mineral oil-based rubber softeners and synthetic resin-based rubber softeners. Among these, mineral oil-based rubber softeners are preferred from the viewpoint of compatibility with other components. Mineral oil-based rubber softeners are generally mixtures of aromatic hydrocarbons, naphthenic hydrocarbons, and paraffinic hydrocarbons. Softeners with a paraffinic hydrocarbon carbon ratio of 50% or more to the total carbon atoms are called paraffinic oils, naphthenic oils with a naphthenic hydrocarbon carbon ratio of 30-45%, and aromatic oils with a aromatic hydrocarbon carbon ratio of 35% or more. Among these, paraffinic rubber softeners (paraffinic oils) are preferred as the hydrocarbon-based rubber softeners for the oil-extended ethylene-α-olefin-conjugated diene copolymer rubber of component (C). The hydrocarbon-based rubber softeners can be used alone in one type, or in any combination and ratio of two or more types.

[0056] The paraffinic oil used in the oil-extended ethylene-α-olefin-non-conjugated diene copolymer rubber of component (C) is not particularly limited, but has a kinematic viscosity at 40°C of usually 10 cSt (centistokes) or more, preferably 20 cSt or more, and usually 800 cSt or less, preferably 600 cSt or less. In addition, a paraffinic oil having a pour point of usually -40°C or more, preferably -30°C or more, and 0°C or less is preferably used. Furthermore, a paraffinic oil having a flash point (COC) of usually 200°C or more, preferably 220°C or more, and usually 400°C or less, preferably 350°C or less is preferably used.

[0057] When an oil-extended ethylene-α-olefin-non-conjugated diene copolymer rubber is used as component (C), the content ratio of the ethylene-α-olefin-non-conjugated diene copolymer rubber to the hydrocarbon-based rubber softener is not particularly limited, but the content of the hydrocarbon-based rubber softener per 100 parts by mass of the ethylene-α-olefin-non-conjugated diene copolymer rubber is usually 10 parts by mass or more, preferably 20 parts by mass or more, and on the other hand, is usually 200 parts by mass or less, preferably 160 parts by mass or less, and more preferably 120 parts by mass or less.

[0058] The method for preparing the oil-extended ethylene-α-olefin-non-conjugated diene copolymer rubber (oil extension method) is not particularly limited, and a known method can be used. Examples of the oil extension method include a method of mechanically kneading the ethylene-α-olefin-non-conjugated diene copolymer rubber and the hydrocarbon-based rubber softener using a mixing roll or a Banbury mixer to extend the oil, a method of adding a predetermined amount of the hydrocarbon-based rubber softener to the ethylene-α-olefin-non-conjugated diene copolymer rubber and then removing the solvent by a method such as steam stripping, and a method of stirring a mixture of the crumb-like ethylene-α-olefin-non-conjugated diene copolymer rubber and the hydrocarbon-based rubber softener with a Henschel mixer to impregnate the mixture. From the viewpoint of preparing a high molecular weight oil-extended ethylene-α-olefin-non-conjugated diene copolymer rubber, a method of adding a predetermined amount of the hydrocarbon-based rubber softener to the polymerization reaction solution or suspension of the ethylene-α-olefin-non-conjugated diene copolymer rubber of component (C) and then removing the solvent is preferred.

[0059] Incidentally, as the ethylene-α-olefin-non-conjugated diene copolymer rubber of component (C), various grades are commercially available from many manufacturers both in Japan and overseas, and commercial products can be used. Examples of commercial products include JSR EPR manufactured by JSR Corporation, Mitsui EPT manufactured by Mitsui Chemicals, Esprene (registered trademark) manufactured by Sumitomo Chemical Co., Ltd., Keltan (registered trademark) manufactured by ARLANXEO, NORDEL (registered trademark) manufactured by DOW CHEMICAL, and KEP manufactured by KUMHO POLYCHEM.

