Method for producing polytetrafluoroethylene powder, and polytetrafluoroethylene powder
The described method efficiently pulverizes PTFE at low temperatures to produce fine powder without drying or dispersion aids, addressing inefficiencies in existing methods and improving industrial productivity and product quality.
Patent Information
- Application Number
- JP2023144462
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-09-27
- Filing Date
- 2023-09-06
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2043-09-06
AI Technical Summary
Existing methods for producing polytetrafluoroethylene (PTFE) powder require post-processing such as drying and are inefficient in achieving fine pulverization without the use of dispersion aids, leading to potential coloring issues.
A method involving pulverization of PTFE at a surface temperature below 35°C using a pulverizer with controlled temperature, preferably metal crushing members, in a dry process, allowing for repeated pulverization steps and continuous operation to achieve fine PTFE powder without the need for drying or dispersion aids.
The method enables efficient fine pulverization of PTFE without post-processing, reducing the likelihood of coloring and enhancing industrial productivity while maintaining high molecular weight and particle size control.
Smart Images

Figure 0007575709000001 
Figure 0007575709000002 
Figure 0007575709000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for producing polytetrafluoroethylene powder and to a polytetrafluoroethylene powder. [Background technology]
[0002] As a method for pulverizing a fluororesin, a method is known in which coarse powder of the fluororesin dispersed in water containing a dispersion aid is pulverized by a wet mill method (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-006578 A Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present disclosure is to provide a method for producing polytetrafluoroethylene powder that is capable of finely pulverizing polytetrafluoroethylene without the need for post-treatment such as drying, and to provide the polytetrafluoroethylene powder. [Means for solving the problem]
[0005] The present disclosure (1) is a method for producing polytetrafluoroethylene powder, comprising a grinding step of grinding polytetrafluoroethylene using a grinder with a surface temperature of a grinding member of the grinder set to less than 35°C.
[0006] The present disclosure (2) is the manufacturing method according to the present disclosure (1), wherein the crushing member is a crushing member capable of crushing the polytetrafluoroethylene.
[0007] The present disclosure (3) is the manufacturing method according to the present disclosure (2), in which, in the pulverizing step, the polytetrafluoroethylene is crushed by at least a pair of the crushing members arranged opposite to each other.
[0008] The present disclosure (4) is a method for producing an arbitrary combination of the present disclosures (1) to (3), in which the polytetrafluoroethylene is polytetrafluoroethylene that has a history of being heated to a temperature equal to or higher than the melting point.
[0009] The present disclosure (5) is a manufacturing method in which the above-mentioned pulverization step is carried out in a dry manner and is any combination with any of the present disclosures (1) to (4).
[0010] The present disclosure (6) is a manufacturing method in any combination with any of the present disclosures (1) to (5), in which the pulverizer has an inlet and an outlet, and the pulverizing step is carried out continuously.
[0011] The present disclosure (7) is a manufacturing method in which the above-mentioned pulverization step is repeated multiple times in any combination with any of the present disclosures (1) to (6).
[0012] The present disclosure (8) is a production method for any combination with any of the present disclosures (1) to (7), further comprising a coarse grinding step of coarsely grinding polytetrafluoroethylene, and subjecting the coarse powder obtained in the coarse grinding step to the above-mentioned grinding step.
[0013] The present disclosure (9) is a polytetrafluoroethylene powder containing scaly polytetrafluoroethylene particles.
[0014] The present disclosure (10) is the polytetrafluoroethylene powder according to the present disclosure (9) having one or more melting points in a temperature range below 333°C.
[0015] The present disclosure (11) is the polytetrafluoroethylene powder according to the present disclosure (9) or (10), having a median diameter of 110 μm or less.
[0016] This disclosure (12) is the L measured on a test piece obtained by molding under the following conditions.* a * b * L in color space * The polytetrafluoroethylene powder is any combination of the polytetrafluoroethylene powder of the present disclosure (9) to (11) in which the molecular weight is 70 or more. (Molding conditions) 54 g of polytetrafluoroethylene powder is placed into a φ120 mm mold and held at 370°C for 30 minutes using a heat press to melt the polytetrafluoroethylene. A load of 3 MPa is then applied for 1 minute to perform compression molding, and the mold is cooled to produce a test specimen.
[0017] This disclosure (13) is the L measured using a test piece obtained by molding under the following conditions. * a * b * L in color space * The L measured with the above polytetrafluoroethylene powder * The polytetrafluoroethylene powder is any combination of the polytetrafluoroethylene powder of the present disclosure (9) to (12), in which the rate of change with respect to the powder is 25% or less. (Molding conditions) 54 g of polytetrafluoroethylene powder is placed into a φ120 mm mold and held at 370°C for 30 minutes using a heat press to melt the polytetrafluoroethylene. A load of 3 MPa is then applied for 1 minute to perform compression molding, and the mold is cooled to produce a test specimen. Effect of the Invention
[0018] According to the present disclosure, it is possible to provide a method for producing polytetrafluoroethylene powder that is capable of finely pulverizing polytetrafluoroethylene without the need for post-treatment such as drying, and the polytetrafluoroethylene powder. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The present disclosure will now be described in detail.
