Glass composition, glass filler and its manufacturing method, and resin composition containing glass filler

A glass composition with controlled SiO2, B2O3, Al2O3, MgO, and alkali metal oxide ratios addresses the challenge of achieving low dielectric constant and water resistance in glass fillers, enhancing resin properties like strength and heat resistance.

JP7576091B2Active Publication Date: 2024-10-30NIPPON SHEET GLASS CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2022530591
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-06-10
Filing Date
2021-06-08
Publication Date
2024-10-30
Estimated Expiration
2041-06-08

AI Technical Summary

Technical Problem

Existing glass fillers used in resin compositions for electronic devices struggle to achieve a low dielectric constant while maintaining excellent water resistance, and existing patents do not address this issue.

Method used

A glass composition with specific ranges of SiO2, B2O3, Al2O3, MgO, CaO, and alkali metal oxides is formulated to provide a low dielectric constant and improved water resistance, with a dielectric constant of 4.6 or less at 1 GHz and an alkali elution of 0.40 mg or less.

Benefits of technology

The glass composition enhances the resin composition's properties by maintaining a low dielectric constant, improving strength, heat resistance, and dimensional stability, while reducing linear thermal expansion and anisotropy in molding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576091000013
    Figure 0007576091000013
  • Figure 0007576091000014
    Figure 0007576091000014
  • Figure 0007576091000015
    Figure 0007576091000015
Patent Text Reader

Abstract

This glass composition includes, in mass%, 50 ≤ SiO2 ≤ 65, 20 ≤ B2O3 ≤ 30, and 5 ≤ Al2O3 ≤ 20 and additionally includes at least one substance selected from the group consisting of MgO and CaO, and one substance selected from the group consisting of Li2O, Na2O, and K2O. The glass composition satisfies 0.1 ≤ (MgO + CaO) < 5, 0 ≤ (Li2O + Na2O + K2O) ≤ 4, and 0.50 < MgO / (MgO + CaO) ≤ 1.00. The glass composition has a low dielectric constant and is suitable for producing a glass filler which can exhibit excellent water resistance.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a glass composition. The present invention also relates to a glass filler, a method for producing the glass filler, and a resin composition containing the glass filler. [Background technology]

[0002] Resin compositions are widely used as electrical insulating members and mechanical members in various parts of electronic devices. Examples of electrical insulating members include connector housings used in SMT (surface mount technology), FPC (flexible printed circuits), board-to-board, CPU (central processing unit) sockets, memory cards, card edges, optical connectors, etc.; reactance bobbins used in LCD (liquid crystal display) backlights, coils, flats, transformers, magnetic heads, etc.; switches used in relay cases, relay base switches, reflow dip switches, tact switches, etc.; sensor cases, capacitor casings, volume casings, and trimmer casings. Examples of mechanical parts include lens holders and pickup bases for optical pickups, insulators and terminals for micromotors, and drums for laser printers. Resin compositions are also used as films such as base films for FPCs and base films for copper-clad laminates. In addition, a type of printed circuit board equipped in electronic devices also has a substrate made of a resin composition. A printed wiring board before electronic components are mounted also has a substrate made of a resin composition. Hereinafter, in this specification, both printed circuit boards and printed wiring boards will be referred to as "printed boards."

[0003] The above-mentioned resin composition usually contains a thermoplastic resin and an inorganic filler, and further contains a curing agent, a modifier, etc. as necessary. As the inorganic filler, a glass filler may be used. A representative glass filler is flake glass. In recent years, in order to meet the demand for miniaturization of electronic devices and the demand for thinning for the purpose of high functionality, there is a demand for a resin composition and its constituent materials to have a low dielectric constant.

[0004] A printed circuit board may further contain glass fibers. There is a demand for these glass fibers to have a low dielectric constant. Patent documents 1 to 3 disclose glass fibers made of a glass composition having a low dielectric constant. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 62-226839 [Patent Document 2] International Publication No. 2017 / 187471 [Patent Document 3] International Publication No. 2018 / 216637 Summary of the Invention [Problem to be solved by the invention]

[0006] Glass fillers used as inorganic fillers are required to have a low dielectric constant and excellent water resistance. However, it is not easy to improve the water resistance of a glass composition having a low dielectric constant. In addition, Patent Documents 1 to 3 do not take water resistance into consideration.

[0007] In view of the above, an object of the present invention is to provide a glass composition suitable for producing a glass filler that has a low dielectric constant and exhibits excellent water resistance. [Means for solving the problem]

[0008] The present invention relates to Expressed in mass%, 50≦SiO 2 <= 65 20≦B 2 O 3 <= 30 5≦Al 2 O 3 <= 20 Including, At least one selected from the group consisting of MgO and CaO; Li 2 O, Na 2 O and K 2 At least one selected from the group consisting of O Further comprising: 0.1≦(MgO+CaO)<5 0≦(Li 2 O+Na 2 O+K 2 O) ≦4, and 0.50 <MgO / (MgO+CaO)≦1.00 The glass composition according to claim 1, to provide.

[0009] From another aspect, the present invention provides A glass filler comprising the glass composition of the present invention; to provide.

[0010] From another aspect, the present invention provides a resin composition comprising the glass filler of the present invention and a thermoplastic resin; to provide.

[0011] From another aspect, the present invention provides A method for producing a glass filler, comprising: a step of melting the glass composition of the present invention; and a step of forming the molten glass composition into a glass filler. to provide. Effect of the Invention

[0012] According to the present invention, a glass composition suitable for producing a glass filler that has a low dielectric constant and exhibits excellent water resistance can be provided. The glass composition of the present invention can produce a glass filler suitable for improving various properties of a resin composition by blending while keeping the dielectric constant of the resin composition low. The improvements in the various properties include, for example, improved strength, heat resistance, and dimensional stability; reduced linear thermal expansion coefficient and anisotropy; and reduced anisotropy of shrinkage during molding. [Brief description of the drawings]

[0013] [Figure 1A] FIG. 1A is a perspective view that typically illustrates an example of a glass flake, which is one type of glass filler of the present invention. [Figure 1B] FIG. 1B is a plan view of the glass flake of FIG. 1A as viewed from above. [Diagram 2] FIG. 2 is a schematic diagram illustrating an example of an apparatus and method for producing glass flakes. [Diagram 3] FIG. 3 is a schematic diagram illustrating another example of an apparatus and method for producing a glass flake. [Figure 4] FIG. 4 is a schematic diagram for explaining an example of a spinning apparatus that can be used to produce chopped strands. [Diagram 5] FIG. 5 is a schematic diagram for explaining an example of an apparatus for producing chopped strands from the strand winding obtained by the spinning apparatus of FIG. [Figure 6] FIG. 6 is a perspective view showing an example of a flat fiber. [Figure 7] FIG. 7 is a perspective view showing another example of a flat fiber. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] In the following, the "%" indications indicating the content of each component are all mass%. "Substantially not contained" means that the content is less than 0.1 mass%, preferably less than 0.07 mass%, more preferably less than 0.05 mass%, particularly preferably less than 0.01 mass%, and most preferably less than 0.005 mass%. The wording "substantially" in the above means that impurities that are inevitably mixed in from industrial raw materials, glass manufacturing equipment, glass molded body manufacturing equipment, etc. are allowed within the above limits. The content, characteristics, and other preferred ranges of each component can be understood by arbitrarily combining the upper and lower limits described individually below.

