Piezoelectric laminate and piezoelectric element
The piezoelectric laminate with an inclined (111) plane lower electrode layer and controlled composition suppresses the pyrochlore phase, enhancing piezoelectric properties and reducing manufacturing costs.
Patent Information
- Application Number
- JP2022553466
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-09-30
- Filing Date
- 2021-06-11
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-06-11
AI Technical Summary
Existing methods to suppress the pyrochlore phase in piezoelectric films, such as using a seed layer, increase manufacturing costs and reduce the net electric field, thereby deteriorating piezoelectric properties.
A piezoelectric laminate structure with a lower electrode layer having a metal layer with a (111) plane inclined at 1° or more relative to the substrate, and a piezoelectric film composed of perovskite oxide, where the lower electrode layer includes a first layer of Ir, Pt, Au, Mo, Ta, or Al, and a second layer containing Ti and W with controlled oxygen or nitrogen content, reducing the pyrochlore phase to 2% or less.
The solution achieves high piezoelectric properties at lower costs by suppressing the pyrochlore phase, improving adhesion and durability, and maintaining effective electric fields.
Smart Images

Figure 0007575472000002 
Figure 0007575472000003 
Figure 0007575472000004
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a piezoelectric laminate and a piezoelectric element. [Background technology]
[0002] Lead zirconate titanate (Pb(Zr,Ti)O) is a material with excellent piezoelectric and ferroelectric properties. 3 PZT is known as a piezoelectric material, hereafter referred to as PZT. Taking advantage of its ferroelectricity, PZT is used in FeRAM (Ferroelectric Random Access Memory), a non-volatile memory. Furthermore, in recent years, by combining with MEMS (Micro Electro-Mechanical Systems) technology, MEMS piezoelectric elements with PZT films are being put to practical use. PZT films are used as the piezoelectric films in piezoelectric elements that have a lower electrode, a piezoelectric film, and an upper electrode on a substrate. These piezoelectric elements are being deployed in a variety of devices, such as inkjet heads (actuators), micromirror devices, angular velocity sensors, gyro sensors, and vibration power generation devices.
[0003] In piezoelectric films containing lead-containing perovskite oxides, such as PZT, the pyrochlore phase, an impurity layer, is easily generated at the interface with the lower electrode layer when the piezoelectric film is formed on the lower electrode layer. Since the pyrochlore phase is a paraelectric, the formation of the pyrochlore phase leads to a deterioration in the dielectric constant and piezoelectric properties of the piezoelectric film. When the piezoelectric film is used as a piezoelectric device, the higher the piezoelectric properties of the piezoelectric film, the better the device performance, and a decrease in the piezoelectric properties leads to a decrease in device performance, so it is desirable for the piezoelectric properties to be high. For this reason, methods are being investigated to suppress the pyrochlore phase and improve the piezoelectric properties.
[0004] For example, Japanese Patent Application Laid-Open No. 11-233733 proposes providing a seed layer between the piezoelectric film and the lower electrode layer to suppress the growth of the pyrochlore phase. Summary of the Invention [Problem to be solved by the invention]
[0005] However, as in JP-A-11-233733, forming a seed layer has the disadvantage of increasing the number of processes for forming the piezoelectric element and increasing the manufacturing cost. In addition, if the seed layer is made of an insulating material or if the seed layer is thick, the net electric field applied to the piezoelectric film among the electric fields applied between the upper and lower electrode layers decreases, which is a disadvantage in that the piezoelectric characteristics of the piezoelectric element decrease.