[0020] The present disclosure provides a method for producing polytetrafluoroethylene powder, comprising a grinding step of grinding polytetrafluoroethylene using a grinder at a surface temperature of a grinding member included in the grinder of less than 35°C.
[0021] Polytetrafluoroethylene (PTFE) has a transition point at which the storage modulus changes around 30°C, and the modulus decreases at temperatures above the transition point, making fine pulverization difficult. In the manufacturing method of the present disclosure, fine pulverization can be easily performed by setting the surface temperature of the pulverizing member to less than 35°C. In addition, since the manufacturing method of the present disclosure can be performed in a dry manner, post-treatment such as drying is not required, which is advantageous for industrial production. Furthermore, since there is no need to use a dispersing agent, there is also the advantage that problems such as coloring caused by the dispersing agent are less likely to occur.
[0022] In the pulverization step, the PTFE is pulverized by setting the surface temperature of the pulverizing member of the pulverizer to less than 35° C. The surface temperature is preferably 30° C. or less, more preferably 25° C. or less, and even more preferably 20° C. or less. The surface temperature is also preferably 1° C. or more, more preferably 5° C. or more, and even more preferably 10° C. or more. The surface temperature is preferably the temperature of the portion of the pulverizing member that is in contact with the PTFE.
[0023] The pulverizer used in the pulverization step includes a pulverizing member that is capable of pulverizing the PTFE.
[0024] The crushing member may be made of metal, ceramic, or the like, but is preferably made of metal in that temperature control is easier.
[0025] The above-mentioned crushing member is preferably a crushing member capable of crushing the above-mentioned PTFE, in that fine crushing is easily achieved. As the above-mentioned crushing member, it is preferable to use a member that utilizes the principle of a mill, in which the material to be crushed is crushed (grinded) by friction between upper and lower mills (grinding stones), and in particular, a member that utilizes the principle of a rotary mill, in which the material is crushed by rotating the mill. The crushing member is preferably disk-shaped, and more preferably mortar-shaped.
[0026] When the pulverizing member is the crushing member, it is preferable to crush the PTFE by at least a pair of the crushing members arranged opposite to each other. In this embodiment, it is preferable to put the PTFE into the gap between the pair of crushing members, rotate one of the crushing members, and crush the PTFE by friction with the other crushing member. At this time, the other crushing member may be fixed or rotated.
[0027] The pulverizer preferably has a temperature control function capable of adjusting the temperature of the pulverizing member, and more preferably has a cooling mechanism capable of cooling the pulverizing member. As the cooling mechanism, a known type such as a water-cooling type or an air-cooling type can be adopted.
[0028] The above-mentioned pulverizer is preferably a mortar-type pulverizer, and examples thereof include mortar-type pulverizers having a temperature control function as described in JP-A-2016-215115, JP-A-2016-209813, JP-A-2003-047867, and the like.
[0029] The crusher preferably has an inlet for feeding the material to be crushed and an outlet for discharging the crushed material. By having the crusher have an inlet and an outlet, the crushing process can be performed continuously. As long as the material can be fed and discharged sufficiently, the shape and size of the inlet and outlet are not important.
[0030] In the above-mentioned grinding step, when grinding is performed by rotating the grinding member, the rotation speed is preferably 45 rpm or more, more preferably 50 rpm or more, and even more preferably 60 rpm or more, and is preferably 120 rpm or less, more preferably 110 rpm or less, and even more preferably 100 rpm or less.
[0031] When at least one pair of crushing members is used, the size of the gap therebetween can be set according to the particle size of the target PTFE powder, but is preferably 10 μm or less, more preferably 5 μm or less, and even more preferably 2 μm or less, for example. The lower limit is not particularly limited, and crushing may be performed in a state where the crushing members are in contact with each other. In this case, it is preferable that the crushing members are in contact within a range where wear of the crushing members does not occur.
[0032] In the above-mentioned pulverization step, the discharge rate of the pulverized PTFE from the pulverizer is preferably 0.5 kg / h or more, more preferably 1 kg / h or more, and even more preferably 1.5 kg / h or more, and is preferably 20 kg / h or less, more preferably 10 kg / h or less, and even more preferably 5 kg / h or less.
[0033] The grinding step is preferably carried out in a dry manner. Carrying out the grinding step in a dry manner means that the grinding step is carried out substantially in the absence of liquid (e.g., water). Substantially no liquid means that the amount of liquid present is 5% by mass or less relative to the PTFE. The amount of liquid present is preferably 3% by mass or less, more preferably 1% by mass or less, and even more preferably 0.1% by mass or less.
