Chloroprene block copolymer, latex, latex composition, and rubber composition
A chloroprene-based block copolymer with specific polymer blocks addresses the need for allergy-free and cost-effective polychloroprene rubber compositions by achieving high tensile strength and flexibility without vulcanizing agents or accelerators.
Patent Information
- Application Number
- JP2022510496
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-26
- Filing Date
- 2021-03-22
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-03-22
AI Technical Summary
Conventional polychloroprene rubber compositions rely on vulcanizing agents and accelerators, which cause skin allergies and increase costs, necessitating the development of a composition that achieves mechanical strength without these components.
A chloroprene-based block copolymer comprising specific polymer blocks with glass transition temperatures above 80°C, formulated without vulcanizing agents or accelerators, ensuring excellent flexibility and tensile properties.
The copolymer achieves tensile strengths of 17 MPa or more and elongations of 900% or more, maintaining mechanical integrity without the use of vulcanizing agents or accelerators, thereby reducing allergies and costs.
Smart Images

Figure 0007575447000001 
Figure 0007575447000002 
Figure 0007575447000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a chloroprene block copolymer, a latex, a latex composition, and a rubber composition. [Background technology]
[0002] Various techniques have been proposed for chloroprene block copolymers containing chloroprene polymer blocks. Prior art documents include a copolymer obtained by polymerizing chloroprene using azo group-containing polystyrene as an initiator (see, for example, Patent Document 1), a copolymer obtained by polymerizing an aromatic vinyl monomer with dithiocarbamated polychloroprene (see, for example, Patent Document 2), a copolymer obtained by linking a hydrophilic oligomer or hydrophilic polymer to a chloroprene polymer (see, for example, Patent Document 3), a copolymer having an aromatic vinyl compound polymer block and a chloroprene polymer block, with the overall number average molecular weight and the number average molecular weight of the chloroprene polymer block specified (see, for example, Patent Document 4), and a copolymer having an acrylic acid ester polymer block and a chloroprene polymer block (see, for example, Patent Document 5). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 3-207710 [Patent Document 2] Japanese Patent Application Publication No. 3-212414 [Patent Document 3] JP 2007-297502 A [Patent Document 4] International Publication No. 2018 / 181801 [Patent Document 5] International Publication No. 2019 / 026914 Summary of the Invention [Problem to be solved by the invention]
[0004] Conventionally, in order to obtain the desired mechanical strength of polychloroprene rubber compositions, it has been necessary to use vulcanizing agents such as sulfur, zinc oxide, magnesium oxide, and vulcanization accelerators such as thiuram, dithiocarbamate, thiourea, guanidine, xanthogenate, and thiazole. Since vulcanization accelerators are causative substances of type IV allergies that cause skin diseases such as dermatitis, reducing or eliminating the use of vulcanization accelerators has become an important theme. In addition, since eliminating the use of vulcanization accelerators leads not only to a reduction in allergies but also to cost reduction, a rubber composition that exhibits sufficient mechanical strength without using vulcanization accelerators is desired.
[0005] Therefore, an object of the present invention is to provide a chloroprene-based block copolymer, a latex, a latex composition, and a rubber composition which can provide products having excellent flexibility and tensile properties without using a vulcanizing agent or a vulcanization accelerator. [Means for solving the problem]
[0006] The present invention relates to the following. (1) A chloroprene-based block copolymer comprising 5 to 30 mass% of a polymer block (A) derived from a monomer which, upon homopolymerization, gives a polymer having a glass transition temperature of 80° C. or higher, and 70 to 95 mass% of a chloroprene-based polymer block (B) containing a chloroprene monomer; A chloroprene block copolymer having a toluene insoluble content of 20 to 100% by mass relative to 100% by mass of the chloroprene block copolymer.
[0007] (2) The chloroprene block copolymer according to (1), comprising 5 to 15 mass% of the polymer block (A) and 85 to 95 mass% of the chloroprene polymer block (B) based on 100 mass% of the chloroprene block copolymer.
[0008] (3) The chloroprene block copolymer according to (1) or (2), wherein a molded body of a latex composition containing the chloroprene block copolymer has a tensile strength at break of 17 MPa or more as measured in accordance with JIS K 6251 after heat-treating the molded body of the latex composition at 130°C for 30 minutes.
[0009] (4) The chloroprene block copolymer according to any one of (1) to (3), wherein the polymer block (A) has a number average molecular weight of 10,000 or more.
[0010] (5) The chloroprene block copolymer according to any one of (1) to (4), wherein the molecular weight distribution of the polymer block (A) is 2.0 or less.
[0011] (6) The chloroprene block copolymer according to any one of (1) to (5), wherein the polymer block (A) is a polymer block composed of aromatic vinyl monomer units.
[0012] (7) The chloroprene block copolymer according to any one of (1) to (6), which has a functional group having a structure represented by chemical formula (1) or chemical formula (2). [ka] (In chemical formula (1), R1 represents hydrogen, chlorine, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkenyl group, a substituted or unsubstituted aryl group, a mercapto group, or a substituted or unsubstituted heterocyclyl group.) [ka]
[0013] (8) A latex comprising the chloroprene block copolymer according to any one of (1) to (7).
[0014] (9) A latex composition comprising 100 parts by mass of the latex according to (8) above and 0.5 to 5.0 parts by mass of an antioxidant.
[0015] (10) The latex composition according to (9), which does not contain a vulcanizing agent and a vulcanization accelerator.
[0016] (11) A rubber composition comprising the chloroprene block copolymer according to any one of (1) to (7).
[0017] (12) A rubber composition comprising the latex of (8) or the latex composition of (9) to (10). Effect of the Invention
[0018] According to the present invention, there are provided a chloroprene block copolymer, a latex, a latex composition and a rubber composition which can provide products having excellent flexibility and tensile properties without using a vulcanizing agent or a vulcanization accelerator. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, embodiments of the present invention will be described in detail. In this specification and claims, the expression "A to B" means A or more and B or less.
[0020] <Chloroprene block copolymer> The chloroprene block copolymer is a block copolymer containing a polymer block (A) derived from a monomer that, when homopolymerized, gives a polymer having a glass transition temperature of 80°C or higher, and a chloroprene polymer block (B) containing a chloroprene monomer. Chloroprene block copolymers also include those having a structure in which block copolymers are chemically bonded to each other.
[0021] [Polymer block (A)] The polymer block (A) is a polymer block derived from a monomer that can give a polymer having a glass transition temperature of 80° C. or more when homopolymerized. By using such a monomer, the tensile strength at break of the obtained chloroprene block copolymer is improved. It is preferable to use a monomer that can give a polymer having a glass transition temperature of 85° C. or more. From the viewpoint of moldability, a monomer that can give a polymer having a glass transition temperature of 150° C. or less is preferable, and a monomer that can give a polymer having a glass transition temperature of 120° C. or less is particularly preferable. The glass transition temperature is, for example, 80, 85, 90, 95, 100, 105, 110, 120, 130, 140, or 150° C., and may be within a range between any two of the values exemplified here. In this specification, the glass transition temperature is the extrapolated glass transition end temperature (T eg ) measured in accordance with JIS K 7121. When the polymer block (A) is a polymer block obtained by polymerizing a monomer (A), the monomer (A) is preferably a monomer that, when the monomer A is homopolymerized to give a homopolymer (A) having a number average molecular weight of 10,000 to 30,000, has the above-mentioned glass transition temperature.
