Polyether-polysiloxane block copolymer composition, foam stabilizer, and method for producing polyurethane foam

A polyether-polysiloxane block copolymer composition with (poly)glycol derivatives replaces aromatic hydrocarbons in the synthesis of polyurethane foam stabilizers, addressing high VOC emissions and scalability issues, enabling efficient, low-emission foam production.

JP7575181B2Active Publication Date: 2024-10-29DOW TORAY CO LTD
View PDF 26 Cites 0 Cited by

Patent Information

Application Number
JP2021566900
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-25
Filing Date
2020-11-12
Publication Date
2024-10-29
Estimated Expiration
2040-11-12

AI Technical Summary

Technical Problem

Existing methods for producing polyurethane foam stabilizers using aromatic hydrocarbon solvents result in high VOC emissions and are difficult to scale up, failing to meet industry demands for low VOC and solvent-free formulations.

Method used

A method involving the use of a polyether-polysiloxane block copolymer composition comprising a linear polyether-organopolysiloxane block copolymer and a (poly)glycol or polyglycol derivative, synthesized in saturated hydrocarbons and then solvent-exchanged to eliminate aromatic hydrocarbons, resulting in a low-VOC foam stabilizer.

Benefits of technology

The method enables the production of high-quality, low-VOC polyurethane foam stabilizers that can be easily manufactured on an industrial scale, meeting industry standards for VOC emissions and solvent-free requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575181000001
    Figure 0007575181000001
  • Figure 0007575181000002
    Figure 0007575181000002
  • Figure 0007575181000003
    Figure 0007575181000003
Patent Text Reader

Abstract

[Problem] The purpose of the present invention is to sufficiently popularize a high-quality foam stabilizer in the market by providing: a method for producing a polyether-polysiloxane block copolymer composition, said method being capable of avoiding use and mixing of an aromatic hydrocarbon solvent, while easily enabling the production of the composition on an industrial scale; and a method for producing a foam stabilizer for polyurethane foams, said method using the above-described composition as a starting material. [Solution] A method for producing a polyether-polysiloxane block copolymer composition, said method being characterized by comprising: a step for obtaining a polyether-polysiloxane block copolymer (A) by a specific reaction in the presence of a saturated hydrocarbon solvent (C) that has an average number of carbon atoms within the range of from 6 to 11; and a step for substituting the solvent (C) used in the reaction with (B) a (poly)glycol or a polyglycol derivative, said step being carried out during or after the above-described step. A method for producing a foam stabilizer or the like, said method being characterized by using a composition that is obtained by the above-described production method.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a foam stabilizer for polyurethane foam (including functions as a foam control agent and a foam stabilizer, the same applies hereinafter) containing (A) a linear polyether-organopolysiloxane block copolymer and (B) a (poly)glycol or a polyglycol derivative. Furthermore, the present invention relates to the foam stabilizer, which is free of aromatic hydrocarbon solvents and has low VOC / emissions, a polyurethane foam-forming composition, and a method for producing a polyurethane foam. [Background technology]

[0002] Linear polyether-organopolysiloxane block copolymers are known as (AB)n-type polyether-modified silicones, and are broadly classified into (A1) non-hydrolyzable copolymers in which the polysiloxane and polyether parts are linked by Si-C bonds, and (A2) hydrolyzable copolymers in which the polysiloxane and polyether parts are linked by Si-OC bonds. The production method of (AB)n-type polyether-modified silicones and their application to foam stabilizers for polyurethane foams have been known for a long time.

[0003] As for (A1), Examples 1 to 7 of Patent Document 1 show an example in which (AB)n-type copolymers are synthesized in a toluene solvent by hydrosilylation reaction between (S1) organopolysiloxane containing SiH groups at both ends and (E2) polyether containing allyl groups at both ends, and then the toluene is removed by an evaporator to obtain a concentrated product. In addition, the results of testing 50% toluene solutions of these (AB)n-type copolymers as surfactants for mechanical froth polyurethane foams are reported. Examples 2, 11 to 24 of Patent Document 2 report that (AB)n-type copolymers are synthesized in a toluene solvent by hydrosilylation reaction between (S1) organopolysiloxane containing SiH groups at both ends and (E3) polyether containing methallyl groups at both ends, and then the toluene solution obtained by filtering off the catalyst is used as a surfactant. Patent Document 3 reported that the products obtained by synthesizing the same copolymers in a toluene solvent and then removing the toluene with an evaporator to concentrate them are useful as surfactants for semi-rigid urethane foams and soft hot-molded urethane foams. The surfactants obtained in this way use aromatic hydrocarbon solvents in their production, so it is difficult to make them free of the solvent, especially on a production scale, and they cannot meet the needs of the current polyurethane industry, which requires strict VOC (volatile organic compounds) management.

[0004] Patent Document 4 reports an example of using a long-chain alkylbenzene solution of an (AB)n-type copolymer as a surfactant for mechanical froth polyurethane foam. Long-chain alkylbenzenes are less harmful than BTX (benzene, toluene, xylene) solvents, and have long been used as diluents for the copolymer. However, polyurethane foams obtained using a long-chain alkylbenzene solution of an (AB)n-type copolymer as a surfactant emit a large amount of VOCs, and one of the main causes of these VOCs is long-chain alkylbenzene, so they cannot meet the needs of the current polyurethane industry, which requires strict VOC / emission management. In addition, long-chain alkylbenzenes can be considered as a type of aromatic hydrocarbon solvent, and there is a problem that they remain in the polyurethane foam and migrate (bleed out) from the final product.

[0005] Patent Document 5 discloses an example in which, after synthesizing an (AB)n-type copolymer in toluene, PPG (polypropylene glycol) is added, and the toluene is further removed by stripping. It also reports that when the PPG solution of the (AB)n-type copolymer thus obtained is used as a foam stabilizer, a mechanical froth polyurethane foam with low VOCs is obtained. The production of such a foam stabilizer requires time because it is necessary to proceed with the process while controlling the foaming that occurs in the process of replacing the reaction solvent with a diluent, but it is possible to do so even with equipment on a production machine scale. The bigger problem is that it is difficult to make the BTX solvent-free because an aromatic hydrocarbon solvent is used. Here, Patent Document 5 specifies isopropyl alcohol (IPA), toluene, and xylene as organic solvents that are reaction solvents when producing the (AB)n-type copolymer. This may lead a person skilled in the art to think that if the copolymer is produced using IPA, a foam stabilizer that does not contain BTX solvent can be obtained by replacing it with PPG. However, according to the study by the present inventors, when an (AB)n type copolymer is produced using IPA as a reaction solvent, in the subsequent solvent replacement step with a diluent, much more intense and persistent foaming occurs than in the case of toluene, and bumping phenomenon is likely to occur during pressure reduction, and it has been found that it is extremely difficult to produce the foam stabilizer according to the specified process even on a laboratory scale (the production time required was 2 to 3 times longer than in the case of toluene. Due to the intense foaming, it was necessary to use half the charge volume of the case of toluene). Considering that the production time is usually more than twice as long on a production machine scale as on a laboratory scale, and considering the occupancy time of the production equipment, deterioration of productivity, cost pressure, safety aspects, etc., it has become clear that it is not at all realistic to produce an (AB)n type foam stabilizer for polyurethane foam using IPA. As far as the inventors have investigated, it has not been reported in the past that IPA cannot be used as a reaction solvent when producing the foam stabilizer. Therefore, it is considered that the problem of there being no practical method for producing an aromatic hydrocarbon solvent-free (AB)n foam stabilizer for low VOC / emission type polyurethane foam has not been recognized in the industry.

[0006] Patent Document 6 discloses a process for synthesizing (AB)n type copolymers under reduced pressure using isopropyl palmitate (IPP) as a reaction solvent and diluent. However, ester oils such as IPP have a boiling point, and thus cause VOC emissions from polyurethane foams obtained using surfactants or foam stabilizers obtained by such a process.

[0007] Patent Document 7 discloses a technique for stably producing (AB)n type copolymers, particularly high molecular weight copolymers, without causing thickening or gelation, but does not specifically mention application to the polyurethane foam field. In Example 1, a linear polyoxyethylene-dimethylpolysiloxane block copolymer is synthesized in liquid isoparaffin, and low boiling points such as unreacted materials are removed by stripping to obtain a liquid isoparaffin solution of the corresponding (AB)n type copolymer. According to the name of the quasi-drug ingredient label, liquid isoparaffin is a hydrogenated copolymer of isobutene and n-butene, and has a degree of polymerization of 5 to 10. Liquid isoparaffin is a mixture of high boiling point components, and it is difficult to remove components with a high degree of polymerization by stripping. Therefore, if liquid isoparaffin is used as a diluent for (AB)n type copolymers for polyurethane foam, it will cause VOC / emissions from the foam.

[0008] Patent Document 8 discloses a foam stabilizer for polyurethane foam containing an (AB)n type copolymer and a specific mono-ol organic compound such as dipropylene glycol monobutyl ether (BDPG). These specific mono-ol organic compounds can be used as a synthesis reaction solvent and diluent for the (AB)n type copolymer, and are incorporated into the reaction system during polyurethane formation, so it was expected that they would reduce foam emissions. However, because not all of the mono-ol organic compounds are consumed depending on the foaming conditions, further improvements were required in terms of minimizing VOCs / emissions.

[0009] Patent Document 7 discloses a large number of reaction solvents that can be used as necessary in producing the (AB)n type copolymer, including aliphatic hydrocarbons such as hexane and heptane, but these are only disclosed as non-limiting examples of selectable solvents. In addition, among these many solvents, many solvents that are not practical to use in producing the (AB)n type copolymer because they inhibit the reaction, cause the reaction system to become non-uniform, or cause side reactions, etc., are listed, and in order to search for the optimal solvent, a person skilled in the art needs to conduct a large number of experiments to verify the reactivity and stability of these solvents, and there is no specific description on selecting a suitable solvent. In particular, there is no description or suggestion of the benefits of using (C) "saturated hydrocarbons having an average carbon number of 6 to 11" as a reaction solvent for synthesizing the (AB)n type copolymer, which is the main component of the polyurethane foam foam stabilizer, and replacing the solvent with (poly)glycol or a polyglycol derivative to obtain a polyurethane foam foam stabilizer with low VOC / emissions that does not contain aromatic hydrocarbon solvents. Therefore, Patent Document 7 does not provide a clear teaching that would enable a person skilled in the art to understand the novel method for producing the foam stabilizer for polyurethane foams comprising (A) a linear polyether-organopolysiloxane block copolymer and (B) a (poly)glycol or a polyglycol derivative of the present invention and its technical advantages.

[0010] As for (A2), Examples 8, 10 to 26 of Patent Document 9 show examples of synthesis of (AB)n-type copolymers in inactive aromatic hydrocarbon solvents such as xylene, o-dichlorobenzene, and alkylated aromatic hydrocarbon mixtures (Solvesso 100, Solvesso 150) by condensation reaction between (S2) organopolysiloxane containing dimethylamino groups at both ends and (E1) polyether (polyglycol) containing hydroxyl groups at both ends. The boiling point range of these aromatic hydrocarbon solvents is 105 to 300°C. Examples 27 to 29 of the same document show examples of synthesis of (AB)n-type copolymers in xylene by condensation reaction between (S3) organopolysiloxane containing ethoxy groups at both ends and (E1) polyether containing hydroxyl groups at both ends. Solutions of these (AB)n-type copolymers in aromatic hydrocarbon solvents were tested as surfactants for mechanical froth polyurethane foams. Patent Document 10 is based on the finding that the production time of the (AB)n-type copolymer is shortened by using carbon dioxide as a catalyst for the condensation reaction between (S2) an organopolysiloxane containing dimethylamino groups at both ends and (E1) a polyether containing hydroxyl groups at both ends, and xylene is used as the reaction solvent in the examples. Patent Document 11 reports a technology in which a tertiary amine such as 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU) is used as a catalyst for the condensation reaction between (S2) an organopolysiloxane containing dimethylamino groups at both ends and (E1) a polyether containing hydroxyl groups at both ends, and in the examples, a linear alkylbenzene with a boiling point range of 280 to 320°C is used as a synthesis reaction solvent and diluent for the (AB)n-type copolymer. However, as mentioned above, there is a problem that high boiling point alkylbenzene is the main cause of VOC / emission or migration from foam, and there is a problem that aromatic hydrocarbon solvents with lower boiling points cannot meet the demand for foam stabilizers that do not contain BTX, etc.

[0011] Patent Document 12 reports an example of synthesizing an (AB)n type copolymer by a condensation reaction between (S1) an organopolysiloxane containing SiH groups at both ends and (E1) a polyether containing hydroxyl groups at both ends in a linear alkylbenzene having a boiling point range of 280 to 320°C, using tris(pentaphenylfluoro)borane as a catalyst. Patent Document 13 reports an example of synthesizing an (AB)n type copolymer by a condensation reaction between (S1) an organopolysiloxane containing SiH groups at both ends and (E1) a polyether containing hydroxyl groups at both ends in a linear alkylbenzene having a boiling point range of 280 to 320°C, using 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU) as a catalyst. It is difficult to remove high boiling point alkylbenzene by stripping. The solution of the (AB)n type copolymer thus obtained was tested as a foam stabilizer (cell stabilizer) for typical flexible polyurethane foams. However, high boiling point alkylbenzenes have the problems already mentioned, and these techniques cannot meet the needs of the current polyurethane industry, which requires strict VOC / emission management. These documents list alkanes, cycloalkanes, and alkylated aromatic hydrocarbons as suitable reaction solvents, specifically high boiling point solvents with boiling points exceeding 120°C. Therefore, it is difficult for a person skilled in the art to come up with the idea of ​​obtaining a foam stabilizer for low VOC / emission type polyurethane foams that is free of aromatic hydrocarbon solvents by selecting (C) "saturated hydrocarbons having an average carbon atom number in the range of 6 to 11" as a reaction solvent for synthesizing (AB)n type copolymers and replacing the solvent with (poly)glycol or a polyglycol derivative. In addition, there is no description or suggestion of the benefits brought about by the new method for producing a foam stabilizer for polyurethane foams of the present invention.