[0060] [Component (D)] The layered silicate of component (D) is used to improve scratch resistance. The silicate has the effect of increasing surface rigidity, and since the silicate is layered, the area of ​​deposition on the surface is increased, thereby further enhancing this effect.

[0061] Examples of the layered silicate of component (D) include silica, anhydrous silica, quartz, silica gel, calcium silicate, sodium silicate, magnesium silicate (talc, florisil), aluminum silicate (kaolin, kaolinite), sodium aluminosilicate, calcium aluminum silicate, etc., of which magnesium silicate (talc, florisil) and aluminum silicate (kaolin, kaolinite) are preferred, and magnesium silicate (talc, florisil) is particularly preferred.

[0062] The thermoplastic elastomer composition of the present invention may contain only one type of layered silicate, or may contain two or more types.

[0063] [Component (E)] The thermoplastic elastomer composition of the present invention uses a phenolic resin as the propylene component (E). The phenolic resin of component (E) partially crosslinks the above-mentioned component (C) in the resin composition during dynamic heat treatment, thereby realizing a dynamically crosslinked thermoplastic elastomer composition.

[0064] Examples of the phenolic resin of component (E) include non-halogen-based phenolic resins such as alkylphenol formaldehyde, and halogen-based phenolic resins such as brominated alkylphenol formaldehyde. These phenolic resins may be used alone or in combination of two or more.

[0065] As the phenolic resin of component (E), a non-halogen type phenolic resin is particularly preferred, and specifically, one represented by the following formula (I) is preferred.

[0066] [ka]

[0067] (In the formula, X is selected from a divalent linking group, -CH2- or -CH2-O-CH2-, r is an integer of 0 to 20, and R is an organic group having less than 20 carbon atoms, preferably 1 to 12 carbon atoms.)

[0068] Examples of the non-halogenated phenolic resins include Tackirol 201 and 202 (trade names) manufactured by Taoka Chemical Industry Co., Ltd., PR-4507 (trade name) manufactured by Gun-ei Chemical Industry Co., Ltd., Vulkaresat 510E, 532E, Vulkaresen E, 105E, 130E, and Vulkaresol 315E (trade names) manufactured by Hoechst, Amberol ST 137X (trade name) manufactured by Rohm & Haas, SUMILITE RESINS PR-22193 (trade name) manufactured by Sumitomo Durez Co., Ltd., Symphorm-C-100 and C-1001 (trade names) manufactured by Anchor Chem., Tamanol 531 (trade name) manufactured by Arakawa Chemical Industries, Ltd., and Schenectady Chem. Examples of such antibacterial agents include SP1045, SP1059 (trade name), CRR-0803 (trade name) manufactured by UCC Corporation, CRM-0803 (trade name) manufactured by Showa Union Synthetic Co., Ltd., and Vulkadur A (trade name) manufactured by Bayer.

[0069] As the non-halogen-based phenolic resin of component (E), a p-octylphenol formaldehyde resin represented by the following formula (II) is particularly preferably used, and among them, one having a mass average molecular weight of 2,500 to 4,000 is most preferably used. As such a non-halogen-based phenolic resin, those commercially available as the above-mentioned Tackirol (registered trademark) 201 and 202 can be used.

[0070] [ka]

[0071] The phenolic resin is usually used together with an activator. Examples of the activator that can be used here include halogen donors such as stannous chloride, ferric chloride, chlorinated paraffin, chlorinated polyethylene, and chlorosulfonated polyethylene, and acid acceptors such as iron oxide, titanium oxide, magnesium oxide, silicon dioxide, and zinc oxide. When the phenolic resin is halogenated, the halogen donor does not need to be used.

[0072] In addition, some commercially available phenolic resins contain a hydrocarbon-based rubber softener, which corresponds to component (F) described below, or a filler, but when the phenolic resin used contains a hydrocarbon-based rubber softener, the hydrocarbon-based rubber softener is considered to be included in the hydrocarbon-based rubber softener as component (F). The same applies to the filler described below.

