Yellowing-resistant polyester and its manufacturing method

Incorporating phosphorus and metal elements into tricyclodecane dimethanol-based polyesters addresses the issue of yellowing resistance, achieving enhanced mechanical strength, heat resistance, and transmittance in polyesters for diverse applications.

JP7576005B2Active Publication Date: 2024-10-30CHANG CHUN PLASTICS CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021110835
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-02-03
Filing Date
2021-07-02
Publication Date
2024-10-30
Estimated Expiration
2041-07-02

AI Technical Summary

Technical Problem

Polyesters used in applications such as food contact materials and packaging suffer from low yellowing resistance, despite improvements in mechanical strength and heat resistance through the use of tricyclodecane dimethanol (TCDDM).

Method used

Incorporating phosphorus and specific metal elements like Ti, Sn, Sb, Ge, Mn, Zn, Ca, Co, Pb, Al, or Zr into the polyester structure, with a weight ratio of phosphorus to metal ranging from 0.05 to 5.00, and using tricyclodecane dimethanol as a key component, enhances mechanical strength, heat resistance, and yellowing resistance.

Benefits of technology

The resulting polyester exhibits high transmittance, excellent yellowing resistance, and maintains appropriate molecular weight, demonstrating improved performance in various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576005000001
    Figure 0007576005000001
  • Figure 0007576005000002
    Figure 0007576005000002
  • Figure 0007576005000003
    Figure 0007576005000003
Patent Text Reader

Abstract

To provide a tricyclodecane dimethanol polyester having high optical transmittance and yellowing resistance.SOLUTION: The polyester comprises one or more repeating units derived from polyols, and one or more repeating units derived from polybasic acids, and contains phosphorus and a metal element, where the one or more repeating units derived from polyols include a repeating unit derived from tricyclodecane dimethanol, the weight ratio of the phosphorus to the metal element ranges from 0.05 to 5.00, and the metal element is selected from the group consisting of Ti, Sn, Sb, Ge, Mn, Zn, Ca, Co, Pb, Al, Zr, and combinations thereof.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Priority claim This application claims priority to Taiwan Patent Application No. 110104076, filed on February 3, 2021, the subject matter of which is incorporated herein by reference in its entirety.

[0002] FIELD OF THEINVENTION The present application provides polyesters, particularly tricyclodecane dimethanol (TCDDM) polyesters, having high light transmittance and resistance to yellowing, and methods for making the polyesters. [Background technology]

[0003] Polyesters are widely used in the fields of food contact, packaging materials, food containers, etc. It is known that the use of tricyclodecane dimethanol (TCDDM) in the preparation of polyesters can improve the mechanical strength and heat resistance of the prepared polyesters. However, the polyester materials still have low yellowing resistance. Summary of the Invention [Means for solving the problem]

[0004] In view of the above technical problems, the present invention provides a polyester having high mechanical strength, high heat resistance, high transmittance, and excellent yellowing resistance, and a method for producing the polyester. The polyester of the present invention can be used in the fields of food contact tools, packaging materials, food containers, moldings, commercial products, household products, electrical products, equipment housings, lighting fixtures, outdoor signs, personal care applications, sporting goods, toys, etc., but the applications of the polyester of the present invention are not limited thereto.

[0005] Therefore, an object of the present invention is to provide a polyester containing one or more repeating units derived from a polyol and one or more repeating units derived from a polybasic acid, and containing phosphorus and a metal element, wherein the one or more repeating units derived from a polyol contain a repeating unit derived from tricyclodecane dimethanol, the weight ratio of phosphorus to the metal element is in the range of 0.05 to 5.00, and the metal element is selected from the group consisting of Ti, Sn, Sb, Ge, Mn, Zn, Ca, Co, Pb, Al, Zr, and combinations thereof.

[0006] In some embodiments of the present invention, the amount of repeat units derived from tricyclodecane dimethanol is 10 mole % or more, based on the total moles of one or more repeat units derived from the polyol.

[0007] In some embodiments of the present invention, phosphorus is phosphorus(III), phosphorus(V), or a combination thereof.

[0008] In some embodiments of the present invention, the metallic element is selected from the group consisting of Ti, Sn, Ge, Sb, and combinations thereof.

[0009] In some embodiments of the present invention, the amount of phosphorus is 3 ppm to 200 ppm based on the total weight of the polyester, and the amount of the metal element is 5 ppm to 500 ppm based on the total weight of the polyester.

[0010] In some embodiments of the present invention, one or more repeating units derived from a polyol further comprises: JPEG0007576005000001.jpg1530 [wherein R1 is C2 to C 17 The repeating units may be linear or branched, and may include one or more repeating units of the formula:

[0011] In some embodiments of the present invention, one or more repeat units derived from a polybasic acid JPEG0007576005000002.jpg2030 [wherein R2 is C4 to C 16The repeating unit is selected from the repeating units represented by the formula:

[0012] Another object of the present invention is to provide a method for producing the above polyester, which comprises polymerizing a polyol component with a polybasic acid component in the presence of phosphorus and a metal element, wherein the polyol component comprises tricyclodecane dimethanol and has a carbonyl value of less than 0.15 mg KOH / g.

