Thermoplastic resin composition and molded article using same

A thermoplastic resin composition with specific copolymers and additives addresses friction noise and mechanical property challenges, enhancing noise reduction in styrene-based molded products, particularly for electric vehicles.

JP7576046B2Active Publication Date: 2024-10-30LOTTE CHEM CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021564477
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-30
Filing Date
2020-04-28
Publication Date
2024-10-30
Estimated Expiration
2040-04-28

AI Technical Summary

Technical Problem

Molded products made of styrene resins, such as ABS, experience frictional noise and stick-slip phenomena due to their high coefficient of friction, which is a concern in applications like electric vehicles where noise reduction is crucial for comfort.

Method used

A thermoplastic resin composition comprising 25-30% acrylonitrile-butadiene-styrene graft copolymer, 45-55% aromatic vinyl-vinyl cyanide copolymer, and 1-6 parts by weight of polyolefin-aromatic vinyl-glycidyl (meth)acrylate graft copolymer, along with optional additives, to enhance friction noise reduction and mechanical properties.

Benefits of technology

The composition achieves significant friction noise reduction and maintains excellent mechanical properties, suitable for applications requiring reduced noise, such as electric vehicle interiors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576046000004
    Figure 0007576046000004
  • Figure 0007576046000001
    Figure 0007576046000001
  • Figure 0007576046000002
    Figure 0007576046000002
Patent Text Reader

Abstract

The present invention relates to a thermoplastic resin composition containing 1 to 6 parts by weight of (D) a polyolefin-aromatic vinyl-glycidyl (meth)acrylate graft copolymer, based on 100 parts by weight of a base resin containing (A) 25 to 30% by weight of an acrylonitrile-butadiene-styrene graft copolymer; (B) 45 to 55% by weight of an aromatic vinyl-vinyl cyanide copolymer; and (C) 20 to 25% by weight of a maleimide copolymer, and a molded article using the same.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermoplastic resin composition and a molded article using the same. [Background technology]

[0002] Styrene-based resins, such as acrylonitrile-butadiene-styrene copolymer (ABS) resin, are widely used in automobiles, home appliances, office equipment, and other applications due to their excellent moldability, mechanical properties, appearance, and secondary processability.

[0003] Molded products using styrene resins can be widely used in various products that require painting or no painting, such as interior and exterior materials for automobiles.

[0004] However, when molded products made of styrene-based resins are used in areas where they come into contact with and rub against other components made of other resins, such as polyethylene or polyvinyl chloride, or lining sheets or foams made of chloroprene rubber, natural rubber, polyester, or polyethylene, friction noise may be generated.

[0005] Because styrene-based resins are non-crystalline resins, they have a higher coefficient of friction than crystalline resins such as polyethylene, polypropylene, and polyacetal. For example, when they fit with components made of other resins, such as air conditioning vents in automobiles or buttons on car stereos, the high coefficient of friction can cause a stick-slip phenomenon, resulting in frictional noise (squeaking noise).

[0006] Recently, with the increasing demand for electric vehicles, which generate less noise when driven compared to conventional automobiles, the friction noise may become a major factor that impairs comfort and quietness during riding. Therefore, there is a need to develop automobile interior materials with excellent friction noise reduction properties. Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention provides a thermoplastic resin composition having excellent friction noise reduction effects and mechanical properties, and a molded article using the same. [Means for solving the problem]

[0008] According to one embodiment, there is provided a thermoplastic resin composition comprising 100 parts by weight of a base resin including (A) 25 to 30% by weight of an acrylonitrile-butadiene-styrene graft copolymer; (B) 45 to 55% by weight of an aromatic vinyl-vinyl cyanide copolymer; and (C) 20 to 25% by weight of a maleimide-based copolymer, and 1 to 6 parts by weight of (D) a polyolefin-aromatic vinyl-glycidyl (meth)acrylate graft copolymer.

[0009] The (A) acrylonitrile-butadiene-styrene graft copolymer may have a core-shell structure including a core made of a butadiene-based rubber polymer and a shell formed by graft polymerizing acrylonitrile and styrene onto the core.

[0010] The (A) acrylonitrile-butadiene-styrene graft copolymer may contain 40 to 70% by weight of the core based on 100% by weight of the acrylonitrile-butadiene-styrene graft copolymer.

