Copper alloy material and its manufacturing method

A copper alloy with a controlled multi-phase structure addresses the issue of poor press punching workability in existing alloys, achieving high conductivity and strength with reduced variations in part shape and size, and lower costs.

JP7575209B2Active Publication Date: 2024-10-29FURUKAWA ELECTRIC CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020117299
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-07
Publication Date
2024-10-29
Estimated Expiration
2040-07-07

AI Technical Summary

Technical Problem

Existing copper alloys used in electrical and automotive components suffer from poor press punching workability, leading to variations in shape and size of formed parts, and do not adequately balance high electrical conductivity and tensile strength.

Method used

A copper alloy material with a multi-phase structure, featuring a Cu matrix and second phases aligned at specific intervals, is produced through a controlled manufacturing process involving annealing and cold rolling, ensuring the second phases extend in fibrous shapes to enhance both tensile strength and press punching workability.

Benefits of technology

The copper alloy achieves high electrical conductivity, tensile strength, and improved press punching workability, reducing variations in part shape and size, while minimizing raw material and manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575209000005
    Figure 0007575209000005
  • Figure 0007575209000006
    Figure 0007575209000006
  • Figure 0007575209000007
    Figure 0007575209000007
Patent Text Reader

Abstract

To provide a copper alloy material having excellent processability for press punching while keeping high electric conductivity and high tensile strength, and a manufacturing method thereof.SOLUTION: A copper alloy material 10 has a multiple-phase structure including a first phase 11, which is a Cu mother phase, and a plurality of second phases 12 extending toward the rolling direction Y with distance d from each other. The phase distance d between neighboring second phases 12, of the plurality of second phases 12, has an average value in the range of 10 nm or more and 150 nm or less measured in the width direction x on the cross section including the rolling direction Y and the width direction x of the copper alloy material 10. The number ratio of second phase(s) 12 with a width size w in the range of 5 nm or more and 50 nm or less, measured in the width direction x, is 80% or more to the total number of second phases 12.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a copper alloy material and a manufacturing method thereof, and particularly to a copper alloy material suitable for use in lead frames, connectors, terminal materials, relays, switches, sockets, etc. for in-vehicle parts and electric / electronic devices, and a manufacturing method thereof. [Background technology]

[0002] Conventionally, copper alloy materials, for example copper alloy materials used for electrical and electronic components and automotive components, have been widely used as high-strength copper alloys strengthened mainly by precipitation strengthening and work hardening, such as Cu-Ni-Si alloys (Corson alloys).

[0003] However, Cu-Ni-Si alloys have a maximum electrical conductivity of about 50% IACS, and when a large current is passed through them, the amount of resistance heat generated increases. This can cause the springiness of the contact area to decrease due to heat, or the mold that secures the terminal to deteriorate, which can significantly reduce the functionality of the terminal, making them unsuitable for use as terminal materials for large currents.

[0004] For this reason, there is a demand to develop terminal materials to replace Cu-Ni-Si alloys. For example, alloys with a multi-phase structure in which phases containing other elements are crystallized in a Cu matrix (multi-phase alloys) can be subjected to heavy processing by cold rolling after heat treatment, in which the phases containing other elements are dispersed in a fibrous form, giving them a strength equivalent to that of phosphor bronze, and because the matrix is ​​Cu, they can also achieve high electrical conductivity. Known examples of this multi-phase alloy system include Cu-Cr, Cu-Fe, Cu-Nb, Cu-Ag, and Cu-Zr.

[0005] For example, Patent Document 1 describes that in a copper alloy containing Cr in the range of 5% by weight or more and 30% by weight or less, and one or both of Zr and Ti in the range of 0.05% by weight or more and 0.5% by weight or less in total, with the balance being Cu and unavoidable impurities, by making the thickness of the Cu matrix phase divided by the fibrous Cr phase 5 μm or less, a copper alloy material having excellent tensile strength and electrical conductivity can be obtained.

[0006] Patent Document 2 also describes that in a copper alloy containing one or more elements selected from the group consisting of Cr, Fe, and Nb in a total amount ranging from 7% by mass to 20% by mass, or containing 7% by mass to 20% by mass of Ag, with the balance being Cu and unavoidable impurities, by setting the average aspect ratio (At) of the second phase containing one or more elements selected from the group consisting of Cr, Fe, and Nb, or containing 60% or more of Ag, in the range of 10 to 80, as viewed in a cross section perpendicular to the rolling direction, excellent strength, electrical conductivity, and bending workability can be obtained, and the anisotropy of the strength and bending workability can be suppressed.

[0007] Patent Document 3 also describes that in a copper alloy containing Zr in the range of 3.0 atomic % or more and 7.0 atomic % or less, with the balance being Cu and unavoidable impurities, a Cu matrix and a composite phase consisting of a copper-Zr compound phase and a copper phase form a matrix-composite phase lamellar structure, and when viewed in a cross section perpendicular to the width direction, the Cu matrix and the composite phase are alternately arranged parallel to the rolling direction, and the copper-Zr compound phase and the copper phase arranged in the rolling direction are alternately stacked in the sheet thickness direction with a phase thickness of 50 nm or less, thereby making it possible to further increase the tensile strength.

[0008] Patent Document 4 also describes that in a copper alloy containing Ag in the range of 7% by mass or more and 15% by mass or less, and containing one or more trace elements selected from the group consisting of Cr, Fe, Nb, Co, Ni, Mg, Sn, Zr, Cd, Ti, P, In, and Si in a total range of 0.05% by mass or more and 1% by mass or less, with the remainder being Cu and unavoidable impurities, by setting the average aspect ratio (At) of the second phase containing Ag in the range of 10 to 80 when viewed in a cross section perpendicular to the rolling direction, excellent tensile strength (0.2% yield strength) can be obtained.

[0009] Patent Document 5 also describes that in a copper alloy wire containing 0.5% by mass or more and 6.0% by mass or less of Ag, 0.01% by mass or more and 1.5% by mass or less in total of one or more types selected from the group consisting of Mg, Cr and Zr, with the remainder being Cu and unavoidable impurities, by making the average nearest interparticle spacing of second phase particles having a particle size of 200 nm or less 580 nm or less when viewed in a cross section perpendicular to the longitudinal direction, excellent tensile strength (0.2% proof stress), flexibility, electrical conductivity and vibration durability can be obtained. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] Patent No. 3490853 [Patent Document 2] Patent No. 4302579 [Patent Document 3] Patent No. 5800301 [Patent Document 4] Patent No. 5048046 [Patent Document 5] Patent No. 6407484 Summary of the Invention [Problem to be solved by the invention]

[0011] However, in the copper alloys described in Patent Documents 1 to 5, in order to densely disperse second phases containing elements such as Cr, Fe, Nb, Ag, and Zr in the Cu matrix in a fibrous form, the elements must be contained in amounts that significantly exceed the solid solubility limit in the Cu matrix, and cold working with a high working rate, such as wire drawing or the lap roll bonding method (ARB method), must be performed.

[0012] Furthermore, parts made of copper alloys for in-vehicle parts and electric / electronic devices are generally formed by pressing a sheet material and then bending it, so they are required to have excellent press punching workability. In particular, in the case of copper alloy sheet material for terminals, if the press punching workability is poor, it is required to make the shape of the cut surface stable when performing press punching. Here, if the shape of the cut surface is unstable, the arrangement interval of parts such as terminals formed in series is likely to vary, and the dimensions and shapes of each formed part are likely to vary. The resulting variation in the shape of the cut surface and the dimensions and shapes of the formed parts are undesirable in manufacturing in-vehicle parts and electric / electronic parts.

[0013] Here, the copper alloys described in Patent Documents 1 and 5 have a large degree of working by obtaining wire rods through wire drawing during cold working, but there is no description of a method for obtaining a copper alloy material when obtaining a foil or plate material to be subjected to press punching.

[0014] Moreover, the copper alloys described in Patent Documents 2 and 4 are rolled plate materials in which the second phase is fiberized by rolling, and it is said that the bending workability in the direction perpendicular to the rolling direction can be improved by defining the shape of the second phase (such as the average aspect ratio expressed as (elongation length of the second phase) / (thickness of the second phase in the rolling thickness direction)). However, the copper alloys described in Patent Documents 2 and 4 make no mention of the press punching workability of the rolled plate materials.

[0015] In addition, in the copper alloys described in Patent Documents 3 and 4, the observation results of the shape of the second phase stretched into a fiber shape are shown, but in both cases, the observation surface of the polished cross section of the copper alloy after rolling (or the observation surface after etching or electrolytic polishing) was observed by SEM (scanning electron microscope), and the shape and distribution of the second phase could not be clearly observed. Therefore, it is difficult to observe the shape and distribution of the fine second phase, especially when the amount of added elements such as Ag is small, and there is no mention of controlling it.

[0016] In this regard, the copper alloys described in Patent Documents 1 to 5 have room for further improvement in terms of press punching workability.

