Aromatic polyester resin expanded particles, their production method, expanded molded article, and automobile component

By adjusting cooling water temperature and die hole diameter, the method addresses die clogging issues in underwater cut methods, producing aromatic polyester resin foam particles with improved mechanical properties and smaller sizes for enhanced foamed product performance.

JP7575310B2Active Publication Date: 2024-10-29SEKISUI PLASTICS CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021044098
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-17
Publication Date
2024-10-29
Estimated Expiration
2041-03-17

AI Technical Summary

Technical Problem

Existing underwater cut methods for producing aromatic polyester resin foam particles face issues with die hole clogging due to cooled and viscous resin, leading to large particle sizes and poor mechanical properties, limiting the filling rate and mechanical strength of foamed products.

Method used

Adjusting the temperature of cooling water and die hole diameter within specific ranges to prevent clogging, allowing for smaller particle sizes and improved mechanical strength through controlled foaming processes.

Benefits of technology

The method enables the production of aromatic polyester resin foam particles with small particle sizes and enhanced mechanical properties, such as increased compressive strength and modulus, by minimizing die hole blockage and optimizing foaming conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575310000004
    Figure 0007575310000004
  • Figure 0007575310000005
    Figure 0007575310000005
  • Figure 0007575310000001
    Figure 0007575310000001
Patent Text Reader

Abstract

To provide an aromatic polyester-based resin foam molding which is excellent in mechanical properties, and aromatic polyester-based resin foam particles having a small particle diameter for producing the foam molding, or a method for producing the foam particles.SOLUTION: Aromatic polyester-based resin foam particles have a particle diameter of 1.5-4.5 mm, and thickness of the resin layer on the surface of 5-40 μm.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an aromatic polyester resin foamed bead for in-mold foam molding, a production method thereof, a foam molded article, and an automobile part. [Background technology]

[0002] In-mold foam molding has been widely used as a method for producing an aromatic polyester resin foam molded article by foaming aromatic polyester resin foam particles. In-mold foam molding is a molding method including a step of filling a mold with resin foam particles, and a step of heating the resin foam particles filled in the mold with a heat medium such as hot water or steam to cause secondary foaming, and heat-fusing and integrating the secondary foam particles together to produce an in-mold foam molded article having a desired shape.

[0003] The expanded aromatic polyester resin particles are produced by melt-kneading in an extruder, extruding and foaming from a die, and then cutting. In this case, the hot cut method, the underwater cut method, etc. are used. The granulator used in the recent underwater cut method has a die equipped with many die holes for extruding the molten resin, and it is possible to extrude the molten resin into water from the multiple locations at once and form a large number of expanded beads by cutting with a cutter at one time, and the production efficiency of expanded beads is further improved. For example, in Patent Document 1, the expanded aromatic polyester resin particles are produced by the underwater cut method, that is, the method of cutting and cooling the extruded molten kneaded resin in water. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] European Patent Application Publication No. 2564799 Summary of the Invention [Problem to be solved by the invention]

[0005] However, in the underwater cut method, the front surface (resin discharge surface) of the mold (die) is in contact with water during the production of expanded beads, and the outlet of the die hole is opened underwater to produce resin particles. Therefore, the resin, which has become highly viscous upon cooling, may partially block or completely block (clog) the flow path of the die hole, which may excessively increase the amount of molten resin discharged from the unblocked die hole, resulting in the formation of coarse expanded beads. Therefore, if the die hole diameter is small, defective products frequently occur due to clogging, so the hole diameter could not be made small. In Patent Document 1, the hole diameter is 1.8 mm to 2.0 mm, the cooling water temperature is 20 ° C to 90 ° C, and the particle diameter of the obtained expanded beads is large, 5 mm or more. However, if the particle diameter of the expanded beads is small, it is easy to increase the filling rate of the expanded beads in the molding die, so expanded beads with a small particle diameter are desirable. If the particle size is large, the foaming power cannot be increased, and the filling rate cannot be increased when the foamed particles are filled into a molding die. As a result, it is difficult to improve the mechanical properties of the resulting foamed molded article, such as the compressive strength and compressive modulus.

[0006] An object of the present invention is to provide an aromatic polyester resin foamed molded article having excellent mechanical properties.An object of the present invention is to provide aromatic polyester resin foamed beads having a small particle size for producing the foamed molded article.An object of the present invention is to provide a method for producing the foamed beads. [Means for solving the problem]

[0007] The present inventors have discovered that in the underwater cut method, by adjusting the cooling water temperature and die hole diameter within a predetermined range, clogging is less likely to occur even if the die hole diameter is made small, and blockage is less likely to occur even when a die with a small hole diameter is used, expanded beads with a small particle size can be obtained, and an expanded molded article obtained from these expanded beads has superior mechanical strength to an expanded molded article obtained from expanded beads with a large particle size, and have completed the present invention.

[0008] The present invention typically includes the following aspects. Section 1. Aromatic polyester resin foamed particles having a particle diameter of 1.5 mm to 4.5 mm and a surface resin layer having a thickness of 5 μm to 40 μm. Section 2. Item 2. The expanded aromatic polyester resin particles according to item 1, wherein the average cell diameter (C) in the center of the particle and the average cell diameter (D) in the surface layer portion of the particle are both 50 μm to 300 μm, and the ratio (D / C) of the average cell diameter in the surface layer portion to the average cell diameter in the center portion is 0.75 to 0.98. Section 3. Item 3. The expanded aromatic polyester resin particle according to item 1 or 2, wherein the crystallinity (A) in the center portion of the particle and the crystallinity (B) in the surface portion of the particle are both 10% or less, and the ratio (B / A) of the crystallinity in the surface portion to the crystallinity in the center portion is 0.90 to 1.5. Section 4. 4. The expanded aromatic polyester resin particle according to any one of items 1 to 3, wherein the degree of crystallinity (A) in the center portion of the particle and the degree of crystallinity (B) in the surface portion of the particle are both 1 to 10%. Section 5. Item 5. An expansion molded product of the expanded aromatic polyester resin particles according to any one of items 1 to 4. Section 6. Density is 0.05g / cm 3 ~0.7g / cm 3 Item 7. The foamed molded article according to item 6, wherein Section 7. Item 7. An automotive component comprising the foamed molded article according to item 5 or 6. Section 8. A method for producing expanded aromatic polyester resin particles, comprising the steps of: supplying an aromatic polyester resin to an extruder and melt-kneading the resin in the presence of a foaming agent; cutting the melt-kneaded aromatic polyester resin extrudate from a die attached to the front end of the extruder while extruding and foaming the extrudate in cooling water to produce granular cut products; and cooling the granular cut products with cooling water, wherein the die has a hole diameter of 0.5 mm to 1.7 mm and the cooling water has a temperature of 55°C to 90°C. Effect of the Invention

