Aluminum-based alloys

The aluminum-based alloy with controlled stress orientations and uniform grain size addresses anisotropy issues, enhancing bendability and yield strength by stabilizing stress distribution, reducing breakage during processing.

JP7575739B2Active Publication Date: 2024-10-30TOHOKU UNIV +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020145525
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-31
Publication Date
2024-10-30
Estimated Expiration
2040-08-31

AI Technical Summary

Technical Problem

Conventional aluminum-based alloys exhibit significant anisotropy in bendability and yield strength, leading to breakage during processing due to differences in surface and internal textures, with yield strength limited to 250 MPa and varying bendability in the extrusion and perpendicular directions.

Method used

An aluminum-based alloy composition with specific element ratios (Mg 0.75-1.0wt%, Si 0.3-0.8wt%, Cu 0.15-0.4wt%, Fe 0.10-0.25wt%, Cr 0.07wt% or less, Mn 0.025wt% or less) and controlled stress orientations, where the surface layer has a maximum principal stress 5°-40° to the extrusion direction and the inner layer 50° or more, with a surface layer depth of 0.10-0.15mm and inner layer depth of 0.3mm or more, achieving uniform grain size and stress distribution.

Benefits of technology

The alloy achieves reduced anisotropy in bendability, resisting breakage during processing with yield strength exceeding 270 MPa and improved bendability, maintaining consistent stress distribution and grain size across different directions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575739000002
    Figure 0007575739000002
  • Figure 0007575739000003
    Figure 0007575739000003
  • Figure 0007575739000004
    Figure 0007575739000004
Patent Text Reader

Abstract

To provide an aluminum based alloy that has small anisotropy of bendability, and is hard to be fractured during processing.SOLUTION: An aluminum based alloy has: a surface layer part which is obtained by extrusion processing, and in which the maximum main stress from a surface toward a depth direction is compression; and an inner layer part in which the maximum main stress is tensility. A direction of the maximum main stress on the surface layer part is 5° or more and 40° or less with respect to an extrusion direction of the extrusion processing, and a direction of the maximum main stress in the inner layer part is 50° or more with respect to the extrusion direction of the extrusion processing. It is preferable in the surface layer part that 80% or more of crystal grains has 150 μm or less of particle diameter, and a crystal orientation has a preferred orientation in <110> direction.SELECTED DRAWING: Figure 10
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an aluminum-based alloy. [Background technology]

[0002] Extruded aluminum-based alloys can be formed into complex cross-sectional shapes, and 6000 series aluminum-based alloys in particular have excellent extrusion workability and formability, and are used as building materials and transportation materials (see, for example, Patent Document 1). This extruded aluminum-based alloy has a large recrystallization texture that is divided into two layers, the surface and the interior, and the interior texture is as follows: <100> The crystal orientation of the alloy is Cube orientation or Goss orientation, which is parallel to the extrusion direction. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. WO2007 / 111002 Summary of the Invention [Problem to be solved by the invention]

[0004] However, conventional aluminum-based alloys such as those described in Patent Document 1 have anisotropy in bendability that differs significantly between the extrusion direction (RD) and the perpendicular direction (TD) in a range exceeding 250 MPa, due to differences in texture between the surface and interior, even if the yield strength is approximately the same. This has led to a problem of being prone to fracture during processing.

[0005] The present invention has been made in view of these problems, and has an object to provide an aluminum-based alloy that has small anisotropy in bendability and is less likely to break during processing. [Means for solving the problem]

[0006] In order to achieve the above object, the aluminum-based alloy according to the present invention is an aluminum-based alloy obtained by extrusion processing, The alloy contains 0.75 wt% to 1.0 wt% Mg, 0.3 wt% to 0.8 wt% Si, 0.15 wt% to 0.4 wt% Cu, 0.10 wt% to 0.25 wt% Fe, 0.07 wt% or less Cr, 0.025 wt% or less Mn, and the balance being Al and unavoidable impurities; The extrusion molding machine is characterized in that it has, from the surface toward the depth direction, a surface layer portion in which the maximum principal stress is compressive and an inner layer portion in which the maximum principal stress is tensile, the direction of the maximum principal stress in the surface layer portion being 5° or more and 40° or less with respect to the extrusion direction of the extrusion processing, and the direction of the maximum principal stress in the inner layer portion being 50° or more with respect to the extrusion direction of the extrusion processing.