[0017] Therefore, an object of the present invention is to provide a copper alloy material having high electrical conductivity and high tensile strength while also being excellent in press punching workability, and a method for producing the same. [Means for solving the problem]

[0018] The present inventors have found that the structure of the second phase, which could not be clearly observed in the past, can be clearly observed by observing the cross section of the rolling direction and width direction of the copper alloy material, which is a rolled material, smoothed by electrolytic polishing with a transmission electron microscope (TEM).The present inventors have also found that, when the copper alloy material is annealed and rolled under specific conditions in the cold rolling process after the aging heat treatment process, as shown in Figure 1, when viewed in the cross section including the rolling direction and width direction, the second phase (the white striped part in the photograph of Figure 1) having a predetermined width dimension extends in a fibrous manner in the rolling direction and the second phase is aligned at a predetermined average interval along the rolling direction, thereby not only obtaining high strength but also improving press punching workability. The present inventors have also found that when viewed in a cross section including the thickness direction and the width direction, the presence of a large number of second phases (white island-like parts in the photograph of FIG. 3) having a predetermined thickness and a longitudinal dimension in the width direction, as shown in FIG. 3 and FIG. 4, not only can high strength be obtained but also press punching workability can be improved. As a result, it has been found that a copper alloy material having high electrical conductivity and high tensile strength, as well as excellent press punching workability can be obtained, and the present invention has been completed.

[0019] In order to achieve the above object, the gist of the present invention is as follows. (1) A copper alloy material having a multi-phase structure including a first phase which is a Cu matrix and a plurality of second phases extending at intervals in a rolling direction, wherein, in a cross section including the rolling direction and the width direction of the copper alloy material, the plurality of second phases have an average phase spacing between adjacent second phases measured along the width direction in a range of 10 nm to 150 nm, and the proportion of second phases having a width dimension in the range of 5 nm to 50 nm, measured along the width direction, in the entire second phases is 80% or more. (2) A copper alloy material having a multi-phase structure including a first phase which is a Cu matrix and a plurality of second phases extending at intervals in a rolling direction, wherein, in a cross section including a thickness direction and a width direction of the copper alloy material, among the plurality of second phases, an abundance ratio of second phases having a thickness dimension measured along the thickness direction in a range of 1 nm or more and 50 nm or less and a width dimension measured along the width direction in a range of 100 nm or more and 500 nm or less is 0.3 pieces / μm 2 More than 4.0 pieces / μm 2 Copper alloy material in the following range: (3) A copper alloy material having a multi-phase structure including a first phase which is a Cu matrix and a plurality of second phases extending at intervals in a rolling direction, wherein, when viewed in a cross section including the rolling direction and width direction of the copper alloy material, the plurality of second phases have an average phase spacing between adjacent two phases measured along the width direction in a range of 10 nm to 150 nm, and a number ratio of second phases having a width dimension measured along the width direction in a range of 5 nm to 50 nm is 80% or more, and when viewed in a cross section including the thickness direction and width direction of the copper alloy material, an existence ratio of second phases having a thickness dimension measured along the thickness direction in a range of 1 nm to 50 nm and a width dimension measured along the width direction in a range of 100 nm to 500 nm is 0.3 pieces / μm 2 More than 4.0 pieces / μm 2 Copper alloy material in the following range: (4) The copper alloy material according to any one of the above (1) to (3), having an alloy composition comprising a single component of Ag: 1.0 mass% or more and 8.0 mass% or less, Zr: 0.5 mass% or more and 5.0 mass% or less, or Ti: 2.0 mass% or more and 5.0 mass% or less, or two components of Ni: 3.6 mass% or more and 6.5 mass% or less and Si: 0.8 mass% or more and 2.0 mass% or less, or Co: 2.0 mass% or more and 4.5 mass% or less and Si: 0.4 mass% or more and 1.5 mass% or less, with the balance being Cu and unavoidable impurities. (5) The copper alloy material according to any one of the above (1) to (3), comprising a single component of Ag: 1.0 mass% or more and 8.0 mass% or less, Zr: 0.5 mass% or more and 5.0 mass% or less, or Ti: 2.0 mass% or more and 5.0 mass% or less, or two components of Ni: 3.6 mass% or more and 6.5 mass% or less and Si: 0.8 mass% or more and 2.0 mass% or less, or Co: 2.0 mass% or more and 4.5 mass% or less and Si: 0.4 mass% or more and 1.5 mass% or less, in which, in the case of containing the two components, a Ni / Si ratio or a Co / Si ratio which is a ratio of the Ni content or the Co content to the Si content is in the range of 3.8 or more and 4.4 or less, and the balance is an alloy composition consisting of Cu and unavoidable impurities. (6) The copper alloy material according to (4) or (5) above, further containing Cr: 0.05% by mass or more and 1.5% by mass or less, Zn: 0.05% by mass or more and 1.0% by mass or less, or Mg: 0.05% by mass or more and 1.0% by mass or less. (7) A method for producing the copper alloy material according to any one of the above (1) to (6), comprising sequentially carrying out at least a casting step [step 1], a homogenization heat treatment step [step 2], a hot rolling step [step 3], a cooling step [step 4], a facing step [step 5], a first cold rolling step [step 6], a solution treatment step [step 7], a first aging heat treatment step [step 8], a second cold rolling step [step 9], a second aging heat treatment step [step 10] and a third cold rolling step [step 11] on a copper alloy material; The copper alloy material contains a single component of Ag: 1.0 mass% to 8.0 mass%, Zr: 0.5 mass% to 5.0 mass%, or Ti: 2.0 mass% to 5.0 mass%, or two components of Ni: 3.6 mass% to 6.5 mass% and Si: 0.8 mass% to 2.0 mass%, or Co: 2.0 mass% to 4.5 mass% and Si: 0.4 mass% to 1.5 mass%, and in the casting step [step 1], the copper alloy material is melted in an inert gas atmosphere or in a vacuum to prepare an ingot, and in the hot rolling step [step 3], a rolling temperature is set to 700°C or higher and a processing rate per pass is set to a total working ratio of 10.0% or more, in the first aging heat treatment step [step 8], a temperature to be reached is in the range of 350°C or more and 550°C or less and a holding time is in the range of 0.1 hour or more and 10.0 hours or less, in the second cold rolling step [step 9], a total working ratio of 5.0% or more and 20.0% or less, in the second aging heat treatment step [step 10], a temperature to be reached is in the range of 400°C or more and 600°C or less and a holding time is in the range of 0.1 hour or more and 10.0 hours or less, and in the third cold rolling step [step 11], a tension during rolling is 490 kPa or less and a total working ratio is in the range of 95.0% or more and 99.0% or less. Effect of the Invention

[0020] According to the present invention, it is possible to provide a copper alloy material having high electrical conductivity and high tensile strength while also being excellent in press punching workability, and a method for producing the same. [Brief description of the drawings]

[0021] [Figure 1] 1 is a transmission electron microscope (TEM) photograph of a cross section of a copper alloy material of the present invention, the cross section including the rolling direction and the width direction. [Diagram 2] FIG. 1 is a schematic diagram for explaining a method for determining an average value of the interphase spacing between adjacent second phases and a width dimension of the second phase from a transmission electron microscope (TEM) photograph when a cross section including the rolling direction and the width direction of the copper alloy material of the present invention is viewed. [Diagram 3]1 is a scanning electron microscope (SEM) photograph of a cross section of a copper alloy material of the present invention, the cross section including a thickness direction and a width direction. [Figure 4] FIG. 4 is a schematic diagram for explaining a method for determining the thickness and width of the second phase using the scanning electron microscope (SEM) photograph shown in FIG. [Diagram 5] FIG. 2 is a schematic diagram showing a cut surface when a press punching process is performed on the copper alloy material of the present invention. [Figure 6] FIG. 11 shows spectra obtained when an energy dispersive X-ray (EDX) analysis was performed on a cross section including the rolling direction and width direction of the copper alloy material of Example 5 of the present invention, where (a) is a spectrum obtained when the EDX analysis was performed on the first phase, and (b) is a spectrum obtained when the EDX analysis was performed on the second phase. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] Hereinafter, preferred embodiments of the copper alloy material of the present invention will be described in detail.

[0023] In a first aspect, the copper alloy material according to the present invention is a copper alloy material having a multi-phase structure including a first phase which is a Cu matrix and a plurality of second phases extending at intervals in the rolling direction, and when viewed in a cross section including the rolling direction and the width direction of the copper alloy material, the plurality of second phases have an average phase spacing between adjacent second phases measured along the width direction in the range of 10 nm or more and 150 nm or less, and the proportion of second phases having a width dimension in the range of 5 nm or more and 50 nm or less as measured along the width direction in the entire second phases is 80% or more.

[0024] In addition, in a second aspect, a copper alloy material according to the present invention is a copper alloy material having a multi-phase structure including a first phase which is a Cu matrix and a plurality of second phases extending at intervals in the rolling direction, and wherein, when viewed in a cross section including the thickness direction and width direction of the copper alloy material, among the plurality of second phases, the presence rate of second phases having a thickness dimension in the range of 1 nm or more and 50 nm or less when measured along the thickness direction and a width dimension in the range of 100 nm or more and 500 nm or less when measured along the width direction is 0.3 pieces / μm 2 More than 4.0 pieces / μm 2 The range is as follows:

[0025] Moreover, the copper alloy material according to the present invention may have both the above-mentioned first and second aspects.

[0026] In this way, when viewed in a cross section including the rolling direction and the width direction, as shown in FIG. 1, the second phase (the white striped portion in the photograph of FIG. 1) having a predetermined width dimension extends in a fibrous manner toward the rolling direction, and the second phase is aligned at a predetermined average interval along the rolling direction, so that not only high strength can be obtained but also press punching workability can be improved. Also, when viewed in a cross section including the thickness direction and the width direction, as shown in FIG. 3 and FIG. 4, the presence of many second phases (the white island-shaped portions in the photograph of FIG. 3) having a predetermined thickness dimension and having the width direction as a longitudinal dimension can not only obtain high strength but also improve press punching workability. As a result, by using the copper alloy material according to the present invention, it is possible to obtain a copper alloy material that has high electrical conductivity and high tensile strength, while also having excellent press punching workability.