[0009] According to the present invention, it is possible to provide an aromatic polyester resin expanded particle capable of producing an expanded molded article having excellent mechanical properties and a method for producing the same. According to the present invention, it is possible to provide an expanded molded article having excellent mechanical properties, such as compressive strength and compressive elastic modulus, and an automobile member containing the same. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a schematic diagram of an underwater cutting type granulator used in one embodiment. [Diagram 2] FIG. 4 is a side cross-sectional view showing the state of a diverter valve. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] As used herein, the phrase "comprising" is intended to encompass the phrases "consisting essentially of" and "consisting of."

[0012] (Aromatic polyester resin foam particles) The expanded aromatic polyester resin particles contain an aromatic polyester resin as a main component. Here, the term "main component" means that the resin constituting the expanded aromatic polyester resin particles contains 80 to 100 mass %, preferably 90 to 100 mass %, of the aromatic polyester resin.

[0013] (Aromatic polyester resin) The aromatic polyester resin is a polyester containing an aromatic dicarboxylic acid component and a diol component, and examples thereof include polyethylene terephthalate, polypropylene terephthalate, polybutylene terephthalate, polycyclohexane dimethylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, etc., with polyethylene terephthalate being preferred. The aromatic polyester resin may be used alone or in combination of two or more kinds.

[0014] In addition to the aromatic dicarboxylic acid component and the diol component, the aromatic polyester resin may contain, as a constituent component, for example, a trivalent or higher polyvalent carboxylic acid such as a tricarboxylic acid such as trimellitic acid, a tetracarboxylic acid such as pyromellitic acid, or an anhydride thereof, a triol such as glycerin, or a trivalent or higher polyhydric alcohol such as a tetraol such as pentaerythritol.

[0015] The aromatic polyester resin may be derived not only from petroleum but also from plants or recycled materials recovered and regenerated from used PET bottles.

[0016] The intrinsic viscosity (IV value) of the aromatic polyester resin is preferably 0.7 to 1.1, and more preferably 0.75 to 1.05, in order to provide excellent extrusion foamability and excellent secondary foamability of the resulting expanded beads.

[0017] The intrinsic viscosity (IV value) of the aromatic polyester resin refers to a value measured in accordance with JIS K7367-5 (2000). Specifically, the aromatic polyester resin is dried at 40° C. under a vacuum of 133 Pa for 15 hours.

[0018] Take 0.1000g of the aromatic polyester resin as a sample and place it in a 20mL measuring flask, then add about 15mL of a mixed solvent (phenol 50% by weight, 1,1,2,2-tetrachloroethane 50% by weight) to the measuring flask. Place the sample in the measuring flask on a hot plate and heat it to about 130°C to melt it. After melting the sample, cool it to room temperature and adjust the volume to 20mL to prepare a sample solution (sample concentration: 0.500g / 100mL).

[0019] 8 mL of the sample solution is supplied to the viscometer using a whole pipette, and the temperature of the sample is stabilized using a water bath filled with 25°C water, after which the flow time of the sample is measured. To change the concentration of the sample solution, 8 mL of the mixed solvent is added to the viscometer in sequence, mixed, and diluted to produce a diluted sample solution. The flow time of the diluted sample solution is then measured. The flow time of the mixed solvent is measured separately from the sample solution. Determine.

[0020] The intrinsic viscosity of the aromatic polyester resin was calculated based on the following formula: The following was calculated from the flow time (t0) of the mixed solvent and the flow time (t) of the sample solution. Relative viscosity (η r ) =t / t0 Specific viscosity (η sp )=(t-t0) / t0=η r -1 Reduced viscosity = η sp / C From the measurement results of diluted sample solutions with various sample solution concentrations C (g / 100 mL), a graph was created with the reduced viscosity on the vertical axis and the sample solution concentration C on the horizontal axis, and the intrinsic viscosity [η] was calculated from the vertical intercept obtained by extrapolating the linear relationship to C = 0.

[0021]

number

[0022] The aromatic polyester resin constituting the aromatic polyester resin foamed particles may be modified aromatic polyester resin crosslinked by a crosslinking agent.As the crosslinking agent, a known one is used, for example, an acid dianhydride such as pyromellitic anhydride, a polyfunctional epoxy compound, an oxazoline compound, an oxazine compound, etc.In addition, the crosslinking agent may be used alone or in combination of two or more kinds.

[0023] When the aromatic polyester resin is modified by crosslinking with a crosslinking agent, the aromatic polyester resin and the crosslinking agent are fed to an extruder during the production of the expanded aromatic polyester resin particles, and the aromatic polyester resin is crosslinked with the crosslinking agent in the extruder. The amount of the crosslinking agent fed to the extruder is preferably 0.01 to 5 parts by mass, more preferably 0.1 to 1 part by mass, per 100 parts by mass of the aromatic polyester resin, from the viewpoint of performing the extrusion foaming well.

[0024] The mass average molecular weight of the aromatic polyester resin constituting the expanded beads of the present invention is preferably 45,000 to 100,000, more preferably 60,000 to 90,000, in order to provide excellent extrusion foamability and excellent secondary foamability of the resulting expanded beads. When the aromatic polyester resin constituting the expanded beads is a modified aromatic polyester resin, the mass average molecular weight of the aromatic polyester resin means the mass average molecular weight of the modified aromatic polyester resin.