[0015] Strictly speaking, the dielectric constant means the relative dielectric constant, but in this specification, it is simply referred to as the dielectric constant in accordance with conventional practice. The dielectric constant is the value at room temperature (25° C.).

[0016] The following description is not intended to limit the present invention, but is presented to illustrate preferred embodiments thereof.

[0017] [Components of glass composition] (SiO 2 ) SiO 2 is the component that forms the glass skeleton and is the main component (the component with the highest content). SiO 2 SiO has the effect of adjusting the devitrification temperature and viscosity during glass formation, and also has the effect of lowering the dielectric constant of the glass. 2 When the content of SiO is 50% or more and 65% or less, the increase in the devitrification temperature that makes it difficult to manufacture the glass filler is suppressed, and the dielectric constant can be adjusted to a range suitable for blending in a resin composition. In addition, within the above range, the melting point of the glass does not become excessively high, and uniformity is increased when the raw material is melted. 2 The lower limit of the SiO content may be 51% or more, 52% or more, 53% or more, 54% or more, 55% or more, or even more than 55%. 2 The upper limit of the content may be less than 64%, 63% or less, 62% or less, less than 62%, 61% or less, 60% or less, 59% or less, or even 58% or less.

[0018] (B 2 O 3 ) B 2 O 3 is a component that forms the glass skeleton. 2 O 3 has the effect of adjusting the devitrification temperature and viscosity during glass formation, and also has the effect of lowering the dielectric constant of the glass. 2 O 3 B is easily volatilized during glass melting, and if its content is too high, it becomes difficult to obtain sufficient homogeneity as a glass. 2 O 3 The inclusion of reduces the water resistance of the glass. 2 O 3 When the content is 20% or more and 30% or less, the increase in the devitrification temperature of the glass that would make the production of the glass filler difficult is suppressed, and the dielectric constant can be adjusted to a range suitable for blending into a resin composition. In addition, within the above range, the melting point of the glass does not become excessively high, and uniformity is improved when the raw materials are melted. Furthermore, within the above range, the water resistance of the glass is high. 2 O 3 The lower limit of the content may be more than 20%, 21% or more, 22% or more, 23% or more, 24% or more, 25% or more, 26% or more, or even more than 26%. 2 O 3 The upper limit of the content may be less than 30%, 29.5% or less, 29% or less, 28.5% or less, or even 28% or less.

[0019] (SiO 2 -B 2 O 3 ) In order to obtain a glass composition with a lower dielectric constant and higher water resistance, SiO 2 From the content of B 2 O 3 The SiO content is subtracted from the 2 -B 2 O 3 may be adjusted to 26% or more, 27% or more, 28% or more, 29% or more, or even 30% or more.

[0020] (Al 2 O3 ) Al 2 O 3 is a component that forms the glass framework. 2 O 3 Al has the effect of adjusting the devitrification temperature and viscosity during glass formation, and also has the effect of improving the water resistance of the glass. 2 O 3 is a component that adjusts the dielectric constant of the glass. 2 O 3 When the Al content is 5% or more and 20% or less, the increase in the devitrification temperature of the glass that would make it difficult to manufacture the glass filler is suppressed, and the water resistance of the glass is increased. In addition, within the above range, the melting point of the glass does not become excessively high, and uniformity is improved when the raw materials are melted. 2 O 3 The lower limit of the Al content may be 6% or more, 8% or more, 9% or more, or even 10% or more. 2 O 3 The upper limit of the Al content may be 18% or less, 16% or less, 15.5% or less, 15.3% or less, 15% or less, 14.5% or less, 14% or less, 13.5% or less, or even 13% or less. 2 O 3 The content of is 13% or less. Note that the larger the temperature difference ΔT, the more improved the moldability of the glass filler becomes.

[0021] (MgO, CaO) MgO and CaO have the effect of adjusting the devitrification temperature and viscosity during glass formation while maintaining the heat resistance of the glass. In addition, MgO and CaO have the effect of improving the water resistance of the glass and are components that adjust the dielectric constant of the glass.

[0022] When the control of the dielectric constant and water resistance of the glass filler is important, MgO+CaO, which is the sum of the contents of MgO and CaO, is important. When MgO+CaO is 0.1% or more and less than 5%, the increase in the devitrification temperature of the glass that makes the production of the glass filler difficult is suppressed, and the dielectric constant can be adjusted within a range suitable for blending into the resin composition. In addition, in the above range, the melting point of the glass does not become excessively high, and uniformity is increased when melting the raw materials. Furthermore, in the above range, the water resistance of the glass is high. The lower limit of MgO+CaO may be 0.5% or more, 1% or more, 1.5% or more, 2% or more, 2.2% or more, 2.4% or more, 2.5% or more, 2.8% or more, 2.9% or more, 3% or more, 3.2% or more, 3.5% or more, or even more than 3.5%. The upper limit of MgO+CaO may be 4.5% or less, or even 4% or less.

[0023] From the viewpoint of reducing the dielectric constant, the addition of MgO is more advantageous than CaO. Also, from the viewpoint of improving water resistance, the addition of MgO is more advantageous than CaO. For this reason, the ratio (by mass) of MgO to MgO+CaO, MgO / (MgO+CaO), is set to be more than 0.50 and not more than 1.00. When MgO / (MgO+CaO) is more than 0.50, the increase in the devitrification temperature of the glass that makes it difficult to manufacture the glass filler is suppressed, and the dielectric constant can be adjusted within a range suitable for blending into the resin composition. In addition, within the above range, the melting point of the glass does not become excessively high, and uniformity is increased when melting the raw materials. Furthermore, within the above range, the water resistance of the glass is increased. The lower limit of MgO / (MgO+CaO) may be 0.55 or more, 0.60 or more, 0.65 or more, 0.70 or more, 0.75 or more, 0.80 or more, or even 0.85 or more. The upper limit of MgO / (MgO+CaO) may be 0.99 or less, or even 0.95 or less. When it is desired to reliably improve the water resistance of the glass while maintaining a low dielectric constant, the range of MgO / (MgO+CaO) is 0.85 or more, or even 0.90 or more.

[0024] Regarding MgO, excessive inclusion increases the dielectric constant of the glass. The content of MgO is, for example, 0.1% or more and less than 5%. In the above range, the increase in the devitrification temperature of the glass that makes it difficult to manufacture the glass filler is more reliably suppressed, and the dielectric constant is more reliably adjusted to a range suitable for blending into the resin composition. In addition, in the above range, the melting point of the glass is prevented from becoming excessively high, and the uniformity when melting the raw materials can be more reliably improved. Furthermore, in the above range, the water resistance of the glass can be more reliably improved. The lower limit of the content of MgO may be 1% or more, 1.5% or more, 1.8% or more, 2% or more, 2.1% or more, 2.3% or more, 2.5% or more, 2.7% or more, or even 3% or more. The upper limit of the content of MgO may be 4.5% or less, 4% or less, or even 3.5% or less.