[0073] Component (E) may be used in combination with a known crosslinking agent. Examples of known crosslinking agents include organic peroxides, silicon hydride compounds such as methyl hydrogen silicon, sulfur, p-quinone dioxime, p-dinitrosobenzene, and peroxide auxiliaries such as 1,3-diphenylguanidine; polyfunctional vinyl compounds such as divinylbenzene, triallyl cyanurate, triallyl isocyanurate, and diallyl phthalate; polyfunctional (meth)acrylate compounds such as ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, and allyl (meth)acrylate; compounds having a bismaleimide structure such as N,N'-m-phenylene bismaleimide and N,N'-m-toluylene bismaleimide; and trimethylolpropane and trimethylolpropane trimethacrylate.

[0074] [Component (F)] From the viewpoints of increasing flexibility and elasticity as well as improving processability and flowability, the thermoplastic elastomer composition of the present invention preferably contains a hydrocarbon-based rubber softener as component (F). When an oil-extended ethylene-α-olefin-non-conjugated diene copolymer rubber is used as component (C) described above, this component (F) includes the hydrocarbon-based rubber softener contained therein. Even when an oil-extended ethylene-α-olefin-non-conjugated diene copolymer rubber is used as component (C), it is preferable to add a hydrocarbon-based rubber softener as component (F) separately from the oil-extended ethylene-α-olefin-non-conjugated diene copolymer rubber. That is, even when oil-extended ethylene-α-olefin-non-conjugated diene copolymer rubber is used as component (C), by adding a hydrocarbon-based rubber softener as component (F), the content ratio of the hydrocarbon-based rubber softener in component (F) can be adjusted as desired, without depending on the content ratio of the hydrocarbon-based rubber softener in the oil-extended ethylene-α-olefin-non-conjugated diene copolymer rubber. In this case, the separately added hydrocarbon-based rubber softener can be the same as, or of the same kind as, or of a different kind from, the hydrocarbon-based rubber softener in the oil-extended ethylene-α-olefin-non-conjugated diene copolymer rubber of component (C). The same applies when the phenolic resin of component (E) contains a hydrocarbon-based rubber softener.

[0075] The hydrocarbon-based rubber softener to be added separately from component (C) can be the same as the hydrocarbon-based rubber softener used in the oil-extended ethylene-α-olefin-conjugated diene copolymer rubber described above. The hydrocarbon-based rubber softener can be used alone or in any combination and ratio of two or more kinds.

[0076] The paraffinic oil is not particularly limited, but has a kinematic viscosity at 40°C of usually 10 cSt (centistokes) or more, preferably 20 cSt or more, and usually 800 cSt or less, preferably 600 cSt or less. In addition, the pour point is usually -40°C or more, preferably -30°C or more, and 0°C or less, and is preferably used. In addition, the pour point is usually -40°C or more, preferably -30°C or more, and 0°C or less, and is preferably used. Furthermore, the flash point (COC) is usually 200°C or more, preferably 250°C or more, and usually 400°C or less, preferably 350°C or less, and is preferably used.

[0077] The hydrocarbon rubber softener of component (F) may be a commercially available product. Examples of commercially available products of component (F) include the "Nippon Oil Polybutene (registered trademark) HV" series manufactured by JX Nippon Oil & Energy Corporation and the "Diana (registered trademark) Process Oil PW" series manufactured by Idemitsu Kosan Co., Ltd., and any of these may be appropriately selected and used.

[0078] [Content ratio] In the thermoplastic elastomer composition of the present invention, the content of component (B) is preferably 1% by mass or more and less than 99% by mass, and more preferably 10% by mass or more and 90% by mass or less, based on 100% by mass of the total of components (A) and (B). When the content of component (B) is equal to or more than the lower limit, scratch resistance and rubber elasticity at high temperatures are good, which is preferable. When the content of component (B) is equal to or less than the upper limit, moldability is good, which is preferable.