[0006] The technique disclosed herein has been made in consideration of the above circumstances, and has an object to provide a piezoelectric laminate and a piezoelectric element having excellent piezoelectric characteristics at low cost. [Means for solving the problem]
[0007] Specific means for solving the above problems include the following aspects. <1> A piezoelectric laminate including a lower electrode layer and a piezoelectric film in this order on a substrate, a region of the lower electrode layer in contact with the piezoelectric film is made of a metal layer, and a (111) surface of the metal layer is inclined at an angle of 1° or more with respect to the surface of the substrate; A piezoelectric laminate, the piezoelectric film comprising a perovskite oxide containing Pb. <2> The metal constituting the metal layer is at least one of Ir, Pt, Au, Mo, Ta, and Al; <1> The piezoelectric laminate according to claim 1. <3> the lower electrode layer includes a first layer made of a metal layer and a second layer adjacent to the first layer and provided on the substrate side; The second layer is mainly composed of at least one of Ti and W, and contains more than 5 at % and less than 50 at % of oxygen or nitrogen. <1> or <2> The piezoelectric laminate according to claim 1. <4> In the X-ray diffraction pattern of the piezoelectric film, the intensity ratio of the pyrochlore phase to the perovskite phase in the piezoelectric film, as represented by the following formula, is 2% or less. <1> from <3> 2. The piezoelectric laminate according to claim 1 . py(222) / {pr(100)+pr(110)+pr(111)}×100% py(222) is the peak intensity of the (222) plane of the pyrochlore phase pr(100) is the peak intensity of the (100) plane of the perovskite phase pr(110) is the peak intensity of the (110) plane of the perovskite phase pr(111) is the peak intensity of the (111) plane of the perovskite phase It is. <5> The piezoelectric film has a columnar crystal film structure composed of a large number of columnar crystals. <1> from <4> 2. The piezoelectric laminate according to claim 1 . <6> The (100) or (001) plane of the columnar crystal has an inclination of 1° or more with respect to the surface of the substrate. <5> The piezoelectric laminate according to claim 1. <7> <1> from <6> and a piezoelectric laminate according to any one of the above. and an upper electrode layer provided on the piezoelectric film of the piezoelectric laminate. <8> The upper electrode layer comprises a metal or metal oxide including at least one of Ir, Pt, Au, Ti, Mo, Ta, Ru, and Al; <7> The piezoelectric element according to claim 1 . Effect of the Invention
[0008] The piezoelectric laminate and piezoelectric element of the present disclosure have high piezoelectric properties and can be manufactured at low cost. [Brief description of the drawings]
[0009] [Figure 1] 1 is a cross-sectional view showing a layer structure of a piezoelectric element according to an embodiment of the present invention. [Diagram 2] FIG. 2 is an explanatory diagram of a metal constituting a first layer of the lower electrode layer. [Diagram 3] 4 is an explanatory diagram of the alignment state of the first layer of the lower electrode layer in the present embodiment. FIG. [Figure 4] FIG. 2 is an enlarged schematic view of a piezoelectric film. [Diagram 5]13 is SIMS data showing the oxygen content in the second layer of the lower electrode layer. [Figure 6] This is rocking curve measurement data showing the inclination of the Ir(111) surface. [Figure 7] 4 is an XRD chart showing the crystallinity of the piezoelectric film of Comparative Example 1. [Figure 8] 4 is an XRD chart showing the crystallinity of the piezoelectric film of Example 1. [Figure 9] 11 is an XRD chart showing the crystallinity of the piezoelectric film of Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In the drawings, the thicknesses and ratios of each layer are appropriately changed for ease of viewing, and do not necessarily reflect the actual thicknesses and ratios.
[0011] "Piezoelectric element of one embodiment" Fig. 1 is a cross-sectional schematic diagram showing a layer structure of a piezoelectric element 1 including a piezoelectric laminate 5 according to an embodiment. As shown in Fig. 1, the piezoelectric element 1 includes a piezoelectric laminate 5 and an upper electrode layer 18. The piezoelectric laminate 5 includes a substrate 11, and a lower electrode layer 12 and a piezoelectric film 15 laminated on the substrate 11. That is, the piezoelectric element 1 is configured such that the upper electrode layer 18 is formed on the piezoelectric film 15 of the piezoelectric laminate 5. Here, "lower" and "upper" do not mean up and down in the vertical direction, but simply refer to the electrode disposed on the substrate 11 side across the piezoelectric film 15 as the lower electrode layer 12, and the electrode disposed on the opposite side of the piezoelectric film 15 to the substrate 11 as the upper electrode layer 18.
[0012] The substrate 11 is not particularly limited, and examples thereof include substrates of silicon, glass, stainless steel, yttrium-stabilized zirconia, alumina, sapphire, silicon carbide, etc. The substrate 11 is a silicon substrate having a SiO 2 A laminated substrate on which an oxide film is formed may also be used.
[0013] The piezoelectric film 15 includes a perovskite oxide containing Pb. The piezoelectric film 15 is basically made of a perovskite oxide containing Pb. However, the piezoelectric film 15 may contain unavoidable impurities in addition to the perovskite oxide containing Pb. The perovskite oxide is generally made of ABO 3 It is expressed by the formula: The standard ratio of A:B:O is 1:1:3, but it may deviate from the standard value as long as the perovskite structure can be obtained. Pb is an A-site element, and is preferably contained as the main component of the A-site. In this specification, the term "main component" means a component that occupies 50 mol% or more. In other words, "containing Pb as the main component of the A-site" means that 50 mol% or more of the A-site elements are Pb. In the perovskite oxide containing Pb, the other elements in the A-site other than Pb and the elements in the B-site are not particularly limited.