[0022] Examples of monomer units constituting the polymer block (A) include aromatic vinyl monomer units, methyl methacrylate monomer units, and acrylonitrile monomer units. Preferably, units derived from aromatic vinyl monomers are used, and styrene units are preferably used. The polymer block (A) may be a polymer block obtained by copolymerization of these monomers, or a polymer block composed of monomer units copolymerizable with these monomers, within the scope of the present invention.
[0023] The number average molecular weight of the polymer block (A) is preferably 10,000 or more from the viewpoint of tensile properties and moldability of the resulting chloroprene block copolymer, and the molecular weight distribution of the polymer block (A) is preferably 2.0 or less from the viewpoint of moldability. In this specification, the number average molecular weight and the weight average molecular weight are values calculated as polystyrene measured by gel permeation chromatography (GPC) under the measurement conditions described below. Device name: HLC-8320 (Tosoh Corporation) Column: 3 TSKgel GMHHR-H in series Temperature: 40℃ Detection: Differential refractive index Solvent: Tetrahydrofuran Calibration curve: Prepared using standard polystyrene (PS).
[0024] [Chloroprene polymer block (B)] The chloroprene polymer block (B) contains chloroprene monomer (2-chloro-1,3-butadiene) units and is mainly composed of chloroprene monomers. The chloroprene polymer block (B) may be a polymer block consisting of chloroprene monomer units and units derived from a monomer copolymerizable with the chloroprene monomer, as long as the object of the present invention is not impaired. The chloroprene polymer block (B) preferably contains 90% by mass or more of structural units derived from chloroprene monomers, when the chloroprene polymer block (B) is taken as 100% by mass. The chloroprene polymer block (B) may also contain no repeating units other than the structural units derived from the chloroprene monomer.
[0025] The content of each structural unit in the chloroprene-based block copolymer is 5-30% by mass for polymer block (A) and 70-95% by mass for chloroprene-based polymer block (B), preferably 5-15% by mass for polymer block (A) and 85-95% by mass for chloroprene-based polymer block (B). When the polymer block (A) is 5% by mass or more, the tensile strength at break of the obtained chloroprene-based block copolymer is improved. When the polymer block (A) is 30% by mass or less, the flexibility of the obtained chloroprene-based block copolymer is improved. The polymer block (A) is preferably 15% by mass or less. When the chloroprene-based polymer block (B) is 70% by mass or more, the flexibility of the obtained chloroprene-based block copolymer is improved. The chloroprene-based polymer block (B) is preferably 85% by mass or more. When the chloroprene-based polymer block (B) is 95% by mass or less, the tensile strength at break of the obtained chloroprene-based block copolymer is improved. When the chloroprene-based block copolymer is taken as 100% by mass, the content of the polymer block (A) contained in the chloroprene-based block copolymer is, for example, 5, 10, 15, 20, 25, or 30% by mass, and may be within a range between any two of the numerical values exemplified here. The chloroprene block copolymer according to one embodiment of the present invention may be composed of a polymer block (A) and a polymer block (B) and may not contain any other polymer block. The chloroprene block copolymer may be a diblock copolymer of polymer block (A) and polymer block (B).
[0026] The weight average molecular weight of the chloroprene block copolymer is not particularly limited, but from the viewpoint of moldability, it is preferably from 50,000 to 600,000, and particularly preferably from 100,000 to 500,000.
[0027] The toluene insoluble content of the chloroprene block copolymer of the present embodiment is in the range of 20 to 100% by mass. When the toluene insoluble content is 20% by mass or more, the tensile strength at break is improved.
[0028] The chloroprene block copolymer of the present embodiment preferably has a tensile strength at break of 17 MPa or more, measured in accordance with JIS K 6251 after a molded article of a latex composition containing the chloroprene block copolymer is heat-treated at 130° C. for 30 minutes. The tensile strength at break is more preferably 18 MPa or more, even more preferably 19 MPa or more, and even more preferably 20 MPa or more. There is no particular upper limit, but it is, for example, 30 MPa or less.
[0029] Furthermore, the chloroprene block copolymer of the present embodiment has an elongation at break of preferably 900% or more, more preferably 905% or more, and even more preferably 910% or more, as measured in accordance with JIS K 6251 after a molded article of a latex composition containing the chloroprene block copolymer is heat-treated at 130° C. for 30 minutes. The upper limit is not particularly limited, but is, for example, 1300% or less.
[0030] The chloroprene block copolymer of the present embodiment has a modulus at 500% elongation of preferably 3.0 MPa or less, more preferably 2.9 MPa or less, and even more preferably 2.8 MPa or less, as measured in accordance with JIS K 6251 after a molded article of a latex composition containing the chloroprene block copolymer is heat-treated at 130° C. for 30 minutes. The lower limit is not particularly limited, but is, for example, 1.0 MPa or more.
[0031] The chloroprene block copolymer of the present embodiment can be such that a molded article made of a rubber composition and a latex composition containing the chloroprene block copolymer has the above-mentioned tensile strength, elongation at break, and modulus at 500% elongation after heat treatment at 130°C for 30 minutes. The molded article can be molded without using a vulcanizing agent or a vulcanization accelerator. The molded article for measuring the tensile strength can be obtained by the method described in the Examples.
[0032] The tensile strength at break, elongation at break, and modulus at 500% elongation of the chloroprene block copolymer can be adjusted by adjusting the toluene insoluble content of the chloroprene block copolymer or by adjusting the content of polymer block (A) in the chloroprene block copolymer.
[0033] [Method for producing chloroprene block copolymer] The method for producing the chloroprene-based block copolymer according to the present invention will be described. The polymerization method is not particularly limited, and the copolymer can be produced by a known method such as solution polymerization, emulsion polymerization, or bulk polymerization, but emulsion polymerization is preferable for obtaining the desired chloroprene-based block copolymer.
[0034] The polymerization method is not particularly limited as long as a desired chloroprene-based block copolymer can be obtained, but it is possible to produce the chloroprene-based block copolymer by a production method that involves a two-step polymerization process consisting of a polymerization process 1 for synthesizing a polymer block (A) followed by a polymerization process 2 for synthesizing a chloroprene-based polymer block (B). A production method for a chloroprene-based block copolymer according to one embodiment of the present invention includes a polymerization process 1 for synthesizing a polymer block (A) by polymerizing a raw material containing a monomer (A), and a polymerization process 2 for obtaining a latex containing a chloroprene-based block copolymer by emulsion polymerization by adding pure water, an emulsifier, and a raw material containing a chloroprene monomer to a latex containing the polymer block (A) obtained by living radical emulsion polymerization in the polymerization process 1.
[0035] (Polymerization step 1) The polymerization step 1 will be specifically described. In the polymerization step 1, the monomers constituting the polymer block (A) are subjected to living radical emulsion polymerization to synthesize the polymer block (A). As described above, the polymer block (A) obtained here preferably has the above-mentioned glass transition temperature. The emulsifier used in the emulsion polymerization is not particularly limited, but an anionic or nonionic emulsifier is preferable from the viewpoint of emulsion stability. In particular, it is preferable to use an alkali metal salt of rosin acid because it can provide the obtained chloroprene block copolymer with appropriate strength and prevent excessive shrinkage and breakage. From the viewpoint of efficient polymerization reaction, the concentration of the emulsifier is preferably 5 to 50% by mass relative to 100% by mass of the monomers constituting the polymer block (A). As the radical polymerization initiator, a known radical polymerization initiator can be used, for example, potassium persulfate, benzoyl peroxide, hydrogen peroxide, azo compounds, etc. can be used. The amount of pure water added is preferably 100 to 300% by mass relative to 100% by mass of the monomers constituting the polymer block (A). When the amount of added pure water is 300% by mass or less, the toluene insoluble content of the obtained chloroprene block copolymer is 20% by mass or more, and the tensile strength at break is improved. The polymerization temperature may be appropriately determined depending on the type of monomer, but is preferably 10 to 100°C, and particularly preferably 20 to 80°C.