[0012] That is, the (AB)n-type polyether-modified silicone or the manufacturing method of a polyurethane foam foam stabilizer containing the same disclosed in Patent Documents 1 to 13 have the problem that they cannot meet the needs of the current polyurethane industry, which requires strict VOC / emission management, or cannot meet the demand for a foam stabilizer that does not contain BTX, etc., and there is still room for improvement. Therefore, these conventional (AB)n-type polyether-modified silicone foam stabilizers are not fully satisfactory in terms of usefulness as polyurethane foam foam foam stabilizers, and have problems in terms of performance and quality, and lack of ability to respond to industry regulations, which hinder their widespread use. Therefore, there has been a demand for the development of a new manufacturing process or formulation for a foam stabilizer containing (AB)n-type polyether-modified silicone that solves these multiple problems, is easy to manufacture, can be supplied to the market in large quantities, and has sufficient usefulness in the application of a polyurethane foam foam foam stabilizer. [Prior art documents] [Patent documents]

[0013] [Patent Document 1] U.S. Patent No. 3,957,842 (JP Patent Publication No. 57-014797) [Patent Document 2] U.S. Pat. No. 4,150,048 [Patent Document 3] Japanese Patent Application Publication No. 07-090102 (Patent No. 3319833) [Patent Document 4] U.S. Patent No. 4,275,172 (JP Patent Publication No. 62-039605) [Patent Document 5] Japanese Patent Application Publication No. 08-156143 [Patent Document 6] U.S. Patent No. 5,869,727 (Patent No. 4,319,711) [Patent Document 7] JP 2006-282820 A (Patent No. 4875314 A) [Patent Document 8] International Publication No. 2016 / 166979 [Patent Document 9] U.S. Patent No. 3,836,560 (JP Patent Publication No. 56-045440) [Patent Document 10] U.S. Patent No. 3,792,073 (JP Patent Publication No. 53-012960) [Patent Document 11] U.S. Patent No. 7,645,848 [Patent Document 12] U.S. Patent No. 7,825,205 (Patent No. 5,422,115) [Patent Document 13] U.S. Patent No. 7,825,209 (Patent No. 5,231,796) [Patent Document 14] JP 2014-210832 A [Patent Document 15] U.S. Pat. No. 3,920,587 [Patent Document 16] U.S. Patent No. 8791168 (Patent No. 5371760) Summary of the Invention [Problem to be solved by the invention]

[0014] The present invention has been made to solve the above-mentioned problems, and has an object to provide a new method for producing a foam stabilizer for low VOC / emission polyurethane foam, which contains (A) a linear polyether-organopolysiloxane block copolymer and (B) a (poly)glycol or a polyglycol derivative.

[0015] Another object of the present invention is to provide a polyether-polysiloxane block copolymer composition which can avoid the use of or contamination with aromatic hydrocarbon solvents, such as BTX (benzene, toluene, xylene), and which is easy to produce on an industrial scale and can be supplied to the market in large quantities, and a method for producing a foam stabilizer for polyurethane foams using the same as a raw material, thereby promoting the widespread use of such high-quality foam stabilizers in the market and contributing to the polyurethane industry as a high-performance raw material and promoting their widespread use. [Means for solving the problem]

[0016] As a result of intensive investigation, the present inventors have found that the above-mentioned problems can be solved by a method for producing a polyether-polysiloxane block copolymer composition, comprising a step of obtaining a polyether-polysiloxane block copolymer (A) by a specific reaction in the presence of a saturated hydrocarbon solvent (C) having an average carbon atom number in the range of 6 to 11, and a step of substituting the solvent (C) used in the reaction with (B) a (poly)glycol or a polyglycol derivative during or after the step, and have arrived at the present invention. They have also found that the above-mentioned problems can be solved by a method for producing a foam stabilizer or the like, comprising using a composition obtained by the same production method, and have arrived at the present invention. Effect of the Invention

[0017] According to the present invention, there is provided a new method for producing a polyether-polysiloxane block copolymer composition containing (A) a linear polyether-organopolysiloxane block copolymer and (B) a (poly)glycol or a polyglycol derivative, and a foam stabilizer for polyurethane foam, which is an application of the composition. The polyether-polysiloxane block copolymer composition obtained by the production method of the present invention has excellent transparency even without using an aromatic hydrocarbon solvent such as BTX, and is advantageous in terms of production efficiency and production costs.

[0018] According to the present invention, it is possible to produce a high-quality foam stabilizer for polyurethane foam that can meet the needs of the current polyurethane industry, which requires strict VOC / emissions management and the absence of BTX, etc., and can contribute to foam manufacturers in producing and selling low VOC / emission PU foam.

[0019] The present invention also provides a method for producing the foam stabilizer for polyurethane foam, which is easy to produce on a production scale and can be supplied to the market in large quantities, thereby making it possible to fully popularize such high-quality foam stabilizers in the market and to widely utilize them as high-performance raw materials. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] Hereinafter, the polyether-polysiloxane block copolymer composition according to the present invention, which contains (A) a polyether-organopolysiloxane block copolymer and (B) a (poly)glycol or a polyglycol derivative, a foam stabilizer using the composition as a raw material, in particular a foam stabilizer for polyurethane foams, and a method for producing the foam stabilizer, which is free of aromatic hydrocarbon solvents and has low VOC / emissions, will be described in detail. First, each component will be described.

[0021] [Component (A)] Component (A) is also called (AB) n-type polyether-modified silicone, and may be (A1) a non-hydrolyzable copolymer in which a polysiloxane portion and a polyether portion are linked by a Si-C bond, or (A2) a hydrolyzable copolymer in which a polysiloxane portion and a polyether portion are linked by a Si-O-C bond.

[0022] The component (A1) is represented by the following general formula (1): [ka] (In the formula, each R independently represents a monovalent hydrocarbon group having 1 to 9 carbon atoms and no aliphatic unsaturated bond, x is a number from 2 to 4, a is a number from 1 to 200, and y is (C x H 2x O) y is a number in which the molecular weight of the polyether portion represented by the formula (I) is in the range of 400 to 5000, n is a number of at least 2, and Y represents a divalent hydrocarbon group having 2 to 8 carbon atoms bonded to the adjacent silicon atom by a carbon-silicon bond and to the polyoxyalkylene block by an oxygen atom), and the terminal group (-Z) of the polyoxyalkylene block is Z 1 an alkenyl group, a hydroxyl group, an alkoxy group, or an acetoxy group attached to a polyether moiety; and Z 2 A monovalent hydrocarbon group, hydroxyl group, or alkoxy group bonded to a silicon atom and having no heteroatoms The block copolymer is a linear polyether-organopolysiloxane block copolymer, the block copolymer having one or more functional groups selected from the group consisting of:

[0023] Preferably, Y is a divalent hydrocarbon group having 3 to 5 carbon atoms, which is bonded to the adjacent silicon atom by a carbon-silicon bond and to the polyoxyalkylene block by an oxygen atom, (C x H 2x O) y The polyether portion represented by (C2H4O) y1 (C2H4O) y1 (C3H6O) y2 , (C2H4O) y1 (C3H6O) y2 (C4H8O) y3 , (C2H4O) y1 (C4H8O) y3 It is a copolymer consisting of an oxyethylene portion and an oxypropylene portion and / or an oxybutylene portion selected from the following. The copolymer is preferably a random copolymer.

[0024] From the viewpoint of use as a foam stabilizer for polyurethane foams in particular, the component (A) according to the present invention preferably contains at least an oxypropylene unit or an oxybutylene unit in the polyether portion, and the number average molecular weight of the copolymer is preferably in the range of 30,000 to 150,000, and particularly preferably in the range of 50,000 to 100,000.

[0025] More preferably, the component (A1) is a compound represented by the following general formula (2): [ka] (In the formula, each R independently represents a monovalent hydrocarbon group having 1 to 9 carbon atoms and no aliphatic unsaturated bond, x is a number from 2 to 4, and a is (RSiO) a The molecular weight of the polysiloxane portion represented by the formula (C) is in the range of 400 to 2500, and y is the number (C x H 2x O) y is a number in the range of 2000 to 4500, the polyether portion is a random copolymer of an oxyethylene portion and an oxypropylene portion, and the mass ratio of the oxyethylene (C2H4O) unit constituting the entire polyether portion is in the range of 30 to 80% on average, and n is a number of at least 4. Z 1 an alkenyl group, a hydroxyl group, an alkoxy group, or an acetoxy group attached to a polyether moiety; and Z 2 A monovalent hydrocarbon group, hydroxyl group, or alkoxy group bonded to a silicon atom and having no heteroatoms The block copolymer is a linear polyether-organopolysiloxane block copolymer, the block copolymer having one or more functional groups selected from the group consisting of:

[0026] In the above general formulas (1) and (2), each R is independently a monovalent hydrocarbon group having 1 to 9 carbon atoms and no aliphatic unsaturated bond, and examples thereof include an alkyl group having 1 to 9 carbon atoms and a phenyl group. Preferred are a methyl group, an ethyl group, and a phenyl group. Industrially, a methyl group is particularly preferred.

[0027] The component (A1) has the specific structural unit described above, and the terminal group (-Z) is the above-mentioned Z 1 and Z 2and a linear polyether-organopolysiloxane block copolymer, in which the functional group is one or more selected from the following. From the viewpoint of usefulness as a foam stabilizer and stability of the copolymer, it is preferable that both ends of the copolymer are blocked with a functional group containing a polyether moiety, and in this case, the terminal group (-Z) is preferably an alkenyl group, a hydroxyl group, an alkoxy group, or an acetoxy group bonded to the polyether moiety, and is particularly preferably a methallyl group.

[0028] On the other hand, from the standpoint of usefulness as a foam stabilizer and the stability and safety of the copolymer, it is necessary that the terminal group (-Z) does not contain a reactive functional group having a heteroatom, and in particular, it is necessary that it does not contain a ring-opening reactive functional group such as an epoxy group, an amine group, etc. When an organopolysiloxane containing SiH groups at both ends is used as a raw material in synthesizing a linear polyether-organopolysiloxane block copolymer, some of the terminal SiH may react with alcohols present in the reaction system as a solvent for the catalyst, and some of the terminal groups (-Z) of the component (A) of the present invention may be residues of alcohols.

[0029] The component (A2) is represented by the following general formula (1'): [ka] (In the formula, each R independently represents a monovalent hydrocarbon group having 1 to 9 carbon atoms and no aliphatic unsaturated bond, x is a number from 2 to 4, a is a number from 7 to 200, and y is (C x H 2x O) y The molecular weight of the polyether portion represented by the formula (I) is in the range of 400 to 5000, and n is at least 2), and the terminal group (-Z) of the polyether portion is represented by the formula (I) Z 1 a hydroxyl, alkoxy or acetoxy group attached to a polyether moiety; and Z 2 : A hydroxyl group, an alkoxy group, a dimethylamino group, a hydrogen atom, a halogen, a carbamate group, or another leaving group bonded to a silicon atom The block copolymer is a linear polyether-organopolysiloxane block copolymer, the block copolymer having one or more functional groups selected from the group consisting of:

[0030] Preferably, in the general formula (3), (C x H 2x O) y The polyether portion represented by (C2H4O) y1 (C2H4O) y1 (C3H6O) y2 , (C2H4O) y1 (C3H6O) y2 (C4H8O) y3 , (C2H4O) y1 (C4H8O) y3 It is a copolymer consisting of an oxyethylene portion and an oxypropylene portion and / or an oxybutylene portion selected from the following. The copolymer is preferably a random copolymer.

[0031] More preferably, in the general formula (3), a is (RSiO) a The molecular weight of the polysiloxane portion represented by the formula (C) is in the range of 600 to 2500, and y is the number (C x H 2x O) y is a number in which the molecular weight of the polyether portion represented by the formula (I) is in the range of 2000 to 4500, the polyether portion is a random copolymer of an oxyethylene portion and an oxypropylene portion, and the mass ratio of the oxyethylene (C2H4O) units constituting the entire polyether portion is in the range of 30 to 80% on average, and n is a number of at least 4.

[0032] The component (A2) has the specific structural unit described above, and the terminal group (-Z) is the Z 1 and Z 2From the viewpoint of usefulness as a foam stabilizer and stability of the copolymer, it is preferable that both ends of the copolymer are blocked with functional groups containing a polyether moiety, and in this case, the terminal group (-Z) is preferably a hydroxyl group, an alkoxy group, or an acetoxy group bonded to the polyether moiety.

[0033] In the above general formula (3), each R is independently a monovalent hydrocarbon group having 1 to 9 carbon atoms and no aliphatic unsaturated bond, and examples thereof include an alkyl group having 1 to 9 carbon atoms and a phenyl group. Preferred are a methyl group, an ethyl group, and a phenyl group. Industrially, a methyl group is particularly preferred.

[0034] Here, the non-hydrolyzable (AB)n-type polyether-modified silicone (A1) can be synthesized by subjecting a polyether raw material having carbon-carbon double bonds such as allyl groups or methallyl groups at both ends of the molecular chain and an organopolysiloxane containing SiH groups at both ends to a hydrosilylation reaction in the presence of the "saturated hydrocarbon solvent (C) having an average carbon number of 6 to 11" according to the present invention. As described above, it is preferable that both ends are blocked with a functional group containing a polyether moiety, and it is particularly preferable that the amount of vinyl groups in the polyether raw material is equal to or slightly in excess of the silicon-bonded hydrogen atoms in the organopolysiloxane containing SiH groups at both ends and then synthesized by subjecting the polyether raw material to a hydrosilylation reaction.

[0035] The linear polyether-organopolysiloxane block copolymer (A1) according to the present invention, which is a non-hydrolyzable copolymer, is an organopolysiloxane (S1) having SiH groups at both ends and represented by the following general formula (4): General formula (4): [ka] (In the formula, a is a number from 1 to 200, and R is the same as above.) and polyether (E4) having alkenyl groups at both ends, represented by the following general formula (5): General formula (5): [ka] (wherein, x and y are the same numbers as defined above, k is a number from 0 to 6, and each R' is independently hydrogen or a monovalent alkyl group having 1 to 6 carbon atoms) It can be obtained by a hydrosilylation reaction with

[0036] When the polyether-organopolysiloxane block copolymer (A) is used as the main component of a foam stabilizer for polyurethane foam, the hydrosilylation reaction must be carried out in the presence of a suitable reaction solvent, and in the present invention, (C) "a saturated hydrocarbon having an average carbon atom number in the range of 6 to 11" is used as the reaction solvent for producing the component (A).

[0037] The polyether (E4) having alkenyl groups at both ends is preferably a polyether (E2) having allyl groups at both ends represented by the following general formula (6) or a polyether (E3) having methallyl groups at both ends represented by the following general formula (7). General formula (6): [ka] (wherein x and y are the same numbers as above) General formula (7): [ka] (wherein x and y are the same numbers as above)

[0038] These polyethers having alkenyl groups at both ends may contain a small amount of an impurity in which one of the terminal groups is a hydroxyl group, depending on the production conditions.

[0039] Here, the hydrolyzable (AB)n-type polyether-modified silicone (A2) is an organopolysiloxane (SX) having SiX groups at both ends, represented by the following general formula (8): General formula (8): [ka] (In the formula, a is a number from 7 to 200, R is the same as above, and X is a reactive group selected from a hydroxyl group, an alkoxy group, a dimethylamino group, hydrogen, a halogen, a carbamate group, or another leaving group.) and a polyether (E1) having hydroxyl groups at both ends, represented by the following general formula (9): General formula (9): [ka] It can be obtained by a condensation reaction with

[0040] When the linear polyether-organopolysiloxane block copolymer (A) is used as the main component of a foam stabilizer for polyurethane foam, the condensation reaction must be carried out in the presence of a suitable reaction solvent, and in the present invention, (C) "a saturated hydrocarbon having an average carbon atom number in the range of 6 to 11" is used as the reaction solvent for producing the foam stabilizer.

[0041] Suitable organopolysiloxanes (SX) containing SiX groups at both ends include organopolysiloxanes (S2) containing dimethylamino groups at both ends, represented by the following general formula (10), organopolysiloxanes (S4) containing carbamate groups at both ends, represented by the following general formula (11), and organopolysiloxanes (S3) containing alkoxy groups at both ends, represented by the following general formula (12). General formula (10): [ka] (In the formula, a is a number from 7 to 200, and R is the same as defined above.) General formula (11): [ka] (In the formula, a is a number from 7 to 200, and R is the same as defined above.) General formula (12): [ka] (In the formula, a is a number from 7 to 200, R is the same as defined above, and R″ is a hydrocarbon group having 8 or less carbon atoms, preferably 4 or less carbon atoms.)