[0007] In the aluminum-based alloy according to the present invention, the surface layer is preferably distributed to a depth of 0.10 mm to 0.15 mm from the surface. The inner layer preferably has a deepest part that is 0.3 mm or more deep from the surface. The inner layer preferably has a maximum von Mises stress (equivalent stress) of 150 MPa or more. In the surface layer, 80% or more of the crystal grains have a grain size of 150 μm or less and a crystal orientation of <110> It is preferred that the ion beam has a preferred orientation in the direction of the ion beam. Effect of the Invention

[0009] According to the present invention, it is possible to provide an aluminum-based alloy that has small anisotropy in bendability and is less likely to break during processing. [Brief description of the drawings]

[0010] [Figure 1] 1 is a process chart showing a manufacturing method of an aluminum-based alloy according to an embodiment of the present invention. [Diagram 2] FIG. 1 shows, after bending test, (a) a metallurgical microscope photograph of a test piece in the L direction, (b) a metallurgical microscope photograph of an enlarged portion of (a), (c) a test piece in the LT direction, and (d) a metallurgical microscope photograph of an enlarged portion of (c), for an aluminum-based alloy according to an embodiment of the present invention. [Diagram 3]FIG. 1 shows, after bending test, (a) a metallurgical microscope photograph of a test piece in the L direction, (b) a metallurgical microscope photograph of an enlarged portion of (a), (c) a test piece in the LT direction, and (d) a metallurgical microscope photograph of an enlarged portion of (c), for comparative examples of an aluminum-based alloy according to an embodiment of the present invention. [Figure 4] 4 is a graph showing the relationship between displacement and bending stress in a bending test for the aluminum-based alloy shown in FIG. 2 and the comparative example of the aluminum-based alloy shown in FIG. 3. [Diagram 5] 1A and 1B are inverse pole figure orientation maps (shown in black and white) illustrating crystal orientations in (a) RD and (b) TD of an aluminum-based alloy according to an embodiment of the present invention. [Figure 6] FIG. 1 shows an inverse pole figure orientation map (left side, shown in black and white) showing the crystal orientation in RD, an inverse pole figure of

[0100] (top right side, shown in black and white), and pole figures (three in the bottom right side, shown in black and white) of an aluminum-based alloy according to an embodiment of the present invention. [Figure 7] FIG. 1 shows an inverse pole figure orientation map (left side, shown in black and white) showing the crystal orientation in RD, an inverse pole figure of