[0013] In order to make the above-mentioned objects, technical features and advantages of the present invention more apparent, the present invention will be described in detail below with reference to several embodiments. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Several embodiments of the present invention are described in detail below, however, the present invention may be embodied in various embodiments and the scope of the invention for which protection is sought should not be limited to the embodiments described herein.

[0015] Unless otherwise explained, the expressions "a," "the," and the like in the specification and claims are intended to include both the singular and the plural forms.

[0016] Unless additionally explained, when describing components in a solution, mixture or composition herein, the amount of each component is calculated on a dry weight basis, i.e., without considering the weight of the solvent.

[0017] As used herein, tricyclodecane dimethanol (TCDDM) polyesters refer to polyesters that contain repeat units derived from TCDDM. The polyesters may or may not further contain one or more repeat units derived from other polyols (e.g., diols). In some embodiments of the present invention, the polyesters of the present invention contain repeat units derived from TCDDM and one or more repeat units derived from other polyols (e.g., diols).

[0018] The effects of the present invention are particularly in that the polyester has high heat resistance, high transmittance and excellent yellowing resistance.The polyester of the present invention and the method for producing the same are described in detail below.

[0019] 1. Polyester The polyester of the present invention contains phosphorus and a metal element. The main chain of the polyester contains one or more repeating units derived from a polyol and one or more repeating units derived from a polybasic acid, or consists essentially of one or more repeating units derived from a polyol and one or more repeating units derived from a polybasic acid. A detailed description of the components of the polyester of the present invention is provided below.

[0020] 1.1. Repeating units derived from polyols The polyesters of the present invention include one or more repeating units derived from a polyol, and the one or more repeating units derived from a polyol include a repeating unit derived from tricyclodecane dimethanol (TCDDM). In some embodiments of the present invention, the repeating unit derived from tricyclodecane dimethanol is JPEG0007576005000003.jpg22164 etc. JPEG0007576005000004.jpg1954, or two or more of these structures, but the present invention is not limited thereto. Without being bound by theory, it is believed that the repeating units derived from tricyclodecane dimethanol can provide the effect of improving the mechanical strength and heat resistance of the polyester.

[0021] In some embodiments of the present invention, the amount of repeating units derived from tricyclodecane dimethanol is preferably 10 mol% or more, particularly 15 mol% to 90 mol%, and more particularly 20 mol% to 80 mol%, based on the total moles of one or more repeating units derived from polyol. For example, the amount of repeating units derived from tricyclodecane dimethanol based on the total moles of one or more repeating units derived from polyol is 21 mol%, 22 mol%, 23 mol%, 24 mol%, 25 mol%, 26 mol%, 27 mol%, 28 mol%, 29 mol%, 30 mol%, 31 mol%, 32 mol%, 33 mol%, 34 mol%, 35 mol%, 36 mol%, 37 mol%, 38 mol%, 39 mol%, 40 mol%, 41 mol%, 42 mol%, 43 mol%, 44 mol%, 45 mol%, 46 mol%, 47 mol%, 48 mol%, 49 mol%, 50 mol%, 51 mol%, 52 mol%, 53 mol%, 54 mol%, 55 mol%, 56 mol%, 57 mol%, 58 mol%, 59 mol%, 60 mol%, 61 mol%, 62 mol%, 63 mol%, 64 mol%, 65 mol%, 66 mol%, 67 mol%, 68 mol%, 69 mol%, 70 mol%, 71 mol%, 72 mol%, 73 mol%, 74 mol%, 75 mol%, 76 mol%, 77 mol%, 78 mol%, 79 mol%, 80 mol%, 81 mol%, 82 mol%, 83 mol%, 84 mol%, 85 mol%, 86 8 mol%, 49 mol%, 50 mol%, 51 mol%, 52 mol%, 53 mol%, 54 mol%, 55 mol%, 56 mol%, 57 mol%, 58 mol%, 59 mol%, 60 mol%, 61 mol%, 62 mol%, 63 mol%, 64 mol%, 65 mol%, 66 mol%, 67 mol%, 68 mol%, 69 mol%, 70 mol%, 71 mol%, 72 mol%, 73 mol%, 74 mol%, 75 mol%, 76 mol%, 77 mol%, 78 mol%, or 79 mol%, or within a range between any two of these listed values. In some embodiments of the present invention, based on the total moles of repeat units derived from polyol, the amount of repeat units derived from tricyclodecane dimethanol is 30 mol% to 80 mol%, more particularly 40 mol% to 70 mol%. When the amount of the repeating unit derived from tricyclodecane dimethanol is within the above range, the polyester provided thereby can have excellent mechanical strength and heat resistance.

