Transparent polyimide film and method for producing same
By blending phosphoric acid esters with polyimide films, the issue of high birefringence is addressed, resulting in transparent films with improved mechanical strength and reduced color shifts, suitable for display applications.
Patent Information
- Application Number
- JP2021526970
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-06-24
- Filing Date
- 2020-06-22
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-06-22
AI Technical Summary
Existing polyimide films exhibit high birefringence, leading to iridescent unevenness and color shifts when viewed from oblique directions, compromising visibility, while reducing birefringence through additives like plasticizers compromises mechanical strength.
Incorporating a phosphoric acid ester into the polyimide film composition to reduce birefringence without significantly decreasing mechanical strength, achieved by blending specific amounts of phosphate esters with polyimide resins.
The resulting polyimide film maintains high mechanical strength while significantly reducing birefringence, enhancing transparency and visibility by minimizing color shifts and iridescent effects.
Smart Images

Figure 0007575379000001 
Figure 0007575379000002 
Figure 0007575379000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a transparent polyimide film and a method for producing the same. [Background technology]
[0002] In recent years, with the rapid progress of electronic devices, there is a demand for devices to be thinner, lighter, and more flexible. In particular, in applications that require high heat resistance, dimensional stability at high temperatures, and high mechanical strength, the use of polyimide films as an alternative material to glass used in substrates, cover windows, etc. has been considered.
[0003] A typical polyimide is colored yellow or brown and does not dissolve in an organic solvent. To produce a film from a polyimide that is insoluble in an organic solvent, a method (thermal imidization) is adopted in which a polyamic acid solution, which is a polyimide precursor, is applied to a substrate, the solvent is removed by heating, and the polyamic acid is dehydrated and cyclized to form an imid (thermal imidization). On the other hand, Patent Documents 1 to 3 describe that the introduction of an alicyclic structure, a bent structure, a fluorine substituent, or the like can impart visible light transparency and solubility to polyimide. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2012-144603 A [Patent Document 2] JP 2016-132686 A [Patent Document 3] WO2017 / 175869 International Publication Pamphlet Summary of the Invention [Problem to be solved by the invention]
[0005] The polyimide resins described in Patent Documents 1 to 3 are also soluble in organic solvents, so that a transparent polyimide film can be prepared from a polyimide solution in which the polyimide resin is dissolved in an organic solvent. Films prepared by solution film formation generally have low birefringence, but polyimide molecules tend to be oriented in the film plane, so the retardation Rth in the thickness direction tends to be large. Films with high Rth tend to show rainbow unevenness and color shifts when viewed from an oblique direction due to the influence of birefringence, and when used as a display material such as a cover film, this can cause a decrease in visibility.
[0006] As a method for reducing the birefringence of a resin film, a method of adding a retardation regulator is known. Retardation regulators generally act as plasticizers, and have the effect of reducing birefringence by relaxing the orientation of molecules. When a retardation regulator that acts as a plasticizer is used, the birefringence of the film is reduced, and at the same time, the mechanical strength tends to decrease.
[0007] Since a member arranged on the outermost surface of a display, such as a cover film, is required to have low birefringence and mechanical strength, if the birefringence is reduced by an additive that acts like a plasticizer, the mechanical strength tends to be insufficient even if the optical problems are solved. In other words, there is generally a trade-off between low birefringence and high mechanical strength. In view of these, the present invention aims to provide a transparent polyimide film having low birefringence and sufficient mechanical strength. [Means for solving the problem]
[0008] As a result of investigations, the present inventors have found that by blending a phosphoric ester, it is possible to reduce birefringence while suppressing a decrease in the tensile modulus of a polyimide film, and have arrived at the present invention.
[0009] One embodiment of the present invention is a transparent polyimide film containing polyimide and a phosphate ester. The polyimide film can be obtained, for example, by dissolving a solvent-soluble polyimide resin and a phosphate ester in an organic solvent that is soluble in the polyimide resin to prepare a polyimide solution, applying the polyimide solution to a substrate, and removing the organic solvent.
[0010] Polyimides are polymers containing repeating units of the general formula (1).
[0011] [ka]
[0012] In the general formula (1), X is any tetravalent organic group and is an acid dianhydride residue. Y is any divalent organic group and is a diamine residue. The organic group X preferably contains a fluoroalkyl group, an ether bond, a thioether bond, an ester bond, a sulfone group, an alicyclic structure, or a straight-chain aliphatic group having two or more carbon atoms. The organic group Y preferably contains a fluoroalkyl group, a sulfone group, a fluorene structure, or an alicyclic structure.
[0013] The content of the phosphate in the polyimide film is 3 parts by mass or more, preferably 5 to 100 parts by mass, and more preferably 15 to 100 parts by mass, based on 100 parts by mass of polyimide.
[0014] Examples of the phosphate ester include an orthophosphate ester represented by the general formula (2) and a condensed phosphate ester represented by the general formula (3).
[0015] [ka]
[0016] R in general formula (2) 1 ~R 3 and R in general formula (3) 4 and R 5R is each independently an optional substituent. 1 ~R 5 Specific examples of R include an aryl group which may have a substituent, an aliphatic group having 1 to 20 carbon atoms which may have a branch, and a poly(oxyalkylene)alkyl group. 1 ~R 5 is preferably an aryl group which may have a substituent.
[0017] In the general formula (3), n is an integer of 1 or more, and Z is a divalent organic group containing at least one aromatic ring. Examples of the divalent organic group Z include the following Z-1 to Z-6.
[0018] [ka]
[0019] R 7 ~R 16 are each independently a hydrogen atom or an optionally branched chain alkyl group having 1 to 6 carbon atoms, and two or more substituents may be bonded to one benzene ring.
[0020] Specific examples of orthophosphate esters include triphenyl phosphate, tricresyl phosphate, cresyl diphenyl phosphate, etc. Specific examples of condensed phosphate esters include resorcinol bisdiphenyl phosphate, bisphenol A bisdiphenyl phosphate, resorcinol bis(di-2,6-xylenyl phosphate), etc.
[0021] The ratio E / E' of the tensile modulus E of the polyimide film containing a phosphate ester to the tensile modulus E' of the film of polyimide alone not containing a phosphate ester is preferably 0.80 or more, more preferably 0.90 or more. The ratio Δn / Δn' of the thickness direction birefringence Δn of the polyimide film containing a phosphate ester to the thickness direction birefringence Δn' of the film of polyimide alone not containing a phosphate ester is preferably less than 0.90, more preferably less than 0.80. The thickness direction birefringence Δn of the polyimide film is preferably 0.050 or less. Effect of the Invention
[0022] According to the present invention, it is possible to provide a transparent polyimide film having reduced birefringence without reducing the mechanical strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] One embodiment of the present invention is a transparent polyimide film that includes a polyimide and a phosphate ester.