[0036] (Polymerization step 2) In the polymerization step 2, pure water, an emulsifier, and a chloroprene monomer are added to the latex containing the polymer block (A) obtained by the living radical emulsion polymerization in the polymerization step 1, and the latex containing the target chloroprene block copolymer is obtained by emulsion polymerization. The chloroprene monomer may be added all at once or in portions. The polymerization temperature in the polymerization step 2 is preferably 10 to 50°C from the viewpoint of ease of polymerization control. The polymerization reaction is terminated by adding a polymerization terminator. Examples of the polymerization terminator include thiodiphenylamine, 4-tert-butylcatechol, and 2,2'-methylenebis-4-methyl-6-tert-butylphenol. Unreacted monomers after the emulsion polymerization can be removed by a conventional method such as reduced pressure distillation. The production method according to one embodiment of the present invention exemplified above makes it easier to obtain a chloroprene block copolymer having an appropriate toluene insoluble content.
[0037] To the latex containing the chloroprene-based block copolymer obtained in the polymerization step 2, a freezing stabilizer, an emulsion stabilizer, a viscosity modifier, an antioxidant, a preservative, etc. can be added arbitrarily after the polymerization within a range not impairing the object of the present invention.
[0038] (Recovery process) The method for recovering the chloroprene-based block copolymer from the latex containing the chloroprene-based block copolymer is not particularly limited, and any known method can be used, such as a method of recovering the chloroprene-based block copolymer by immersing the copolymer in a coagulation liquid or a method of precipitating the copolymer using a poor solvent such as methanol.
[0039] The chloroprene-based block copolymer preferably has a functional group having a structure represented by the following chemical formula (1) or chemical formula (2).
[0040] [ka] (In chemical formula (1), R1 represents hydrogen, chlorine, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkenyl group, a substituted or unsubstituted aryl group, a mercapto group, or a substituted or unsubstituted heterocyclyl group.)
change
[0041] The terminal structure represented by the above chemical formula (1) or chemical formula (2) is introduced into a block copolymer by emulsion polymerization in the presence of a known RAFT agent. The compound leading to the structure represented by the above chemical formula (1) is not particularly limited, and general compounds can be used, such as dithiocarbamates and dithioesters. Specifically, benzyl 1-pyrrole carbodithioate (common name: benzyl 1-pyrrole dithiocarbamate), benzyl phenyl carbodithioate, 1-benzyl-N,N-dimethyl-4-aminodithiobenzoate, 1-benzyl-4-methoxydithiobenzoate, 1-phenylethyl imidazole carbodithioate (common name: 1-phenylethyl imidazole dithiocarbamate), benzyl-1-(2-pyrrolidinone) carbodithioate, etc. oate) (common name: benzyl-1-(2-pyrrolidinone)dithiocarbamate), benzyl phthalimidyl carbodithioate, (common name: benzyl phthalimidyl dithiocarbamate), 2-cyanoprop-2-yl-1-pyrrole carbodithioate, (common name: 2-cyanoprop-2-yl-1-pyrrole dithiocarbamate), 2-cyanobut-2-yl-1-pyrrole carbodithioate, (common name: 2-cyanobut-2-yl- 1-Pyrrole dithiocarbamate), benzyl-1-imidazole carbodithioate, (common name benzyl-1-imidazole dithiocarbamate), 2-cyanoprop-2-yl-N,N-dimethyldithiocarbamate, benzyl-N,N-diethyldithiocarbamate, cyanomethyl-1-(2-pyrrolidone)dithiocarbamate, 2-(ethoxycarbonylbenzyl)prop-2-yl-N,N-diethyldithiocarbamate, 1-phenyl nylethyl dithiobenzoate, 2-phenylprop-2-yl dithiobenzoate, 1-acetate-1-yl-ethyl dithiobenzoate, 1-(4-methoxyphenyl)ethyl dithiobenzoate, benzyl dithioacetate, ethoxycarbonylmethyl dithioacetate, 2-(ethoxycarbonyl)prop-2-yl dithiobenzoate, 2-cyanoprop-2-yl dithiobenzoate, tert-butyl dithiobenzoate, 2,4,4-Trimethylpent-2-yldithiobenzoate, 2-(4-chlorophenyl)-prop-2-yldithiobenzoate, 3-vinylbenzyldithiobenzoate, 4-vinylbenzyldithiobenzoate, benzyldiethoxyphosphinyldithioformate, tert-butyltrithioperbenzoate, 2-phenylprop-2-yl-4-chlorodithiobenzoate, naphthalene-1-carboxylic acid-1-methyl-1-phenyl-ethyl ester, 4-cyano-4-methyl-4-thiobenzylsulfanylbutyric acid, dibenzyltetrathioterephthalate, carboxymethyldithiobenzoate, poly(ethylene oxide) with dithiobenzoate end groups, poly(ethylene oxide) with 4-cyano-4-methyl-4-thiobenzylsulfanylbutyric acid end groups, 2-[(2-phenylethanethioyl)sulfanyl]propane Acid, 2-[(2-phenylethanethioyl)sulfanyl]succinic acid, potassium 3,5-dimethyl-1H-pyrazole-1-carbodithioate, cyanomethyl-3,5-dimethyl-1H-pyrazole-1-carbodithioate, cyanomethylmethyl-(phenyl)dithiocarbamate, benzyl-4-chlorodithiobenzoate, phenylmethyl-4-chlorodithiobenzoate, 4-nitrobenzyl-4-chlorodithiobenzoate, phenylprop-2-yl-4-chlorodithiobenzoate, 1-cyano-1-methylethyl-4-chlorodithiobenzoate, 3-chloro-2-butenyl-4-chlorodithiobenzoate, 2-chloro-2-butenyl dithiobenzoate, benzyl dithioacetate, 3-chloro-2-butenyl-1H-pyrrole-1-dithiocarboxylic acid, 2-cyanobutan-2-yl 4-chloro-3,Examples of the compound that leads to the structure represented by the above chemical formula (2) include 5-dimethyl-1H-pyrazole-1-carbodithioate and cyanomethylmethyl(phenyl)carbamodithioate. Among these, benzyl 1-pyrrole carbodithioate and benzylphenyl carbodithioate are particularly preferred. The compound that leads to the structure represented by the above chemical formula (2) is not particularly limited and can be a general compound, for example, 2-cyano-2-propyldodecyltrithiocarbonate, dibenzyltrithiocarbonate, butylbenzyltrithiocarbonate, 2-[[(butylthio)thioxomethyl]thio]propionic acid, 2-[[(dodecylthio)thioxomethyl]thio]propionic acid, 2-[[(butylthio)thioxomethyl]thio]succinic acid, 2-[[(dodecyl ... ]-2-methylpropionic acid, 2,2'-[carbonothioylbis(thio)]bis[2-methylpropionic acid], 2-amino-1-methyl-2-oxoethylbutyl trithiocarbonate, benzyl 2-[(2-hydroxyethyl)amino]-1-methyl-2-oxoethyltrithiocarbonate, 3-[[[(tert-butyl)thio]thioxomethyl]thio]propionic acid, cyanomethyldodecyltrithiocarbonate, diethylaminobenzyltrithiocarbonate, dibutylaminobenzyltrithiocarbonate and other trithiocarbonates are included. Among these, dibenzyltrithiocarbonate and butylbenzyltrithiocarbonate are particularly preferred.
