Propylene-based resin composition and film using same

A tailored propylene-based resin composition with specific components addresses blocking issues in high-temperature, high-humidity environments, ensuring flexibility, transparency, and resistance to film adhesion, enhancing manufacturing stability.

JP7574684B2Active Publication Date: 2024-10-29JAPAN POLYPROPYLENE CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021020122
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-10
Publication Date
2024-10-29
Estimated Expiration
2041-02-10

AI Technical Summary

Technical Problem

Propylene-based resin films used in retorts and high-temperature, high-humidity sterilization processes face issues with blocking resistance, leading to manufacturing process interruptions due to films adhering to each other under these conditions.

Method used

A propylene-based resin composition comprising specific proportions of propylene resin, ethylene-α-olefin copolymer, propylene homopolymer, and propylene homopolymer, optimized for flexibility, transparency, and low-temperature impact resistance, with controlled melt flow rates and crystallinity to prevent blocking.

Benefits of technology

The composition maintains excellent flexibility and transparency while effectively suppressing the blocking phenomenon during high-temperature heat treatment, ensuring stable film formation and improved manufacturing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574684000001
    Figure 0007574684000001
  • Figure 0007574684000002
    Figure 0007574684000002
  • Figure 0007574684000003
    Figure 0007574684000003
Patent Text Reader

Abstract

To provide a propylene-based resin composition that is excellent in inhibitory effect to a blocking phenomenon occurring in high-temperature heating processing while maintaining excellent flexibility, transparency, and low-temperature impact resistance, and to provide a film made of the same.SOLUTION: A propylene-based resin composition contains a propylene-based resin (A) satisfying conditions (A-i)-(A-iii) of 35-89 wt.%, an ethylene-α-olefin copolymer (B) satisfying conditions (B-i)-(B-ii) of 10-35 wt.%, a propylene homopolymer (C) satisfying conditions (C-i)-(C-ii) of 0-15 wt.%, and a propylene homopolymer (D) satisfying conditions (D-i)-(D-ii) of 1-15 wt.% (where, the sum total of the propylene-based resin (A), the ethylene-α-olefin copolymer (B), the propylene homopolymer (C), and the propylene homopolymer (D) is 100 wt.%.).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a propylene-based resin composition and a film using the same. More specifically, the present invention relates to a propylene-based resin composition which is excellent in flexibility, transparency and low-temperature impact resistance and has an excellent effect of suppressing a blocking phenomenon that occurs during high-temperature heat treatment, and therefore is capable of giving a film having excellent strength and appearance, and a film using the same. [Background technology]

[0002] Films obtained from propylene-based resins have excellent heat resistance and optical properties such as flexibility, transparency, and gloss, and are therefore widely used as various packaging films and containers. However, in recent years, there have been efforts to expand their use to the fields of retort and high-temperature and high-humidity (high-pressure steam) sterilization, which require blocking resistance in addition to these properties. In response to these demands, the applicant has previously invented and filed applications for a propylene-based resin composition characterized by containing a specific propylene-ethylene random copolymer component obtained by sequential polymerization, an ethylene-α-olefin copolymer having a specific density and MFR, and a propylene-based (co)polymer having a specific melting peak temperature in a specific ratio, the propylene-based resin composition having excellent flexibility, transparency, and strength (drop resistance and low-temperature impact resistance), excellent moldability such as reduced appearance defects such as interface roughness and thickness variation during multi-layer molding, and excellent suppression effect against the phenomenon of molten resin flow and thinning during secondary processing such as heat sealing (see, for example, Patent Document 1).

[0003] However, it has been found that when a bag made from the obtained film of the propylene-based resin composition is subsequently used in a retort or high-temperature, high-humidity sterilization process, the propylene-based resin composition gives rise to a problem that blocking resistance is difficult to exhibit.

[0004] This problem is particularly prevalent in areas such as retort and high-temperature, high-humidity sterilization. When stacking products and subjecting them to high-temperature, high-humidity treatment, the bags can block each other, causing the manufacturing process to stop. Thus, there is currently a demand for a film which does not suffer from the above-mentioned problems even under high temperature and high humidity processing conditions. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2010-138211 A Summary of the Invention [Problem to be solved by the invention]

[0006] In order to obtain a film made of a propylene-based resin composition that is excellent in flexibility, transparency, and low-temperature impact resistance, and has excellent moldability such as poor appearance such as interface roughness and thickness variation during multilayer molding, and also has a sufficient effect of suppressing the phenomenon of molten resin flowing and thinning during secondary processing such as heat sealing, it is effective to use a propylene-based resin containing a specific propylene-ethylene random copolymer component obtained by sequential polymerization, an ethylene-α-olefin copolymer having a specific density and MFR, and a propylene-based (co)polymer having a specific melting peak temperature. However, when a film containing the propylene-based (co)polymer is stacked and subjected to high-temperature and high-humidity treatment, the bags are blocked from each other. Therefore, an object of the present invention is to provide a propylene-based resin composition which has an excellent effect of suppressing the blocking phenomenon that occurs during high-temperature heat treatment while maintaining excellent flexibility, transparency and low-temperature impact resistance, and a film using the same. [Means for solving the problem]

[0007] The present inventors have carried out various studies and analyses to solve the above problems, and have found that these problems are due to the fact that the propylene-based resin composition has an extremely small amount of low MFR and highly crystalline components, and therefore, when the composition is molded into a film, a film with a high surface roughness cannot be molded, and when the composition is subjected to high temperature and high humidity treatment, blocking occurs between the films. The inventors have found that low MFR and highly crystalline components are necessary to solve this problem. On the other hand, the inventors have found that the addition of a specific ethylene-α-olefin copolymer to impart flexibility can maintain a balance between transparency and flexibility, since the addition of a highly crystalline component impairs flexibility, and have arrived at the present invention.

[0008] That is, according to the first aspect of the present invention, there is provided a propylene-based resin composition comprising 35 to 89% by weight of a propylene-based resin (A) satisfying the following conditions (Ai) to (A-iii), 10 to 35% by weight of an ethylene-α-olefin copolymer (B) satisfying the following conditions (Bi) to (B-ii), 0 to 15% by weight of a propylene homopolymer (C) satisfying the following conditions (Ci) to (C-ii), and 1 to 15% by weight of a propylene homopolymer (D) satisfying the following conditions (Di) to (D-ii) (wherein the total of the propylene-based resin (A), the ethylene-α-olefin copolymer (B), the propylene homopolymer (C) and the propylene homopolymer (D) is taken as 100% by weight). (A) Propylene-based resin (Ai) A metallocene-based propylene-α-olefin block copolymer (A) which is a multistage polymer comprising 50 to 60% by weight of a propylene-α-olefin random copolymer component (A1) having a melting peak temperature Tm (A1) of 125 to 135°C in a DSC measurement and an α-olefin content E (A1) of 1.5 to 3.0% by weight, and 50 to 40% by weight of a propylene-ethylene random copolymer component (A2) having an ethylene content E (A2) of 8 to 14% by weight. (A-ii) The melt flow rate (MFR(A): 230°C, 2.16 kg) is in the range of 4 to 10 g / 10 min. (A-iii) In a temperature-loss tangent (tan δ) curve obtained by solid-state viscoelastic measurement (DMA), the peak of the tan δ curve representing the glass transition observed in the range of -60 to 20°C shows a single peak at or below 0°C. (B) Ethylene-α-olefin copolymer (Bi) Density 0.860~0.900g / cm 3 The range is as follows. (B-ii) The melt flow rate (MFR(B): 190°C, 2.16 kg) is 2.0 g / 10 min or more. (C) Propylene homopolymer (Ci) The melt flow rate (MFR(C): 230°C, 2.16 kg) is in the range of 1.9 to 100 g / 10 min. (C-ii) Having no long chain branches. (D) Propylene homopolymer (Di) The melt flow rate (MFR(D): 230°C, 2.16 kg) is in the range of 0.1 to 15 g / 10 min. (D-ii) Having long chain branches.

[0009] According to a second aspect of the present invention, there is provided a propylene-based resin composition according to the first aspect, characterized in that the propylene homopolymer (C) and the propylene homopolymer (D) further satisfy a melt flow rate ratio (MFR(C) / MFR(D)) of 1 to 100. According to a third aspect of the present invention, there is provided a film comprising the propylene-based resin composition according to the first or second aspect of the present invention. Effect of the Invention

[0010] A basic requirement for the propylene-based resin composition of the present invention and the film using the same is that a specific propylene-based resin (A), a specific ethylene-α-olefin copolymer (B), a specific propylene homopolymer (C) and a specific propylene homopolymer (D) are used in specific ratios. The propylene-based resin (A) is a propylene-ethylene block copolymer obtained using a metallocene catalyst, and is the main component of the propylene-based resin composition of the present invention, which can impart a good balance of transparency and flexibility to the resulting film. The propylene-based resin (A) is a propylene-ethylene block copolymer (A) obtained by sequentially polymerizing in a first step a propylene-ethylene random copolymer component (A1) that exhibits a melting peak temperature in a specific range controlled by the ethylene content, and in a second step a propylene-ethylene random copolymer component (A2) that has a specific ethylene content and is therefore highly flexible, and that does not deteriorate transparency and is specified as not forming a phase separation structure by exhibiting a single peak of glass transition temperature of 0°C or lower, as observed as a peak in a tan δ curve in the range of -60 to 20°C in solid viscoelasticity measurement. The ethylene-α-olefin copolymer (B) is specified by its density and melt flow rate, and can impart flexibility to the resulting film without impairing transparency. The propylene homopolymer (C) has a melt flow rate (MFR(C): 230°C, 2.16 kg) in the range of 1.9 to 100 g / 10 min and does not have long chain branches, so that it can impart flowability control properties during film molding. The propylene homopolymer (D) has a melt flow rate (MFR(D): 230°C, 2.16 kg) in the range of 0.5 to 15 g / 10 min and has long chain branches, so that it can impart a function of increasing the surface roughness of the film during film formation.

[0011] Therefore, the propylene-based resin composition of the present invention has excellent flexibility, transparency, and low-temperature impact resistance, and also has an excellent effect of suppressing the blocking phenomenon that occurs during high-temperature heat treatment, and can therefore be suitably used as a film having excellent strength and appearance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention relates to a propylene-based resin composition containing a propylene-based resin (A), an ethylene-α-olefin copolymer (B), a propylene homopolymer (C) and a propylene homopolymer (D), and a film obtained therefrom. The components of the propylene-based resin composition of the present invention, a method for producing the propylene-based resin composition, and the film will be described in detail below.

[0013] [I] Constituents of propylene-based resin composition 1. Propylene-based resin (A) The propylene-based resin (A) (hereinafter, sometimes referred to as component (A)) used as the main component of the propylene-based resin composition of the present invention is required to have high transparency, flexibility, and impact resistance. In order to meet these requirements at a high level, the component (A) is required to satisfy the following requirements (Ai) to (A-iii). Characteristics of component (A) (Ai) Basic provisions The component (A) used in the present invention is a metallocene-based propylene-α-olefin block copolymer (A), which is a multistage polymer produced using a metallocene catalyst and which comprises 50 to 60% by weight of a propylene-α-olefin random copolymer component (A1) having a melting peak temperature Tm (A1) of 125 to 135°C in a DSC measurement and an α-olefin content E (A1) of 1.5 to 3.0% by weight, and 50 to 40% by weight of a propylene-ethylene random copolymer component (A2) having an ethylene content E (A2) of 8 to 14% by weight.

[0014] (i) Melting peak temperature Tm(A1) of component (A1) The component (A1) produced in the first step is a component that determines the crystallinity of the component (A) used in the present invention. In order to improve the heat resistance of the component (A), it is necessary that the melting peak temperature Tm(A1) (hereinafter, sometimes referred to as Tm(A1)) of the component (A1) is high. When Tm(A1) is 135°C or less, the flexibility and transparency are good. When Tm(A1) is 125°C or more, the heat resistance is good and thinning during heat sealing is suppressed. Tm(A1) must be in the range of 125 to 135°C, and is preferably 128 to 133°C. Here, the melting peak temperature Tm is a value determined by a differential scanning calorimeter (DSC manufactured by Seiko Instruments Inc.), and specifically, the melting peak temperature Tm is determined as a value obtained by taking a 5.0 mg sample, holding it at 200°C for 5 minutes, crystallizing it to 40°C at a temperature drop rate of 10°C / min, and then melting it at a temperature increase rate of 10°C / min.

[0015] (ii) Ethylene content E(A1) of component (A1) The melting peak temperature Tm(A1) of component (A1) is controlled by the ethylene content, and the ethylene content E(A1) (hereinafter sometimes referred to as E(A1)) of component (A1) in the present invention is in the range of 1.5 to 3.0% by weight. When E(A1) is 1.5% by weight or more, Tm(A1) is low and flexibility and transparency are good, and when it is 3.0% by weight or less, Tm(A1) is high and thinning during heat sealing is suppressed.

[0016] (iii) Proportion of component (A1) in component (A) The proportion of component (A1) in component (A), W(A1), is a component that imparts heat resistance to component (A), and when W(A1) is 60% by weight or less, flexibility, impact resistance, and transparency can be sufficiently exhibited, so the proportion of component (A1) needs to be 60% by weight or less. On the other hand, when the proportion of component (A1) is 50% by weight or more, Tm(A1) is sufficient, heat resistance is improved, and thinning during heat sealing is suppressed, so the proportion of component (A1) must be 50% by weight or more.