[0027] In addition, in the copper alloys described in the above Patent Documents 2 and 4, among the elements constituting the second phase, Nb and Ag are expensive compared to Cu, but are added in large amounts to the copper alloy, which is undesirable because it leads to an increase in raw material costs. In addition, if an element having a higher melting point than Cu, such as Nb, Cr, Fe, or Zr, is added in large amounts to the copper alloy, the molten metal temperature must be high (1400°C or higher depending on the composition) during casting, which makes it difficult to manufacture using general copper alloy casting equipment, and therefore the manufacturing cost is likely to be high. In particular, the copper alloys described in Patent Documents 2 and 4 require the addition of 7 mass% or more of one or more selected from the group consisting of Ag, Cr, Fe, and Nb as an element contained in the second phase, and the raw material cost and manufacturing cost are higher than those of general copper alloys. In this regard, in the copper alloy material of the present invention, it is possible to reduce the content of Ag, Zr, Ti, Ni, and Co, which are components contained in the second phase, so it is also possible to obtain a copper alloy material that is excellent in terms of raw material cost and manufacturing cost.

[0028] [1] Metal structure of copper alloy material The copper alloy material 10 of the present invention has a multi-phase structure including a first phase 11 which is a Cu matrix phase, and a plurality of second phases extending at intervals in the rolling direction y.

[0029] Hereinafter, the metal structure appearing in a cross section including the rolling direction y and the width direction x, and the metal structure appearing in a cross section including the thickness direction z and the width direction x will be described separately.

[0030] <Metal structure appearing in a cross section including the rolling direction and width direction> Fig. 1 is a transmission electron microscope (TEM) photograph of a cross section including the rolling direction y and the width direction x of a copper alloy material 10 of the present invention. Also, Fig. 2 is a schematic diagram for explaining a method for determining an average value of the interphase spacing d between adjacent second phases 12 and a width dimension w of the second phase 12 from a transmission electron microscope (TEM) photograph of a cross section including the rolling direction y and the width direction x of a copper alloy material 10 of the present invention.

[0031] The copper alloy material 10 of the present invention has a multi-phase structure in which a plurality of second phases 12 are formed in a striped pattern, as shown in Fig. 1, when viewed in a cross section including the rolling direction y and the width direction x. In this multi-phase structure in a striped pattern, the average phase spacing d between adjacent second phases 12 measured along the width direction x is in the range of 10 nm or more and 150 nm or less (requirement (I)).

[0032] In this regard, a method of pinning dislocations at the interface between the first phase 11, which is the Cu matrix phase, and the second phase by rolling is known as a method of improving tensile strength by narrowing the interval between the second phases 12 in the thickness direction z, but a method of narrowing the interval between the second phases 12 in the width direction x was not known. In this regard, the present inventor discovered that not only can high tensile strength be obtained, but also press punching workability can be improved by narrowing the interval between the second phases 12 in the width direction x by controlling the alloy composition and the manufacturing process in combination.

[0033] In particular, by setting the average value of the phase spacing d between adjacent second phases 12 measured along the width direction x to 10 nm or more, the press punching workability can be improved. Also, by setting the average value of the phase spacing d between adjacent second phases 12 measured along the width direction x to 150 nm or less, the tensile strength of the copper alloy material 10 can be increased.

[0034] Here, the average value of the phase spacing d between adjacent second phases 12 measured along the width direction x when viewed in a cross section including the rolling direction y and the width direction x can be obtained using a transmission electron microscope (TEM) photograph as shown in FIG. 1. More specifically, as shown in the schematic diagram of FIG. 2, for example, a perpendicular line E perpendicular to the rolling direction y is drawn along the width direction x in the transmission electron microscope (TEM) photograph, the number of second phases 12 crossing the perpendicular line E is counted, and then the sum of the lengths of the perpendicular lines E drawn in the width direction x is divided by the total number of second phases 12 crossing the perpendicular line E plus 1, whereby the average value of the phase spacing d between adjacent second phases 12 measured along the width direction x can be calculated. Here, the perpendicular line E drawn in the transmission electron microscope (TEM) photograph may be one as shown in the schematic diagram of FIG. 2, or multiple perpendicular lines E parallel to each other may be drawn. Alternatively, this average value may be calculated from the total length of the perpendicular lines E and the total number of the second phases 12 crossing the perpendicular lines E using a plurality of transmission electron microscope (TEM) photographs.

[0035] When viewed in a cross section including the rolling direction y and the width direction x, the length of the second phase 12 along the rolling direction y is not particularly limited. From the viewpoint of increasing the tensile strength and press punching processability by increasing the fibrous second phase, the second phase 12 may have a length along the rolling direction y that is 5 times or more longer than the length along the width direction x.

[0036] In addition, in the copper alloy material 10 of the present invention, when viewed in a cross section including the rolling direction y and the width direction x, the proportion of the number of second phases 12 having a width dimension w in the range of 5 nm to 50 nm when measured along the width direction x is 80% or more of the entire second phases 12 (requirement (II)). In this way, by increasing the proportion of the number of second phases 12 having a small width dimension w, dislocations are fixed by the division of the first phase 11, which is the Cu matrix, and the strength is increased, and the second phases 12 become the starting points of cracks when performing press punching. It is considered that this has increased the tensile strength of the copper alloy material 10 and also increased the press punching workability.

[0037] The width dimension w of the second phases 12 when viewed in a cross section including the rolling direction y and the width direction x, and the proportion of the number of the second phases 12 having a width dimension w in the range of 5 nm to 50 nm can be obtained, for example, as shown in the schematic diagram of FIG. 2, by drawing a perpendicular line E perpendicular to the rolling direction y along the width direction x on a transmission electron microscope (TEM) photograph and measuring the width dimension w of the second phases 12 in a portion where the perpendicular line E and the second phases 12 overlap.

[0038] The copper alloy material 10 of the present invention may contain a second phase 12 having a width dimension w that does not fall within the range of 5 nm or more and 50 nm or less. That is, the copper alloy material 10 may contain a second phase 12 having a width dimension w of less than 5 nm or a second phase 12 having a width dimension w of more than 50 nm.

[0039] <Metal structure appearing in a cross section including the rolling direction and width direction> Fig. 3 is a scanning electron microscope (SEM) photograph of a cross section including a thickness direction z and a width direction x of the copper alloy material 10 of the present invention. Fig. 4 is a schematic diagram for explaining a method of determining a thickness dimension h and a width dimension w of the second phase 12 using the scanning electron microscope (SEM) photograph shown in Fig. 3.

[0040] The copper alloy material 10 of the present invention includes island-like second phases 12 with the width direction x as a longitudinal dimension when viewed in a cross section including the thickness direction z and the width direction x, as shown in Fig. 3, for example. More specifically, when viewed in a cross section including the thickness direction z and the width direction x, the second phases 12 having a thickness dimension h measured along the thickness direction z in the range of 1 nm to 50 nm and a width dimension w measured along the width direction x in the range of 100 nm to 500 nm are present at a density of 0.3 particles / μm 2 More than 4.0 pieces / μm 2 It is contained in the following range of abundance.

[0041] Such island-like second phases 12 are formed at a density of 0.3 particles / μm 2By containing the second phase 12 at the above-mentioned ratio, a relatively large second phase 12 is contained in large amounts, so that the second phase 12 is easily broken at the starting point during press punching, and as a result, the press punching workability of the copper alloy material 10 can be improved. In particular, if the thickness dimension h or width dimension w of the island-shaped second phase 12 is too small, it does not become a starting point of breakage during press punching, and if the ratio of the island-shaped second phase 12 of a predetermined size is small, the number of starting points of breakage decreases, and in either case, the press punching workability decreases. On the other hand, if the thickness dimension h of the second phase 12 exceeds 50 nm, the cross-sectional shape of the second phase 12 approaches a circle from a shape close to a rectangle, so that the direction of cracks generated during press punching is not aligned, and the press punching workability decreases. The upper limit of the width dimension w is not particularly limited, but can be set to 500 nm based on the size of the width dimension w that can actually be obtained. In addition, the upper limit of the abundance ratio of the second phase 12 having a predetermined size is set to 4.0 particles / μm from the size of the abundance ratio that can be actually obtained. 2 It can be said that:

[0042] The abundance ratio of the second phase 12 having a predetermined size when viewed in a cross section including the thickness direction z and the width direction x can be obtained using a scanning electron microscope (SEM) photograph as shown in FIG. 3. More specifically, from the scanning electron microscope (SEM) photograph as shown in FIG. 3, a region occupied by the second phase 12 is specified, for example as shown in the schematic diagram of FIG. 4, and the number of the second phases 12 having a thickness dimension h and a width dimension w within a predetermined range is counted. Here, the scanning electron microscope (SEM) photograph used for the measurement may be one or more. Then, the abundance ratio of the second phase 12 having a predetermined size can be calculated by dividing the number of the measured second phases 12 by the area of ​​the field of view of the scanning electron microscope (SEM) photograph.

[0043] The copper alloy material 10 of the present invention may include a second phase 12 having a thickness dimension h outside the range of 1 nm or more and 50 nm or less, or a second phase 12 having a width dimension w outside the range of 100 nm or more and 500 nm or less.