[0025] The mass average molecular weight (Mw) of the aromatic polyester resin constituting the expanded beads of the present invention means the mass average molecular weight in terms of polystyrene (PS) measured using gel permeation chromatography (GPC). Specifically, the mass average molecular weight is measured as follows. 0.5 mL of hexafluoroisopropanol (HFIP) and 0.5 mL of chloroform are added to 5 mg of sample in this order to dissolve the sample (immersion time: 6.0±1.0 hr (complete dissolution)) to obtain a sample solution. After confirming that the sample is completely dissolved in the solution, chloroform is added to the sample solution to dilute it to a volume of 10 mL, and the solution is shaken and mixed. The sample solution is filtered through a non-aqueous 0.45 μm syringe filter manufactured by Shimadzu GLC Co., Ltd. to obtain a filtrate. The filtrate is measured using a chromatograph under the following measurement conditions. The mass average molecular weight (Mw) is determined from a standard polystyrene calibration curve prepared in advance. Equipment used: Tosoh Corporation's "HLC-8320GPC EcoSEC" gel permeation chromatograph (with built-in RI and UV detectors) (GPC measurement conditions) column Sample side Guard column = TSK guardcolumn HXL-H (6.0mm x 4.0cm) x 1, manufactured by Tosoh Corporation Measurement column: Tosoh Corporation's TSKgel GMHXL (7.8 mm I.D. x 30 cm) x 2 in series Reference Side Resistance tube (inner diameter 0.1 mm x 2 m) x 2 in series Column temperature = 40 °C Mobile phase = chloroform Mobile phase flow rate Sample pump: 1.0 mL / min Reference pump = 0.5mL / min Detector: UV detector Wavelength: 254nm Injection volume: 15μL Measurement time: 10 minutes - 32 minutes Runtime: 20min Sampling pitch: 500msec The standard polystyrene samples used for the calibration curve were "STANDARD SM-105" and "STANDARD SH-75" manufactured by Showa Denko K.K., with mass average molecular weights of 5,620,000, 3,120,000, 1,250,000, 442,000, 151,000, 53,500, 17,000, 7,660, 2,900, and 1,320. The above-mentioned standard polystyrene for the calibration curve is grouped into A (5,620,000, 1,250,000, 151,000, 17,000, 2,900) and B (3,120,000, 442,000, 53,500, 7,660, 1,320), and then A (2mg, 3mg, 4mg, 4mg, 4mg) is weighed and dissolved in 30mL of chloroform, and B (3mg, 4mg, 4mg, 4mg) is also weighed and dissolved in 30mL of chloroform. The standard polystyrene calibration curve is obtained by injecting 50μL of each prepared A and B solution and creating a calibration curve (cubic equation) from the retention time obtained after measurement. The mass average molecular weight is calculated using the calibration curve.

[0026] (Method of producing expanded aromatic polyester resin particles) The expanded beads of the present invention can be produced by a production method that includes, for example, a step of feeding an aromatic polyester resin to an extruder and melt-kneading it in the presence of a foaming agent, a step of cutting the melt-kneaded aromatic polyester resin extrudate from a die attached to the front end of the extruder while extruding and foaming it in cooling water to produce particulate cut pieces, and a step of cooling the particulate cut pieces with cooling water, in which the hole diameter of the die is 0.5 mm to 1.7 mm and the temperature of the cooling water is 55 ° C. to 90 ° C. Such a production method is also one of the present inventions. Note that, although this production method will be described below, the production method of the expanded aromatic polyester resin beads of the present invention is not limited to the following method.

[0027] First, an example of a production apparatus used for producing expanded aromatic polyester resin beads will be described. The production apparatus shown in Fig. 1 is a so-called underwater cutting type granulator T, which is commonly used in the field of expanded bead production. The granulation device T is equipped with an extruder 2 having a granulation die 1 attached to its tip, and a cutter 3 that cuts the molten aromatic polyester resin 20 (aromatic polyester resin in a molten state containing a foaming agent) discharged from the die hole 15 of the granulation die 1 shown in Figure 2, and a chamber 4 for bringing a cooling water flow into contact with the resin discharge surface 10f, which is the front surface of the granulation die 1. A pipe 5 for circulating cooling water is connected to the chamber 4 , and one end of the pipe 5 (upstream of the chamber 4 ) is connected to a water tank 7 via a water pump 6 . Further, at the other end of the pipe 5 (downstream of the chamber 4), a dehydration treatment section 8 is provided which separates the expandable resin particles from the cooling water and dehydrates and dries them. The expandable resin particles separated, dehydrated and dried in the dehydration treatment unit 8 are sent to a container 9, and the cooling water is returned to the water tank 7. Reference numeral 21 denotes a hopper, 22 denotes a blowing agent supply port, and 23 denotes a high-pressure pump. In the following description, the granulating device T and the granulating die 1 will be referred to consistently as the "front" or "front end" from which the resin is extruded, and the "rear" or "rear end" on the opposite side.

[0028] As shown in Figure 2, the granulation die 1 consists of a die body 10 (also called a die plate) and a die holder 11 fixed to the tip side (right side in the figure) of the extruder 2, and the die body 10 is fixed to the tip side of the die holder 11 by a plurality of bolts, and a portion of the tip side of the die holder 11 to which the die body 10 is fixed is movable and functions as a diverter valve 13.

[0029] The die holder 11 is provided in communication with the cylinder of the extruder 2, and has a rear end side flow passage 11a and a tip side flow passage 11b formed in that order from the rear end side to the tip side. The diverter valve 13 has a first flow passage 11c that penetrates from the rear end side to the tip side and a second flow passage 11d that passes from the rear end side to the side portion of the die holder 11, and relays the rear end side flow passage 11a and the tip side flow passage 11b via the first flow passage 11c.

[0030] The die body 10 has a cone-shaped protrusion 10 protruding rearward at the center of the rear end face. In a state in which the die body 10 and the die holder 11 are connected, the conical protrusion 10a is inserted into the tip side flow passage 11b of the die holder 11 with a predetermined gap therebetween. That is, the molten aromatic polyester resin 20 that passes through the rear end flow passage 11a of the die holder 11 flows along the circumferential surface of the conical convex portion 10a in the tip end flow passage 11b, and passes through multiple resin flow passages 14 to communicate with multiple die holes 15 that open into the tip end surface of the die body 10.

[0031] The die body 10 is roughly configured to include a resin discharge surface 10f whose tip surface comes into contact with the cooling water flow, a plurality of resin flow paths 14 for transporting the molten aromatic polyester resin 20 extruded from the extruder 2 toward the resin discharge surface 10f, a plurality of die holes 15 provided at the tips of the plurality of resin flow paths 14 and opening into the resin discharge surface 10f, an insulating material 16 provided at the center position of the resin discharge surface 10f, a cartridge heater 17 for heating the resin discharge surface 10f and the resin flow paths 14 at a position closer to the extruder 2 than the resin discharge surface 10f, and a short heater 18 for heating the die body 10.