[0042] [Component (B)] Component (B) is a (poly)glycol or a polyglycol derivative. Component (B) is a solvent for linear polyether-organopolysiloxane block copolymer (A) and is introduced into the system after or during the synthesis reaction of component (A) in the presence of "saturated hydrocarbon having an average carbon number of 6 to 11". By replacing the reaction solvent (C) "saturated hydrocarbon having an average carbon number of 6 to 11" with component (B), a polyether-polysiloxane block copolymer composition containing (A) and (B) is produced. By using this composition as a raw material, it is possible to produce a polyurethane foam foam stabilizer, a polyurethane foam-forming composition, and a polyurethane foam that are free of aromatic hydrocarbon solvents and have low VOC / emissions.

[0043] Component (B) must be a liquid having affinity with component (A), and preferably has a pour point of 0°C or less. Examples of (B) include propylene glycol, butylene glycol, dipropylene glycol, tripropylene glycol, polypropylene glycol, polybutylene glycol, polypropylene glycol-polyethylene glycol copolymer, polypropylene glycol monobutyl ether, polypropylene glycol-polyethylene glycol monobutyl ether, polypropylene glycol monomethyl ether, and polypropylene glycol-polyethylene glycol monomethyl ether. Component (B) can be selected according to the required properties of the polyurethane foam produced using the polyether-polysiloxane block copolymer composition or foam stabilizer according to the present invention. For example, when a foam with high breathability is required, it is advantageous to use a monool compound such as polypropylene glycol monobutyl ether as component (B), and when a foam with low breathability is required, it is advantageous to use a diol compound such as polypropylene glycol as component (B). When it is desired to balance the breathability, a monool compound and a diol compound can be used in combination as component (B).

[0044] Component (B) functions as a solvent for component (A). In the method for producing a polyether-polysiloxane block copolymer composition of the present invention, it is important that the mass ratio of these components, (A) / (B), is within the range of 10 / 90 to 60 / 40 in terms of performance, convenience during use, ease of handling, suitability for polyurethane foam formulations, and the like, and preferably the mass ratio of (A) / (B) is within the range of 20 / 80 to 50 / 50.

[0045] It is important that the polyether-polysiloxane block copolymer composition of the present invention containing the components (A) and (B) has a viscosity in the range of 1,000 to about 60,000 mm2 / s at 25° C. from the standpoint of convenience during use, handling, etc. The viscosity of the foam stabilizer is preferably in the range of 1,000 to about 30,000 mm2 / s, more preferably in the range of 1,000 to about 10,000 mm2 / s.

[0046] [Production of composition free of aromatic hydrocarbon solvents] In the production method of the present invention, the component (A) is synthesized in the presence of a saturated hydrocarbon solvent having an average carbon number of 6 to 11, which is the component (C) described below, and the reaction solvent, component (C), is replaced with component (B) after or during the reaction step. Therefore, the polyether-polysiloxane block copolymer composition obtained by the production method of the present invention is substantially free of aromatic hydrocarbon solvents such as BTX (benzene, toluene, xylene) solvent. In particular, it is preferable that no aromatic hydrocarbon solvent is used in the production method of the present invention, and the aromatic hydrocarbon solvent in the finally obtained polyether-polysiloxane block copolymer composition is preferably 1000 ppm (weight) or less, particularly preferably 100 ppm (weight) or less, and most preferably 10 ppm (weight) or less. The production method of the present invention can provide a polyether-polysiloxane block copolymer composition suitable as a foam stabilizer for low VOC / emission type polyurethane foam with industrially sufficient production efficiency even without using any aromatic hydrocarbon solvent such as BTX (benzene, toluene, xylene) solvent.

[0047] In addition, when the polyether-polysiloxane block copolymer composition according to the present invention is used as a foam stabilizer for polyurethane foams that are free of aromatic hydrocarbon solvents and have low VOC / emissions, it can be used in combination with or mixed with another silicone foam stabilizer for polyurethane foams depending on the foam type to be applied, within a range that does not impair the technical features of the present invention. In this case, it is preferable that the content of these second silicone foam stabilizers does not exceed the same amount relative to the mass of the component (A) in the entire composition. In addition, it is preferable that the second silicone foam stabilizer is also free of aromatic hydrocarbon solvents and has low VOC / emissions.

[0048] The polyether-polysiloxane block copolymer composition according to the present invention, which contains the components (A) and (B), is gradually oxidized and deteriorated by oxygen in the air. To prevent this, it is possible and preferable to add an antioxidant such as phenols, hydroquinones, benzoquinones, aromatic amines, or vitamins to increase the oxidation stability. From the viewpoint of low VOC / emissions, it is preferable to use a non-volatile antioxidant such as vitamin E. In this case, the amount of the antioxidant added is in the range of 10 to 1000 ppm, preferably 50 to 500 ppm, by mass, relative to the component (A), and 10 to 10000 ppm, preferably 100 to 5000 ppm, by mass, relative to the component (B).

[0049] [Reduction of low molecular weight siloxane] When the polyether-polysiloxane block copolymer composition according to the present invention is used as a foam stabilizer for an aromatic hydrocarbon solvent-free, low VOC / emission type polyurethane foam, it is preferable that the composition does not substantially contain low molecular weight siloxanes having 20 or less silicon atoms. Specifically, the content of low molecular weight siloxanes having 20 or less silicon atoms in the polyether-polysiloxane block copolymer composition obtained by the production method of the present invention is preferably 5000 ppm (weight) or less, and particularly preferably 2000 ppm (weight) or less. If this value exceeds 5000 ppm, the composition may contaminate the surrounding members around the location where the polyurethane foam produced using the foam stabilizer is installed, or may cause contact failure in electric and electronic devices. Such low molecular weight siloxanes include cyclic and linear ones, and for example, those represented by the formula, [(CH3)2SiO] n’ (wherein n' is an integer of 3 to 10), and cyclic dimethylsiloxanes represented by the formula: CH3[(CH3)2SiO] m There are linear dimethylsiloxane oligomers represented by the formula Si(CH3)3 (wherein m is an integer of 1 to 10), and there are also those in which some of the methyl groups have been replaced with other organic groups. More specific examples of such low molecular weight siloxanes include octamethyltetrasiloxane, decamethylpentacyclosiloxane, and dimethylsiloxane oligomers blocked at both ends with trimethylsiloxy groups. The content of such low molecular weight siloxanes can be measured, for example, by heating the foam stabilizer according to the present invention, introducing the generated volatile components into a gas chromatography analyzer, and analyzing them.

[0050] The reduction of low molecular weight siloxanes is achieved by applying the method described in JP-A-2000-313730 to the foam stabilizer of the present invention, thereby removing low molecular weight siloxanes. There are many methods for removing low molecular weight siloxanes. For example, there is a method of treating the silicone foam stabilizer at high temperature and high vacuum while blowing in small amounts of inert gas such as argon gas or nitrogen gas into the silicone foam stabilizer, a method of forming the foam stabilizer of the present invention into a thin film and stripping it under heating conditions of 50 to 130°C under reduced pressure of 0.5 mm or less, and a method of adding an organic solvent that dissolves low molecular weight siloxanes but does not dissolve polymeric siloxanes to the silicone foam stabilizer to extract and remove the low molecular weight siloxanes. Here, if there is a concern about thermal decomposition during high temperature treatment, an antioxidant can be added in advance.

[0051] [Production method according to the present invention] The method for producing a polyether-polysiloxane block copolymer composition of the present invention includes a step (I) of synthesizing a polyether-polysiloxane block copolymer by a condensation reaction or a hydrosilylation reaction in the presence of a saturated hydrocarbon solvent (C) having an average carbon number of 6 to 11, and a step (B) of reducing the reaction solvent (C) during or after the step. (B) Substitution with (poly)glycol or polyglycol derivative The present invention is characterized by comprising the following: After explaining the reaction solvent (C) which characterizes the present invention, the production methods of the copolymer (A1) via a hydrosilylation reaction and the production method of the copolymer (A2) via a condensation reaction will be separately described in detail below.

[0052] [Hydrocarbon solvent (C)] The method for producing a polyether-polysiloxane block copolymer composition according to the present invention is characterized in that a saturated hydrocarbon (C) having an average carbon atom number ranging from 6 to 11 is used in step (I) for synthesizing the copolymer (A) by a condensation reaction or a hydrosilylation reaction. Unlike other organic solvents with high polarity, such a saturated hydrocarbon solvent does not make the appearance of the copolymer (A) or a foam stabilizer using the same opaque or inhomogeneous, and does not cause excessive stabilization of bubbles in the subsequent solvent replacement step (step (II)). This makes it possible to efficiently produce a polyether-polysiloxane block copolymer composition that is free of aromatic hydrocarbon solvents and has low VOC / emissions, and a foam stabilizer for polyurethane foam, which is an application of the composition. In addition, these solvents are components that do not fall under the above-mentioned aromatic hydrocarbon solvents or low-molecular-weight siloxanes, and even if the amount of these solvents used is substantially zero, the polyether-polysiloxane block copolymer composition can be suitably produced.

[0053] Specific examples of such reaction solvents (C) include methylcyclohexane, n-heptane, heptane mixtures, heptane (commercial grade), isooctane, 2,2,4-trimethylpentane, octane mixtures, ethylcyclohexane, dimethylcyclohexane, n-hexane, isohexane, hexane mixtures, cyclohexane, 2-methylpentane, 2-methylheptane, 3-methylheptane, Isopar E (C7-C9 saturated hydrocarbon mixture), Isopar C (C7-C8 saturated hydrocarbon mixture), IP solvent 1016 (C6-C9 saturated hydrocarbon mixture), Isopar G (C10-C11 saturated hydrocarbon mixture), etc. Among these, methylcyclohexane or n-heptane is preferred. In addition, these "saturated hydrocarbons having an average carbon atom number in the range of 6 to 11" solvents may be used alone or in combination of two or more. In particular, it is preferable to use only saturated hydrocarbons having an average carbon atom number in the range of 6 to 9, and from the viewpoint of industrial production, it is particularly preferable to use a saturated hydrocarbon solvent that is substantially free of saturated hydrocarbons having an average carbon atom number exceeding 12.

[0054] [Production method of (A1)] The non-hydrolyzable linear polyether-organopolysiloxane block copolymer (A1) according to the present invention is preferably obtained by subjecting an organopolysiloxane containing SiH groups at both ends, represented by the above general formula (4), to a hydrosilylation reaction with a polyether having allyl or methallyl groups at both molecular chain ends, represented by the above general formula (6) or (7). In this case, the step of initiating or progressing the hydrosilylation reaction is carried out in the presence of (C) a "saturated hydrocarbon having an average carbon atom number in the range of 6 to 11" as a reaction solvent.

[0055] The hydrosilylation catalyst is not limited to any specific one as long as it can promote the hydrosilylation reaction. Many metals and compounds have been known as hydrosilylation catalysts, and one can be appropriately selected from them and used in the present invention. Specific examples of hydrosilylation catalysts include finely divided platinum adsorbed on silica fine powder or carbon powder carrier, chloroplatinic acid, alcohol-modified chloroplatinic acid, olefin complex of chloroplatinic acid, coordination compound of chloroplatinic acid and vinylsiloxane, platinum black, palladium, and rhodium catalysts. In the production method of the present invention, it is preferable to use a solution of chloroplatinic acid, an alcohol-modified chloroplatinic acid, a solution of platinum-2,4,6,8-tetramethyl-2,4,6,8-tetravinyltetrasiloxane complex, or a solution of tetramethyldisiloxane of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum complex.

[0056] The amount of the hydrosilylation catalyst used is not particularly limited as long as it is an effective amount and promotes the formation reaction of the copolymer (A1) according to the present invention. Specifically, the amount of metal atoms in the catalyst is 0.1 to 1,000 ppm by mass, preferably 0.5 to 200 ppm by mass, based on the sum of the organopolysiloxane containing SiH groups at both ends of the molecular chain represented by the general formula (4) and the polyether having allyl or methallyl groups at both ends of the molecular chain represented by the general formula (6) or (7) (total is 100 mass%). If the content of the hydrosilylation catalyst is less than the lower limit of the above range, the copolymerization reaction may be insufficient, and if it exceeds the upper limit of the above range, it is uneconomical and may have an adverse effect on the transparency, such as coloring, of the obtained composition of the present invention.

[0057] Furthermore, so long as the technical effects of component (A1) according to the present invention are not impaired, an alkali metal carboxylate, such as potassium acetate or potassium propionate, may be added to the reaction system for the purpose of suppressing side reactions, and then the hydrosilylation, which is the main reaction, may be carried out.

[0058] As described above, from the standpoint of usefulness as a foam stabilizer and stability of the copolymer, component (A1) according to the present invention is preferably a linear polyether-organopolysiloxane block copolymer capped at both ends with functional groups containing polyether moieties, and it is preferable to carry out a hydrosilylation reaction by adding a polyether raw material having methallyl groups or the like at both ends to an organopolysiloxane containing SiH groups at both ends in an amount such that the amount of C=C groups in the polyether raw material is equal to or slightly in excess of the silicon-bonded hydrogen atoms in the organopolysiloxane containing SiH groups at both ends. Specifically, Vi ) to the amount of silicon-bonded hydrogen atoms (Si-H) in the organopolysiloxane containing SiH groups at both ends (molar ratio), Vi It is preferable to react them in an amount that satisfies the following formula: ] / [Si-H]=1.0 to 1.50, preferably 1.0 to 1.20.

[0059] The hydrosilylation reaction conditions require (C) "a saturated hydrocarbon having an average carbon atom number in the range of 6 to 11" as a reaction solvent. The component (A1) according to the present invention can be obtained by adding a small amount of an antioxidant such as tocopherol (vitamin E) and heating and stirring at room temperature to 140°C (below the boiling point of the reaction solvent), preferably 70 to 120°C, under an inert gas atmosphere such as nitrogen. The antioxidant may be added after the completion of hydrosilylation. The reaction time can be selected depending on the reaction scale, the amount of catalyst used, and the reaction temperature, and is generally in the range of several minutes to several hours. The reaction may also be carried out under reduced pressure, and for example, the conditions proposed in Patent Document 6 can be applied without any particular restrictions.

[0060] The end point of the hydrosilylation reaction can be confirmed by the disappearance of Si-H bond absorption by infrared spectroscopy (IR) or by the disappearance of hydrogen gas generation using the following alkali decomposition gas generation method. The amount of hydrogen gas generated can also be determined by analyzing silicon-bonded hydrogen atoms (Si-H) in the reaction raw material, organopolysiloxane containing SiH groups at both ends, using the same method.