[0034] The grinding step is preferably carried out substantially in the absence of a dispersing aid. Substantially no dispersing aid means that the amount of dispersing aid present is 0.5% by mass or less relative to the PTFE. The amount of dispersing aid present is preferably 0.1% by mass or less, more preferably 0.01% by mass or less, and even more preferably 0.001% by mass or less.
[0035] The dispersion aid is a compound capable of dispersing the PTFE in water. Examples of the dispersion aid include alcohol, anionic surfactants, and nonionic surfactants.
[0036] The above-mentioned pulverization step may be carried out only once or may be repeated several times. When repeated several times, the above-mentioned PTFE can be further pulverized finely. The number of times of repetition is not particularly limited and may be determined according to the target particle size, but may be, for example, two or more times, or five or less times. The period from when PTFE is fed into the pulverizer until the pulverized PTFE is discharged is counted as one time (one pass).
[0037] It is also preferable to carry out the above-mentioned pulverization step continuously using a pulverizer having an inlet and an outlet. By arranging a plurality of pulverizers having an inlet and an outlet in series, the above-mentioned repeated operation can be carried out continuously.
[0038] The PTFE to be pulverized in the above pulverization step may be high molecular weight PTFE.
[0039] The PTFE may be a homopolymer of tetrafluoroethylene (TFE), or a modified PTFE containing 99.0% by mass or more of polymerization units based on TFE (TFE units) and 1.0% by mass or less of polymerization units based on a modified monomer (modified monomer units). The modified PTFE may be composed only of TFE units and modified monomer units.
[0040] The modified PTFE preferably has a modified monomer unit content in the range of 0.00001 to 1.0% by mass based on the total polymerized units. The lower limit of the modified monomer unit content is more preferably 0.0001% by mass, more preferably 0.001% by mass, even more preferably 0.005% by mass, and even more preferably 0.010% by mass. The upper limit of the modified monomer unit content is preferably 0.90% by mass, more preferably 0.50% by mass, even more preferably 0.40% by mass, even more preferably 0.30% by mass, even more preferably 0.20% by mass, and especially preferably 0.10% by mass. In this specification, the modified monomer unit means a portion of the molecular structure of PTFE that is derived from a modified monomer.
[0041] The above-mentioned modified monomer is not particularly limited as long as it can be copolymerized with TFE, and examples thereof include perfluoroolefins such as hexafluoropropylene [HFP], hydrogen-containing fluoroolefins such as trifluoroethylene and vinylidene fluoride [VDF], perhaloolefins such as chlorotrifluoroethylene, perfluorovinyl ether, perfluoroallyl ether, (perfluoroalkyl)ethylene, ethylene, etc. The modified monomer used may be one type or multiple types.
[0042] The perfluorovinyl ether is not particularly limited, and examples thereof include perfluorovinyl ethers represented by the following general formula (A): CF2=CF-ORf (A) (wherein Rf represents a perfluoro organic group). In this specification, the "perfluoro organic group" refers to an organic group in which all hydrogen atoms bonded to carbon atoms are replaced with fluorine atoms. The perfluoro organic group may have an ether oxygen.
[0043] An example of the perfluorovinyl ether is perfluoro(alkyl vinyl ether) [PAVE], where Rf in the general formula (A) is a perfluoroalkyl group having 1 to 10 carbon atoms. The number of carbon atoms in the perfluoroalkyl group is preferably 1 to 5.
[0044] Examples of the perfluoroalkyl group in the PAVE include a perfluoromethyl group, a perfluoroethyl group, a perfluoropropyl group, a perfluorobutyl group, a perfluoropentyl group, and a perfluorohexyl group.
[0045] The perfluorovinyl ether further includes those in which Rf in the above general formula (A) is a perfluoro(alkoxyalkyl) group having 4 to 9 carbon atoms, and those in which Rf is the following formula:
[0046] [ka]
[0047] (wherein m represents 0 or an integer of 1 to 4), Rf is a group represented by the following formula:
[0048] [ka]
[0049] (wherein n represents an integer of 1 to 4).
[0050] The (perfluoroalkyl)ethylene (PFAE) is not particularly limited, and examples thereof include (perfluorobutyl)ethylene (PFBE) and (perfluorohexyl)ethylene.
[0051] The perfluoroallyl ether may, for example, be a compound represented by the general formula (B): CF2=CF-CF2-ORf 1 (B) (In the formula, Rf 1 represents a perfluoro organic group.