[0044] The sheet thickness of the copper alloy material 10 of the present invention is not particularly limited, but from the viewpoint of improving the workability of the copper alloy material 10 and making it easier to obtain the desired second phase 12, it is preferably in the range of 0.03 mm or more and 0.20 mm or less.

[0045] [2] Composition of copper alloy The copper alloy material of the present invention only needs to have a multi-phase structure including a first phase, which is a Cu matrix, and a plurality of second phases extending at intervals in the rolling direction, and the components to be included for generating this multi-phase structure are not particularly limited.

[0046] Among these, examples of alloy compositions of copper alloy materials capable of generating such a multi-phase structure include a single component of Ag: 1.0 mass% to 8.0 mass%, Zr: 0.5 mass% to 5.0 mass%, or Ti: 2.0 mass% to 5.0 mass%, or two components of Ni: 3.6 mass% to 6.5 mass% and Si: 0.8 mass% to 2.0 mass%, or Co: 2.0 mass% to 4.5 mass% and Si: 0.4 mass% to 1.5 mass%.

[0047] Below, we will explain each of the following cases: (a) a case containing a single component of Ag, (b) a case containing a single component of Zr, (c) a case containing a single component of Ti, (d) a case containing two components of Ni and Si, and (e) a case containing two components of Co and Si.

[0048] <(a) When containing only Ag> (Ag: 1.0 mass% or more and 8.0 mass% or less) Ag (silver) is finely precipitated in the first phase 11, which is the Cu matrix, as a compound or a simple substance, in the form of precipitates having a size of, for example, about 1 to 100 nm. The precipitates are fibrous by rolling to form a multi-phase structure containing an Ag-containing phase as the second phase 12, and the tensile strength of the multi-phase alloy can be improved. In order to exert this effect, it is preferable that the Ag content is 1.0 mass% or more. On the other hand, if the Ag content exceeds 8.0 mass%, the raw material cost becomes very high, which is undesirable. For this reason, the Ag content is preferably 1.0 to 7.2 mass%, more preferably in the range of 1.5 to 6.0 mass%, and even more preferably in the range of 2.0 to 5.5 mass%.

[0049] <(b) When only Zr is contained> (Zr: 0.5 mass% or more and 5.0 mass% or less) Zr (zirconium) is a component that causes the crystallization of a dendritic compound phase having a dendrite arm spacing (DAS) of about 100 to 1000 nm in the first phase 11, which is the Cu parent phase (matrix), and also causes the crystallization of fine precipitates having a size of about 1 to 100 nm. These precipitates and crystallizations are fiberized by rolling to form a multi-phase structure in which the second phase 12 is included at short phase intervals, and therefore have the effect of increasing the tensile strength of the copper alloy material. In order to exert this effect, it is preferable that the Zr content is 0.5 mass% or more. On the other hand, if the Zr content exceeds 5.0 mass%, the second phase 12 becomes coarse during casting, which significantly reduces the workability in the cold rolling process described below, making manufacturing difficult, and is therefore unsuitable. Therefore, the Zr content is preferably in the range of 0.8 to 5.0 mass%, more preferably in the range of 1.0 to 5.0 mass%, and further preferably in the range of 1.5 to 4.5 mass%.

[0050] <(c) When only Ti is included> (Ti: 2.0 mass% or more and 5.0 mass% or less) Ti (titanium) is a component that dissolves in the Cu matrix by performing the homogenization heat treatment process and the solution treatment process described later, and also precipitates discontinuously by performing the aging heat treatment process. The precipitates are fibrous by rolling to form a multi-phase structure in which the second phase 12 is included at short phase intervals, and therefore have the effect of increasing the tensile strength of the copper alloy material. In order to exert this effect, the Ti content is preferably 2.0 mass% or more. On the other hand, if the Ti content exceeds 5.0 mass%, the workability of the copper alloy material decreases, and the material becomes more likely to crack during the rolling process. Therefore, the Ti content is preferably in the range of 2.0 to 4.5 mass%, more preferably in the range of 2.0 to 4.0 mass%, and even more preferably in the range of 2.7 to 4.0 mass%.

[0051] <(d) When containing two components, Ni and Si> (Ni: 3.6 mass% or more and 6.5 mass% or less) Ni (nickel) is a component that discontinuously precipitates in the first phase 11, which is the Cu matrix, either as a simple substance or as a compound with Si. The precipitates elongate and fiberize in the rolling direction by rolling to form a multi-phase structure in which the second phase 12 is included at short phase intervals, and therefore have the effect of increasing the tensile strength of the copper alloy material. In order to exert this effect, it is preferable that the Ni content is 3.6 mass% or more. On the other hand, if the Ni content exceeds 6.5 mass%, the electrical conductivity decreases significantly, and Ni cannot be solid-dissolved in the homogenization heat treatment process and solution treatment process described later, so that when the aging heat treatment process is performed, the precipitation of precipitates becomes excessive, and the precipitates do not contribute to the improvement of the tensile strength. Therefore, the Ni content is preferably in the range of 3.8 to 6.2 mass%, and more preferably in the range of 4.0 to 6.0 mass%.

[0052] (Si: 0.8 mass% or more and 2.0 mass% or less) Si (silicon) is a component that discontinuously precipitates as a compound with Ni in the first phase 11, which is the Cu matrix, to become the second phase 12. To exert this effect, the Si content is preferably 0.8 mass% or more. On the other hand, if the Si content exceeds 2.0 mass%, the electrical conductivity decreases significantly, and Si cannot be dissolved in the homogenization heat treatment process or the solution treatment process described later, so that the precipitation of precipitates becomes excessive when the aging heat treatment process is performed, and the precipitates do not contribute to the improvement of the tensile strength. Therefore, the Si content is preferably in the range of 1.0 to 1.7 mass%, and more preferably in the range of 1.0 to 1.5 mass%.

[0053] Here, when the two components Ni and Si are contained, the Ni / Si ratio, which is the ratio (mass ratio) of the Ni content to the Si content, is preferably in the range of 3.8 to 4.4. By setting the Ni / Si ratio in the range of 3.8 to 4.4, it is possible to obtain a copper alloy material having a high electrical conductivity relative to the tensile strength. Therefore, the Ni / Si ratio is preferably in the range of 3.8 to 4.2.

[0054] <(e) When containing two components, Co and Si> (Co: 2.0 mass% or more and 4.5 mass% or less) Co (cobalt) is a component that discontinuously precipitates in the first phase 11, which is the Cu matrix, either as a simple substance or as a compound with Si. The precipitates elongate and fiberize in the rolling direction by rolling to form a multi-phase structure in which the second phase 12 is included at short phase intervals, and therefore have the effect of increasing the tensile strength of the copper alloy material. In order to exert this effect, it is preferable that the Co content is 2.0 mass% or more. On the other hand, if the Co content exceeds 4.5 mass%, the electrical conductivity decreases significantly, and Co cannot be solid-dissolved in the homogenization heat treatment process and solution treatment process described later, so that when the aging heat treatment process is performed, the precipitation of precipitates becomes excessive, and the precipitates do not contribute to the improvement of the tensile strength. Therefore, the Co content is preferably in the range of 2.5 to 4.2 mass%, and more preferably in the range of 2.5 to 3.5 mass%.

[0055] (Si: 0.4 mass% or more and 1.5 mass% or less) Si (silicon) is a component that discontinuously precipitates as a compound with Co in the first phase 11, which is the Cu matrix, to become the second phase 12. To achieve this effect, the Si content is preferably 0.4 mass% or more. On the other hand, if the Si content exceeds 1.5 mass%, the electrical conductivity decreases significantly, and Si cannot be dissolved in the homogenization heat treatment process or the solution treatment process described below. When the aging heat treatment process is performed, the precipitates are excessive, and the precipitates do not contribute to improving the tensile strength. Therefore, the Si content is preferably in the range of 0.6 to 1.1 mass%, and more preferably in the range of 0.6 to 1.0 mass%.

[0056] Here, when the two components Co and Si are contained, the Co / Si ratio, which is the ratio (mass ratio) of the Co content to the Si content, is preferably in the range of 3.8 to 4.4. By setting the Co / Si ratio in the range of 3.8 to 4.4, a copper alloy material having high electrical conductivity relative to tensile strength can be obtained. Therefore, the Co / Si ratio is preferably in the range of 3.8 to 4.2.

[0057] <Other optional ingredients> The copper alloy material of the present invention may contain, as other optional additive components, Cr: 0.05% by mass to 1.5% by mass, Zn: 0.05% by mass to 1.0% by mass, or Mg: 0.05% by mass to 1.0% by mass.

[0058] (Cr: 0.05 mass% or more and 1.5 mass% or less) Cr (chromium) is a component that does not form a compound with Ag, but precipitates in the Cu parent phase (matrix) by aging heat treatment, and thus has the effect of further increasing the tensile strength of the copper alloy material. In order to exert this effect, it is preferable that the Cr content is 0.05 mass% or more. On the other hand, by making the Cr content 1.5 mass% or less, the electrical conductivity of the copper alloy material is less likely to decrease, so that it is easy to obtain a desired high electrical conductivity. In addition, it is possible to make it difficult for the press punching workability to decrease due to the Cr phase that is not dissolved and is unevenly dispersed. Therefore, it is preferable that the Cr content is in the range of 0.1 mass% to 1.4 mass%.