[0061] <Alkaline decomposition gas generation method: A solution in which a sample is dissolved in toluene or IPA is reacted with a mixed solution of 28.5% caustic potassium in ethanol / water at room temperature, and the generated hydrogen gas is collected in a collection tube and its volume is measured.>

[0062] [Solvent exchange from reaction solvent (C) to component (B)] The polyether-polysiloxane block copolymer composition according to the present invention and the foam stabilizer for aromatic hydrocarbon solvent-free and low VOC / emission type polyurethane foam using the same can be produced by solvent exchange of the reaction solvent (C) with the diluent component (B) during or after the synthesis reaction of component (A1). Since component (A1) is usually a high molecular weight and high viscosity fluid, it is preferable to remove the reaction solvent (C) by stripping in an amount of about 50 / 100 to 99 / 100 after the synthesis reaction of component (A1), then add the same amount of component (B): (poly)glycol or polyglycol derivative, and further completely remove the remaining reaction solvent (C) by stripping, and then add and mix the remaining part of (B). Component (B) can be selected according to the required properties of the polyurethane foam produced using the polyether-polysiloxane block copolymer composition or foam stabilizer according to the present invention. Therefore, monool / diol can be used alone or in combination, and multiple polypropylene glycols of different types and molecular weights can be used in combination. In this solvent exchange process, bubbles generated during stirring tend to be stabilized, so in industrial production, it is preferable to appropriately control the degree of vacuum, heating temperature, and stirring speed during stripping. In order to suppress an increase in production time due to bubbles generated during the stripping process, the reaction can be started in a state where the pressure is reduced to a certain extent in advance. The residual reaction solvent (C) in the finally obtained polyether-polysiloxane block copolymer composition is preferably 5000 ppm (weight) or less, particularly preferably 1000 ppm (weight) or less, and most preferably 100 ppm (weight) or less.

[0063] [Optional purification / low bromide treatment] Furthermore, depending on the application of the polyether-polysiloxane block copolymer composition according to the present invention and the foam stabilizer using the same, when purification of the crude product or reduction of odor is required, known purification methods such as hydrogenation, contact with an acidic substance, and removal of the aldehydes generated may be added. These methods can be selected without particular limitation from, for example, purification method 1 and purification method 2 proposed in paragraph 0031 of JP-A-2007-186557, the odor reduction method proposed in JP-A-2000-327785, the treatment method using an acidic inorganic salt proposed by the present applicant in JP-A-2011-116902, etc. In particular, by carrying out these purification methods, the amount of harmful aldehydes generated over time is extremely reduced even when the composition is incorporated into a polyurethane foam, and the usefulness of the composition as a foam stabilizer for polyurethane foams applied to building materials, the automobile industry (for example, automobile interior materials), furniture such as beds and sofas, bedding, clothing, etc. is enhanced.

[0064] [Production method of (A2)] The hydrolyzable linear polyether-organopolysiloxane block copolymer (A2) according to the present invention can be obtained by a condensation reaction between an organopolysiloxane (SX) containing SiX groups at both ends, represented by the general formula (8), and a polyether (E1) containing hydroxyl groups at both ends, represented by the general formula (9). In this case, the step of initiating or advancing the condensation reaction is carried out in the presence of (C) "a saturated hydrocarbon having an average carbon atom number in the range of 6 to 11" as a reaction solvent.

[0065] The reaction may be carried out under reduced pressure if desired and / or in the presence of a catalytic amount (e.g., o, oi or double part with respect to the total amount of reactants) of a catalyst, such as a carboxylic acid or mixture thereof including trifluoroacetic acid, perfluorobutyric acid, monochloroacetic acid, etc., if an acid catalyst is used in the condensation reaction, it is necessary to remove or neutralize it in order to obtain a stable block copolymer (AB)n. However, the reaction proceeds fairly quickly even without the addition of such a catalyst. The condensation reaction may be carried out under reduced pressure if desired and / or in the presence of a catalytic amount (e.g., 0.01 to 2 parts by weight with respect to the total amount of reactants) of a catalyst, such as a carboxylic acid or mixture thereof including trifluoroacetic acid, perfluorobutyric acid, monochloroacetic acid, etc., if an acid catalyst is used in the condensation reaction, it is necessary to remove or neutralize it in order to obtain a stable block copolymer (A2). Therefore, in addition to the above-mentioned acid, a buffer component such as a methanol solution of sodium acetate may be added to proceed with the reaction. (For example, when the leaving group X=OR″) However, depending on the type of leaving group X, the condensation reaction proceeds quite rapidly without adding such a catalyst (for example, when X=NMe2, OCONMe2). When X=Cl, it is preferable to add an acid acceptor such as a tertiary amine or use it as a catalyst to trap the hydrochloric acid liberated by the condensation. When X=H, hydrogen gas is generated by the condensation, and as a catalyst for this, an organometallic compound containing tin or platinum, a tertiary amine compound such as DBU, etc. can be used. For details on suitable catalysts for each condensation reaction and the amounts to be added, please refer to Patent Documents 9 to 13.

[0066] As described above, from the viewpoint of usefulness as a foam stabilizer and stability of the copolymer, the component (A2) according to the present invention is preferably a linear polyether-organopolysiloxane block copolymer with both ends blocked with functional groups containing polyether moieties, and is preferably added to an organopolysiloxane containing SiX groups at both ends in an amount such that the amount of OH groups in the polyether raw material is equal to or slightly in excess of the amount of silicon-bonded X groups in the organopolysiloxane containing SiX groups at both ends, and then subjected to a condensation reaction. Specifically, it is preferable to react in an amount such that the ratio (molar ratio) of the amount of OH groups in the polyether raw material to the amount of silicon-bonded X groups (Si-X) in the organopolysiloxane containing SiX groups at both ends is [OH] / [Si-X]=1.0-1.50, preferably 1.0-1.20.

[0067] The conditions for the condensation reaction require (C) "a saturated hydrocarbon having an average carbon atom number in the range of 6 to 11" as the reaction solvent. The component (A1) according to the present invention can be obtained by adding a small amount of an antioxidant such as tocopherol (vitamin E) and heating and stirring at 50 to 140°C (below the boiling point of the reaction solvent), preferably 70 to 120°C, under an inert gas atmosphere such as nitrogen. The antioxidant may be added after the completion of hydrosilylation. The reaction time can be selected depending on the reaction scale, the amount of catalyst used, and the reaction temperature, and is generally in the range of several hours to half a day. The reaction may be carried out under reduced pressure depending on the type of leaving group. For details of the reaction conditions, refer to Patent Documents 9 to 13.

[0068] The end point of the condensation reaction depends on the type of leaving group X in the raw material (SX) organopolysiloxane containing SiX groups at both ends, as follows: 29 This can be confirmed by spectroscopic analysis such as SiNMR or IR, or it can be determined whether the target value has been reached by measuring the viscosity or GPC of the reaction solution.

[0069] [Solvent exchange from reaction solvent (C) to component (B)] The foam stabilizer for polyurethane foams free of aromatic hydrocarbon solvents and low VOC / emission type according to the present invention can be produced by solvent exchange of the reaction solvent (C) with the diluent component (B) during or after the synthesis reaction of component (A2). Since component (A2) is usually a high molecular weight and high viscosity fluid, it is preferable to remove the reaction solvent (C) by stripping in an amount of about 50 / 100 to 99 / 100 after the synthesis reaction of component (A2), then add the same amount of component (B): (poly)glycol or polyglycol derivative, and further completely remove the remaining reaction solvent (C) by stripping, and then add and mix the remaining part of (B). Component (B) can be selected according to the required properties of the polyurethane foam produced by using the polyether-polysiloxane block copolymer composition or foam stabilizer according to the present invention. Therefore, monool / diol can be used alone or in combination, and multiple polypropylene glycols of different types and molecular weights can be used in combination. In this solvent exchange step, bubbles generated during stirring tend to be stabilized, so in industrial production, it is preferable to appropriately control the degree of vacuum, heating temperature, and stirring speed during stripping. In order to suppress an increase in production time due to bubble generation during the stripping step, the reaction can be started in a state where the pressure has been reduced to a certain degree in advance. The amount of residual reaction solvent (C) in the finally obtained polyether-polysiloxane block copolymer composition is preferably 5000 ppm (weight) or less, particularly preferably 1000 ppm (weight) or less, and most preferably 100 ppm (weight) or less.

[0070] [Use of the foam stabilizer obtained by the production method of the present invention] The foam stabilizer for polyurethane foams which is free of aromatic hydrocarbon solvents and has low VOC / emissions and contains (A) a linear polyether-organopolysiloxane block copolymer and (B) a (poly)glycol or a polyglycol derivative, and which is obtained by the production method of the present invention, is a solution of so-called (AB)n-type polyether-modified silicone in a (poly)glycol or a polyglycol derivative, and can be used without particular restriction for the applications of (AB)n-type polyether-modified silicone foam stabilizers for polyurethane foams obtained by conventional production methods.

[0071] In addition, the "foam stabilizer for polyurethane foams containing no aromatic hydrocarbon solvents and low VOC / emission type" obtained by the manufacturing method of the present invention can be easily manufactured on a production scale and can be supplied to the market in large quantities, and can meet the needs of the current polyurethane industry, which requires strict VOC / emission control and the absence of BTX, etc., and can contribute to foam manufacturers' production and sale of low VOC / emission type PU foams. Therefore, the present invention makes it possible to fully popularize such high-quality foam stabilizers in the market and widely use them as high-performance raw materials.

[0072] [Polyurethane foam-forming composition] The foam stabilizer is used in the production of polyurethane foam. Specifically, the foam stabilizer is used as a raw material of a polyurethane foam-forming composition by adding it to the composition to form a good foam, or it may be used as a premix by mixing it with a part of the other raw materials (including catalyst) constituting the composition. The premix can be stored, and is mixed with the remaining reactive raw materials just before foaming to form a polyurethane foam. The foam stabilizer is not particularly limited in the type, characteristics, or type of formulation applied to the polyurethane foam, but is preferably used in the production of low VOC / emission PU foam as described above.

[0073] Form Type Generally, polyurethane foams are classified into hard and soft types, and are broadly divided into soft polyurethane foams, high elasticity polyurethane foams, hard polyurethane foams, and special foams, depending on the hardness, physical properties, density, etc. of the foam. The polyurethane foam foam stabilizer containing the (AB)n-type polyether-modified silicone obtained by the manufacturing method of the present invention does not use a high boiling point solvent, which is the main cause of VOC / emissions, and does not use an aromatic hydrocarbon solvent, so it is easy to make it free of BTX solvents. Therefore, it makes it easy for foam manufacturers and foam formulation (system) designers to manufacture BTX-free foams or premix systems. It can also contribute to providing polyurethane foams with low VOC / emissions. In addition, it can exert an excellent effect as a foam stabilizer in various polyurethane foam formulations.

[0074] Flexible urethane foam is widely used as a cushioning material for sofas and beds, and as a seat for automobiles. The viscosity of the raw material system for flexible slab foam is relatively low, and the expansion ratio is high, so stabilization of the cell membrane during cell growth is a major key. A foam stabilizer with a relatively high molecular weight (polyether-modified silicone) is well suited for this system. In addition, to ensure compatibility with 3000-number polyol, a type in which a polyether with a relatively high propylene oxide ratio is graft-modified is widely used. The type in which the terminal of the modified polyether is uncapped (hydroxyl group) has the effect of strengthening the independent foaming of the cells, so a type in which the polyether terminal is capped (mostly methoxy capped) is widely used, helping to facilitate the interconnection of the cell membrane. The (AB) n-type polyether-modified silicone foam stabilizer according to the present invention is a foam stabilizer containing (A) a high molecular weight main surfactant and (B) a diluent (poly)glycol or polyglycol derivative, and can be suitably used in this system. The recipe for flexible slab foam is shown, for example, in the examples of Patent Document 12, and the "aromatic hydrocarbon solvent-free (AB)n-type polyether-modified silicone foam stabilizer" according to the present invention can be formulated in place of the foam stabilizer used therein. However, since the hydroxyl value of the foam stabilizer changes depending on the type and amount of diluent, it is necessary to fine-tune the amount of isocyanate added so that the crosslink density of the urethane resin system is designed as desired. On the other hand, the flexible hot mold formulation is composed of a urethane stock solution system that is quite close to the flexible slab formulation, and since it is fast in reactivity and is under packed conditions in the mold, it is important to ensure high breathability. The (AB)n-type polyether-modified silicone foam stabilizer according to the present invention can achieve high breathability and can be used in the formulation. The recipe for flexible hot mold foam is shown, for example, in Patent Document 3, and the "aromatic hydrocarbon solvent-free (AB)n-type polyether-modified silicone foam stabilizer" according to the present invention can be formulated in place of the surfactant used therein. However, since the hydroxyl value of the foam stabilizer varies depending on the type and amount of diluent, it is necessary to fine-tune the amount of isocyanate added so that the crosslink density of the urethane resin system can be designed as desired.

[0075] A foam stabilizer suitable for flame retardant foams is defined as a type that can reduce the amount of flame retardant added in the formulation and reduces the adverse effects on foam properties caused by the addition of flame retardants. However, silicone foam stabilizers are generally considered to be flame improvers. This is because when the foam is melted into a liquid state by heat, the silicone foam stabilizer gathers on the liquid surface due to its surface activity effect, preventing carbonization. For this reason, foam stabilizers with a relatively low silicone content and low foam-stabilizing activity are suitable for flame retardant foams. The (AB)n-type polyether-modified silicone foam stabilizer according to the present invention may be used as a foam stabilizer suitable for flame retardant foams.

[0076] High elasticity foam (HR foam) is mainly used for molded foaming of car seats and the like, so it is required to improve moldability and breathability. HR foam has a high viscosity and high reactivity, so it is relatively easy to stabilize the cell membrane, but since the interconnection does not progress, it is necessary to prevent problems such as cracking due to gas accumulated inside the foam and shrinkage after demolding. For this reason, foam stabilizers with very weak foam stabilization and cell opening properties are generally widely used. This type is designed with a very small molecular weight of the foam stabilizer, and while it achieves the initial emulsification of the raw material components, it has the characteristic of having very weak cell membrane retention.

[0077] Furthermore, in this system, the relatively low molecular weight dimethylpolysiloxane that does not modify the polyether is said to impart regularity (homogeneity) to the foam cell size, and is used as a foam stabilizer or surfactant. In combination with polyether-modified silicone, these function as foam stabilizer assistants that impart stable foam stabilizing activity (moldability), while the strength of cell opening and foam stabilizing power can be adjusted by optimizing the molecular weight distribution.

[0078] For TDI-based formulations that require high activity, a type with stronger foam stabilization and fine cell formation is suitable, while for MDI-based formulations that have relatively strong closed-cell properties, a type with weaker foam stabilization, good crushing properties, and high breathability is suitable. Also, adjusting the cell size and breathability by combining a type with strong and weak foam stabilization is widely applied in production, and is a method unique to this system.

[0079] However, the very low molecular weight polyether-modified silicone and low molecular weight dimethyl polysiloxane that are widely used for high elasticity foams have a problem of narrow process range (narrow degree of freedom and tolerance of foam formulation), and in order to solve this problem, it is possible to use an appropriate amount of the (AB)n-type polyether-modified silicone foam stabilizer of the present invention in combination. A recipe for high elasticity foam using the (AB)n-type polyether-modified silicone foam stabilizer is shown in, for example, Patent Document 14, and the "(AB)n-type polyether-modified silicone foam stabilizer free of aromatic hydrocarbon solvents" of the present invention can be formulated instead of the (AB)n-type foam stabilizer used there. However, since the hydroxyl value of the foam stabilizer changes depending on the type and amount of diluent, it is necessary to finely adjust the amount of isocyanate, polyol, and water added so that the crosslink density of the urethane resin system is designed as desired.

[0080] Rigid urethane foam is widely used as an insulating material for building materials and refrigerators because it is lightweight, has excellent insulating properties, and is highly productive. In order to improve the insulating properties of rigid urethane foam, it is important to make the cell size as small as possible. The number of cells in the final foam is almost the same as the number of entrained gases dispersed during initial mixing of the urethane foaming liquid. Therefore, a foam stabilizer that strengthens the emulsifying power during initial mixing is optimal. On the other hand, the finer the cells, the more likely the foam is to shrink. In this case, a type with relatively low foam stabilizing activity is prescribed, and the effect of preventing shrinkage is enhanced by increasing the cell size. Polyisocyanurate foam, which has excellent flame retardancy, is also classified as a type of rigid urethane foam.