[0022] Optionally, the polyester of the present invention can further include one or more repeat units derived from a polyol other than TCDDM. For example, the polyester of the present invention can further include one or more repeat units derived from a diol other than TCDDM. The diol can be, for example, a C2-C7 diol. Examples of C2-C7 diols include ethylene glycol, propylene glycol, 2-methyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol, 2-butyl-2-ethyl-1,3-propanediol, butylene glycol, pentylene glycol, 3-methyl-1,5-pentanediol, hexylene glycol, heptylene glycol, octylene glycol, 1,4-cyclohexanedimethanol, pentacyclo[6.5.1.1 3-6 .0 2-7 .0 9-13 ]pentadecanedimethanol, and pentacyclo[9.2.1.1 4-7 .0 2-10 .0 3-8]pentadecanedimethanol. In some embodiments of the present invention, the polyester further comprises one or more repeat units derived from a C2-C9 linear or branched diol or 1,4-cyclohexanedimethanol. Examples of C2-C9 linear or branched diols include, but are not limited to, ethylene glycol, propylene glycol, 2-methyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol, 2-butyl-2-ethyl-1,3-propanediol, butylene glycol, pentylene glycol, 3-methyl-1,5-pentanediol, hexylene glycol, heptylene glycol, and octylene glycol. In some embodiments of the present invention, the polyester further comprises one or more repeat units derived from a C2-C6 linear diol. Examples of C2-C6 linear diols include, but are not limited to, ethylene glycol, propylene glycol, butylene glycol, pentylene glycol, and hexylene glycol. In some embodiments of the present invention, the polyester of the present invention further comprises one or more repeat units derived from a C2-C4 linear diol. Examples of C2-C4 linear diols include, but are not limited to, ethylene glycol, propylene glycol, and butylene glycol. In the accompanying examples, the polyester of the present invention further comprises a repeat unit derived from ethylene glycol.

[0023] Thus, in some embodiments of the present invention, one or more repeat units derived from a polyol further comprises: JPEG0007576005000005.jpg1530 [wherein R1 is C2 to C 17 Linear or branched hydrocarbyl groups, or C3-C 17 It is a cyclic or bridged polycyclic hydrocarbyl group. It contains one or more repeating units represented by the formula: 17 Examples of linear or branched hydrocarbyl groups include C2-C 17 Contains linear or branched alkenes. C3-C 17Examples of cyclic or bridged polycyclic hydrocarbyl groups include C3-C 17 Includes cyclic or bridged polycyclic alkyl. C2-C 17 Examples of linear or branched alkenes include ethylene, propylene, butylene, pentylene, hexylene, heptylene, octylene, JPEG0007576005000006.jpg20165 (wherein * indicates the bonding position). 17 Examples of cyclic or bridged polycyclic alkyls include cyclohexanedimethyl: JPEG0007576005000007.jpg1538, Pentacyclo[6.5.1.1 3-6 .0 2-7 .0 9-13 ]Pentadecane dimethyl: JPEG0007576005000008.jpg1553, and Pentacyclo[9.2.1.1 4-7 .0 2-10 .0 3-8 ]Pentadecane dimethyl: In some embodiments of the present invention, one or more repeat units derived from a polyol further include, but are not limited to, JPEG0007576005000010.jpg1530 [wherein R1 is a C2 to C9 linear or branched alkylene or cyclic alkyl, for example, ethylene, propylene, butylene, pentylene, hexylene, heptylene, octylene, JPEG0007576005000011.jpg41158 (wherein * indicates a bond position). In some embodiments of the present invention, the one or more repeating units derived from a polyol further include one or more repeating units represented by: JPEG0007576005000012.jpg1530 (wherein R1 is a C2-C6 linear or branched alkylene, such as ethylene, propylene, butylene, pentylene, or hexylene.) In some embodiments of the present invention, the one or more repeating units derived from a polyol further include JPEG0007576005000013.jpg1530, where R1 is a C2-C4 linear or branched alkylene, such as ethylene, propylene, or butylene. In the accompanying examples, the polyol-derived repeating unit further comprises: JPEG0007576005000014.jpg1530 (wherein R1 is ethylene).

[0024] 1.2. Repeating units derived from polybasic acids The polyester of the present invention contains one or more repeating units derived from a polybasic acid. Examples of the one or more repeating units derived from a polybasic acid include repeating units derived from a polybasic acid. Examples of the polybasic acid include C6 to C 18 Dicarboxylic acids, for example, include, but are not limited to, adipic acid, sebacic acid, phthalic acid, isophthalic acid, terephthalic acid, and naphthalenedicarboxylic acid.

[0025] In some embodiments of the present invention, one or more repeat units derived from a polybasic acid are JPEG0007576005000015.jpg2030 [wherein R2 is C4 to C 16 Linear or branched hydrocarbyl groups, and C4-C 16 C4-C, including cyclic or polycyclic hydrocarbyl groups 16 is a hydrocarbyl group. 16 Examples of linear or branched hydrocarbyl groups include C4-C 16 Includes straight or branched chain alkylene. C4-C 16 Examples of cyclic or polycyclic hydrocarbyl groups include C4-C 16 Includes cyclic or polycyclic aryl. C4-C 16 Examples of linear or branched alkylene include, but are not limited to, butylene and octylene. 16Examples of cyclic or polycyclic aryl include, but are not limited to, phenylene and naphthalene. In some embodiments of the present invention, one or more repeat units derived from a polybasic acid further comprises: JPEG0007576005000016.jpg3897 [wherein R3 is C3 to C 20 R4, R5 and R6 are independently a C1 to C6 hydrocarbyl group. n1, n2, n3, n4, n5 and n6 are independently 0 or 1. And, * indicates a bonding position.] is included as one or more repeating units. The amount of repeating units represented by JPEG0007576005000017.jpg3897 is 0.7% or less, based on the total number of repeating units of the polyester.