[0052] Above Rf 1 is preferably a perfluoroalkyl group having 1 to 10 carbon atoms or a perfluoroalkoxyalkyl group having 1 to 10 carbon atoms. The perfluoroallyl ether is preferably at least one selected from the group consisting of CF2=CF-CF2-O-CF3, CF2=CF-CF2-O-C2F5, CF2=CF-CF2-O-C3F7, and CF2=CF-CF2-O-C4F9, more preferably at least one selected from the group consisting of CF2=CF-CF2-O-C2F5, CF2=CF-CF2-O-C3F7, and CF2=CF-CF2-O-C4F9, and further preferably CF2=CF-CF2-O-CF2CF2CF3.
[0053] The standard specific gravity (SSG) of the PTFE is preferably 2.280 or less, more preferably 2.10 or less, and more preferably 1.50 or more, more preferably 1.60 or more. The SSG is measured by the water displacement method according to ASTM D-792 using a sample molded according to ASTM D 4895.
[0054] The PTFE generally has non-melt secondary processability, which means that the melt flow rate cannot be measured at a temperature higher than the melting point in accordance with ASTM D-1238 and D-2116, in other words, that the PTFE does not flow easily even in the melting temperature range.
[0055] The PTFE preferably has a history of being heated to a temperature above its melting point. In general, it is not easy to pulverize the PTFE that has a history of being heated to a temperature above its melting point while maintaining its high molecular weight. According to the manufacturing method of the present disclosure, even the PTFE that has a history of being heated to a temperature above its melting point can be pulverized by a simple process. The heating may be for the purposes of molding, heat treatment, or the like.
[0056] The PTFE has one of its melting points preferably being 310° C. or higher, more preferably 320° C. or higher, and more preferably lower than 333° C. It may also have a melting point in the temperature range of 333° C. or higher. The fact that the melting point is within the above range indicates that the material has a history of being heated to a temperature equal to or higher than the melting point. In this specification, the melting point is the temperature corresponding to the minimum point in the heat of fusion curve obtained by performing differential scanning calorimetry (DSC) at a heating rate of 10° C. / min using an X-DSC7000 (manufactured by Hitachi High-Tech Science Corp.) When there are two or more minimum points in one melting peak, each of them is regarded as a melting point.
[0057] The PTFE is preferably not crosslinked. The crosslinking may be by irradiation with ionizing radiation, for example, by irradiation with ionizing radiation at a temperature equal to or higher than the melting point of PTFE.
[0058] The PTFE may further include a filler. Examples of the filler include at least one selected from the group consisting of glass fiber, glass beads, carbon fiber, spherical carbon, carbon black, graphite, silica, alumina, mica, silicon carbide, boron nitride, titanium oxide, bismuth oxide, cobalt oxide, molybdenum disulfide, bronze, gold, silver, copper, and nickel. Among them, at least one selected from the group consisting of glass fiber, carbon fiber, carbon black, and bronze is preferable.
[0059] The PTFE used in the above pulverization step may be in powder form.
[0060] The size of the PTFE used in the above pulverization step is not particularly limited, and it is sufficient if it can be fed into a pulverizer, and the maximum particle diameter may be about 10 mm or about 5 mm. There is also no problem with a diameter of 1 mm or less. However, from the viewpoint of obtaining a powder having a smaller particle size after pulverization, it is preferable that the particle size at the time of charging is small. The maximum diameter of the PTFE particles used in the above pulverization step may be 10 mm or less, 5 mm or less, or 1 mm or less. In this specification, the maximum diameter of particles is measured using a digital microscope for particles of 1 mm or more, and is evaluated as the median diameter for particles less than 1 mm. The median diameter is measured using a Beckman Coulter laser diffraction particle size analyzer (LS13 320) in a dry condition at a vacuum pressure of 20 mH2O, and is equal to the particle diameter corresponding to 50% of the integrated particle size distribution (volume basis).
[0061] The PTFE used in the pulverization step may be one that has been coarsely pulverized in advance. The manufacturing method of the present disclosure further includes a coarse pulverization step of coarsely pulverizing the PTFE, and it is preferable that the coarse powder obtained in the coarse pulverization step is subjected to the pulverization step.
[0062] As the PTFE to be coarsely pulverized in the coarse pulverization step, for example, a molded product obtained by molding and baking PTFE that has not been heated to a temperature above its melting point, cutting chips thereof, or end pieces of the molded product after cutting can be used. The shape of the molded product is not particularly limited. As the PTFE to be coarsely pulverized, PTFE that has not been molded and has been heated to a temperature above its melting point can also be used.
[0063] The coarse pulverization can be carried out by a pulverizer or the like. The pulverizer is not particularly limited, and may be any pulverizer capable of pulverizing PTFE to a certain degree. Examples of the pulverizer include a cutter mill, an air jet mill, a hammer mill, a force mill, and a freeze pulverizer.