[0014] As the Pb-containing perovskite oxide constituting the piezoelectric film 15, for example, a perovskite oxide represented by the following general formula (1) is preferable. (Pb a1 α a2 )(Zr b1 Ti b2 β b3 )O c (1) In the formula, Pb and α are A-site elements, and α is at least one element other than Pb. Zr, Ti, and β are B-site elements. a1≧0.5, b1>0, b2>0, b3≧0, and (a1+a2):(b1+b2+b3):c=1:1:3 is the standard, but may deviate from the standard value within the range in which the perovskite structure can be obtained.
[0015] In the perovskite oxide containing Pb, the A-site elements other than Pb include lithium (Li), sodium (Na), potassium (K), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), lanthanum (La), cadmium (Cd), and bismuth (Bi). α is one or a combination of two or more of these.
[0016] In addition, examples of B-site elements other than Ti and Zr include scandium (Sc), vanadium (V), niobium (Nb), tantalum (Ta), chromium (Cr), molybdenum (Mo), tungsten (W), manganese (Mn), iron (Fe), ruthenium (Ru), cobalt (Co), iridium (Ir), nickel (Ni), copper (Cu), zinc (Zn), gallium (Ga), indium (In), tin (Sn), antimony (Sb), and lanthanide elements. β is one or a combination of two or more of these.
[0017] The thickness of the piezoelectric film 15 is not particularly limited and is usually 200 nm or more, for example, 0.2 μm to 5 μm. The thickness of the piezoelectric film 15 is preferably 1 μm or more.
[0018] The lower electrode layer 12 is an electrode for applying a voltage to the piezoelectric film 15. At least the region of the lower electrode layer 12 that is in contact with the piezoelectric film 15 is made of a metal layer, and the (111) plane of the metal layer is inclined by 1° or more with respect to the surface of the substrate 11. The metal layer contains a metal that becomes an oriented film with a (111) plane parallel to the surface of the glass substrate when the metal layer is formed on the glass substrate by sputtering, that is, a metal that is preferentially oriented in the (111) plane. In this example, the lower electrode layer 12 includes a first layer 21 that is in contact with the piezoelectric film 15, and a second layer 22 that is adjacent to the first layer 21 and disposed on the substrate 11 side. The first layer 21, which is the region in contact with the piezoelectric film 15, is made of a metal layer that contains a metal that is preferentially oriented in the (111) plane when the metal layer is formed on the glass substrate by sputtering. In this specification, the "metal layer" may have an oxide region (oxide film) formed by natural oxidation on the surface. In this first layer 21, the (111) plane of the metal layer has an inclination of 1° or more with respect to the surface 11a (hereinafter referred to as the substrate surface 11a) of the substrate 11. The (111) plane has an inclination of preferably 1° to 15°, more preferably 1° to 8°, with respect to the substrate surface 11a.
[0019] FIG. 2 is a diagram showing a schematic view of the orientation of a layer made of the metal forming the first layer 21 when it is formed on the glass substrate 20 by sputtering. Particles 21b in FIG. 2 indicate metal elements. The metal used here is oriented so that the growth plane parallel to the surface 20a of the glass substrate 20 becomes the (111) plane when it is formed on the glass substrate 20 by sputtering. That is, the (111) plane is oriented so as to be parallel to the surface 20a of the substrate 20. However, in this example, as shown in FIG. 3, the (111) plane of the first layer 21 has an inclination α of 1° or more with respect to the substrate surface 11a.
[0020] The inclination α of the (111) plane in the first layer 21 is defined as a value measured by rocking curve measurement using X-ray diffraction. Specifically, the inclination of the (111) plane is calculated from the split width of the (111) diffraction peak in the rocking curve measurement data (see Examples).