[0011] The (A) acrylonitrile-butadiene-styrene graft copolymer may have an average particle size of the rubber polymer of 200 to 400 nm.

[0012] The (B) aromatic vinyl-vinyl cyanide copolymer may be a copolymer of a monomer mixture containing 60 to 80% by weight of an aromatic vinyl compound and 20 to 40% by weight of a vinyl cyanide compound, based on 100% by weight of the aromatic vinyl-vinyl cyanide copolymer.

[0013] The (B) aromatic vinyl-vinyl cyanide copolymer may have a weight average molecular weight of 80,000 to 200,000 g / mol.

[0014] The aromatic vinyl-vinyl cyanide copolymer (B) may be a styrene-acrylonitrile copolymer.

[0015] The (C) maleimide-based copolymer may be an N-phenylmaleimide-styrene-maleic anhydride copolymer.

[0016] The maleimide copolymer (C) may have a glass transition temperature (Tg) of 150 to 200°C.

[0017] The polyolefin-aromatic vinyl-glycidyl (meth)acrylate graft copolymer (D) may be one in which an aromatic vinyl-glycidyl (meth)acrylate copolymer is grafted onto a substituted or unsubstituted polyolefin main chain.

[0018] The (D) polyolefin-aromatic vinyl-glycidyl (meth)acrylate graft copolymer can contain 70 to 95% by weight of the substituted or unsubstituted polyolefin and 5 to 30% by weight of the aromatic vinyl-glycidyl (meth)acrylate copolymer, based on 100% by weight of the polyolefin-aromatic vinyl-glycidyl (meth)acrylate graft copolymer.

[0019] The substituted or unsubstituted polyolefin may be one or more selected from the group including polyethylene and ethylene-vinyl acetate copolymer.

[0020] The aromatic vinyl-glycidyl (meth)acrylate copolymer may be a styrene-glycidyl methacrylate copolymer.

[0021] The styrene-glycidyl methacrylate copolymer may be a copolymer of a monomer mixture containing 50 to 95% by weight of styrene and 5 to 50% by weight of glycidyl methacrylate.

[0022] The (D) polyolefin-aromatic vinyl-glycidyl (meth)acrylate graft copolymer may be at least one selected from the group including polyethylene-styrene-glycidyl methacrylate graft copolymer and ethylene-vinyl acetate-styrene-glycidyl methacrylate graft copolymer.

[0023] The thermoplastic resin composition may further include at least one additive selected from a nucleating agent, a coupling agent, a filler, a plasticizer, a lubricant, a release agent, an antibacterial agent, a heat stabilizer, an antioxidant, an ultraviolet stabilizer, a flame retardant, an antistatic agent, a colorant, and an impact modifier.

[0024] Meanwhile, a molded article can be provided using the thermoplastic resin composition according to one embodiment. Effect of the Invention

[0025] The thermoplastic resin composition according to an embodiment and a molded article using the same have excellent friction noise reduction effects and mechanical properties, and therefore can be widely applied to molding of various products to be used with or without painting, and can be particularly usefully applied to applications such as interior materials for automobiles, for example, electric vehicles, where a reduction in friction noise is highly required. [Brief description of the drawings]

[0026] [Figure 1] This is a diagram of the basic principles of VDA230-206. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, embodiments of the present invention will be described in detail, which are given by way of example only and are not intended to limit the present invention, which is defined solely by the appended claims.

[0028] In the present invention, unless otherwise specified, the average particle size is a volume average diameter, and means a Z-average particle size measured using a dynamic light scattering analysis device.

[0029] According to one embodiment, there is provided a thermoplastic resin composition comprising 100 parts by weight of a base resin including (A) 25 to 30% by weight of an acrylonitrile-butadiene-styrene graft copolymer; (B) 45 to 55% by weight of an aromatic vinyl-vinyl cyanide copolymer; and (C) 20 to 25% by weight of a maleimide-based copolymer, and 1 to 6 parts by weight of (D) a polyolefin-aromatic vinyl-glycidyl (meth)acrylate graft copolymer.

[0030] Hereinafter, each component contained in the thermoplastic resin composition will be specifically described.