[0079] The thermoplastic elastomer composition of the present invention preferably contains 10 to 600 parts by mass, more preferably 15 to 500 parts by mass, of component (C) per 100 parts by mass of the total of components (A) and (B). When the content of component (C) is equal to or more than the lower limit, the rubber elasticity and moldability at high temperatures are good, which is preferable. When the content of component (C) is equal to or less than the upper limit, the scratch resistance is good, which is preferable.

[0080] The thermoplastic elastomer composition of the present invention preferably contains 1 to 200 parts by mass, more preferably 5 to 150 parts by mass, of component (D) per 100 parts by mass of the total of components (A) and (B). When the content of component (D) is equal to or more than the lower limit, scratch resistance is good, which is preferable. When the content of component (D) is equal to or less than the upper limit, rubber elasticity and moldability at high temperatures are good, which is preferable.

[0081] The thermoplastic elastomer composition of the present invention preferably contains 0.5 to 15 parts by mass of component (E) relative to 100 parts by mass of the total of components (A) and (B). When the content of component (E) is equal to or more than the lower limit, the rubber elasticity is good, which is preferable. When the content of component (E) is equal to or less than the upper limit, the moldability is good, which is preferable.

[0082] When the thermoplastic elastomer composition of the present invention contains component (F), the content of component (F) is preferably 10 parts by mass or more and 1000 parts by mass or less, and more preferably 20 parts by mass or more and 900 parts by mass or less, relative to 100 parts by mass of the total of components (A) and (B). When the content of component (F) is equal to or more than the lower limit, the moldability and rubber elasticity are good, which is preferable. When the content of component (F) is equal to or less than the upper limit, the oil-bleed resistance is good, which is preferable. In addition, the content of component (F) here means, when an oil-extended ethylene-α-olefin-non-conjugated diene copolymer rubber is used as component (C), the total content of the hydrocarbon-based rubber softener in component (C) and the hydrocarbon-based rubber softener as component (F) which is added separately from component (C); when a hydrocarbon-based rubber softener is contained in component (E), the content means the total content including said hydrocarbon-based rubber softener.

[0083] [Other ingredients] In addition to the components (A) to (F), other components may be blended into the thermoplastic elastomer composition of the present invention, if necessary, within the range that does not impair the effects of the present invention.

[0084] Examples of other components include thermoplastic resins and elastomers other than the components (A) to (C), antioxidants, fillers other than the component (D), heat stabilizers, light stabilizers, UV absorbers, neutralizers, lubricants, antifogging agents, antiblocking agents, slip agents, dispersants, colorants, flame retardants, antistatic agents, conductivity imparting agents, metal deactivators, molecular weight regulators, antibacterial agents, antifungal agents, fluorescent whitening agents, and other various additives, which may be blended within the range that does not impair the effects of the present invention. Any of these may be used alone or in combination.

[0085] Examples of thermoplastic resins other than components (A) to (C) include polyphenylene ether resins, polyamide resins such as nylon 6 and nylon 66, polyester resins such as polyethylene terephthalate and polybutylene terephthalate, polyoxymethylene resins such as polyoxymethylene homopolymers and polyoxymethylene copolymers, polymethyl methacrylate resins, and polyolefin resins (excluding those corresponding to components (A) and (B)). Examples of elastomers other than components (A) to (C) include polyester elastomers and polybutadiene.

[0086] Examples of the antioxidant include phenol-based antioxidants, phosphite-based antioxidants, and thioether-based antioxidants. When an antioxidant is used, it is usually used in the range of 0.01 to 3.0 parts by mass per 100 parts by mass of the total of component (A) and component (B).

[0087] Examples of fillers other than component (D) include zeolite, glass fiber, hollow glass spheres, carbon fiber, calcium carbonate, potassium titanate fiber, metal soap, titanium dioxide, and carbon black. When a filler is used, it is usually used in an amount of 0.1 to 50 parts by mass per 100 parts by mass of the total of components (A) and (B).