[0032] The resin discharge surface 10f of the die body 10 has a heat insulating material 16 with a circular cross section arranged in the center, and a plurality of die holes 15 are provided radially outside the heat insulating material 16 with their openings lined up in the circumferential direction. The central portion of the resin discharge surface 10 f , on which the heat insulating material 16 is arranged and on which the plurality of die holes 15 are formed, is adapted to come into contact with cooling water inside the chamber 4 .

[0033] The resin flow paths 14 have a circular cross section, extend in a direction perpendicular to the resin discharge surface 10f, and are arranged at regular intervals along a circumference (a circumference drawn on the resin discharge surface 10f) centered on the central axis of the die body 10. In this embodiment, eight resin flow paths 14 are provided, and the central angle between adjacent resin flow paths 14 in the circumferential direction of the circumference is 45°. As described above, each resin flow path 14 is connected to the tip side flow path 11b of the die holder 11 and is configured to allow the molten polystyrene-based resin 20 to flow to the die hole 15 through the first flow path 11c of the diverter valve 13.

[0034] The die holes 15 are arranged at predetermined intervals along a circumference drawn on the resin discharge surface 10f, and the insulation material 16 is provided on the resin discharge surface 10f inside the circumference on which the die holes 15 are arranged, in order to prevent heat from the die body 10 from escaping to the cooling water in the chamber 4, thereby suppressing a drop in temperature of the die body 10.

[0035] The cartridge heater 17 and the short heater 18 each have a rod-like heater shape, and the cartridge heater 17 is located closer to the resin discharge surface 10f side than the short heater 18 in the direction of the front and rear ends of the granulating die 1. The cartridge heaters 17 are arranged on both circumferential sides of the circumference of the resin flow path 14, and are arranged with their longitudinal direction extending radially across the circumference, and have the function of heating the resin discharge surface 10f, the die hole 15, and the resin flow path 14 in the vicinity of the resin discharge surface 10f. In this embodiment, eight cartridge heaters 17 are provided, each at a predetermined central angle (here, an angle of 45°) in the circumferential direction. In other words, each die hole 15 is disposed so as to be sandwiched between two cartridge heaters 17 in the circumferential direction of the circumference.

[0036] The short heaters 18 are disposed at a predetermined interval behind each cartridge heater 17, and the same number (8) of short heaters 18 are disposed as the number of cartridge heaters 17, and have the function of heating the rear end side of the resin flow path 14. The length dimension of the short heaters 18 is shorter than that of the cartridge heaters 17.

[0037] The granulating die 1 is also provided with temperature measuring devices 19A and 19B for measuring the temperature of the die body 10 and the temperature of the molten resin. The first temperature measuring element 19A measures the temperature at the center of the die body 10 (temperature of the die body: die holding temperature). The second temperature measuring element 19B is for measuring the temperature and resin pressure of the molten aromatic polyester resin 20 flowing inside the die holder 11.

[0038] The extruder 2 used in the granulation apparatus T shown in FIG. 1 is not particularly limited as long as it is a conventionally used extruder. For example, a single screw extruder, a twin screw extruder, or a tandem extruder in which multiple extruders are connected together can be used. The chamber 4 housing the cutter 3 may be a conventional one used in the hot cutting method.

[0039] In the manufacturing method of the present invention, the diameter of the die hole is 0.5 mm to 1.7 mm, and preferably 0.5 mm to 1.6 mm. In the production method of the present invention, the temperature of the cooling water is 55°C to 90°C, and preferably 60°C to 90°C. By setting the pore size and water temperature within the above ranges, the pores are less likely to be blocked by the resin, and expanded beads having a particle size of 1.5 mm to 4.5 mm and a surface resin layer thickness of 5 μm to 40 μm can be produced.

[0040] The foaming agent may be one that has been widely used in the past. Examples of the foaming agent include chemical foaming agents such as azodicarbonamide, dinitrosopentamethylenetetramine, hydrazoyldicarbonamide, and sodium bicarbonate; saturated aliphatic hydrocarbon foaming agents such as propane, normal butane, isobutane, normal pentane, isopentane, and hexane; ether foaming agents such as dimethyl ether; fluorocarbon foaming agents such as methyl chloride, 1,1,1,2-tetrafluoroethane, 1,1-difluoroethane, and monochlorodifluoromethane; and inorganic foaming agents such as carbon dioxide and nitrogen. Dimethyl ether, propane, normal butane, isobutane, and carbon dioxide are preferred, propane, normal butane, isobutane, and carbon dioxide are more preferred, and normal butane, isobutane, and carbon dioxide are particularly preferred. The foaming agent may be used alone or in combination of two or more.

[0041] The amount of the foaming agent supplied to the extruder is preferably 0.1 to 5 parts by mass, more preferably 0.2 to 4 parts by mass, and particularly preferably 0.5 to 4 parts by mass, per 100 parts by mass of the aromatic polyester resin, in order to easily set the expansion ratio of the expanded beads in an appropriate range.

[0042] It is preferable that a bubble regulator is supplied to the extruder, and examples of such bubble regulators include polytetrafluoroethylene powder, polytetrafluoroethylene powder modified with an acrylic resin, and talc.

[0043] The amount of the cell control agent supplied to the extruder is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 3 parts by mass, and particularly preferably 0.1 to 2 parts by mass, per 100 parts by mass of the aromatic polyester resin, in order to set the cell diameter of the expanded beads in an appropriate range.

[0044] The expanded aromatic polyester resin beads obtained by the production method of the present invention have a sufficiently small particle diameter, which allows a high filling rate when filling a molding die. In addition, the production method of the present invention allows the resin layer of the expanded beads to have a thickness within a range suitable for expansion, for example, 5 μm to 40 μm, so that the expandability is high. Therefore, the in-mold foamed article obtained from the expanded beads has excellent mechanical properties, such as compressive strength or compressive elastic modulus.

[0045] The bulk density of the aromatic polyester resin expanded particles is 0.05 g / cm from the viewpoint of improving the expansion power and the fusion power of the secondary expanded particles. 3 ~0.7g / cm 3 is preferred, and 0.07 g / cm 3 ~0.6g / cm 3 More preferably, 0.08 g / cm 3 ~0.5g / cm 3 is particularly preferred.

[0046] The bulk density of the expanded aromatic polyester resin particles is measured in accordance with JIS K6911: 1995 "General testing method for thermosetting plastics." In detail, it is determined by the method described in the examples.