[0017] (iv) Ethylene content E(A2) in component (A2) The component (A2) produced in the second step is a component necessary for improving the flexibility, impact resistance, and transparency of the component (A). In general, as the ethylene content in a propylene-ethylene random copolymer increases, the crystallinity decreases and the effect of improving flexibility increases, so the ethylene content E(A2) (hereinafter sometimes referred to as E(A2)) in the component (A2) must be 8% by weight or more. When E(A2) is 8% by weight or more, sufficient flexibility can be exhibited, and it is preferably 10% by weight or more. On the other hand, if E(A2) is 14% by weight or less in order to reduce the crystallinity of component (A2), the compatibility is improved and no phase separation structure is formed. If E(A2) is increased too much, the compatibility between component (A1) and component (A2) is reduced, and component (A2) is not compatible with component (A1) and forms a domain. In such a phase separation structure, if the refractive index of the matrix and the domain differs, the transparency is rapidly reduced. Therefore, E(A2) of component (A2) in component (A) used in the present invention must be 14% by weight or less, and is preferably 12% by weight or less.

[0018] (v) Proportion of component (A2) in component (A) When the proportion W(A2) of component (A2) in component (A) is 50% by weight or less, heat resistance is improved, so W(A2) needs to be kept at 50% by weight or less. On the other hand, when W(A2) is 40% by weight or more, the effect of improving flexibility and impact resistance is obtained, so that W(A2) must be 40% by weight or more.

[0019] Here, W(A1) and W(A2) are values ​​determined by temperature-rising elution fractionation (TREF), and the ethylene contents E(A1) and E(A2) are 13 This value is determined by C-NMR. Specifically, the method is as follows. Identification of W(A1) and W(A2) by temperature-rising elution fractionation (TREF) The method of evaluating the crystallinity distribution of propylene-ethylene random copolymers by temperature-rising elution fractionation (TREF) is well known to those skilled in the art, and detailed measurement methods are described, for example, in the following literature. ·G.Glockner,J.Appl.Polym.Sci.:Appl.Polym.Symp.;45,1-24(1990) ·L.Wild,Adv.Polym.Sci.;98,1-47(1990) ·JBPSoares,AE Hamielec,Polymer;36,8,1639-1654(1995)

[0020] The component (A) used in the present invention has a large difference in crystallinity between the components (A1) and (A2). In addition, since the component (A) is produced using a metallocene catalyst, the crystallinity distribution of each component is narrow, and therefore there are very few intermediate components between the two. Therefore, it is possible to precisely separate the two components using TREF. In the present invention, the measurement is specifically performed as follows. A sample is dissolved in o-dichlorobenzene (containing 0.5 mg / ml BHT) at 140°C to obtain a solution. This is introduced into a TREF column at 140°C, and then cooled to 100°C at a temperature drop rate of 8°C / min, and then cooled to -15°C at a temperature drop rate of 4°C / min, and held for 60 minutes. Then, o-dichlorobenzene (containing 0.5 mg / ml BHT) at -15°C as a solvent is passed through the column at a flow rate of 1 ml / min, and the components dissolved in o-dichlorobenzene at -15°C in the TREF column are eluted for 10 minutes, and then the column is linearly heated to 140°C at a temperature rise rate of 100°C / hour to obtain an elution curve. In the obtained elution curves, components (A1) and (A2) show elution peaks at temperatures T(A1) and T(A2), respectively, due to the difference in crystallinity, and the difference between these peaks is large enough that they can be almost completely separated at the intermediate temperature T(A3) (={T(A1) + T(A2)} / 2). Here, if the cumulative amount of the component that dissolves up to T(A3) is defined as W(A2) weight %, and the cumulative amount of the component that dissolves at or above T(A3) is defined as W(A1) weight %, then W(A2) corresponds to the amount of component (A2), and the cumulative amount W(A1) of the component that dissolves at or above T(A3) corresponds to the amount of component (A1) with relatively high crystallinity. The equipment and specifications used for the measurements are shown below. (TREF section) TREF column: 4.3mmφ x 150mm stainless steel column Column packing material: 100 μm surface deactivated glass beads Heating method: Aluminum heat block Cooling method: Peltier element (Peltier element is water-cooled) Temperature distribution: ±0.5℃ Temperature controller: Chino Co., Ltd. Digital program controller KP1000 (valve oven) Heating method: Air bath oven Temperature during measurement: 140℃ Temperature distribution: ±1℃ Valve: 6-way valve 4-way valve (Sample injection part) Injection method: Loop injection method Injection volume: Loop size 0.1ml Inlet heating method: Aluminum heat block Temperature during measurement: 140℃ (Detection unit) Detector: Fixed wavelength infrared detector FOXBORO MIRAN 1A Detection wavelength: 3.42 μm High temperature flow cell: Micro flow cell for LC-IR, optical path length 1.5 mm, window shape 2φ×4mm long round, synthetic sapphire window plate Temperature during measurement: 140℃ (Pump section) Liquid delivery pump: SSC-3461 pump manufactured by Senshu Scientific Co., Ltd. [Measurement conditions] Solvent: o-dichlorobenzene (containing 0.5 mg / ml BHT) Sample concentration: 5mg / ml Sample injection volume: 0.1 ml Solvent flow rate: 1ml / min

[0021] Identification of ethylene content E(A1) and E(A2) The ethylene content of each component, E(A1) and E(A2), was determined by separating each component using a temperature-programmed column fractionation method using a preparative fractionation device. 13 The ethylene content of each component is determined by C-NMR. The temperature-programmed column fractionation method refers to, for example, a measurement method such as that disclosed in Macromolecules 21, 314-319 (1988). Specifically, the following method was used in the present invention.

[0022] Temperature-programmed column fractionation A cylindrical column with a diameter of 50 mm and a height of 500 mm is filled with glass bead carriers (80-100 mesh) and maintained at 140°C. Next, 200 ml of an o-dichlorobenzene solution (10 mg / ml) of the sample dissolved at 140°C is introduced into the column. The temperature of the column is then cooled to 0°C at a temperature drop rate of 10°C / hour. After maintaining at 0°C for 1 hour, the column temperature is heated to T(A3) (obtained in TREF measurement) at a temperature increase rate of 10°C / hour and maintained for 1 hour. The temperature control accuracy of the column throughout the series of operations is ±1°C. Next, while maintaining the column temperature at T(A3), 800 ml of o-dichlorobenzene from T(A3) is passed through the column at a flow rate of 20 ml / min to elute and recover the components present in the column that are soluble in T(A3). Next, the column temperature is raised to 140°C at a heating rate of 10°C / min, and after standing at 140°C for 1 hour, 800 ml of o-dichlorobenzene solvent at 140°C is passed through at a flow rate of 20 ml / min to elute and recover the components insoluble in T(A3). The solution containing the polymer obtained by fractionation is concentrated to 20 ml using an evaporator, and then precipitated in 5 times the amount of methanol. The precipitated polymer is recovered by filtration and dried overnight in a vacuum dryer.

[0023] 13 Measurement of ethylene content by C-NMR The ethylene content of each of the components (A1) and (A2) obtained by the above fractionation was measured by a proton complete decoupling method under the following conditions: 13 It is determined by analyzing the C-NMR spectrum. Model: JEOL Ltd. GSX-400 or equivalent (Carbon nuclear resonance frequency 100MHz or higher) Solvent: o-dichlorobenzene / heavy benzene = 4 / 1 (volume ratio) Concentration: 100mg / ml Temperature: 130℃ Pulse angle: 90° Pulse interval: 15 seconds Number of times: 5,000 or more Spectral assignments can be made with reference to, for example, Macromolecules 17 1950 (1984). The assignments of the spectra measured under the above conditions are shown in Table 1. In the table, symbols such as Sαα follow the notation of Carman et al. (Macromolecules 10 536 (1977)), where P represents a methyl carbon, S represents a methylene carbon, and T represents a methine carbon.

[0024] [Table 1]

[0025] In the following, if "P" is a propylene unit in the copolymer chain and "E" is an ethylene unit, six types of triads, PPP, PPE, EPE, PEP, PEE, and EEE, can exist in the chain. As described in Macromolecules 15 1150 (1982) and elsewhere, the concentrations of these triads and the peak intensities of the spectrum are related by the following equations (1) to (6). [PPP] = k × I(Tββ) … (1) [PPE] = k × I(Tβδ) … (2) [EPE] = k × I(Tδδ) … (3) [PEP] = k × I(Sββ) … (4) [PEE] = k × I(Sβδ) … (5) [EEE]=k×{I(Sδδ) / 2+I(Sγδ) / 4} …(6) Here, [ ] denotes the fraction of triads, e.g., [PPP] is the fraction of PPP triads among all triads. therefore, [PPP]+[PPE]+[EPE]+[PEP]+[PEE]+[EEE]=1 …(7) In addition, k is a constant, and I indicates the spectrum intensity, for example, I(Tββ) means the intensity of the peak at 28.7 ppm that is assigned to Tββ. The fraction of each triad is determined by using the above relational expressions (1) to (7), and the ethylene content is further determined by the following formula. Ethylene content (mol%) = ([PEP] + [PEE] + [EEE]) x 100 The propylene-ethylene random copolymer of the present invention contains a small amount of propylene hetero bonds (2,1-bonds and / or 1,3-bonds), which causes the small peaks shown in Table 2.

[0026] [Table 2]

[0027] In order to obtain an accurate ethylene content, it is necessary to take into account the peaks derived from these heterogeneous bonds and include them in the calculation. However, since it is difficult to completely separate and identify the peaks derived from the heterogeneous bonds and the amount of the heterogeneous bonds is small, the ethylene content in the present invention is obtained using the relational equations (1) to (7) in the same manner as in the analysis of copolymers produced with a Ziegler-Natta catalyst that does not substantially contain heterogeneous bonds. The ethylene content is converted from mole % to weight % using the following formula: Ethylene content (wt%) = (28 x X / 100) / {28 x X / 100 + 42 x (1 - X / 100)} x 100 (wherein X is the ethylene content in mole percent).

[0028] (A-ii) Melt flow rate MFR(A) of component (A) The melt flow rate MFR(A) (hereinafter sometimes referred to as MFR(A)) of the component (A) used in the present invention must be in the range of 4 to 10 g / 10 min. MFR(A) is determined by the ratio of the MFRs of components (A1) and (A2) (hereinafter, sometimes referred to as MFR(A1) and MFR(A2)), but in the present invention, as long as MFR(A) is in the range of 4 to 10 g / 10 min, MFR(A1) and MFR(A2) can be any value within the range that does not impair the object of the present invention. However, since the appearance is good when the difference between the MFRs of both is small, it is desirable that both MFR(A1) and MFR(A2) are in the range of 4 to 10 g / 10 min. When the MFR(A) is 4 g / 10 min or more, the resistance to screw rotation is small, so that the motor load and tip pressure decrease, and problems such as the film surface becoming rough and deteriorating the appearance do not occur. Therefore, the MFR(A) needs to be 4 g / 10 min or more, preferably 5 g / 10 min or more. On the other hand, if the MFR(A) is 10 g / 10 min or less, molding is stable and it is easy to obtain a uniform film, so the MFR(A) must be 10 g / 10 min or less, preferably 8 g / 10 min or less. Here, the MFR is a value measured in accordance with JIS K7210.

[0029] (A-iii) tan δ curve peak The component (A) used in the present invention is required to have a temperature-loss tangent (tan δ) curve obtained by solid-state viscoelastic analysis (DMA), in which the tan δ curve showing the glass transition observed in the range of -60 to 20°C shows a single peak at or below 0°C. When component (A) has a phase-separated structure, the glass transition temperatures of the amorphous parts contained in component (A1) and (A2) are different from each other, resulting in multiple peaks, which causes a problem of significant deterioration in transparency. Generally, the glass transition temperature of a propylene-ethylene random copolymer is observed in the range of -60 to 20°C, and whether or not the copolymer has a phase-separated structure can be determined from the tan δ curve obtained by measuring the solid viscoelasticity in this range. The phase-separated structure, which affects the transparency of the film, can be avoided by having a single peak at or below 0°C.

[0030] Here, the solid viscoelasticity measurement is specifically performed by applying a sinusoidal strain of a specific frequency to a rectangular sample piece and detecting the stress that occurs. The frequency is 1 Hz, and the measurement temperature is gradually increased from -60°C until the sample melts and becomes unmeasurable. The recommended magnitude of strain is about 0.1 to 0.5%. From the obtained stress, the storage modulus G' and the loss modulus G" are obtained by a known method, and the loss tangent (= loss modulus / storage modulus) defined as the ratio between these is plotted against temperature, showing a sharp peak in the temperature range below 0°C. Generally, the peak of the tan δ curve below 0°C is observed as the glass transition of the amorphous part, and in the present invention, this peak temperature is defined as the glass transition temperature Tg (°C).

[0031] Manufacturing method of component (A) The component (A) used in the present invention can be produced by the method described in JP-A-2005-132979.

[0032] Proportion of component (A) in the propylene-based composition The proportion of component (A) in the propylene-based composition must be in the range of 35 to 89% by weight, preferably 45 to 85% by weight, and more preferably 40 to 80% by weight. When the content of component (A) is 35% by weight or more, good flexibility and transparency are obtained, whereas when the content of component (A) is 88% by weight or less, thinning during secondary processing such as heat sealing is suppressed.