[0025] Excessive inclusion of CaO increases the dielectric constant of the glass. The lower limit of the CaO content may be 0.1% or more, or even 0.2% or more. The upper limit of the CaO content may be less than 2.5%, 2% or less, 1.5% or less, 1.2% or less, 1% or less, 0.75% or less, 0.7% or less, or even 0.5% or less. When it is desired to reliably improve the water resistance of the glass while maintaining a low dielectric constant, the CaO content suitable is 0.5% or less.

[0026] (SrO) The glass composition may contain SrO. SrO may have the effect of adjusting the devitrification temperature and viscosity during glass formation. On the other hand, excessive SrO content increases the dielectric constant of the glass. The upper limit of the SrO content may be 5% or less, 3.5% or less, 2% or less, 1.5% or less, 1% or less, 0.5% or less, less than 0.5%, or even 0.1% or less. SrO may not be substantially contained.

[0027] (BaO) The glass composition may contain BaO. BaO may have the effect of adjusting the devitrification temperature and viscosity during glass formation. On the other hand, excessive inclusion of BaO increases the dielectric constant of the glass. The upper limit of the BaO content may be 5% or less, 2% or less, 1% or less, less than 1%, 0.5% or less, or even 0.1% or less. BaO may not be substantially contained. When it is particularly important to uniformly melt the glass raw materials and stably produce the glass composition, the lower limit of the BaO content may be 0.1% or more.

[0028] (ZnO) The glass composition may contain ZnO. ZnO may have the effect of adjusting the devitrification temperature and viscosity during glass formation. ZnO may also have the effect of adjusting the dielectric constant of the glass. On the other hand, excessive inclusion of ZnO increases the dielectric constant of the glass. The lower limit of the ZnO content may be 0.1% or more. The upper limit of the ZnO content may be 5% or less, 4% or less, 3.5% or less, 3% or less, 2% or less, 1.5% or less, 1% or less, less than 1%, 0.5% or less, or even 0.1% or less. ZnO may not be substantially contained.

[0029] (MgO+CaO+ZnO) When ZnO is contained, from the viewpoint of placing importance on the dielectric constant of the glass filler, MgO+CaO+ZnO, which is the sum of the contents of MgO, CaO and ZnO, may be controlled. MgO+CaO+ZnO may be 0.1% or more and 6% or less. In the above range, the increase in the devitrification temperature of the glass that makes it difficult to manufacture the glass filler is more reliably suppressed, and the dielectric constant is more reliably adjusted to a range suitable for blending in the resin composition. In addition, in the above range, the melting point of the glass is prevented from becoming excessively high, and the uniformity when melting the raw material can be more reliably improved. The lower limit of MgO+CaO+ZnO may be 1% or more, 1.5% or more, 2% or more, 2.5% or more, 2.8% or more, 2.9% or more, 3% or more, 3.2% or more, 3.3% or more, or even 3.5% or more. The upper limit of MgO+CaO+ZnO may be 6% or less, 5.5% or less, less than 5%, 4.5% or less, or even 4% or less.

[0030] (Li 2 O, Na 2 OK 2 O) Alkali metal oxide Li 2 O, Na 2 O and K 2 O has the effect of adjusting the devitrification temperature and viscosity during glass formation while maintaining the heat resistance of the glass. On the other hand, an excessive content of alkali metal oxides increases the dielectric constant of the glass and reduces the water resistance. For this reason, the total content of alkali metal oxides Li 2 O+Na 2 O+K 2 O is between 0% and 4%. 2 O+Na 2 O+K 2 The lower limit of O may be 0.1% or more, 0.2% or more, 0.3% or more, 0.4% or more, 0.5% or more, more than 0.5%, 0.6% or more, 0.7% or more, or even more than 0.7%. 2 O+Na 2 O+K 2 The upper limit of O may be 4% or less, 3% or less, 2% or less, 1.5% or less, 1% or less, or even 0.9% or less.

[0031] Li 2 Excessive inclusion of O increases the dielectric constant of the glass and reduces the water resistance. 2 The lower limit of the O content may be 0.1% or more, 0.2% or more, 0.3% or more, 0.4% or more, or even 0.5% or more. 2 The upper limit of the O content may be 4% or less, 3% or less, 2% or less, 1.5% or less, 1% or less, or even 0.9% or less.

[0032] Na 2 Excessive inclusion of O increases the dielectric constant of the glass and reduces the water resistance. 2 The increase in the dielectric constant due to O is 2 It is larger than O. 2 The upper limit of the O content may be 4% or less, 2% or less, 1.5% or less, 1% or less, 0.5% or less, 0.3% or less, or even 0.2% or less.

[0033] K 2 Excessive O content increases the dielectric constant of the glass and reduces the water resistance. 2 The increase in the dielectric constant due to O is 2 It is larger than O. 2 The upper limit of the O content may be 4% or less, 2% or less, 1% or less, 0.5% or less, 0.2% or less, or even less than 0.1%. 2 O may not be substantially contained.

[0034] (TiO 2 ) The glass composition is TiO 2 It may contain TiO 2 TiO can have the effect of improving the meltability and chemical durability of the glass, as well as improving the ultraviolet absorbing properties of the glass. On the other hand, an excessive content of TiO increases the dielectric constant of the glass. 2 The lower limit of the content of TiO may be 0.1% or more. 2 The upper limit of the content of TiO may be 5% or less, 2% or less, less than 1%, 0.9% or less, 0.8% or less, 0.7% or less, less than 0.5%, 0.4% or less, 0.3% or less, 0.2% or less, or even 0.1% or less. 2 The increase in the devitrification temperature of molten glass, which is caused by the inclusion of TiO and affects the production of glass fillers, can be suppressed. 2 may not be substantially contained.

[0035] (ZrO 2 ) The glass composition is ZrO 2 It may contain ZrO 2 ZrO can have the effect of adjusting the devitrification temperature and viscosity during glass formation. On the other hand, excessive content increases the dielectric constant of the glass. 2 The upper limit of the content of ZrO may be 5% or less, 2% or less, less than 1%, less than 0.5%, 0.2% or less, or even 0.1% or less. 2It is possible to suppress the increase in the devitrification temperature of molten glass, which is caused by the inclusion of ZrO and affects the production of glass fillers. 2 The lower limit of the content of ZrO may be 0.1% or more, and further 0.15% or more. 2 may not be substantially contained.

[0036] (Fe) The glass composition may contain Fe. The Fe in the glass is usually Fe 2+ and / or Fe 3+ It exists in the state of Fe 3+ Fe can have the effect of enhancing the ultraviolet absorbing properties of the glass. 2+ It can have the effect of enhancing the heat ray absorption properties of glass. Even if it is not intentionally added, Fe can be unavoidably mixed in as a result of industrial raw materials. If the Fe content is small, it is possible to prevent the glass from becoming discolored. The upper limit of the Fe content is T-Fe 2 O 3 (T-Fe 2 O 3 is Fe 2 O 3 The Fe content may be expressed in terms of total iron oxide (T-Fe) or less, 5% or less, 2% or less, less than 1.8%, 1.5% or less, less than 1%, less than 0.5%, or even 0.2% or less. 2 O 3 The content of Fe may be expressed as T-Fe. 2 O 3 It is acceptable for the content to be expressed by "substantially not contained."