[0100] (upper right side, shown in black and white), and pole figures (three in the lower right side, shown in black and white) of a comparative example of an aluminum-based alloy according to an embodiment of the present invention. [Figure 8] FIG. 1 shows an aluminum-based alloy according to an embodiment of the present invention, with (a) a perspective view showing the direction of stress components for a sample, and (b) a graph showing residual stress distribution in the depth direction, showing (σy) the extrusion direction, (σx) the perpendicular direction thereto, (c) the shear direction therebetween (σxy), (d) the maximum principal stress (σ1), (e) the minimum principal stress (σ2), and (f) the von Mises stress. [Figure 9] FIG. 1 shows a comparative example of an aluminum-based alloy according to an embodiment of the present invention, with (a) a perspective view showing the direction of stress components for the sample, and (b) the extrusion direction (σy), (b) the perpendicular direction (σx), (c) the shear direction (σxy) therebetween, (d) the maximum principal stress (σ1), (e) the minimum principal stress (σ2), and (f) a graph of the von Mises stress showing residual stress distribution in the depth direction. [Figure 10]FIG. 1A is a three-dimensional graph showing the direction of principal stress at each depth, (b) an inverse pole figure orientation map of RD (shown in black and white), and (c) a graph showing the depth distribution of von Mises stress for an aluminum-based alloy according to an embodiment of the present invention; and (d) a three-dimensional graph showing the direction of principal stress at each depth, (e) an inverse pole figure orientation map of RD (shown in black and white), and (f) a graph showing the depth distribution of von Mises stress for a comparative example of an aluminum-based alloy according to an embodiment of the present invention. [Figure 11] 11 is a graph showing the change in maximum principal stress direction with respect to depth for the aluminum-based alloy shown in FIG. 10 and a comparative example of the aluminum-based alloy. [Figure 12] FIG. 1 shows (a) an inverse pole figure orientation map showing crystal orientation at RD, (b) a KAM map, and (c) a graph showing the depth distribution of von Mises stress of an aluminum-based alloy according to an embodiment of the present invention, and (d) an inverse pole figure orientation map showing crystal orientation at RD, (e) a KAM map, and (f) a graph showing the depth distribution of von Mises stress of a comparative example of an aluminum-based alloy according to an embodiment of the present invention. [Figure 13] FIG. 1A is a graph showing the depth distribution of von Mises stress for an aluminum-based alloy according to an embodiment of the present invention; (b) a graph showing the distribution of Σ of corresponding grain boundaries at a depth of 30 μm, (c) a depth of 170 μm, and (d) a depth of 260 μm; and (e) a graph showing the depth distribution of von Mises stress for a comparative example of an aluminum-based alloy according to an embodiment of the present invention; and (f) a graph showing the distribution of Σ of corresponding grain boundaries at a depth of 30 μm, (g) a depth of 105 μm, and (h) a depth of 220 μm. [Figure 14] FIG. 1A is a graph showing the distribution of Σ of corresponding grain boundaries in the depth range of 0 to 200 μm and (b) in the depth range of 0 to 400 μm for an aluminum-based alloy according to an embodiment of the present invention; and FIG. 1D is a graph showing the distribution of Σ of corresponding grain boundaries in the depth range of 0 to 200 μm and (d) in the depth range of 0 to 400 μm for a comparative example of an aluminum-based alloy according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, the embodiment of the present invention will be described based on examples. The aluminum-based alloy according to the embodiment of the present invention is obtained by extrusion processing, and contains Mg. 0.75 % to 1.0 wt%, Si at 0.3 wt% to 0.8 wt%, Cu at 0.15 wt% to 0.4 wt%, Fe at 0.10 wt% to 0.25 wt%, Cr at 0.07 wt% or less, Mn at 0.025 wt% or less, with the remainder being Al and unavoidable impurities.

[0012] The aluminum-based alloy according to the embodiment of the present invention has, from the surface to the depth direction, a surface layer portion in which the maximum principal stress is compressive, and an inner layer portion in which the maximum principal stress is tensile. In the surface layer portion, 80% or more of the crystal grains have a grain size of 150 μm or less and a crystal orientation of <110> It has a preferred orientation in the direction.

[0013] The surface layer is distributed from the surface to a depth of 0.10 mm to 0.15 mm. The surface layer has an Euler angle of 5° to 40° with respect to the extrusion direction of the extrusion process. The surface layer has stable grain boundaries with Σ values ​​of 3 to 13 of 10% or more, and in particular, twin crystals with Σ3 of 5% or more and a crystal grain abundance ratio of 1.0 deg or less KAM average value proportional to intragranular strain of 40% or more.

[0014] The inner layer has a maximum depth of 0.3 mm or more from the surface. The inner layer has a maximum principal stress direction of 50° or more with respect to the extrusion direction of the extrusion process. The inner layer also has a maximum von Mises stress of 150 MPa or more. EXAMPLES

[0015] An aluminum-based alloy was manufactured, and bending tests, crystal orientation analysis by EBSD method, stress measurement, etc. were performed on the manufactured alloy. Two types of alloy samples having the compositions shown in Table 1 were manufactured as the aluminum-based alloy. These alloy samples are A6000 series aluminum alloys used as structural materials, with alloy sample 1 corresponding to A6061 and alloy sample 2 corresponding to A6005C. Note that alloy sample 1 is an aluminum-based alloy according to an embodiment of the present invention, and alloy sample 2 is a comparative example.