[0042] [Toluene insolubles] The toluene insoluble content of the chloroprene block copolymer of the present embodiment is in the range of 20 to 100% by mass relative to 100% by mass of the chloroprene block copolymer. When the toluene insoluble content is 20% by mass or more, the block copolymers contain a structure in which they are chemically bonded to each other, and therefore the tensile strength at break is improved. The toluene insoluble content can be, for example, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, or 100, and may be within a range between any two of the numerical values exemplified here. In this specification, the toluene insoluble content is calculated by dissolving a freeze-dried latex containing a chloroprene block copolymer in toluene, centrifuging the gel content, separating it using a 200-mesh wire net, and measuring the weight of the dried product, and then calculating it from the following formula. (Weight of solid obtained by separating and drying gel fraction) / (Weight of solid obtained by freeze-drying latex containing chloroprene-based block copolymer)×100 The toluene-insoluble content can be adjusted by controlling the types and amounts of raw materials used in polymerization of the chloroprene block copolymer as well as the polymerization conditions, and by controlling the type and amount of polymer blocks, for example, the type, amount and structure of functional groups derived from a RAFT agent or the like.
[0043] <Latex> The latex according to the present embodiment is a latex containing a chloroprene-based block copolymer. The latex can be immersed in a coagulating liquid and molded to obtain a dip-molded product. The dip-molded product can be suitably used for gloves, balloons, catheters, boots, etc.
[0044] The latex of the present embodiment can be obtained by a method in which a liquid synthesized by emulsion polymerization at the end of polymerization is used as a latex as it is, as described in the above-mentioned method for producing a chloroprene-based block copolymer, or a method in which a recovered chloroprene-based block copolymer is forcibly emulsified using an emulsifier to obtain a latex, and the like. The method in which a liquid synthesized by emulsion polymerization at the end of polymerization is used as a latex as it is, as it is, is preferable because a latex can be obtained easily.
[0045] <Latex composition / rubber composition> The latex composition according to the present embodiment includes a chloroprene-based block copolymer. The rubber composition according to the present embodiment is a rubber composition including a chloroprene-based block copolymer. Raw materials other than the chloroprene-based block copolymer are not particularly limited and can be appropriately selected according to the purpose and application. Examples of raw materials that can be included in the latex composition / rubber composition including the chloroprene-based block copolymer include vulcanizing agents, vulcanization accelerators, fillers or reinforcing agents, plasticizers, processing aids and lubricants, antiaging agents, and silane coupling agents.
[0046] The latex composition / rubber composition of the present embodiment may contain a vulcanizing agent or a vulcanization accelerator. When the latex composition / rubber composition of the present embodiment contains a vulcanizing agent and / or a vulcanization accelerator, the total content of the vulcanizing agent and the vulcanization accelerator can be 5% by mass or less, more preferably 1% by mass or less, and more preferably 0.1% by mass, when the latex composition / rubber composition is taken as 100% by mass. However, the latex composition / rubber composition containing the chloroprene block copolymer of the present embodiment exhibits sufficient mechanical strength even without vulcanization. For this reason, it is preferable that the latex composition / rubber composition does not contain a vulcanizing agent or a vulcanization accelerator from the viewpoint of reducing allergies and reducing costs.
[0047] As the antiaging agent for improving heat resistance, a primary antiaging agent that traps radicals to prevent autoxidation and a secondary antiaging agent that renders hydroperoxide harmless, which are used in normal rubber applications, can be added. These antiaging agents can be added in a ratio of 0.1 to 10 parts by mass, preferably 2 to 5 parts by mass, per 100 parts by mass of the latex composition and the latex component in the rubber composition. These antiaging agents can be used alone or in combination of two or more kinds. Examples of the primary antiaging agent include phenol-based antiaging agents, amine-based antiaging agents, acrylate-based antiaging agents, imidazole-based antiaging agents, carbamic acid metal salts, and waxes. Examples of the secondary antiaging agent include phosphorus-based antiaging agents, sulfur-based antiaging agents, and imidazole-based antiaging agents. Examples of antioxidants include, but are not limited to, N-phenyl-1-naphthylamine, alkylated diphenylamines, octylated diphenylamines, 4,4'-bis(α,α-dimethylbenzyl)diphenylamine, p-(p-toluenesulfonylamido)diphenylamine, N,N'-di-2-naphthyl-p-phenylenediamine, N,N'-diphenyl-p-phenylenediamine, N-phenyl-N'-isopropyl-p-phenylenediamine, N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine, N-phenyl-N'-(3-methacryloyloxy-2-hydroxypropyl)-p-phenylenediamine, 1,1,3-tris-(2 -methyl-4-hydroxy-5-t-butylphenyl)butane, 4,4'-butylidenebis-(3-methyl-6-t-butylphenol), 2,2-thiobis(4-methyl-6-t-butylphenol), 7-octadecyl-3-(4'-hydroxy-3',5'-di-t-butylphenyl)propionate, tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane, pentaerythritol-tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], triethylene glycol-bis[3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate], 1,6-Hexanediol-bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 2,4-bis(n-octylthio)-6-(4-hydroxy-3,5-di-t-butylanilino)-1,3,5-triazine, tris-(3,5-di-t-butyl-4-hydroxybenzyl)-isocyanurate, 2,2-thio-diethylenebis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], N,N'-hexamethylenebis(3,5-di-t-butyl-4-hydroxy)-hydrocinnamate Amide, 2,4-bis[(octylthio)methyl]-o-cresol, 3,5-di-t-butyl-4-hydroxybenzyl-phosphonate-diethyl ester, tetrakis[methylene(3,5-di-t-butyl-4-hydroxyhydrocinnamate)]methane, octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate ester and 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxo Xaspiro[5.5]undecane, tris(nonylphenyl)phosphite, tris(mixed mono- and di-nonylphenyl)phosphite, diphenyl mono(2-ethylhexyl)phosphite, diphenyl monotridecyl phosphite, diphenyl isodecyl phosphite, diphenyl isooctyl phosphite, diphenyl nonylphenyl phosphite, triphenyl phosphite, tris(tridecyl)phosphite, triisodecyl phosphite, tris(2-ethylhexyl) Phosphite, tris(2,4-di-t-butylphenyl)phosphite, tetraphenyl dipropylene glycol diphosphite, tetraphenyl tetra(tridecyl)pentaerythritol tetraphosphite, 1,1,3-tris(2-methyl-4-di-tridecylphosphite-5-t-butylphenyl)butane, 4,4'-butylidenebis-(3-methyl-6-t-butyl-di-tridecylphosphite), 2,2'-ethylidenebis(4,6-di-t-butylphenol)fluorophosphite, 4,Examples of such phosphite include 4'-isopropylidene-diphenol alkyl (C12-C15) phosphite, cyclic neopentanetetrayl bis(2,4-di-t-butylphenyl phosphite), cyclic neopentanetetrayl bis(2,6-di-t-butyl-4-phenyl phosphite), cyclic neopentanetetrayl bis(nonylphenyl phosphite), bis(nonylphenyl) pentaerythritol diphosphite, dibutyl hydrogen phosphite, distearyl pentaerythritol diphosphite, hydrogenated bisphenol A pentaerythritol phosphite polymer, 2-mercaptobenzimidazole, and butylated reaction product of p-cresol and dicyclopentadiene.