[0037] (P 2 O 5 ) The glass composition is P 2 O 5 It can include 2 O 5 is a component that forms the skeleton of the glass and can also have the effect of adjusting the devitrification temperature and viscosity during glass formation. 2 O 5 can have the effect of adjusting the dielectric constant of the glass. 2 O 5If the content exceeds 2%, it is said that the walls of the melting kiln and the heat storage kiln are corroded when melting glass, and the life of the kiln is significantly shortened. 2 O 5 The upper limit of the content of may be 5% or less, 2% or less, less than 1%, less than 0.5%, 0.3% or less, 0.2% or less, or even less than 0.1%. 2 O 5 may not be substantially contained.

[0038] (F 2 , Cl 2 ) The glass composition is F 2 and / or Cl 2 It can include F 2 and Cl 2 When contained in the glass composition, F improves the uniformity of the glass when the raw materials are melted without excessively increasing the melting point of the glass. 2 and Cl 2 F is prone to volatilization, and therefore may scatter during melting. In addition, there is also the problem that it is difficult to control the content in the glass. 2 The upper limit of the content of may be 5% or less, 2% or less, 1% or less, 0.5% or less, 0.2% or less, or even 0.1% or less. 2 may not be substantially contained. 2 The upper limit of the content of Cl may be 5% or less, 2% or less, 1% or less, 0.5% or less, 0.2% or less, or even 0.1% or less. 2 may not be substantially contained.

[0039] (Other Ingredients) The glass composition contains, as other components, La 2 O 3 , WO 3 , Nb 2 O 5 , Y 2 O 3 , MoO 3 , Ta 2 O 5 , MnO 2 and Cr 2 O 3At least one selected from the group consisting of may be contained in the range of 0% to 5%. The upper limit of the content of each component may be less than 2%, less than 1%, less than 0.5%, or even less than 0.1%. The upper limit of the total content of each component may be less than 5%, less than 2%, less than 1%, less than 0.5%, or even less than 0.1%. Any one component selected from the above group may not be substantially contained. Furthermore, any combination of two or more components selected from the above group may not be substantially contained.

[0040] The glass composition contains, as an additive, Br 2 , I 2 , SnO 2 , CEO 2 , As 2 O 3 and Sb 2 O 3 At least one selected from the group consisting of may be contained in the range of 0% to 1%. The upper limit of the content of each component may be less than 0.5%, less than 0.2%, or even less than 0.1%. The upper limit of the total content of each component may be less than 1%, less than 0.5%, less than 0.2%, or even less than 0.1%. Any one component selected from the above group may not be substantially contained. Furthermore, any combination of two or more components selected from the above group may not be substantially contained.

[0041] The glass composition is H 2 O, OH, H 2 , CO 2 , CO, He, Ne, Ar and N 2At least one selected from the group consisting of may be contained in the range of 0% or more and 0.1% or less. The upper limit of the content of each component may be less than 0.05%, less than 0.03%, or even less than 0.01%. The upper limit of the total content of each component may be 0.1% or less, less than 0.05%, less than 0.03%, or even less than 0.01%. Any one component selected from the above group may not be substantially contained. Furthermore, any combination of two or more components selected from the above group may not be substantially contained.

[0042] The glass composition may contain a trace amount of a precious metal element. Examples of the precious metal element are Pt, Rh, Au, and Os. The content of each of the precious metal elements is 0% or more and 0.1% or less. The upper limit of the content allowed for each component may be less than 0.1%, less than 0.05%, less than 0.03%, or even less than 0.01%. The upper limit of the total content of each component may be less than 0.1%, less than 0.05%, less than 0.03%, or even less than 0.01%. Each component may be substantially absent.

[0043] The glass composition may consist essentially of any combination of the above-mentioned components and contents. The term "substantially" in "consist essentially of" means that the glass composition may contain impurities with a content of less than 0.1 mass%, preferably less than 0.07 mass%, more preferably less than 0.05 mass%, particularly preferably less than 0.01 mass%, and most preferably less than 0.005 mass%.

[0044] (Example of a preferred composition) In one preferred embodiment, the glass composition comprises Expressed in mass%, 55≦SiO 2 <= 65 20≦B 2 O 3 <= 30 5≦Al 2 O 3 <= 20 Including, 0.1≦(MgO+CaO)<5 0≦(Li 2 O+Na 2 O+K 2 O) ≦4, and 0.75≦MgO / (MgO+CaO)≦1.00 holds true.

[0045] In another preferred embodiment, the glass composition comprises Expressed in mass%, 50≦SiO 2 <= 65 20≦B 2 O 3 <= 30 5≦Al 2 O 3 <= 20 0≦F 2 ≦0.5 Including, 0.1≦(MgO+CaO)<5 0.1≦(Li 2 O+Na 2 O+K 2 O) ≦4, and 0.50 <MgO / (MgO+CaO)≦1.00 holds true.

[0046] In another preferred embodiment, the glass composition comprises Expressed in mass%, 50≦SiO 2 <= 65 20≦B 2 O 3 <= 30 5≦Al 2 O 3 <= 15 Including, 0.1≦(MgO+CaO)<5 0≦(Li 2 O+Na 2 O+K 2 O) ≦4, and 0.50 <MgO / (MgO+CaO)≦1.00 holds true.

[0047] In another preferred embodiment, the glass composition comprises Expressed in mass%, 50≦SiO 2 <= 65 20≦B 2 O 3 <= 30 5≦Al 2 O 3 <= 20 0.1≦TiO 2 <=5 Including, 0.1≦(MgO+CaO)<5 0.1≦(MgO+CaO+ZnO)≦6 0≦(Li 2 O+Na 2 O+K 2 O) ≦4, and 0.50 <MgO / (MgO+CaO)≦1.00 holds true.

[0048] In another preferred embodiment, the glass composition has a content of 0.1≦Li, expressed in mass %. 2 O≦4 is included. The glass composition of this aspect may be any of the glass compositions of the above preferred aspects.

[0049] In another preferred embodiment, the glass composition has a content of 0≦P, expressed in mass %. 2 O 5 The glass composition of this aspect may be any of the glass compositions of the above preferred aspects.

[0050] In another preferred embodiment, the glass composition is 2 The glass composition of this embodiment may be any of the glass compositions of the above preferred embodiments.

[0051] The glass composition in another preferred embodiment further contains, expressed in mass %, 0≦ZnO≦5. The glass composition of this embodiment may be any of the glass compositions of the above preferred embodiments.

[0052] The glass composition in another preferred embodiment further contains, expressed in mass %, 0≦BaO≦5. The glass composition of this embodiment may be any of the glass compositions of the above preferred embodiments.

[0053] In another preferred embodiment, the glass composition further contains, expressed in mass %, 0≦SrO≦5. The glass composition of this embodiment may be any of the glass compositions of the above preferred embodiments.

[0054] In another preferred embodiment, the glass composition has a content of 0≦ZrO 2 The glass composition of this aspect may be any of the glass compositions of the above preferred aspects.