[0026] 1.3. Phosphorus The polyester of the present invention contains phosphorus as an essential component. The weight ratio of phosphorus to the metal elements shown below is between 0.05 and 5.00. For example, the weight ratio of phosphorus to the metal elements shown below is 0.06, 0.07, 0.08, 0.09, 0.10, 0.15, 0.20, 0.25, 0.30, 0.35, 0.40, 0.45, 0.50, 0.55, 0.60, 0.65, 0.70, 0.75, 0.80, 0.85, 0.90, 0.95, 1.00, 1. 05, 1.10, 1.15, 1.20, 1.25, 1.30, 1.35, 1.40, 1.45, 1.50, 1.55, 1.60, 1.65, 1.70, 1.75, 1.80, 1.85, 1.90, 1.95, 2.00, 2.05, 2.10, 2.15, 2.20, 2.25, 2.30, 2.35, 2.40, 2.45 ,2.50,2.55,2.60,2.65,2.70,2.75,2.80,2.85,2.90,2.95,3.00,3.05,3.10,3.15,3.20,3.25,3.30,3.35,3.40,3.45,3.50,3.55,3.60,3.65,3.70,3.75,3.80,3.85,3 The weight ratio of phosphorus to metal element may be 0.90, 3.95, 4.00, 4.05, 4.10, 4.15, 4.20, 4.25, 4.30, 4.35, 4.40, 4.45, 4.50, 4.55, 4.60, 4.65, 4.70, 4.75, 4.80, 4.85, 4.90 or 4.95, or within a range between any two of these listed values. If the weight ratio of phosphorus to metal element is lower than the lower limit of the above range, the polyester prepared will have low yellowing resistance. If the weight ratio of phosphorus to metal element is higher than the upper limit of the above range, the polymerization efficiency will be low, and the polyester will not have an acceptable molecular weight, resulting in low mechanical strength.

[0027] The phosphorus in the polyester of the present invention can be in elemental form or in oxidized form. That is, the oxidation number of phosphorus can be 0 or more. In some embodiments of the present invention, the phosphorus is phosphorus(III). In some embodiments of the present invention, the phosphorus is phosphorus(V). In some embodiments of the present invention, the phosphorus is a combination of phosphorus(III) and phosphorus(V). Surprisingly, it has been found that polyesters containing phosphorus(III) have better transmittance and yellowing resistance. Therefore, the phosphorus in the polyester of the present invention preferably comprises phosphorus(III).

[0028] The source of phosphorus in the polyester of the present invention is not particularly limited and includes any phosphorus-containing component. For example, at least one of phosphoric acid (H3PO4), sodium dihydrogen phosphate (H2NaPO4), and trimethyl phosphate (TMPA) can be added to the raw material for producing the polyester as a source of phosphorus (V). At least one of tris(nonylphenyl)phosphite (e.g., product numbered AO 1178, Chang Chun Petrochemical Co., Ltd., Taiwan), tris(2,4-di-tert-butylphenyl)phosphite (e.g., product numbered 2112, Chang Chun Petrochemical Co., Ltd., Taiwan), tetrakis(2,4-di-tert-butylphenyl)-4,4'-biphenyl diphosphonite (e.g., product numbered PEPQ, Clariant Corporation, Switzerland), dioctadecyl pentaerythritol bis(phosphite) (e.g., product numbered PEP-8T, Chang Chun Petrochemical Co., Ltd., Taiwan), and bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite (e.g., product numbered PEP-36, ADEKA Corporation, Japan) can be added to the raw material for producing polyester as a source of phosphorus (III). However, the present invention is not limited to these.

[0029] The amount of phosphorus in the polyester of the present invention can be adjusted as necessary. In some embodiments of the present invention, based on the total weight of the polyester, the amount of phosphorus in the polyester is preferably 3 ppm to 200 ppm, more particularly 5 ppm to 150 ppm. For example, based on the total weight of the polyester, the amount of phosphorus in the polyester can be 10 ppm, 15 ppm, 20 ppm, 25 ppm, 30 ppm, 35 ppm, 40 ppm, 45 ppm, 50 ppm, 55 ppm, 60 ppm, 65 ppm, 70 ppm, 75 ppm, 80 ppm, 85 ppm, 90 ppm, 95 ppm, 100 ppm, 105 ppm, 110 ppm, 115 ppm, 120 ppm, 125 ppm, 130 ppm, 135 ppm, 140 ppm or 145 ppm, or within a range between these two values. In the accompanying examples, the amount of phosphorus in the polyester is from 15 ppm to 75 ppm, based on the total weight of the polyester.

[0030] 1.4. Metal elements The polyester of the present invention contains a metal element as an essential component. The metal element is selected from the group consisting of Ti, Sn, Sb, Ge, Mn, Zn, Ca, Co, Pb, Al, Zr, and combinations thereof, and is preferably selected from the group consisting of Ti, Sn, Ge, Sb, and combinations thereof. In addition, the ratio of the metal element to phosphorus in the polyester is as described above.

[0031] The metal elements in the polyesters of the present invention can be in elemental or oxidized form, i.e., the oxidation number of the metal element can be zero or higher.