[0081] HCFC141b, which has been used as a blowing agent in rigid urethane foams in the past, is now restricted from the perspective of the global environment, and there are plans to further restrict its substitute, HFC compounds, in the near future. The blowing agent has a large impact on the urethane foam formulation, so it is necessary to select the most suitable foam stabilizer depending on the type of blowing agent.

[0082] In water formulations and HFC formulations with a high water content, the initial emulsifying power is lower than in HCFC-141b formulations, which had good compatibility with urethane concentrate systems. Therefore, by formulating a foam stabilizer with high foam-stabilizing activity, it is expected that good cells can be obtained. In addition, in formulations that use hydrocarbon blowing agents such as cyclopentane, premix compatibility may be required from the perspective of storage stability. In this case, the compatibility of the foam stabilizer with the base polyol is important, and types with a high EO (ethylene oxide) ratio in the modified polyether portion and hydroxyl groups (-OH) at the end show relatively good compatibility.

[0083] (AB)n-type polyether modified silicone has long been known to be useful for forming open-cell rigid polyurethane foam, which means that the modified silicone is not suitable for the production of typical rigid foams for insulation applications that require closed cells and fine cells. A recipe for open-cell rigid foam is shown in the examples of Patent Document 15, but since it uses chlorofluorocarbon gas (CFCl3), which is currently prohibited as a blowing agent, adjustments including the number of parts added are necessary so that the foam recipe can be replaced with less harmful blowing agents such as carbon dioxide or water. On the other hand, it has been reported recently that a polyurethane foam foam stabilizer containing (AB)n-type polyether modified silicone and a specific mono-ol organic compound such as dipropylene glycol monobutyl ether is useful for forming closed-cell rigid polyurethane foam with fine cells (Patent Document 8).

[0084] Examples of special foams include semi-rigid foams (see Patent Document 3 for an example of a recipe) that are intermediate between soft and hard foams and are used as shock absorbers and ceiling materials for automobiles, low-rebound foams (also called shape-memory foams or viscoelastic foams) that are derived from soft foams but have established their unique uses and position due to their unique viscoelastic behavior, high-density foams called integral skins that are used for shoe soles, and microcellular foams manufactured by mechanical foaming (mechanical flossing). Microcellular foams can be considered a type of soft foam, but they generally have a high density and an appearance and feel similar to elastomers. They are used in electronic parts, sealing materials, sound-absorbing materials, vibration-absorbing materials, and other applications, as well as carpet backing cushioning materials. Examples of microcellular foam recipes are given in Patent Documents 1 and 5. It is preferable to formulate the "(AB)n-type polyether-modified silicone foam stabilizer free of aromatic hydrocarbon solvents" according to the present invention instead of the (AB)n-type foam stabilizer used in these documents. However, since the hydroxyl value of the foam stabilizer varies depending on the type and amount of diluent, it is necessary to fine-tune the amount of isocyanate added so that the crosslink density of the urethane resin system can be designed as desired.

[0085] In addition, foams produced using polyester-type polyols rather than the common polyether-type polyols as the raw polyol material for urethane foams are called ester foams, and are also classified according to the foam characteristics as described above.

[0086] Since heat insulation is important in many applications of rigid foams, closed-cell foams with a high closed cell ratio are usually required, but in some applications, dimensional stability is emphasized, and the surfactant is selected and the foam composition is formulated to partially open cells. Conversely, in general flexible foams, the formation of a polyurethane structure by the reaction of polyol and isocyanate, and the foam swelling caused by the reaction heat and blowing agent are stopped as the structure becomes stronger due to the progress of crosslinking, so that all the cell (air bubble) membranes in the structure break (open) and become interconnected (continuous ventilation).

[0087] The formulation of low-resilience (viscoelastic) foam is similar to that of general soft foam, but the raw material polyol is designed to incorporate structural elements with viscoelasticity. This makes it more difficult to achieve cell interconnection, and surfactants with high open cell effect are becoming more important. Furthermore, in the fields of HR foam and microcellular foam by mechanical foaming method, various applications have been created by managing the open cell rate. The foam stabilizer suitable for low-resilience urethane foam is selected depending on the type of isocyanate compound used. Normally, in formulations using high-viscosity polymeric isocyanates such as MDI, the foam state is easily stabilized, so it is sufficient to use a polyether-modified silicone foam stabilizer (main component is a structure in which polyether side chains are grafted to an organopolysiloxane main chain) for general soft foam. On the other hand, in formulations using TDI as the main component of isocyanate, the viscosity of the system is low, so stabilization is difficult with the general foam stabilizers mentioned above, and (AB)n-type polyether-modified silicone foam stabilizer with excellent foam retention is required. A recipe for viscoelastic foam is exemplified in Patent Document 16, and it is preferable to use the "aromatic hydrocarbon solvent-free (AB)n-type polyether-modified silicone foam stabilizer" of the present invention instead of the "organosilicone surfactant" used therein. However, since the hydroxyl value of the foam stabilizer changes depending on the type and amount of diluent, it is necessary to fine-tune the amount of isocyanate added so that the crosslink density of the urethane resin system can be designed as desired.

[0088] In this way, the "aromatic hydrocarbon solvent-free (AB)n-type polyether-modified silicone foam stabilizer" of the present invention can be used in polyurethane foam formulations of various foam types, and can meet the needs of the current polyurethane industry, which requires strict VOC (volatile organic compound) control and emission control.

[0089] Preferably, the "aromatic hydrocarbon solvent-free (AB)n type polyether-modified silicone foam stabilizer" of the present invention can be used as one raw material in the following polyurethane foam-forming composition. (a) a polyol, (b) polyisocyanates, (c) a catalyst; (d) a foam stabilizer according to the present invention, and (e) Optionally, at least one additive component other than component (d) may be contained, which is selected from the group consisting of foam stabilizers, blowing agents, diluents, chain extenders, crosslinking agents, water, non-aqueous blowing agents, fillers, reinforcing agents, pigments, dyes, colorants, flame retardants, antioxidants, anti-ozone agents, ultraviolet stabilizers, antistatic agents, bactericides, and antibacterial agents. Each component is outlined below.

[0090] [(a) Polyol] Examples of polyols include polyether polyols and polyester polyols. Polyether polyols are those obtained by adding alkylene oxides to polyhydric alcohols, sugars, phenols, phenol derivatives, aromatic amines, etc., and include those obtained by adding alkylene oxides to one or more of glycerin, propylene glycol, dipropylene glycol, ethylene glycol, diethylene glycol, trimethylolpropane, pentaerythritol, sucrose, sorbitol, novolac, nonylphenol, bisphenol A, bisphenol F, tolylenediamine, diphenylmethanediamine, etc. Other useful polyols are polymer polyols or graft polymer polyols, graft polyols, or copolymer polyols, which are dispersions of vinyl polymers in a base polyol produced by polymerization of a vinyl monomer (usually styrene or acrylonitrile) in the base polyol. Also included are polyols derived from natural materials such as castor oil, chemically modified soybean oil, and chemically modified fatty acid oils, and polyols produced by alkoxylation of natural materials such as castor oil and soybean oil. Examples of polyester polyols include polyols having terminal hydroxyl groups produced by condensation polymerization of polyfunctional carboxylic acids such as adipic acid, phthalic acid, and succinic acid with polyfunctional hydroxyl compounds such as glycerin, propylene glycol, dipropylene glycol, ethylene glycol, diethylene glycol, trimethylolpropane, and pentaerythritol. The polyols may be used alone or in combination of two or more. In order to produce polyurethane foams with low VOC / emissions or odors, it is preferable to add a non-volatile antioxidant to the polyols.

[0091] Suitable polyols for preparing the polyurethane foams of the present invention have from 2 to 8 hydroxyl groups per molecule and have a number average molecular weight of from 200 to 10,000, preferably from 500 to 7500. Examples of useful polyether polyols include Voranol 220-028, Voranol 220-094, Voranol 225, Voranol 270, Voranol 490 and Voranol 800 products (Dow Chemical Company) and Arcol 11-34 (Bayer Material Science), and the like.

[0092] Polyols, such as polyether polyols and polyester polyols, usually have a hydroxyl number in the range of about 15 to about 700. The hydroxyl number is preferably about 20 to 60 for flexible foams, about 100 to 300 for semi-flexible (or semi-rigid) foams, and about 250 to 700 for rigid foams. For flexible foams, the preferred functionality, i.e., the average number of hydroxyl groups per polyol molecule of the polyol, is about 2 to 4, most preferably about 2.3 to about 3.5. For rigid foams, the preferred functionality is about 2 to about 8, most preferably about 3 to about 5.

[0093] As a foam stabilizer suitable for most polyurethane foam formulations, the "(AB)n-type polyether-modified silicone foam stabilizer free of aromatic hydrocarbon solvents" obtained by the manufacturing method of the present invention can be used. The blending amount of the (A) linear polyether-organopolysiloxane block copolymer in the (AB)n-type polyether-modified silicone foam stabilizer is in the range of 0.1 to 10 parts by mass, preferably 0.5 to 5 parts by mass, and more preferably 1.0 to 3.0 parts by mass, per 100 parts by mass of polyol.

[0094] [(b) Polyisocyanate] As the polyisocyanate, any of the known organic polyisocyanates can be used, but the most common are tolylene diisocyanate (hereinafter abbreviated as "TDI") and diphenylmethane diisocyanate (hereinafter abbreviated as "MDI"). TDI can be a mixture of isomers, i.e., 100% 2,4-isomer, 2,4-isomer / 2,6-isomer = 80 / 20, 65 / 35 (mass ratios), etc., as well as crude TDI containing multifunctional tar. As for MDI, in addition to pure products mainly composed of 4,4'-diphenylmethane diisocyanate, polymeric MDI containing trinuclear or higher polynuclears can be used. In addition, naphthalene diisocyanate (NDI) is suitable for applications requiring particular strength.

[0095] Of these isocyanate compounds, MDI is usually used for the production of rigid polyurethane foams, while TDI is often used for the production of flexible polyurethane foams.

[0096] Among the polyisocyanates, isocyanate prepolymers of MDI are prepared by reacting MDI with polyols, such as those modified with uretonimine, and any ratio of combinations with the above-mentioned MDI derivatives. Also suitable are prepolymers based on toluene diisocyanate (TDI), including isocyanate prepolymers of TDI prepared by reacting the 2,4 and 2,6 isomers of TDI with polyols, and other aromatic or aliphatic polyisocyanates and uretonimine modified polyisocyanates and their prepolymers. Mixtures of different types of polyisocyanates can also be used.

[0097] The amount of polyisocyanate in the formulation relative to the amount of isocyanate-reactive materials is expressed by the "isocyanate index". The "isocyanate index" is the actual amount of polyisocyanate used divided by the stoichiometric amount of polyisocyanate required to react with all active hydrogens in the reaction mixture, multiplied by 100. The isocyanate index in polyurethane foam-forming compositions is generally 60 to 140. Typically, the isocyanate index is generally 85 to 120 for flexible TDI foams, usually 90 to 105 for molded TDI foams, which are high resilience (HR) foams, usually 70 to 90 for molded MDI foams, and generally 90 to 130 for rigid MDI foams. Some examples of polyisocyanurate rigid foams are produced with a high index of 250 to 400.

[0098] [(c) Catalyst] Nickel acetoacetonate, iron acetoacetonate, tin catalyst, bismuth catalyst, zinc catalyst, titanium catalyst, aluminum complex, zirconium complex, potassium octylate, potassium acetate, sodium acetate, sodium octylate, metal oxide particles having solid acid sites on the surface, triethylenediamine, tertiary amine urethane catalyst such as bis(dimethylaminoethyl)ether, imidazole derivative, quaternary ammonium carboxylate, delayed-acting tertiary amine catalyst, general-type tertiary amine catalyst, low-emission tertiary amine catalyst, non-emission tertiary amine catalyst, and DABCO (registered trademark) catalyst can be used. In order to produce polyurethane foam with low VOC / emission or odor, it is preferable to use a reactive amine catalyst in which the catalyst is incorporated into the resin skeleton during the urethane-forming reaction.

[0099] Of these catalysts, amine-based catalysts are preferred for the production of rigid polyurethane foams, while a combination of amine-based catalysts and tin-based catalysts is preferred for the production of flexible polyurethane foams.

[0100] [(d) A foam stabilizer for polyurethane foams comprising (A) a linear polyether-organopolysiloxane block copolymer obtained by the production method of the present invention and (B) a (poly)glycol or a polyglycol derivative] The details of the "aromatic hydrocarbon solvent-free (AB)n-type polyether-modified silicone foam stabilizer" according to the present invention are as described above. In general, there is a correlation between the compatibility of the polyether-modified silicone, which is the main component of the foam stabilizer, with the type of polyurethane foam. The foams suitable for low molecular weight substances are listed in order from those suitable for high molecular weight substances, as follows: High elasticity foam < Hard foam < Soft foam < Microcellular foam It becomes.

[0101] In addition, the structure of the polyether group of the polyether-modified silicone also greatly affects the size of the foam, so there are methods for broadening the molecular weight distribution of the polyether portion, such as selecting a polyether structure with a high EO content when reducing the cell size and reducing the breathability, selecting a polyether with a high molecular weight when stabilizing and maintaining bubbles, widening the process range, and using multiple polyethers with different molecular weights and structures as raw materials to make it compatible with a wide range of applications and formulations, which can also be applied to the (AB)n-type polyether-modified silicone foam stabilizer of the present invention. Also, since polyol, one of the main raw materials for polyurethane, has a PPG structure, it is often desirable to have the polyether portion in the polyether-modified silicone also contain a PO (propyleneoxy) chain from the viewpoint of compatibility in the foam formulation or premix.

[0102] The requirements for the foam stabilizer vary depending on the type of polyurethane foam into which the "aromatic hydrocarbon solvent-free (AB)n-type polyether-modified silicone foam stabilizer" of the present invention is blended; however, the surfactant ability and affinity for the urethane foam system can be controlled by, for example, appropriately adjusting the chain length of the organopolysiloxane containing SiH groups at both ends, represented by the general formula (4) above, the type of polyether containing alkenyl groups at both ends, represented by the general formula (5) above, and the reaction ratios thereof, or by the EO / PO% and molecular weight of the polyether portion, so that a suitable foam stabilizer can be freely designed as desired.

[0103] [(e) Optional component] Of particular importance among the optional components (e) in polyurethane foam-forming compositions are water and non-aqueous blowing agents. Water acts as a chemical blowing agent by reacting with the polyisocyanate to produce carbon dioxide gas. In addition, one or more non-aqueous blowing agents of the physical and / or chemical type may be included in the reaction mixture. Alternatively, water may be omitted in some formulations. These blowing agents may include hydrofluorocarbons such as HFC-245fa and HFC-134a, hydrofluoroolefins such as HFOs and HCFOs, and low boiling hydrocarbons such as iso-, cyclo-, and n-pentane, supercritical carbon dioxide, formic acid, and the like.