[0055] [Characteristics of glass composition] The properties that the glass composition of the present invention can have will be described below. The glass filler containing the glass composition of the present invention can have the following properties.

[0056] (Dielectric constant) When the glass filler is blended in the resin composition, if the dielectric constant of the glass composition constituting the glass filler at a frequency of 1 GHz is 4.6 or less, the loss of the dielectric properties of the resin composition can be suppressed. In a preferred embodiment, the dielectric constant of the glass composition at a frequency of 1 GHz may be 4.6 or less, 4.5 or less, 4.4 or less, or even 4.3 or less. The lower limit of the dielectric constant at a frequency of 1 GHz may be 3.5 or more, 3.8 or more, 3.9 or more, or even 4.0 or more. If the dielectric constant at a frequency of 1 GHz is 3.5 or more, the adjustment of the glass composition becomes relatively easy.

[0057] (melting characteristics) The temperature at which the viscosity of the molten glass is 1000 dPa·sec (1000 poise) is called the working temperature, and is the temperature most suitable for forming glass. When producing flaky glass or glass fiber as a glass filler, if the working temperature of the glass is 1100°C or higher, the variation in the thickness of the flaky glass or the diameter of the glass fiber can be reduced. If the working temperature is 1450°C or lower, the fuel cost for melting the glass can be reduced, the glass manufacturing equipment is less susceptible to corrosion due to heat, and the equipment life can be extended. In a preferred embodiment, the lower limit of the working temperature of the glass composition may be 1100°C or higher, 1150°C or higher, 1200°C or higher, 1250°C or higher, 1300°C or higher, or even 1320°C or higher. The upper limit of the working temperature may be 1450°C or lower, 1420°C or lower, 1410°C or lower, 1400°C or lower, 1390°C or lower, or even 1380°C or lower.

[0058] The larger the temperature difference ΔT obtained by subtracting the devitrification temperature from the working temperature, the less likely devitrification occurs during glass molding, and a homogeneous glass filler can be produced with a high yield. In other words, the larger the temperature difference ΔT, the more improved the moldability (mass productivity) of the glass filler. In a preferred embodiment, ΔT of the glass composition may be 0°C or more, 17°C or more, 20°C or more, 30°C or more, 40°C or more, 50°C or more, 60°C or more, 70°C or more, 75°C or more, 80°C or more, 90°C or more, 100°C or more, 125°C or more, 150°C or more, 170°C or more, 190°C or more, or even 200°C or more. On the other hand, if ΔT is 500°C or less, adjustment of the glass composition is relatively easy. ΔT may be 500°C or less, 400°C or less, 300°C or less, 250°C or less, or even 200°C or less.

[0059] (water resistance) The amount of alkali elution can be used as an index of water resistance. The smaller the amount of alkali elution, the higher the water resistance of the glass. When a glass filler is blended into a resin composition, if the amount of alkali elution of the glass composition is 0.40 mg or less, the strength of the resin composition is suppressed from decreasing due to water. In a preferred embodiment, the upper limit of the amount of alkali elution of the glass composition may be 0.40 mg or less, 0.37 mg or less, 0.35 mg or less, 0.34 mg or less, or even 0.33 mg or less. The lower limit of the amount of alkali elution is usually about 0.001 mg, and may be 0.01 mg or more, or even 0.03 mg or more.

[0060] [Glass filler] The glass filler of the present invention includes the glass composition of the present invention. An example of the form of the glass filler is at least one selected from the group consisting of flake glass, chopped strands, milled fibers, glass powder, glass beads, flat fibers, and fine flakes. However, the form of the glass filler is not limited to the above examples. In addition, the above forms are not strictly distinguished from each other. Two or more glass fillers having different forms may be combined and used as a filler, for example, a mixture. Each form will be described below.

[0061] The glass flakes are typically thin particles having an average thickness t of 0.1 μm to 15 μm, an average particle diameter a of 0.2 μm to 15,000 μm, and an aspect ratio (average particle diameter a / average thickness t) of 2 to 1,000 (see FIG. 1A and FIG. 1B; FIG. 1A and FIG. 1B show an example of glass flake 1). The average thickness t of the glass flakes can be evaluated by extracting at least 100 glass flakes, measuring the thickness of each of the extracted glass flakes using a magnifying observation means such as a scanning electron microscope (SEM), and calculating the average value of the measured thicknesses. The average particle diameter a of the glass flakes can be determined by the particle diameter (D50) corresponding to a cumulative volume percentage of 50% in the particle size distribution measured by a laser diffraction scattering method.

[0062] Glass flakes can be obtained by known methods such as the blowing method and the cup method. A manufacturing apparatus using the blowing method is shown in Fig. 2. In this apparatus, glass base 11 having a predetermined composition molten in a refractory kiln tank 12 is expanded into a balloon shape by gas sent into a blow nozzle 15, forming a hollow glass film 16. This hollow glass film 16 is crushed by a pair of pressure rolls 17, thereby obtaining glass flakes 1.

[0063] A manufacturing apparatus using the cup method is shown in Fig. 3. In this apparatus, molten glass base material 11 is poured from a nozzle 21 into a rotating cup 22 and flows out radially from the upper edge of the rotating cup 22 due to centrifugal force generated by the rotation of the rotating cup 22. The flowed-out base material 11 is sucked by air flow through upper and lower annular plates 23, 23 and introduced into an annular cyclone collector 24. While passing through the annular plates 23, 23, the glass cools and solidifies into a thin film, and is then crushed into minute pieces, obtaining glass flakes 1.

[0064] The chopped strand has a shape in which glass fibers are cut into short pieces. The chopped strand has a fiber diameter of, for example, 1 to 50 μm, and an aspect ratio of, for example, 2 to 1000. The cross-sectional shape of the chopped strand may or may not be circular, and may be, for example, a flat cross-sectional shape. The fiber diameter of the chopped strand is defined as the diameter of a circle having the same area as the cross-sectional area of ​​the strand. The aspect ratio of the chopped strand can be determined by dividing the fiber length by the fiber diameter. The chopped strand can be produced, for example, by using the apparatus shown in FIG. 4 and FIG. 5.

[0065] As shown in FIG. 4, a glass base material having a predetermined composition is melted in a refractory kiln and drawn out from a bushing 30 having a number of (e.g., 2,400) nozzles at the bottom, and drawn out as a number of glass filaments 31. After cooling water is sprayed onto the glass filaments 31, a binder (bundling agent) 34 is applied by an application roller 33 of a binder applicator 32. The number of glass filaments 31 to which the binder 34 has been applied are bundled by a reinforcing pad 35 into three strands 36, each of which is composed of, for example, about 800 glass filaments 31. Each strand 36 is traversed by a traverse finger 37 and wound up on a cylindrical tube 39 fitted in a collet 38. The cylindrical tube 39 on which the strand 36 has been wound is removed from the collet 38, and a cake (strand winding body) 40 is obtained.

[0066] 5, the cake 40 is placed in a creel 41, and the strands 36 are pulled out from the cake 40 and bundled into a strand bundle 43 by a bundling guide 42. Water or a treatment liquid is sprayed onto the strand bundle 43 by a spray device 44. The strand bundle 43 is cut by a rotary blade 46 of a cutting device 45 to obtain chopped strands 47.

