Flexible polyurethane foam and formulations thereof

Low surface area fumed silica with trimethylsilyl groups and a tertiary amine catalyst improve the mechanical properties of flexible polyurethane foams by enhancing compressive force deflection and reducing dry compression set during in-situ polymerization.

JP7576168B2Active Publication Date: 2024-10-30CABOT CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023519973
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-10-01
Filing Date
2021-09-29
Publication Date
2024-10-30
Estimated Expiration
2041-09-29

AI Technical Summary

Technical Problem

Existing polyurethane foam formulations face challenges in achieving optimal mechanical properties and stability during in-situ polymerization processes, particularly in the formation of flexible open-cell foams, due to interference from fillers like fumed silica that can affect viscosity and cell structure.

Method used

The use of low surface area fumed silica with trimethylsilyl groups in combination with a tertiary amine catalyst allows for controlled polymerization, resulting in flexible polyurethane foams with improved properties such as increased compressive force deflection and reduced dry compression set.

Benefits of technology

The solution enhances the mechanical properties of flexible polyurethane foams by increasing compressive force deflection and maintaining flexibility, while minimizing interference with polymerization processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576168000017
    Figure 0007576168000017
  • Figure 0007576168000018
    Figure 0007576168000018
  • Figure 0007576168000019
    Figure 0007576168000019
Patent Text Reader

Abstract

50~150m 2 A flexible polyurethane foam comprising 10% by weight or less of fumed silica having a surface area of ​​1 / g, the fumed silica having C1-C3 alkylsilyl groups on its surface, wherein the flexible polyurethane foam has a resilience of at least 40%, e.g., 40% to 70%, a dry compression set of 15% or less, e.g., 3% to 15%, or both. Alternatively, or in addition, the flexible polyurethane foam can have a compression deflection at 50% that is at least 30%, e.g., at least 50%, at least 70%, or 30% to 155% greater, as measured by ASTM D3574, than a flexible polyurethane foam having the same composition but in which the silica is replaced with a polyol.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to formulations for flexible polyurethane foams and polymer foams made therewith. [Background technology]

[0002] The term "polyurethane" describes a wide range of polymer compositions, each of which includes polymers whose repeating units include (-N-CO-O-) linkages. In addition, polyurethanes can also include urea (-N-CO-N-) linkages. However, the composition of the molecular chain between the urethane and urea linkages and the method of preparation of the polymer also influence the final properties. Thus, polyurethanes of different compositions and / or made by different methods are used in a variety of applications, from adhesives to coatings, elastomers, to different types of foams. Typically, polyurethanes are produced by the reaction of polyisocyanates with polyols (or polyamines to produce polyureas). Two different polyols can be used to produce a block copolymer. For example, low molecular weight glycols and diamines result in the formation of short chains that, together with hydrogen bonding, form crystalline domains. A second "soft" block can be formed with the use of polyether or polyester polyols, which result in amorphous domains. Such block copolymer compositions are typically used to form thermoplastic polyurethanes (TPUs). The tensile properties of this polymer are determined by how tensile stress disrupts hydrogen bonds in the crystalline domains.

[0003] Alternatively, polyurethane foams are typically formed by the reaction of diisocyanates with polyols and polyamines in the presence of a foaming agent. Rather than utilizing crystalline domains, the mechanical properties are determined in part by the contrast between the rigid urea linkages and the more flexible urethane linkages. The foaming agent can be an adjuvant, such as a volatile organic compound, or can be generated in situ. The addition of water to the reaction mixture results in two competing reactions, polycondensation and the generation of carbon dioxide by the reaction between the isocyanate and water. Increasing the functionality of the polyol and isocyanate increases the crosslink density during the early stages of polymerization, strengthening the cell walls and largely preventing the cell walls from collapsing due to increased carbon dioxide pressure, thereby increasing the rigidity of the foam. Rigid (closed cell) polyurethane foams are typically used for thermal insulation, while flexible (open cell) polyurethane foams are used for cushioning and soundproofing.

[0004] Various fillers are commonly used in polyurethanes to modify their mechanical, electrical, and other properties. They can be mixed with the polymerized material, for example by melt mixing, or mixed into the prepolymer composition prior to polycondensation in an in situ process. Fillers used in the in situ process must have two functions: not only do they need to impart the desired properties to the final product, but they also must not interfere with the polymerization and foaming processes that produce the product.