[0031] (A) Acrylonitrile-butadiene-styrene graft copolymer In one embodiment, the acrylonitrile-butadiene-styrene graft copolymer imparts excellent impact resistance to the thermoplastic resin composition. In one embodiment, the acrylonitrile-butadiene-styrene graft copolymer may have a core-shell structure in which a core is made of a butadiene-based rubber polymer component and a shell is formed by graft polymerization of acrylonitrile and styrene on the core.

[0032] The rubber polymer component constituting the core improves impact resistance, particularly at low temperatures, and the shell component can lower the interfacial tension and improve the adhesive strength at the interface.

[0033] The acrylonitrile-butadiene-styrene graft copolymer according to one embodiment can be prepared by adding styrene and acrylonitrile to a butadiene-based rubber polymer and graft-copolymerizing the mixture by a conventional polymerization method such as emulsion polymerization or bulk polymerization.

[0034] The butadiene-based rubbery polymer is selected from the group consisting of butadiene rubbery polymers, butadiene-styrene rubbery polymers, butadiene-acrylonitrile rubbery polymers, butadiene-acrylate rubbery polymers, and mixtures thereof.

[0035] The acrylonitrile-butadiene-styrene graft copolymer may have an average particle size of the butadiene rubber polymer of, for example, 200 to 400 nm, for example, 200 to 350 nm, for example, 250 to 350 nm. When the above range is satisfied, the thermoplastic resin composition can ensure excellent impact resistance and appearance properties.

[0036] The butadiene-based rubber polymer core is contained in an amount of 40 to 70% by weight based on 100% by weight of the acrylonitrile-butadiene-styrene graft copolymer, while the shell may be a styrene-acrylonitrile copolymer copolymerized from a monomer mixture in which the weight ratio of the styrene and the acrylonitrile is 6:4 to 8:2.

[0037] The acrylonitrile-butadiene-styrene graft copolymer is contained in an amount of 25 to 30% by weight, for example, 26 to 29% by weight, relative to 100% by weight of the base resin.

[0038] If the content of the acrylonitrile-butadiene-styrene graft copolymer in the base resin is less than 25% by weight, it is difficult to achieve excellent impact resistance, and if it exceeds 30% by weight, heat resistance and fluidity may decrease.

[0039] (B) Aromatic vinyl-vinyl cyanide copolymer In one embodiment, the aromatic vinyl-vinyl cyanide copolymer functions to improve the flowability of the thermoplastic resin composition and to maintain a certain level of compatibility between the components.

[0040] In one embodiment, the aromatic vinyl-vinyl cyanide copolymer can have a weight average molecular weight of 80,000 g / mol or more, for example, 85,000 g / mol or more, for example, 90,000 g / mol or more, for example, 200,000 g / mol or less, for example, 150,000 g / mol or less, for example, 80,000 g / mol to 200,000 g / mol, for example, 80,000 g / mol to 150,000 g / mol.

[0041] In the present invention, the weight average molecular weight is measured by dissolving a powder sample in tetrahydrofuran (THF) and then using an Agilent Technologies 1200 series gel permeation chromatography (GPC) (Shodex LF-804 column and Shodex polystyrene standard).

[0042] The aromatic vinyl compound may be at least one selected from styrene, α-methylstyrene, p-methylstyrene, pt-butylstyrene, 2,4-dimethylstyrene, chlorostyrene, vinyltoluene, and vinylnaphthalene.

[0043] The vinyl cyanide compound may be at least one selected from acrylonitrile, methacrylonitrile, and fumaronitrile.

[0044] In one embodiment, the vinyl aromatic compound-vinyl cyanide copolymer may be a copolymer of a monomer mixture including a vinyl aromatic compound and a vinyl cyanide compound.

[0045] In this case, the aromatic vinyl compound may be contained in an amount of, for example, 60% by weight or more, for example, 65% by weight or more, for example, 70% by weight or more, for example, 80% by weight or less, for example, 75% by weight or less, for example, 60 to 80% by weight, for example, 65 to 75% by weight, relative to 100% by weight of the aromatic vinyl-vinyl cyanide copolymer.

[0046] Furthermore, the vinyl cyanide compound may be contained in an amount of, for example, 20% by weight or more, such as 25% by weight or more, for example, 40% by weight or less, such as 35% by weight or less, for example, 20 to 40% by weight, for example, 25 to 35% by weight, relative to 100% by weight of the aromatic vinyl-vinyl cyanide copolymer.