[0104] In both flexible and rigid foams, water is often used as a reactive blowing agent. In the production of flexible slab foams, water can generally be used at a concentration of, for example, 2 to 6.5 parts per 100 parts of polyol, typically 3.5 to 5.5 parts. In high resilience (HR) foams, the water content in TDI molded foams is typically, for example, 3 to 4.5 parts. In MDI molded foams, the water content is typically, for example, 2.5 to 5 parts. On the other hand, the water content in rigid foams is, for example, 0.5 to 5 parts, typically 0.5 to 1 part. Physical blowing agents such as blowing agents based on volatile or halogenated hydrocarbons or other non-reactive gases can also be used. A significant proportion of the rigid insulating foam produced is blown with volatile or halogenated hydrocarbons, with the preferred blowing agents being hydrofluorocarbons (HFCs) and the volatile hydrocarbons pentane and cyclopentane. Hydrofluoroolefins (HFOs, HCFOs) can also be used. In the production of flexible slab foams, water is the primary blowing agent, although other blowing agents can be used as auxiliary blowing agents. In flexible slab foams, the preferred auxiliary blowing agents are carbon dioxide and dichloromethane. High resilience (HR) foams generally do not use inert auxiliary blowing agents, and in any case have lower amounts of auxiliary blowing agent than slab foams. However, in some molding techniques, the use of carbon dioxide is paramount. The amount of blowing agent varies depending on the desired foam density and foam hardness. When a hydrocarbon type blowing agent is used, the amount can be, for example, a trace amount to 50 parts per 100 parts polyol, and CO2 can be, for example, about 1 to about 10%.

[0105] However, especially for microcellular applications, polyurethane foams produced by chemical foaming using water, hydrofluorocarbons, low boiling point hydrocarbons, etc. as a blowing agent have too low hardness, making it difficult to achieve the dimensional accuracy required for the final product, and also have insufficient mechanical strength such as tensile strength and abrasion resistance, so high density foams are usually produced by mechanical foaming. That is, air or nitrogen gas, etc., entrained by mechanical stirring, mainly constitutes the core of the bubbles. However, for applications requiring low cost such as carpet backing materials, microcellular foams are produced by mechanical foaming using a small amount of water as a blowing agent to increase the foam volume and a large amount of inorganic filler to provide strength.

[0106] Here, the polyol a), polyisocyanate b), catalyst c), "aromatic hydrocarbon solvent-free (AB)n-type polyether-modified silicone foam stabilizer" d), optional component e), water, non-aqueous blowing agent, and other components that can be contained in the polyurethane foam-forming composition can vary over a wide range, for example, as shown below. The blending ratios and ranges described in the cited patent documents taken up for each foam type are suitable. The reason for allowing a wide range is that the formulation of the polyurethane foam-forming composition must be adjusted depending on the required foam properties, application, foaming type, equipment, etc.

[0107] 6 to 85 parts by mass of polyol a), 10 to 80 parts by mass of polyisocyanate b), 0.01 to 5.0 parts by mass of catalyst c), 0.1 to 20 parts by mass of the polyether-polysiloxane block copolymer composition d) of the present invention, and as optional components, 0 to 6 parts by mass of water and 0 to 45 parts by mass of a non-aqueous blowing agent.

[0108] Furthermore, the mass of water that can be contained in the polyurethane foam-forming composition is preferably within the range of 0 to 10% relative to the mass of the polyol.

[0109] Other optional components e) may include any known in the art such as other polymers and / or copolymers, diluents, chain extenders, crosslinkers, fillers, reinforcing agents, pigments, dyes, colorants, flame retardants, antioxidants, anti-ozonants, UV stabilizers, antistatic agents, bactericides and antimicrobial agents, within their usual ranges of content.

[0110] For example, optional component e) may contain polyhydroxyl-terminated compounds having 2 to 8 hydroxyl groups per molecule and a molecular weight of 62 to 500, which act as crosslinkers or chain extenders. Crosslinkers having 3 to 8 hydroxyl groups include glycerin, trimethylolpropane, pentaerythritol, mannitol, sorbitol, etc. Examples of useful chain extenders having two hydroxyl groups include dipropylene glycol, tripropylene glycol, propylene glycol, diethylene glycol, triethylene glycol, 1,4-butanediol, 1,3-butanediol, ethylene glycol, 2,3-butanediol, 2-methyl-1,3-propanediol, 1,2-propanediol, 1,3-propanediol, and neopentyl glycol, etc. Diethanolamine and monoethanolamine can also be used.

[0111] Optional component e) may also include, for example, an inorganic filler or combination of fillers. Fillers include those for improving density modification, mechanical or physical performance such as sound absorption, flame retardancy or other benefits including improved economics such as calcium carbonate or other fillers to reduce the cost of foam production, aluminum hydroxide or other flame retardant fillers, barium sulfate or other high density fillers used for sound absorption, microspheres of materials such as glass or polymers to further reduce foam density. High aspect ratio fillers or reinforcing agents used to modify mechanical performance such as foam stiffness or flexibility module include manmade fibers such as crushed glass or graphite fibers; natural mineral fibers such as wollastonite; natural animal fibers such as wool or plant fibers such as cotton; manmade plate-like fibers such as crushed glass; natural mineral plate-like fillers such as mica. Any of the pigments, dyes, and colorants that may be added. Additionally, organic flame retardants, anti-ozonants, antioxidants, heat or heat-oxygen degradation inhibitors, UV stabilizers, UV absorbers or any other additives which, when added to the foam-forming composition, avoid or inhibit heat, light and / or chemical degradation of the resulting foam. Any of the known and conventional antistatic agents, germicides, antimicrobial agents and gas fade inhibitors may be included.

[0112] The polyurethane foam obtainable from the polyurethane foam-forming composition which uses the "aromatic hydrocarbon solvent-free (AB)n-type polyether-modified silicone foam stabilizer" of the present invention is preferably an aromatic hydrocarbon solvent-free, low VOC / emission type rigid foam, semi-rigid foam, flexible foam, HR foam, or microcellular foam.

[0113] Regarding the process for producing low VOC / emission type polyurethane foam from a polyurethane foam-forming composition using the "aromatic hydrocarbon solvent-free (AB)n-type polyether-modified silicone foam stabilizer" according to the present invention, various existing manufacturing processes can be used. For example, for flexible foam, polyurethane foam can be produced using the one-shot foaming method, the quasi-prepolymer method, and the prepolymer method. Common flexible foams are usually produced industrially as slab foam. Some slab foams are produced by pouring the reactant mixture into a large box (a discontinuous method called box foam), while typical slabstock foams are produced continuously by discharging the reactant mixture onto a paper-lined conveyor. The foam expands and hardens as the conveyor advances, and is cut into large blocks as it leaves the foaming machine.

[0114] In the case of rigid foams, more detailed manufacturing methods are used depending on the purpose and use. For example, "spray foam" is a method in which polyurethane foam-forming composition is sprayed and foamed at the construction site or other site to harden. "Lamination board" is mainly used as insulation material for prefabricated buildings, but it is also called "insulation board" or "continuous lamination board stock". In the manufacture of lamination board, the foamed foam-forming composition is continuously supplied through a roller between the upper and lower facing panels, and hardens as it flows, eventually resulting in a board-shaped foam with a thickness of about 10 cm. "Appliance" is foam exclusively for refrigerator insulation, and is produced in a factory in a fully automated process using the injection molding method. However, in this case, the foam-forming composition is injected into the mold, foamed and hardened, and the process is completed, and the foam is not removed from the mold. The characteristic of the formula for refrigerator foam is that water is not used as a blowing agent because insulation is emphasized (because carbon dioxide has the property of easily transmitting heat). "In-situ injection" is exactly what it sounds like: a method in which a foam-forming composition is injected into a mold on-site, foamed, and cured, and is used for purposes other than refrigeration.

[0115] Microcellular, a type of special foam, is produced by a mechanical foaming method called the mechanical froth system, which produces homogeneous, fine, high-density foam. No foaming agents are used here, and air or nitrogen gas entrained by mechanical agitation mainly forms the core of the bubbles.

[0116] Low-rebound foam, which is one of the special or flexible foams, is manufactured in the same way as general flexible or HR foams, in slab or molded form. Slab products are made by pouring the mixed liquid on a continuous conveyor, and then continuously foaming into a square or kamaboko-shaped cross section, usually 1-2m wide and 0.2-0.6m high, and then cutting into a loaf of bread of a specified length (usually 1-2m). It is shipped to processing plants in this form, and products of various shapes can be cut and processed from the slab products. Molded products are made by injecting the liquid into a plastic or metal mold, foaming it, and then removing it from the mold, and even products with complex shapes can be molded in large quantities with good dimensional accuracy.

[0117] In addition, individual polyurethane foam manufacturing methods can be appropriately selected, but in particular, the "aromatic hydrocarbon solvent-free (AB)n-type polyether-modified silicone foam stabilizer" according to the present invention can be suitably applied by replacing silicone foam stabilizers, silicone surfactants, or silicone copolymer surfactants in the polyurethane foam manufacturing methods described in the detailed descriptions, particularly the Examples, of the following patent publications or patent publications, and can contribute to low VOC / emissions of foams. Note that these detailed descriptions and disclosures of the Examples include disclosures of manufacturing equipment, and a person skilled in the art may further replace some of the components through normal design changes and appropriately change the manufacturing conditions in response to changes in viscosity, etc. Methods for producing polyurethane foams described in JP-T-2005-534770, JP-T-2005-534770, and JP-T-2010-535931; The manufacturing process for open-cell polyurethane described in JP2010-539280A Sealing materials containing urethane foams as described in JP 2012-246397 A and JP 2009-265425 A Production of urethane foams described in JP 2012-082273 A, JP 2010-247532 A, JP 2010-195870 A, JP 2002-137234 A, etc. Manufacturing of viscoelastic polyurethane foams described in JP-T-2010-500447, JP-T-2010-504391, JP-T-2010-538126, JP-T-2011-528726, JP-T-2013-529702, etc.

[0118] It is also possible to use the method for producing a polyether-polysiloxane block copolymer composition according to the present invention as a reference to synthesize a general-purpose polyether-modified silicone, the main component of which is a structure in which a polyether side chain is grafted onto an organopolysiloxane main chain, using a saturated hydrocarbon having an average carbon atom number in the range of 6 to 11 as a reaction solvent, and to obtain a foam stabilizer for low-VOC / emission polyurethane foam that is free of aromatic hydrocarbon solvents by replacing the solvent with a (poly)glycol or a (poly)glycol derivative. EXAMPLES

[0119] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited thereto. In the following composition formula, the Me3SiO group (or Me3Si group) is represented as "M", the Me2SiO group is represented as "D", and the MeHSiO group is represented as "M H " and the unit in which the methyl group in M ​​and D is modified by any of the substituents is represented as M R and D. R It is written as

[0120] <Example 1-1> In a 500 mL reactor, the average composition formula M H D 18 M H58.08g (14.52 parts) of methylhydrogenpolysiloxane represented by the average composition formula CH2=C(CH3)CH2-O(C2H4O) 35 (C3H6O) 26 Bismethallyl polyether represented by -CH2-C(CH3)=CH2 *) 141.92g (35.48 parts) of the reaction mixture and 200g (50 parts) of methylcyclohexane (MCH, boiling point 101°C) as a reaction solvent were charged, and 0.05g of a tetramethyldisiloxane solution of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum complex (Pt concentration 4.2wt%) was added while stirring under nitrogen flow. The oil bath was set to 90°C and heating of the reactor was started, and after the appearance of the internal liquid became transparent at around 60-70°C, aging was performed at 75-85°C for 3 hours. Next, 1g of the reaction liquid was sampled and confirmed by the alkali decomposition gas generation method, and the reaction was completed. The oil bath was set to 120°C and slowly reduced pressure to around 270mmHg while heating, and about 3 / 4 of the MCH was distilled off while being careful of foaming, and then the pressure was restored to 100% to add the diluent n-BuO(C3H6O) 13 200 g (50 parts) of polypropylene glycol monobutyl ether {BPPG-13} represented by -H was added. After carefully reducing the pressure to 5 mmHg or less again, the oil bath was set to 130°C and stripping was carried out at an internal liquid temperature of 105-120°C for 3 hours. This gives the average composition formula [ka] (where a=18, x1=35, y1=26, n=10) The "(AB) n-type polyether-modified silicone foam stabilizer free of aromatic hydrocarbon solvents" was obtained as a light brown transparent viscous liquid, containing (A) a linear polyether-organopolysiloxane block copolymer containing the structural unit represented by the formula (I) and (B) polypropylene glycol monobutyl ether {BPPG-13} in a ratio of 50:50. The average composition formula is shown simply, but since the molar ratio of the C=C group and the Si-H group in the raw material is C=C / SiH=1.1, both ends of the copolymer are blocked with polyether. The polyether portion here is a random adduct of ethylene oxide and propylene oxide. This foam stabilizer is particularly suitable for the production of highly breathable microcellular foam or highly breathable low-rebound foam, which is free of aromatic hydrocarbon solvents and has few environmental, health, and safety concerns. *) Contains 500ppm of natural Vitamin E

[0121] <Example 1-2> The experiment was carried out in the same manner as in Example 1-1, except that MCH was replaced with n-heptane (boiling point 98°C). The reactivity in the synthesis reaction of the linear linear polyether-organopolysiloxane block copolymer, behavior such as foaming in the diluent replacement step, and appearance of the product were the same as in Example 1-1. This foam stabilizer can be particularly suitably used for the same applications as in Example 1-1.

[0122] <Example 1-3> In a 1L reactor, the average composition formula M H D 18 M H 58.08g (14.52 parts) of methylhydrogenpolysiloxane represented by the average composition formula CH2=C(CH3)CH2-O(C2H4O) 35 (C3H6O) 26 Bismethallyl polyether represented by -CH2-C(CH3)=CH2 *)141.92g (35.48 parts) of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum complex was added to the reactor while stirring under nitrogen flow. The oil bath was set to 75°C and heating of the reactor was started. After the appearance of the internal liquid became transparent at around 70°C, aging was performed at 75-80°C for 3 hours. Next, 1g of the reaction liquid was sampled and confirmed by the alkali decomposition gas generation method, and the reaction was completed. 200g (50 parts) of polypropylene glycol monobutyl ether {BPPG-13}, a diluent, was added, the oil bath was set to 95°C, and the pressure was slowly reduced to around 60mmHg while paying attention to foaming. After the bubbling had subsided, the oil bath was heated to 120°C and stripping was carried out for 5 hours at an internal liquid temperature of 100-125°C. As a result, an "aromatic hydrocarbon solvent-free (AB) n-type polyether-modified silicone foam stabilizer" was obtained, which contains (A) a linear polyether-organopolysiloxane block copolymer and (B) polypropylene glycol monobutyl ether {BPPG-13} in a ratio of 50:50, similar to that of Example 1-1. This foam stabilizer is particularly suitable for use in the same applications as those of Example 1-1. *) Contains 500ppm of natural Vitamin E

[0123] <Example 1-4> For a 2L reactor, the average composition M H D 17 M H 217.80 g (14.52 parts) of methylhydrogenpolysiloxane represented by the average composition formula CH2=C(CH3)CH2-O(C2H4O) 35 (C3H6O) 26 Bismethallyl polyether represented by -CH2-C(CH3)=CH2 *)532.20g (35.48 parts), 0.75g of natural vitamin E, and 750g (50 parts) of 2,2,4-trimethylpentane (isooctane, boiling point 99°C) as a reaction solvent were charged, and 0.17g of tetramethyldisiloxane solution of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum complex (Pt concentration 4.2wt%) was added while stirring under nitrogen flow. The oil bath was set to 95°C and heating of the reactor was started, and after the appearance of the internal liquid became transparent at around 80-90°C, aging was performed for 2 hours. Next, 1g of the reaction liquid was sampled and confirmed by alkali decomposition gas generation method, and the reaction was completed. The oil bath was set to 130-170°C, and slowly reduced pressure to around 310-40mmHg while heating. After about 3 / 4 of the isooctane was distilled off while being careful not to foam, the pressure was restored and 750g (50 parts) of polypropylene glycol monobutyl ether {BPPG-13}, a diluent, was added. After carefully reducing the pressure to 20mmHg or less again, the oil bath was set to 150°C, and stripping was carried out for 4 hours at an internal liquid temperature of 130-145°C. As a result, an "aromatic hydrocarbon solvent-free (AB) n-type polyether-modified silicone foam stabilizer" was obtained, which contains (A) a linear polyether-organopolysiloxane block copolymer and (B) polypropylene glycol monobutyl ether {BPPG-13} in a ratio of 50:50, similar to that of Example 1-1. This foam stabilizer is particularly suitable for use in the same applications as those of Example 1-1. *) Contains 500ppm of natural Vitamin E

[0124] <Comparative Example 1-1> The experiment was carried out in the same manner as in Example 1-3, except that Isopar E (C7-C9 saturated hydrocarbon, boiling point range 115-140°C) was replaced with IP solvent 1620 (mixture containing at least C12-C13 saturated hydrocarbon, boiling point 166-202°C). The reactivity and appearance in the synthesis reaction of linear linear polyether-organopolysiloxane block copolymer were the same as in Example 1-3, but in the process of replacing the reaction solvent under reduced pressure after adding the diluent polypropylene glycol monobutyl ether {BPPG-13}, persistent bubbling occurred violently, and it took more than 6 hours for the bubbling to subside and for the state to move to the stripping keep state.