[0033] 2. Ethylene-α-olefin copolymer (B) Characteristics of component (B) The ethylene-α-olefin copolymer (B) (hereinafter, sometimes referred to as component (B)) used in the propylene-based resin composition of the present invention is a copolymer obtained by copolymerizing ethylene with an α-olefin having 3 to 20 carbon atoms, and examples of the α-olefin include those having 3 to 20 carbon atoms, such as propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, and 1-heptene. Component (B) is a component that functions to improve the transparency and flexibility of the propylene-based resin composition, and is required to satisfy the following requirements (Bi) to (B-ii). The propylene-based resin composition of the present invention is required to have flexibility and transparency. Regarding transparency, if the refractive index of component (B) is significantly different from that of component (A), the transparency of the obtained film is deteriorated, so it is important to match the refractive index. The refractive index can be controlled by the density, and in order to obtain the transparency required in the present invention, it is important to set the density within a specific range. In addition, component (A) has excellent flexibility, but this flexibility is lost by adding component (C), so it is necessary to add component (B), which can improve flexibility.

[0034] (Bi) Density The component (B) used in the present invention has a density of 0.860 to 0.900 g / cm 3 It is necessary that the range is within the range. Density is 0.860g / cm 3 When the refractive index difference is 0.860 g / cm or more, the transparency is good because the refractive index difference is small. 3 In the above cases, the transparency required for the present invention can be ensured. On the other hand, the density is 0.900g / cm 3 If it is less than 0.900 g / cm, the crystallinity is low and the flexibility is sufficient. 3 It must be less than or equal to 0.885 g / cm 3 The following is the result. Here, the density is a value measured in accordance with JIS K7112.

[0035] (B-ii) Melt flow rate MFR(B) of component (B) The propylene-based resin composition of the present invention must have a suitable fluidity in order to ensure moldability. Therefore, when the melt flow rate MFR(B) of component (B) (hereinafter sometimes referred to as MFR(B)) is 2.0 g / 10 min or more, the fluidity is sufficient, and the dispersibility is good, thereby improving the transparency. Therefore, MFR(B) must be 2.0 g / 10 min or more, and is preferably 2.5 g / 10 min or more. On the other hand, if the MFR(B) is 20 g / 10 min or less, molding is stable and there is no film thickness variation, so the MFR(B) is preferably 20 g / 10 min or less, and particularly preferably 15 g / 10 min or less. Here, the MFR is a value measured in accordance with JIS K7210.

[0036] Manufacturing method of component (B) In order to reduce the refractive index difference between component (A) and component (B) used in the present invention, it is necessary to reduce the density difference between component (A) and component (B), and further, in order to suppress stickiness and bleed-out, it is desirable for the component (B) to have a narrow crystallinity and a narrow molecular weight distribution. Therefore, it is desirable to use a metallocene catalyst that can narrow the crystallinity and molecular weight distribution in the production of component (B).

[0037] (i) Metallocene catalyst As the metallocene catalyst, various known catalysts used in the polymerization of ethylene-α-olefin copolymers can be used. Specific examples include metallocene catalysts described in JP-A-58-19309, JP-A-59-95292, JP-A-60-35006, JP-A-3-163088, and the like.

[0038] (ii) Polymerization method Specific polymerization methods include a slurry method, a gas-phase fluidized bed method, a solution method, or a method in the presence of these catalysts under a pressure of 200 kg / cm. 2(19.6 MPa) or higher and a polymerization temperature of 100° C. or higher. A preferred production method is the high pressure bulk polymerization method. The component (B) may be appropriately selected from commercially available metallocene polyethylenes, such as Affinity and Engage, manufactured by DuPont Dow, Kernel, manufactured by Japan Polyethylene Co., Ltd., and EXACT, manufactured by Exxon Corp. In these uses, a grade that satisfies the density and MFR requirements of the present invention may be appropriately selected.

[0039] Proportion of component (B) in the propylene-based resin composition The content of component (B) in the propylene-based resin composition must be in the range of 10 to 35% by weight. When the content of component (B) is 10% by weight or more, sufficient flexibility is imparted, and the sacrifice of flexibility caused by the addition of component (C) can be recovered. On the other hand, when the content of component (B) is 35% by weight or less, the moldability is sufficient, the thickness of the film is uniform, and a film with a good appearance can be obtained. Therefore, the proportion of component (B) in the composition must be in the range of 10 to 35% by weight, and is preferably 20 to 30% by weight.

[0040] 3. Propylene homopolymer (C) (1) Characteristics of component (C) The propylene homopolymer (C) (hereinafter sometimes referred to as component (C)) used in the propylene-based resin composition of the present invention is used as a flowability adjusting component for ensuring moldability. In the present invention, component (A) used as the main component is extremely effective in imparting high flexibility and transparency to the film. However, since it is produced using a metallocene catalyst, it has problems such as poor flowability during molding due to its narrow molecular weight distribution. Therefore, broadening the molecular weight distribution of component (A) inevitably leads to an increase in low crystallinity and low molecular weight components, which in turn cause problems such as stickiness and poor appearance due to bleed-out onto the surface of the molded film, making the product unsuitable for applications requiring transparency. Therefore, by adding a specific amount of component (C) to component (A) with a narrow molecular weight distribution, it is possible to increase the amount of highly crystalline, low molecular weight components without increasing the amount of low crystalline, low molecular weight components. As a result, it is possible to suppress poor flow during molding without causing appearance defects such as bleed-out.

[0041] (Ci) Melt flow rate MFR(C) of component (C) The melt flow rate MFR(C) of the propylene homopolymer (C) (hereinafter, sometimes referred to as MFR(C)) is 1.9 to 100 g / 10 min, preferably 2.0 to 90 g / 10 min, and more preferably 4.0 to 80 g / 10 min. When the MFR(C) is 1.9 g / 10 min or more, the flowability is good and extrusion defects during film formation can be reduced. On the other hand, when the MFR(C) is 100 g / 10 min or less, the dispersibility of the propylene-based resin (A) in the propylene homopolymer (C) is increased, and the appearance of the film is excellent. Here, the MFR is a value measured in accordance with JIS K7210. The MFR(C) of the propylene homopolymer (C) can be easily adjusted by changing the polymerization temperature and polymerization pressure conditions, or by adding a chain transfer agent such as hydrogen during polymerization.

[0042] (C-ii) No long chain branches The propylene homopolymer (C) is a propylene homopolymer having no long chain branching. The absence of long chain branching results in excellent film formation stability and excellent film appearance. The absence of long chain branching in the propylene homopolymer (C) can be confirmed by the branching index g' described below.

[0043] (2) Manufacturing method of component (C) The propylene homopolymer (C) may be produced by any method as long as it satisfies the above-mentioned properties. A preferred method is to polymerize propylene and a necessary comonomer using a Ziegler-Natta catalyst. Ziegler-Natta catalysts are catalyst systems such as those outlined in Section 2.3.1 (pp. 20-57) of "Polypropylene Handbook," edited by Edward P. Moore Jr., translated and supervised by Yasuda Tetsuo and Sakuma Nobuo, published by the Industrial Research Institute (1998). Examples of such catalysts include titanium trichloride catalysts consisting of titanium trichloride and organoaluminum halide, magnesium-supported catalysts consisting of a solid catalyst component essentially containing magnesium chloride, titanium halide, and an electron donor compound, and an organoaluminum and organosilicon compound, and a catalyst in which an organosilicon-treated solid catalyst component formed by contacting a solid catalyst component with an organoaluminum and organosilicon compound is combined with an organoaluminum compound component. The method for producing the propylene homopolymer (C) is not particularly limited, and it can be produced by any of the conventionally known methods such as slurry polymerization, bulk polymerization, and gas phase polymerization. In addition, it is also possible to produce a propylene homopolymer of a multistage polymer by utilizing a multistage polymerization method, so long as the properties are within the range described above.

[0044] (3) Proportion of component (C) in the propylene-based resin composition The content of component (C) in the propylene-based resin composition must be in the range of 0 to 15% by weight. Even if the content of component (C) is 0% by weight, practical moldability can be obtained by including propylene homopolymer (D). By including component (C), the amount of highly crystalline and low molecular weight components becomes sufficient, and sufficient moldability can be obtained, so the content of component (C) needs to be 0% by weight or more, preferably exceeds 0% by weight, more preferably is 1% by weight or more, and even more preferably is 5% by weight or more. On the other hand, if the content of component (C) is 15% by weight or less, the improvement of physical properties such as flexibility and transparency becomes significant, and the quality required for the resin composition of the present invention can be satisfied, so the content needs to be 15% by weight or less, preferably is 13% by weight or less.

[0045] 4. Propylene homopolymer (D) (1) Characteristics of component (D) The propylene homopolymer (D) (hereinafter, sometimes referred to as component (D)) used in the propylene-based resin composition of the present invention is used as a component capable of improving the surface roughness during film formation in order to suppress the blocking phenomenon that occurs during high-temperature heat treatment. In the present invention, component (A) used as the main component is extremely effective in imparting high flexibility and transparency to the film, but since it has a narrow molecular weight distribution and is very flexible, it has the problem of a blocking phenomenon when the formed film is heated at high temperatures. Therefore, broadening the molecular weight distribution of component (A) inevitably leads to an increase in low crystallinity and low molecular weight components, which in turn cause problems such as stickiness and poor appearance due to bleed-out onto the surface of the molded film, making the product unsuitable for applications requiring transparency. Therefore, by adding a specific amount of component (D) to component (A) with a narrow molecular weight distribution, it is possible to increase the amount of highly crystalline, high molecular weight components without increasing the amount of low crystalline, low molecular weight components. As a result, it is possible to roughen the surface of the film during molding without causing appearance defects such as bleed-out, and it is possible to suppress the blocking phenomenon that occurs during high-temperature heat treatment.

[0046] (Di) Melt flow rate MFR(D) of component (D) The melt flow rate MFR(D) of the propylene homopolymer (D) (hereinafter, sometimes referred to as MFR(D)) is 15 g / 10 min or less, preferably 12 g / 10 min or less, more preferably 10 g / 10 min or less. When MFR(D) is 15 g / 10 min or less, the surface roughness of the film during film formation can be improved. On the other hand, if the MFR(D) is 0.1 g / 10 min or more, the dispersibility is good and fish eye (FE) is unlikely to occur. Therefore, the MFR(D) is 0.1 g / 10 min or more, preferably 0.3 g / 10 min or more, and more preferably 0.5 g / 10 min or more. Here, the MFR is a value measured in accordance with JIS K7210. The MFR of the propylene homopolymer (D) can be easily adjusted by changing the polymerization temperature and polymerization pressure conditions, or by adding a chain transfer agent such as hydrogen during polymerization.

[0047] (D-ii) Having long chain branches The propylene homopolymer (D) is a propylene homopolymer having long chain branches. The presence of long chain branches can improve the surface roughness of the film during film formation. The presence of long chain branches in the propylene homopolymer (D) can be confirmed by the branching index g'.

[0048] Branching index g' The branching index g' can be used as a direct indicator of whether the propylene homopolymer (C) has no long chain branched structure or whether the propylene homopolymer (D) has a long chain branched structure. Absolute molecular weight M of propylene homopolymer (D) with long chain branching determined by light scattering abs The g' of the component having a molecular weight of 1 million is 0.30 or more and less than 0.95, preferably 0.55 or more and less than 0.95, more preferably 0.75 or more and less than 0.95, and even more preferably 0.78 or more and less than 0.95. When g' is less than 0.30, the proportion of main chains is small and the proportion of side chains is extremely large, and in such cases, the melt tension may not be improved or gel may be generated. On the other hand, when g' of the propylene homopolymer (C) is 0.95 to 1.05, this means that there is no branch, i.e., there is no long chain branch structure, and the melt tension tends to be insufficient, and there is a risk that the effect of suppressing the blocking phenomenon occurring during high-temperature heat treatment may not be obtained. g' is the intrinsic viscosity [η] of the polymer with long chain branching structure br Intrinsic viscosity [η] of a linear polymer with the same molecular weight lin The ratio of, i.e., [η] br / [η] lin When long chain branches are present, the value is smaller than 1.0. The definitions are described, for example, in "Developments in Polymer Characterization-4" (JV Dawkins ed. Applied Science Publishers, 1983), and are known guidelines for those skilled in the art. g' is, for example, determined by using a GPC equipped with a light scattering meter and a viscometer as detectors as described below to obtain the absolute molecular weight M abs can be obtained as a function of The propylene homopolymer (D) having a long chain branched structure preferably has a comb chain structure.