[0067] The milled fiber has a shape in which glass fibers are cut into a powder form. The milled fiber has a fiber diameter of, for example, 1 to 50 μm, and an aspect ratio of, for example, 2 to 500. The cross-sectional shape of the milled fiber may or may not be circular, and may be, for example, a flat cross-sectional shape. The fiber diameter of the milled fiber is defined as the diameter of a circle having the same area as the cross-section of the strand. The aspect ratio of the milled fiber can be determined by dividing the fiber length by the fiber diameter. The milled fiber can be obtained by a known method.

[0068] The glass powder can be produced by pulverizing glass. The average particle size of the glass powder is, for example, 1 to 500 μm. The particle size of the glass powder is defined as the diameter of a sphere having the same volume as a particle of the glass powder. The average particle size of the glass powder can be defined by D50 (particle size corresponding to a cumulative volume percentage of 50%) evaluated by particle size distribution measurement by a laser diffraction scattering method for at least 0.1 g of glass powder. The glass powder can be obtained by a known method.

[0069] The glass beads have a spherical or nearly spherical shape. The average particle size of the glass beads is, for example, 1 to 500 μm. The particle size of the glass beads is defined as the diameter of a sphere having the same volume as a glass bead particle. The average particle size of the glass beads can be determined by D50 (particle size corresponding to a cumulative volume percentage of 50%) evaluated by particle size distribution measurement by a laser diffraction scattering method for at least 0.1 g of glass beads. The glass beads can be obtained by a known method.

[0070] The flat fiber has a shape obtained by cutting a glass fiber having a flat cross section such as an ellipse. As shown in FIG. 6, the major axis D2 of the cross section of the flat fiber 50 is larger than the minor axis D1, and D2 / D1 is, for example, 1.2 or more. The minor axis D1 is, for example, 0.5 to 25 μm. The major axis D2 is, for example, 0.6 to 300 μm. The length L of the flat fiber is, for example, 10 to 1000 μm. As shown in FIG. 7, the cross section of the flat fiber 60 may have a shape that is constricted at the center. In other words, the cross section of the flat fiber 60 may have a concave shape in which the surface extending along the major axis D2 is recessed from the ends at the center. This cross section is approximately gourd-shaped or approximately hourglass-shaped, with the center in the direction along the major axis D2 recessed from both sides.

[0071] Fine flakes are thin flake glass. Fine flakes may be composed of glass flakes having an average thickness of 0.1 to 2.0 μm, or may contain glass flakes having a thickness in the range of 0.01 to 2.0 μm at a ratio of 90 mass % or more. Fine flakes having such a small average thickness and small thickness variation are highly effective in reinforcing resin and are also excellent in reducing the molding shrinkage rate of resin. Fine flakes can be obtained by the above-mentioned method.

[0072] The glass filler can be produced by a method including a step of melting the above-mentioned glass composition and a step of forming the molten glass composition into a desired glass filler. The temperature at which the glass composition is melted is, for example, 1400° C. or higher.

[0073] [Granulation of glass filler] The glass filler may be at least partially granulated. Granulation is a process in which the glass filler is subjected to a binder treatment, and the individual glass fillers are bound to each other by the binder to form granules. Granular glass filler has low scattering properties and is therefore excellent in workability and dispersibility in resin. The use of granular glass filler improves the feedability and enables more reliable quantitative feeding. The binder used for granulation is described below.

[0074] The binder preferably contains a surfactant and a binding component. The surfactant may be any of anionic, cationic, amphoteric, and nonionic. However, when the binding component contains an epoxy resin or a urethane resin, the use of a nonionic surfactant is preferable. This is because it is possible to suppress the aggregation of the binder and stabilize it. Examples of anionic surfactants are sodium dioctyl sulfosuccinate, fatty acid salts, alkyl sulfate ester salts, alkyl sulfonate salts, alkylaryl sulfonate salts, alkylnaphthalene sulfonate salts, alkyl sulfosuccinate salts, alkyl diphenyl ether disulfonate salts, alkyl phosphate salts, polyoxyethylene alkyl sulfate ester salts, polyoxyethylene alkylaryl sulfate ester salts, and sulfosuccinate ester salts. Examples of cationic surfactants are higher amine halogen acid salts, alkyl pyridinium halides, and quaternary ammonium salts. Examples of amphoteric surfactants are lauryl aminopropionate salts and lauryl dimethyl betaine. Examples of nonionic surfactants include polyoxyethylene glycol alkyl ethers such as polyoxyethylene lauryl ether, polyoxyethylene higher alcohol ether, and polyoxyethylene octylphenyl ether, polyethylene glycol fatty acid esters such as polyethylene glycol monostearate, sorbitan fatty acid esters such as sorbitan monolaurate and polyoxyethylene sorbitan monolaurate, glycol fatty acid esters such as glycol monostearate, and fatty acid monoglycerides. Two or more of these may be used in combination.

[0075] The binder binding component is not particularly limited, and organic or inorganic components can be used. Examples of organic binding components include methyl cellulose, carboxymethyl cellulose, starch, carboxymethyl starch, hydroxyethyl cellulose, hydroxypropyl cellulose, polyvinyl alcohol, silane coupling agents, acrylic resins, epoxy resins, phenolic resins, vinyl acetate, and urethane resins. Examples of inorganic binding components include water glass, colloidal silica, colloidal alumina, and aminosilane. The binding component preferably contains at least one selected from a silane coupling agent, an epoxy resin, and a urethane resin. The silane coupling agent has two or more reactive groups in the molecule, one of which reacts with the surface of the glass filler and the other reacts with the organic binding component and the thermoplastic resin, improving the compatibility between the glass filler and the thermoplastic resin. The epoxy resin and the urethane resin have good compatibility with the silane coupling agent and the thermoplastic resin.

[0076] The binder is preferably adjusted in concentration to allow each component to be uniformly present on the surface of the glass filler using water or alcohol as a solvent. The binder concentration is preferably 1 to 10 mass% expressed as total solids concentration. The binder can be produced, for example, by adding a binding component, a surfactant, etc. to a solvent at room temperature and atmospheric pressure as appropriate and stirring until it becomes uniform.

[0077] The ratio of the binder in the granulated glass filler, in other words, the adhesion rate of the binder, is, for example, 0.1 to 2 mass% in terms of solid mass ratio. An adhesion rate of 0.1 mass% or more is suitable for sufficiently suppressing the scattering of the glass filler. An adhesion rate of 2 mass% or less is suitable for suppressing gas generation during extrusion molding of the resin composition and discoloration of the resin composition.

[0078] The method for granulating the glass filler is not particularly limited, and for example, agitation granulation, fluidized bed granulation, spray granulation, rotary granulation, etc. can be used. Specifically, a method can be applied in which a glass filler to which an appropriate amount of binder has been attached by spraying or the like is spread in a rotating drum or on a vibrating tray, and granulated while being heated to evaporate the solvent. Granular glass filler of a desired size can be produced by appropriately adjusting the rotation speed of the rotating drum or the vibration frequency of the vibrating tray, and further the evaporation rate of the solvent.