[0047] In one embodiment, the vinyl aromatic-vinyl cyanide copolymer may be a styrene-acrylonitrile copolymer (SAN).

[0048] In one embodiment, the aromatic vinyl-vinyl cyanide copolymer is contained in an amount of 45 to 55% by weight, for example 47 to 53% by weight, based on 100% by weight of the base resin.

[0049] If the content of the aromatic vinyl-cyanide vinyl copolymer is less than 45% by weight, the moldability of the thermoplastic resin composition may be reduced, and if it exceeds 55% by weight, the mechanical properties of a molded product using the thermoplastic resin composition may be reduced.

[0050] (C) Maleimide copolymer In one embodiment, the maleimide copolymer imparts excellent heat resistance to the thermoplastic resin composition. The maleimide copolymer may be a terpolymer of N-phenylmaleimide, styrene, and maleic anhydride, and can be prepared by imidization reaction of a copolymer of styrene and maleic anhydride.

[0051] In one embodiment, the N-phenylmaleimide is contained in an amount of 10% by weight to 55% by weight, for example, 15% by weight to 55% by weight, for example, 15% by weight to 50% by weight, based on 100% by weight of the maleimide-based copolymer.

[0052] Meanwhile, in one embodiment, the styrene is contained in an amount of 40% by weight to 80% by weight, and the maleic anhydride is contained in an amount of 1% by weight to 10% by weight, based on 100% by weight of the maleimide-based copolymer.

[0053] In the maleimide-based copolymer according to one embodiment, if the N-phenylmaleimide content is less than 10% by weight, the heat resistance improving effect of the maleimide-based copolymer is unlikely to be exhibited, and if it exceeds 55% by weight, the appearance properties of the thermoplastic resin composition and molded articles using the same may be significantly deteriorated.

[0054] The maleimide copolymer may have a glass transition temperature (Tg) of, for example, 150 to 200°C, for example, 160 to 200°C, for example, 170 to 200°C.

[0055] The maleimide copolymer is contained in an amount of 20 to 25% by weight, for example 21 to 24% by weight, relative to 100% by weight of the base resin.

[0056] When the content of the maleimide copolymer in the base resin satisfies the above-mentioned range, the heat resistance can be significantly improved while maintaining a balance with other physical properties such as mechanical properties and moldability of the thermoplastic resin composition, and molded products produced using the same can also exhibit excellent heat resistance.

[0057] (D) Polyolefin-aromatic vinyl-glycidyl (meth)acrylate graft copolymer In one embodiment, the polyolefin-aromatic vinyl-glycidyl (meth)acrylate graft copolymer reduces the friction coefficient of a thermoplastic resin composition and a molded article made therefrom, while improving the durability of the friction noise reduction, thereby exhibiting excellent friction noise reduction properties.

[0058] In one embodiment, the polyolefin-aromatic vinyl-glycidyl (meth)acrylate graft copolymer may be an aromatic vinyl-glycidyl (meth)acrylate copolymer grafted onto a substituted or unsubstituted polyolefin backbone.

[0059] The substituted or unsubstituted polyolefin may be one or more selected from the group including polyethylene and ethylene-vinyl acetate copolymer. The ethylene-vinyl acetate copolymer may be a copolymer of ethylene and vinyl acetate.

[0060] The aromatic vinyl-glycidyl (meth)acrylate copolymer grafted onto the polyolefin main chain may be a copolymer of an aromatic vinyl compound and glycidyl (meth)acrylate.

[0061] The aromatic vinyl compound may be any one or more selected from styrene, C1-C10 alkyl-substituted styrene, halogen-substituted styrene, vinyltoluene, vinylnaphthalene, and mixtures thereof. Specific examples of the alkyl-substituted styrene include α-methylstyrene, p-methylstyrene, o-ethylstyrene, m-ethylstyrene, p-ethylstyrene, pt-butylstyrene, and 2,4-dimethylstyrene.

[0062] The glycidyl (meth)acrylate may be at least one selected from the group consisting of glycidyl acrylate, glycidyl methacrylate, and a mixture thereof.