[0049] A specific method for calculating g' is as follows. The GPC apparatus used is Alliance GPCV2000 manufactured by Waters Corporation, equipped with a differential refractometer (RI) and a viscometer. In addition, a multi-angle laser light scattering detector (MALLS) manufactured by Wyatt Technology Corporation, DAWN-E, is used as the light scattering detector. The detectors are connected in the order of MALLS, RI, and viscometer. The mobile phase solvent is 1,2,4-trichlorobenzene (with the antioxidant Irganox1076 manufactured by BASF Japan Ltd. added at a concentration of 0.5 mg / mL). The flow rate is 1 mL / min, and two columns, GMHHR-H(S) HT manufactured by Tosoh Corporation, are connected in series. The temperature of the column, sample injection section, and each detector is 140° C. The sample concentration is 1 mg / mL, and the injection volume (sample loop volume) is 0.2175 mL. Absolute molecular weight obtained from MALLS (M abs ), the root mean square radius of gyration (Rg), and the intrinsic viscosity ([η]) obtained from the Viscometer are calculated using the data processing software ASTRA (version 4.73.04) attached to MALLS, with reference to the following literature. References: · "Developments in Polymer Characterization-4" (JV Dawkins ed. Applied Science Publishers, 1983. Chapter 1.) · Polymer, 45, 6495-6505(2004) · Macromolecules, 33, 2424-2436(2000) · Macromolecules, 33, 6945-6952(2000)

[0050] The branching index g' is the intrinsic viscosity ([η] br ) and the intrinsic viscosity ([η] obtained by separately measuring a linear polymer lin ) and the ratio ([η] br / [η] lin ) is calculated as follows. When a long chain branch structure is introduced into a polymer molecule, the radius of gyration becomes smaller compared to a linear polymer molecule of the same molecular weight. Since a smaller radius of gyration results in a smaller intrinsic viscosity, the intrinsic viscosity ([η]) of a linear polymer of the same molecular weight increases with the introduction of a long chain branch structure. lin ) versus the intrinsic viscosity of branched polymers ([η] br ) ratio ([η] br / [η] lin ) becomes smaller. Therefore, the branching index g'([η] br / [η] lin ) is a value smaller than 1.0, it means that the polymer has a long chain branched structure. Here, [η] lin As the linear polymer to obtain the above, a commercially available propylene homopolymer (Novatec PP (registered trademark) manufactured by Japan Polypropylene Corporation, grade name: FY6) is used. [η] of the linear polymer lin The logarithm of is linearly related to the logarithm of the molecular weight, as known by the Mark-Houwink-Sakurada equation, so [η] lin can be obtained by extrapolating to the low molecular weight side or the high molecular weight side as appropriate.

[0051] The branching index g' of 0.30 or more and less than 0.95 can be achieved by introducing a large amount of long chain branches, and this can be achieved by controlling the selection of catalysts, their combinations, and their quantitative ratios, as well as the prepolymerization conditions.

[0052] (2) Manufacturing method of component (D) The propylene homopolymer (D) having a long chain branch structure is not particularly limited in the production method as long as it satisfies the above-mentioned characteristics, but for example, there is a method using a macromer copolymerization method using a combination of metallocene catalysts. An example of the macromer copolymerization method using a combination of metallocene catalysts is the method disclosed in JP-A-2009-57542. This method is capable of producing a polypropylene resin having a comb structure and long chain branches by using a catalyst that combines a catalyst component having a specific structure capable of producing a propylene macromer and a catalyst component having a specific structure capable of copolymerizing a propylene macromer with propylene. According to this method, it is possible to produce a polypropylene resin having a comb structure and long chain branches with the desired physical properties by an industrially effective method such as a bulk polymerization method or a gas phase polymerization method, particularly a single-stage polymerization method under practical polymerization temperature and pressure conditions, and by using hydrogen as a molecular weight modifier.

[0053] (3) Proportion of component (D) in the propylene-based resin composition The content of component (D) in the propylene-based resin composition must be in the range of 1 to 15% by weight. When the content of component (D) is 1% by weight or more, the highly crystalline and high molecular weight components are sufficient, and sufficient surface roughness can be obtained on the film surface, so it is necessary that the content is 1% by weight or more, and preferably 2% by weight or more. On the other hand, when the content of component (D) is 15% by weight or less, the improvement of physical properties such as flexibility and transparency becomes significant, and the load on the molding machine is also reduced. In order to satisfy the quality required for the resin composition of the present invention, it is necessary that the content is 15% by weight or less, and preferably 13% by weight or less.

[0054] (4) Melt flow rate ratio of propylene homopolymer (C) to propylene homopolymer (D) The melt flow rate ratio (MFR(C) / MFR(D)) of the propylene homopolymer (C) and the propylene homopolymer (D) is preferably in the range of 1-100. When the melt flow rate ratio of component (C) to component (D) is 1 or more, the molecular weight distribution can be broadened, the moldability is improved, and the load on the motor of the molding machine is reduced. Therefore, the melt flow rate ratio of component (C) to component (D) (MFR(C) / MFR(D)) is preferably 1 or more, more preferably 2 or more. On the other hand, when the melt flow rate ratio of component (C) to component (D) is 100 or less, the compatibility is improved, and the improvement in physical properties such as transparency is remarkable, and the quality required for the resin composition of the present invention can be satisfied, so that it is preferably 100 or less, more preferably 80 or less.

[0055] 5. Additional ingredients (additives) Since the propylene-based resin composition of the present invention is preferably used as a film, any additive can be blended within a range that does not significantly impair the effects of the present invention, such as bleed-out. Such optional components include antioxidants, crystal nucleating agents, clarifying agents, lubricants, antiblocking agents, antistatic agents, antifogging agents, neutralizing agents, metal deactivators, colorants, dispersants, peroxides, fillers, and fluorescent whitening agents that are commonly used in polyolefin resin materials. Various additives are described in detail below.

[0056] Antioxidants Specific examples of the antioxidants that can be used as phenol-based antioxidants include tris(3,5-di-t-butyl-4-hydroxybenzyl)isocyanurate, 1,1,3-tris(2-methyl-4-hydroxy-5-t-butylphenyl)butane, octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, pentaerythrityl-tetrakis{3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate}, 1 ,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane, and 1,3,5-tris(4-t-butyl-3-hydroxy-2,6-dimethylbenzyl)isocyanuric acid.

[0057] Specific examples of phosphorus-based antioxidants include tris(mixed, mono and dinonylphenyl phosphite), tris(2,4-di-t-butylphenyl)phosphite, 4,4'-butylidenebis(3-methyl-6-t-butylphenyl-di-tridecyl)phosphite, 1,1,3-tris(2-methyl-4-di-tridecylphosphite-5-t-butylphenyl)butane, bis(2,4-di-t-butylphenyl)pentaerythritol- diphosphite, bis(2,4-di-cumylphenyl)pentaerythritol-diphosphite, tetrakis(2,4-di-t-butylphenyl)-4,4'-biphenylene diphosphonite, tetrakis(2,4-di-t-butyl-5-methylphenyl)-4,4'-biphenylene diphosphonite, bis(2,6-di-t-butyl-4-methylphenyl)pentaerythritol-diphosphite, and the like. Specific examples of sulfur-based antioxidants include di-stearyl-thio-di-propionate, di-myristyl-thio-di-propionate, pentaerythritol-tetrakis(3-lauryl-thio-propionate), and the like. These antioxidants can be used alone or in combination of two or more kinds within the scope that does not impair the intended effect.

[0058] The amount of the antioxidant is preferably 0.01 to 1.0 parts by weight, more preferably 0.02 to 0.5 parts by weight, and even more preferably 0.05 to 0.1 parts by weight, relative to 100 parts by weight of the propylene-based resin composition. If the amount is 0.01 part by weight or more, the effect of thermal stability is obtained, and deterioration during the production of the resin is prevented, and the resulting discoloration that causes fisheyes is prevented. If the amount is 1.0 part by weight or less, the antioxidant itself becomes a foreign matter and does not cause fisheyes, which is preferable.

[0059] Anti-blocking Agent The antiblocking agent has an average particle size of preferably 1 to 7 μm, more preferably 1 to 5 μm, and even more preferably 1 to 4 μm. When the average particle size is 1 μm or more, the obtained film has excellent slip properties and opening properties, which is preferable. On the other hand, when the average particle size is 7 μm or less, the transparency and scratch resistance are excellent, which is preferable. Here, the average particle size is a value measured by a Coulter counter.

[0060] Specific examples of the antiblocking agent that can be used include inorganic synthetic or natural silica (silicon dioxide), magnesium silicate, aluminosilicate, talc, zeolite, aluminum borate, calcium carbonate, calcium sulfate, barium sulfate, calcium phosphate, etc. As organic materials, polymethyl methacrylate, polymethyl silsesquioxane (silicone), polyamide, polytetrafluoroethylene, epoxy resin, polyester resin, benzoguanamine-formaldehyde condensate (benzoguanamine resin), urea resin, phenol resin, etc. can be used. In particular, synthetic silica and polymethyl methacrylate are preferred from the viewpoint of the balance of dispersibility, transparency, blocking resistance, and scratch resistance. The antiblocking agent may be surface-treated, and examples of the surface treatment agent include surfactants, metal soaps, organic acids such as acrylic acid, oxalic acid, citric acid, and tartaric acid, higher alcohols, esters, silicones, fluororesins, silane coupling agents, and condensed phosphates such as sodium hexametaphosphate, sodium pyrophosphate, sodium tripolyphosphate, and sodium trimetaphosphate, and among organic acid treatments, those treated with citric acid are particularly preferred. The treatment method is not particularly limited, and known methods such as surface spraying and immersion can be used. The antiblocking agent may be of any shape, including spherical, angular, columnar, needle-like, plate-like, and amorphous shapes. These antiblocking agents can be used alone or in combination of two or more kinds, so long as the intended effect is not impaired.

[0061] When an antiblocking agent is blended, the blending amount is preferably 0.01 to 1.0 parts by weight, more preferably 0.05 to 0.7 parts by weight, and even more preferably 0.1 to 0.5 parts by weight, based on 100 parts by weight of the propylene-based resin composition. When the blending amount is 0.01 part by weight or more, the antiblocking property, slip property, and opening property of the film are excellent. When the blending amount is 1.0 part by weight or less, the transparency of the film is not impaired, and the agent itself does not become a foreign matter and cause fisheyes, which is preferable.

[0062] Slip Agent Examples of slip agents include monoamides, substituted amides, bisamides, etc., and these can be used alone or in combination of two or more. Specific examples of monoamides include saturated fatty acid monoamides such as lauric acid amide, palmitic acid amide, stearic acid amide, behenic acid amide, and hydroxystearic acid amide. Examples of the unsaturated fatty acid monoamide include oleic acid amide, erucic acid amide, and ricinoleic acid amide. Specific examples of the substituted amides include N-stearyl stearamide, N-oleyl oleamide, N-stearyl oleamide, N-oleyl stearamide, N-stearyl erucamide, and N-oleyl palmitic amide. Specific examples of bisamides include saturated fatty acid bisamides such as methylene bisstearic acid amide, ethylene biscapric acid amide, ethylene bislauric acid amide, ethylene bisstearic acid amide, ethylene bisisostearic acid amide, ethylene bishydroxystearic acid amide, ethylene bisbehenic acid amide, hexamethylene bisstearic acid amide, hexamethylene bisbehenic acid amide, hexamethylene bishydroxystearic acid amide, N,N'-distearyl adipic acid amide, and N,N'-distearyl sebacate amide. Examples of the unsaturated fatty acid bisamides or unsaturated hydrocarbon-substituted saturated fatty acid bisamides include ethylene bisoleic acid amide, hexamethylene bisoleic acid amide, N,N'-dioleyl adipic acid amide, and N,N'-dioleyl sebacate amide. Examples of the aromatic bisamide include m-xylylene bisstearic acid amide and N,N'-distearyl isophthalic acid amide. Among these, among the fatty acid amides, oleic acid amide, erucic acid amide, and behenic acid amide are particularly preferably used.

[0063] The amount of slip agent to be added is preferably 0.01 to 1.0 parts by weight, more preferably 0.05 to 0.7 parts by weight, and even more preferably 0.1 to 0.4 parts by weight, based on 100 parts by weight of the propylene-based resin composition. When the amount is 0.01 part by weight or more, the opening property and slipping property are excellent. When the amount is 1.0 part by weight or less, the slip agent does not protrude excessively and does not bleed onto the film surface, thereby causing a deterioration in transparency.

[0064] Nucleating Agent Specific examples of nucleating agents include sodium 2,2-methylene-bis(4,6-di-t-butylphenyl)phosphate, talc, sorbitol-based compounds such as 1,3,2,4-di(p-methylbenzylidene)sorbitol and 1,3,2,4-di(p-propylbenzylidene)propyl sorbitol, hydroxy-di(t-butylbenzoate)aluminum, a mixture of hydroxy-bis[2,2-methylene-bis(4,6-di-t-butylphenyl)phosphate]aluminum and a lithium salt of an aliphatic monocarboxylate having 8 to 20 carbon atoms (manufactured by ADEKA CORPORATION, trade name Adeka STAB NA21), and 1,3,5-tris[2,2-dimethylpropionylamino]benzene. The amount of the nucleating agent, when blended, is preferably 0.0005 to 0.5 parts by weight, more preferably 0.001 to 0.1 parts by weight, and even more preferably 0.005 to 0.05 parts by weight, based on 100 parts by weight of the propylene-based resin composition. When the amount is 0.0005 parts by weight or more, the effect as a nucleating agent can be obtained. When the amount is 0.5 parts by weight or less, the agent itself does not become a foreign matter and cause fisheyes, which is preferable.

[0065] In addition, other nucleating agents include high-density polyethylene resins. The density of the high-density polyethylene resins is preferably 0.940 to 0.980 g / cm. 3 , more preferably 0.950 to 0.970 g / cm 3 When the density is within this range, a transparency improving effect can be obtained. The melt flow rate (MFR: 190°C, 2.16 kg) of the high-density polyethylene resin is preferably 5 g / 10 min or more, more preferably 7 to 500 g / 10 min, and even more preferably 10 to 100 g / 10 min. When the MFR is 5 g / 10 min or more, the dispersion diameter of the high-density polyethylene resin becomes sufficiently small, and the high-density polyethylene resin itself does not become a foreign matter and cause fisheyes, which is preferable. In order to finely disperse the high-density polyethylene resin, it is preferable that the MFR of the high-density polyethylene resin is larger than the MFR of the propylene-based resin (A) used in the present invention.