[0047] Although the aromatic polyester resin expanded particles have improved heat resistance of the expanded molded article when the crystallinity is high, the fusion strength of the secondary expanded particles is not increased, and as a result, it is difficult to improve the mechanical strength of the expanded molded article. For this reason, the crystallinity (A) at the particle center and the crystallinity (B) at the particle surface are both preferably 10% or less, more preferably 1 to 10%, and particularly preferably 2 to 8%.

[0048] The central portion and the surface portion of the expanded beads are determined as follows. The expanded bead is cut approximately in half at the center using a razor blade, and the portion of the exposed cross section ranging from the center of the particle to 20% of the expanded bead in the radial direction is defined as the central portion, and the portion of the exposed cross section ranging from the surface of the particle to 20% of the expanded bead in the radial direction is defined as the surface portion.

[0049] The crystallinity of the expanded beads is determined by the method described in JIS K7122:1987 and JIS K7122:2012, and more specifically, by the method described in the Examples.

[0050] The ratio (B / A) of the crystallinity (B) in the surface layer to the crystallinity (A) in the center of the expanded aromatic polyester resin particles is preferably 0.90 to 1.5, more preferably 0.95 to 1.4, and particularly preferably 0.95 to 1.3, from the viewpoint of improving the expandability or the fusion strength of the secondary expanded particles.

[0051] From the viewpoint of improving the expansion power or the fusion power of the secondary expanded particles, the thickness of the resin layer on the surface of the expanded aromatic polyester resin particles is preferably 5 μm to 40 μm, more preferably 10 μm to 35 μm. Here, the thickness of the resin layer on the surface of the expanded particles is determined from an image of the surface layer of a cross section of the expanded particle approximately divided into two at the center, taken with a scanning electron microscope at a magnification of 500 times, and in detail is determined by the method described in the Examples.

[0052] It is preferable that the average cell diameter (C) at the particle center of the expanded aromatic polyester resin particles and the average cell diameter (D) at the particle surface layer portion are both 50 μm to 300 μm from the viewpoint of improving the expandability or the fusion strength of the secondary expanded particles.

[0053] It is preferable that the bubble diameter of the surface layer of the expanded aromatic polyester resin particles is slightly smaller than that of the center, because the expansion is good and the fusion strength of the secondary expanded particles is high. Therefore, the ratio (D / C) of the average bubble diameter (D) of the surface layer to the average bubble diameter (C) of the center of the expanded beads is preferably 0.75 to 0.98, more preferably 0.77 to 0.96, and particularly preferably 0.79 to 0.95.

[0054] The aromatic polyester resin foamed particles of the present invention are filled into the cavity of a mold, heated, and expanded, and the secondary expanded particles obtained by expanding the aromatic polyester resin foamed particles are heat-fused together by their expansion pressure, thereby obtaining an in-mold foamed article having a desired shape and excellent mechanical properties. The heating medium for the aromatic polyester resin foamed particles filled in the mold is not particularly limited, and examples thereof include hot air, hot water, and the like in addition to steam.

[0055] The present invention also includes an expansion molded article of the expanded aromatic polyester resin beads of the present invention. This expansion molded article is obtained by in-mold expansion molding of the expanded aromatic polyester resin beads of the present invention.

[0056] The density of the aromatic polyester resin foam molded body is set to 0.05 g / cm3 from the viewpoints of light weight and mechanical strength. 3 ~0.7g / cm 3 is preferred, and 0.07 g / cm 3 ~0.6g / cm 3 More preferably, 0.08 g / cm 3 ~0.5g / cm 3 is particularly preferred.

[0057] Furthermore, the aromatic polyester resin foam particles may be impregnated with an inert gas immediately before the in-mold foaming to improve the foaming power of the aromatic polyester resin foam particles. By improving the foaming power of the aromatic polyester resin foam particles in this way, the thermal fusion between the aromatic polyester resin foam particles during the in-mold foaming is improved, and the obtained in-mold foamed article has even better mechanical strength. Examples of the inert gas include carbon dioxide, nitrogen, helium, and argon, and carbon dioxide is preferred.

[0058] As a method for impregnating the expanded aromatic polyester resin particles with an inert gas, for example, a method for impregnating the expanded aromatic polyester resin particles with an inert gas by placing the expanded aromatic polyester resin particles in an inert gas atmosphere having a pressure equal to or higher than normal pressure can be mentioned. In such a case, the expanded aromatic polyester resin particles may be impregnated with an inert gas before being filled into a mold, or the expanded aromatic polyester resin particles may be impregnated with an inert gas by placing the expanded aromatic polyester resin particles together with the mold in an inert gas atmosphere after being filled into the mold.

[0059] The temperature when the expanded aromatic polyester resin particles are impregnated with an inert gas is preferably from 5°C to 40°C, and more preferably from 10°C to 30°C.

[0060] The pressure when the expanded aromatic polyester resin particles are impregnated with an inert gas is preferably 0.2 to 2.0 MPa, more preferably 0.25 to 1.5 MPa. When the inert gas is carbon dioxide, the pressure is preferably 0.2 to 1.5 MPa, more preferably 0.25 to 1.2 MPa.

[0061] The time for impregnating the expanded aromatic polyester resin particles with the inert gas is preferably from 10 minutes to 72 hours, more preferably from 15 minutes to 64 hours, and particularly preferably from 20 minutes to 48 hours.

[0062] The expanded aromatic polyester resin particles impregnated with the inert gas are expanded (pre-expanded) by heating to, for example, 55° C. to 90° C. to produce pre-expanded particles.

[0063] A composite structural member can be produced by using a foamed molded body as a core material and laminating and integrating a skin material onto the surface of the foamed molded body. A composite structural member including a foamed molded body and a skin material laminated and integrated onto the surface of the foamed molded body can also be one aspect of the present invention. The thickness of the foamed molded body used as the core material of the composite structural member is preferably 1 mm to 40 mm in terms of strength, weight, and impact resistance.

[0064] The skin material is not particularly limited, and examples thereof include a fiber-reinforced synthetic resin sheet, a metal sheet, a synthetic resin sheet, etc. The skin material is preferably a fiber-reinforced synthetic resin because of its excellent mechanical strength and light weight.

[0065] The fiber-reinforced synthetic resin sheet is a sheet formed by bonding fibers together with a matrix resin. The fibers constituting the fiber-reinforced synthetic resin sheet are not particularly limited, and examples thereof include carbon fibers, glass fibers, aramid fibers, boron fibers, and metal fibers. As the fibers, carbon fibers, glass fibers, and aramid fibers are preferred, and carbon fibers are more preferred, because they have excellent mechanical strength and heat resistance.