[0021] When the (111) plane is preferentially oriented on the surface of the lower electrode layer 12 on which the piezoelectric film 15 is formed, the pyrochlore phase is likely to be formed during the formation of the piezoelectric film 15 containing a perovskite oxide containing Pb. However, in the lower electrode layer 12 of this embodiment, as shown in FIG. 3, the (111) plane of the metal layer constituting the first layer 21 of the lower electrode layer 12 has an inclination α of 1° or more with respect to the deposition surface parallel to the substrate surface 11a. Therefore, the generation of the pyrochlore phase is suppressed, and a piezoelectric film 15 with a reduced pyrochlore phase can be formed compared to when the surface of the lower electrode layer 12 is a (111) plane. If the generation of the pyrochlore phase in the piezoelectric film 15 is suppressed, the ratio of the perovskite phase in the piezoelectric film 15 increases, and the piezoelectric laminate 5 and the piezoelectric element 1 can be obtained with high piezoelectric properties. In addition, compared to the case where a seed layer for suppressing the pyrochlore phase is provided on the lower electrode layer, a seed layer formation process is not required, so that an increase in cost is suppressed and the piezoelectric laminate 5 and the piezoelectric element 1 can be obtained at low cost.
[0022] Moreover, by suppressing the occurrence of the pyrochlore phase at the interface between the piezoelectric film 15 and the lower electrode layer 12, it is possible to expect the effects of improving adhesion, suppressing electrical failures, and improving long-term durability.
[0023] It is preferable that the inclination α of the (111) plane in the first layer 21 relative to the substrate surface 11a is greater, since this has a greater effect in suppressing the growth of the pyrochlore phase. On the other hand, by setting the inclination to 15° or less, it is possible to suppress the dominance of other oriented planes, which is also preferable.
[0024] In the lower electrode layer 12, the metal constituting the first layer 21 is preferably at least one of iridium (Ir), platinum (Pt), gold (Au), molybdenum (Mo), tantalum (Ta), and aluminum (Al). Ir or Pt is more preferable, and Ir is particularly preferable.
[0025] The second layer 22 of the lower electrode layer 12 contains at least one of Ti and W as a main component, and oxygen or nitrogen in an amount of more than 5 at% and less than 50 at%. When the second layer 22 contains both oxygen and nitrogen, the total content of both may be more than 5 at% and less than 50 at%. As described above, when the metal constituting the first layer 21 is formed by sputtering, the (111) plane is usually parallel to the substrate surface 11a. However, by providing the above-mentioned second layer below the first layer 21, the (111) plane can be oriented so as to have an inclination with respect to the substrate surface 11a.
[0026] The method of forming a metal film whose (111) plane is inclined from the deposition surface in the region of lower electrode layer 12 adjacent to piezoelectric film 15 is not limited to the method including second layer 22 described above.
[0027] The second layer is preferably Ti or TiW, and when it is TiW, a ratio of Ti:W of 10 wt%:90 wt% is particularly preferred.
[0028] The amount of impurities such as oxygen and nitrogen added to the second layer 22 can be controlled by the conditions during sputtering. The sputtering is performed in a vacuum chamber, and some oxygen and the like remain in the vacuum chamber as background. The amount of impurities taken into the film from the background can be adjusted by adjusting the distance between the substrate and the target during sputtering and the film formation rate. By increasing the distance between the substrate and the target or slowing down the film formation rate, the gas species used for sputtering, such as oxygen and argon, can be taken into the film. Also, by introducing oxygen or nitrogen gas into the sputtering gas flowed during film formation, more oxygen or nitrogen can be taken into the film. The higher the oxygen and nitrogen content in the second layer 22, the lower the crystallinity of the second layer 22. By lowering the crystallinity of the second layer 22, the (111) plane of the metal layer, which is the first layer 21 to be formed on the second layer 22, has an inclination with respect to the substrate surface 11a. If the oxygen or nitrogen content in the second layer 22 is more than 5 at %, the inclination of the (111) plane of the metal layer can be made sufficiently large. If the content of oxygen or nitrogen in the second layer 22 is less than 50%, good adhesion to the substrate 11 can be maintained.
[0029] The total thickness of the lower electrode layer 12 including the first layer 21 and the second layer 22 is not particularly limited as long as the conductivity required for the device is ensured as the lower electrode layer 12. For example, it may be about 50 nm to 300 nm, or may be 100 nm to 300 nm. In this embodiment, the lower electrode layer 12 has a two-layer structure, but as long as the metal layer constituting at least the region in contact with the piezoelectric film 15 is an alignment film and its (111) plane is inclined from the substrate surface 11a, the lower electrode layer 12 may be a single layer or a laminated structure of three or more layers.