[0066] The method for producing the high density polyethylene resin used as a nucleating agent is not particularly limited with respect to the polymerization method or catalyst, as long as it can produce a polymer having the desired physical properties. The catalyst may be a Ziegler type catalyst (i.e., based on a combination of a supported or unsupported halogen-containing titanium compound and an organoaluminum compound), or a Kaminsky type catalyst (i.e., based on a combination of a supported or unsupported metallocene compound and an organoaluminum compound, particularly an alumoxane). There is no limitation on the shape of the high density polyethylene resin, and it may be in the form of pellets or powder.

[0067] When used as a nucleating agent, the amount of high-density polyethylene to be blended is preferably 0.01 to 5 parts by weight, more preferably 0.05 to 3 parts by weight, and even more preferably 0.1 to 1 part by weight, based on 100 parts by weight of the propylene-based resin composition. When the amount is 0.01 part by weight or more, the effect as a nucleating agent is obtained. When the amount is 5 parts by weight or less, the polyethylene itself does not become a foreign matter and cause fisheyes, which is preferable.

[0068] Neutralizer Specific examples of the neutralizing agent include calcium stearate, zinc stearate, hydrotalcite (trade name: DHT-4A, manufactured by Kyowa Chemical Industry Co., Ltd.), and Mizukalac (trade name, manufactured by Mizusawa Chemical Industry Co., Ltd.). When a neutralizing agent is blended, the blending amount is preferably 0.01 to 1.0 parts by weight, more preferably 0.02 to 0.5 parts by weight, and even more preferably 0.05 to 0.1 parts by weight, based on 100 parts by weight of the propylene-based resin composition. When the blending amount is 0.01 or more, the effect of the neutralizing agent is obtained, and deterioration during the production of the resin is prevented, and the resulting discoloration that causes fisheyes is prevented. In addition, when the blending amount is 1.0 part by weight or less, the agent itself becomes a foreign matter and does not cause fisheyes, which is preferable.

[0069] Light stabilizers As the light stabilizer, a hindered amine stabilizer is preferably used, and a conventionally known compound having a structure in which all hydrogen atoms bonded to the carbon atoms at the 2- and 6-positions of piperidine are substituted with methyl groups can be used without any particular limitation. Specifically, the following compounds are used: Specific examples include polycondensates of dimethyl succinate and 1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethylpiperidine, tetrakis(1,2,2,6,6-pentamethyl-4-piperidyl)1,2,3,4-butanetetracarboxylate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate, N,N-bis(3-aminopropyl)ethylenediamine·2,4-bis[N-butyl-N-(1,2,2,6,6-pentamethyl-4-piperidyl)amino]-6-chloro-1,3,5-triazine condensate, and bis( 2,2,6,6-tetramethyl-4-piperidyl) sebacate, poly[{6-(1,1,3,3-tetramethylbutyl)imino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidyl)imino}hexamethylene{2,2,6,6-tetramethyl-4-piperidyl}imino], poly[(6-morpholino-s-triazine-2,4-diyl)[(2,2,6,6-tetramethyl-4-piperidyl)imino]hexamethylene{(2,2,6,6-tetramethyl-4-piperidyl)imino}], and the like. These hindered amine stabilizers can be used alone or in combination of two or more kinds within a range that does not impair the intended effect.

[0070] When a hindered amine stabilizer is used, the amount is preferably 0.005 to 2 parts by weight, more preferably 0.01 to 1 part by weight, and even more preferably 0.05 to 0.5 parts by weight, based on 100 parts by weight of the propylene resin composition. When the content of the hindered amine stabilizer is 0.005 parts by weight or more, the effect of improving stability such as heat resistance and aging resistance is obtained, and when it is 2 parts by weight or less, the stabilizer itself does not become a foreign matter and cause fisheyes, which is preferable.

[0071] Antistatic Agent The antistatic agent can be used without any particular limitation as long as it is a known antistatic agent or an antistatic agent that has been conventionally used, and examples of the antistatic agent include anionic surfactants, cationic surfactants, nonionic surfactants, and amphoteric surfactants.

[0072] Examples of the anionic surfactant include carboxylates such as fatty acid or rosin acid soap, N-acylcarboxylates, ethercarboxylates, and fatty acid amine salts; sulfonates such as sulfosuccinates, ester sulfonates, and N-acylsulfonates; sulfate ester salts such as sulfated oils, sulfate ester salts, alkyl sulfates, alkyl polyoxyethylene sulfates, sulfate ether salts, and sulfate amide salts; and phosphate ester salts such as alkyl phosphates, alkyl polyoxyethylene phosphates, phosphate ether salts, and phosphoric acid amide salts.

[0073] Examples of the cationic surfactant include amine salts such as alkylamine salts; quaternary ammonium salts such as alkyltrimethylammonium chloride, alkylbenzyldimethylammonium chloride, alkyldihydroxyethylmethylammonium chloride, dialkyldimethylammonium chloride, tetraalkylammonium salts, N,N-di(polyoxyethylene)dialkylammonium salts, and N-alkylalkaneamide ammonium salts; alkylimidazoline derivatives such as 1-hydroxyethyl-2-alkyl-2-imidazoline and 1-hydroxyethyl-1-alkyl-2-alkyl-2-imidazoline; imidazolinium salts, pyridinium salts, and isoquinolinium salts.

[0074] Examples of the nonionic surfactants include ether types such as alkyl polyoxyethylene ethers and p-alkylphenyl polyoxyethylene ethers; ether ester types such as fatty acid sorbitan polyoxyethylene ethers, fatty acid sorbitol polyoxyethylene ethers and fatty acid glycerin polyoxyethylene ethers; ester types such as fatty acid polyoxyethylene esters, monoglycerides, diglycerides, sorbitan esters, sucrose esters, dihydric alcohol esters and boric acid esters; and nitrogen-containing types such as dialcohol alkylamines, dialcohol alkylamine esters, fatty acid alkanolamides, N,N-di(polyoxyethylene) alkanamides, alkanolamine esters, N,N-di(polyoxyethylene) alkanamines, amine oxides and alkyl polyethyleneimines.

[0075] Examples of the amphoteric surfactants include amino acid types such as monoaminocarboxylic acids and polyaminocarboxylic acids; N-alkylaminopropionate salts, N,N-di(carboxyethyl)alkylamine salts, and other N-alkyl-β-alanine types; betaine types such as N-alkylbetaine, N-alkylamidobetaine, N-alkylsulfobetaine, N,N-di(polyoxyethylene)alkylbetaine, and imidazolinium betaine; and alkylimidazoline derivatives such as 1-carboxymethyl-1-hydroxy-1-hydroxyethyl-2-alkyl-2-imidazoline and 1-sulfoethyl-2-alkyl-2-imidazoline.

[0076] Of these, nonionic surfactants and amphoteric surfactants are preferred, and among these, ester-type or nitrogen-containing nonionic surfactants such as monoglycerides, diglycerides, boric acid esters, dialcohol alkylamines, dialcohol alkylamine esters, and amides; and betaine-type amphoteric surfactants are preferred.

[0077] As the antistatic agent, commercially available products can be used, for example, Electrostripper TS5 (manufactured by Kao Corporation, trade name: glycerin monostearate), Electrostripper TS6 (manufactured by Kao Corporation, trade name: stearyl diethanolamine), Electrostripper EA (manufactured by Kao Corporation, trade name: lauryl diethanolamine), Electrostripper EA-7 (manufactured by Kao Corporation, trade name: polyoxyethylene laurylamine capryl ester), Denon 331P ( Examples of such an agent include: Stearyl diethanolamine monostearate (manufactured by Marubishi Oil Chemical Co., Ltd.), Denon 310 (manufactured by Marubishi Oil Chemical Co., Ltd., product name: alkyl diethanolamine fatty acid monoester), Resistat PE-139 (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., product name: stearic acid mono- and diglyceride borate ester), Chemistat 4700 (manufactured by Sanyo Chemical Industries, Ltd., product name: alkyl dimethyl betaine), and Rheostat S (manufactured by Lion Corporation, product name: alkyl diethanolamide).

[0078] When an antistatic agent is used, the amount is preferably 0.01 to 2 parts by weight, more preferably 0.05 to 1 part by weight, even more preferably 0.1 to 0.8 parts by weight, and most preferably 0.2 to 0.5 parts by weight, based on 100 parts by weight of the propylene-based resin composition. These antistatic agents can be used alone or in combination of two or more types within a range that does not impair the intended effect. When the amount of the antistatic agent is 0.01 part by weight or more, the surface resistivity can be reduced to prevent damage caused by static electricity. When the amount is 2 parts by weight or less, powdering due to bleeding is less likely to occur on the film surface.

[0079] [II] Method for producing propylene-based resin composition The propylene-based resin composition of the present invention can be obtained by mixing the above-mentioned propylene-based resin (A), ethylene-α-olefin copolymer (B), propylene homopolymer (C), propylene homopolymer (D) and, if necessary, other additives using a Henschel mixer (trade name), a V blender, a ribbon blender, a tumbler blender or the like, and then melt-kneading the mixture using a kneader such as a single-screw extruder, a multi-screw extruder, a kneader or a Banbury mixer.

[0080] [III] Film The film of the present invention can be produced by using the above propylene-based resin composition by a known method, for example, by a known technique such as extrusion molding using a T-die or a circular die. The film of the present invention has excellent flexibility, is capable of suppressing deterioration of transparency due to poor appearance such as uneven thickness and rough interfaces, is capable of suppressing thinning in secondary processing such as deep drawing, and therefore maintains mechanical strength, and is capable of suppressing thinning and the associated unevenness due to excessive flow of resin that occurs in heat sealing, etc., thereby maintaining a good appearance, and is excellent in suppressing the blocking phenomenon that occurs during high-temperature heat treatment.

[0081] The film of the present invention is characterized by excellent flexibility, and the tensile modulus, which is a measure of flexibility, is desirably 250 MPa or less. If the tensile modulus is 230 MPa or less, preferably 210 MPa or less, the film has a good touch and is excellent in terms of being able to create a luxurious feel.

[0082] The method of using the film of the present invention is not limited, but it is suitable for containers obtained by deep drawing, etc. exposed to a semi-molten state for a certain period of time, and containers and bags that require high-strength sealing obtained by high temperature, high pressure, and long-term heat sealing, such as water packaging, liquid-filled packaging, and heavy-weight packaging, for example, standing pouches with spouts. As a container, it is characterized by high transparency and uniform thickness, and as a bag, it is characterized by excellent appearance such as suppression of print blurring due to high transparency and heat sealing and the associated unevenness due to the absence of thinning and the suppression of blocking phenomenon that occurs during high-temperature heat treatment. In addition, it is characterized by extremely high peel strength (high-strength seal) due to the ability to suppress thinning.

[0083] The film of the present invention is excellent in that the content can be clearly seen when the haze, which is a measure of transparency, is 10% or less, preferably 8.0% or less, and particularly preferably 7.0% or less, and that the blocking phenomenon that occurs during high-temperature heat treatment can be prevented when the surface roughness of the film is 1 or more, preferably 1.5 or more, and more preferably 2 or more, thereby making it possible to improve the line speed of the manufacturing process. EXAMPLES

[0084] In the following, in order to more specifically and clearly explain the present invention, the present invention will be described in comparison with examples and comparative examples to demonstrate the rationality and significance of the configuration requirements of the present invention, but the present invention is not limited to these examples. The physical property measurement methods, characteristic evaluation methods, and resin materials used in the examples and comparative examples are as follows.