[0064] The manufacturing method of the present disclosure may further include a step of heat-treating the PTFE powder obtained in the above-mentioned pulverization step at a temperature of 100 to 340° C. By carrying out the above-mentioned heat treatment, it is possible to eliminate distortion of the particles caused by the pulverization.
[0065] The manufacturing method of the present disclosure preferably does not include an embrittlement treatment by exposure to ionizing radiation.
[0066] In the manufacturing method of the present disclosure, a PTFE powder having a small particle size can be obtained by carrying out the above-mentioned pulverization step.
[0067] In the manufacturing method of the present disclosure, the above-mentioned pulverization step can be carried out continuously, and therefore, compared with methods that have been carried out using freeze pulverization or the like, it is possible to provide a PTFE powder having a small particle size with higher productivity.
[0068] The PTFE powder obtained by the manufacturing method of the present disclosure has a D10 of preferably 50 μm or less, more preferably 40 μm or less, and even more preferably 30 μm or less, and preferably 5 μm or more, more preferably 10 μm or more, and even more preferably 20 μm or more. D10 is measured using a Beckman Coulter laser diffraction particle size analyzer (LS13 320) in a dry condition at a vacuum pressure of 20 mH2O, and is equal to the particle size corresponding to 10% of the integrated particle size distribution (volume basis).
[0069] The PTFE powder obtained by the manufacturing method of the present disclosure has a median diameter (D50) of preferably 150 μm or less, more preferably 110 μm or less, even more preferably 100 μm or less, even more preferably 90 μm or less, even more preferably 80 μm or less, even more preferably 70 μm or less, and particularly preferably 50 μm or less. The lower limit is not particularly limited, but may be, for example, 1 μm or 10 μm. The median diameter is measured using a Beckman Coulter laser diffraction particle size analyzer (LS13 320) in a dry condition at a vacuum pressure of 20 mH2O, and is equal to the particle diameter corresponding to 50% of the integrated particle size distribution (volume basis).
[0070] The PTFE powder obtained by the manufacturing method of the present disclosure has a D90 of preferably 300 μm or less, more preferably 250 μm or less, even more preferably 200 μm or less, even more preferably 150 μm or less, and preferably 50 μm or more, more preferably 60 μm or more, and even more preferably 70 μm or more. D90 is measured using a Beckman Coulter laser diffraction particle size analyzer (LS13 320) in a dry condition at a vacuum pressure of 20 mH2O, and is equal to the particle size corresponding to 90% of the integrated particle size distribution (volume basis).
[0071] The present disclosure also provides a PTFE powder comprising flake-like PTFE particles.
[0072] The above-mentioned scaly PTFE particles preferably have a ratio of diameter to thickness (diameter / thickness) of 3.0 or more, more preferably 4.0 or more, and even more preferably 5.0 or more, and preferably 20 or less, more preferably 15 or less, and even more preferably 10 or less. The above ratio is determined by observing the PTFE particles with a scanning electron microscope (SEM), processing the images, and calculating the diameter and thickness. The ratio is determined for 20 particles, and the average value is used.
[0073] The PTFE powder of the present disclosure preferably has a history of being heated to a temperature equal to or higher than its melting point. The PTFE powder of the present disclosure preferably has one or more melting points in a temperature range below 333° C. The above temperature range is preferably 310° C. or higher, and more preferably 320° C. or higher. Having a melting point in the above temperature range indicates that there is a history of heating to a temperature equal to or higher than the melting point. The PTFE powder of the present disclosure may also have a melting point in the temperature range of 333° C. or higher.
[0074] The PTFE powder of the present disclosure has a D10 of preferably 50 μm or less, more preferably 40 μm or less, and even more preferably 30 μm or less, and preferably 5 μm or more, more preferably 10 μm or more, and even more preferably 20 μm or more.
[0075] The PTFE powder of the present disclosure has a median diameter (D50) of preferably 150 μm or less, more preferably 110 μm or less, even more preferably 100 μm or less, even more preferably 90 μm or less, even more preferably 80 μm or less, even more preferably 70 μm or less, and particularly preferably 50 μm or less. The lower limit is not particularly limited, but may be, for example, 1 μm or 10 μm.
[0076] The PTFE powder of the present disclosure has a D90 of preferably 300 μm or less, more preferably 250 μm or less, even more preferably 200 μm or less, even more preferably 150 μm or less, and preferably 50 μm or more, more preferably 60 μm or more, and even more preferably 70 μm or more.
[0077] The PTFE powder of the present disclosure has an L measured using a test piece obtained by molding under the following conditions. * a * b * L in color space * It is preferable that the ratio is 70 or more. (Molding conditions) 54 g of polytetrafluoroethylene powder is placed into a φ120 mm mold and held at 370°C for 30 minutes using a heat press to melt the polytetrafluoroethylene. A load of 3 MPa is then applied for 1 minute to perform compression molding, and the mold is cooled to produce a test specimen.