[0063] Examples of the aromatic vinyl-glycidyl (meth)acrylate copolymer include a copolymer of styrene and glycidyl acrylate, a copolymer of styrene and glycidyl methacrylate, a copolymer of α-methylstyrene and glycidyl acrylate, a copolymer of α-methylstyrene and glycidyl methacrylate, a copolymer of styrene, α-methylstyrene and glycidyl acrylate, a copolymer of styrene, α-methylstyrene and glycidyl methacrylate, or a copolymer of styrene, α-methylstyrene, glycidyl acrylate and glycidyl methacrylate, and preferably a copolymer of styrene-glycidyl methacrylate. In this case, the styrene-glycidyl methacrylate copolymer may be a copolymer of a monomer mixture containing 50 to 95% by weight of styrene and 5 to 50% by weight of glycidyl methacrylate.

[0064] As an example, the polyolefin-aromatic vinyl-glycidyl (meth)acrylate graft copolymer may be at least one selected from the group including polyethylene-styrene-glycidyl methacrylate graft copolymer (PE-g-SGMA) and ethylene-vinyl acetate-styrene-glycidyl methacrylate graft copolymer (EVA-g-SGMA).

[0065] In one embodiment, the polyolefin-aromatic vinyl-glycidyl (meth)acrylate graft copolymer contains 70 to 95% by weight of the substituted or unsubstituted polyolefin and 5 to 30% by weight of the aromatic vinyl-glycidyl (meth)acrylate copolymer, based on 100% by weight of the polyolefin-aromatic vinyl-glycidyl (meth)acrylate graft copolymer.

[0066] The polyolefin-aromatic vinyl-glycidyl (meth)acrylate graft copolymer is contained in an amount of, for example, 1 to 6 parts by weight, for example, 2 to 6 parts by weight, for example, 2 to 5 parts by weight, relative to 100 parts by weight of the base resin. If the polyolefin-aromatic vinyl-glycidyl (meth)acrylate graft copolymer is contained in an amount of less than 1 part by weight, the friction noise reduction characteristics of the molded product using the same are unlikely to be exhibited, and if it exceeds 6 parts by weight, mechanical properties such as rigidity may be reduced.

[0067] (E) Other additives In addition to the components (A) to (D), the thermoplastic resin composition according to one embodiment may further include one or more additives required to balance the various physical properties under the condition of maintaining excellent friction noise reduction effects and mechanical properties, or depending on the end use of the thermoplastic resin composition.

[0068] Specifically, the additives that can be used include nucleating agents, coupling agents, fillers, plasticizers, lubricants, release agents, antibacterial agents, heat stabilizers, antioxidants, UV stabilizers, flame retardants, antistatic agents, colorants, and impact modifiers, and these can be used alone or in combination of two or more kinds.

[0069] These additives are appropriately included within a range that does not impair the physical properties of the thermoplastic resin composition, and specifically, are included in an amount of 20 parts by weight or less per 100 parts by weight of the base resin, but are not limited to this amount.

[0070] The thermoplastic resin composition according to the present invention can be produced by a known method for producing a thermoplastic resin composition.

[0071] For example, the thermoplastic resin composition according to the present invention can be prepared in the form of pellets by simultaneously mixing the components of the present invention and other additives and then melt-kneading them in an extruder.

[0072] A molded article according to one embodiment of the present invention can be produced from the thermoplastic resin composition described above.

[0073] The thermoplastic resin composition has excellent friction noise reduction effects and mechanical properties, and therefore can be widely applied to various products used with or without painting. In particular, since the stick-slip phenomenon is minimized, the composition can be usefully applied to applications such as interior materials for automobiles, for example, electric vehicles, which require a large reduction in friction noise.

[0074] The present invention will now be described in more detail with reference to examples and comparative examples. However, the following examples and comparative examples are for illustrative purposes only and are not intended to limit the present invention.

[0075] Example 1, Example 2, and Comparative Examples 1 to 4 The thermoplastic resin compositions of Examples 1 and 2 and Comparative Examples 1 to 4 were produced according to the content ratios of the components shown in Table 1 below.

[0076] In Table 1, (A), (B), and (C) are contained in the base resin and are expressed as weight percent based on the total weight of the base resin, and (D), (D'), and (D") are added to the base resin and are expressed as parts by weight based on 100 parts by weight of the base resin.