[0066] The matrix resin constituting the fiber-reinforced synthetic resin includes thermosetting resin and thermoplastic resin. Examples of the thermosetting resin include epoxy resin, unsaturated polyester resin, and phenol resin. The thermosetting resin may be used alone or in combination of two or more. Examples of the thermoplastic resin include polyamide (nylon 6, nylon 66, etc.), polyolefin (polyethylene, polypropylene, etc.), polyphenylene sulfide, polyethylene terephthalate, polybutylene terephthalate, polycarbonate, polystyrene, ABS, and copolymers of acrylonitrile and styrene. The thermoplastic resin may be used alone or in combination of two or more.

[0067] The thickness of the fiber-reinforced synthetic resin sheet is preferably 0.2 mm to 2.0 mm in terms of strength, weight, and impact resistance.

[0068] The method for producing the composite structural member is not particularly limited. For example, the method may be a method in which a skin material is laminated onto the surface of a foamed molded body that serves as a core material using an adhesive, or a method generally used for molding a fiber-reinforced synthetic resin sheet. Examples of methods used in molding fiber-reinforced synthetic resin sheets include the autoclave method, the hand lay-up method, the spray-up method, the PCM (Prepreg Compression Molding) method, the RTM (Resin Transfer Molding) method, and the VaRTM (Vacuum assisted Resin Transfer Molding) method.

[0069] Such composite structural members are useful for applications such as automobile members, aircraft members, railroad vehicle members, building materials, etc. Examples of automobile members include door panels, door inners, bumpers, fenders, fender supports, engine covers, roof panels, trunk lids, floor panels, center tunnels, crash boxes, etc. For example, when a composite structural member is used for a door panel that has conventionally been made of steel plate, the door panel has substantially the same rigidity as a steel plate door panel, but the weight can be significantly reduced, resulting in a significant effect in reducing the weight of the automobile. EXAMPLES

[0070] Hereinafter, one embodiment of the present invention will be described in more detail with reference to examples, but the present invention is not limited to these. The methods for determining various physical properties in the examples are described below.

[0071] (Bulk density) The bulk density was measured in accordance with JIS K6911:1995 "General testing method for thermosetting plastics" using an apparent density measuring device in accordance with JIS K6911. Bulk density of foam particles (g / cm 3) = [mass of the measuring cylinder containing the sample (g) - mass of the measuring cylinder (g)] / [capacity of the measuring cylinder (cm 3 )〕

[0072] (Particle size) The average particle size of the resin particles was measured by the following method. First, several types of sieves having different mesh sizes as specified by JIS (mesh size 6.70 mm, 5.60 mm, 4.75 mm, 4.00 mm, 3.35 mm, 2.80 mm, 2.36 mm, 2.00 mm, 1.70 mm, 1.40 mm, 1.18 mm, 1.00 mm, 0.850 mm, 0.710 mm, 0.600 mm, 0.500 mm) were prepared, and 50 g of expanded particles were sieved through the sieves from the larger mesh size to the smaller mesh size. Then, the expanded particles were unable to pass through the sieve with the predetermined mesh size according to the particle size of each particle, and remained on each sieve. The average particle size of the expanded particles remaining on each sieve is determined based on the size of the mesh size of the sieve, as shown in the following table. For example, the particle size of the expanded particles remaining on a sieve with a mesh size of 1.70 mm is set to 1.85 mm. [Table 1]

[0073] The average particle size of the expanded beads remaining on each sieve was determined as the arithmetic mean value of the mesh size of the sieve and the mesh size of the sieve with the next largest mesh size. In the case of a sieve with a mesh size of 1.70 mm, the arithmetic mean value of the mesh size of the sieve with the next largest mesh size specified by JIS, 2.00 mm, was used. Next, the weight W of the expanded particles remaining on the sieve was measured for each sieve, and the weight ratio R (weight %) of the expanded particles remaining on the sieve to the total expanded particles was calculated for each sieve. The particle diameter D of the expanded particles for each sieve was multiplied by the weight ratio R of the expanded particles to calculate the average particle diameter (mm) of the expanded particles. Average particle size = Σ (particle size D of expanded particles on each sieve × weight ratio R of expanded particles / 100)

[0074] (Crystallization degree) The crystallinity was measured according to the methods described in JIS K7122:1987 and JIS K7122:2012. However, the sampling method and temperature conditions were as follows. Samples were taken from the surface and center of the expanded beads. The surface samples were taken from a portion that was approximately bisected at the center of the expanded beads using a razor blade, and was located within 20% of the area in the radial direction of the expanded beads from the surface of the expanded beads. Similarly, the center samples were taken from a portion that was approximately 20% of the area in the radial direction of the expanded beads from the center of the bisected expanded beads. 5.5±0.5mg of sample was packed into an aluminum measuring container so that there were no gaps at the bottom, and then an aluminum lid was placed on it. Differential scanning calorimetry was then performed using a Hitachi High-Tech Science DSC7000X, AS-3 differential scanning calorimeter. The sample was heated in the following steps under a nitrogen gas flow rate of 20mL / min to obtain a DSC curve. (Step 1) Hold at 30°C for 2 minutes. (Step 2) The temperature was raised from 30°C to 290°C at a rate of 10°C / min. Alumina was used as the reference material. The difference between the heat of fusion (J / g) calculated from the area of ​​the melting peak and the heat of crystallization (J / g) calculated from the area of ​​the crystallization peak was calculated. The ratio obtained by dividing this difference by the theoretical heat of fusion of 140.1 J / g for polyethylene terephthalate perfect crystal was taken as the degree of crystallization. The heat of fusion and the heat of crystallization were calculated using the analysis software attached to the device. Specifically, the heat of fusion was calculated from the straight line connecting the point where the DSC curve leaves the low-temperature baseline and the point where the DSC curve returns to the high-temperature baseline, and the part enclosed by the DSC curve. The heat of crystallization was calculated from the straight line connecting the point where the DSC curve leaves the low-temperature baseline and the point where the DSC curve returns to the high-temperature baseline, and the area enclosed by the DSC curve. In other words, the degree of crystallization was calculated from the following formula. Crystallinity (%) = (heat of fusion (J / g) - heat of crystallization (J / g)) / 140.1 (J / g) x 100