[0048] The rubber composition can be produced in a conventional manner using known machines and devices. EXAMPLES
[0049] The present invention will be described below with reference to examples and comparative examples, but these are merely illustrative and do not limit the content of the present invention.
[0050] Example 1 (Polymerization step 1) Synthesis of polymer block (A-1) Polymerization was carried out using a 10L autoclave equipped with a stirrer and a jacket for heating and cooling. 5450g of pure water, 262g of potassium disproportionated rosinate (Harima Chemicals), 42.5g of potassium hydroxide, 21.8g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), 2500g of styrene monomer, and 43.3g of butylbenzyl trithiocarbonate were charged, and the internal temperature was set to 80°C and stirred at 200 rpm under a nitrogen stream. 27.3g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrogen chloride (Fujifilm Wako Pure Chemical Industries, product name: VA-044) was added as a polymerization initiator to start polymerization. 20ml of the obtained latex was sampled for physical property measurement, and the remaining latex was used in polymerization step 2.
[0051] The sampled latex was mixed with a large amount of methanol to precipitate the resin, which was then filtered and dried to obtain a sample of polymer block (A-1). The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A) were determined from the obtained sample. The analysis results are shown in Table 1. The methods for measuring the "number average molecular weight," "molecular weight distribution," and "glass transition temperature" will be described later.
[0052] (Polymerization step 2) Synthesis of chloroprene-based polymer block (B-1) Polymerization was carried out using a 10L autoclave equipped with a stirrer and a jacket for heating and cooling. 2732g of pure water, 131g of disproportionated potassium rosinate (Harima Chemicals), 21.3g of potassium hydroxide, 10.9g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), and 783g of latex containing the polymer block (A-1) produced in polymerization step 1 were charged, and the internal temperature was set to 45°C and stirred at 200 rpm under a nitrogen stream. Then, 3000g of chloroprene monomer was slowly added over 2 hours to carry out polymerization. When the polymerization rate of the chloroprene monomer reached 80%, a 10% by weight aqueous solution of N,N-diethylhydroxylamine, which is a polymerization terminator, was added to terminate the polymerization, and unreacted chloroprene monomer was removed by distillation under reduced pressure. 20ml of the obtained latex was sampled for physical property measurement, and the remaining latex was used to produce a film for evaluation.
[0053] The sampled latex was mixed with a large amount of methanol to precipitate the resin, which was then filtered and dried to obtain a chloroprene block copolymer sample. The obtained sample was analyzed to determine the contents (mass%) of the polymer block (A-1) and the chloroprene polymer block (B-1) of the chloroprene block copolymer. The analysis results are shown in Table 1. The measurement method will be described later. Furthermore, the toluene insoluble matter was determined from the sampled latex. The analysis results are shown in Table 1. The measurement method will be described later.
[0054] Example 2 (Polymerization step 1) Synthesis of polymer block (A-2) Polymerization was carried out in the same manner as in Example 1 to synthesize a polymer block (A-2). 20 ml of the obtained latex was sampled for measuring physical properties, and the remaining latex was used in polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-2) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0055] (Polymerization step 2) Synthesis of chloroprene-based polymer block (B-2) Polymerization was carried out using a 10L autoclave equipped with a stirrer and a jacket for heating and cooling. 2950g of pure water, 142g of disproportionated potassium rosinate (Harima Chemicals), 23g of potassium hydroxide, 11.8g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), and 448g of latex containing the polymer block (A-2) produced in polymerization step 1 were charged, and the internal temperature was set to 45°C and stirred at 200 rpm under a nitrogen stream. Then, 3000g of chloroprene monomer was slowly added over 2 hours to carry out polymerization. When the polymerization rate of the chloroprene monomer reached 80%, a 10% by weight aqueous solution of N,N-diethylhydroxylamine, which is a polymerization terminator, was added to terminate the polymerization, and unreacted chloroprene monomer was removed by distillation under reduced pressure. 20ml of the obtained latex was sampled for physical property measurement, and the remaining latex was used to produce a film for evaluation. The contents (mass %) of the polymer block (A-2) and the chloroprene polymer block (B-2) of the chloroprene block copolymer and the toluene insoluble matter were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0056] Example 3 (Polymerization step 1) Synthesis of polymer block (A-3) Polymerization was carried out in the same manner as in Example 1 to synthesize a polymer block (A-3). 20 ml of the obtained latex was sampled for measuring physical properties, and the remaining latex was used in polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-3) were determined by analysis in the same manner as in Example 1. The analytical results are shown in Table 1.
[0057] (Polymerization step 2) Synthesis of chloroprene-based polymer block (B-3) Polymerization was carried out using a 10L autoclave equipped with a stirrer and a jacket for heating and cooling. 2334g of pure water, 112g of disproportionated potassium rosinate (Harima Chemicals), 18.2g of potassium hydroxide, 9.3g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), and 1392g of latex containing the polymer block (A-3) produced in polymerization step 1 were charged, and the internal temperature was set to 45°C and stirred at 200 rpm under a nitrogen stream. Then, 3000g of chloroprene monomer was slowly added over 2 hours to carry out polymerization. When the polymerization rate of the chloroprene monomer reached 80%, a 10% by weight aqueous solution of N,N-diethylhydroxylamine, which is a polymerization terminator, was added to terminate the polymerization, and unreacted chloroprene monomer was removed by distillation under reduced pressure. 20ml of the obtained latex was sampled for physical property measurement, and the remaining latex was used to prepare a film for evaluation. The contents (mass %) of the polymer block (A-3) and the chloroprene polymer block (B-3) of the chloroprene block copolymer and the toluene insoluble matter were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0058] Example 4 (Polymerization step 1) Synthesis of polymer block (A-4) Polymerization was carried out using a 10L autoclave equipped with a stirrer and a jacket for heating and cooling. 5450g of pure water, 262g of potassium disproportionated rosinate (Harima Chemicals), 42.5g of potassium hydroxide, 21.8g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), 2500g of styrene monomer, and 32.5g of butylbenzyl trithiocarbonate were charged, and the internal temperature was set to 80°C and stirred at 200 rpm under a nitrogen stream. 20.5g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrogen chloride (Fujifilm Wako Pure Chemical Industries, product name: VA-044) was added as a polymerization initiator to start polymerization. 20ml of the obtained latex was sampled for physical property measurement, and the remaining latex was used in polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-4) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0059] (Polymerization step 2) Synthesis of chloroprene-based polymer block (B-4) Polymerization was carried out using a 10L autoclave equipped with a stirrer and a jacket for heating and cooling. 1188g of pure water, 57g of disproportionated potassium rosinate (Harima Chemicals), 9.3g of potassium hydroxide, 4.8g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, trade name: Demol N), and 3147g of latex containing the polymer block (A-4) produced in polymerization step 1 were charged, and the internal temperature was set to 45°C and stirred at 200 rpm under a nitrogen stream. Then, 3000g of chloroprene monomer was slowly added over 2 hours to carry out polymerization. When the polymerization rate of the chloroprene monomer reached 80%, a 10% by weight aqueous solution of N,N-diethylhydroxylamine, which is a polymerization terminator, was added to terminate the polymerization, and unreacted chloroprene monomer was removed by distillation under reduced pressure. 20ml of the obtained latex was sampled for physical property measurement, and the remaining latex was used to produce a film for evaluation. The contents (mass %) of the polymer block (A-4) and the chloroprene polymer block (B-4) of the chloroprene block copolymer and the toluene insoluble matter were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0060] Example 5 (Polymerization step 1) Synthesis of polymer block (A-5) Polymerization was carried out using a 10L autoclave equipped with a stirrer and a jacket for heating and cooling. 5450g of pure water, 262g of potassium disproportionated rosinate (Harima Chemicals), 42.5g of potassium hydroxide, 21.8g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), 2500g of methyl methacrylate monomer, and 29.6g of butyl-2-cyanoisopropyl trithiocarbonate were charged, and the internal temperature was set to 80°C and stirred at 200 rpm under a nitrogen stream. 20.5g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrogen chloride (Fujifilm Wako Pure Chemical Industries, product name: VA-044) was added as a polymerization initiator to start polymerization. 20ml of the obtained latex was sampled for physical property measurement, and the remaining latex was used in polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-5) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0061] (Polymerization step 2) Synthesis of chloroprene-based polymer block (B-5) Polymerization was carried out using a 10L autoclave equipped with a stirrer and a jacket for heating and cooling. 