[0085] 1. Measurement methods for physical properties (1) MFR: Propylene resin (A), propylene homopolymer (C) and propylene homopolymer (D) were measured according to JIS K7210 Method A Condition M at a test temperature of 230°C, a nominal load of 2.16 kg, and a die shape of 2.095 mm diameter and 8.00 mm length. Ethylene-α-olefin copolymer (B) was measured according to JIS K7210 Method A Condition D at a test temperature of 190°C, a nominal load of 2.16 kg, and a die shape of 2.095 mm diameter and 8.00 mm length. (Unit: g / 10 min) (2) Density: Using the extruded strand obtained during the MFR measurement, the density was measured by the density gradient tube method in accordance with JIS K7112 D method. (3) Melting peak temperature: Using a Seiko Instruments Inc. DSC, 5.0 mg of sample was taken, held at 200°C for 5 minutes, crystallized at a temperature drop rate of 10°C / min to 40°C, and then melted at a temperature rise rate of 10°C / min, and the melting peak temperature was measured (unit: °C). (4) Solid viscoelasticity measurement: The specimens used were cut into strips measuring 10 mm wide x 18 mm long x 2 mm thick from a 2 mm thick sheet injection molded under the following conditions. The equipment used was the ARES manufactured by Rheometric Scientific. The frequency was 1 Hz. The measurement temperature was raised from -60°C to 20°C at a rate of 3°C / 30 seconds, and above 20°C, the temperature was raised stepwise at a rate of 3°C / 40 seconds, and the measurement was continued until the specimen melted and could no longer be measured. The strain was in the range of 0.1 to 0.5%. It was then confirmed whether the peak of the tan δ curve below 0°C was single or separated in the temperature-loss tangent (tan δ) curve obtained by the measurement. [Preparation of test pieces] Standard number: JIS-7152 (ISO294-1) Molding machine: Toshiba Machine EC-20 injection molding machine Molding machine temperature settings: From the bottom of the hopper: 80℃, 80℃, 160℃, 200℃, 200℃, 200℃ Mold temperature: 40℃ Injection speed: 200mm / sec (speed inside the mold cavity) Holding pressure: 20MPa Pressure retention time: 40 seconds Mold shape: Flat plate (thickness 2mm, width 40mm, length 80mm)

[0086] (5) W(A1), W(A2), E(A1), and E(A2) of component (A): Measured as described above. (6) Weight average molecular weight: The measurement was performed by gel permeation chromatography (GPC). In the GPC measurement, the retention volume is converted into the molecular weight using a calibration curve prepared in advance using standard polystyrene. The standard polystyrene used is the following brand manufactured by Tosoh Corporation. F380, F288, F128, F80, F40, F20, F10, F4, F1, A5000, A2500, A1000 A calibration curve is prepared by injecting 0.2 ml of a solution of each of the compounds dissolved in o-dichlorobenzene (containing 0.5 mg / ml of BHT) at a concentration of 0.5 mg / ml. The calibration curve is a cubic equation obtained by approximating with the least squares method. The viscosity formula [η] = K × M used for conversion to molecular weight α The following values ​​are used: PS:K = 1.38 x 10 -4 α=0.7 PE:K = 3.92 x 10 -4 α=0.733 PP:K = 1.03 x 10 -4 α=0.78 The GPC measurement conditions are as follows: Apparatus: WATERS GPC (ALC / GPC 150C) Detector: FOXBORO MIRAN 1A IR detector (measurement wavelength: 3.42 μm) Column: Showa Denko AD806M / S (3 columns in series) Mobile phase solvent: o-dichlorobenzene Measurement temperature: 140℃ Flow rate: 1.0ml / min Injection amount: 0.2ml Sample preparation The sample is dissolved in a 1 mg / ml solution prepared in o-dichlorobenzene (containing 0.5 mg / ml BHT) at 140° C. for approximately 1 hour. (7) Branching index (g') According to the above-mentioned method, the viscosity was measured by GPC equipped with a differential refractometer (RI), a viscosity detector (Viscometer), and a light scattering detector (MALLS) as detectors.

[0087] Evaluation method Transparency (HAZE): The transparency of the obtained laminated film was measured with a haze meter in accordance with JIS-K7136-2000.The smaller the obtained value (unit: %), the better the transparency.When this value is 10% or less, the contents can be easily confirmed and it is excellent in terms of obtaining a display effect.When this value is 10% or less, 8% or less is preferable, and 7% or less is particularly preferable. Tensile Modulus: The tensile modulus in the machine direction (MD) of the laminated film was measured under the following conditions in accordance with JIS K-7127-1989. The smaller the obtained value (unit: MPa), the better the flexibility. A value of 250 MPa or less is excellent in terms of providing a pleasant feel to the touch and a luxurious feel, with a value of 230 MPa or less being preferable, and a value of 210 MPa or less being particularly preferable. Sample length: 150mm Sample width: 15mm Chuck distance: 100mm Crosshead speed: 1mm / min

[0088] Surface roughness: After conditioning the film for 24 hours or more in an atmosphere of 23°C and 50% RH, the center surface average value (Ra) without cutoff value was measured for the contact surface with the cooling roll immediately after the die during film forming in accordance with JIS B-0601, and used as an index of film surface roughness. The larger the obtained value, the greater the unevenness of the film surface. (4)0℃ Impact: An apparatus conforming to JIS P8134 was used under the condition of an atmospheric temperature of 0°C. A film test piece was fixed to a holder with a diameter of 50 mm and struck with a 25.4 mm hemispherical metal penetration part, and the work required for penetration destruction (kJ) was measured and divided by the film thickness (unit: kJ / m). Film test pieces that did not break were indicated as NB. Blocking resistance: Two pieces of film were placed on top of each other, and stored in a 120°C atmosphere for 0.5 hours. After 0.5 hours, the films were returned to room temperature and the adhesion between the films was checked. Depending on the adhesion, the blocking resistance was evaluated according to the following criteria. If there was no adhesion at all, the blocking resistance was said to be excellent. ○: Not sticky at all. ×: Sticky.

[0089] Resins and additives used (1) Additives Antioxidants Phenolic antioxidant "IR1010" Tetrakis[methylene-3-(3',5'-di-t-butyl-4'-hydroxylphenyl)propionate]methane. Manufactured by BASF Japan Ltd., product name "IRGANOX1010". Phosphorus-based antioxidant "IF168" Tris(2,4-di-t-butylphenyl)phosphite. Manufactured by BASF Japan Ltd., product name "IRGAFOS168". Neutralizer "DHT4A" hydrotalcite. Manufactured by Kyowa Chemical Industry Co., Ltd., product name "DHT-4A". Neutralizing agent "CAST" calcium stearate. Manufactured by Nitto Kasei Kogyo Co., Ltd., product name "Ca-St". Organic peroxide "LP101" 2,5-dimethyl-2,5-di(t-butylperoxy)hexane. Manufactured by Atochem Yoshitomi Co., Ltd., product name "LUPEROX101". (2) Propylene-based resin (A) The resin obtained in the following Production Example (A-1) was used.

[0090] (Manufacturing example A-1) (i) Preparation of prepolymerized catalyst (Chemical treatment of silicates) In a 10-liter glass separable flask equipped with a stirring blade, 3.75 liters of distilled water was slowly added, followed by 2.5 kg of concentrated sulfuric acid (96%). At 50°C, 1 kg of montmorillonite (Mizusawa Chemical Industry Co., Ltd., trade name Benclay SL; average particle size = 25 μm, particle size distribution = 10 to 60 μm) was further dispersed, and the temperature was raised to 90°C and maintained at that temperature for 6.5 hours. After cooling to 50°C, the slurry was filtered under reduced pressure and a cake was collected. 7 liters of distilled water was added to the cake to re-slurry it, and then filtered. This washing operation was carried out until the pH of the washing liquid (filtrate) exceeded 3.5. The collected cake was dried overnight at 110°C under a nitrogen atmosphere. The weight after drying was 707 g. (Drying of silicates) The previously chemically treated silicate was dried in a kiln dryer under the following specifications and drying conditions: Rotating cylinder: cylindrical, inner diameter 50 mm, heating zone 550 mm (electric furnace) with scraping blades, rotation speed: 2 rpm, inclination angle: 20 / 520, silicate supply rate: 2.5 g / min, gas flow rate: nitrogen 96 liters / hour, countercurrent drying temperature: 200°C (powder temperature) (Catalyst Preparation) An autoclave with an internal volume of 16 liters and equipped with stirring and temperature control devices was thoroughly purged with nitrogen. 200 g of dried silicate was introduced, 1160 ml of mixed heptane, and 840 ml of a heptane solution of triethylaluminum (0.60 M) were added, and the mixture was stirred at room temperature. After one hour, the mixture was washed with mixed heptane, and the silicate slurry was adjusted to 2,000 ml. Next, 9.6 ml of a heptane solution of triisobutylaluminum (0.71 M) was added to the silicate slurry prepared above, and the mixture was reacted at 25°C for one hour. In parallel, 33.1 ml of a heptane solution (0.71 M) of triisobutylaluminum was added to 2,177 mg (0.3 mmol) of (r)-dichloro[1,1'-dimethylsilylenebis{2-methyl-4-(4-chlorophenyl)-4H-azulenyl}]zirconium (synthesis was carried out according to the example in JP-A-10-226712) and 870 ml of mixed heptane, and the mixture was reacted at room temperature for 1 hour. The resulting reaction mixture was added to the silicate slurry, stirred for 1 hour, and then the mixed heptane was added to adjust the volume to 5,000 ml. (Prepolymerization / Washing) Next, the temperature in the tank was raised to 40° C., and when the temperature was stabilized, propylene was fed at a rate of 100 g / hour to maintain the temperature. After 4 hours, the propylene feed was stopped and the temperature was maintained for another 2 hours. After the preliminary polymerization was completed, the remaining monomer was purged, the stirring was stopped, and the mixture was left to stand for about 10 minutes, after which 2,400 ml of the supernatant was decanted. Next, 9.5 ml of a heptane solution of triisobutylaluminum (0.71 M) and 5,600 ml of mixed heptane were added, and the mixture was stirred at 40°C for 30 minutes. After leaving the mixture to stand for 10 minutes, 5,600 ml of the supernatant was removed. This operation was repeated three times. Analysis of the components of the final supernatant revealed that the concentration of the organoaluminum component was 1.23 mM and the Zr concentration was 8.6 x 10 -6g / L, and the amount of Zr present in the supernatant (weight ratio) relative to the amount charged was 0.018 wt%. Then, 170 ml of a heptane solution of triisobutylaluminum (0.71 M) was added, and drying under reduced pressure was carried out at 45°C. A prepolymerization catalyst containing 2.0 g of polypropylene per 1 g of catalyst was obtained. Using this prepolymerized catalyst, a propylene-ethylene block copolymer was produced according to the following procedure.

[0091] (ii) First polymerization step A horizontal reactor (L / D=6, internal volume 100 liters) with stirring blades was thoroughly dried, and the inside was thoroughly replaced with nitrogen gas. In the presence of a polypropylene powder bed, while stirring at a rotation speed of 30 rpm, the prepolymerized catalyst prepared by the above method was continuously fed to the upstream part of the reactor at 0.568 g / hr (as the amount of solid catalyst excluding the prepolymerized powder) and triisobutylaluminum at 15.0 mmol / hr. The temperature of the reactor was kept at 65°C, the pressure at 2.1 MPaG, and the monomer mixed gas was continuously circulated through the reactor so that the ethylene / propylene molar ratio in the gas phase part of the reactor was 0.07 and the hydrogen concentration was 100 ppm by volume, to perform gas phase polymerization. The polymer powder generated by the reaction was continuously withdrawn from the downstream part of the reactor so that the amount of the powder bed in the reactor was constant. At this time, the amount of polymer withdrawn when the steady state was reached was 10.0 kg / hr. The propylene-ethylene random copolymer obtained in the first polymerization step was analyzed to find that it had an MFR of 6.0 g / 10 min (MFR: 230° C., 2.16 kg) and an ethylene content of 2.2% by weight.

[0092] (iii) Second polymerization step The propylene-ethylene copolymer extracted from the first step was continuously fed into a horizontal reactor (L / D=6, internal volume 100 liters) equipped with an agitator blade. While stirring at a rotation speed of 25 rpm, the temperature of the reactor was kept at 70°C, the pressure at 2.0 MPaG, and the monomer mixed gas was continuously circulated through the reactor so that the ethylene / propylene molar ratio in the gas phase of the reactor was 0.453 and the hydrogen concentration was 330 ppm by volume, to carry out gas phase polymerization. The polymer powder generated by the reaction was continuously extracted from the downstream part of the reactor so that the powder bed amount in the reactor was constant. At this time, oxygen was supplied as an activity inhibitor so that the polymer extraction rate was 17.9 kg / hr, and the polymerization reaction amount in the second polymerization step was controlled. The activity was 31.4 kg / g-catalyst. The results of various analyses of the thus obtained propylene-based resin (A-1) are shown in Table 3.

[0093] [Table 3]

[0094] (3) Ethylene-α-olefin copolymer (B) The following resins were used:

[0095] (B-1) An ethylene-α-olefin copolymer, trade name "Kernel" manufactured by Japan Polyethylene Co., Ltd., and grade name "KS340T" was used. The melt flow rate (MFR: 190°C, 2.16 kg) was 3.5 g / 10 min, and the density was 0.880 g / cm 3 It is. (B-2) An ethylene-α-olefin copolymer, trade name "Kernel" manufactured by Japan Polyethylene Co., Ltd., and grade name "KF360T" was used. The melt flow rate (MFR: 190 °C, 2.16 kg) was 3.5 g / 10 min, and the density was 0.898 g / cm 3 It is. (B-3) An ethylene-α-olefin copolymer, "Tafmer" (manufactured by Mitsui Chemicals, Inc.), with a grade of "P0280", was used. The melt flow rate (MFR: 190°C, 2.16 kg) was 3.0 g / 10 min, and the density was 0.869 g / cm 3 It is.

[0096] (4) Propylene homopolymer (C) The resins obtained in the following Production Examples (C-1) to (C-3) were used.