[0088] Examples of the lubricant include fatty acid amides, fatty acid metal salts, and organopolysiloxanes. When a lubricant is used, it is usually used in the range of 0.01 to 10.0 parts by mass per 100 parts by mass of the total of components (A) and (B).

[0089] [Method of producing thermoplastic elastomer composition] As described above, the thermoplastic elastomer composition of the present invention is produced by dynamically heat treating a composition containing components (A), (B), (C) and (D), preferably further component (F), and predetermined amounts of other components used as necessary, in the presence of component (E).

[0090] In the present invention, "dynamic heat treatment" means kneading in a molten or semi-molten state in the presence of a crosslinking agent. This dynamic heat treatment is preferably performed by melt kneading, and as a melt kneading device for this purpose, for example, a non-open type Banbury mixer, a mixing roll, a kneader, or a twin-screw extruder is used. Among these, it is preferable to use a twin-screw extruder. In a preferred embodiment of the production method using this twin-screw extruder, each component is supplied to a raw material supply port (hopper) of a twin-screw extruder having multiple raw material supply ports, and dynamic heat treatment is performed.

[0091] The temperature when the dynamic heat treatment is carried out is usually 80 to 300° C., and preferably 100 to 250° C. The time for which the dynamic heat treatment is carried out is usually 0.1 to 30 minutes.

[0092] When the thermoplastic elastomer composition of the present invention is produced by subjecting it to dynamic heat treatment using a twin-screw extruder, it is preferable to extrude the composition while maintaining the relationship represented by the following formula (i) among the barrel radius (R (mm)), screw rotation speed (N (rpm)), and discharge rate (Q (kg / hour)) of the twin-screw extruder, and it is more preferable to extrude the composition while maintaining the relationship represented by the following formula (ii). 2.6 <NQ / R 3 <22.6 (i) 3.0 <NQ / R 3 <20.0 (ii)

[0093] In order to efficiently produce a thermoplastic elastomer composition, it is preferable that the above relationship between the barrel radius (R (mm)), the screw rotation speed (N (rpm)), and the discharge rate (Q (kg / hour)) of the twin-screw extruder is larger than the above lower limit value. On the other hand, it is preferable that the above relationship is smaller than the above upper limit value in order to suppress heat generation due to shear and suppress the generation of foreign matter that causes a defective appearance.

[0094] In producing the thermoplastic elastomer composition of the present invention, the ethylene-α-olefin-non-conjugated diene copolymer rubber of component (B) can also be treated with at least a portion of the hydrocarbon-based rubber softener of component (F) to use component (B) as an oil-extended ethylene-α-olefin-non-conjugated diene copolymer rubber.

[0095] As a method for producing the oil-extended ethylene-α-olefin-non-conjugated diene copolymer rubber from components (B) and (F) (oil extension method), a method similar to the method for preparing the oil-extended ethylene-α-olefin-non-conjugated diene copolymer rubber described above can be used.

[0096] [Physical properties of thermoplastic elastomer composition] The molded article obtained by molding the thermoplastic elastomer composition of the present invention preferably has a Duro hardness A (value after 15 seconds) measured in accordance with JIS K6253 (2006 edition) (Duro-A) of 95 or less, more preferably in the range of 20 to 90, and even more preferably in the range of 25 to 85. When the Duro hardness A is equal to or more than the lower limit, scratch resistance is good, which is preferable. When the Duro hardness A is equal to or less than the upper limit, rubber elasticity at high temperatures is good, which is preferable.

[0097] Furthermore, the molded article obtained by molding the thermoplastic elastomer composition of the present invention has a compression set of preferably 50% or less, more preferably 45% or less, measured at 70°C for 22 hours under 25% compression conditions in accordance with JIS K6262. If the compression set is equal to or less than the upper limit, the rubber elasticity at high temperatures is good, which is preferable.