[0024] [Polyimide] Polyimide has a repeating unit represented by the following general formula (1).
[0025] [ka]
[0026] Polyimides are generally obtained by cyclizing and dehydrating a polyamic acid obtained by reacting a tetracarboxylic dianhydride (hereinafter sometimes simply referred to as an "acid dianhydride") represented by the following formula (A) with a diamine represented by the following formula (B). That is, polyimides have a structure derived from an acid dianhydride and a structure derived from a diamine.
[0027] [ka]
[0028] In the general formula (1), X is a residue of a tetracarboxylic dianhydride. The residue of a tetracarboxylic dianhydride is a portion other than the two acid anhydride groups (-CO-O-CO-) in the compound of the general formula (A) (tetracarboxylic dianhydride), and is a tetravalent organic group. In the tetracarboxylic dianhydride, two of the four carbonyl groups bonded to X form pairs to form a five-membered ring together with X and an oxygen atom. In the general formula (1), Y is a residue of a diamine. The residue of a diamine is a portion other than the two amino groups (-NH2) in the compound of the general formula (B), and is a divalent organic group.
[0029] (acid dianhydride) Examples of acid dianhydrides that can be used as raw materials for transparent polyimides include ethylene tetracarboxylic dianhydride, butane tetracarboxylic dianhydride, 1,2,3,4-cyclobutane tetracarboxylic dianhydride, 1,2,3,4-cyclopentane tetracarboxylic dianhydride, 1,2,4,5-cyclohexane tetracarboxylic dianhydride, 1,1'-bicyclohexane 3,3',4,4'-tetracarboxylic acid-3,4,3',4'-dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 2,2',3,3'-benzophenone tetracarboxylic dianhydride, 2, 2',3,3'-Biphenyltetracarboxylic dianhydride, pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, 2,2-bis(2,3-dicarboxyphenyl)propane dianhydride, bis(3,4-dicarboxyphenyl)ether dianhydride, bis(3,4-dicarboxyphenyl)sulfone dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, bis(2,3-dicarboxyphenyl)methane dianhydride, bis(3,4-dicarboxy 2,2-bis(3,4-dicarboxyphenyl)-1,1,1,3,3,3-hexafluoropropane dianhydride, 2,2-bis(2,3-dicarboxyphenyl)-1,1,1,3,3,3-hexafluoropropane dianhydride, 2,2-bis{4-[4-(1,2-dicarboxy)phenoxy]phenyl}-1,1,1,3,3,3-hexafluoropropane dianhydride, 1,3-bis[(3,4-dicarboxy)benzoyl]benzene dianhydride, 1,4-bis[(3,4-dicarboxy)benzoyl]benzene dianhydride, 2, 2-Bis{4-[4-(1,2-dicarboxy)phenoxy]phenyl}propane dianhydride, 2,2-bis{4-[3-(1,2-dicarboxy)phenoxy]phenyl}propane dianhydride, bis{4-[4-(1,2-dicarboxy)phenoxy]phenyl}ketone dianhydride, bis{4-[3-(1,2-dicarboxy)phenoxy]phenyl}ketone dianhydride, 4,4'-bis[4-(1,2-dicarboxy)phenoxy]biphenyl dianhydride, 4,4'-bis[3-(1,2-dicarboxy)phenoxy]biphenyl dianhydride, bis{4-[4-(1,2-dicarboxy)phenoxy]phenyl}ketone dianhydride, bis{4-[3-(1,2-dicarboxy)phenoxy]phenyl}ketone dianhydride, bis{4-[4-(1,2-dicarboxy)phenoxy]phenyl}sulfone dianhydride, bis{4-[3-(1,2-dicarboxy)phenoxy]phenyl}sulfone dianhydride, bis{4-[4-(1,2-dicarboxy)phenoxy]phenyl}sulfide dianhydride, bis{4-[3-(1,2-dicarboxy)phenoxy]phenyl}sulfide dianhydride, 2,2-bis{4-[3-(1,2-dicarboxy)phenoxy]phenyl}-1,1,1,3,3,3-propane dianhydride, 2,3,6,7-naphthalene Examples of suitable dianhydrides include 1,4,5,8-naphthalenetetracarboxylic dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 1,2,3,4-benzenetetracarboxylic dianhydride, 3,4,9,10-perylenetetracarboxylic dianhydride, 2,3,6,7-anthracenetetracarboxylic dianhydride, 1,2,7,8-phenanthrenetetracarboxylic dianhydride, bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-carboxylic acid) 1,4-phenylene, and bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-carboxylic acid) 2,2',3,3',5,5'-hexamethylbiphenyl-4,4'-diyl.
[0030] The acid dianhydride used as a raw material for transparent polyimide preferably contains, as the residue X, any one of a fluoroalkyl group, an ether bond, a thioether bond, an ester bond, a sulfone group, an alicyclic structure, and a straight-chain aliphatic group having two or more carbon atoms. As the fluoroalkyl group, a perfluoroalkyl group is preferable, and among these, a trifluoromethyl group is preferable.
[0031] In particular, from the viewpoint of reducing the birefringence of the polyimide film, preferred are acid dianhydrides in which X is any one of the following X-1 to 4, or any one of the following X-7 to 13. From the viewpoint of increasing the solubility of the polyimide resin in an organic solvent and increasing the elastic modulus of the polyimide film, preferred are acid dianhydrides in which X is the following X-5 (bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-carboxylic acid)2,2',3,3',5,5'-hexamethylbiphenyl-4,4'-diyl) or acid dianhydrides in which X is the following X-6 (bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-carboxylic acid)1,4-phenylene).
[0032] [ka]
[0033] [ka]
[0034] [ka]
[0035] As a raw material for polyimide, multiple types of acid dianhydrides may be used in combination. That is, polyimide may contain multiple types of acid dianhydride residues X. For example, by using an acid dianhydride in which X is any of the above X-1 to 4 in combination with an acid dianhydride in which X is the above X-5 or X-6 in combination, a polyimide resin has excellent solubility in organic solvents, and a polyimide film with high elastic modulus and low birefringence can be obtained. An acid dianhydride other than the above may be used in combination within a range that does not impair solubility in organic solvents or transparency.