[0097] (Manufacturing example C-1) (1) First polymerization step A horizontal polymerization vessel (L / D = 5.2, internal volume 50 m) with an agitator blade rotating around a horizontal axis 3The first polymerization step was carried out to produce a propylene homopolymer at a first polymerization step under the conditions of a first polymerization vessel of 19.5 rpm, a reaction pressure of 2.25 MPaG, and a polymerization temperature of 60 to 70°C. However, the catalyst was fed so that the production rate after the second polymerization step was 8 t / h, using a Ziegler-based polymerization catalyst prepared according to Example 1 described in JP-A-2008-150466 so as to achieve the target production amount of the first polymerization step. Triethylaluminum was fed so that the Al / Mg molar ratio was 10 relative to Mg in the catalyst after the preliminary polymerization. In addition, hydrogen and propylene were fed at a hydrogen / propylene molar ratio of 0.010 to produce a propylene homopolymer component. (2) Second polymerization step A horizontal polymerization vessel (L / D = 5.2, internal volume 50 m) with an agitator blade rotating around a horizontal axis 3 The propylene homopolymer component from the first polymerization step was received in the second polymerization vessel (100° C.), and the same propylene homopolymer component as in the first polymerization step was produced. At this time, the stirring speed was 18 rpm, the reaction pressure was 2.20 MPaG, and the polymerization temperature was 70° C., and hydrogen and propylene were fed so as to achieve the target MFR of the propylene homopolymer component, and the hydrogen / propylene molar ratio was adjusted to 0.010, to produce the propylene homopolymer component. 100 parts by weight of the obtained propylene homopolymer powder was mixed with 0.02 parts by weight of antioxidant IR1010, 0.1 parts by weight of IR168, and 0.05 parts by weight of neutralizer DHT4A, and melt-kneaded at a die outlet temperature of 190 to 230°C using an extruder, and pelletized. The MFR of this pellet was 4.2g / 10min (MFR: 230°C, 2.16kg), g'=1.00. This was named C-1 pellet. (Production Example C-2): 100 parts by weight of propylene homopolymer powder produced by the same polymerization method as above (C-1) so that the hydrogen / propylene molar ratio was 0.040 was mixed with 0.05 parts by weight of antioxidant IR1010, 0.05 parts by weight of IF168, and 0.05 parts by weight of neutralizer CAST, and dry-blended with a super mixer, and then melt-kneaded at a die outlet temperature of 190 to 230°C using an extruder to pelletize. The MFR of this pellet was 40g / 10min (MFR: 230°C, 2.16kg), g'=1.00. This was named C-2 pellet. (Production Example C-3): 100 parts by weight of propylene homopolymer powder produced by the same polymerization method as above (C-1) so that the hydrogen / propylene molar ratio was 0.025 was blended with 0.01 parts by weight of antioxidant IR1010, 0.05 parts by weight of neutralizer CAST, and 0.03 parts by weight of organic peroxide LP101, and melt-kneaded at a die outlet temperature of 190 to 230°C using an extruder to form pellets. The MFR of this pellet was 75g / 10min (MFR: 230°C, 2.16kg), g'=1.00. This was named C-3 pellets.

[0098] (5) Propylene homopolymers and others (D) The resins obtained in the following Production Examples (D-1) to (D-6) were used. The ethylene content in Production Example D-2 was measured according to the method for measuring the ethylene contents E(A1) and E(A2) of the component (A) described above. (D-1) Propylene homopolymer with long chain branches produced by macromer copolymerization method, product name "WAYMAX (registered trademark) MFX8" manufactured by Japan Polypropylene Corporation. Melt flow rate (MFR: 230°C, 2.16 kg) is 1.3 g / 10 min, g' = 0.89. (Manufacturing example D-2) (1) First polymerization step A horizontal polymerization vessel (L / D = 5.6, internal volume 100 m) with an agitator blade rotating around a horizontal axis 3The first polymerization step of the propylene-ethylene random copolymer was produced in a first polymerization vessel of 13 rpm, a reaction pressure of 2.45 MPaG, and a polymerization temperature of 63 to 70°C. However, the catalyst was fed in such a way that the production rate after the second polymerization step was 30 t / h, using a Ziegler-based polymerization catalyst prepared according to Example 1 described in JP-A-2008-150466. Triisobutylaluminum was fed in such a way that the Al / Mg molar ratio was 5 relative to Mg in the catalyst after the preliminary polymerization. In addition, a propylene-ethylene random copolymer component was produced while feeding hydrogen, ethylene, and propylene in such a way that the hydrogen / propylene molar ratio was 0.002 and the ethylene / propylene molar ratio was 0.004. (2) Second polymerization step A horizontal polymerization vessel (L / D = 5.6, internal volume 100 m) with an agitator blade rotating around a horizontal axis 3 The propylene-ethylene random copolymer component from the first polymerization step was received in the second polymerization vessel (100° C.), and the same propylene-ethylene random copolymer component as in the first polymerization step was produced. At this time, the stirring speed was 16 rpm, the reaction pressure was 2.40 MPaG, the polymerization temperature was 70° C., and the propylene-ethylene random copolymer component was produced while feeding hydrogen, ethylene, and propylene so that the hydrogen / propylene molar ratio was 0.002 and the ethylene / propylene molar ratio was 0.004. The obtained propylene-ethylene random copolymer powder was mixed with 0.10 parts by weight of antioxidant IR1010, 0.10 parts by weight of IF168, and 0.10 parts by weight of neutralizer CAST, and then dry-blended in a super mixer, and then melt-kneaded at a die outlet temperature of 190 to 230°C using an extruder, and pelletized. The MFR of this pellet was 0.5g / 10min (MFR: 230°C, 2.16kg), the ethylene content was 0.4% by weight, and g'=1.00. This was named D-2 pellet. (Manufacturing example D-3) The propylene homopolymer powder produced by feeding hydrogen and propylene to a hydrogen / propylene molar ratio of 0.006 in the same polymerization method as (D-2) was mixed with 0.05 parts by weight of antioxidant IR1010, 0.10 parts by weight of IF168, and 0.05 parts by weight of neutralizer CAST, and was melt-kneaded at a die outlet temperature of 190 to 230°C using an extruder, and pelletized. The MFR of this pellet was 1.9g / 10min (MFR: 230°C, 2.16kg), g'=1.00. This was named D-3 pellet. (D-4) Instead of propylene homopolymer, low-density polyethylene, manufactured by Japan Polyethylene Co., Ltd. under the trade name "Novatec LD" and the grade name "LM360", was used. The melt flow rate (MFR: 190°C, 2.16 kg) was 0.9 g / 10 min, and the density was 0.928 g / cm 3 It is. Incidentally, since D-4 is a low-density polyethylene resin and not a polypropylene resin, it is outside the scope of the measurement of the branching index (g') described above. (D-5) Propylene homopolymer with long chain branches produced by macromer copolymerization method, product name "WAYMAX (registered trademark) MFX6" manufactured by Japan Polypropylene Corporation. Melt flow rate (MFR: 230°C, 2.16 kg) is 2.8 g / 10 min, g' = 0.87. (D-6) Propylene homopolymer having long chain branches produced by macromer copolymerization method, product name "WAYMAX (registered trademark) MFX3" manufactured by Japan Polypropylene Corporation. Melt flow rate (MFR: 230°C, 2.16 kg) is 8.0 g / 10 min, g' = 0.86.

[0099] (6) Propylene-ethylene block copolymer (CD) The resin obtained in the following Production Example (CD-1) was used, that is, a propylene-ethylene block copolymer (CD), which is a multi-stage polymer consisting of a propylene homopolymer component (first stage) and a propylene-ethylene random copolymer component (second stage). The propylene homopolymer component in the first stage corresponds to the propylene homopolymer (C). The ethylene content of (Production Example CD-1) was measured according to the method for measuring the ethylene contents E(A1) and E(A2) of the component (A) described above. (Production Example CD-1) (1) First polymerization step A horizontal polymerization vessel (L / D = 5.2, internal volume 50 m) with an agitator blade rotating around a horizontal axis 3 The first polymerization step was carried out to produce a propylene homopolymer in the first polymerization step, using a first polymerization vessel of 19.5 rpm, a reaction pressure of 2.25 MPaG, and a polymerization temperature of 60 to 70°C. However, the catalyst was fed in such a way that the production rate after the second polymerization step was 8 t / h, using a Ziegler-based polymerization catalyst prepared according to Example 1 described in JP-A-2008-150466. Triethylaluminum was fed in such a way that the Al / Mg molar ratio was 10 relative to Mg in the catalyst after the preliminary polymerization. In addition, hydrogen and propylene were fed at a hydrogen / propylene molar ratio of 0.012 to produce a propylene homopolymer component. The propylene homopolymer obtained in the first polymerization step was analyzed and found to have an MFR of 5.4 g / 10 min (MFR: 230° C., 2.16 kg). (2) Second polymerization step A horizontal polymerization vessel (L / D = 5.2, internal volume 50 m) with an agitator blade rotating around a horizontal axis 3 The propylene homopolymer component from the first polymerization step was received in the second polymerization vessel (100° C.), and a propylene-ethylene random copolymer component was produced. At this time, the stirring speed was 18 rpm, the reaction pressure was 2.20 MPaG, and the polymerization temperature was 60° C., and hydrogen, propylene, and ethylene were fed at hydrogen / propylene molar ratios of 0.009 and ethylene / propylene molar ratios of 0.450, respectively, and oxygen was fed at 1.0 mol / h to control the reaction amount in the second polymerization step, to produce a propylene-based polymer component. 100 parts by weight of the obtained propylene-ethylene block copolymer powder was blended with 0.05 parts by weight of antioxidant IR1010, 0.10 parts by weight of IF168, and 0.05 parts by weight of neutralizer CAST, and melt-kneaded at a die outlet temperature of 190 to 230°C using an extruder, and pelletized. The MFR of this pellet was 2.5g / 10min (MFR: 230°C, 2.16kg), and the ethylene content was 10.1% by weight. Here, the index of the propylene-ethylene random copolymer component produced in the second stage (second polymerization step) was calculated, and the production amount was 21.5% by weight relative to the total polymer weight, the MFR was 0.15g / 10min (MFR: 230°C, 2.16kg), the ethylene content was 47.0% by weight, and g'=1.00. Example 1 (1) Combination The propylene-based resin composition was prepared by weighing out the propylene-based resin (A-1) obtained in Production Example A-1 as component (A), the ethylene-α-olefin copolymer (B-1) as component (B), the propylene homopolymer (C-2) obtained in Production Example C-2 as component (C), and the propylene homopolymer (D-1) as component (D) to be 63 wt%, 27 wt%, 7 wt%, and 3 wt%, respectively, into a Henschel mixer (product name). Then, 0.07 parts by weight of an antioxidant IR1010, 0.07 parts by weight of an antioxidant IF168, and 0.01 parts by weight of a neutralizer CAST were added relative to 100 parts by weight of the propylene-based resin composition, and the mixture was thoroughly stirred to obtain a compound.

[0100] (2) Granulation The obtained compound was melt-kneaded in a single-screw or twin-screw extruder at a screw rotation speed of 200 rpm, a discharge rate of 10 to 25 kg / hr, and an extruder temperature of 190 to 230°C. The molten resin extruded from the strand die was withdrawn while being cooled and solidified in a cooling water tank, and the strands were cut into a diameter of approximately 2 mm and a length of approximately 3 mm using a strand cutter to obtain raw material pellets.

[0101] (3) Evaluation of film properties The obtained raw material pellets were extruded at a set temperature of 167°C from a circular die with a mandrel diameter of 50 mm and a lip width of 0.6 mm using a single screw extruder with a diameter of 30 mm and L / D=28 as an intermediate layer extruder and two single screw extruders with a diameter of 18 mm and L / D=28 as skin layer extruders, cooled with water, and molded at a speed of 2 m / min to obtain a cylindrical molded body with a thickness of 300 μm. Next, one side of the obtained cylindrical molded body was cut with a cutter to obtain a film, and the film was conditioned for 24 hours or more under an atmosphere of 23°C and 50% RH. The skin layer is made of the same raw material pellets as above and is laminated on the intermediate layer. The physical properties of the resulting three-layer laminate film were evaluated, and the evaluation results are shown in Table 4. A film satisfying the constitution of the present invention maintains excellent transparency, flexibility and low-temperature impact resistance, and has sufficient surface roughness, so that it has excellent blocking resistance.

[0102] Example 2 The propylene-based resin composition obtained by weighing the propylene-based resin (A-1) obtained in Production Example A-1 as component (A), the ethylene-α-olefin copolymer (B-1) as component (B), the propylene homopolymer (C-3) obtained in Production Example C-3 as component (C), and the propylene homopolymer (D-1) as component (D) to be 63% by weight, 27% by weight, 7% by weight, and 3% by weight, respectively, was put into a Henschel mixer (trade name), and additives were blended, granulated, and a film was obtained in the same manner as in Example 1, and the physical properties were evaluated. The evaluation results are shown in Table 4. A film satisfying the constitution of the present invention maintains excellent transparency, flexibility and low-temperature impact resistance, and has sufficient surface roughness, so that it has excellent blocking resistance.

[0103] Example 3 The propylene-based resin composition obtained by weighing the propylene-based resin (A-1) obtained in Production Example A-1 as component (A), the ethylene-α-olefin copolymer (B-2) as component (B), the propylene homopolymer (C-1) obtained in Production Example C-1 as component (C), and the propylene homopolymer (D-1) as component (D) to 62% by weight, 24% by weight, 10% by weight, and 4% by weight, respectively, was put into a Henschel mixer (trade name), and additives were blended, granulated, and a film was obtained in the same manner as in Example 1, and the physical properties were evaluated. The evaluation results are shown in Table 4. A film satisfying the constitution of the present invention maintains excellent transparency, flexibility and low-temperature impact resistance, and has sufficient surface roughness, so that it has excellent blocking resistance.