[0098] [Molded objects / Applications] The thermoplastic elastomer composition of the present invention can be molded into a molded article by various molding methods generally used for thermoplastic elastomer compositions, such as injection molding, extrusion molding, blow molding, compression molding, etc. Among these, injection molding and extrusion molding are preferred. In addition, the composition can be molded into a molded article by carrying out secondary processing such as lamination molding and thermoforming after the above molding.

[0099] The thermoplastic elastomer composition of the present invention has excellent scratch resistance while maintaining rubber elasticity at high temperatures, and can be used in a wide range of fields, such as automobile parts (mats, seals, cushions, boots, etc.), building parts (gaskets, packings, mats, etc.), various other miscellaneous parts, sporting goods (golf club and tennis racket grips, etc.), industrial parts (hose tubes, gaskets, etc.), home appliance parts (hoses, packings, etc.), medical parts (medical containers, gaskets, packings, etc.), food parts (containers, packings, etc.), medical equipment parts, electric wires, and other miscellaneous goods. Among them, it is preferable to use a molded article made of the thermoplastic elastomer composition of the present invention as an anti-slip mat. EXAMPLES

[0100] The present invention will be described in more detail below using examples, but the present invention is not limited to the following examples as long as it does not exceed the gist of the invention. The values ​​of various production conditions and evaluation results in the following examples are meant as preferred upper or lower limit values ​​in the embodiment of the present invention, and the preferred range may be a range defined by a combination of the above-mentioned upper or lower limit values ​​and the values ​​of the following examples or values ​​between the examples.

[0101] [raw materials] The raw materials used in the following Examples and Comparative Examples are as follows.

[0102] <Component (A)> (A-1): Propylene homopolymer / Novatec (registered trademark) PP FY6 manufactured by Japan Polypropylene Corporation Propylene unit content: 100% by mass MFR (230℃, 21.18N): 2.5g / 10min

[0103] <Ingredient (B)> (B-1): High density polyethylene / Novatec (registered trademark) HD ​​HJ580N manufactured by Japan Polyethylene Co., Ltd. Density: 0.960g / cm 3 MFR (190℃, 21.18N): 12g / 10min (B-2): Linear low-density polyethylene / Saudi Petrochemical Company SABIC (registered trademark) LLDPE M200024 Density: 0.924g / cm 3 MFR (190℃, 21.18N): 20g / 10min (B-3): Low-density polyethylene / Novatec (registered trademark) LD LF405 manufactured by Japan Polyethylene Co., Ltd. Density: 0.919g / cm 3 MFR (190℃, 21.18N): 2g / 10min

[0104] <Component (C)> (C-1) + (F) mixture: oil-extended ethylene-propylene-5-ethylidene-2-norbornene copolymer (a mixture of 100 parts by mass of component (C-1) and 40 parts by mass of component (F)) / 3072EPM manufactured by Mitsui Chemicals, Inc. Mooney Viscosity ML 1+4 (125℃):51 Component (C-1): Ethylene-propylene-5-ethylidene-2-norbornene copolymer Mooney Viscosity ML 1+4 (125℃):94 Ethylene unit content: 64% by mass 5-Ethylidene-2-norbornene unit content: 5.4% by mass Density: 0.88g / cm 3

[0105] <Ingredient (D)> (D-1): Magnesium silicate filler (talc) / Takehara Chemical Industry Co., Ltd. PHSH, layered (D-2): Aluminum silicate filler (kaolin) / Satintone (registered trademark) SP-33, layered, manufactured by BASF Japan Ltd.