[0005] Fumed silica is often used to control the thixotropy and pore size of polyurethane foams. In Japanese Patent No. 04850574, fumed silica is melt mixed into a polymerized polyurethane composition, followed by carbon dioxide injection to generate pores. Similarly, fumed silica is used in US Patent Application Publication No. 2008 / 0153935 as a foam stabilizer. Furthermore, it is desirable to mix fumed silica into flexible polyurethane foams in an in situ process, in which fumed silica is mixed with precursor materials prior to polycondensation and allows the silica to contribute to the mechanical properties of the final material. Summary of the Invention [Means for solving the problem]

[0006] The use of low surface area silica bearing trimethylsilyl groups on the surface in combination with a tertiary amine catalyst enables an in situ polymerization process resulting in flexible polyurethane foams with beneficial properties.

[0007] In one embodiment, a method for producing a flexible polyurethane foam includes: At least a first polyol, and 10% by weight or less of 50 to 150 m 2 a polyol composition comprising a fumed silica having a surface area of ​​1 / g; a first polyol having a weight average molecular weight of 3000 to 6000 and a functionality of 2.5 to 3.5; and the fumed silica having a C1 to C3 alkylsilyl group on its surface. combining the polyol composition, a polyisocyanate having a functionality of 1.8 to 2.5, water, and a tertiary amine catalyst to form a prepolymer composition; polymerizing said prepolymer composition to form an open cell foam structure having a density of 1.8 to 4 pcf and a) a resilience of at least 40%, e.g., 40% to 70%, b) a dry compression set of 15% or less, e.g., 3% to 15%, or both; The flexible polyurethane foam may exhibit a density of 1.8-3 pcf, or a density of 2-4 pcf.

[0008] The polyisocyanate may include hexamethylene diisocyanate (HDI), phenylene diisocyanate (PDI), 2,4-toluene diisocyanate (2,4-TDI), 2,6-toluene diisocyanate (2,6-TDI), 4,4'-diphenylmethane diisocyanate (MDI), an isomeric mixture of diphenylmethane diisocyanate, or a mixture of two or more of these. The first polyol may include a polyether polyol or a polyester polyol. The polyol composition may further include a second polyol, the second polyol having a mass average molecular weight of 2000 to 10000. The fumed silica may include a polyether polyol having a mass average molecular weight of 50 to 150 m. 2 / g or 50~100m 2 / g BET surface area. The C1-C3 alkylsilyl group can be trimethylsilyl or dimethylsilyl.

[0009] The step of polymerizing the prepolymer composition to form an open cell foam structure can include filling the prepolymer composition into a mold open on one side to the atmosphere, and the resulting flexible polyurethane foam can have a density of 1.8 to 3 pcf. Alternatively, the prepolymer composition can be filled into a mold and the mold closed, and the resulting flexible polyurethane foam can have a density of 2 to 4 pcf.

[0010] The flexible polyurethane foam can have a compression force deflection at 50%, as measured by ASTM D3574, that is improved by at least 30%, such as at least 50%, at least 70%, or from 30% to 155%, relative to a flexible polyurethane foam produced by the same method, but in which the silica is replaced with the same parts by weight of the first polyol.

[0011] In another embodiment, the flexible polyurethane foam has a thickness of 50 to 150 mm. 2 The flexible polyurethane foam includes 10% by weight or less of fumed silica having a surface area of ​​50-150 m / g, the fumed silica having C1-C3 alkylsilyl groups on its surface, and the flexible polyurethane foam exhibits a resilience of at least 40%, e.g., 40%-70%, a dry compression set of 15% or less, e.g., 3%-15%, or both. The fumed silica has a surface area of ​​50-150 m / g. 2 / g or 50~100m 2 The flexible polyurethane foam may have a BET surface area of ​​1.8-4 pcf / g. The C1-C3 alkylsilyl group may be trimethylsilyl or dimethylsilyl. The flexible polyurethane foam may be a molded foam or a free rise foam. The polyurethane foam may include a polyether polyurethane or a polyester polyurethane. The flexible polyurethane foam may have a density of 1.8-4 pcf, such as a density of 1.8-3 pcf, or a density of 2-4 pcf.

[0012] The flexible polyurethane foam can have a compression force deflection at 50%, as measured by ASTM D3574, that is at least 30%, e.g., at least 50%, at least 70%, or from 30% to 155% greater, than a flexible polyurethane having the same composition but substituting a polyol for the silica.