2732g of pure water, 131.14g of disproportionated potassium rosinate (Harima Chemicals), 21.3g of potassium hydroxide, 10.9g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), and 783g of latex containing the polymer block (A-5) produced in polymerization step 1 were charged, and the internal temperature was set to 45°C and stirred at 200 rpm under a nitrogen stream. Then, 3000g of chloroprene monomer was slowly added over 2 hours to carry out polymerization. When the polymerization rate of the chloroprene monomer reached 80%, a 10% by weight aqueous solution of N,N-diethylhydroxylamine, which is a polymerization terminator, was added to terminate the polymerization, and unreacted chloroprene monomer was removed by distillation under reduced pressure. 20ml of the obtained latex was sampled for physical property measurement, and the remaining latex was used to produce a film for evaluation. The contents (mass %) of the polymer block (A-5) and the chloroprene polymer block (B-5) of the chloroprene block copolymer and the toluene insoluble matter were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0062] Comparative Example 1 (Polymerization step 1) Synthesis of polymer block (A-6) Polymerization was carried out in the same manner as in Example 1 to synthesize a polymer block (A-6). 20 ml of the obtained latex was sampled for measuring physical properties, and the remaining latex was used in polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-6) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0063] (Polymerization step 2) Synthesis of chloroprene-based polymer block (B-6) Polymerization was carried out using a 10L autoclave equipped with a stirrer and a jacket for heating and cooling. 3036g of pure water, 146g of disproportionated potassium rosinate (Harima Chemicals), 23.7g of potassium hydroxide, 12.2g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, trade name: Demol N), and 316.5g of latex containing the polymer block (A-6) produced in polymerization step 1 were charged, and the internal temperature was set to 45°C and stirred at 200 rpm under a nitrogen stream. Then, 3000g of chloroprene monomer was slowly added over 2 hours to carry out polymerization. When the polymerization rate of the chloroprene monomer reached 80%, a 10% by weight aqueous solution of N,N-diethylhydroxylamine, which is a polymerization terminator, was added to terminate the polymerization, and unreacted chloroprene monomer was removed by distillation under reduced pressure. 20ml of the obtained latex was sampled for physical property measurement, and the remaining latex was used to produce a film for evaluation. The contents (mass %) of the polymer block (A-6) and the chloroprene polymer block (B-6) of the chloroprene block copolymer and the toluene insoluble matter were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0064] Comparative Example 2 (Polymerization step 1) Synthesis of polymer block (A-7) Polymerization was carried out using a 10L autoclave equipped with a stirrer and a jacket for heating and cooling. 5450g of pure water, 262g of potassium disproportionated rosinate (Harima Chemicals), 42.5g of potassium hydroxide, 21.8g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), 2500g of styrene monomer, and 21.4g of butylbenzyl trithiocarbonate were charged, and the internal temperature was set to 80°C and stirred at 200 rpm under a nitrogen stream. 13.5g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrogen chloride (Fujifilm Wako Pure Chemical Industries, product name: VA-044) was added as a polymerization initiator to start polymerization. 20ml of the obtained latex was sampled for physical property measurement, and the remaining latex was used in polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-7) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0065] (Polymerization step 2) Synthesis of chloroprene-based polymer block (B-7) Polymerization was carried out using a 10L autoclave equipped with a stirrer and a jacket for heating and cooling. 747g of pure water, 36g of disproportionated potassium rosinate (Harima Chemicals), 5.8g of potassium hydroxide, 3.0g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), and 3822.9g of latex containing the polymer block (A-7) produced in polymerization step 1 were charged, and the internal temperature was set to 45°C and stirred at 200 rpm under a nitrogen stream. Then, 3000g of chloroprene monomer was slowly added over 2 hours to carry out polymerization. When the polymerization rate of the chloroprene monomer reached 80%, the polymerization was stopped by adding a 10% by weight aqueous solution of N,N-diethylhydroxylamine, which is a polymerization terminator, and the unreacted chloroprene monomer was removed by distillation under reduced pressure. For physical property measurement, 20ml of the obtained latex was sampled, and the remaining latex was used to produce a film for evaluation. The contents (mass%) of the polymer block (A-7) and the chloroprene polymer block (B-7) of the chloroprene block copolymer and the toluene insoluble matter were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0066] Comparative Example 3 Synthesis of copolymers consisting only of chloroprene-based polymer blocks (B-8) Polymerization was carried out using a 10L autoclave equipped with a stirrer and a jacket for heating and cooling. 3600g of pure water, 175g of potassium disproportionated rosinate (Harima Chemicals), 28.4g of potassium hydroxide, 16.0g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), 4000g of chloroprene monomer, and 4.72g of butylbenzyl trithiocarbonate were charged, and the internal temperature was set to 45°C and stirred at 200 rpm under a nitrogen stream. 2.96g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrogen chloride (Fujifilm Wako Pure Chemical Industries, product name: VA-044) was added as a polymerization initiator to start polymerization. When the polymerization rate of the chloroprene monomer reached 80%, a 10% by weight aqueous solution of N,N-diethylhydroxylamine, which is a polymerization terminator, was added to terminate the polymerization, and the unreacted chloroprene monomer was removed by distillation under reduced pressure. For the measurement of physical properties, 20 ml of the obtained latex was sampled, and the remaining latex was used to prepare a film for evaluation. The toluene insoluble content was determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0067] Comparative Example 4 (Polymerization step 1) Synthesis of polymer block (A-9) Polymerization was carried out using a 10L autoclave equipped with a stirrer and a jacket for heating and cooling. 4616g of pure water, 206g of potassium disproportionated rosinate (Harima Chemicals), 2.3g of potassium hydroxide, 46.2g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), 462g of styrene monomer, and 9.2g of butylbenzyl trithiocarbonate were charged, and the internal temperature was set to 80°C and stirred at 200 rpm under a nitrogen stream. 6.0g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrogen chloride (Fujifilm Wako Pure Chemical Industries, product name: VA-044) was added as a polymerization initiator to start polymerization. 20ml of the obtained latex was sampled for physical property measurement, and the remaining latex was used in polymerization step 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-9) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0068] (Polymerization step 2) Synthesis of chloroprene-based polymer block (B-9) After the polymerization step 1, when the internal temperature dropped to 45°C, 4154g of chloroprene monomer was slowly added over 2 hours to carry out polymerization. When the polymerization rate of the chloroprene monomer reached 80%, a 10% by weight aqueous solution of N,N-diethylhydroxylamine, which is a polymerization terminator, was added to terminate the polymerization, and the unreacted chloroprene monomer was removed by distillation under reduced pressure. For physical property measurement, 20ml of the obtained latex was sampled, and the remaining latex was used to prepare a film for evaluation. The contents (mass%) of the polymer block (A-9) and the chloroprene polymer block (B-9) of the chloroprene block copolymer and the toluene insoluble content were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0069] Comparative Example 5 (Polymerization step 1) Synthesis of polymer block (A-10) Polymerization was carried out using a 10L autoclave equipped with a stirrer and a jacket for heating and cooling. 4616g of pure water, 206g of potassium disproportionated rosinate (Harima Chemicals), 2.3g of potassium hydroxide, 46.2g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), 692g of styrene monomer, and 9.2g of butylbenzyl trithiocarbonate were charged, and the internal temperature was set to 80°C and stirred at 200 rpm under a nitrogen stream. 6.0g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrogen chloride (Fujifilm Wako Pure Chemical Industries, product name: VA-044) was added as a polymerization initiator to start polymerization. 20ml of the obtained latex was sampled for physical property measurement, and the remaining latex was used in polymerization process 2. The number average molecular weight, molecular weight distribution, and glass transition temperature of the polymer block (A-10) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0070] (Polymerization step 2) Synthesis of chloroprene-based polymer block (B-10) After the polymerization step 1, when the internal temperature dropped to 45°C, 3924g of chloroprene monomer was slowly added over 2 hours to carry out polymerization. When the polymerization rate of the chloroprene monomer reached 80%, a 10% by weight aqueous solution of N,N-diethylhydroxylamine, which is a polymerization terminator, was added to terminate the polymerization, and the unreacted chloroprene monomer was removed by distillation under reduced pressure. For physical property measurement, 20ml of the obtained latex was sampled, and the remaining latex was used to prepare a film for evaluation. The contents (mass%) of the polymer block (A-10) and the chloroprene polymer block (B-10) of the chloroprene block copolymer and the toluene insoluble content were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 1.