[0036] (Diamine) Examples of diamines that can be used as raw materials for transparent polyimides include 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl sulfide, 3,4'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, and bis[4-(4-aminophenoxy)phenyl]sulfone. sulfone, 4,4'-bis[4-(4-amino-α,α-dimethylbenzyl)phenoxy]diphenyl sulfone, 4,4'-bis[4-(4-aminophenoxy)phenoxy]diphenyl sulfone, 3,3'-diaminobenzophenone, 4,4'-diaminobenzophenone, 3,4'-diaminobenzophenone, 3,3'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 2,2-di(3-aminophenyl)propane, 2,2-di(4-aminophenyl)propane, 2-(3-aminophenyl)- 2-(4-aminophenyl)propane, 1,4-diamino-2-fluorobenzene, 1,4-diamino-2,3-difluorobenzene, 1,4-diamino-2,5-difluorobenzene, 1,4-diamino-2,6-difluorobenzene, 1,4-diamino-2,3,5-trifluorobenzene, 1,4-diamino-2,3,5,6-tetrafluorobenzene, 1,4-diamino-2-(trifluoromethyl)benzene, 1,4-diamino-2,3-bis(trifluoromethyl)benzene, 1,4-diamino-2,5-bis(trifluoromethyl)benzene , 1,4-diamino-2,6-bis(trifluoromethyl)benzene, 1,4-diamino-2,3,5-tris(trifluoromethyl)benzene, 1,4-diamino-2,3,5,6-tetrakis(trifluoromethyl)benzene, 2-fluorobenzidine, 3-fluorobenzidine, 2,3-difluorobenzidine, 2,5-difluorobenzidine, 2,6-difluorobenzidine, 2,3,5-trifluorobenzidine, 2,3,6-trifluorobenzidine, 2,3,5,6-tetrafluorobenzidine, 2,2'-difluorobenzidine, 3,3'-Difluorobenzidine, 2,3'-Difluorobenzidine, 2,2',3-Trifluorobenzidine, 2,3,3'-Trifluorobenzidine, 2,2',5-Trifluorobenzidine, 2,2',6-Trifluorobenzidine, 2,3',5-Trifluorobenzidine, 2,3',6-Trifluorobenzidine, 2,2',3,3'-Tetrafluorobenzidine, 2,2',5,5'-Tetrafluorobenzidine, 2,2',6,6'-Tetrafluorobenzidine, 2,2',3,3',6,6'-Hexafluorobenzidine , 2,2',3,3',5,5',6,6'-octafluorobenzidine, 2-(trifluoromethyl)benzidine, 3-(trifluoromethyl)benzidine, 2,3-bis(trifluoromethyl)benzidine, 2,5-bis(trifluoromethyl)benzidine, 2,6-bis(trifluoromethyl)benzidine, 2,3,5-tris(trifluoromethyl)benzidine, 2,3,6-tris(trifluoromethyl)benzidine, 2,3,5,6-tetrakis(trifluoromethyl)benzidine, 2,2'-bis(trifluoro methyl)benzidine, 3,3'-bis(trifluoromethyl)benzidine, 2,3'-bis(trifluoromethyl)benzidine, 2,2',3-bis(trifluoromethyl)benzidine, 2,3,3'-tris(trifluoromethyl)benzidine, 2,2',5-tris(trifluoromethyl)benzidine, 2,2',6-tris(trifluoromethyl)benzidine, 2,3',5-tris(trifluoromethyl)benzidine, 2,3',6,-tris(trifluoromethyl)benzidine, 2,2',3,3'-tetrakis(trif 2,2',5,5'-tetrakis(trifluoromethyl)benzidine, 2,2',6,6'-tetrakis(trifluoromethyl)benzidine, 2,2-di(3-aminophenyl)-1,1,1,3,3,3-hexafluoropropane, 2,2-di(4-aminophenyl)-1,1,1,3,3,3-hexafluoropropane, 2-(3-aminophenyl)-2-(4-aminophenyl)-1,1,1,3,3,3-hexafluoropropane, 1,1-di(3-aminophenyl)-1-phenylethane, 1,1-di(4-aminophenyl)-1-phenylethane, 1-(3-aminophenyl)-1-(4-aminophenyl)-1-phenylethane, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(3-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminobenzoyl)benzene, 1,3-bis(4-aminobenzoyl)benzene, 1,4-bis(3-aminobenzoyl)benzene, 1,4-bis(4-aminobenzoyl)benzene, 1,3 -Bis(3-amino-α,α-dimethylbenzyl)benzene, 1,3-bis(4-amino-α,α-dimethylbenzyl)benzene, 1,4-bis(3-amino-α,α-dimethylbenzyl)benzene, 1,4-bis(4-amino-α,α-dimethylbenzyl)benzene, 1,3-bis(3-amino-α,α-ditrifluoromethylbenzyl)benzene, 1,3-bis(4-amino-α,α-ditrifluoromethylbenzyl)benzene, 1,4-bis(3-amino-α,α-ditrifluoromethylbenzyl)benzene, 1,4-bis(4-amino-α,α-di (trifluoromethylbenzyl)benzene, 2,6-bis(3-aminophenoxy)benzonitrile, 2,6-bis(3-aminophenoxy)pyridine, 4,4'-bis(3-aminophenoxy)biphenyl, 4,4'-bis(4-aminophenoxy)biphenyl, bis[4-(3-aminophenoxy)phenyl]ketone, bis[4-(4-aminophenoxy)phenyl]ketone, bis[4-(3-aminophenoxy)phenyl]sulfide, bis[4-(4-aminophenoxy)phenyl]sulfide, bis[4-(3-aminophenoxy)phenyl]sulfide , bis[4-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(4-aminophenoxy)phenyl]ether, 2,2-bis[4-(3-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[3-(3-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 1,3-bis[4-(3-aminophenoxy)benzoyl]benzene, 1,3-bis[4-(4-aminophenoxy)benzoyl]benzene, 1,4-bis[4-(3-aminophenoxy)benzoyl]benzene, 1,4-bis[4-(4-aminophenoxy)benzoyl]benzene, 1,3-bis[4-(3-aminophenoxy)-α,α-dimethylbenzyl]benzene, 1,3-bis[4-(4-aminophenoxy)-α,α-dimethylbenzyl]benzene, 1,4-bis[4-(3-aminophenoxy)-α,α-dimethylbenzyl]benzene Zene, 1,4-bis[4-(4-aminophenoxy)-α,α-dimethylbenzyl]benzene, 4,4'-bis[4-(4-aminophenoxy)benzoyl]diphenyl ether, 4,4'-bis[4-(4-amino-α,α-dimethylbenzyl)phenoxy]benzophenone, 4,4'-bis[4-(4-amino-α,α-dimethylbenzyl)phenoxy]diphenyl sulfone, 4,4'-bis[4-(4-aminophenoxy)phenoxy]diphenyl sulfone, 3,3'-diamino-4,4'-diphenoxybenzophenone, 3,3'- Diamino-4,4'-diviphenoxybenzophenone, 3,3'-diamino-4-phenoxybenzophenone, 3,3'-diamino-4-biphenoxybenzophenone, 6,6'-bis(3-aminophenoxy)-3,3,3',3'-tetramethyl-1,1'-spirobiindane, 6,6'-bis(4-aminophenoxy)-3,3,3',3'-tetramethyl-1,1'-spirobiindane, 1,3-bis(3-aminopropyl)tetramethyldisiloxane, 1,3-bis(4-aminobutyl)tetramethyldisiloxane, α,ω-bis (3-aminopropyl)polydimethylsiloxane, α,ω-bis(3-aminobutyl)polydimethylsiloxane, bis(aminomethyl)ether, bis(2-aminoethyl)ether, bis(3-aminopropyl)ether, bis(2-aminomethoxy)ethyl]ether, bis[2-(2-aminoethoxy)ethyl]ether, bis[2-(3-aminoprotoxy)ethyl]ether, 1,2-bis(aminomethoxy)ethane, 1,2-bis(2-aminoethoxy)ethane, 1,2-bis[2-(aminomethoxy)ethoxy]ethane, 1,2-Bis[2-(2-aminoethoxy)ethoxy]ethane, ethylene glycol bis(3-aminopropyl)ether, diethylene glycol bis(3-aminopropyl)ether, triethylene glycol bis(3-aminopropyl)ether, ethylenediamine, 1,3-diaminopropane, 1,4-diaminobutane, 1,5-diaminopentane, 1,6-diaminohexane, 1,7-diaminoheptane, 1,8-diaminooctane, 1,9-diaminononane, 1,10-diaminodecane, 1,11-diaminoundecane, 1,12-diaminododecane, 1,2 -diaminocyclohexane, 1,3-diaminocyclohexane, 1,4-diaminocyclohexane, 1,2-di(2-aminoethyl)cyclohexane, 1,3-di(2-aminoethyl)cyclohexane, 1,4-di(2-aminoethyl)cyclohexane, bis(4-aminocyclohexyl)methane, 2,6-bis(aminomethyl)bicyclo[2.2.1]heptane, 2,5-bis(aminomethyl)bicyclo[2.2.1]heptane, 9,9'-bis(4-aminophenyl)fluorene, 9,9'-bis(4-amino-3-fluorophenyl)fluorene.