[0013] It is to be understood that both the foregoing general description and the following detailed description are exemplary and explanatory only and are intended to provide further explanation of the invention as claimed. [Brief description of the drawings]

[0014] The invention will now be described with reference to several figures of the drawing.

[0015] [Figure 1] FIG. 1 shows the viscosity of polyol dispersions prepared with fumed silica having different surface chemistries.

[0016] [Diagram 2] FIG. 2 shows the viscosity of polyol dispersions prepared with fumed silica having different surface areas.

[0017] [Diagram 3] FIG. 3 shows the viscosity of polyol dispersions prepared with hydrophobic and hydrophilic (untreated) fumed silica. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] In one embodiment, a method for producing a flexible polyurethane foam includes: At least the first polyle, 50-150m 2 a polyol composition comprising 10 mass % or less of fumed silica having a surface area of ​​1 / g; the first polyol has a mass average molecular weight of 3000 to 6000 and a functionality of 2.5 to 3.5; and the fumed silica has C1 to C3 alkylsilyl groups on its surface; combining the polyol composition, a polyisocyanate having a functionality of 1.8 to 2.5, e.g., 1.8 to 2.25, water, and a tertiary amine catalyst to form a prepolymer composition; and polymerizing the prepolymer composition under conditions to form an open cell structure having a density of 1.8 to 4 pcf; Contains:

[0019] Flexible polyurethane foams are typically formed by the reaction of diisocyanates with polyols and polyamines in the presence of a foaming agent. For flexible, open-cell foams, the polyols typically have a functionality of 2.5 to 3.5, however, in some instances, higher functionality polyols can be used. This results in less crosslinking than in rigid foams where the polyol functionality is significantly higher, e.g., 4.5 to 5. Similarly, the use of polyisocyanates with a functionality of 2.5 or less, e.g., diisocyanates or polyisocyanates with a functionality of 1.8 to 2.25, also reduces the crosslink density compared to rigid foams where the isocyanate functionality is typically about 2.7 or more.

[0020] Suitable isocyanates for use in the formulations and processes provided herein include any organic isocyanate used in polyurethane foams. Aromatic isocyanates are preferred, however aliphatic, cycloaliphatic, and araliphatic isocyanates can also be used. Exemplary isocyanates include m-phenylene diisocyanate, 2,4- and / or 2,6-toluene diisocyanate (TDI), various isomers of diphenylmethane diisocyanate (MDI), hexamethylene-1,6-diisocyanate, tetramethylene-1,4-diisocyanate, cyclohexane-1,4-diisocyanate, hexahydrotoluene diisocyanate, hydrogenated MDI (H12 MDI), naphthylene-1,5-diisocyanate, methoxyphenyl-2,4-diisocyanate, 4,4'-biphenylene diisocyanate, 3,3'-dimethoxy-4,4'-biphenyl diisocyanate, 3,3'-dimethyldiphenylmethane-4,4'-diisocyanate, 4,4',4''-triphenylmethane triisocyanate, polymethylene polyphenylisocyanate or mixtures thereof with MDI, hydrogenated polymethylene polyphenylisocyanate, toluene-2,4,6-triisocyanate, and 4,4'-dimethyldiphenylmethane-2,2',5,5'-tetraisocyanate, or mixtures thereof. The triisocyanates are preferably used in mixtures with sufficient diisocyanates to give a total functionality of 2 to 2.25.

[0021] Suitable polymer polyols for use in the formulations and processes provided herein include both polyether polyols and polyester polyols and other polymer polyols known to those skilled in the art. Suitable polyols typically have a molecular weight, preferably a weight average molecular weight of 3000 to 6000. Suitable polymer polyols for use in open-cell foams have a hydroxyl number of 2.5 to 3.5, for example 2.5 to 3. Polyol mixtures can also be used. For example, polyols having lower or higher molecular weights can be mixed to give the desired average polyol molecular weight. Thus, one or more additional polyols having a weight average molecular weight of 2000 to 10000 can be mixed with the first polyol.

[0022] Polyether polyols can be obtained by reacting small molecule polyols with alkylene oxides to form polyether polyols. Exemplary small molecule polyols include, but are not limited to, ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, trimethylene glycol, tetramethylene glycol, hexamethylene glycol, glycerol, diglycerol, sorbitol, pentaerythritol, sucrose, and bisphenol A. Exemplary polyethers include polyalkylene oxides, such as polyethylene oxide, polypropylene oxide, and polytetramethylene oxide. Alternatively, or in addition, polymer polyols can be produced by copolymerization of vinyl polymers, such as styrene or acrylonitrile, with polyols.