[0071] Comparative Example 6 Synthesis of triblock copolymers (Synthesis of the first block) Polymerization was carried out using a 10L autoclave equipped with a stirrer and a jacket for heating and cooling. 4613g of pure water, 204.4g of potassium disproportionated rosinate (Harima Chemicals), 2.3g of potassium hydroxide, 46.1g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), 230g of styrene monomer, and 9.2g of benzyl 1-pyrrole carbodithioate were charged, and the internal temperature was set to 80°C and stirred at 200 rpm under a nitrogen stream. 6.0g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrogen chloride (Fujifilm Wako Pure Chemical Industries, product name: VA-044) was added as a polymerization initiator to start polymerization. 20ml of the obtained latex was sampled for physical property measurement, and the remaining latex was used in the next polymerization step. The number average molecular weight, molecular weight distribution, and glass transition temperature of the first block were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 2. (Synthesis of the second block) After the synthesis of the first block, when the internal temperature dropped to 45°C, 4424 g of chloroprene monomer was added and polymerization was carried out. When the polymerization rate of the chloroprene monomer reached 80%, a 10 wt% aqueous solution of N,N-diethylhydroxylamine, a polymerization terminator, was added to terminate the polymerization, and the unreacted chloroprene monomer was removed by vacuum distillation. The obtained latex was used in the next polymerization step. (Synthesis of the third block) After the synthesis of the second block, the internal temperature was raised to 80°C, 230g of styrene monomer was charged, and 6.0g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrogen chloride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., product name: VA-044) was added as a polymerization initiator to start polymerization. After polymerization, the polymerization was stopped by cooling to 25°C. For physical property measurement, 20ml of the obtained latex was sampled, and a film for evaluation was produced using the remaining latex. The content (mass%) of the styrene block, which is the first block and the third block of the synthesized triblock copolymer, and the chloroprene block, which is the second block, and the toluene insoluble content were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 2.
[0072] Comparative Example 7 Preparation of a mixture of homopolymers of polymer block (A) and homopolymers of chloroprene-based polymer block (B) (Synthesis of homopolymer of polymer block (A)) Polymerization was carried out using a 10L autoclave equipped with a stirrer and a jacket for heating and cooling. 4666g of pure water, 224g of disproportionated potassium rosinate (Harima Chemicals), 36.4g of potassium hydroxide, 18.7g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), 350g of styrene monomer, and 6.07g of butylbenzyl trithiocarbonate were charged, and the internal temperature was set to 80°C and stirred at 200 rpm under a nitrogen stream. Polymerization was started by adding 3.82g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane]2hydrogen chloride (Fujifilm Wako Pure Chemical Industries, product name: VA-044) as a polymerization initiator. When the polymerization rate of the styrene monomer reached 95%, the polymerization was stopped by adding a 10% by weight aqueous solution of N,N-diethylhydroxylamine as a polymerization terminator. 20 ml of the obtained latex was sampled for measuring physical properties. The number average molecular weight, molecular weight distribution and glass transition temperature of the homopolymer of the polymer block (A) were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 3.
[0073] (Synthesis of homopolymer of chloroprene polymer block (B)) Polymerization was carried out using a 10L autoclave equipped with a stirrer and a jacket for heating and cooling. 3960g of pure water, 193g of disproportionated potassium rosinate (Harima Chemicals), 31.2g of potassium hydroxide, 17.6g of sodium salt of β-naphthalenesulfonic acid formalin condensate (Kao Corporation, product name: Demol N), 4400g of chloroprene monomer, 89.8g of 1.9-nonanediol dimethacrylate, and 5.19g of butylbenzyl trithiocarbonate were charged, and the internal temperature was set to 45°C and stirred at 200 rpm under a nitrogen stream. 3.26g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrogen chloride (Fujifilm Wako Pure Chemical Industries, product name: VA-044) was added as a polymerization initiator to start polymerization. When the polymerization rate of the chloroprene monomer reached 80%, the polymerization was terminated by adding a 10% by weight aqueous solution of N,N-diethylhydroxylamine, which serves as a polymerization terminator, and the unreacted chloroprene monomer was removed by reduced pressure distillation.
[0074] (Mixing of homopolymer latex of polymer block (A) and homopolymer latex of chloroprene-based polymer block (B)) 4000 g of the obtained homopolymer latex of the polymer block (A) and 4000 g of the homopolymer latex of the chloroprene polymer block (B) were charged into a 10 L capacity autoclave equipped with a stirrer and a jacket for heating and cooling, and the inside temperature was set to 45° C. and stirred at 200 rpm. For physical property measurement, 20 ml of the obtained latex was sampled, and the remaining latex was used to prepare a film for evaluation. The contents (mass%) of the homopolymer of the polymer block (A) and the homopolymer of the chloroprene polymer block (B) in the polymer obtained by mixing and the toluene insoluble content were determined by analysis in the same manner as in Example 1. The analysis results are shown in Table 3.
[0075] [analysis] (Measurement of number average molecular weight and molecular weight distribution of polymer block (A)) The number average molecular weight and molecular weight distribution are values calculated as polystyrene by gel permeation chromatography (GPC) and are values measured under the measurement conditions described below. Device name: HLC-8320 (Tosoh Corporation) Column: 3 TSKgel GMHHR-H in series Temperature: 40℃ Detection: Differential refractive index Solvent: Tetrahydrofuran Calibration curve: Prepared using standard polystyrene (PS).