[0037] The diamine used as the raw material of the transparent polyimide preferably contains any one of a fluoroalkyl group, a sulfone group, a fluorene structure, and an alicyclic structure as the residue Y. As the fluoroalkyl group, a perfluoroalkyl group is preferable, and among them, a trifluoromethyl group is preferable.
[0038] In particular, from the viewpoint of reducing the birefringence of the polyimide film, a diamine in which Y is any one of the following Y-1 to 5 is preferred. From the viewpoint of increasing the transparency and elastic modulus of the polyimide film, a diamine in which Y is the following Y-6 (2,2'-bis(trifluoromethyl)benzidine) is preferred.
[0039] [ka]
[0040] As a raw material of polyimide, multiple kinds of diamines may be used in combination. That is, polyimide may contain multiple kinds of diamine residues Y. For example, by using a diamine in which Y is any one of Y-1 to Y-5 and a diamine in which Y is Y-6 in combination, a polyimide resin has excellent solubility in organic solvents, and a polyimide film having high transparency, high elasticity, and low birefringence can be obtained. Diamines other than the above may be used in combination within a range that does not impair solubility in organic solvents or transparency.
[0041] <Polyimide manufacturing method> As described above, polyimide can be obtained by cyclizing a polyamic acid as a polyimide precursor through dehydration.
[0042] A polyamic acid solution is obtained by reacting an acid dianhydride with a diamine in a solvent. For example, an acid dianhydride and a diamine are dissolved in an organic solvent in approximately equimolar amounts (molar ratio of 95:100 to 105:100) and stirred until polymerization of the acid dianhydride and the diamine is completed, thereby obtaining a polyamic acid solution. If either the acid dianhydride or the diamine is in excess, the molecular weight of the polyamic acid and the polyimide may not be sufficiently large, and the mechanical strength of the polyimide film may decrease.
[0043] In the polymerization, in order to suppress ring-opening of the acid dianhydride, a method of adding the acid dianhydride to the diamine is preferable. When multiple types of diamines or multiple types of acid dianhydrides are added, they may be added at once or in multiple portions. By adjusting the order of addition of the monomers, various physical properties of the polyimide can also be controlled. The solid content concentration of the polyamic acid solution (the charged concentration of the diamine and acid dianhydride in the reaction solution) is usually about 5 to 35% by weight, and preferably 10 to 30% by weight.
[0044] The organic solvent used for the polymerization of polyamic acid is not particularly limited as long as it does not react with diamines and acid dianhydrides and can dissolve polyamic acid. Examples of the organic solvent include urea-based solvents such as methylurea and N,N-dimethylethylurea, sulfoxide or sulfone-based solvents such as dimethylsulfoxide, diphenylsulfone, and tetramethylsulfone, amide-based solvents such as N,N-dimethylacetamide (DMAc), N,N-dimethylformamide (DMF), N,N'-diethylacetamide, N-methyl-2-pyrrolidone (NMP), γ-butyrolactone, and hexamethylphosphoric acid triamide, halogenated alkyl solvents such as chloroform and methylene chloride, aromatic hydrocarbon solvents such as benzene and toluene, and ether-based solvents such as tetrahydrofuran, 1,3-dioxolane, 1,4-dioxane, dimethyl ether, diethyl ether, and p-cresol methyl ether. Usually, these solvents are used alone or in appropriate combination of two or more as necessary. From the viewpoint of the solubility and polymerization reactivity of the polyamic acid, DMAc, DMF, NMP, and the like are preferred.
[0045] Polyimide is obtained by dehydration and cyclization of polyamic acid. Methods for producing a polyimide film from a polyamic acid solution include a method in which the polyamic acid solution is formed into a film and then imidized by heating to obtain a polyimide film; and a method in which a dehydrating agent, an imidization catalyst, etc. are added to the polyamic acid solution, imidization is allowed to proceed in the solution, and then the polyimide solution is formed into a film to obtain a polyimide film. The latter method is preferred because it does not require high-temperature heating for imidization and it is easy to obtain a polyimide film with high transparency.
[0046] In the imidization in the solution, the polyamic acid solution may be heated to promote the progress of imidization. A solution containing the polyimide resin obtained by imidization of polyamic acid is mixed with a poor solvent, the polyimide resin is precipitated as a solid, recovered, and dissolved in a solvent used for film formation to obtain a polyimide resin solution for producing a polyimide film. By precipitating the polyimide resin once as a solid, it is possible to wash and remove impurities generated during polymerization of the polyamic acid, residual dehydrating agents, imidization catalysts, etc. with a poor solvent, and coloring of the polyimide and an increase in yellowness can be prevented. In addition, the method of precipitating the polyimide resin once is also preferable in that a solvent suitable for the film formation conditions of the polyimide film can be applied.
[0047] [Phosphate ester] As will be described in detail later, polyimide films containing phosphate esters tend to have smaller birefringence than polyimide films not containing phosphate esters. The phosphate esters are orthophosphate esters represented by the general formula (2) or condensed phosphate esters represented by the general formula (3).