[0059] (Zn: 0.05 mass% or more and 1.0 mass% or less) Zn (zinc) is a component that improves bending workability and also improves the adhesion and migration properties of Sn plating and solder plating. To achieve this effect, the Zn content is preferably 0.05% by mass or more. On the other hand, by setting the Zn content to 1.0% by mass or less, the electrical conductivity is less likely to decrease, making it easier to obtain a desired high electrical conductivity. For this reason, the Zn content is preferably set to a range of 0.1% by mass or more and 0.7% by mass or less, and more preferably set to a range of 0.1% by mass or more and 0.5% by mass or less.

[0060] (Mg: 0.05 mass% or more and 1.0 mass% or less) Mg (magnesium) is a component that has the effect of further increasing the tensile strength of a copper alloy material by dissolving in the Cu parent phase (matrix). To achieve this effect, the Mg content is preferably 0.05 mass% or more. On the other hand, by setting the Mg content to 1.0 mass% or less, the electrical conductivity is less likely to decrease, making it easier to obtain a desired high electrical conductivity. Therefore, the Mg content is preferably set to a range of 0.1 mass% or more and 0.4 mass% or less.

[0061] In addition, when Cr is particularly contained as another optional added component, the phase containing Cr may be precipitated as a fiberized fine precipitate similar to the second phase 12. In this case, it is preferable to distinguish the phase containing Cr from the second phase 12 by mapping the contained elements using energy dispersive X-ray analysis (EDX) or the like for a cross section including the rolling direction y and the width direction x of the copper alloy material 10 and a cross section including the thickness direction z and the width direction x.

[0062] <Balance: Cu and unavoidable impurities> Other than the above-mentioned components, the remainder is made up of Cu (copper) and inevitable impurities. Note that the "unavoidable impurities" referred to here generally refer to those present in the raw materials of metal products or those inevitably mixed in during the manufacturing process, which are essentially unnecessary but are permitted because they are present in trace amounts and do not affect the properties of the metal product. Examples of components that can be cited as inevitable impurities include tin (Sn) and oxygen (O). Note that the upper limit of the content of these components can be, for example, 0.05 mass% for each of the above components, and 0.20 mass% for the total amount of the above components.

[0063] [3] Tensile strength The copper alloy material 10 of the present invention has a tensile strength of preferably 700 MPa or more, more preferably 800 MPa or more, and more preferably 900 MPa or more when pulled in a direction parallel to the rolling direction y. As a result, even when the copper alloy material 10 is used for applications such as a connector, the desired springiness can be obtained, and high connectivity can be obtained with respect to an electrical device or the like to which it is connected. Here, the tensile strength is measured using three test pieces of No. 13B as specified in JIS Z2241:2011, cut out so that the direction parallel to the rolling direction is the longitudinal direction, and the average value of the tensile strengths obtained from the three test pieces is taken as the measured value of the tensile strength.

[0064] [4] Electrical conductivity (EC) The copper alloy material of the present invention preferably has an electrical conductivity equal to or greater than a reference value E [% IACS] represented by the following formula (A), where T [MPa] is the tensile strength. E=1200×EXP(-0.004×T) ····(A)

[0065] By making the electrical conductivity equal to or greater than the above-mentioned reference value E, the heat generated during electrical current can be reduced even when the copper alloy material is used for applications such as high-current connectors. Here, the electrical conductivity can be calculated from the resistivity measured by the four-terminal method in a thermostatic chamber maintained at 20°C (±0.5°C). In general, the electrical conductivity of copper alloys tends to decrease as the tensile strength increases. Therefore, in order to show that the electrical conductivity of copper alloys is superior to that of ordinary copper alloys even if the tensile strength is high, the smaller of the value E calculated by the above formula (A) based on the tensile strength of the copper alloy material and the electrical conductivity of oxygen-free copper, 101 [% IACS], was set as the reference value of electrical conductivity.

[0066] Furthermore, the copper alloy material of the present invention preferably has an electrical conductivity of more than 10% IACS, more preferably more than 30% IACS, even more preferably more than 60% IACS, and even more preferably more than 70% IACS.

[0067] [6] Press punching processability The copper alloy material of the present invention is a copper alloy material having a maximum value t of the total thickness of the shear surface and the fracture surface along the thickness direction when the copper alloy material is subjected to a press punching process under the condition that the clearance between the upper die and the lower die is 5.0% of the thickness of the copper alloy material. max and the minimum value t min It is preferable that the difference Δt is 30% or less of the thickness of the copper alloy material.

[0068] Fig. 5 is a schematic diagram showing a cut surface when the copper alloy material of the present invention is subjected to a press punching process. The copper alloy material 10 shown in Fig. 5 shows a cut surface 2 after press punching, which is performed by lowering an upper die (punch) while the copper alloy material 10 is fixed on a lower die (die) not shown. Here, the cut surface 2 has a sag 3, a shear surface 4, and a fracture surface 5 formed in this order from the upper surface 10a side of the copper alloy material 10 that has been press punched. In addition, a burr 6 is often formed on the lower edge of the cut surface 2 so as to extend outward from the fracture surface 5.

[0069] At this time, the maximum value t of the total thickness of the shear surface 4 and the fracture surface 5 along the thickness direction z on the cut surface 2 max and the minimum value t min The present inventors have found that the press punching workability is significantly improved by making the difference Δt between the total thickness of the shear surface 4 and the fracture surface 5 smaller than the thickness T of the copper alloy material 10. max and the minimum value t min By making the difference Δt between the thicknesses T and z smaller, when the copper alloy material 10 is subjected to a press punching process, cracks are likely to occur at the same position in the thickness direction z, so that the variation in the arrangement intervals of the formed parts and the variation in the dimensions and shapes of the formed parts can be reduced. max and the minimum value t min The difference Δt is preferably 30% or less of the plate thickness T, and more preferably 15% or less.

[0070] Here, the thickness T of the copper alloy material 10 and the maximum value t of the total thickness of the shear surface 4 and the fracture surface 5 max and the minimum value t min The measurement of the difference Δt can be performed using a scanning electron microscope (SEM) photograph of the cut surface 2. In this case, the cut surface 2 to be measured may be a cut surface 2 along the width direction x as shown in Fig. 5, but may also be a cut surface along, for example, the rolling direction y.

[0071] In addition, since the cut surface 2 formed by the press punching process often has sagging 3 and burrs 6, the sheet thickness T of the copper alloy material 10 and the total thickness of the sheared surface 4 and the fractured surface 5 often cannot be measured correctly. For this reason, it is preferable to measure the sheet thickness T of the copper alloy material 10 by measuring the sheet thickness of the unprocessed copper alloy material 10 or the unprocessed portion of the copper alloy material 10. In addition, the maximum value t max and the minimum value t minThe difference Δt may be the difference between the thickness position closest to the upper surface 10a and the thickness position closest to the lower surface 10b of the boundary between the cut surface 2 (shear surface 4) and the sag 3, with the lower surface 10b in the unprocessed portion of the copper alloy material 10 as the reference.

[0072] [7] An example of a manufacturing method for copper alloy materials The above-mentioned copper alloy material can be realized by controlling the alloy composition and the manufacturing process in combination, and the manufacturing process is not particularly limited. Among them, the following method can be mentioned as an example of the manufacturing process capable of generating such a multi-phase structure.

[0073] As an example of the manufacturing method of the copper alloy material of the present invention, at least the casting step [step 1], the homogenization heat treatment step [step 2], the hot rolling step [step 3], the cooling step [step 4], the facing step [step 5], the first cold rolling step [step 6], the solution treatment step [step 7], the first aging heat treatment step [step 8], the second cold rolling step [step 9], the second aging heat treatment step [step 10], and the third cold rolling step [step 11] are sequentially performed on a copper alloy material having substantially the same alloy composition as the above-mentioned copper alloy material. Among these, in the casting step [step 1], the copper alloy material is melted in an inert gas atmosphere or in a vacuum to prepare an ingot. In addition, in the hot rolling step [step 3], the rolling temperature is set to 700°C or higher, and the processing rate per pass is set to 10% or higher. In the first aging heat treatment step [step 8], the temperature to be reached is in the range of 350°C to 550°C, and the holding time is in the range of 0.1 hours to 10.0 hours. In the second cold rolling step [step 9], the total working ratio is set to be in the range of 5.0% to 20.0%. In the second aging heat treatment step [step 10], the temperature to be reached is in the range of 400°C to 600°C, and the holding time is in the range of 0.1 hours to 10.0 hours. In the third cold rolling step [step 11], the tension during rolling is set to 490 kPa or less, and the sum of the rolling working ratios (total working ratio) in all cold rolling steps including the first cold rolling step [step 6] and the second cold rolling step [step 9] is set to be in the range of 95.0% to 99.0%.

[0074] (i) Casting process [Process 1] In the casting process [Step 1], a copper alloy material having the above-mentioned alloy composition is melted in an inert gas atmosphere or in a vacuum using a high-frequency melting furnace, and then cast into an ingot of a given shape (e.g., 300 mm thick, 500 mm wide, and 3000 mm long). Note that the alloy composition of the copper alloy material may not necessarily be completely identical to that of the copper alloy material produced due to the fact that additive components adhere to or volatilize in the melting furnace during each manufacturing process, but it has substantially the same alloy composition as that of the copper alloy material.