[0075] (crystallinity ratio) The crystallinity ratio was calculated by the following formula. Crystallinity ratio = Crystallinity of the surface layer of the expanded bead (%) / Crystallinity of the center of the expanded bead (%)

[0076] (average bubble diameter) The surface layer and the center of a cross section of an expanded bead roughly divided in two at the center were photographed at 100x magnification using a scanning electron microscope "SU1510" manufactured by Hitachi High-Technologies Corp. The surface layer was taken as the area within 20% of the expanded bead surface in the radial direction, and the center was taken as the area within 20% of the expanded bead surface in the radial direction. The captured microscopic images were arranged side by side on one A4 sheet of paper in landscape orientation and printed on A4 paper. For each image of the cross section of the printed foamed beads, three arbitrary straight lines (60 mm long) parallel to the vertical and horizontal directions were drawn. That is, for each of two microscopic images, six arbitrary straight lines were drawn in the vertical direction and six in the horizontal direction. The lines were drawn so that they would not come into contact with the bubbles only at their contact points as much as possible. The number of bubbles that the straight lines passed through was then counted. If a bubble came into contact with the line only at its contact point, this bubble was also included in the count. The number of bubbles counted for the six arbitrary straight lines in each of the vertical and horizontal directions was calculated as the number of bubbles in each direction. The average chord length t of the bubbles was calculated from the magnification of the image where the number of bubbles was counted and the number of bubbles using the following formula. Average chord length t(mm)=60 / (number of bubbles x image magnification) The image magnification was calculated by measuring the scale bar on the image to the nearest 1 / 100 mm using a Mitutoyo Digimatic Caliper and using the following formula: Image magnification = Scale bar actual value (mm) / Scale bar display value (mm) The bubble diameters in the vertical and horizontal directions were calculated using the following formula. Vertical or horizontal bubble diameter D(mm)=t / 0.616 Furthermore, the square root of the product of the air bubble diameter D in the vertical direction and the air bubble diameter D in the horizontal direction was defined as the air bubble diameter. Bubble diameter (μm) = 1000 x (D length x D width) 1 / 2 The above procedure was carried out on the surface and center with an N number of 10, and the average value was taken as the average bubble diameter.

[0077] (Average bubble diameter ratio) The average cell diameter ratio was calculated by the following formula. Average bubble diameter ratio = Average bubble diameter at the surface of the expanded particle (μm) / Average bubble diameter at the center of the expanded particle (μm)

[0078] (Thickness of surface resin) The surface layer of a cross section roughly divided in two at the center of an expanded bead was photographed at 500x magnification using a Hitachi High-Technologies Corporation "SU1510" scanning electron microscope. At any position on the surface of the expanded bead in the microscope image, five straight lines perpendicular to the tangent were drawn in the radial direction of the expanded bead, and the distance from the surface to the first air bubble that came into contact with each straight line was measured. In other words, five such distances were measured for one cross-sectional image. The above procedure was carried out with an N number of 10, and the average value was taken as the thickness (μm) of the surface resin.

[0079] (Moldability evaluation) The moldability was evaluated according to the following criteria. ○: The foam particles were thermally fused together, firmly bonded, and integrated. ×: The expanded particles were not bonded to each other and easily fell off.

[0080] (Density of foamed molded body) The mass (a) and volume (b) of a rectangular parallelepiped test piece (e.g., 75 mm x 300 mm x 30 mm) cut out from a foamed molded product (dried at 55°C for 20 hours or more after molding) are measured to have three or more significant figures, and the density of the foamed molded product (g / cm3) is calculated using the formula (a) / (b). 3 ) was sought.

[0081] (Compression test: 5% compressive strength and compressive modulus) The 5% compression strength and compression modulus were measured in accordance with JIS K6767:1999. That is, the 5% compression strength was measured using a Shimadzu Corporation "Autograph AG-X plus 100kN" universal testing machine and Shimadzu Corporation "TRAPEZIUM X" universal testing machine data processing software. The test piece size was 50mm x 50mm x thickness 25mm, and the number of test pieces was 3. The test pieces were conditioned for 16 hours under the standard atmosphere of JIS K 7100:1999 symbol "23 / 50" (temperature 23°C, relative humidity 50%), class 2, and then used for measurement under the same standard atmosphere. The compression speed was 2.5mm / min. From the obtained graph, the load region with the maximum slope was set, and the compression modulus was calculated using the universal testing machine data processing software. The intersection point of the straight line of this elastic modulus and the stroke was set as the origin of elongation, and the compression strength at 5% compression was automatically calculated.

[0082] (Evaluation of mechanical properties of molded products) The mechanical properties of the molded product were evaluated according to the following criteria. ○: 5% compressive strength is 0.80 MPa or more and compressive modulus is 30 MPa or more. ×: 5% compressive strength is less than 0.80 MPa or compressive modulus is less than 30 MPa.

[0083] Example 1 (Expanded particle manufacturing process) An underwater cutting type granulator was used, which has a diverter valve as shown in Figure 2, a die with 38 die holes (diameter 0.6 mm, land length 2.0 mm), and a diverter valve set so that the molten resin supplied from the extruder to the die through the resin flow path on the outside discharge side of the diverter valve is discharged outside the machine. In addition, a single-screw extruder with a hole diameter of 65 mm and an L / D ratio of 34 was used as the extruder that supplies the molten resin to this granulator.

[0084] First, the temperature was adjusted by a heater so that the temperature of the die hole of the die was 300° C., and the temperature of the extruder was also adjusted. Specifically, the upstream extruder was set at a higher temperature than the downstream extruder to increase the solubility of the foaming agent, and the extruder temperature was set so that the molten resin was finally supplied to the die at a resin temperature of 290° C. This extruder was charged with plant-derived polyethylene terephthalate (intrinsic viscosity: 0.80, density: 1400 kg / m 3 A polyethylene terephthalate composition containing 100 parts by weight of a polyethylene terephthalate copolymer having a melting point of 247.2°C, a glass transition temperature of 78.7°C, a mass average molecular weight of 74,000, and a plant content of 30%), 1.8 parts by weight of a master batch obtained by incorporating talc into polyethylene terephthalate (polyethylene terephthalate content: 60% by weight, talc content: 40% by weight, intrinsic viscosity of polyethylene terephthalate: 0.82), and 0.22 parts by weight of pyromellitic anhydride was supplied at a rate of 30 kg / h and melt-kneaded.