[0048] [ka]
[0049] R in general formula (2) 1 ~R 3 and R in general formula (3) 4 and R 5 are each independently any monovalent organic group, and are preferably an aryl group which may have a substituent, an aliphatic group having 1 to 20 carbon atoms which may have a branch, or a poly(oxyalkylene)alkyl group.
[0050] Z in the general formula (3) is any divalent organic group, and preferably contains at least one directional ring. n in the general formula (3) is an integer of 1 or more. The condensed phosphate ester represented by the general formula (3) may be a mixture of compounds having different numbers of n.
[0051] The type of phosphoric acid ester is not particularly limited as long as it is compatible with the polyimide. From the viewpoint of suppressing volatilization of the phosphoric acid ester due to heating during the preparation of the polyimide film, the boiling point of the phosphoric acid ester is preferably 200° C. or higher, more preferably 220° C. or higher, further preferably 250° C. or higher, and particularly preferably 280° C. or higher.
[0052] From the viewpoint of reducing volatility, the orthophosphate ester represented by the general formula (2) has a substituent R 1 ~R 3 At least one of R is preferably an aryl group which may have a substituent. 1 ~R 3 Particularly preferred is a wholly aromatic phosphate ester in which all of are aryl groups which may have a substituent.
[0053] Specific examples of wholly aromatic orthophosphate esters include triphenyl phosphate (TPP), tricresyl phosphate (TCP), trixylenyl phosphate (TXP), cresyl diphenyl phosphate (CDP), and cresyl 2,6-xylenyl phosphate (e.g., "PX-110" manufactured by Daihachi Chemical Industry Co., Ltd.).
[0054] From the viewpoint of reducing volatility, the condensed phosphate ester represented by the general formula (3) has a substituent R 4 and R 5 At least one of R is preferably an aryl group which may have a substituent. 4 and R 5 It is particularly preferable that both of the above groups are aryl groups which may have a substituent.
[0055] Specific examples of the divalent substituent Z in the general formula (3) include the following Z-1 to Z-6.
[0056] [ka]
[0057] R in Z-1 to Z-6 7 ~R 16 are each independently a hydrogen atom or an arbitrary substituent (monovalent organic group). In Z-1 to Z-6, two or more substituents may be bonded to one benzene ring. R 6 ~R 16 When is a monovalent organic group, specific examples thereof include chain alkyl groups having 1 to 6 carbon atoms which may have a branch.
[0058] Specific examples of wholly aromatic condensed phosphate esters include resorcinol bisdiphenyl phosphate (e.g., "CR-733S" manufactured by Daihachi Chemical Industry Co., Ltd., and "ADK STAB PFR" manufactured by ADEKA), bisphenol A bisdiphenyl phosphate (e.g., "CR-741" manufactured by Daihachi Chemical Industry Co., Ltd., and "ADK STAB FP-600" manufactured by ADEKA), and resorcinol bisdi-2,6-xylenyl phosphate (e.g., "PX-200" manufactured by Daihachi Chemical Industry Co., Ltd.).
[0059] In addition to the above, commercially available phosphate ester products include "DAIGUARD-1000", "DAIGUARD-580", "DAIGUARD-880", "DAIGUARD-850", and "DAIGUARD-540" manufactured by Daihachi Chemical Industry Co., Ltd., and the "POLYSTEP" series and "STEPFAC" series manufactured by STEPAN Company.
[0060] [Polyimide film] As described above, methods for producing a polyimide film include a method in which a polyamic acid solution is formed into a film and then imidized by heating to obtain a polyimide film; and a method in which an isolated polyimide resin is dissolved in an organic solvent compatible with the polyimide resin to prepare a polyimide solution, the polyamic acid solution is applied onto a substrate, and the organic solvent is removed.
[0061] When preparing a polyimide film containing a phosphoric acid ester, the phosphoric acid ester may be added at any stage. For example, the phosphoric acid ester may be added to a solution during polymerization of polyamic acid or during imidization of polyamic acid. The phosphoric acid ester may also be added when preparing a polyimide solution by dissolving an isolated polyimide resin in an organic solvent. From the viewpoint of suppressing the volatilization of the phosphoric acid ester and increasing the transparency of the polyimide film, a method is preferred in which a polyimide resin and a phosphoric acid ester are dissolved in an organic solvent to prepare a polyimide solution, and the organic solvent is removed from the polyimide solution applied in a film form.
[0062] The organic solvent for dissolving the polyimide resin (and the phosphate ester) is not particularly limited as long as it can dissolve the polyimide resin, and examples of the organic solvent include N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, methyl ethyl ketone, ethyl acetate, methyl acetate, cyclohexanone, dichloromethane, etc. Among them, methyl ethyl ketone, dichloromethane, etc. are preferred because the solvent can be easily dried and removed, and the amount of the solvent remaining in the polyimide film can be reduced.
[0063] The amount of phosphoric acid ester is preferably 3 parts by mass or more, more preferably 5 parts by mass or more, per 100 parts by mass of polyimide. The more phosphoric acid ester is added, the smaller the birefringence of the polyimide film tends to be. In general, additives (retardation regulators) used to reduce the birefringence of resin films tend to act as plasticizers, and mechanical strength such as the tensile modulus of the film tends to decrease with the reduction in retardation. In contrast, when phosphoric acid ester is added to polyimide resin, the tensile modulus of the film is difficult to decrease, even though the phosphoric acid ester has a birefringence reducing effect, and may act as an anti-plasticizer and increase the tensile modulus. Therefore, a transparent polyimide film containing phosphoric acid ester has a lower birefringence than a polyimide film not containing phosphoric acid ester, and may have a tensile modulus equivalent to or higher than a polyimide film not containing phosphoric acid ester.
[0064] Furthermore, the addition of phosphoric ester tends to reduce the yellowness of the polyimide film and increase the light transmittance in the short wavelength region of visible light (around 400 nm), resulting in a polyimide film with little coloring and high transparency.
[0065] From the viewpoint of lowering the birefringence and increasing the transparency (reducing coloration) of the polyimide film, the more the amount of the phosphate ester added, the more preferable. The amount of the phosphate ester relative to 100 parts by mass of polyimide is preferably 10 parts by mass or more, more preferably 15 parts by mass or more, and may be 20 parts by mass or more, 25 parts by mass or more, or 30 parts by mass or more. The condensed phosphate ester of general formula (3) tends to reduce the birefringence of the polyimide film even in a small amount added, compared to the orthophosphate ester of general formula (2).
[0066] The upper limit of the amount of phosphoric acid ester added is not particularly limited, but if it is too large, the effect of reducing birefringence due to an increase in the amount added will saturate, while it may cause film turbidity (increase in haze), a decrease in mechanical strength, and contamination due to bleed-out. The amount of the orthophosphate ester of general formula (2) is preferably 200 parts by mass or less, more preferably 100 parts by mass or less, even more preferably 80 parts by mass or less, and may be 70 parts by mass or less or 60 parts by mass or less, relative to 100 parts by mass of polyimide. The amount of the condensed phosphoric acid ester of general formula (3) is preferably 99 parts by mass or less, more preferably 90 parts by mass or less, even more preferably 80 parts by mass or less, and may be 70 parts by mass or less or 60 parts by mass or less, relative to 100 parts by mass of polyimide.