[0030] The upper electrode layer 18 is an electrode that pairs with the lower electrode layer 12 and applies a voltage to the piezoelectric film 15. There are no particular limitations on the main component of the upper electrode layer 18, and examples thereof include the materials exemplified for the lower electrode layer 12, as well as electrode materials that are generally used in semiconductor processes, such as chromium (Cr), and combinations thereof. The upper electrode layer 18 preferably contains a metal or metal oxide that contains at least one of Ir, Pt, Au, Ti, Mo, Ta, Ru, and Al.
[0031] The thickness of the upper electrode layer 18 is not particularly limited, but is preferably about 50 nm to 300 nm, and more preferably 100 nm to 300 nm.
[0032] As described above, in the piezoelectric stack 5 and piezoelectric element 1 of this embodiment, the region of the lower electrode layer 12 that contacts the piezoelectric film 15 (first layer 21 in this example) is made of a metal layer that contains a metal that becomes an oriented film with a (111) plane parallel to the surface of the glass substrate when formed on a glass substrate by sputtering, and the (111) plane of the metal layer is inclined by 1° or more with respect to the surface of the substrate. This makes it possible to suppress the formation of a pyrochlore phase between the piezoelectric film 15 and the lower electrode layer 12.
[0033] 4 is a diagram showing the interface between the piezoelectric film 15 and the lower electrode layer 12, and the piezoelectric film 15. As shown in FIG. 4, a pyrochlore phase 16 that grows in a triangular shape in cross section is formed at the interface between the piezoelectric film 15 and the lower electrode layer 12, while the other regions are composed of perovskite oxides. When the piezoelectric film 15 is formed on a metal layer having a (111) plane parallel to the substrate surface 11a, a pyrochlore phase having a thickness of several hundred nm is formed. However, in the piezoelectric stack and piezoelectric element of this embodiment, the thickness of the pyrochlore phase 16 can be made approximately 100 nm or less (see Examples below).
[0034] In an X-ray diffraction pattern obtained by X-ray diffraction measurement of the piezoelectric film 15, the intensity ratio of the pyrochlore phase to the perovskite phase in the piezoelectric film, represented by the following formula, is preferably 2% or less. py(222) / {pr(100)+pr(110)+pr(111)}×100% Where: py(222) is the peak intensity of the (222) plane of the pyrochlore phase pr(100) is the peak intensity of the (100) plane of the perovskite phase pr(110) is the peak intensity of the (110) plane of the perovskite phase pr(111) is the peak intensity of the (111) plane of the perovskite phase It is.
[0035] If the strength ratio of the pyrochlore phase to the perovskite phase in the piezoelectric film is 2% or less, the piezoelectricity due to the perovskite phase is not hindered, and sufficiently high piezoelectric properties can be obtained.
[0036] As shown in Fig. 4, the piezoelectric film 15 is preferably a columnar structure film including a large number of columnar crystals 17. The large number of columnar crystals 17 preferably extend non-parallel to the substrate surface 11a and are a uniaxially oriented film with a uniform crystal orientation. By using an oriented structure, greater piezoelectricity can be obtained. The piezoelectric film 15, which is a columnar structure film, can be obtained by, for example, the method described in JP 2008-270704 A.
[0037] In the example shown in FIG. 4, the longitudinal direction of the columnar crystal has an inclination β of 1° or more with respect to the normal line of the substrate. This means that the orientation plane of the piezoelectric film 15 has an inclination of 1° or more with respect to the surface of the substrate. Here, the orientation plane is the (100) plane or the (001) plane. In this example, the lattice constants of the a-axis and the c-axis in the perovskite structure are almost the same, and it is not possible to distinguish which plane is the orientation plane by analysis using XRD (X-ray diffraction). In the following, the description of the perovskite phase (100) means the orientation plane (100) plane or the (001) plane. Since the (111) plane of the metal layer constituting the region adjacent to the piezoelectric film 15 of the lower electrode layer 12 (i.e., the first layer 21) is inclined by 1° or more, the piezoelectric film 15 formed on the upper layer tends to show approximately the same inclination due to the influence of the orientation of the metal layer.
[0038] The piezoelectric element 1 of the above embodiment is applicable to ultrasonic devices, mirror devices, sensors, memories, and the like. EXAMPLES
[0039] Examples and comparative examples of the present disclosure will be described below.
[0040] (Preparation of Examples 1 to 13 and Comparative Example 1) The substrate used was a 25 mm square silicon substrate with a thermally oxidized film.