[0078] L * When L is within the above range, coloring during molding is reduced and an excellent appearance is obtained. * is more preferably equal to or greater than 75, and even more preferably equal to or greater than 80. The upper limit is not particularly limited, but may be, for example, 90. The above L * The L value for reflected light was measured using the SCI method with a Konica Minolta spectrophotometer CM-5, a C light source, and a 2° field of view. * a * b * is measured and determined.
[0079] The PTFE powder of the present disclosure has an L measured using a test piece obtained by molding under the following conditions. * a * b * L in color space * The L measured with the above PTFE powder * It is preferable that the rate of change (rate of decrease) is 25% or less. (Molding conditions) 54 g of polytetrafluoroethylene powder is placed into a φ120 mm mold and held at 370°C for 30 minutes using a heat press to melt the polytetrafluoroethylene. A load of 3 MPa is then applied for 1 minute to perform compression molding, and the mold is cooled to produce a test specimen.
[0080] The above L * When the rate of change of L is within the above range, coloring during molding is further reduced, and a more excellent appearance is obtained. * The rate of change is more preferably 20% or less. The lower limit is not particularly limited, but may be, for example, 5%. The above L * The rate of change is determined by the following method. The PTFE powder was filled into a φ30mm CM-5 petri dish using a Konica Minolta spectrophotometer CM-5, and the L against reflected light was measured using the SCI method with a C light source and a 2° field of view. * a * b * Measure L * In addition, the L of the test piece obtained by molding the PTFE powder under the above conditions was similarly determined. * Measure the L before and after molding. * Using the measured values, calculate the rate of change using the following formula. L * Rate of change (%) = |{(L of the test piece after molding) * )-(L of PTFE powder before molding * )} / (L of PTFE powder before molding * )×100|
[0081] The PTFE constituting the PTFE powder of the present disclosure may be a high molecular weight PTFE, and the standard specific gravity (SSG) is preferably 2.280 or less, more preferably 2.10 or less, and is preferably 1.50 or more, more preferably 1.60 or more.
[0082] The PTFE constituting the PTFE powder of the present disclosure is preferably not crosslinked.
[0083] The PTFE constituting the PTFE powder of the present disclosure may have the same composition and physical properties as the PTFE in the production method of the present disclosure.
[0084] The PTFE constituting the PTFE powder of the present disclosure preferably does not exhibit melt fluidity, taking into consideration the physical properties after molding and the wear resistance and heat resistance as an additive. Not exhibiting melt fluidity means that the particle shape is maintained even when the particles are heated to exceed the melting point. The fact that the PTFE does not exhibit melt fluidity can be confirmed by observing with a microscope equipped with a hot stage.
[0085] The PTFE powder of the present disclosure may further include a filler. Examples of the filler include at least one selected from the group consisting of glass fiber, glass beads, carbon fiber, spherical carbon, carbon black, graphite, silica, alumina, mica, silicon carbide, boron nitride, titanium oxide, bismuth oxide, cobalt oxide, molybdenum disulfide, bronze, gold, silver, copper, and nickel. Among them, at least one selected from the group consisting of glass fiber, carbon fiber, carbon black, and bronze is preferable.
[0086] The PTFE powder of the present disclosure is preferably not subjected to an embrittlement treatment by exposure to ionizing radiation.
[0087] The PTFE powder of the present disclosure can be suitably produced by the production method of the present disclosure described above.
[0088] The PTFE powder obtained by the manufacturing method of the present disclosure and the PTFE powder of the present disclosure can be suitably used as a molding material. The method for molding the PTFE powder is not particularly limited, but includes compression molding, ram extrusion molding, hot coining molding, isostatic molding, etc. Among them, ram extrusion molding and hot coining molding are preferred.
[0089] The molded article obtained from the PTFE powder obtained by the manufacturing method of the present disclosure and the molded article obtained from the PTFE powder of the present disclosure can be suitably used for lining sheets, packings, gaskets, diaphragm valves, heat-resistant electric wires, heat-resistant insulating tapes for vehicle motors and generators, etc., release sheets, sealing materials, casings, sleeves, bellows, hoses, piston rings, butterfly valves, square tanks, wafer carriers, etc.
[0090] The PTFE powder obtained by the manufacturing method of the present disclosure and the PTFE powder of the present disclosure can be manufactured without embrittlement treatment by irradiation with ionizing radiation, and therefore can retain the properties that conventional PTFE has, such as wear resistance, etc. Therefore, they can be suitably used as an additive for imparting wear resistance, heat resistance, etc.
[0091] Although the embodiments have been described above, it will be understood that various changes in form and details are possible without departing from the spirit and scope of the claims. EXAMPLES
[0092] The present disclosure will now be described in more detail with reference to examples, but the present disclosure is not limited to these examples.