[0104] Example 4 The propylene-based resin composition obtained by weighing the propylene-based resin (A-1) obtained in Production Example A-1 as component (A), the ethylene-α-olefin copolymer (B-3) as component (B), the propylene homopolymer (C-3) obtained in Production Example C-3 as component (C), and the propylene homopolymer (D-1) as component (D) to be 63% by weight, 27% by weight, 3% by weight, and 7% by weight, respectively, was put into a Henschel mixer (trade name), and additives were blended, granulated, and a film was obtained in the same manner as in Example 1, and the physical properties were evaluated. The evaluation results are shown in Table 4. A film satisfying the constitution of the present invention maintains excellent transparency, flexibility and low-temperature impact resistance, and has sufficient surface roughness, so that it has excellent blocking resistance.

[0105] Example 5 The propylene-based resin composition obtained by weighing the propylene-based resin (A-1) obtained in Production Example A-1 as component (A), the ethylene-α-olefin copolymer (B-1) as component (B), and the propylene homopolymer (D-1) as component (D) to be 63% by weight, 27% by weight, and 10% by weight, respectively, was charged into a Henschel mixer (trade name), and additives were blended, granulated, and a film was obtained in the same manner as in Example 1, and the physical properties were evaluated. The evaluation results are shown in Table 4. A film satisfying the constitution of the present invention maintains excellent transparency, flexibility and low-temperature impact resistance, and has sufficient surface roughness, so that it has excellent blocking resistance.

[0106] Example 6 The propylene-based resin composition obtained by weighing the propylene-based resin (A-1) obtained in Production Example A-1 as component (A), the ethylene-α-olefin copolymer (B-2) as component (B), and the propylene homopolymer (D-1) as component (D) to be 61% by weight, 27% by weight, and 12% by weight, respectively, was charged into a Henschel mixer (trade name), and additives were blended, granulated, and a film was obtained in the same manner as in Example 1, and the physical properties were evaluated. The evaluation results are shown in Table 4. A film satisfying the constitution of the present invention maintains excellent transparency, flexibility and low-temperature impact resistance, and has sufficient surface roughness, so that it has excellent blocking resistance.

[0107] Example 7 The propylene-based resin composition obtained by weighing the propylene-based resin (A-1) obtained in Production Example A-1 as component (A), the ethylene-α-olefin copolymer (B-3) as component (B), and the propylene homopolymer (D-1) as component (D) to be 61% by weight, 27% by weight, and 12% by weight, respectively, was charged into a Henschel mixer (product name), and additives were blended, granulated, and a film was obtained in the same manner as in Example 1, and the physical properties were evaluated. The evaluation results are shown in Table 4. A film satisfying the constitution of the present invention maintains excellent transparency, flexibility and low-temperature impact resistance, and has sufficient surface roughness, so that it has excellent blocking resistance.

[0108] Example 8 The propylene-based resin composition obtained by weighing the propylene-based resin (A-1) obtained in Production Example A-1 as component (A), the ethylene-α-olefin copolymer (B-1) as component (B), and the propylene homopolymer (D-5) as component (D) to be 61% by weight, 27% by weight, and 12% by weight, respectively, was charged into a Henschel mixer (trade name), and additives were blended, granulated, and a film was obtained in the same manner as in Example 1, and the physical properties were evaluated. The evaluation results are shown in Table 4. A film satisfying the constitution of the present invention maintains excellent transparency, flexibility and low-temperature impact resistance, and has sufficient surface roughness, so that it has excellent blocking resistance.

[0109] Example 9 The propylene-based resin composition obtained by weighing the propylene-based resin (A-1) obtained in Production Example A-1 as component (A), the ethylene-α-olefin copolymer (B-1) as component (B), the propylene homopolymer (C-1) obtained in Production Example C-1 as component (C), and the propylene homopolymer (D-6) as component (D) to 61% by weight, 24% by weight, 3% by weight, and 12% by weight, respectively, was put into a Henschel mixer (trade name), and additives were blended, granulated, and a film was obtained in the same manner as in Example 1, and the physical properties were evaluated. The evaluation results are shown in Table 4. A film satisfying the constitution of the present invention maintains excellent transparency, flexibility and low-temperature impact resistance, and has sufficient surface roughness, so that it has excellent blocking resistance.

[0110] Comparative Example 1 The propylene-based resin composition obtained by weighing out the propylene-based resin (A-1) obtained in Production Example A-1 as component (A), the ethylene-α-olefin copolymer (B-1) as component (B), and the propylene homopolymer (C-1) obtained in Production Example C-1 as component (C) to be 63% by weight, 27% by weight, and 10% by weight, respectively, was put into a Henschel mixer (trade name), and additives were blended, granulated, and a film was obtained in the same manner as in Example 1, and the physical properties were evaluated. The evaluation results are shown in Table 4. It is clear that the film not using the propylene homopolymer (D-1) has insufficient surface roughness and undergoes blocking during high-temperature heat treatment, making it unsuitable for applications that include a high-temperature heat treatment process.

[0111] Comparative Example 2 The propylene-based resin composition obtained by weighing the propylene-based resin (A-1) obtained in Production Example A-1 as component (A), the ethylene-α-olefin copolymer (B-1) as component (B), the propylene homopolymer (C-1) obtained in Production Example C-1 as component (C), and the low-density polyethylene (D-4) as component (D) to 63.5% by weight, 22.5% by weight, 10% by weight, and 4% by weight, respectively, was put into a Henschel mixer (trade name), and additives were blended, granulated, and a film was obtained in the same manner as in Example 1, and the physical properties were evaluated. The evaluation results are shown in Table 4. The film using low density polyethylene (D-4) instead of propylene homopolymer (D-1) has insufficient surface roughness, and the films block each other during high-temperature heat treatment, making it unsuitable for applications that include a high-temperature heat treatment process.

[0112] Comparative Example 3 The propylene-based resin composition obtained by weighing the propylene-based resin (A-1) obtained in Production Example A-1 as component (A), the ethylene-α-olefin copolymer (B-1) as component (B), and the propylene-ethylene block copolymer (CD-1) obtained in Production Example CD-1 to be 63% by weight, 24% by weight, and 13% by weight, respectively, was put into a Henschel mixer (product name), and additives were blended, granulated, and a film was obtained in the same manner as in Example 1, and the physical properties were evaluated. The evaluation results are shown in Table 4. The film of Comparative Example 3, which uses a propylene-ethylene block copolymer (CD-1) in which the first-stage propylene homopolymer component corresponds to the propylene homopolymer (C) and the second-stage propylene-ethylene random copolymer component does not correspond to the propylene homopolymer (D-1), does not use the propylene homopolymer (D-1), so that the surface roughness is insufficient and the films block each other during high-temperature heat treatment. This shows that the film is unsuitable for applications that include a high-temperature heat treatment process.

[0113] Comparative Example 4 The propylene-based resin composition obtained by weighing the propylene-based resin (A-1) obtained in Production Example A-1 as component (A), the ethylene-α-olefin copolymer (B-1) as component (B), the propylene homopolymer (C-2) obtained in Production Example C-2 as component (C), and the propylene-ethylene random copolymer (D-2) obtained in Production Example D-2 as component (D) to 59% by weight, 27% by weight, 10% by weight, and 4% by weight, respectively, was put into a Henschel mixer (trade name), and additives were blended, granulated, and a film was obtained in the same manner as in Example 1, and the physical properties were evaluated. The evaluation results are shown in Table 4. A film using a propylene-ethylene random copolymer (D-2) instead of a propylene homopolymer (D-1) has insufficient surface roughness, and the films block each other during high-temperature heat treatment, making it unsuitable for applications that include a high-temperature heat treatment process.

[0114] Comparative Example 5 The propylene-based resin composition obtained by weighing the propylene-based resin (A-1) obtained in Production Example A-1 as component (A), the ethylene-α-olefin copolymer (B-1) as component (B), the propylene homopolymer (C-3) obtained in Production Example C-3 as component (C), and the propylene-ethylene random copolymer (D-2) obtained in Production Example D-2 as component (D) to 59% by weight, 27% by weight, 6% by weight, and 8% by weight, respectively, was put into a Henschel mixer (trade name), and additives were blended, granulated, and a film was obtained in the same manner as in Example 1, and the physical properties were evaluated. The evaluation results are shown in Table 4. The film with increased amount of propylene-ethylene random copolymer (D-2) added has insufficient surface roughness, and the films block each other during high-temperature heat treatment, which shows that the film is unsuitable for applications that include a high-temperature heat treatment process.

[0115] Comparative Example 6 The propylene-based resin composition obtained by weighing the propylene-based resin (A-1) obtained in Production Example A-1 as component (A), the ethylene-α-olefin copolymer (B-1) as component (B), the propylene homopolymer (C-3) obtained in Production Example C-3 as component (C), and the propylene-ethylene random copolymer (D-2) obtained in Production Example D-2 as component (D) to 58% by weight, 27% by weight, 5% by weight, and 10% by weight, respectively, was put into a Henschel mixer (trade name), and additives were blended, granulated, and a film was obtained in the same manner as in Example 1, and its physical properties were evaluated. The evaluation results are shown in Table 4. The film with the added amount of propylene-ethylene random copolymer (D-2) further increased had insufficient surface roughness, and the films were blocked during high-temperature heat treatment, which shows that the film is unsuitable for applications that include a high-temperature heat treatment process.

[0116] Comparative Example 7 The propylene-based resin composition obtained by weighing the propylene-based resin (A-1) obtained in Production Example A-1 as component (A), the propylene-α-olefin copolymer (B-1) as component (B), the propylene homopolymer (C-2) obtained in Production Example C-2 as component (C), and the propylene homopolymer (D-3) obtained in Production Example D-3 as component (D) to be 58% by weight, 27% by weight, 7% by weight, and 8% by weight, respectively, was put into a Henschel mixer (trade name), and additives were blended, granulated, and a film was obtained in the same manner as in Example 1, and the physical properties were evaluated. The evaluation results are shown in Table 4. It is clear that a film using a propylene homopolymer (D-3) having no long chain branches and having g' = 1.00 has insufficient surface roughness and undergoes blocking of the films during high-temperature heat treatment, making it unsuitable for applications that include a high-temperature heat treatment process.

[0117] [Table 4]

[0118] By comparing the above-mentioned Examples and Comparative Examples, it is clear that the novel propylene-based resin composition of the present invention, which satisfies the respective requirements in the configuration of the present invention, can provide a film having excellent suppression effect against the blocking phenomenon occurring during high-temperature heat treatment while maintaining excellent flexibility, transparency and low-temperature impact resistance. [Industrial Applicability]

[0119] The propylene-based resin composition can provide a film that has sufficient surface roughness while maintaining excellent flexibility, transparency, and low-temperature impact resistance, and is therefore less susceptible to the blocking phenomenon that occurs during high-temperature heat treatment. The propylene-based resin composition and the film using the same are extremely useful for heavy-duty packaging applications such as standing pouches and water packaging, and for containers obtained by deep drawing.

Claims

1. A propylene-based resin composition comprising 35 to 80% by weight of a propylene-based resin (A) satisfying the following conditions (A-i) to (A-iii), 10 to 35% by weight of an ethylene-α-olefin copolymer (B) satisfying the following conditions (B-i) to (B-ii), 5 to 15% by weight of a propylene homopolymer (C) satisfying the following conditions (C-i) to (C-ii), and 1 to 15% by weight of a propylene homopolymer (D) satisfying the following conditions (D-i) to (D-ii) (wherein the total of the propylene-based resin (A), the ethylene-α-olefin copolymer (B), the propylene homopolymer (C), and the propylene homopolymer (D) is taken as 100% by weight), and wherein the melt flow rate ratio (MFR(C) / MFR(D)) of the propylene homopolymer (C) and the propylene homopolymer (D) satisfies a range of 2 to 100. (A) Propylene-based resin (A-i) A metallocene-based propylene-α-olefin block copolymer (A) which is a multistage polymer comprising 50 to 60% by weight of a propylene-α-olefin random copolymer component (A1) having a melting peak temperature Tm (A1) of 125 to 135°C in a DSC measurement and an α-olefin content E (A1) of 1.5 to 3.0% by weight, and 50 to 40% by weight of a propylene-ethylene random copolymer component (A2) having an ethylene content E (A2) of 8 to 14% by weight. (A-ii) The melt flow rate (MFR(A): 230°C, 2.16 kg) is in the range of 4 to 10 g / 10 min. (A-iii) In a temperature-loss tangent (tan δ) curve obtained by solid state viscoelastic analysis (DMA), the peak of the tan δ curve representing the glass transition observed in the range of -60 to 20°C shows a single peak at or below 0°C. (B) Ethylene-α-olefin copolymer (Bi) The density is in the range of 0.860 to 0.900 g / cm3. (B-ii) The melt flow rate (MFR(B): 190°C, 2.16 kg) is 2.0 g / 10 min or more and 15 g / 10 min or less. (C) Propylene homopolymer (C-i) The melt flow rate (MFR(C): 230°C, 2.16 kg) is in the range of 1.9 to 100 g / 10 min. (C-ii) Having no long chain branches. (D) Propylene homopolymer (Di) The melt flow rate (MFR(D): 230°C, 2.16 kg) is in the range of 0.1 to 15 g / 10 min. (D-ii) Having long chain branches.

2. A film comprising the propylene-based resin composition according to claim 1.

Citation Information

Patent Citations

  • Propylene-based resin composition and multilayer sheet using the same

    JP2010138211A

  • Resin composition for sheet molding, resin sheet using the same and package for heat treatment

    JP2014101497A

  • Thermoforming sheet and formed body

    WO2017061530A1