[0075] In this casting process [Step 1], it is preferable to cool the melted copper alloy material from the molten metal to a temperature in the range of 300°C or less. This allows the second phase to crystallize in the ingot and suppresses the growth of the crystallized second phase, so that the second phase can be uniformly contained in the ingot. At the same time, the thickness of the second phase is reduced by rolling, which will be described later, and the second phase extends in the rolling direction, so that the tensile strength of the copper alloy material can be increased.

[0076] (ii) Homogenization heat treatment process [Process 2] The homogenization heat treatment step [step 2] is a step of performing heat treatment on the ingot after the casting step [step 1]. The homogenization heat treatment step [step 2] is performed to homogenize the metal structure of the ingot and promote the formation of a fibrous second phase in a subsequent step. The conditions of the homogenization heat treatment are not particularly limited as long as they are normally used. An example of the homogenization heat treatment conditions is a holding temperature in the range of 700°C to 1000°C and a holding time in the range of 0.1 hours to 10 hours.

[0077] (iii) Hot rolling process [Process 3] The hot rolling step [step 3] is a step of producing a hot rolled material by hot rolling the ingot that has been subjected to homogenization heat treatment until it has a predetermined thickness. The conditions of the hot rolling are, for example, preferably a rolling temperature in the range of 700°C to 1000°C, which may be the same as the holding temperature in the homogenization heat treatment step [step 2] described above. In addition, the minimum value of the processing rate per pass in the hot rolling is preferably 10% or more. Here, if the rolling temperature is less than 700°C or the minimum value of the processing rate per pass is less than 10%, the second phase generated in the casting step [step 1] does not deform together with the Cu matrix and becomes the starting point of cracking, so that cracks are likely to occur in the hot rolled material. In addition, it becomes difficult to obtain a second phase having a desired size and distribution in a subsequent step, so that it becomes difficult to obtain a copper alloy material having high press punching workability. The upper limit of the rolling temperature is not particularly limited, but may be set to, for example, 900° C. from the viewpoint of increasing the manufacturing efficiency by providing a temperature difference from the homogenization heat treatment step [step 2].

[0078] Here, the "rolling reduction rate" is a value obtained by subtracting the cross-sectional area after rolling from the cross-sectional area before rolling, dividing the value by the cross-sectional area before rolling, and multiplying the result by 100, and expressed as a percentage, and is expressed by the following formula. [Rolling reduction rate] = {([Cross-sectional area before rolling] - [Cross-sectional area after rolling]) / [Cross-sectional area before rolling]} x 100 (%)

[0079] (iv) Cooling process [Process 4] The cooling step is a step of cooling the hot-rolled material after the hot rolling step [step 3]. Here, the cooling means in the cooling step is not particularly limited, but from the viewpoint of preventing the coarsening of the second phase, it is preferable to increase the cooling rate as much as possible, and it is preferable to set the cooling rate to 50° C. / sec or more by means of water cooling, for example.

[0080] (v) Facing process [Process 5] The facing step [step 5] is a step of scraping the surface of the hot-rolled material after the cooling step [step 4]. By performing the facing step, it is possible to remove the oxide film and defects on the surface that occurred in the hot rolling step [step 3]. The conditions of the facing step are not particularly limited as long as they are usually performed. The amount of the surface of the hot-rolled material to be scraped off can be appropriately adjusted based on the conditions of the hot rolling step [step 3], and can be, for example, about 0.5 to 4 mm from the surface of the hot-rolled material.

[0081] (vi) First cold rolling process [Process 6] The first cold rolling step [step 6] is a step in which the hot rolled material after the facing step is cold rolled at an arbitrary processing rate according to the product plate thickness. The rolling conditions in the first cold rolling step [step 6] can be set according to the plate thickness of the hot rolled material. In particular, from the viewpoint of refining the crystal grains contained in the cold rolled material after the solution treatment step [step 7] described later, and thereby promoting the precipitation of the second phase that is uniformly dispersed in the first phase in the first aging heat treatment step [step 8], it is preferable to set the total processing rate in the first cold rolling step [step 6] to 60% or more.

[0082] (vii) Solution treatment process [Step 7] The solution treatment step [step 7] is a step of performing a heat treatment on the cold-rolled material after the first cold rolling step [step 6]. The heat treatment can be performed at any temperature according to the solution temperature of each composition in the Cu matrix. For example, it is preferable to set the temperature to be reached in the range of 700°C to 1000°C and the holding time at the temperature to be in the range of 10 seconds to 300 seconds. By performing the solution treatment step [step 7], coarse precipitates that do not contribute to improving the tensile strength or press punching formability can be dissolved in the Cu matrix.

[0083] (viii) First aging heat treatment step [Step 8] The first aging heat treatment step [step 8] is a step of performing heat treatment on the cold-rolled material after the solution treatment step [step 7]. Here, the conditions of the heat treatment in the first aging heat treatment step [step 8] are that the temperature reached is in the range of 350°C or more and 550°C or less, and the holding time is in the range of 0.1 hours or more and 10.0 hours or less. On the other hand, if the temperature reached is less than 350°C or the holding time is less than 0.1 hours, it becomes difficult to generate the second phase, so that the tensile strength, electrical conductivity, and press punching formability decrease. Also, if the temperature reached is more than 550°C or the holding time is more than 10.0 hours, the second phase is re-dissolved in the first phase, or the second phase is coarsened and the number decreases, so that it becomes difficult to generate the second phase in the first phase with the desired size and existence ratio, and the tensile strength and press punching formability decrease.

[0084] (ix) Second cold rolling process [Process 9] In the second cold rolling step [step 9], the cold rolled material after the first aging heat treatment step [step 8] is further subjected to cold rolling. The total processing ratio in the second cold rolling step [step 9] is preferably in the range of 5% to 20% from the viewpoint of sufficiently precipitating a second phase of a desired size in the second aging heat treatment step [step 10] described later, thereby improving the tensile strength, electrical conductivity, and press punching formability.

[0085] Here, the rolling directions in the first cold rolling step [step 6] and the second cold rolling step [step 9] are preferably substantially the same, and in that case, the second phase can be extended along the rolling direction.

[0086] (x) Second aging heat treatment step [Step 10] The second aging heat treatment step [step 10] is a step in which the cold-rolled material after the second cold rolling step [step 9] is subjected to heat treatment at an ultimate temperature in the range of 400°C to 600°C and a holding time in the range of 0.1 hours to 10.0 hours. Here, if the ultimate temperature is less than 400°C or the holding time is less than 0.1 hours, the second phase is not sufficiently generated, and the tensile strength and press punching formability are reduced. Also, if the ultimate temperature exceeds 600°C or exceeds 10.0 hours, the second phase is redissolved in the first phase, or the second phase is coarsened and the proportion of the second phase is reduced, and the tensile strength, electrical conductivity, and press punching formability are reduced.

[0087] (xi) Third cold rolling process [Process 11] In the third cold rolling step [step 11], the cold rolled material after the second aging heat treatment step [step 10] is further subjected to cold rolling. Here, in the third cold rolling step [step 11], it is preferable to set the tension during rolling to 490 kPa or less. This prevents the width of the second phase 12 from becoming too narrow when the second phase 12 extends along the rolling direction y, and also appropriately controls the magnitude of the shear strain applied to the inside of the copper alloy material 10, so that the copper alloy material 10 having high tensile strength, electrical conductivity, and press punching formability can be obtained.

[0088] Furthermore, in the third cold rolling step [step 11], the total processing rate including the first cold rolling step [step 6] and the second cold rolling step [step 9] is adjusted to be 95.0% or more and 99.5% or less. By making this total processing rate 95.0% or more, the second phases 12 are generated in large amounts along the rolling direction y, and the intervals between the second phases 12 become smaller, so that the tensile strength and press punching formability of the copper alloy material 10 can be improved. In addition, by making the total processing rate 99.5% or less, second phases of a desired size can be easily obtained, so that the press punching formability can be improved.

[0089] Here, it is preferable that the rolling direction in the third cold rolling step [step 11] is substantially the same as the rolling directions in the first cold rolling step [step 6] and the second cold rolling step [step 9], and in that case, the second phase can be extended along these rolling directions.

[0090] [8] Applications of copper alloys The copper alloy material of the present invention is suitable for use in, for example, in vehicle-mounted parts and lead frames, connectors, terminal materials, relays, switches, sockets, and the like for electric and electronic equipment.

[0091] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and includes all aspects encompassed by the concept of the present invention and the scope of the claims, and can be modified in various ways within the scope of the present invention. EXAMPLES

[0092] Next, in order to further clarify the effects of the present invention, examples of the present invention and comparative examples will be described, but the present invention is not limited to these examples.

[0093] (Examples 1 to 33 of the present invention and Comparative Examples 1 to 24) A copper alloy material having the alloy composition shown in Table 1 was melted, and the molten alloy was cooled to 300°C and cast in a casting process [Step 1] to obtain an ingot. This ingot was subjected to a homogenization heat treatment process [Step 2] in which heat treatment was performed at a holding temperature of 950°C for a holding time of 3 hours, and then a hot rolling process [Step 3] was performed in one pass at the rolling temperature shown in Table 3, with the longitudinal direction being the rolling direction, so that the minimum value of the processing rate per pass was the value shown in Table 3, to obtain a hot-rolled material. Then, a cooling process [Step 4] was performed in which the material was cooled to room temperature by water cooling.

[0094] After the cooling process [step 4], the hot-rolled material was subjected to a facing process [step 5] to remove both the front and back surfaces and the oxide film on the surface, and then the first cold rolling process [step 6] was performed in which the material was rolled along the longitudinal direction at a total processing rate of 75%.