[0077] The components shown in Table 1 were dry mixed and continuously fed quantitatively into the feed section of a twin-screw extruder (L / D=36, Φ=45mm) for melting / kneading. Next, the thermoplastic resin composition pelletized by the twin-screw extruder was dried at about 80°C for about 4 hours, and then a test piece for evaluating mechanical properties and a test piece for evaluating squeak noise measuring 100mm x 100mm x 3.2mm (width x length x thickness) were produced using a 6oz injection molding machine with a cylinder temperature of about 220°C and a mold temperature of about 60°C.

[0078] [Table 1]

[0079] The explanation of each component listed in Table 1 is as follows.

[0080] (A) Acrylonitrile-butadiene-styrene graft copolymer Acrylonitrile-butadiene-styrene graft copolymer (Lotte Advanced Materials) containing approximately 58% by weight of a core (average particle size: approximately 250 nm) made of butadiene rubber polymer, and a shell formed by graft polymerizing acrylonitrile and styrene onto the core. (B) Aromatic vinyl-vinyl cyanide copolymer Styrene-acrylonitrile copolymer with a weight average molecular weight of approximately 110,000 g / mol, copolymerized from a monomer mixture containing approximately 28% by weight of acrylonitrile and approximately 72% by weight of styrene (Lotte Advanced Materials) (C) Maleimide copolymer N-phenylmaleimide-styrene-maleic anhydride copolymer (Denka) with a glass transition temperature (Tg) of approximately 185°C (D) Polyolefin-aromatic vinyl-glycidyl methacrylate graft copolymer Polyethylene-styrene-glycidyl methacrylate graft copolymer (PE-g-SGMA, NOF Corporation), in which styrene-glycidyl methacrylate copolymer is grafted onto the polyethylene main chain (D') Polyethylene-styrene-acrylonitrile graft copolymer Styrene-acrylonitrile copolymer grafted onto polyethylene main chain (PE-g-SAN, NOF) (D") Dimethylpolysiloxane Dimethylpolysiloxane with a kinematic viscosity of approximately 100 cSt at 25°C (Shin-Etsu Chemical Co., Ltd.) Experimental Example The experimental results are shown in Table 3 below.

[0081] (1) Tensile strength (MPa): The tensile strength of test pieces for evaluating mechanical properties was measured according to ISO 527-1.

[0082] (2) Flexural strength (MPa): The flexural strength of the test specimen for evaluating mechanical properties was measured according to ISO178.

[0083] (3) Flexural modulus (MPa): The flexural modulus of the test specimen for evaluating mechanical properties was measured according to ISO178.

[0084] (4) Impact resistance (kJ / m 2 ): The notched Izod impact strength of the test pieces for evaluating mechanical properties was measured according to ISO180.

[0085] (5) Squeak noise: Friction noise of test pieces for evaluating squeak noise corresponding to the following condition 1 (normal temperature condition) and condition 2 (severe condition) was measured according to VDA230-206.

[0086] - Condition 1 (room temperature condition): The test piece is left at room temperature without any additional heat treatment. -Condition 2 (severe condition): The test piece is left in an oven at approximately 80°C for approximately 300 hours. Figure 1 illustrates the basic principle of VDA230-206. Referring to Figure 1, material A and material B are the same material that have been heat-treated under the same conditions, and the spring component moves material A in the moving phase relative to material B. The force (F N ) is 40N, and the moving speed of the sliding carriage (V s ) is 4 mm / s, and the contact area of ​​the two material specimens is 1,250 mm 2The spring movement phenomenon is caused by stick and slip, and this was used to evaluate the squeak noise.

[0087] Table 2 below shows the evaluation criteria for squeak noise; the closer the RPN is to 1, the better the effect of reducing fricative noise.

[0088] [Table 2]

[0089] Referring to Table 2, RPN1-3 means that there is almost no noise, RPN4-5 means that the noise is at the limit and cannot be eliminated due to the stick-slip effect, and RPN6-10 means that the stick-slip effect is obvious and noise is always present.