[0079] The glass filler may be surface-treated with a surface treatment agent. This treatment may improve the reinforcing effect of the glass filler. Examples of the surface treatment agent include silicon-based coupling agents such as γ-aminopropyltriethoxysilane, vinyltriethoxysilane, and γ-methacryloxypropyltrimethoxysilane, and titanium-based coupling agents. The amount of the surface treatment agent used is, for example, 0.05 to 0.20% by mass of the glass filler.

[0080] [Resin composition] The resin composition according to the present invention contains a thermoplastic resin together with the glass filler according to the present invention. The thermoplastic resin is not particularly limited, but may be, for example, polyvinyl chloride, polypropylene, polyethylene, polystyrene, polyester, polyamide, polycarbonate, polybutylene, polybutylene terephthalate, or a copolymer thereof. When polybutylene terephthalate is used, the effect of suppressing warpage of a molded product and improving dimensional stability due to mixing with the glass filler is increased.

[0081] The content of glass filler such as glass flakes in the resin composition is preferably 5 to 70% by mass. By making it 5% by mass or more, the glass filler is more likely to fully exhibit its function as a reinforcing material. By making it 70% by mass or less, it is easier to uniformly disperse the glass filler in the resin composition. In order to sufficiently suppress the molding shrinkage rate, the content of the glass filler is more preferably 30% by mass or more.

[0082] The resin composition may contain a reinforcing material other than the glass filler as appropriate. For example, in applications requiring high strength, glass fibers may be contained. In this case, the glass fibers may be added at a content similar to that of the glass filler.

[0083] Glass flakes, flat fibers, and fine flakes have a relatively large specific surface area and are suitable for securing bonding strength with thermoplastic resins. From this viewpoint, the flat fiber shown in Fig. 7 is preferable because its concave surface shape contributes to increasing the specific surface area.

[0084] The resin composition according to the present invention has a low dielectric constant and is suitable for improving various properties such as improving strength, heat resistance, dimensional stability, lowering the coefficient of linear thermal expansion and reducing anisotropy, and reducing the anisotropy of shrinkage during molding. EXAMPLES

[0085] The present invention will be described in more detail below with reference to examples. The present invention is not limited to the following examples. ~8、 11 ~ 14. 16~20 , 22, 23, 25~ 31 , 33-36, 38、 40, 41、 43 ~ Nos. 47 and 50 are reference examples.

[0086] (Examples 1 to 53 and Comparative Examples 1 to 6) Common glass raw materials such as silica sand were weighed out to obtain each composition shown in Tables 1 to 12 (the unit of the content of the components is mass %), and mixed to obtain a homogeneous state to prepare a glass raw material mixed batch. Next, the prepared mixed batch was melted at 1500 to 1600°C in an electric furnace and maintained as such for about 4 hours until the composition became homogeneous. After that, a part of the obtained molten glass (glass melt) was poured onto an iron plate and slowly cooled to room temperature in the electric furnace to obtain a bulk glass composition sample (plate-shaped) to be used for evaluation.

[0087] The glass samples thus prepared were evaluated for working temperature, devitrification temperature, temperature difference ΔT, amount of alkali elution, and dielectric constant at a frequency of 1 GHz. The evaluation methods are as follows.

[0088] [Working temperature] The viscosity was measured using the platinum sphere pulling method, and the temperature at which the measured viscosity reached 1000 dPa·sec was defined as the working temperature. The platinum sphere pulling method is a method for measuring the viscosity of molten glass by applying the relationship between the load (resistance) applied when the immersed platinum sphere is pulled up at a uniform speed and the gravity and buoyancy acting on the platinum sphere to Stokes' law, which shows the relationship between the viscosity and falling speed of microscopic particles as they sink through a fluid.

[0089] [Devitrification temperature and temperature difference ΔT] 25 g of glass sample crushed to a particle size of 1.0 to 2.8 mm was placed in a platinum boat (a rectangular platinum vessel without a lid) and held in an electric furnace with a temperature gradient (800 to 1400 ° C) for 2 hours, then removed from the furnace, and the maximum temperature of the electric furnace corresponding to the position where crystals were observed inside the glass was taken as the devitrification temperature. The above particle size range was determined by a sieving method. Specifically, the glass sample was crushed, passed through a sieve with a mesh size of 2.8 mm (mesh sieve, the same applies below for sieves), and the particles remaining on a sieve with a mesh size of 1.0 mm were sieved out. The temperature difference ΔT was determined by subtracting the devitrification temperature from the working temperature.

[0090] [Alkaline elution amount] The amount of alkaline elution was measured in accordance with the alkaline elution test stipulated in JIS R3502:1995 "Testing methods for glassware for chemical analysis." Specifically, the procedure is as follows. The glass sample was crushed, passed through a sieve with 420 μm openings, and the particles remaining on a sieve with 250 μm openings were sieved. Next, particles with the same mass as the specific gravity of the glass sample were weighed out from the sieved particles. The weighed particles were immersed in 50 mL of distilled water at 100°C for 1 hour, and the alkaline components contained in the water after immersion were titrated with sulfuric acid with a concentration of 0.01 N. The amount of Na was determined by multiplying the number of milliliters of sulfuric acid required for the titration by 0.31. 2The amount of alkali elution was determined as the number of milligrams of the alkali component converted into O. The smaller the amount of alkali elution, the higher the water resistance of the glass sample.

[0091] [Dielectric constant] The dielectric constant at a frequency of 1 GHz was measured using a dielectric constant measurement device using a cavity resonator perturbation method. The measurement temperature was 25°C, and the dimensions of the measurement sample were a rectangular parallelepiped with a height of 100 mm and a square base with sides of 1.5 mm.

[0092] The evaluation results are shown in Tables 1 to 12.

[0093] [Table 1]

[0094] [Table 2]

[0095] [Table 3]

[0096] [Table 4]

[0097] [Table 5]

[0098] [Table 6]

[0099] [Table 7]

[0100] [Table 8]

[0101] [Table 9]

[0102] [Table 10]

[0103] [Table 11]

[0104] [Table 12]

[0105] For Examples 1 to 53, the working temperature was 1340 to 1441° C., the temperature difference ΔT (=working temperature−devitrification temperature) was 39 to 408° C., the alkali elution amount was 0.03 to 0.33 mg, and the dielectric constant at a frequency of 1 GHz was 4.1 to 4.5.

[0106] In contrast, Comparative Example 1, which had a glass composition equivalent to conventional E-glass, exhibited a high dielectric constant exceeding 6.0.

[0107] Comparative Example 2, which had a glass composition equivalent to the conventional D-glass, showed a higher amount of alkaline elution than Examples 1-53.

[0108] In Comparative Example 3, SiO 2 and B. 2 O 3 The content of was outside the range defined in the present invention. Comparative Example 3 showed a high alkali elution amount exceeding 1.0 mg.

[0109] Comparative Example 4 did not contain MgO or CaO and showed a high amount of alkaline elution exceeding 1.0 mg.

[0110] In Comparative Example 5, MgO / (MgO+CaO) was outside the range defined in the present invention. Comparative Example 5 showed a higher amount of alkaline elution than Examples 1-53.