[0095] The rolled material after the first cold rolling step [step 6] was subjected to a solution treatment step [step 7] under conditions of an ultimate temperature of 700 to 1000°C and a holding time of 10 to 300 seconds, and then the first aging heat treatment step [step 8] was performed under the ultimate temperature and holding time conditions shown in Table 3.Then, the second cold rolling step [step 9] was performed in which the material was rolled so that the longitudinal direction was the rolling direction under the total rolling reduction ratio conditions shown in Table 3.

[0096] The rolled material after the second cold rolling step [step 9] was subjected to a second aging heat treatment step [step 10] under the conditions of the attained temperature and holding time shown in Table 3, and then a third cold rolling step [step 11] was performed in which the material was rolled such that the longitudinal direction was the rolling direction under the conditions of the tension during rolling and the total rolling reduction ratio (the sum of the rolling reduction ratios of the first cold rolling step [step 6], the second cold rolling step [step 9], and the third cold rolling step [step 11]) shown in Table 3. In this manner, the copper alloy material of the present invention was produced.

[0097] In Table 1, Ag, Zr, Ti, Ni, Co and Si are listed as second phase constituents, regardless of whether a second phase is formed or not, and constituents other than the second phase constituents and copper (Cu) are listed as other optional added components. Also, in Table 1, a horizontal line "-" is entered in the column for components that are not included in the alloy composition of the copper alloy material, to clarify that the corresponding component is not included, or even if it is included, it is below the detection limit.

[0098] [Various measurement and evaluation methods] The copper alloy materials according to the above-mentioned invention examples and comparative examples were used to carry out the following characteristic evaluations. The evaluation conditions for each characteristic were as follows.

[0099] [1] Phase 2 Observations and Measurements For each of the prepared test materials (copper alloy materials 10), a cross section including the rolling direction y and the width direction x was electrolytically polished, and then Ar ion milling was performed to prepare a TEM sample, which was observed at an acceleration voltage of 200 kV using a transmission electron microscope (TEM) (manufactured by JEOL Ltd., product name: JEM-2100Plus). At this time, a portion that appeared in one field of view and had a different color tone from the Cu parent phase (first phase 11) was defined as a second phase 12.

[0100] The cross section including the rolling direction y and the width direction x was observed by a transmission electron microscope (TEM) at 10 randomly selected points in the cross section in a field of view of 800 nm horizontal × 600 nm vertical. Next, for each transmission electron microscope (TEM) photograph, three lines (perpendicular lines E) with a length of 0.5 μm were drawn along the width direction x at intervals of 0.2 μm in the rolling direction y, and the number of second phases 12 crossing these lines was counted. The sum of the lengths of the lines drawn in the width direction x was then divided by the total number of second phases 12 crossing the lines plus 1 to calculate the average value of the phase spacing d between adjacent second phases 12 when measured along the width direction x, which is requirement (I).

[0101] Furthermore, for these transmission electron microscope (TEM) photographs, three lines (perpendicular lines E) each having a length of 0.5 μm were drawn along the width direction x at intervals of 0.2 μm in the rolling direction y, and the width dimension w of the second phase 12 was determined at the portions where the lines overlapped with the second phase 12. Then, from the determined width dimension w of the second phase 12, the proportion by number of second phases having a width dimension w in the range of 5 nm to 50 nm inclusive, which is requirement (II), was calculated.

[0102] For each of the prepared test materials (copper alloy materials 10), a cross section including the thickness direction z and the width direction x was subjected to Ar ion milling to prepare a SEM sample, and a secondary electron image was observed at an accelerating voltage of 5 kV using a scanning electron microscope (SEM) (manufactured by Hitachi High-Tech Corporation, product name: SU8020). At this time, a portion that appears in one field of view and has a different color tone from the Cu parent phase (first phase 11) was designated as a second phase 12.

[0103] The cross section including the thickness direction z and the width direction x was observed by a scanning electron microscope (SEM) at 10 randomly selected locations within the cross section in a field of view of 4 μm horizontal × 3 μm vertical. For these scanning electron microscope (SEM) photographs, the number of second phases 12 having a thickness dimension in the thickness direction z in the range of 1 nm to 50 nm and a width dimension in the width direction x in the range of 100 nm to 500 nm was counted. The number of second phases 12 thus counted was then multiplied by the total area (120 μm) of the scanning electron microscope (SEM) photographs. 2 ) to calculate the presence ratio of the second phase 12 having a thickness dimension in the range of 1 nm or more and 50 nm or less and a width dimension in the range of 100 nm or more and 500 nm or less, which satisfies requirement (III). The results of these requirements (I) to (III) are shown in Table 2.

[0104] [2] Tensile strength measurement method The tensile strength was measured using three test pieces of JIS Z2241:2011 No. 13B, cut out from the test material so that the longitudinal direction was parallel to the rolling direction, and the average value of the tensile strength obtained from the three test pieces was taken as the measured value. In this example, a tensile strength of 700 MPa or more was considered to be the pass level. The results are shown in Table 4.

[0105] [3] Electrical conductivity (EC) measurement method The electrical conductivity was calculated from the resistivity measured by the four-terminal method in a thermostatic chamber maintained at 20°C (±0.5°C). The distance between the terminals was 100 mm. In this example, the standard value E [%IACS] of electrical conductivity was calculated by the following formula (A) based on the measured tensile strength T [MPa] of the above-mentioned test material, and the measured electrical conductivity M was determined to be equal to or greater than the standard value E as a pass level. The results are shown in Table 4. E=1200×EXP(-0.004×T) ····(A)

[0106] [4] Method for measuring press punching workability Each of the prepared test materials (copper alloy materials) was subjected to a punching process with the clearance between the upper die (punch) and the lower die (die) adjusted to 5.0% of the sheet thickness T, and the test material was punched into a rectangle with a long side of 3.0 mm along the width direction x and a short side of 1.0 mm along the rolling direction y to form a cut surface 2. In this example, the surface along the width direction x of the formed cut surfaces 2 was observed at a magnification of 100 to 500 times using a scanning electron microscope (SEM) (manufactured by Hitachi, Ltd., SEMEDX Type M). Then, from the scanning electron microscope (SEM) photograph of the cut surface 2, the sheet thickness T of each test material and the maximum value t of the total thickness of the shear surface 4 and the fracture surface 5 along the thickness direction z were obtained. max and the minimum value t min The difference Δt was measured. This difference Δt was determined as the difference between the thickness position at the boundary between the cut surface 2 and the sag 3 closest to the upper surface 10a and the thickness position at the boundary between the cut surface 2 and the sag 3 closest to the lower surface 10b, with the lower surface 10b in the unprocessed portion of the copper alloy material 10 as a reference.

[0107] The maximum total thickness of the measured shear and fracture surfaces, t max and the minimum value t min When the difference Δt was within the range of 15% or less of the plate thickness T, the press punching workability was evaluated as excellent and was marked with a "◎". When the difference Δt was within the range of 15% or more and 30% or less of the plate thickness T, the press punching workability was evaluated as being at an acceptable level and was marked with a "○". On the other hand, when the difference Δt was more than 30% of the plate thickness T, the press punching workability was evaluated as being unacceptable and was marked with a "×". The results are shown in Table 4.

[0108] [Table 1]

[0109] [Table 2]

[0110] [Table 3]

[0111] [Table 4]

[0112] From the results of Tables 1 to 3, the copper alloy materials 10 of Examples 1 to 3, 5, 6, 8 to 10, 13 to 15, 17, 19, 21 to 23, 25 to 27, 29, 30, and 33 have alloy compositions within the appropriate range of the present invention, and when viewed in a cross section including the rolling direction y and the width direction x of the copper alloy material 10, the average value of the phase spacing d between adjacent second phases 12 measured along the width direction x is in the range of 10 nm to 150 nm, so that the requirement (I) is satisfied. In addition, the number ratio of the second phases 12 having a width dimension w in the range of 5 nm to 50 nm in the entire second phases 12 is 80% or more, so that the requirement (II) is satisfied. Therefore, the tensile strength is 700 MPa or more, the electrical conductivity is higher than the reference value E, and the press punching workability is evaluated as "◎" or "◯".

[0113] In addition, the copper alloy materials 10 of Examples 1, 2, 4, 5, 7 to 9, 11 to 13, 15 to 21, 23 to 25, 27 to 29, and 31 to 33 have an alloy composition within the appropriate range of the present invention, and when viewed in a cross section including the thickness direction z and the width direction x of the copper alloy material, the presence ratio of the second phase 12 having a thickness dimension h in the range of 1 nm to 50 nm and a width dimension w in the range of 100 nm to 500 nm is 0.3 particles / μm 2 More than 4.0 pieces / μm 2 In order to satisfy requirement (III) by being within the following range, the tensile strength must be 700 MPa or more, the electrical conductivity must be higher than the standard value E, and the press-punching processability must be evaluated as "◎" or "〇".

[0114] Therefore, the copper alloy materials 10 of Examples 1 to 33 satisfied both the requirements (I) and (II), or satisfied the requirement (III), and therefore had a high tensile strength of 700 MPa or more, a conductivity higher than the reference value E, and the press-punching processability was evaluated as "◎" or "◯", and therefore had excellent press-punching processability.