[0076] (Glass transition temperature of polymer block (A)) The glass transition temperature was measured using a differential scanning calorimeter in accordance with JIS K 7121 by the following method. Device name: DSC1 (Mettler Toledo) Procedure: Under a nitrogen flow of 50 ml / min, the sample was heated to 120°C at a rate of 10°C / min, kept at 120°C for 10 minutes, then cooled to -60°C. The sample was then heated to 120°C at a rate of 10°C / min to obtain a DSC curve. The glass transition temperature was determined as the temperature at the intersection of a straight line extending the base line on the high temperature side to the low temperature side and a tangent line drawn at the point where the slope of the curve on the high temperature side of the peak is maximum.
[0077] (Measurement of the content of polymer block (A) and chloroprene polymer block (B) in chloroprene block copolymer) The measurements were carried out using pyrolysis gas chromatogram and 1H-NMR as follows. Pyrolysis gas chromatogram Instrument name: HP5890-II Column: DB-5 0.25 mm diameter x 30 m (film thickness 1.0 μm) Column temperature: 50℃(5min)→10℃ / min→150℃→25℃ / min→300℃ Inlet temperature: 250℃ Detector temperature: 280℃ Detector: FID 1H-NMR Equipment name: JNM-ECX-400 (manufactured by JEOL Ltd.) Procedure: A chloroprene-based block copolymer consisting of a polymer block (A) and a chloroprene-based polymer block (B) was measured by pyrolysis gas chromatography, and a calibration curve was prepared from the area ratio of the peak derived from the polymer block (A) to the peak derived from the chloroprene-based polymer block (B) and the contents of the polymer block (A) and the chloroprene-based polymer block (B) in the chloroprene-based block copolymer obtained by measuring 1H-NMR. A sample of the chloroprene-based block copolymer precipitated by mixing the sampled latex with methanol was measured by pyrolysis gas chromatography, and the contents of the polymer block (A) and the chloroprene-based polymer block (B) in the chloroprene-based block copolymer were calculated from the area ratio of the peak derived from the polymer block (A) to the peak derived from the chloroprene-based polymer block (B) using the calibration curve prepared above.
[0078] [Preparation of samples for tensile tests] (Preparation of latex containing chloroprene-based block copolymer) To 100 parts by mass (solid content equivalent) of the chloroprene block copolymer in the latex obtained in polymerization step 2, 2 parts by mass of a butylated reaction product of p-cresol and dicyclopentadiene (trade name "Nocrac PBK", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) as an antiaging agent, 0.3 parts by mass of sodium lauryl sulfate (trade name "EMAL 10", manufactured by Kao Corporation), and water were added to adjust the solid content concentration of the blend to 30% by mass, and the mixture was mixed at 20°C for 16 hours using a ceramic ball mill to prepare the blend. (Film Creation) A ceramic cylinder with an outer diameter of 50 mm was immersed for 1 second in a coagulation liquid containing 62 parts by mass of water, 35 parts by mass of potassium nitrate tetrahydrate, and 3 parts by mass of calcium carbonate, and then removed. After drying for 4 minutes, the cylinder was immersed for 2 minutes in the latex prepared above. The cylinder was then washed with running water at 45°C for 1 minute, and heated at 130°C for 30 minutes to remove moisture, producing a film (140 x 150 mm, thickness: 0.2 mm) for tensile testing.
[0079] [Evaluation of tensile properties] The prepared film was heat-treated at 130°C for 30 minutes, and then the modulus at 500% elongation, tensile strength at break, and elongation at break were measured in accordance with JIS K 6251. A modulus at 500% elongation of 3.0 MPa or less, a tensile strength at break of 17 MPa or more, and an elongation at break of 900% or more were considered to be acceptable.
[0080] [Measurement of toluene insolubles] The latex obtained in the polymerization step 2 was freeze-dried, and 1 g of the solid was cut into 2 mm squares, placed in a conical beaker, and dissolved in toluene for 16 hours. After that, the mixture was centrifuged, and the gel fraction was separated using a 200 mesh wire screen. The dried weight was measured, and the toluene insoluble fraction was calculated using the following formula. (Weight of solid obtained by separating and drying gel fraction) / (Weight of solid obtained by freeze-drying latex containing chloroprene-based block copolymer)×100
[0081] [Table 1]
[0082] [Table 2]
[0083] [Table 3]
[0084] In Examples 1 to 5, even without using a vulcanizing agent or vulcanization accelerator, the modulus at 500% elongation was 3.0 MPa or less, which was excellent in flexibility, the tensile strength at break was 17 MPa or more, and the elongation at break was 900% or more, which was excellent in tensile properties. On the other hand, in Comparative Examples 1 to 7, either the flexibility or the tensile properties were poor.
Claims
1. a chloroprene-based block copolymer comprising 5 to 15 mass% of a polymer block (A) derived from a monomer which, upon homopolymerization, gives a polymer having a glass transition temperature of 80° C. or higher, and 85 to 95 mass% of a chloroprene-based polymer block (B) containing a structural unit derived from a chloroprene monomer, the chloroprene-based polymer block (B) contains 90 mass% or more of a structural unit derived from a chloroprene monomer, when the chloroprene-based polymer block (B) is taken as 100 mass%, The chloroprene block copolymer has a toluene insoluble content of 20 to 100% by mass relative to 100% by mass of the chloroprene block copolymer.
2. 2. The chloroprene block copolymer according to claim 1, wherein a molded product of a latex composition containing the chloroprene block copolymer has a tensile strength at break of 17 MPa or more as measured in accordance with JIS K 6251 after heat-treating the molded product at 130°C for 30 minutes.
3. The chloroprene block copolymer according to claim 1 or 2, wherein the polymer block (A) has a number average molecular weight of 10,000 or more.
4. The chloroprene block copolymer according to any one of claims 1 to 3, wherein the molecular weight distribution of the polymer block (A) is 2.0 or less.
5. 5. The chloroprene block copolymer according to claim 1, wherein the polymer block (A) is a polymer block comprising an aromatic vinyl monomer unit.
6. The chloroprene block copolymer according to any one of claims 1 to 5, having a functional group having a structure represented by chemical formula (1) or chemical formula (2). 【Chemistry 1】 (In chemical formula (1), R 1 represents hydrogen, chlorine, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkenyl group, a substituted or unsubstituted aryl group, or a substituted or unsubstituted heterocyclyl group. 【Chemistry 2】
7. A latex comprising the chloroprene block copolymer according to any one of claims 1 to 6.
8. A latex composition comprising 100 parts by mass of the latex according to claim 7 and 0.5 to 5.0 parts by mass of an antioxidant.
9. 9. The latex composition according to claim 8, which is free of vulcanizing agents and vulcanization accelerators.
10. A rubber composition comprising the chloroprene block copolymer according to any one of claims 1 to 6.
11. A rubber composition comprising the latex of claim 7.
12. A rubber composition comprising the latex composition according to claim 8 or 9.
Citation Information
Patent Citations
Copolymer and production thereof
JP1991207710A
Chloroprene block copolymer
JP1991212414A
Elastomer composition containing block copolymer, and molded form therefrom
JP2003292719A
Soapless polychloroprene-based latex and method for producing the same
JP2007297502A
Polychloroprene latex and method of manufacturing the same
JP2010001458A
Cited By
Diene-based block copolymer, diene-based block copolymer latex, diene-based copolymer latex composition, and molded body
JP2022147759A