[0041] <Lower electrode layer> A 20 nm thick Ti layer or TiW layer was formed as the second layer of the lower electrode layer on the substrate by RF (Radio Frequency) sputtering under the following sputtering conditions. -Second layer sputtering conditions- Target-substrate distance L (see Table 1, varies depending on each example) Target input power P (see Table 1, varies depending on each example) Ar gas pressure 0.5Pa Substrate temperature 350℃ In Comparative Example 1, the target-substrate distance and input power shown in Table 1 were used. In Examples 1 to 11, in order to increase the amount of oxygen mixed in from the background, the target-substrate distance was widened or the input power was reduced to slow down the film formation rate. In Example 12, a gas in which 1% oxygen was mixed with Ar was used as the sputtering gas. In Example 13, a gas in which 1% nitrogen was mixed with Ar was used as the sputtering gas. In Examples 1 to 11 and Comparative Example 1, oxygen contained in the background in the chamber was mixed into the film.
[0042] Next, a 150 nm thick Ir layer was continuously formed as a first layer on the second layer under the following sputtering conditions. -First layer sputtering conditions- Target-substrate distance: 100 mm Target input power 600W Ar gas pressure 0.1Pa Substrate temperature 350℃
[0043] <Piezoelectric film> The substrate with the lower electrode layer was placed in an RF sputtering device, and an Nb-doped PZT film with an Nb doping amount of 12 at % in the B site was formed under the following sputtering conditions. -Piezoelectric film sputtering conditions- Target-substrate distance: 60 mm Target input power 500W Vacuum degree 0.3Pa Ar / O 2 Mixed atmosphere (O 2 volume fraction 2.0%) Substrate temperature setting: 700℃
[0044] <Top electrode layer> The substrate on which the Nb-doped PZT film was formed as described above was placed in an RF sputtering device, and a two-layer upper electrode layer of Ti 20 nm and Au 100 nm was formed under the following sputtering conditions. -Upper electrode layer sputtering conditions- Target-substrate distance: 100 mm, Target input power 600W Ar gas pressure 0.5Pa Substrate temperature RT (room temperature)
[0045] (evaluation) Each of the examples and comparative examples was evaluated as follows.
[0046] <Amount of oxygen or nitrogen in the first layer of the lower electrode layer> In the manufacturing methods of the above-mentioned Examples 1 to 13 and Comparative Example 1, samples were manufactured by forming the first layer of the lower electrode layer on the substrate under each sputtering condition, and Ar + A secondary ion mass spectrometry (SIMS) analysis was performed to measure the elemental content in the film while irradiating ions and cutting from the surface side of the first layer.
[0047] FIG. 5 shows the SIMS data for Example 3. The horizontal axis represents the sputtering time, and the position of 0 on the horizontal axis represents the surface of the first layer (here, the Ti layer). From the SIMS data, the ratio of oxygen element to all elements contained in the first layer was calculated. In the case of Example 12, the ratio of nitrogen element to all elements contained in the first layer was calculated. The results are shown in Table 1.
[0048] <Tilt of the (111) surface of the first layer of the lower electrode from the substrate surface> For the examples and comparative examples, the crystallinity of the first layer was evaluated by XRD using a RINT-ULTIMAIII manufactured by RIGAKU, using samples before the upper electrode layer was formed. Specifically, the tilt of the (111) plane was obtained by measuring the rocking curve and determining the deviation of the peak of the Ir (111) plane from the Ir peak position when the (111) plane is not tilted. Figure 6 shows rocking curve measurement data for Example 3. The reference position shown in the figure is the peak position of the (111) plane that occurs when the (111) plane is parallel to the surface of the substrate. In the example shown in Figure 6, there is a first peak P1 and a second peak P2, and the split width is 10°. The center of the split width of the first peak P1 and the second peak P2 is the reference position, which means that in this example, the (111) plane of the first layer is tilted by 5° with respect to the state parallel to the substrate.
[0049] <Pyrochlore phase thickness evaluation> For the examples and comparative examples, TEM (Transmission Electron Microscope) images were taken, and the thickness of the pyrochlore phase was determined from the TEM images. Since the contrast in the TEM images of the pyrochlore phase and the perovskite phase in the piezoelectric film is different, the region of the pyrochlore phase can be identified and the thickness can be calculated. It was observed that columnar crystals of perovskite-type oxide were formed in the parts of the piezoelectric film other than the pyrochlore phase. The thickness of the pyrochlore phase was calculated as the average film thickness because the pyrochlore phase was not uniformly formed on the surface of the lower electrode layer.