[0106] <Ingredient (E)> (E-1) + (F-1) mixture: phenolic resin (mixture of 30 parts by mass of component (E-1) and 70 parts by mass of component (F-1) (E-1): Alkylphenol formaldehyde resin having methylol groups at both ends / Tackirol (registered trademark) 201 manufactured by Taoka Chemical Co., Ltd. (F-1): Paraffin-based oil / Idemitsu Kosan Co., Ltd. Diana (registered trademark) Process Oil PW-32 Kinematic viscosity at 40℃: 30.60cSt Pour point: -17.5℃ Flash point: 222℃

[0107] <Component (F)> (F-1): Paraffin-based oil / Idemitsu Kosan Co., Ltd. Diana (registered trademark) Process Oil PW-32 Kinematic viscosity at 40℃: 30.60cSt Pour point: -17.5℃ Flash point: 222℃ (F-2): Paraffin-based oil / Idemitsu Kosan Co., Ltd. Diana (registered trademark) Process Oil PW-90 Kinematic viscosity at 40℃: 95.54cSt Pour point: -15℃ Flash point: 272℃

[0108] <Ingredient (e)> (e-1): A mixture of 40% by mass of 2,5-dimethyl-2,5-di(t-butylperoxy)hexane (organic peroxide) and 60% by mass of calcium carbonate / Trigonox (registered trademark) 101-40C manufactured by Nouryon Chemical Co., Ltd. (e-2): A mixture of 57% by mass of divinylbenzene, 40% by mass of ethylvinylbenzene, and 3% by mass of diethylbenzene / DVB-570 manufactured by Nippon Steel Chemical & Material Co., Ltd.

[0109] <Ingredients (G)> (G-1): Halogen donor / Stannic chloride manufactured by Wako Pure Chemical Industries, Ltd.

[0110] <Ingredients (H)> (H-1): Acid acceptor / Zinc oxide manufactured by Wako Pure Chemical Industries, Ltd.

[0111] <Component (I)> (I-1): Antioxidant / BASF Japan Ltd. Irganox (registered trademark) 1076

[0112] [Evaluation method] The thermoplastic elastomer compositions in the following Examples and Comparative Examples were evaluated as follows. In the measurements of (1) to (4) below, each thermoplastic elastomer composition was injection molded using an in-line screw type injection molding machine ("IS130" manufactured by Toshiba Machine Co., Ltd.) under conditions of an injection pressure of 50 MPa, a cylinder temperature of 220°C, and a mold temperature of 40°C to obtain a sheet having a thickness of 2 mm x width of 120 mm x length of 120 mm. In the measurement of compression set in (4), a test piece was prepared by stacking six Type A disks (29 mmφ) obtained by punching out the obtained sheet (thickness of 2 mm x width of 120 mm x length of 120 mm) in accordance with JIS K6262, and the measurement was performed using this test piece.

[0113] (1) Bleeding resistance The above test pieces were left to stand for 168 hours under conditions of a temperature of 23±2°C and a humidity of 50±5% Rh, after which the appearance was observed and the degree of oil bleeding was evaluated according to the following three-level scale. ◎: No bleeding 〇: Some bleeding ×: Bleeding occurs over the entire sheet

[0114] (2) Scratch resistance The surface of the test piece was scratched with a Taber scratch tester manufactured by Toyo Seiki Co., Ltd. The specimen was scratched with a stainless steel carbide cutter at a specified load. The surface was visually observed to confirm the load at which a wedge began to form on the surface. It was determined that the higher the load, the higher the scratch resistance.

[0115] (3) Durohardness A The hardness (after 15 seconds) was measured in accordance with JIS K6253 (Duro-A).

[0116] (4) Compression set In accordance with the JIS K6262 standard, measurements were taken at 70°C for 22 hours at 25% compression. The lower the value, the better the rubber elasticity.

[0117] [Examples / Comparative Examples] <Example 1> 50 parts by mass of component (A-1), 50 parts by mass of component (B-1), 206 parts by mass of a mixture of components (C-1) and (F) (breakdown: 147 parts by mass of component (C-1), 59 parts by mass of (F)), 17 parts by mass of component (D-1), 2.1 parts by mass of component (G-1), 1.0 part by mass of component (H-1), and 0.4 parts by mass of component (I-1) were blended for 1 minute using a Henschel mixer. The mixture was fed into the upstream feed port of a unidirectional twin-screw extruder (Japan Steel Works "TEX30", L / D=52.5, number of cylinder blocks: 14) using a gravimetric feeder. Next, 21 parts by mass of the mixture of components (E-1) + (F-1) (breakdown: components (E-1): 6.3 parts by mass, (F-1): 14.7 parts by mass) and 110 parts by mass of component (F-2) were each fed from a feed port in the middle of the extruder using a liquid addition pump, and the temperature was raised from the upstream to downstream in the range of 140 to 200 ° C. at a total discharge rate of 20 kg / h to carry out a dynamic crosslinking treatment, and the mixture was pelletized to produce a thermoplastic elastomer composition. The obtained thermoplastic elastomer composition was evaluated in the above-mentioned (1) to (4). The obtained evaluation results are shown in Table 1.