[0067] The polyimide solution may contain additives (organic or inorganic low-molecular or high-molecular compounds) in addition to the polyimide and phosphate ester. Examples of additives include ultraviolet absorbers, crosslinking agents, dyes, surfactants, leveling agents, plasticizers, fine particles, and sensitizers. The fine particles include organic fine particles such as polystyrene and polytetrafluoroethylene, and inorganic fine particles such as colloidal silica, carbon, and layered silicate, and may have a porous or hollow structure.
[0068] The method of applying the polyimide solution to the substrate can be a known method, for example, by using a bar coater or a comma coater. The substrate to which the polyimide solution is applied can be a glass substrate, a metal substrate such as SUS, a metal drum, a metal belt, a plastic film, or the like. From the viewpoint of improving productivity, it is preferable to use an endless support such as a metal drum or a metal belt, or a long plastic film, or the like, as the substrate, and produce the film by roll-to-roll. When using a plastic film as the substrate, it is sufficient to appropriately select a material that is not dissolved in the solvent of the film-forming dope, and the plastic material can be polyethylene terephthalate, polycarbonate, polyacrylate, polyethylene naphthalate, or the like.
[0069] A transparent polyimide film is obtained by applying a polyimide solution onto a substrate and drying and removing the solvent. It is preferable to perform heating when drying the solvent. The heating temperature is not particularly limited as long as the solvent can be removed and coloring of the obtained transparent polyimide film can be suppressed, and is appropriately set at about room temperature to 250°C. The heating temperature may be increased stepwise. Among them, 50°C to 220°C is more preferable. If the temperature is within this range, coloring of the polyimide can be suppressed and volatilization of the phosphate ester can also be suppressed. In order to increase the efficiency of removing the solvent, the polyimide film may be peeled off from the support after drying has progressed to a certain extent and then dried. In order to promote the removal of the solvent, heating may be performed under reduced pressure.
[0070] The thickness of the polyimide film is not particularly limited and may be appropriately set depending on the application. The thickness of the polyimide film is, for example, 5 μm or more. From the viewpoint of obtaining a film that is both self-supporting and flexible and has high transparency, the thickness of the polyimide film is preferably 20 μm to 100 μm, more preferably 30 μm to 90 μm, further preferably 40 μm to 80 μm, and particularly preferably 50 μm to 80 μm. The thickness of the transparent polyimide film used as a cover film for a display is preferably 50 μm or more.
[0071] The polyimide film preferably has a transmittance of 45% or more at a wavelength of 400 nm, more preferably 50% or more, and even more preferably 55% or more. The yellowness index YI of the polyimide film is preferably 3.0 or less, more preferably 2.5 or less, and may be 2.2 or less or 2.0 or less. As described above, by blending a phosphoric ester, the transmittance at a wavelength of 400 nm tends to increase and the yellowness index tends to decrease. The haze of the polyimide film is preferably 1.5% or less, more preferably 1.2% or less, and may be 1.0% or less, 0.8% or less, or 0.7% or less.
[0072] The tensile modulus E of the polyimide film is preferably 3.0 GPa or more, more preferably 3.5 GPa or more, even more preferably 4.0 GPa or more, and may be 4.5 Ga or more or 5.0 GPa or more. A film with a high tensile modulus tends to have a high scratch hardness according to JIS K5600, and can be suitably used for a member arranged on the outermost surface, such as a cover film for a display layer. The upper limit of the tensile modulus E is not particularly limited, but is generally 10 GPa or less.
[0073] The thickness direction birefringence Δn of the polyimide film is preferably 0.050 or less, and may be 0.040 or less, 0.030 or less, or 0.020 or less. From the viewpoint of suppressing a decrease in visibility such as rainbow unevenness and color shift when viewed from an oblique direction, it is preferable that Δn is as small as possible. The thickness direction birefringence is a value defined by Δn=(Nx+Ny) / 2-Nz. Nx is the refractive index in the slow axis direction in the film plane, Ny is the refractive index in the fast axis direction in the film plane, and Nz is the refractive index in the thickness direction.
[0074] As described above, by blending a phosphate ester, it is possible to reduce birefringence without substantially changing (or increasing) the tensile modulus E. In addition, when a specific phosphate ester such as a condensed phosphate ester is used, the effect of reducing birefringence tends to be greater.
[0075] The birefringence reduction effect by blending a phosphate ester can be evaluated by preparing a polyimide film (a film of polyimide alone) that does not contain a phosphate ester using the same polyimide, and based on the ratio Δn / Δn' of the thickness direction birefringence Δn of the polyimide film containing a phosphate ester to the thickness direction birefringence Δn' of the film of polyimide alone that does not contain a phosphate ester. The smaller Δn / Δn' means the greater the birefringence reduction effect. Δn / Δn' is preferably less than 0.90, more preferably less than 0.80, and even more preferably less than 0.70, and may be less than 0.60, less than 0.50, or less than 0.40. The smaller Δn / Δn' is the better, but it is generally 0.01 or more.
[0076] The suppression of the decrease in modulus of elasticity when a phosphoric acid ester is blended can be evaluated based on the ratio E / E' of the tensile modulus of elasticity E of a polyimide film containing a phosphoric acid ester to the tensile modulus of elasticity E' of a film of polyimide alone not containing a phosphoric acid ester. The closer E / E' is to 1, the more the decrease in tensile modulus of elasticity is suppressed, and when E / E' is greater than 1, it means that the phosphoric acid ester acts as an antiplasticizer. The polyimide film preferably has Δn / Δn' in the above range and E / E' of 0.8 or more. E / E' is more preferably 0.85 or more, even more preferably 0.90 or more, and particularly preferably 0.95 or more. E / E' may be 1 or more, or may be greater than 1. The larger E / E' is, the more preferable, but it is generally 1.2 or less.
[0077] As described above, even when a phosphate ester is blended into a polyimide at a high concentration, a high E / E' ratio is maintained, and thus a polyimide film having a high tensile modulus E and a small thickness direction birefringence Δn can be obtained. At the same blending amount, the condensed phosphate ester represented by general formula (3) tends to have a higher birefringence reducing effect than the orthophosphate ester represented by general formula (2). In an embodiment of the present invention, by adjusting the blending amount according to the type of phosphate ester, a polyimide film having a high tensile modulus ratio E / E' and a small thickness direction birefringence ratio Δn / Δn' can be obtained.