[0032] The source of the metal element is not particularly limited, and can be various components containing the metal element, such as an oxide or salt of the metal element. For example, titanium butoxide (e.g., product number TBT, Dorf&Ketal) or titanium isopropoxide (e.g., product number AQ-5000, Borica) can be added to the raw material for the production of polyester as a source of titanium. Butyltin tris(2-ethylhexanoate) can be added to the raw material for the production of polyester as a source of tin. Antimony oxide (Sb2O3) or antimony acetate (Sb(OAc)3) can be added to the raw material for the production of polyester as a source of antimony. Germanium oxide (GeO2) can be added to the raw material for the production of polyester as a source of germanium. However, the present invention is not limited thereto.

[0033] The amount of metal element in the polyester of the present invention can be adjusted as necessary. In some embodiments of the present invention, based on the total weight of the polyester, the amount of metal element in the polyester is 5 ppm to 500 ppm, more particularly 8 ppm to 200 ppm. For example, based on the total weight of the polyester, the amount of metal element in the polyester is 9 ppm, 10 ppm, 11 ppm, 12 ppm, 13 ppm, 14 ppm, 15 ppm, 20 ppm, 25 ppm, 30 ppm, 35 ppm, 40 ppm, 45 ppm, 50 ppm, 55 ppm, 60 ppm, 65 ppm, 70 ppm, 75 ppm, 80 ppm, 85 ppm, 90 ppm, 95 ppm , 100 ppm, 105 ppm, 110 ppm, 115 ppm, 120 ppm, 125 ppm, 130 ppm, 135 ppm, 140 ppm, 145 ppm, 150 ppm, 155 ppm, 160 ppm, 165 ppm, 170 ppm, 175 ppm, 180 ppm, 185 ppm, 190 ppm or 195 ppm, or within a range between any two of these recited values. In the accompanying examples, based on the total weight of the polyester, the amount of metal element is 8 ppm to 200 ppm.

[0034] In some embodiments of the present invention, the metal element is Sn. Based on the total weight of the polyester, the amount of Sn in the polyester is 30 ppm to 300 ppm, more particularly 50 ppm to 200 ppm. For example, based on the total weight of the polyester, the amount of Sn in the polyester can be 55 ppm, 60 ppm, 65 ppm, 70 ppm, 75 ppm, 80 ppm, 85 ppm, 90 ppm, 95 ppm, 100 ppm, 105 ppm, 110 ppm, 115 ppm, 120 ppm, 125 ppm, 130 ppm, 135 ppm, 140 ppm, 145 ppm, 150 ppm, 155 ppm, 160 ppm, 165 ppm, 170 ppm, 175 ppm, 180 ppm, 185 ppm, 190 ppm or 195 ppm, or within the range between these two values. In the attached example, the amount of the metallic element Sn is 60 ppm.

[0035] In some embodiments of the present invention, the metal element is Ge. Based on the total weight of the polyester, the amount of Ge in the polyester is 100 ppm to 400 ppm, more particularly 150 ppm to 300 ppm. For example, based on the total weight of the polyester, the amount of Ge in the polyester can be 155 ppm, 160 ppm, 165 ppm, 170 ppm, 175 ppm, 180 ppm, 185 ppm, 190 ppm, 195 ppm, 200 ppm, 205 ppm, 210 ppm, 215 ppm, 220 ppm, 225 ppm, 230 ppm, 235 ppm, 240 ppm, 245 ppm, 250 ppm, 255 ppm, 260 ppm, 265 ppm, 270 ppm, 275 ppm, 280 ppm, 285 ppm, 290 ppm, or 295 ppm, or within a range between any two of these recited values.

[0036] In some embodiments of the present invention, the metal element is Ti. Based on the total weight of the polyester, the amount of Ti in the polyester is 5 ppm to 100 ppm, more particularly 10 ppm to 50 ppm. For example, based on the total weight of the polyester, the amount of Ti in the polyester can be 11 ppm, 12 ppm, 13 ppm, 14 ppm, 15 ppm, 20 ppm, 25 ppm, 30 ppm, 35 ppm, 40 ppm, or 45 ppm, or within a range between these two values. In the accompanying examples, the amount of the metal element Ti is 10 ppm to 15 ppm.

[0037] In some embodiments of the present invention, the metal element is Sb. The amount of Sb in the polyester is from 100 ppm to 400 ppm, more particularly from 150 ppm to 300 ppm, based on the total weight of the polyester. For example, based on the total weight of the polyester, the amount of Sb in the polyester can be 155 ppm, 160 ppm, 165 ppm, 170 ppm, 175 ppm, 180 ppm, 185 ppm, 190 ppm, 195 ppm, 200 ppm, 205 ppm, 210 ppm, 215 ppm, 220 ppm, 225 ppm, 230 ppm, 235 ppm, 240 ppm, 245 ppm, 250 ppm, 255 ppm, 260 ppm, 265 ppm, 270 ppm, 275 ppm, 280 ppm, 285 ppm, 290 ppm, or 295 ppm, or within a range between two of these recited values. In the accompanying examples, the amount of metallic element Sb is 200 ppm.

[0038] 2. Polyester manufacturing method The present application also provides a method for producing a polyester, which can be produced by polymerizing a polyol component with a polybasic acid component in the presence of the phosphorus and metal elements, wherein the polyol component comprises tricyclodecane dimethanol and any one or more polyols other than tricyclodecane dimethanol, the polybasic acid component comprises one or more polybasic acids, and the polyol component has a carbonyl value of less than 0.15 mg KOH / g.