[0118] <Examples 2 to 4 and Comparative Examples 1 to 4> In Examples 2 to 4 and Comparative Examples 1 to 3, pellets of thermoplastic elastomer composition were obtained in the same manner as in Example 1, except that the blending compositions of the components other than the components (G-1), (H-1), and (I-1) were changed as shown in Table 1. In Comparative Example 4, pellets of a thermoplastic elastomer composition were obtained in the same manner as in Example 1, except that components (G-1) and (H-1) were not blended and the blending composition of components other than component (I-1) was changed as shown in Table 1. The obtained thermoplastic elastomer composition was subjected to the same evaluation as in Example 1. The obtained evaluation results are shown in Table 1.

[0119] [Table 1]

[0120] [Evaluation Results] As shown in Table 1, Examples 1 to 4 have sufficient bleeding resistance, compression set (high-temperature rubber elasticity), and good scratch resistance for practical use. In particular, Examples 1 and 4 show good rubber elasticity. On the other hand, Comparative Examples 1 to 3 are examples that do not contain either or both of component (B): ethylene polymer and component (D): layered silicate, but the scratch resistance deteriorates. Comparative Example 4 is an example that uses a mixture of component (e-1) organic peroxide and component (e-2) divinylbenzene instead of component (E): phenol resin, but the bleeding resistance deteriorates, and the evaluations of (2) to (4) cannot be performed, making it unsuitable for practical use. [Industrial Applicability]

[0121] The thermoplastic elastomer composition of the present invention has excellent scratch resistance while maintaining rubber elasticity at high temperatures. The thermoplastic elastomer composition of the present invention has scratch resistance while maintaining rubber elasticity at high temperatures, and is therefore useful for automobile parts, building parts, medical parts, electric wire coating materials, miscellaneous goods, particularly anti-slip mats, etc.

Claims

1. A thermoplastic elastomer composition comprising the following components (A) to (D) and dynamically crosslinked in the presence of the following component (E), wherein the density of the component (B) measured in accordance with JIS K7112 is 0.935 g / cm 3 or more and 1.00 g / cm 3 or less. Component (A): Propylene-based polymer Component (B): Ethylene-based polymer Component (C): Ethylene / α-olefin / non-conjugated diene copolymer rubber Component (D): Layered silicate Component (E): Phenolic resin

2. The thermoplastic elastomer composition according to claim 1, wherein the component (B) is contained in an amount of 1 to 99 parts by mass per 100 parts by mass of the total of the components (A) and (B).

3. The thermoplastic elastomer composition according to claim 1 or 2, wherein the component (D) is contained in an amount of 1 to 200 parts by mass per 100 parts by mass of the total of the components (A) and (B).

4. The thermoplastic elastomer composition according to any one of claims 1 to 3, further comprising the following component (F): Component (F): Hydrocarbon-based rubber softener

5. A molded article obtained by molding the thermoplastic elastomer composition according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Thermoplastic elastomer composition

    JP1997302156A

  • Thermoplastic elastomer composition

    JP2005002304A

  • Thermoplastic vulcanizates containing ethylene / α-olefin copolymers

    JP2008540696A

  • Microcellular foam of thermoplastic vulcanizate

    JP2009511662A

  • Bellows-like molding composed of thermoplastic elastomer composition

    JP2019127543A