[0111] In Comparative Example 6, Li 2 O+Na 2 O+K 2 O was outside the range defined in the present invention. Comparative Example 6 showed a high alkaline elution amount of more than 1.0 mg.

[0112] (Examples 54 to 106) Glass flakes were produced using each of the glass compositions produced in Examples 1 to 53. Specifically, each glass composition was remelted in an electric furnace, and then molded into pellets while cooling. The resulting pellets were placed in a melting furnace to produce glass flakes having an average thickness of 1 to 2 μm and an average particle size of 100 to 500 μm.

[0113] (Examples 107 to 159) Using each of the glass compositions produced in Examples 1 to 53, chopped strands that can be used as glass fillers were produced. Specifically, each glass composition was remelted in an electric furnace, and then molded into pellets while cooling. The obtained pellets were fed into the production apparatus shown in Figs. 4 and 5 to produce chopped strands with an average fiber diameter of 10 to 20 µm and a length of 3 mm.

[0114] (Examples 160 to 212) Milled fibers were produced using the chopped strands produced in Examples 107 to 159. Specifically, chopped strands having an average fiber diameter of 10 to 20 μm and a length of 3 mm were pulverized in an alumina ball mill to produce milled fibers having an average fiber diameter of 10 to 20 μm and an average length of 50 to 100 μm.

[0115] (Examples 213 to 265) Fine flakes were produced using each of the glass compositions produced in Examples 1 to 53. Specifically, each glass composition was remelted in an electric furnace, and then molded into pellets while cooling. The resulting pellets were placed in a melting furnace to produce fine flakes with an average thickness of 0.5 to 1 μm and an average particle size of 100 to 300 μm. [Industrial Applicability]

[0116] The glass composition of the present invention can be used, for example, for producing a glass filler. The glass filler of the present invention can be used in the same applications as conventional glass fillers.

Claims

1. Expressed in mass %, 50≦SiO 2 ≦65 20≦B 2 O 3 ≦30 5≦Al 2 O 3 ≦12.68 Including, At least one selected from the group consisting of MgO and CaO; Li 2 O, Na 2 O and K 2 At least one selected from the group consisting of O; Further comprising: 0.1≦(MgO+CaO)≦4 0.7 ≤ (Li 2 O + Na 2 O + K 2 O) ≤ 4, and 0.80≦MgO / (MgO+CaO)≦1.00 is established, A glass composition having a BaO content of 0.5% or less.

2. The glass composition comprises, expressed in mass %, 55≦SiO 2 ≦65 20≦B 2 O 3 ≦30 5≦Al 2 O 3 ≦12.68 Including, 0.1≦(MgO+CaO)≦4 0.7 ≤ (Li 2 O + Na 2 O + K 2 O) ≤ 4, and 0.80≦MgO / (MgO+CaO)≦1.00 The glass composition according to claim 1 , wherein

3. The glass composition comprises, expressed in mass %, 50≦SiO 2 ≦65 20≦B 2 O 3 ≦30 5≦Al 2 O 3 ≦12.68 0≦F 2 ≦0.5 Including, 0.1≦(MgO+CaO)≦4 0.7 ≤ (Li 2 O + Na 2 O + K 2 O) ≤ 4, and 0.80≦MgO / (MgO+CaO)≦1.00 The glass composition according to claim 1 , wherein

4. The glass composition comprises, expressed in mass %, 50≦SiO 2 ≦65 20≦B 2 O 3 ≦30 5≦Al 2 O 3 ≦12.68 0.1≦TiO 2 ≦5 Including, 0.1≦(MgO+CaO)≦4 0.1≦(MgO+CaO+ZnO)≦6 0.7 ≤ (Li 2 O + Na 2 O + K 2 O) ≤ 4, and 0.80≦MgO / (MgO+CaO)≦1.00 The glass composition according to claim 1 , wherein

5. The glass composition comprises, expressed in mass %, 0.1≦Li 2 O≦4 The glass composition according to any one of claims 1 to 4, comprising:

6. The glass composition comprises, expressed in mass %, 0.18≦Li 2 O≦4 The glass composition of claim 5 , comprising:

7. The glass composition comprises, expressed in mass %, 0≦T-Fe 2 O 3 ≦1.5、 The glass composition according to any one of claims 1 to 6, further comprising: However, T-Fe 2 O 3 is Fe 2 O 3 This is the total iron oxide converted to

8. The glass composition comprises, expressed in mass %, 0≦P 2 O 5 ≦5、 The glass composition according to any one of claims 1 to 7, further comprising:

9. The glass composition is F 2 The glass composition according to any one of claims 1 to 8, which is substantially free of:

10. The glass composition comprises, expressed in mass %, 0≦ZnO≦5, The glass composition according to any one of claims 1 to 9, further comprising:

11. The glass composition comprises, expressed in mass %, 0≦BaO≦0.1, The glass composition according to any one of claims 1 to 10, further comprising:

12. The glass composition comprises, expressed in mass %, 0≦SrO≦5, The glass composition according to any one of claims 1 to 4, further comprising:

13. The glass composition comprises, expressed in mass %, 0≦ZrO 2 ≦5、 The glass composition according to any one of claims 1 to 12, further comprising:

14. 14. The glass composition according to claim 1, wherein the glass composition has a dielectric constant of 4.6 or less at a frequency of 1 GHz.

15. The glass composition according to any one of claims 1 to 14, wherein the working temperature of the glass composition is 1450°C or less. However, the working temperature is a temperature at which the viscosity of the glass composition is 1000 dPa·sec.

16. The glass composition according to any one of claims 1 to 15, wherein the glass composition has a temperature difference ΔT obtained by subtracting the devitrification temperature from the working temperature of the glass composition of 0°C or more. However, the working temperature is a temperature at which the viscosity of the glass composition is 1000 dPa·sec.

17. 17. The glass composition according to claim 1, wherein an amount of alkali elution from the glass composition measured in accordance with an alkali elution test specified in JIS R3502:1995 is 0.001 to 0.40 mg.

18. A glass filler comprising the glass composition according to any one of claims 1 to 17.

19. The glass filler according to claim 18, which corresponds to at least one selected from the group consisting of glass flakes, chopped strands, milled fibers, glass powders, glass beads, flat fibers, and fine flakes.

20. The glass filler according to claim 18, which is a glass flake.

21. 19. The glass filler according to claim 18, which is a chopped strand.

22. 19. The glass filler according to claim 18, which is a milled fiber.

23. 19. The glass filler according to claim 18, which is a fine flake.

24. A resin composition comprising the glass filler according to any one of claims 18 to 23 and a thermoplastic resin.

25. The method includes melting the glass composition according to any one of claims 1 to 17, and forming the molten glass composition into a glass filler. A method for manufacturing a glass filler.

Citation Information

Patent Citations

  • Method of producing multilayer circuit board

    JP1984009992A

  • Glass fiber having low dielectric constant

    JP1987226839A

  • Glass fiber having low dielectric loss tangent

    JP1997002839A

  • Low-dielectric constant glass powder and printed circuit board using the same and resin-mixed material

    JP1997268025A

  • Low dielectric constant low dielectric dissipation factor glass, and glass fiber and glass fiber fabric using the glass

    JP2003137590A