[0039] In some embodiments of the present invention, the polyester is produced by subjecting a polyol containing tricyclodecane dimethanol and a polybasic acid component to an esterification and condensation polymerization reaction in the presence of phosphorus and a metal element. In particular, the method for producing a polyester of the present invention can include the following steps (a) to (c). Step (a) A step of mixing tricyclodecane dimethanol, a polybasic acid component, and any other polyol to produce a mixture. Step (b) A step of heating the mixture under appropriate pressure conditions to carry out an esterification reaction to produce an oligomer. Step (c) A step of heating the mixture containing the oligomer while removing unreacted monomers using a vacuum pump to carry out a condensation reaction of the oligomer to obtain the polyester of the present invention. The component containing a metal element can be added in step (a), (b) or (c), and the component containing phosphorus can be added in step (a), (b) or (c).

[0040] In the above reaction, the reaction temperature and pressure conditions are not particularly limited, and a person skilled in the art can select appropriate conditions based on the disclosure of this specification and the prior art. For example, in some embodiments of the present invention, the reaction temperature in step (b) can be 220°C to 270°C. The reaction pressure in step (b) can be 0 atm to 6 atm, preferably 0 atm to 4 atm. The reaction temperature in step (c) can be 250°C to 300°C. The reaction pressure in step (c) can be 3 Torr or less, preferably 1 Torr or less.

[0041] In the above reaction, the polyol component, including tricyclodecane dimethanol and any other polyols, has a carbonyl value of less than 0.15 mg KOH / g, preferably less than 0.03 mg KOH / g, and more preferably 0 mg KOH / g (i.e., an instrumentally unmeasurable carbonyl value). The carbonyl value can be achieved by subjecting the reactants to a purification step prior to the polymerization reaction. Examples of purification steps include the following methods:

[0042] Method I: A method in which a fixed bed equipped with a circulation pipe and a circulation pump is prepared, the fixed bed is filled with a transition metal hydrogenation catalyst, preferably a Group VIIIB hydrogenation catalyst, more preferably a catalyst containing a transition metal such as Ni, Pd, Rh or Pt, and then hydrogen is introduced into the fixed bed. The polyol component to be purified is caused to flow through the circulation pipe, and circulation hydrogenation is repeated in which the back pressure of the system is preferably 5 bar to 100 bar, more preferably 10 bar to 30 bar, and the temperature of the system is preferably 0°C to 200°C, more preferably 60°C to 150°C.

[0043] Method II: The polyol component to be purified is added to a round-bottom flask, and 1 ppm to 1000 ppm, preferably 10 ppm to 100 ppm, of p-toluenesulfonic acid (PTSA) is added thereto based on the total weight of the polyol component, and the temperature is raised to 80°C, and the mixture is stirred continuously for 30 minutes, and then the pressure of the system is adjusted to 2 torr to 10 torr by a vacuum pump, and the temperature is raised to the boiling point of the polyol component, and the polyol component is distilled out of the system. For example, TCDDM can be distilled out of the system at 172°C to 180°C and 2 torr.

[0044] Method III: A method in which the polyol component to be purified is added to a high-pressure autoclave, and a catalyst is added thereto, the catalyst being a transition metal catalyst, preferably a Group VIIIB catalyst, more preferably a catalyst containing a transition metal such as Ni, Pd, Rh or Pt, and the amount of the catalyst is 10 ppm to 10,000 ppm, preferably 100 ppm to 5,000 ppm, based on the total weight of the polyol component, and then the reaction is carried out at a pressure of 20 bar to 100 bar for 2 hours to 10 hours, for example, 3 hours, to complete the purification. EXAMPLES

[0045] 3. Working Example Test Method The present invention will be further described in the following embodiments. The test apparatus and test method are as follows.

[0046] [Carbonyl value test] The carbonyl value test is carried out using an automatic titration device equipped with an electrode and a stirrer, and the amount of carbonyl groups per gram of sample is calculated. The test method is as follows: 50 g of sample is added to a beaker, 10 ml of 0.1 N NH2OH·HCl is added to the beaker, and the sample solution is stirred with a stirrer until the components of the resulting sample solution are well mixed, and then the sample solution is titrated with 0.05 N KOH solution, and the titration volume at the first equilibrium point (pH<5) is recorded, and the result is compared with the titration of the blank, and the carbonyl value is calculated according to the following formula: Carbonyl number (mgKOH / g) = ((AB) x N x 56.11) / W (Where A is the amount of KOH solution (unit: ml) used in titrating the sample. B is the amount of KOH solution (unit: ml) used in titrating the blank. N is the normal concentration (i.e., normality) of the KOH solution. W is the weight of the sample (unit: g).)

[0047] [Viscosity test] The prepared samples are subjected to viscosity testing according to ASTM D4603. The viscosity is recorded as IV (Inherent Viscosity). The lower the IV value, the lower the molecular weight of the polyester.