[0016] [Table 1]

[0017] As a method for producing each alloy sample, as shown in Fig. 1, the alloy raw materials adjusted to each composition in Table 1 were heated to 700°C, melted, cast, cooled, and then homogenized at 570°C for 3.7 hours. After cooling, the alloy raw materials were heated to 480-500°C and extruded, and water-cooled at 3000°C / min. Then, aging treatment was performed at 200°C for 2.5 hours to obtain each alloy sample.

[0018] A bending test was carried out on each of the manufactured alloy samples. The bending test was carried out using a three-point bending tester in accordance with JIS Z2248. The test pieces for the bending test were 60 mm long, 20 mm wide, and 2.0 mm thick. One specimen whose length was parallel to the extrusion direction (L direction) and the other whose length was perpendicular to the extrusion direction (LT direction) were cut out from each alloy sample. The bending test was also carried out while changing the radius of the indenter.

[0019] Among the alloy samples after the bending test, metallurgical microscope photographs (dark field images) of the cross sections of the test piece of alloy sample 1 in the L direction with an indenter radius of 4 mm (4R) and the test piece of the LT direction with an indenter radius of 5 mm (5R) are shown in Figure 2. Also, metallurgical microscope photographs (dark field images) of the cross sections of the test piece of alloy sample 2 in the L direction with an indenter radius of 4 mm (4R) and the test piece of the LT direction with an indenter radius of 9 mm (9R) are shown in Figure 3. As shown in Figures 2(a) and (b), it was confirmed that no cracks were generated in the bending test in the L direction of alloy sample 1. Also, as shown in Figures 2(c) and (d), it was confirmed that no cracks were generated in the bending test in the LT direction of alloy sample 1.

[0020] As shown in Figures 3(a) and (b), in the bending test of the L direction of alloy sample 2, it was confirmed that many cracks (circles in Figure 3(b)) occurred not only on the surface of the test piece but also in the range of 100 to 400 μm deep from the surface. In addition, as shown in Figures 3(c) and (d), in the LT direction of alloy sample 2, it was confirmed that the test piece was cracked during the bending test, and many cracks (circles in Figure 3(d)) also occurred inside the test piece.

[0021] The relationship between the displacement and bending stress obtained by the bending test for each test piece is shown in Figure 4. As shown in Figure 4, it was confirmed that each test piece of alloy sample 1 did not break even after the yield stress, and bending deformation continued slowly. In addition, it was confirmed that the test piece in the L direction of alloy sample 2 did not break even after the yield stress, but the bending stress dropped rapidly. In addition, it was confirmed that the test piece in the LT direction of alloy sample 2 broke near the yield stress. From the above test results, it can be said that alloy sample 1 has small anisotropy of bendability and has excellent bending workability.

[0022] Next, crystal orientation analysis was performed on each alloy sample using the EBSD method. For the crystal orientation analysis, an "OIM crystal orientation analyzer" manufactured by TSL Solutions Co., Ltd. was used. Figure 5 shows the inverse pole figure orientation map of the rolling direction (RD) and the direction perpendicular to the rolling direction in the rolling plane (TD; transverse direction) of alloy sample 1. Figure 6 shows the inverse pole figure orientation map of RD, the inverse pole figure of

[0100] , and the pole figure of alloy sample 1. Figure 7 shows the inverse pole figure orientation map of RD, the inverse pole figure of

[0100] , and the pole figure of alloy sample 2. The rolling direction is the extrusion direction during extrusion processing.

[0023] As shown in Figures 5 and 6, in alloy sample 1, more than 80% of the crystal grains were aligned in the extrusion direction from the surface to a depth of 0.5 mm in both RD and TD. <110> It was confirmed that the grains had a preferred orientation. In addition, the grain size of these grains was almost uniform and was 150 μm or less. In contrast, as shown in Figure 7, in alloy sample 2, in both RD and TD, from the surface to a depth of 0.5 mm, about 30% of the grains were almost uniform and had a grain size of 150 μm or less, and were aligned in the extrusion direction. <110> It was confirmed that the specimen had a preferred orientation. In addition, it was confirmed that many coarse grains existed in the range of 0.1 to 0.3 mm deep from the surface in both the RD and TD. This region with many coarse grains was not observed in alloy sample 1 (see Figures 5 and 6).