[0078] As described above, by blending a phosphate ester, in addition to reducing the birefringence of the polyimide film, the transparency tends to increase (reduce coloring). The transparency improvement effect by blending a phosphate ester can be evaluated by the ratio T / T' of the transmittance T of a polyimide film containing a phosphate ester at a wavelength of 400 nm to the transmittance T' of a polyimide film alone not containing a phosphate ester at a wavelength of 400 nm, and the larger T / T' means the higher the transparency improvement effect. T / T' is preferably larger than 1, more preferably 1.05 or more, even more preferably 1.10 or more, and may be 1.15 or more, 1.20 or more, or 1.25 or more. T / T' tends to increase with an increase in the blending amount of the phosphate ester. However, if the blending amount of the phosphate ester is excessively large, the haze may increase.
[0079] The transparency improvement effect can also be evaluated from the ratio YI / YI' of the yellowness YI of a polyimide film containing a phosphate ester to the yellowness YI' of a polyimide film alone not containing a phosphate ester, and a smaller YI / YI' indicates a higher transparency improvement effect. YI / YI' is preferably smaller than 1, more preferably 0.95 or less, and even more preferably 0.90 or less, and may be 0.85 or less, 0.80 or less, 0.75 or less, or 0.70 or less.
[0080] [Polyimide film applications] The transparent polyimide film according to the embodiment of the present invention is suitable for use as a display material because of its high transparency and low birefringence. In particular, the polyimide film having high mechanical strength can be applied to a surface member such as a cover film of a display. When used in practical use, the transparent polyimide film may be provided on its surface with an antistatic layer, an easy-adhesion layer, a hard coat layer, an antireflection layer, or the like. EXAMPLES
[0081] The present invention will be described in more detail below based on examples of preparing polyimide films, although the present invention is not limited to the following specific examples.
[0082] The organic solvents and compounds are described by the following abbreviations: TFMB: 2,2'-bis(trifluoromethyl)benzidine 3,3'-DDS: 3,3'-diaminodiphenyl sulfone CBDA: 1,2,3,4-cyclobutanetetracarboxylic dianhydride 6FDA: 2,2-bis(3,4-dicarboxyphenyl)-1,1,1,3,3,3-hexafluoropropane dianhydride BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride TMHQ: bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-carboxylic acid) 1,4-phenylene TAHMBP: bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-carboxylic acid) 2,2',3,3',5,5'-hexamethylbiphenyl-4,4'-diyl
[0083] [Production Examples 1 to 3: Preparation of polyimide resin] <Preparation of polyamic acid solution> DMF was placed in a separable flask and stirred under a nitrogen atmosphere. Diamine and dianhydride were added in the ratios shown in Table 1, and the mixture was reacted by stirring under a nitrogen atmosphere for 5 to 10 hours to obtain a polyamic acid solution with a solid content of 18%.
[0084] [Table 1]
[0085] <Imidization and separation of polyimide resin> 5.5 g of pyridine was added as an imidization catalyst to the polyamic acid solution and completely dispersed, after which 8 g of acetic anhydride was added and stirred at 90°C for 3 hours. While stirring the solution cooled to room temperature, 100 g of 2-propyl alcohol (hereinafter referred to as "IPA") was added dropwise at a rate of 2 to 3 drops per second to precipitate polyimide. Further, 150 g of IPA was added, and after stirring for about 30 minutes, suction filtration was performed using a Kiriyama funnel. The obtained solid was washed with 100 g of IPA. After repeating the washing process six times, the solution was dried for 12 hours in a vacuum oven set at 120°C to obtain polyimide resins 1 to 3.
[0086] [Reference Examples 1 to 3: Preparation of polyimide films not containing phosphate ester] <Reference example 1> Polyimide resin 1 was dissolved in methylene chloride to prepare a polyimide solution with a solid content of 11%. The polyimide solution was applied to a non-alkali glass plate and heated in air at 40°C for 60 minutes, 70°C for 30 minutes, 150°C for 30 minutes, and 170°C for 30 minutes to remove the solvent, obtaining a polyimide film with the thickness shown in Table 2. The film thickness was measured using a length gauge (ND-CT2501 manufactured by Heidenhain).
[0087] <Reference examples 2 and 3> A polyimide film was prepared in the same manner as in Reference Example 1, except that polyimide resins 2 and 3 were used instead of polyimide resin 1.
[0088] [Preparation of polyimide film containing phosphate ester] In preparing the polyimide solution, the type and amount of phosphoric ester shown in Table 2 was added to 100 parts by mass of the polyimide resin. Otherwise, polyimide films 1A to 1L were prepared in the same manner as in Reference Example 1; polyimide films 2A to 2N were prepared in the same manner as in Reference Example 2; and polyimide film 3A was prepared in the same manner as in Reference Example 3. The polyimide solution was applied to a non-alkali glass plate, and the solvent was removed to prepare a film. Details of phosphoric esters 1 to 8 are as follows.
[0089] Phosphate ester 1: Triphenyl phosphate (Tokyo Chemical Industry Co., Ltd.) Phosphate ester 2: Non-halogen type orthophosphate ester (Daihachi Chemical Industry "DAIGUARD-1000" Phosphate ester 3: Resorcinol bisdiphenyl phosphate (Daihachi Chemical Industry "CR-733S") Phosphate ester 4: Bisphenol A bisdiphenyl phosphate (Daihachi Chemical Industry "CR-741" Phosphate ester 5: Tricresyl phosphate (Tokyo Chemical Industry Co., Ltd.) Phosphate ester 6: Tris(2-ethylhexyl)phosphate (Tokyo Chemical Industry Co., Ltd.) Phosphate ester 7: Cresyl diphenyl phosphate (Tokyo Chemical Industry Co., Ltd.) Phosphate ester 8: Resorcinol bis(di-2,6-xylenyl phosphate) ("PX-200" manufactured by Daihachi Chemical Industry Co., Ltd.)
[0090] [Evaluation of polyimide film] <Thickness direction birefringence (△n)> The polyimide film was cut into 3 cm squares, and the thickness retardation Rth and in-plane retardation Re were measured at a wavelength of 590 nm using an automatic birefringence meter "KOBRA" manufactured by Oji Scientific Instruments, with the average refractive index set to 1.60. The thickness direction birefringence △n = (Nx + Ny) / 2 - Nz was calculated from the three-dimensional refractive index calculated from the measured values (refractive indexes Nx and Ny in the in-plane direction, and refractive index Nz in the thickness direction).
[0091] <Tensile modulus> Measurements were performed using Shimadzu Corporation's "AUTOGRAPH AGS-X" under the following conditions: Sample measurement range: width 10 mm, grip distance: 100 mm, tensile speed: 20.0 mm / min, measurement temperature: 23°C. The samples were left to stand at 23°C / 55% RH for one day to condition the humidity.
[0092] <Yellowness (YI)> Measurements were taken using a 3cm square sample with a spectrophotometer "SC-P" manufactured by Suga Test Instruments.