[0023] Polyester polyols can be obtained by reacting small molecule polyols, such as those mentioned above, with polyesters. Exemplary polyesters include any polyester known to those skilled in the art for use in flexible polyurethane foams, and can be made from organic dicarboxylic acids, such as C2-C12 unbranched aliphatic chains terminated with carboxylic acid groups, and di- or tri-functional alcohols, such as C2-C12 alkylene glycols or polyether alcohols.

[0024] Mixtures of polymer polyols can also be used. Exemplary polymer polyols include those disclosed in US Patent Publication No. 201800223030, US Patent No. 9034936 and US Patent No. 10119002, the entire contents of which are incorporated herein by reference, except that the polyol blend (one or more polyols) must have a total functionality (i.e., the number of hydroxyl groups per molecule) of 2.5 to 3.

[0025] Tertiary amine catalysts are preferred over metal and lower amine catalysts to reduce catalytic competition between the fumed silica and the polyol. Exemplary tertiary amine catalysts include any tertiary amine catalyst known to those skilled in the art to be suitable for the production of polyurethane foams, including, but not limited to, dimethylethanolamine, triethylenediamine, tetramethylpropanediamine, tetramethylhexamethylediamine, and dimethylcyclohexylamine.

[0026] Additional ingredients known to those skilled in the art for use in open-cell polyurethane foams can also be used. Examples include surfactants, viscosity modifiers, crosslinkers, chain extenders, pigments, flame retardants, auxiliary gelling catalysts, auxiliary blowing catalysts, and any combination thereof. Additional polyols can also be used to introduce different copolymers or functions into the polyurethane, such as promoting cell formation or opening cells. Additional fillers, such as styrene acrylonitrile beads, barium sulfate, or calcium carbonate, can be used in combination with the fumed silica provided herein.

[0027] Fumed silica is typically produced by a pyrolysis process, in which a gaseous feedstock containing fuel, such as methane or hydrogen, oxygen, and a volatile silicon compound is fed into a burner. The water formed by the combustion of the fuel in oxygen reacts with the volatile silicon compound, either in liquid or gas form, to produce silicon dioxide particles. The particles fuse and agglomerate to form fumed silica.

[0028] During the formation of polyurethane foam, it is desirable to balance the properties of the formulation to regulate the growth of carbon dioxide bubbles and the crosslinking of the polyol components. If the formulation is too viscous, the diffusion of carbon dioxide formed by the reaction of water with the isocyanate is slowed down. Furthermore, the expanding gas forms bubbles of the appropriate size without exerting pressure to displace the liquid formulation. Silica dispersed in a liquid system affects its rheological properties through two different interactions. The first is the attraction between the individual silica particles. The aggregated structure of fumed silica allows it to form chain-like networks, but the network can be disrupted under agitation or shear, making fumed silica an effective thixotrope. The formation of these networks is favored in systems with high surface area (small primary particles) silica. Thus, in a preferred embodiment, the fumed silica used herein is a 150 m 2 / g or less, e.g. 130m 2 / g or less, or 100m 2 / g or less as measured by nitrogen adsorption (ASTM D1993). The second interaction is between the liquid matrix and the silica surface. In a hydrophilic polyol system, surface-treated silica, which is highly hydrophobic and has a low affinity for the polyol, is expected to have strong particle-particle interactions and promote high yield stress. In contrast, untreated silica disperses well in liquids, such as water or methanol, and does not significantly change viscosity. Thus, in complex formulations, careful modification of the silica surface can have a dramatic effect on the rheology of the system.

[0029] The as-produced fumed silica is hydrophilic and has a large number of Si-OH groups on the surface. Those silanol groups can interact with alcohols by hydrogen bonding and with the oxyalkylene groups of the polyether by acid-base interactions. Therefore, unreacted silica is expected to have a small effect on the viscosity of the polyol. However, the hydroxyl groups of the silica may compete with the hydroxyl groups of the polyol during polymerization. Hydrophobization of the silica closes some of the silanol groups. However, hydrophobization also changes the interfacial interactions between the silica and both the prepolymer formulation and the final polymer, which may change the viscosity behavior of the prepolymer formulation and / or the mechanical properties of the flexible polyurethane foam. Moreover, the hydrophobization treatment preferably does not interfere with the polymerization reaction.