[0050] Specifically, the original image is binarized at a predetermined threshold value using the contrast adjustment function of the image processing software, and the pyrochlore phase is extracted using the edge extraction function of the image processing software. The threshold value in this case is set to remove as much noise as possible and to extract only those that are clearly distinguishable as pyrochlore phase. If the outline of the pyrochlore-type oxide layer is unclear in the binarized image, a contour line is empirically drawn while looking at the binarized image, and the inside is filled in. The area of the extracted pyrochlore phase is calculated from the number of pixels in the image processing software and divided by the field of view width of the TEM image to obtain the average layer thickness. Photoshop (registered trademark) was used as the image processing software here. The thickness of the pyrochlore phase obtained as described above is shown in Table 1.
[0051] <Evaluation of peak intensity derived from pyrochlore phase> PZT crystallinity was evaluated by XRD using RINT-ULTIMAIII manufactured by RIGAKU. The intensity of the heterogeneous pyrochlore phase (222) was determined from the XRD chart obtained for each example. The region in the XRD chart where the pyrochlore phase (222) was detected was near 29°, and the peak intensity derived from the pyrochlore phase (222) was determined by removing background noise from the obtained XRD diffraction intensity (counts). Also, from the XRD chart, py(222) / {pr(100)+pr(110)+pr(111)}×100% was calculated.
[0052] The strength from each side was determined as follows. The average number of counts at 2θ of 25° to 28° was taken as background noise N. The intensity of py(222) was determined by dividing N by the maximum number of counts in the range of 2θ from 28° to 30°. The pr(100) intensity was determined by dividing N by the maximum number of counts in the range of 2θ from 21° to 23°. The intensity of pr(110) was determined by dividing N by the maximum number of counts in the range of 2θ from 30° to 32°. The intensity of pr(111) was determined by dividing N by the maximum number of counts in the range of 2θ from 37.5° to 39.5°.
[0053] As an example of XRD measurement for evaluating the peak intensity derived from the pyrochlore phase, the XRD charts of Comparative Example 1 are shown in FIG. 7, Example 1 in FIG. 8, and Example 3 in FIG. 9. In FIGS. 7 to 9, the peak values of the perovskite phase (100) are similar. On the other hand, differences are observed in the pyrochlore phase (222). As shown in FIG. 7, in Comparative Example 1, there is a clear pyrochlore phase (222) peak at about 29°. In Example 1 shown in FIG. 8, the pyrochlore phase (222) peak value is lower than that of Comparative Example 1, and in Example 3 shown in FIG. 9, the pyrochlore phase (222) peak is not observed. In Table 1, including Example 3, the peak intensity of the pyrochlore phase (222) is 40 or less, and almost no peak is observed in the XRD chart, which is equivalent to the background.
[0054] Even in cases where almost no peaks of the pyrochlore phase are observed in the XRD chart, as in Example 3, a small amount of the pyrochlore phase is observed between the lower electrode layer and the piezoelectric film in the TEM image, and the thickness of the pyrochlore phase is therefore calculated.
[0055] <Piezoelectric property evaluation> The piezoelectric properties of each example and comparative example were evaluated using the piezoelectric constant d 31 was measured. Piezoelectric constant d 31 The measurement was performed by cutting the piezoelectric element prepared as above into a rectangular shape of 2 mm x 25 mm to prepare a cantilever, and applying a sinusoidal voltage of -10 V ± 10 V according to the method described in I. Kanno et. al. Sensor and Actuator A 107 (2003) 68. The results are shown in Table 1.
[0056] [Table 1]
[0057] In Table 1, the numerical values shown in the column for the oxygen amount or nitrogen amount of the second layer for Examples 1 to 11, 13 and Comparative Example 1 are the oxygen amount, and the nitrogen amount for Example 12. Moreover, +N in Example 12 means that nitrogen gas was added to the sputtering gas, and similarly +O in Example 13 means that oxygen gas was added to the sputtering gas.
[0058] In Examples 1 to 13, in which the (111) plane of the Ir layer, which is the first layer in contact with the piezoelectric film in the lower electrode layer, is inclined by 1° or more with respect to the surface of the substrate, the pyrochlore phase can be suppressed compared to Comparative Example 1, and a large piezoelectric constant d 31 The results showed that the greater the amount of oxygen or nitrogen in the second layer, the greater the inclination of the (111) plane of the first layer. In addition, a high suppression effect was observed when the inclination of the (111) plane was 3° or more, and an especially high suppression effect was obtained at an inclination of 6° to 8°. In addition, the smaller the amount of pyrochlore phase, the greater the piezoelectric constant tended to be.