[0048] [Measurement of phosphorus and metal element content] The amount of phosphorus and metal elements is measured by plasma optical emission spectrometer (ICP-OES) according to US EPA 3052 microwave digestion. In order to reach the accuracy of 1mg / kg, a calibration curve is made using phosphorus standard and metal element standard before measurement. The test method is as follows: The prepared polyester is cut into 2mm x 2mm pieces, 0.2g of the cut polyester is weighed as a sample, the sample is added to a digestion vessel, 3ml of HNO3 (concentration: 70%), 9ml of HCl (concentration: 31%) and 3ml of HF (concentration: 40%) are added therein, the digestion vessel is placed in a microwave digestion device, and the digestion is carried out until the sample is completely dissolved, then after the digestion vessel is cooled to room temperature, the sample is quantified to 25ml with pure water, and the amount of phosphorus and metal elements is analyzed by plasma optical emission spectrometer.

[0049] [Yellowing resistance test] b in Lab color space for polyester * The YI (Yellowness Index) value of polyester is measured according to ASTM D6290. * The higher the YI value, the less resistant the polyester is to yellowing.

[0050] [Transmittance test] A polyester sample of 60 mm x 60 mm x 2 mm is prepared with an injection molding machine (Injection Molding Machine V90, Year-Chance Machinery Co., Ltd., Taiwan). The total transmittance of the polyester sample is measured with a Nippon Denshoku NH5000 haze meter and recorded as the TT% value. The higher the TT% value, the better the transmittance.

[0051] 3.2. List of raw materials used in the examples and comparative examples [Table 1]

[0052] 3.3. Preparation and properties of polyesters 3.3.1. Examples 1 to 5 and Comparative Examples 1 to 9: Preparation of Polyesters [Example 1] 393g of TCDDM, 279g of EG, 830g of PTA, 0.14g of H3PO4 and 0.131g of TBT were added to a high-pressure autoclave and stirred uniformly at a stirring speed of 150 rpm to produce a mixture. The polyol component in the resulting mixture has a carbonyl value of less than 0.03. The pressure of the high-pressure autoclave was then set to 4 atmospheres. The temperature was slowly raised from room temperature to 220°C to carry out an esterification reaction. After the amount of water produced in the esterification reaction reached 90% of the theoretical value of water, the temperature of the high-pressure autoclave was raised to 250°C and the vacuum pump was operated for 30 minutes. The temperature of the high-pressure autoclave was then maintained at 280°C to carry out a condensation reaction. After the reaction was completed, the temperature of the high-pressure autoclave was lowered and the polyester product was collected.

[0053] [Example 2] H3PO4 was replaced with 0.143 g of H2NaPO4, and TBT was replaced with 0.376 g of BuSn(OOC8H 15 A polyester was prepared according to the preparation method of Example 1, except that 3) was changed.

[0054] [Example 3] A polyester was prepared according to the preparation method of Example 1, except that the amount of H3PO4 was changed to 0.092 g and TBT was changed to 0.604 g of Sb(OAc)3.

[0055] [Example 4] A polyester was prepared according to the preparation method of Example 1, except that H3PO4 was replaced with 2.051 g of AO 1178.

[0056] [Example 5] A polyester was prepared according to the preparation method of Example 1, except that the H3PO4 was replaced with 0.377 g of PEP-36 and the polyol component used had a carbonyl number of 0.11.

[0057] [Comparative Example 1] A polyester was prepared according to the preparation method of Example 1, except that no TCDDM was used, the amount of EG was changed to 403 g, and H3PO4 was changed to 0.295 g of PEP-36.

[0058] [Comparative Example 2] A polyester was prepared according to the preparation method of Example 1, except that H3PO4 was not used and the amount of TBT was changed to 0.087 g.

[0059] [Comparative Example 3] A polyester was prepared according to the preparation method of Example 3, except that H3PO4 was replaced with 0.048 g of H2NaPO4.

[0060] [Comparative Example 4] The amount of H3PO4 was changed to 5g and TBT was replaced with 0.627g of BuSn(OOC8H 15A polyester was prepared according to the preparation method of Example 1, except that 3) was changed.

[0061] [Comparative Example 5] A polyester was prepared according to the preparation method of Example 1, except that H3PO4 was replaced with 1.256 g of PEP-36.

[0062] [Comparative Example 6] A polyester was prepared according to the preparation method of Example 5, except that no PEP-36 was used.

[0063] [Comparative Example 7] A polyester was prepared according to the preparation method of Example 1, except that H3PO4 was replaced with 0.126 g of PEP-36 and TBT was replaced with 0.302 g of Sb(OAc)3.

[0064] [Comparative Example 8] A polyester was prepared according to the preparation method of Example 1, except that H3PO4 was replaced with 4.103 g of AO 1178 and TBT was replaced with 0.091 g of Sb(OAc)3.

[0065] [Comparative Example 9] A polyester was prepared according to the preparation method of Example 3, except that the amount of Sb(OAc)3 was changed to 1.207 g.

[0066] 3.3.2. Examples 1 to 5 and Comparative Examples 1 to 9: Properties of Polyester The amount of phosphorus, the amount of metal element, the weight ratio of phosphorus to metal element (P / M ratio) of the polyesters of Examples 1 to 5 and Comparative Examples 1 to 9, * The properties including the value, YI value, TT% value, and IV value were tested according to the above-mentioned test methods, and the results are shown in Tables 2-1 and 2-2.