[0024] Next, stress measurements were performed on each alloy sample. During stress measurements, samples were cut out from the surface of each alloy sample, and the samples were immersed in a 6 vol% perchloric acid ethanol solution. The samples were sequentially electrolytically polished from the surface at 0°C and DC15V, while measuring the residual stress distribution in the depth direction from the surface. Sequential electrolytic polishing was performed for 20 minutes each, and the samples were polished about 25μm at a time from the surface. Residual stress was measured using a portable X-ray residual stress measurement device "μ-X360s" manufactured by Pulstec Industrial Co., Ltd., using the cosα method (ray source: φ2mm Cr-kα, 30kV, 1.5mA, diffraction surface: Al(311), 2θ=139.32°) while oscillating ψ, φ, and ω at 10° in three axes.

[0025] The residual stress distribution in the depth direction of alloy sample 1 is shown in FIG. 8. The residual stresses were obtained in the extrusion direction (σy), the perpendicular direction (σx), the shear direction between them (σxy), the maximum principal stress (σ1), the minimum principal stress (σ2), and the von Mises stress. Similarly to alloy sample 1, the residual stress distribution in the depth direction of alloy sample 2 is shown in FIG. 9. The directions of the principal stresses at each depth of alloy sample 1 are shown in FIG. 10(a)-(c) together with the inverse pole figure orientation maps of RD shown in FIG. 5 and FIG. 6, and the depth distribution of von Mises stress shown in FIG. 8(g). The directions of the principal stresses at each depth of alloy sample 2 are shown in FIG. 10(d)-(f) together with the inverse pole figure orientation maps of RD shown in FIG. 7, and the depth distribution of von Mises stress shown in FIG. 9(g). FIG. 11 summarizes the change in the maximum principal stress direction with respect to the depth and the extrusion direction for alloy samples 1 and 2 shown in FIG.

[0026] As shown in Figs. 8, 10 and 11, in the alloy sample 1, in the region (surface layer) up to a depth of 80 μm where the von Mises stress is small and the maximum principal stress is compressive, the Euler angle in the principal stress direction was confirmed to be 9° to 35° with respect to the extrusion direction. In addition, in the region (inner layer) deeper than 150 μm where the maximum principal stress is tensile, the Euler angle in the principal stress direction was confirmed to be 50° or more with respect to the extrusion direction. In addition, in the tensile region, it was confirmed that the maximum von Mises stress of 150 MPa or more was obtained at a depth of 170 μm. It was also confirmed that the same crystal structure and stress distribution were obtained even if the added elements Cr were reduced to 0.03 wt% and Mn to 0.01 wt%. In addition, the proof stress was 270 MPa or more in both RD and TD, and the bendability was good with R2 to 3 mm in both RD and TD, and it was confirmed that the anisotropy was small.

[0027] As shown in FIG. 9 to FIG. 11, in the alloy sample 2, in the region up to a depth of 50 μm where the von Mises stress is small and the maximum principal stress is compressive, the Euler angle in the principal stress direction was confirmed to be 15° to 70° with respect to the extrusion direction. In addition, it was confirmed that the maximum principal stress becomes tensile and the Euler angle in the principal stress direction is about 50° with respect to the extrusion direction at a depth of about 100 μm. It was confirmed that the von Mises stress was about 120 MPa at a depth of 105 μm. It was also confirmed that the maximum principal stress becomes compressive again at a depth of 150 to 250 μm and the Euler angle in the principal stress direction is 20° or less with respect to the extrusion direction. It was also confirmed that the maximum principal stress becomes tensile again at a depth of 250 μm or more and the Euler angle in the principal stress direction is 35° to 40° with respect to the extrusion direction. It was confirmed that the maximum von Mises stress was 50 MPa or more at a depth of 300 μm. The yield strength was 270 MPa or more in both RD and TD, but the bending property was R3 mm in RD and R10 mm in TD, confirming that the material has anisotropy.

[0028] 10 and 11, in alloy sample 2, the direction of the maximum principal stress changes from compression to extrusion as the depth increases, and then becomes compression again in the region where many coarse grains exist (depth 150 to 250 μm), so it is believed that the stress is released by recrystallization at this depth. In contrast, in alloy sample 1, the direction of the maximum principal stress changes from compression to extrusion as the depth increases, but does not become compression again, and no region where many coarse grains exist is observed, so it is believed that recrystallization is suppressed.