[0059] By controlling the crystallinity of the surface on which the piezoelectric film of the lower electrode layer is laminated so as to prevent the growth of the pyrochlore phase, the piezoelectricity of the piezoelectric film can be improved. In the region adjacent to the piezoelectric film of the lower electrode layer, high melting point metals such as Ir, which is used in this embodiment, are often used. These precious metals have the characteristic of naturally growing with a (111) preferred orientation when sputtered. If the (111) plane is formed on the surface of the lower electrode layer, the pyrochlore layer is likely to grow. In this embodiment, it was revealed that the pyrochlore phase can be suppressed by shifting the surface of the lower electrode layer from the (111) plane. According to this method, there is no need to insert an additional layer such as a seed layer to control the crystallinity, and since it is only necessary to control the crystallinity, there is no need to change the film configuration, so it is possible to suppress an increase in costs.
[0060] The disclosure of Japanese Patent Application No. 2020-166409, filed on September 30, 2020, is incorporated herein by reference in its entirety. All publications, patent applications, and standards mentioned in this specification are herein incorporated by reference to the same extent as if each individual publication, patent application, or standard was specifically and individually indicated to be incorporated by reference.
Claims
1. A piezoelectric laminate including a lower electrode layer and a piezoelectric film in this order on a substrate, a region of the lower electrode layer that is in contact with the piezoelectric film is made of a metal layer, and a (111) plane of the metal layer is inclined at an angle of 1° or more with respect to a surface of the substrate; the piezoelectric film includes a perovskite oxide containing Pb, the lower electrode layer includes a first layer made of the metal layer, and a second layer adjacent to the first layer and provided on the substrate side; A piezoelectric laminate, wherein the second layer is composed mainly of at least one of Ti and W, and contains more than 5 at % and less than 50 at % of oxygen or nitrogen.
2. A piezoelectric laminate comprising a lower electrode layer and a piezoelectric film, in that order, on a substrate, a region of the lower electrode layer that is in contact with the piezoelectric film is made of a metal layer, and a (111) plane of the metal layer is inclined at an angle of 1° or more with respect to a surface of the substrate; the piezoelectric film includes a perovskite oxide containing Pb, A piezoelectric laminate, wherein in an X-ray diffraction pattern of the piezoelectric film, an intensity ratio of a pyrochlore phase in the piezoelectric film to a perovskite phase, as represented by the following formula, is 2% or less. py(222) / {pr(100)+pr(110)+pr(111)}×100% py(222) is the peak intensity of the (222) plane of the pyrochlore phase pr(100) is the peak intensity of the (100) plane of the perovskite phase pr(110) is the peak intensity of the (110) plane of the perovskite phase pr(111) is the peak intensity of the (111) plane of the perovskite phase It is.
3. the lower electrode layer includes a first layer made of the metal layer, and a second layer adjacent to the first layer and provided on the substrate side; 3. The piezoelectric stack according to claim 2, wherein the second layer is composed mainly of at least one of Ti and W, and contains more than 5 at % and less than 50 at % of oxygen or nitrogen.
4. A piezoelectric laminate described in any one of claims 1 to 3, wherein the metal constituting the metal layer is at least one of Ir, Pt, Au, Mo, Ta and Al.
5. 5. The piezoelectric laminate according to claim 1, wherein the piezoelectric film has a columnar crystal film structure made up of a large number of columnar crystals.
6. 6. The piezoelectric stack according to claim 5, wherein the (100) or (001) plane of the columnar crystal has an inclination of 1° or more with respect to the surface of the substrate.
7. The piezoelectric laminate according to any one of claims 1 to 6, and an upper electrode layer provided on the piezoelectric film of the piezoelectric laminate.
8. 8. The piezoelectric element of claim 7, wherein the upper electrode layer comprises a metal or metal oxide including at least one of Ir, Pt, Au, Ti, Mo, Ta, Ru, and Al.
Citation Information
Patent Citations
Piezoelectric / electrostrictive element structure, method of manufacturing piezoelectric / electrostrictive element structure, and method of manufacturing liquid jet head
JP2006100814A
Ferroelectric film and its manufacturing method, dielectric element, and liquid discharge apparatus
JP2008270704A
Piezoelectric thin-film element and piezoelectric thin-film device equipped with same
WO2011118093A1