[0067] [Table 2-1]

[0068] [Table 2-2]

[0069] As shown in Tables 2-1 and 2-2, the polyester of the present invention can be produced within a suitable polymerization time, and the polyester of the present invention has a suitable molecular weight and good yellowing resistance and transmittance. In particular, Examples 1 to 5 show that polyesters having the above-mentioned excellent properties can be provided using different phosphorus-containing compounds (P) and metal element-containing compounds (M) as long as the P / M ratio is within the specified range of the present invention. Comparative Example 1 shows that polyesters prepared without TCDDM have low yellowing resistance. Comparative Examples 2 to 4, 6 to 7 and 9 show that polyesters prepared using P / M ratios lower than the specified range of the present invention have low yellowing resistance and transmittance. Comparative Examples 5 and 8 show that P / M ratios higher than the specified range of the present invention inhibit the polymerization of polyester. As a result, polyesters cannot be synthesized well (Comparative Example 8) or the obtained polyesters do not have a suitable molecular weight (Comparative Example 5, IV value is too low) and therefore have low strength.

[0070] 3.3.3. Examples 6 to 12 and Comparative Examples 10 and 11: Preparation of Polyesters The polyester products of Examples 6 to 12 and Comparative Examples 10 and 11 were prepared using the same TCDDM, EG and PTA blending composition, but adjusting the ratio and type of phosphorus and metal elements as shown in Tables 2-3 and 2-4. In particular, each component was added to a high-pressure autoclave and stirred at a stirring speed of 250 rpm to produce a mixture. The polyol component in the mixture has a carbonyl value of less than 0.03. The pressure of the high-pressure autoclave was then set to 2 atmospheres. The temperature was slowly raised from room temperature to 240°C to carry out the esterification reaction. After the amount of water produced in the esterification reaction reached 90% of the theoretical value of water, the temperature of the high-pressure autoclave was raised to 260°C and the vacuum pump was operated for 30 minutes. The temperature of the high-pressure autoclave was then maintained at 280°C to carry out the condensation reaction. After the reaction was completed, the temperature of the high-pressure autoclave was lowered and the polyester product was collected.

[0071] 3.3.4. Examples 6 to 12 and Comparative Examples 10 and 11: Properties of Polyester Weight ratio of phosphorus to metal element (P / M ratio) of polyesters in Examples and Comparative Examples, b * The properties including the value, YI value, and TT% value were tested according to the test methods described above, and the results are shown in Tables 2-3 and 2-4.

[0072] [Table 2-3]

[0073] [Table 2-4]

[0074] As further shown in Tables 2-3 and 2-4, when the P / M ratio is within the specified range of the present invention, the polyesters containing phosphorus (III) (Examples 6-10) have better yellowing resistance than the polyesters containing phosphorus (V) (Examples 11 and 12). Furthermore, when the P / M ratio is not within the specified range of the present invention, the polyesters have poor yellowing resistance, regardless of whether phosphorus (V) is used (Comparative Example 10) or phosphorus (III) is used (Comparative Example 11).

[0075] The above embodiments are used to explain the principles and effects of the present invention and to illustrate its inventive features, but are not used to limit the scope of the present invention. Those skilled in the art can make various modifications and replacements based on the disclosure and suggestions of the invention described. Therefore, the protection scope of the present invention is defined in the appended claims.

Claims

1. A polyester containing one or more repeating units derived from a polyol and one or more repeating units derived from a polybasic acid, and containing phosphorus and a metal element, one or more of the repeat units derived from a polyol include a repeat unit derived from tricyclodecane dimethanol; The weight ratio of phosphorus to metal element is in the range of 0.50 to 4.86; the phosphorus comprises phosphorus(III); The metal element is Ti; A polyester having an amount of phosphorus of from 5 ppm to 200 ppm based on the total weight of the polyester.

2. 2. The polyester of claim 1, wherein the amount of repeat units derived from tricyclodecane dimethanol is 10 mole percent or greater, based on the total moles of the one or more repeat units derived from the polyol.

3. 2. The polyester of claim 1, wherein the phosphorus further comprises phosphorus(V).

4. The polyester of claim 1, wherein the amount of the metal element is from 5 ppm to 500 ppm based on the total weight of the polyester.

5. The one or more repeat units derived from a polyol further include [In the formula, R 1 is C 2 ~C 17 5. The polyester according to claim 1, comprising one or more repeating units represented by the formula:

6. At least one repeating unit derived from a polybasic acid [In the formula, R 2 is C 4 ~C 16 5. The polyester according to claim 1, wherein the repeating unit is selected from the repeating units represented by the formula:

7. A method for producing the polyester according to any one of claims 1 to 6, comprising polymerizing a polyol component with a polybasic acid component in the presence of phosphorus and a metal element, A method of making wherein the polyol component comprises tricyclodecane dimethanol and has a carbonyl number of less than 0.15 mg KOH / g.

Citation Information

Patent Citations

  • Production of polyester

    JP1994100680A

  • Moldable resin composition

    JP1996301958A

  • Polyester polymerization catalyst and method for producing polyester by using the same

    JP2004189962A

  • Method for producing polyester

    JP2009235298A

  • Method for producing copolyester and copolyester

    JP2012229369A