[0125] <Comparative Example 1-2> In a 1L reactor, the average composition formula M H D 18 M H 58.08g (14.52 parts) of methylhydrogenpolysiloxane represented by the average composition formula CH2=C(CH3)CH2-O(C2H4O) 35 (C3H6O) 26 Bismethallyl polyether represented by -CH2-C(CH3)=CH2 *)141.92g (35.48 parts) of acetone (boiling point 56 ° C) as a reaction solvent was charged, and 0.05g of tetramethyldisiloxane solution of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum complex (Pt concentration 4.2 wt%) was added while stirring under nitrogen flow. The oil bath was set to 60-70 ° C and heating of the reactor was started, and aging was performed for 2 hours under acetone reflux conditions at around 60, but since the appearance of the internal liquid was cloudy and the reaction rate was low, 0.05g of the platinum catalyst was added. When the reaction rate was confirmed after aging for another 3 hours, the reaction was completed but the appearance remained cloudy. The pressure was slowly reduced to around 40 mmHg, the acetone was distilled off, and the pressure was restored and 200g (50 parts) of polypropylene glycol monobutyl ether {BPPG-13} as a diluent was added. There was little foaming during this solvent-diluent exchange process. After carefully reducing the pressure to 5 mmHg or less again, the oil bath was set to 120-130°C and stripping was performed for 1 hour at an internal liquid temperature of 100-120°C. As a result, a gray-brown opaque viscous liquid was obtained.

[0126] <Comparative Example 1-3> In a 1L reactor, the average composition formula M H D 18 M H 58.08g (14.52 parts) of methylhydrogenpolysiloxane represented by the average composition formula CH2=C(CH3)CH2-O(C2H4O) 35 (C3H6O) 26 Bismethallyl polyether represented by -CH2-C(CH3)=CH2 *)141.92g (35.48 parts) of the mixture and 200g (50 parts) of ethyl acetate (boiling point 77°C) as a reaction solvent were charged, and 0.05g of a tetramethyldisiloxane solution of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum complex (Pt concentration 4.2wt%) was added while stirring under nitrogen flow. The oil bath was set to 70-80°C and heating of the reactor was started, and aging was performed for 2 hours under ethyl acetate reflux conditions at around 80°C, but the appearance of the internal liquid was cloudy and the reaction rate was low, so 0.05g of the platinum catalyst was added. When the reaction rate was confirmed after aging for another 3 hours, the reaction was completed but the appearance remained cloudy. The diluent polypropylene glycol monobutyl ether {BPPG-13} (200g (50 parts)) was added, and the oil bath was set to 120°C to gradually reduce the pressure of the reaction system in an attempt to remove the ethyl acetate. However, vigorous and persistent bubbling occurred, and it took six hours to reduce the pressure to 50mmHg or less. Bumping also occurred during the process. The appearance of the resulting liquid was a gray-brown, opaque, viscous liquid.

[0127] <Comparative Example 1-4> In a 1L reactor, the average composition formula CH2=C(CH3)CH2-O(C2H4O) 35 (C3H6O) 26 Bismethallyl polyether represented by -CH2-C(CH3)=CH2 *) 141.92g (35.48 parts) of the mixture and 0.08g of a 5% methanol solution of sodium acetate were charged, and the mixture was heated at 80°C for 1 hour under reduced pressure to 30mmHg or less to distill off the methanol. H D 18 M H58.08g (14.52 parts) of methyl hydrogen polysiloxane represented by the formula (I) and 200g (50 parts) of isopropyl alcohol (IPA, boiling point 82°C) as a reaction solvent were charged, and 0.05g of a tetramethyl disiloxane solution of 1,3-divinyl-1,1,3,3-tetramethyl disiloxane platinum complex (Pt concentration 4.2wt%) was added while stirring under nitrogen flow. After confirming that the reaction liquid had become transparent at 75°C, the reaction was completed when aging was performed for 3 hours at around 80°C. 200g (50 parts) of polypropylene glycol monobutyl ether {BPPG-13}, which is a diluent, was added, and the oil bath was set to 120°C to gradually reduce the pressure of the reaction system to remove IPA, but violent and persistent bubbling occurred, and it took 6 hours to reach a reduced pressure of 50mmHg or less. Bumping also occurred during the process. The appearance of the product was the same as in Example 1-1.

[0128] <Comparative Example 1-5> The reactor is charged with a mixture of the average composition M H D 18 M H 14.52 parts of methylhydrogenpolysiloxane represented by the average composition formula CH2=C(CH3)CH2-O(C2H4O) 35 (C3H6O) 26 35.48 parts of bismethallyl polyether represented by -CH2-C(CH3)=CH2 and 70 parts of toluene as a reaction solvent were charged and heated to 70-80°C while stirring under nitrogen flow. When 10 ppm of chloroplatinic acid in IPA solution (Pt concentration 3.8 wt%) was added, the appearance became transparent at around 85°C. The reaction was then carried out for 2 hours. 1 g of the reaction liquid was then sampled and confirmed by the alkali decomposition gas generation method, and the reaction was completed. The reaction system was gradually reduced in pressure and further heated to 125°C, and toluene was distilled off little by little while being careful about foaming. The pressure was restored when about 3 / 4 of the toluene was removed, and 25 parts of polypropylene glycol monobutyl ether {BPPG-13} was added to the reaction system, and the pressure was reduced again to carefully distill off the remaining toluene. The pressure was restored and 25 parts of BPPG-13 was added and mixed and homogenized. As a result, the average composition formula [ka] (where a=18, x1=35, y1=26, n=6) A foam stabilizer for polyurethane foam was obtained, which contains a linear polyether-organopolysiloxane block copolymer containing the structural unit represented by the formula (1) and polypropylene glycol monobutyl ether {BPPG-13} in a ratio of 50:50. The average composition formula is shown simply, but since the molar ratio of the C=C group and the Si-H group in the raw material is approximately 7:6, both ends of the copolymer are blocked with polyether. In addition, since some of the Si-H groups can undergo dehydrogenation condensation reaction with the hydroxyl groups of IPA during the reaction, it is believed that some of the copolymer ends contain the SiO-iPr structure. The polyether portion here is a random adduct of ethylene oxide and propylene oxide.

[0129] <Comparative Example 1-6> An experiment was carried out in the same manner as in Comparative Example 1-5, except that the amount of toluene used was changed from 70 parts to 50 parts. However, the appearance after the reaction was opaque. Therefore, the experiment was interrupted without carrying out the planned solvent-diluent replacement process.

[0130] <Example 2-1> In a 300 mL reactor, the average composition formula M H D 18 M H 31.64 g (15.82 parts) of methylhydrogenpolysiloxane represented by the average composition formula CH2=C(CH3)CH2-O(C2H4O) 38 (C3H6O) 19 Bismethallyl polyether represented by -CH2-C(CH3)=CH2 *)68.36g (34.18 parts) of ethanol and 100g (50 parts) of Isopar E (C7-C9 saturated hydrocarbon, boiling point range 115-140 ° C) as a reaction solvent were charged, and 0.03g of tetramethyldisiloxane solution of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum complex (Pt concentration 4.2 wt%) was added while stirring under nitrogen flow. The oil bath was set to 80 ° C and heating of the reactor was started, and after the appearance of the internal liquid became transparent at around 80-85 ° C, aging was performed for 3 hours. Next, 1g of the reaction liquid was sampled and confirmed by the alkali decomposition gas generation method, and the reaction was completed. 300g (150 parts) of polypropylene glycol monobutyl ether {BPPG-13} as a diluent was added, the oil bath was set to 100-115 ° C, and the pressure was slowly reduced to 30 mmHg or less while paying attention to foaming. Stripping was carried out at an internal liquid temperature of 110-120°C for 1.5 hours. This gives the average composition formula [ka] (where a=18, x1=38, y1=19, n=20) The "(AB) n-type polyether-modified silicone foam stabilizer free of aromatic hydrocarbon solvents" was obtained as a pale yellow transparent liquid, containing (A) a linear polyether-organopolysiloxane block copolymer containing the structural unit represented by the formula (I) and (B) polypropylene glycol monobutyl ether {BPPG-13} in a ratio of 25:75. Note that the average composition formula is shown simply, but since the molar ratio of the C=C group and the Si-H group in the raw material is C=C / SiH=1.05, both ends of the copolymer are blocked with polyether. Note that the polyether portion here is a random adduct of ethylene oxide and propylene oxide. *) Contains 500ppm of natural Vitamin E This foam stabilizer does not contain aromatic hydrocarbon solvents and poses few environmental, health and safety concerns, and is particularly suitable for producing low-density microcellular foams or for reducing the cell size of microcellular foams.

[0131] <Example 2-2> The experiment was carried out in the same manner as in Example 2-1, except that Isopar E was replaced with methylcyclohexane (MCH, boiling point 101°C). The reactivity in the synthesis reaction of the linear linear polyether-organopolysiloxane block copolymer and the appearance of the product were the same as in Example 2-1, and the foaming during the diluent replacement step was less than in Example 2-1 and was good. This foam stabilizer can be particularly suitably used for the same applications as in Example 2-1.

[0132] <Comparative Example 2-1> The experiment was conducted in the same manner as in Example 2-1, except that Isopar E (C7-C9 saturated hydrocarbon, boiling point range 115-140°C) was replaced with IP solvent 1620 (mixture containing at least C12-C13 saturated hydrocarbon, boiling point 166-202°C). The reactivity and appearance in the synthesis reaction of linear linear polyether-organopolysiloxane block copolymer were similar to those in Example 1-3, but in the process of replacing the reaction solvent under reduced pressure after adding the diluent polypropylene glycol monobutyl ether {BPPG-13}, bubbling was more intense than in Example 2-1, and careful and slower decompression operation was required. Stripping was performed for 1.5 hours at 50 mmHg or less and an internal liquid temperature of 105-115°C.

[0133] <Comparative Example 2-2> In a 1L reactor, the average composition formula CH2=C(CH3)CH2-O(C2H4O) 38 (C3H6O) 19 Bismethallyl polyether represented by -CH2-C(CH3)=CH2 *) The mixture was charged with 68.36 g (34.18 parts) of sodium acetate and 0.08 g of a 5% methanol solution of sodium acetate, and the pressure was reduced to 30 mmHg or less at 80°C for 1 hour to distill off the methanol. H D 18 M H31.64g (15.82 parts) of methyl hydrogen polysiloxane represented by the formula (I) and 200g (50 parts) of isopropyl alcohol (IPA, boiling point 82°C) as a reaction solvent were charged, and 0.05g of a tetramethyl disiloxane solution of 1,3-divinyl-1,1,3,3-tetramethyl disiloxane platinum complex (Pt concentration 4.2wt%) was added while stirring under nitrogen flow. After that, aging was performed for 3 hours at about 80°C, and the reaction was completed. 300g (75 parts) of polypropylene glycol monobutyl ether {BPPG-13} as a diluent was added, and the oil bath was set to 120°C to gradually reduce the pressure of the reaction system to remove the IPA, but very violent and persistent bubbling occurred, and it took 7 hours to reach a reduced pressure of 50mmHg or less. Bumping also occurred during the process. The appearance of the product was the same as in Example 2-1.

[0134] [Physical properties of foam stabilizers according to examples and comparative examples] The design structure, contents, appearance, kinetic viscosity (mm2 / s) at 25°C, number average molecular weight Mn of the main component (A) measured by GPC for each of the foam stabilizers obtained in the above Examples 1-1 to 1-4, Examples 2-1 and 2-2, Comparative Examples 1-1 to 1-5, and Comparative Examples 2-1 and 2-2 are shown in Tables 1 and 2 below.

[0135] All of the above foam stabilizers contain the linear polyether-organopolysiloxane block copolymer shown below as component (A). [ka]

[0136] All of the above foam stabilizers contain polypropylene glycol monobutyl ether (BPPG-13) as component (B). n-BuO(PO) 13 -H

[0137] [Table 1]: Design structure and contents of foam stabilizer obtained in the examples [Table 1]

[0138] [Table 2]: Design structure and contents of foam stabilizer obtained in comparative examples [Table 2]

[0139] The measurement conditions for the above GPC analysis are as follows. "GPC measurement conditions" Eluent: Chloroform (special grade reagent) Measurement temperature: 40℃ Detector: Refractometer (peak detection on the positive side) Flow rate: 1.0mL / min Calibration: Performed with standard polystyrene Sample solution injection volume: 100μL (sample concentration 1% by weight)

[0140] [Suitability of reaction solvents according to the examples and comparative examples to the foam stabilizer manufacturing process] Regarding the reaction solvents used in the above Examples 1-1 to 1-5, Examples 2-1, 2-3, and 2-5, Comparative Examples 1-1 to 1-5, and Comparative Examples 2-1 and 2-4, a list was compiled showing the suitability of each solvent from the standpoint of conformity with the requirement of not containing (using) an aromatic hydrocarbon solvent, productivity in the production of the foam stabilizer (including ease of the process, the degree / time of the foaming phenomenon, and safety), reactivity in hydrosilylation, and product appearance (compatibility (presence or absence of turbidity), etc.). The criteria for reactivity, compatibility, and productivity are as follows:

[0141] Reactivity "Excellent": The reaction solvent is essentially inert to the hydrosilylation reaction, and the reaction is confirmed to be complete within 2 to 3 hours of aging in the reaction process. "Good": A side reaction may occur due to the reaction solvent having a hydroxyl group, but the side reaction can be suppressed by improving the formulation by using a buffer component, and the hydrosilylation reaction is completed within 2 to 3 hours of aging. "Fair": The hydrosilylation reaction was not completed after aging for 2 to 3 hours, but the reaction was completed after adding the same amount of catalyst as the initial amount and aging for another 3 hours. "Bad": The hydrosilylation reaction is slow and does not reach completion even after aging for more than 6 hours despite the above measures.