[0093] Various physical properties were measured by the following methods.
[0094] (Melting Point) The melting point was determined as the temperature corresponding to the minimum point in the heat of fusion curve obtained by differential scanning calorimetry (DSC) at a heating rate of 10°C / min using an X-DSC7000 (Hitachi High-Tech Science Corporation). When there are two or more minimum points in one melting peak, each of them was regarded as the melting point.
[0095] (Standard specific gravity (SSG)) Using samples molded in accordance with ASTM D4895, the measurement was performed by the water displacement method in accordance with ASTM D792.
[0096] (particle size distribution) Measurements were performed using a Beckman Coulter laser diffraction particle size distribution analyzer (LS13 320) in a dry state at a vacuum pressure of 20 mH2O, and the particle size distribution (volume basis) was calculated. The particle size corresponding to 10% of the particle size distribution accumulation was defined as D10, the particle size corresponding to 50% was defined as D50 (median diameter), and the particle size corresponding to 90% was defined as D90.
[0097] (diameter / thickness ratio) The PTFE particles in the powder were observed with a scanning electron microscope (SEM) and the images were processed to determine their diameter and thickness. Measurements were taken for 20 particles, and the average values were used.
[0098] (L * value) 54g of PTFE powder was placed in a φ120mm mold and held at 370℃ for 30 minutes using a heat press machine to melt the PTFE. A load of 3MPa was applied for 1 minute to perform compression molding, and the mold was cooled to obtain a test piece. The L against reflected light was measured using a Konica Minolta CM-5 spectrophotometer with a C light source and a 2° field of view using the SCI method. * a * b * was measured and found. The L of the obtained PTFE powder * The value was measured by filling the PTFE powder into a 30 mm diameter CM-5 dedicated petri dish and using a Konica Minolta CM-5 spectrophotometer under the same conditions as those for the above test piece.
[0099] (L * Rate of change (decrease) of value The L of the PTFE powder before molding measured by the above method * value and the L of the molded test piece * Using the value and the formula below, L * The rate of change of the value was determined. L * Rate of change (%) = |{(L of the test piece after molding) * )-(L of PTFE powder before molding * )} / (L of PTFE powder before molding * )×100|
[0100] Production Example 1 (Preparation of PTFE Powder A-1) The homo-PTFE coarse powder obtained by suspension polymerization of TFE monomer alone was crushed in a crusher to obtain PTFE molding powder (standard specific gravity (SSG): 2.159, melting point: 345.0°C). 35 g of this powder was compression molded in a φ100 mm mold at 30 MPa for 1 minute and then baked at 370°C for 3 hours to obtain a molded product. The molded product obtained was crushed in a crusher to obtain PTFE powder A-1. The melting point of PTFE powder A-1 was 328°C, the maximum particle diameter was confirmed to be 1-5 mm using a microscope, and the L of the powder was 1.5 mm. * was 97.
[0101] Production Example 2 (Preparation of PTFE Powder A-2) A molded product was obtained in the same manner as in Production Example 1, and pulverized in a pulverizer to obtain PTFE powder A-2. The melting point of PTFE powder A-2 was 328°C, the median diameter was 208 μm, and the L of the powder was 1. * was 97.
[0102] Example 1 The PTFE powder A-1 was crushed using a stone mill type crusher having an inlet and an outlet, a rotatable crushing part with a diameter of φ250 mm, and water channels in the upper and lower crushing parts for water temperature control. Cooling water was run through the mill of the crusher, and the mill surface temperature was measured with a contact thermometer to be 20°C. In the state where the upper and lower mills were in contact (clearance 0 mm), the mill rotation speed was set to 75 rpm, and the PTFE powder A-1 was supplied at a discharge rate of 2.3 kg / h to perform the crushing operation, thereby obtaining PTFE resin powder B-1. Various physical properties of the obtained PTFE powder were measured. The results are shown in Table 1.
[0103] Example 2 A PTFE powder was obtained in the same manner as in Example 1, except that the pulverization step was repeated three times. Various physical properties of the obtained PTFE powder were measured. The results are shown in Table 1.
[0104] Example 3 A PTFE powder was obtained in the same manner as in Example 1, except that the rotation speed of the mill was changed to 120 rpm. Various physical properties of the obtained PTFE powder were measured. The results are shown in Table 1.
[0105] Example 4 A PTFE powder was obtained in the same manner as in Example 1, except that the set temperature of the mill was changed to 10° C. and the rotation speed of the mill was changed to 120 rpm. Various physical properties of the obtained PTFE powder were measured. The results are shown in Table 1.
[0106] Example 5 A PTFE powder was obtained in the same manner as in Example 1, except that the rotation speed of the mill was changed to 45 rpm. Various physical properties of the obtained PTFE powder were measured. The results are shown in Table 1.