[0093] <Transmittance at 400 nm> The light transmittance of the film was measured in the range of 300 to 800 nm using a UV-visible spectrophotometer "V-560" manufactured by JASCO Corporation, and the light transmittance at a wavelength of 400 nm was read.
[0094] <Haze> The haze was measured using a haze meter "HZ-V3" manufactured by Suga Test Instruments according to the method described in JIS K7136.
[0095] The compositions of the polyimide films (type of polyimide resin, type and content of phosphate ester) and the evaluation results of the polyimide films are shown in Table 2. The elastic modulus ratio in Table 2 is the ratio E / E' of the tensile elastic modulus E of the polyimide film containing phosphate ester to the tensile elastic modulus E' of the polyimide film of the Reference Example not containing phosphate ester. Similarly, the birefringence ratio, YI ratio and transmittance ratio are the ratios of the thickness direction birefringence Δn, yellowness index YI and transmittance at a wavelength of 400 nm, respectively, relative to the Reference Example. Note that Film 1J was significantly cloudy, so no evaluation was performed other than for thickness.
[0096] [Table 2]
[0097] Films 1A to 1L made using polyimide resin 1, except for film 1J, showed a lower birefringence than Reference Example 1 without a significant increase in haze, and a tendency was observed for the birefringence to decrease with an increase in the amount of phosphate added. A comparison of films 1C, 1F, 1H, and 1K to which 40 parts by mass of phosphate was added shows that the birefringence-reducing effect of adding phosphate is more significant in films 1H and 1K, which use condensed phosphate.
[0098] In Film 1L, the tensile modulus was reduced to about half that of Reference Example 1. It can be seen that in Films 1A to 1H and 1K, the addition of phosphate ester reduces birefringence while maintaining the tensile modulus. Among them, Films 1A, 1F, 1G and 1H had modulus ratios exceeding 1, indicating that the phosphate ester tends to act as an antiplasticizer. Furthermore, the addition of phosphate ester tended to increase the transmittance at a wavelength of 400 nm and decrease the yellowness index.
[0099] The same tendency as above was confirmed in films 2A to 2N made using polyimide resin 2 and film 3A made using polyimide resin 3, but film 2K using phosphate ester 6 had a higher yellowness index than Reference Example 2 and a lower elastic modulus than the other examples. From these results, it is considered that aromatic phosphate esters are suitable for obtaining polyimide films with high mechanical strength and transparency and small birefringence.
[0100] In Films 2D to 2H, the birefringence tended to decrease with increasing amount of phosphate ester added, but in Films 2D and 2E, the birefringence ratio was greater than 0.9 and the effect of reducing birefringence was insufficient. The same was true for Film 2M, which contained 3 parts by mass of phosphate ester added.
[0101] From the above results, it is clear that the inclusion of a phosphate ester makes it possible to achieve high transparency and low birefringence while maintaining or improving the elastic modulus of the polyimide film, and that by adjusting the type and amount of phosphate ester added, a transparent polyimide film with excellent mechanical strength and extremely low birefringence can be obtained.
Claims
1. A transparent polyimide film comprising a polyimide and a phosphoric acid ester, The polyimide contains a repeating unit represented by general formula (1), 【Chemistry 3】 In general formula (1), X is any tetravalent organic group; Y is a divalent organic group and contains at least one selected from the group consisting of a fluoroalkyl group, a sulfone group, a fluorene structure, and an alicyclic structure; The phosphate ester is an orthophosphate ester represented by general formula (2) or a condensed phosphate ester represented by general formula (3), 【Chemistry 1】 In formula (2), R 1 to R 3 each independently represent an aryl group which may have a substituent; In general formula (3), n is an integer of 1 or more, R 4 and R 5 each independently represent an aryl group which may have a substituent, Z is a divalent organic group containing at least one aromatic ring, The content of the phosphoric acid ester relative to 100 parts by mass of the polyimide is 5 to 100 parts by mass. Transparent polyimide film.
2. The ratio E / E' of the tensile modulus E of the transparent polyimide film to the tensile modulus E' of a film of the polyimide alone containing no phosphate ester is 0.80 or more, a ratio Δn / Δn′ of the birefringence in the thickness direction of the transparent polyimide film to the birefringence in the thickness direction of a film of the polyimide alone not containing a phosphate ester is less than 0.90; The transparent polyimide film according to claim 1 .
3. 3. The transparent polyimide film according to claim 2, wherein E / E' is 0.95 or more.
4. A transparent polyimide film described in any one of claims 1 to 3, wherein the content of the phosphate ester per 100 parts by mass of the polyimide is 15 to 100 parts by mass.
5. The phosphate ester is a condensed phosphate ester represented by the general formula (3), The transparent polyimide film according to any one of claims 1 to 4, wherein the organic group Z is any one of the following Z-1 to Z-6: 【Chemistry 2】 R 7 ~R 16 are each independently a hydrogen atom or an optionally branched chain alkyl group having 1 to 6 carbon atoms, and two or more substituents may be bonded to one benzene ring.
6. 5. The transparent polyimide film according to claim 1, wherein the phosphate ester is at least one selected from the group consisting of triphenyl phosphate, tricresyl phosphate, cresyl diphenyl phosphate, resorcinol bisdiphenyl phosphate, bisphenol A bisdiphenyl phosphate, and resorcinol bis(di 2,6-xylenyl phosphate).
7. The transparent polyimide film according to claim 1, wherein in the polyimide, the organic group X in the general formula (1) includes one or more selected from the group consisting of a fluoroalkyl group, an ether bond, a thioether bond, an ester bond, a sulfone group, an alicyclic structure, and a linear aliphatic group having two or more carbon atoms.
8. The thickness is 5 μm or more and 100 μm or less, The haze is 1.5% or less, The yellowness index is 3.0 or less, The tensile modulus E is 3.0 GPa or more. The transparent polyimide film according to any one of claims 1 to 7.
9. 9. The transparent polyimide film according to claim 1, wherein the thickness direction birefringence Δn is 0.050 or less.
10. A method for producing the transparent polyimide film according to any one of claims 1 to 9, comprising the steps of: preparing a polyimide solution by dissolving a solvent-soluble polyimide resin and a phosphoric acid ester in an organic solvent that is soluble in the polyimide resin; applying the polyimide solution to a substrate and removing the organic solvent; A method for producing a transparent polyimide film.
Citation Information
Patent Citations
Photosensitive resin composition and photosensitive dry film resist and photosensitive coverlay film using the same
JP2007108761A
Transparent polyimide film and method of manufacturing the same
JP2012144603A
Manufacturing method of flexible device
JP2016062965A
Polyimide, method for producing polyimide, polyimide solution and polyimide film
JP2016132686A
Polyimide resin, polyimide solution, film, and method for producing same
WO2017175869A1