[0090] [Table 3]

[0091] From Tables 1 and 3, it can be seen that by using the acrylonitrile-butadiene-styrene graft copolymer, aromatic vinyl-vinyl cyanide copolymer, maleimide copolymer, and polyolefin-aromatic vinyl-glycidyl (meth)acrylate graft copolymer in optimal amounts as in Examples 1 and 2, it is possible to provide a thermoplastic resin composition and a molded article using the same that exhibit superior friction noise reduction effect and mechanical properties (impact resistance and rigidity) compared to the comparative examples.

[0092] Although the present invention has been described above through the preferred embodiments, it will be readily understood by those skilled in the art to which the present invention pertains that the present invention is not limited thereto, and various modifications and variations are possible without departing from the concept and scope of the claims set forth below.

Claims

1. (A) 25 to 30% by weight of an acrylonitrile-butadiene-styrene graft copolymer; (B) 45 to 55% by weight of an aromatic vinyl-vinyl cyanide copolymer; and (C) Maleimide copolymer 20 to 25% by weight For 100 parts by weight of the base resin, (D) 1 to 6 parts by weight of a polyethylene-aromatic vinyl-glycidyl (meth)acrylate graft copolymer; The polyethylene-aromatic vinyl-glycidyl (meth)acrylate graft copolymer (D) is a polyethylene main chain to which a styrene-glycidyl (meth)acrylate copolymer is grafted, Based on the total weight of the graft copolymer, The polyethylene comprises 70 to 95% by weight, and the styrene-glycidyl (meth)acrylate copolymer comprises 5 to 30% by weight, The styrene-glycidyl (meth)acrylate copolymer is a thermoplastic resin composition which is a copolymer of a mixture containing 50 to 95% by weight of styrene and 5 to 50% by weight of glycidyl methacrylate.

2. The (A) acrylonitrile-butadiene-styrene graft copolymer is A core made of a butadiene-based rubber polymer, and 2. The thermoplastic resin composition according to claim 1, which has a core-shell structure comprising a shell formed by graft polymerization of acrylonitrile and styrene onto the core.

3. The thermoplastic resin composition according to claim 2, wherein the (A) acrylonitrile-butadiene-styrene graft copolymer comprises 40 to 70% by weight of the core, based on 100% by weight.

4. The thermoplastic resin composition according to any one of claims 1 to 3, wherein the acrylonitrile-butadiene-styrene graft copolymer (A) has an average particle size of a rubber polymer of 200 to 400 nm.

5. The thermoplastic resin composition according to any one of claims 1 to 4, wherein the aromatic vinyl-cyanide vinyl copolymer (B) is a copolymer of a monomer mixture containing 60 to 80% by weight of an aromatic vinyl compound and 20 to 40% by weight of a vinyl cyanide compound, based on 100% by weight of the aromatic vinyl-cyanide vinyl copolymer.

6. The thermoplastic resin composition according to any one of claims 1 to 5, wherein the weight average molecular weight of the aromatic vinyl-cyanated vinyl copolymer (B) is 80,000 to 200,000 g / mol.

7. The thermoplastic resin composition according to any one of claims 1 to 6, wherein the aromatic vinyl-vinyl cyanide copolymer (B) is a styrene-acrylonitrile copolymer.

8. The thermoplastic resin composition according to any one of claims 1 to 7, wherein the maleimide-based copolymer (C) is an N-phenylmaleimide-styrene-maleic anhydride copolymer.

9. The thermoplastic resin composition according to any one of claims 1 to 8, wherein the maleimide copolymer (C) has a glass transition temperature (Tg) of 150 to 200°C.

10. The thermoplastic resin composition according to any one of claims 1 to 9, further comprising at least one additive selected from the group consisting of nucleating agents, coupling agents, fillers, plasticizers, lubricants, release agents, antibacterial agents, heat stabilizers, antioxidants, UV stabilizers, flame retardants, antistatic agents, colorants, and impact modifiers.

11. A molded article comprising the thermoplastic resin composition according to any one of claims 1 to 10.

Citation Information

Patent Citations

  • Motor vehicle trim parts

    JP1988152659A

  • Thermoplastic resin composition and molded product

    JP2008056904A

  • Method for producing thermoplastic resin composition

    JP2015218309A

  • ABS resin composition, and resin molding

    JP2017066216A

  • Thermoplastic resin composition and molded article using the same

    JP2017536428A