[0107] Example 6 A PTFE powder was obtained in the same manner as in Example 1, except that the set temperature of the mill was changed to 25° C. and the rotation speed of the mill was changed to 45 rpm. Various physical properties of the obtained PTFE powder were measured. The results are shown in Table 1.
[0108] Comparative Example 1 As the pulverizer, a stone mill type pulverizer having an inlet and an outlet, a rotatable pulverizer part with a diameter of φ250 mm, and an upper pulverizer part capable of being heated by a heater was used, and the PTFE powder was obtained in the same manner as in Example 1, except that the set temperature of the mill was changed to 35°C and the discharge rate to 2.2 kg / h. Various physical properties of the obtained PTFE powder were measured. The results are shown in Table 1.
[0109] Comparative Example 2 A PTFE powder was obtained in the same manner as in Comparative Example 1, except that the set temperature of the die was changed to 100° C. Various physical properties of the obtained PTFE powder were measured. The results are shown in Table 1.
[0110] Comparative Example 3 A PTFE powder was obtained in the same manner as in Comparative Example 1, except that the set temperature of the die was changed to 150° C. Various physical properties of the obtained PTFE powder were measured. The results are shown in Table 1.
[0111] Comparative Example 4 The liquid to be treated was prepared by mixing 1 kg of PTFE powder A-2, 4 kg of pure water, and 10 g of a surfactant (Cadenax DM10D-W, manufactured by Lion Specialty Chemicals). A mill-type grinder having an inlet and an outlet and a rotatable grinding part with a diameter of φ250 mm was used, and the liquid to be treated was fed in with the upper and lower mill surfaces brought close enough to each other to provide a clearance of 0 mm. The mill was rotated at 1500 rpm to grind the liquid, and a suspension containing PTFE powder was obtained by three passes. The suspension was filtered, and the wet PTFE powder was taken out and dried at 150°C for 15 hours to obtain a PTFE powder. Various physical properties of the obtained PTFE powder were measured. The results are shown in Table 2.
[0112] [Table 1]
[0113] [Table 2]
Claims
1. A method for producing polytetrafluoroethylene powder, comprising: a grinding step of grinding polytetrafluoroethylene using a grinder by setting the surface temperature of a grinding member of the grinder to less than 35°C, the grinding member being a grinding member capable of grinding the polytetrafluoroethylene, and the grinding step being carried out in a dry manner.
2. 2. The method according to claim 1, wherein in the crushing step, the polytetrafluoroethylene is crushed by at least a pair of the crushing members disposed opposite to each other.
3. 3. The method according to claim 1, wherein the polytetrafluoroethylene has a history of being heated to a temperature equal to or higher than the melting point.
4. 3. The method according to claim 1, wherein the crusher has an inlet and an outlet, and the crushing step is carried out continuously.
5. The method according to claim 1 or 2, wherein the grinding step is repeated multiple times.
6. The method according to claim 1 or 2, further comprising a coarse pulverizing step of coarsely pulverizing the polytetrafluoroethylene, and the coarse powder obtained in the coarse pulverizing step is subjected to the pulverizing step.
7. The present invention is characterized in that it contains scaly non-crosslinked polytetrafluoroethylene particles, has one or more melting points in a temperature range below 333°C, has a median diameter of 150 μm or less, and has an L measured using a test piece obtained by molding under the following conditions: * a * b * L in color system * Polytetrafluoroethylene powder having a molecular weight of 70 or more. (Molding conditions) 54 g of polytetrafluoroethylene powder is placed into a φ120 mm mold and held at 370°C for 30 minutes using a heat press to melt the polytetrafluoroethylene. A load of 3 MPa is then applied for 1 minute to perform compression molding, and the mold is cooled to prepare a test piece.
8. The polytetrafluoroethylene powder according to claim 7, having a median diameter of 110 μm or less.
9. The L measured using test pieces molded under the following conditions * a * b * L in color system * The L measured with the polytetrafluoroethylene powder * 9. The polytetrafluoroethylene powder according to claim 7 or 8, which has a rate of change of 25% or less. (Molding conditions) 54 g of polytetrafluoroethylene powder is placed into a φ120 mm mold and held at 370°C for 30 minutes using a heat press to melt the polytetrafluoroethylene. A load of 3 MPa is then applied for 1 minute to perform compression molding, and the mold is cooled to prepare a test piece.
Citation Information
Patent Citations
JP1972-043900A
Molding powder of polytetrafluoroethylene and method for producing the same
JP1996506850A
Modified fluoro resin powder and molded product thereof
JP1998316761A
PTFE (polytetrafluoroethylene) powder and process for production of powder for molding PTFE
JP2007321157A
Production method of fluorocarbon resin powders
JP2020006578A