[0115] On the other hand, in the copper alloy materials of Comparative Examples 1 to 24, at least one of the requirements (I) and (II) is outside the appropriate range of the present invention, and the requirement (III) is outside the appropriate range of the present invention, so that at least one of the tensile strength, the difference between the reference value E and the measured value M of the electrical conductivity, and the press punching workability did not reach the acceptable level. Among them, in Comparative Examples 2, 16, and 23, the precipitation of the second phase was not observed or was small. In particular, in Comparative Examples 2, 16, and 23, even after the second aging heat treatment step [step 10] was performed, the second phase having a width dimension w in the range of 5 nm to 50 nm in the requirement (II) and the second phase having a thickness dimension h in the range of 1 nm to 50 nm and a width dimension w in the range of 100 nm to 500 nm in the requirement (III) were not precipitated, so that the specified copper alloy material could not be obtained. In addition, in Comparative Example 11, cracks were found in the ingot during the hot rolling step [step 3], and therefore the desired copper alloy material could not be obtained.

[0116] 6 shows a spectrum obtained when an energy dispersive X-ray (EDX) analysis was performed on a cross section including the rolling direction y and the width direction x for the copper alloy material 10 of the present invention example 5. Here, FIG. 6(a) shows a spectrum obtained when an EDX analysis was performed on the first phase 11 of the copper alloy material 10, and FIG. 6(b) shows a spectrum obtained when an EDX analysis was performed on the second phase 12 of the copper alloy material 10. From the result of the EDX analysis, it was confirmed that the copper alloy material 10 of the present invention example has the first phase 11 constituted by a phase made of Cu, and the second phase 12 constituted by a phase containing Cu and Ag. [Explanation of symbols]

[0117] 10 Copper alloy material 10a Top surface of copper alloy material 10b Bottom surface of copper alloy material 11 Phase 1 12 Phase 2 2 Cut surface 3 Sauce 4 Shear plane 5 Fracture surface 6. Bali d, d1 to d4: Interphase spacing between adjacent second phases w Width of second phase h Thickness of the second phase t max Maximum total thickness of shear and fracture surfaces t min Minimum total thickness of shear and fracture surfaces T Thickness of copper alloy material 10 E Perpendicular x width direction y rolling direction z thickness direction

Claims

1. A single component comprising Ag: 1.0% by mass or more and 8.0% by mass or less, Zr: 0.5% by mass or more and 5.0% by mass or less, or Ti: 2.0% by mass or more and 5.0% by mass or less, or Two components: Ni: 3.6% by mass to 6.5% by mass and Si: 0.8% by mass to 2.0% by mass, or Co: 2.0% by mass to 4.5% by mass and Si: 0.4% by mass to 1.5% by mass. and the balance being Cu and unavoidable impurities, A copper alloy material having a multi-phase structure including a first phase which is a Cu matrix phase and a plurality of second phases extending at intervals in a rolling direction, When viewed in a cross section including a thickness direction and a width direction of the copper alloy material, Among the plurality of second phases, the presence rate of second phases having a thickness dimension measured along the thickness direction in the range of 1 nm to 50 nm and a width dimension measured along the width direction in the range of 100 nm to 500 nm is 0.3 particles / μm 2 4.0 pieces / μm or more 2 Copper alloy material in the following range:

2. A single component comprising Ag: 1.0% by mass or more and 8.0% by mass or less, Zr: 0.5% by mass or more and 5.0% by mass or less, or Ti: 2.0% by mass or more and 5.0% by mass or less, or Two components: Ni: 3.6% by mass to 6.5% by mass and Si: 0.8% by mass to 2.0% by mass, or Co: 2.0% by mass to 4.5% by mass and Si: 0.4% by mass to 1.5% by mass. and the balance being Cu and unavoidable impurities, A copper alloy material having a multi-phase structure including a first phase which is a Cu matrix phase and a plurality of second phases extending at intervals in a rolling direction, When viewed in a cross section including the rolling direction and the width direction of the copper alloy material, The second phases have an average phase spacing between adjacent two phases measured along the width direction in a range of 10 nm to 150 nm, and the proportion of second phases having a width dimension in the range of 5 nm to 50 nm as measured along the width direction in the entire second phase is 80% or more; and When viewed in a cross section including a thickness direction and a width direction of the copper alloy material, Among the plurality of second phases, the presence rate of second phases having a thickness dimension measured along the thickness direction in the range of 1 nm to 50 nm and a width dimension measured along the width direction in the range of 100 nm to 500 nm is 0.3 particles / μm 2 4.0 pieces / μm or more 2 Copper alloy material in the following range:

3. A single component of Ag: 1.0% by mass or more and 8.0% by mass or less, Zr: 0.5% by mass or more and 5.0% by mass or less, or Ti: 2.0% by mass or more and 5.0% by mass or less, or Two components: Ni: 3.6% by mass to 6.5% by mass and Si: 0.8% by mass to 2.0% by mass, or Co: 2.0% by mass to 4.5% by mass and Si: 0.4% by mass to 1.0% by mass. Contains When the two components are contained, the Ni / Si ratio or the Co / Si ratio, which is the ratio of the Ni content or the Co content to the Si content, is in the range of 3.8 to 4.4, The balance has an alloy composition consisting of Cu and unavoidable impurities, A copper alloy material having a multi-phase structure including a first phase which is a Cu matrix phase and a plurality of second phases extending at intervals in a rolling direction, When viewed in a cross section including a thickness direction and a width direction of the copper alloy material, The copper alloy material has a ratio of second phases having a thickness dimension of 1 nm or more and 50 nm or less when measured along the thickness direction and a width dimension of 100 nm or more and 500 nm or less when measured along the width direction, the ratio being in the range of 0.3 pieces / μm 2 to 4.0 pieces / μm 2 .

4. A single component comprising Ag: 1.0% by mass or more and 8.0% by mass or less, Zr: 0.5% by mass or more and 5.0% by mass or less, or Ti: 2.0% by mass or more and 5.0% by mass or less, or Two components: Ni: 3.6% by mass to 6.5% by mass and Si: 0.8% by mass to 2.0% by mass, or Co: 2.0% by mass to 4.5% by mass and Si: 0.4% by mass to 1.0% by mass. Contains When the two components are contained, the Ni / Si ratio or the Co / Si ratio, which is the ratio of the Ni content or the Co content to the Si content, is in the range of 3.8 to 4.4, The balance has an alloy composition consisting of Cu and unavoidable impurities, A copper alloy material having a multi-phase structure including a first phase which is a Cu matrix phase and a plurality of second phases extending at intervals in a rolling direction, When viewed in a cross section including the rolling direction and the width direction of the copper alloy material, The second phases have an average phase spacing between adjacent two phases measured along the width direction in a range of 10 nm to 150 nm, and the proportion of second phases having a width dimension in the range of 5 nm to 50 nm as measured along the width direction in the entire second phase is 80% or more; and When viewed in a cross section including a thickness direction and a width direction of the copper alloy material, The copper alloy material has a ratio of second phases having a thickness dimension of 1 nm or more and 50 nm or less when measured along the thickness direction and a width dimension of 100 nm or more and 500 nm or less when measured along the width direction, the ratio being in the range of 0.3 pieces / μm 2 to 4.0 pieces / μm 2 .

5. The copper alloy material according to any one of claims 1 to 4, further containing Cr: 0.05 mass% or more and 1.5 mass% or less, Zn: 0.05 mass% or more and 1.0 mass% or less, or Mg: 0.05 mass% or more and 1.0 mass% or less.

6. A method for producing the copper alloy material according to any one of claims 1 to 5, The copper alloy material is sequentially subjected to at least a casting step [step 1], a homogenization heat treatment step [step 2], a hot rolling step [step 3], a cooling step [step 4], a facing step [step 5], a first cold rolling step [step 6], a solution treatment step [step 7], a first aging heat treatment step [step 8], a second cold rolling step [step 9], a second aging heat treatment step [step 10], and a third cold rolling step [step 11]; The copper alloy material contains a single component of Ag: 1.0 mass% or more and 8.0 mass% or less, Zr: 0.5 mass% or more and 5.0 mass% or less, or Ti: 2.0 mass% or more and 5.0 mass% or less, or two components of Ni: 3.6 mass% or more and 6.5 mass% or less and Si: 0.8 mass% or more and 2.0 mass% or less, or Co: 2.0 mass% or more and 4.5 mass% or less and Si: 0.4 mass% or more and 1.5 mass% or less, In the casting step [step 1], the copper alloy material is melted in an inert gas atmosphere or in a vacuum to prepare an ingot, In the hot rolling step [step 3], the rolling temperature is set to 700° C. or more, and the processing rate per pass is set to 10% or more, In the first aging heat treatment step [step 8], the attained temperature is in the range of 350° C. or more and 550° C. or less, and the holding time is in the range of 0.1 hours or more and 10.0 hours or less, In the second cold rolling step [step 9], the total processing rate is set to a range of 5.0% or more and 20.0% or less, In the second aging heat treatment step [step 10], the attained temperature is in the range of 400° C. or more and 600° C. or less, and the holding time is in the range of 0.1 hours or more and 10.0 hours or less, In the third cold rolling step [step 11], a tension during rolling is set to 490 kPa or less, and a total working ratio is set to a range of 95.0% or more and 99.0% or less.

Citation Information

Patent Citations

  • JP1975048046A

  • Blooming method

    JP1983000301A

  • Connection of oxide superconductive matter

    JP1989007484A

  • High-strength copper alloy sheet and manufacturing method therefor

    JP2005089843A

  • Cu-Co-Si-BASED ALLOY FOR ELECTRONIC MATERIAL

    JP2013117060A