[0029] Next, the KAM maps of each alloy sample were obtained by crystal orientation analysis using the EBSD method, and are shown in Figure 12. In alloy sample 1, the KAM values ​​are distributed relatively uniformly, as shown in Figure 12(b), whereas in alloy sample 2, large KAM values ​​are concentrated in the area where many coarse grains exist, as shown in Figure 12(e). From this, it is considered that the distortion is large in the coarse grains of alloy sample 2.

[0030] Next, the correspondence grain boundary Σ, which is an index of grain boundary stability, was investigated for each alloy sample. The distribution of Σ of the correspondence grain boundary near the depth where the von Mises stress shows the peaks of compression and tension for each alloy sample was obtained by crystal orientation analysis using the EBSD method, and is shown in Figure 13. In addition, the distribution of Σ values ​​in the depth range of 0 to 200 μm and 0 to 400 μm for each alloy sample is summarized and shown in Figure 14. Comparing the distribution of Σ of alloy sample 1 in Figures 13(b) to (d) and Figures 14(a and (b) with the distribution of Σ of alloy sample 2 in Figures 13(f) to (h) and Figures 14(c and (d), it was confirmed that alloy sample 2 has more correspondence grain boundaries of Σ3, 5, and 7 than alloy sample 1 at a depth shallower than 200 μm, but that alloy sample 1 has more correspondence grain boundaries of Σ3, 5, and 7 than alloy sample 2 at a depth deeper than 200 μm. In addition, the distribution of Σ for alloy sample 1 shown in Figures 14(a) and (b) shows that the coincidence boundaries of Σ3, 5, and 7 hardly change with depth, whereas the distribution of Σ for alloy sample 2 shown in Figures 14(c) and (d) shows that the coincidence boundaries of Σ3, 5, and 7 decrease with depth. From these results, it is considered that alloy sample 1 has an interface that is more energetically stable (stronger interface) than alloy sample 2.

Claims

1. An aluminum-based alloy obtained by extrusion processing, 0.75 wt% to 1.0 wt% Mg, 0.3 wt% to 0.8 wt% Si, 0.15 wt% to 0.4 wt% Cu, 0.10 wt% to 0.25 wt% Fe, 0.07 wt% or less Cr, 0.025 wt% or less Mn, with the balance being Al and unavoidable impurities; The steel sheet has a surface layer portion in which the maximum principal stress is compressive and an inner layer portion in which the maximum principal stress is tensile, from the surface to the depth direction; The direction of the maximum principal stress in the surface layer portion is 5° or more and 40° or less with respect to the extrusion direction of the extrusion processing, and the direction of the maximum principal stress in the inner layer portion is 50° or more with respect to the extrusion direction of the extrusion processing. An aluminum-based alloy characterized by a yield strength exceeding 250 MPa.

2. 2. The aluminum-based alloy according to claim 1, wherein the inner layer is distributed to a depth of 0.3 mm or more from the surface.

3. The surface layer portion is distributed from the surface to a depth of 0.10 mm to 0.15 mm, The inner layer portion has a maximum von Mises stress of 150 MPa or more.

3. An aluminum-based alloy according to claim 1 or 2.

4. 4. The aluminum-based alloy according to claim 1, wherein 80% or more of the crystal grains in the surface layer have a grain size of 150 μm or less and a preferred crystal orientation in the <110> direction.

Citation Information

Patent Citations

  • Aluminum alloy extruded material excellent in bendability and its production

    JP1998046279A

  • Aluminum alloy extrusion profile material having excellent bending workability and production method therefor

    JP2002241880A

  • Aluminum alloy extruded hollow shape material excellent in bending workability and crush resistance

    JP2005105317A

  • Aluminum alloy extruded material having excellent bending-crashed property and corrosion resistance and method for manufacturing the same

    JP2009228111A

  • Aluminum alloy hollow-shaped material excellent in fatigue strength, and manufacturing method of the same

    JP2012172176A