[0142] compatibility "Excellent": The reaction solvent was essentially inert to the hydrosilylation reaction, and the appearance of the solution at the end of the reaction was transparent (because the reaction solvent used was compatible with both the main raw materials, organopolysiloxane and polyether, and it can be considered that it promoted the contact and reaction between the two). "Good": The reaction solvent is essentially inert to the hydrosilylation reaction, and the appearance of the solution at the end of the reaction is semi-transparent and uniform to almost transparent. "OK": When a buffer component is added to suppress the side reaction of Si-OC formation, such as when an alcohol-based solvent is used, a transparent to semi-transparent, uniform solution appearance is obtained at the end of the reaction. "Bad": The solution is opaque and very turbid at the end of the reaction.

[0143] Productivity "Good": The process can be safely carried out while controlling foaming during the solvent-diluent replacement process, and the time required to reach full vacuum operation is judged to be at the same level as the current product with "reaction solvent = toluene" (2 to 3 hours on a lab scale). "OK": The process can be safely carried out while controlling foaming during the solvent-diluent replacement process, but the time required to reach full vacuum operation is slightly longer than in the case of "reaction solvent = toluene" (4 to 5 hours on a lab scale). "Bad": The process was able to proceed while somehow managing the foaming during the solvent-diluent replacement process, but the time it took to reach full vacuum operation was much longer than in the "reaction solvent = toluene" case, and it is considered unrealistic to carry out this as a production activity (more than 6 hours on a lab scale). "Not acceptable": In the solvent-diluent replacement process, bubbling is intense and persistent, making process management difficult, and bumping occurs even with careful pressure reduction operations, or the product is cloudy in appearance and does not meet the standards, making it impossible to apply to production.

[0144] [Table 3]: Characteristics of reaction solvents used in the examples and their suitability for foam stabilizer manufacturing processes [Table 3]

[0145] [Table 4] Characteristics of reaction solvents used in the comparative examples and their suitability for foam stabilizer manufacturing processes [Table 4] *) When IPA is used, it is necessary to add a buffer component such as sodium acetate to control the side reaction of Si-OC formation in order to achieve molecular weight growth of the (AB)n copolymer. Without this, the hydrosilylation reaction rate decreases and the product may become cloudy in appearance, so the compatibility of the reaction solvent was judged to be acceptable. #) Toluene is different from "saturated hydrocarbon solvents having an average carbon atom number of 6 to 11" in that it does not give a product with a transparent appearance when used in an amount of 50 parts (Comparative Example 1-6), but it finally gave a product with a transparent appearance when used in an amount of 70 parts. Therefore, the compatibility was determined to be "good."

[0146] From the above results, it can be seen that the method for producing a polyether-polysiloxane block copolymer composition, which includes a step of selecting a saturated hydrocarbon having an average carbon number of 6 to 11 and using it as a synthetic reaction solvent for an (AB)n copolymer, and replacing the solvent with a (poly)glycol or a (poly)glycol derivative, makes it possible to efficiently and safely produce an "aromatic hydrocarbon solvent-free (AB)n polyether-modified silicone foam stabilizer". It has been found that saturated hydrocarbons having an average carbon number of 6 to 11 are excellent as a synthetic reaction solvent for an (AB)n copolymer, and a transparent product appearance can be achieved with fewer parts than the conventionally used toluene. The foam stabilizer thus obtained can be used as a raw material for low VOC / emission polyurethane foams free of aromatic hydrocarbon solvents or premixes therefor, and contributes to expanding the scope of use of the foam in the electronic materials field and as environmentally friendly automotive parts or consumer goods (bed mats, sofas, pillows, etc.).

[0147] <Example 3-1> For a 2L reactor, the average composition M H D 14 M H 84.30 g (11.24 parts) of methylhydrogenpolysiloxane represented by the average composition formula CH2=C(CH3)CH2-O(C2H4O) 39 (C3H6O) 20 Bismethallyl polyether represented by -CH2-C(CH3)=CH2 *)215.70g (28.76 parts) of the mixture and 300g (40 parts) of methylcyclohexane (MCH, boiling point 101°C) as a reaction solvent were charged, the oil bath was set to 90°C, and heating and stirring were started under nitrogen flow. 0.13g of a 10wt% IPA solution of chloroplatinic acid (Pt concentration 4.8wt%) was added, and after 15 minutes the internal liquid reached 79°C and became transparent in appearance, so aging was performed from this point for 3.5 hours. Next, 1g of the reaction liquid was sampled and confirmed by the alkali decomposition gas generation method, and the reaction was completed. The oil bath was set to 110°C, and the pressure was slowly reduced to around 270-110mmHg while heating, and about 3 / 4 of the MCH was distilled off while paying attention to foaming, and then the pressure was restored and 225g (30 parts) of polypropylene glycol represented by HO(C3H6O)7-H, which is the first diluent, was added. Next, set the oil bath to 140°C, slowly reduce the pressure to 190-20mmHg while heating, and while being careful not to foam, distill off the remaining MCH. Then, restore the pressure and add the second diluent, HO(C3H6O). 34 225 g (30 parts) of polypropylene glycol represented by -H was added and mixed with the internal liquid to make a homogenate. This gives the average composition formula [ka] (where a=14, x1=39, y1=20, n=20) The "(AB) n-type polyether-modified silicone foam stabilizer free of aromatic hydrocarbon solvents" was obtained as a light brown, transparent, viscous liquid, containing (A) a linear polyether-organopolysiloxane block copolymer containing the structural unit represented by the formula (1) and (B) polypropylene glycol (wherein the two types, 7-mer and 34-mer, are contained in equal amounts by mass) in a ratio of 40:60. The kinetic viscosity of this foam stabilizer was 29,600 mm2 / s (25°C). Although the average composition formula is shown simply, the molar ratio of the C=C group and the Si-H group in the raw material is around C=C / SiH=1.05, so both ends of the copolymer are blocked with polyether. The polyether portion here is a random adduct of ethylene oxide and propylene oxide. This foam stabilizer is particularly suitable for producing low-breathability or low-density microcellular foams that do not contain aromatic hydrocarbon solvents and have few environmental, health, and safety concerns. *) Contains 500ppm of natural Vitamin E

[0148] <Example 3-2> For a 2L reactor, the average composition M H D 17 M H 92.48g (12.33 parts) of methylhydrogenpolysiloxane represented by the average composition formula CH2=C(CH3)CH2-O(C2H4O) 39 (C3H6O) 20 Bismethallyl polyether represented by -CH2-C(CH3)=CH2 *) 207.53g (27.67 parts) of the mixture and 300g (40 parts) of methylcyclohexane (MCH, boiling point 101°C) as a reaction solvent were charged, the oil bath was set to 90°C, and heating and stirring were started under nitrogen flow. 0.13g of a 10wt% IPA solution of chloroplatinic acid (Pt concentration 4.8wt%) was added, and after 20 minutes the internal liquid reached 77°C and became transparent in appearance, so aging was performed for about 3 hours from this point. Next, 1g of the reaction liquid was sampled and confirmed by the alkali decomposition gas generation method, and the reaction was completed. The oil bath was set to 120°C, and the pressure was slowly reduced to around 280-110mmHg while heating, and about 3 / 4 of the MCH was distilled off while paying attention to foaming, and then the pressure was restored and 225g (30 parts) of polypropylene glycol represented by HO(C3H6O)7-H, which is the first diluent, was added. Next, set the oil bath to 135°C, slowly reduce the pressure to 170-6mmHg while heating, and while being careful not to foam, distill off the remaining MCH. Then, restore the pressure and add the second diluent, HO(C3H6O). 34 225 g (30 parts) of polypropylene glycol represented by -H was added and mixed with the internal liquid to make a homogenate. This gives the average composition formula [ka] (where a=17, x1=39, y1=20, n=20) The "(AB) n-type polyether-modified silicone foam stabilizer free of aromatic hydrocarbon solvents" was obtained as a light brown, transparent, viscous liquid, containing (A) a linear polyether-organopolysiloxane block copolymer containing the structural unit represented by the formula (1) and (B) polypropylene glycol (wherein the two types, 7-mer and 34-mer, are contained in equal amounts by mass) in a ratio of 40:60. The dynamic viscosity of this foam stabilizer was 33,400 mm2 / s (25°C). Although the average composition formula is shown simply, the molar ratio of the C=C group and the Si-H group in the raw material is around C=C / SiH=1.05, so both ends of the copolymer are blocked with polyether. The polyether portion here is a random adduct of ethylene oxide and propylene oxide. This foam stabilizer is particularly suitable for producing low-breathability or low-density microcellular foams that do not contain aromatic hydrocarbon solvents and have few environmental, health, and safety concerns. *) Contains 500ppm of natural Vitamin E

[0149] <Example 3-3> The experiment was carried out in the same manner as in Example 1-1, except that 0.05 g of the tetramethyldisiloxane solution (Pt concentration 4.2 wt%) of the 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum complex was replaced with 0.06 g of a 10% IPA solution (Pt concentration 3.8 wt%) of chloroplatinic acid. The reactivity and transparency of the composition in the synthesis reaction of the linear polyether-organopolysiloxane block copolymer were the same as in Example 1-1, and behavior such as foaming in the diluent replacement process was suppressed in this experiment. The reason for this is that when an alcohol solution of chloroplatinic acid is used, a part of the SiH group reacts with the hydroxyl group of the alcohol, resulting in a slightly lower molecular weight of the linear polyether-organopolysiloxane block copolymer (A), and the viscosity of the reaction system is slightly reduced. This foam stabilizer can be particularly suitably used for the same applications as in Example 1-1.

Claims

1. Step (I): (C) in the presence of a saturated hydrocarbon solvent having an average carbon atom number in the range of 6 to 11, Structural formula: 【Chemistry 1】 (wherein a is a number from 1 to 200, each R is independently a monovalent hydrocarbon group having 1 to 9 carbon atoms and no aliphatic unsaturated bond, and X is a reactive group selected from a hydroxyl group, an alkoxy group, a dimethylamino group, a hydrogen atom, a halogen atom, a carbamate group, or another leaving group), and (A) a step of obtaining a polyether-polysiloxane block copolymer by reacting a polyether compound having, at both ends of the molecular chain, reactive groups capable of undergoing a condensation reaction or a hydrosilylation reaction with the reactive group (X); and Step (II): During or after the step, the solvent (C) used in the reaction is (B) Substitution with (poly)glycol or (poly)glycol derivative A method for producing a polyether-polysiloxane block copolymer composition, comprising:

2. 2. The method for producing a polyether-polysiloxane block copolymer composition according to claim 1, wherein the polyether-polysiloxane block copolymer (A) is a copolymer having, in the molecule, a structural unit represented by the following formula (1) or formula (2): General formula (1): 【Chemistry 2】 (In the formula, each R independently represents a monovalent hydrocarbon group having 1 to 9 carbon atoms and no aliphatic unsaturated bonds, x is a number from 2 to 4, a is a number from 1 to 200, y is a number such that the molecular weight of the polyether portion represented by (CxH2xO)y is in the range of 400 to 5000, n is a number of at least 2, and Y represents a divalent hydrocarbon group having 2 to 8 carbon atoms bonded to an adjacent silicon atom by a carbon-silicon bond and bonded to the polyoxyalkylene block by an oxygen atom.) General formula (2): 【Chemistry 3】 (In the formula, R is the same group as defined above, and x, a, y, and n are the same numbers as defined above.)

3. 3. The method for producing a polyether-polysiloxane block copolymer composition according to claim 1 or 2, wherein the polyether portion of the polyether-polysiloxane block copolymer (A) contains at least an oxypropylene unit or an oxybutylene unit, and the number average molecular weight of the copolymer is in the range of 30,000 to 150,000.

4. The method for producing a polyether-polysiloxane block copolymer composition according to any one of claims 1 to 3, wherein component (C) is a saturated hydrocarbon solvent that is substantially free of saturated hydrocarbons having an average number of carbon atoms exceeding 12.

5. The method for producing a polyether-polysiloxane block copolymer composition according to any one of claims 1 to 4, characterized in that the mass ratio (A) / (B) of the polyether-polysiloxane block copolymer (A) to the diluent (B) (poly)glycol or polyglycol derivative in the composition is within the range of 10 / 90 to 60 / 40.

6. 6. The method for producing the polyether-polysiloxane block copolymer composition according to claim 1, wherein the composition is substantially free of aromatic hydrocarbon solvents.

7. 7. The method for producing the polyether-polysiloxane block copolymer composition according to claim 1, wherein the composition is substantially free of low molecular weight siloxanes having 20 or less silicon atoms.

8. The step (I) is a step of preparing an organopolysiloxane having SiH groups at both ends, which is represented by the following formula (3): 【Chemistry 4】 (3) (In the formula, R is the same group as defined above, and a is the same number as defined above.) , and a polyether compound having carbon-carbon double bonds at both ends of the molecular chain is subjected to a hydrosilylation reaction in the presence of a saturated hydrocarbon solvent (C) having an average carbon number of 6 to 11, General formula (2): 【Chemistry 5】 (In the formula, R is the same group as defined above, and x, a, y, and n are the same numbers as defined above.) The method for producing the polyether-polysiloxane block copolymer composition according to any one of claims 1 to 7, wherein the polyether-polysiloxane block copolymer (A) has in its molecule a structural unit represented by the following formula:

9. The step (I) comprises preparing an organopolysiloxane having reactive groups at both ends, which is represented by the following formula (8): 【Chemistry 6】 (8) (In the formula, a is a number from 1 to 200, each R is independently a monovalent hydrocarbon group having 1 to 9 carbon atoms and no aliphatic unsaturated bonds, and X is a reactive group selected from a hydroxyl group, an alkoxy group, a dimethylamino group, hydrogen, a halogen, a carbamate group, or another leaving group.) and a polyether compound having hydroxyl groups at both ends, represented by the following formula (9): 【Chemistry 7】 (9) (wherein x and y are the same numbers as defined above) and (C) are subjected to a condensation reaction in the presence of a saturated hydrocarbon solvent having an average carbon number of 6 to 11, General formula (1'): 【Chemistry 8】 (In the formula, R is the same group as defined above, and x, a, y, and n are the same numbers as defined above.) The method for producing the polyether-polysiloxane block copolymer composition according to any one of claims 1 to 7, wherein the polyether-polysiloxane block copolymer (A) has in its molecule a structural unit represented by the following formula:

10. A method for producing a foam stabilizer, comprising using as a raw material a composition obtained by the method for producing a polyether-polysiloxane block copolymer composition according to any one of claims 1 to 9.

11. A method for producing a polyurethane foam-forming composition, comprising using as a raw material a composition obtained by the method for producing a polyether-polysiloxane block copolymer composition according to any one of claims 1 to 9.

12. A method for producing a polyurethane foam, comprising using as a raw material a composition obtained by the method for producing a polyether-polysiloxane block copolymer composition according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • JP1973075314A

  • Gas chromatography

    JP1977031796A

  • Method of molding insert

    JP1978012960A

  • Hydraulic driving gear