[0085] Next, butane consisting of 35% by weight of isobutane and 65% by weight of normal butane was pressurized into the molten polyethylene terephthalate composition midway through the extruder in an amount of 3.0 parts by weight per 100 parts by weight of polyethylene terephthalate to uniformly disperse it in the polyethylene terephthalate. Then, a molten polyethylene terephthalate composition was supplied to the die and discharged to the outside of the machine through the resin flow path of the diverter valve. When the temperature of the extruder, the pressure of the foaming agent, etc. became stable, a cutter was operated in the chamber attached in front of the die, the flow path of the molten polyethylene terephthalate composition was switched by the diverter valve, and 12 m of cooling water at 90°C and a water pressure of 0.3 MPa was poured into the chamber. 3 / h and granulation was started.

[0086] The molten polyethylene terephthalate extrudate extruded while foaming in the cooling water was cut with a rotary blade to produce foamed particles. The cut particles were foamed in the cooling water to produce polyethylene terephthalate foamed particles. The cooling water containing the foamed particles was transported from the chamber to a dehydration treatment section, where the cooling water was removed from the foamed particles.

[0087] (molding process) The obtained foamed beads were left at 23° C. under atmospheric pressure for 30 days, then filled into a 30 mm×300 mm×400 mm molding die, heated with 0.05 MPa water vapor for 180 seconds and with 0.10 MPa water vapor for 30 seconds, and then cooled until the maximum surface pressure of the foamed molded product decreased to 0.01 MPa, thereby obtaining a foamed molded product.

[0088] Example 2 Polyethylene terephthalate expanded beads and expanded molded products were obtained in the same manner as in Example 1, except that a die having 22 die holes with a diameter of 0.8 mm and a land length of 2.0 mm was used and the cooling water temperature was set to 80°C.

[0089] Example 3 Polyethylene terephthalate expanded beads and expanded molded products were obtained in the same manner as in Example 1, except that a die having 10 die holes with a diameter of 1.2 mm and a land length of 2.0 mm was used and the cooling water temperature was set to 70°C.

[0090] Example 4 Polyethylene terephthalate expanded beads and expanded molded products were obtained in the same manner as in Example 1, except that a die having seven die holes with a diameter of 1.5 mm and a land length of 2.0 mm was used and the cooling water temperature was set to 70°C.

[0091] Comparative Example 1 Polyethylene terephthalate expanded beads were obtained in the same manner as in Example 1, except that a die having five die holes with a diameter of 2.0 mm and a land length of 2.0 mm was used and the cooling water temperature was set to 80° C. The obtained expanded beads were molded in the same manner as in Example 1, but the expanded beads were not bonded to each other and easily fell off, and no expanded molded product was obtained.

[0092] Comparative Example 2 Polyethylene terephthalate expanded beads and expanded molded products were obtained in the same manner as in Example 1, except that a die having seven die holes with a diameter of 1.5 mm and a land length of 2.0 mm was used and the cooling water temperature was set to 50°C.

[0093] Comparative Example 3 Polyethylene terephthalate expanded beads and expanded molded products were obtained in the same manner as in Example 1, except that a die having seven die holes with a diameter of 1.5 mm and a land length of 2.0 mm was used and the cooling water temperature was set to 95°C.

[0094] Comparative Example 4 Polyethylene terephthalate expanded beads were produced in the same manner as in Example 1, except that a die having seven die holes with a diameter of 1.5 mm and a land length of 2.0 mm was used and the cooling water temperature was set to 25°C. However, blockage of the die holes occurred and expanded beads could not be obtained.

[0095] Table 2 shows the physical properties measured for the expanded beads and expanded molded articles obtained in the above Examples and Comparative Examples.

[0096] [Table 2]

[0097] By setting the pore size to about 0.5 mm to 1.7 mm and the cooling water temperature to about 55° C. to 90° C., expanded beads with a particle size of about 1.5 mm to 4.5 mm and a resin layer thickness on the particle surface of about 5 μm to 40 μm were obtained. The expanded molded article obtained by in-mold expansion molding of these expanded beads had excellent compressive strength and compressive elastic modulus.

Claims

1. The expanded aromatic polyester resin particles have a particle diameter of 1.5 mm to 4.5 mm and a surface resin layer thickness of 5 μm to 40 μm.

2. 2. The expanded aromatic polyester resin particle according to claim 1, wherein the average cell diameter (C) in the center of the particle and the average cell diameter (D) in the surface layer portion are both 50 μm to 300 μm, and the ratio (D / C) of the average cell diameter in the surface layer portion to the average cell diameter in the center portion is 0.75 to 0.

98.

3. 3. The expanded aromatic polyester resin particle according to claim 1, wherein the crystallinity (A) in the center portion of the particle and the crystallinity (B) in the surface portion of the particle are both 10% or less, and the ratio (B / A) of the crystallinity in the surface portion to the crystallinity in the center portion is 0.90 to 1.

5.

4. 4. The expanded aromatic polyester resin particle according to claim 1, wherein the degree of crystallinity (A) in the central portion of the particle and the degree of crystallinity (B) in the surface portion of the particle are both 1 to 10%.

5. 5. An expansion molded product of the expanded aromatic polyester resin particles according to claim 1.

6. Density is 0.05 g / cm 3 ~0.7g / cm 3 The foamed molded article according to claim 5,

7. An automobile component comprising the foamed molded article according to claim 5 or 6.

8. 5. The method for producing expanded aromatic polyester resin particles according to claim 1, comprising the steps of: supplying an aromatic polyester resin to an extruder and melt-kneading the resin in the presence of a foaming agent; cutting the melt-kneaded aromatic polyester resin extrudate from a die attached to the front end of the extruder while extruding and foaming the extrudate in cooling water to produce particulate cut pieces; and cooling the particulate cut pieces with cooling water, wherein the die has a hole diameter of 0.5 mm to 1.7 mm and the cooling water has a temperature of 55° C. to 90° C.

Citation Information

Patent Citations

  • Surgical metatarsal compression nail

    EP2564799A1

  • Method for producing aromatic polyester-based resin pre-expanded bead

    JP2001329101A

  • Wax-containing foamed particles, foamed molding, and method for producing them

    JP2019065272A

  • Expandable pelletized materials based on polyester

    US20120041086A1

  • Foam particles, methods of making and using the same

    US20160325472A1