[0030] It has been unexpectedly found that hydrophobization of fumed silica with reagents that leave short chain alkylsilyl groups on the surface reduces competition between the silica and polymeric polyols without undesirable viscosity increases. In contrast, surface treatment with larger alkyl or siloxyl chains on the surface is excessively hydrophobic and adversely affects bubble growth. Preferably, the surface leaves C1-C3 alkylsilyl groups on the surface, such as trimethylsilyl, dimethylsilyl, ethylsilyl, or methylethylsilyl groups. The silyl groups may be bonded to the surface of the fumed silica by one, two, or three siloxane bonds, or to one or two adjacent alkylsilane groups by siloxane bonds.

[0031] Thus, the fumed silica can be hydrophobized with a silazane, such as hexamethyldisilazane, or an alkylsilane, such as dimethyldichlorosilane, methyltrimethoxysilane, methyltrichlorosilane, methyltrimethoxysilane, methyltriethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, trimethylchlorosilane, trimethylmethoxysilane, trimethylethoxysilane, ethyltriethoxysilane, ethyltrichlorosilane, ethyltrimethoxysilane, propyltrichlorosilane, propyltrimethoxysilane, propyltriethoxysilane, ethylmethyldichlorosilane, and other C1-C3 linear and branched alkylsilanes.

[0032] The high surface area and branched structure of fumed silica also promotes its surface interaction with the surrounding polymer matrix. This interaction allows the silica to reinforce polymer foams more effectively than sol-gel or precipitated silica. Thus, silica must have a sufficient surface area, e.g., at least 50 or 60 m, to provide reinforcement. 2 It is desirable to have a molecular weight of 1 / g.

[0033] The polyurethane components can be mixed and polymerized using any method known to those skilled in the art. Preferably, the fumed silica is dispersed in a polyol according to methods known to those skilled in the art, which is then mixed with the remaining non-isocyanate components of the polyurethane(s) before being mixed with the polyisocyanate and polymerized. The polyurethane foam can be a free rise foam, where the polymerization occurs in a vessel open to atmospheric pressure, or a molded foam, where the polymerization occurs in a closed mold. The mold is filled with unpolymerized material, and then closed, creating a restricted space for the expansion of the polyurethane foam. Thus, the density of the foam can be controlled in part by varying the amount of material in the closed mold, while the density of the free rise foam can be controlled by adjusting the formulation to control the relative rates of carbon dioxide evolution and polymerization and carbon dioxide formation. A typical free rise foam has a density of 1.8-3 pcf, while a typical molded foam has a density of 2-4 pcf.

[0034] In either free rise or molded foams, the use of silica as described herein provides reinforcement to the foam without dramatically reducing the flexibility provided by the open cell structure of the foam. Preferably, the polyurethane foam has a resilience of at least 40%, e.g., 40% to 70%. Alternatively, or in addition, the polyurethane foam has a dry compression set of 15% or less, e.g., 3% to 15%. Alternatively, or in addition, the addition of fumed silica as described herein improves compression deflection. For example, the CFD at 50% measured by ASTM D3574, Test C, may be improved by at least 30%, e.g., at least 50%, at least 70%, or 30% to 155%, relative to a formulation without silica. EXAMPLES

[0035] The present invention will be further clarified by the following examples, which of course are intended to be illustrative only.

[0036] Example 1 85m 2CAB-O-SIL TG-6110 hydrophobic fumed silica (Cabot Corporation) with a BET surface area of ​​1 / g and trimethylsilyl groups on the surface was dispersed in Pluracol 2090 polyol triol (BASF) to form a 15 wt% dispersion. The silica dispersion was made in 350 g batches using a SpeedMixer (Flackteck, Landrum, SC) followed by a plenary mixer (PC Laborsystem Labotop). The polyol was weighed into a 600 g plastic container and the silica was added until all materials were mixed. The materials were then mixed at 2350 rpm for 5 minutes and cooled to room temperature. This mixing procedure was repeated three more times for a total of 20 minutes of mixing to ensure complete mixing. Two batches were mixed and degassed in the plenary mixer under 1 bar vacuum for 15 minutes. As shown in Table 1-1, appropriate amounts of dispersion and additional Pluracol 2090 polyol were charged into a 400 mL polyethylene beaker along with the amounts of additional ingredients listed in Table 1-2 to prepare polyol component formulations having 0%, 2%, 4%, 6%, 8%, and 10% fumed silica based on the total weight of the polyol component. The silica-polyol dispersion was used as a drop-in replacement for an equal amount of neat polyol by weight to obtain the desired fumed silica concentration in the polyol component. A control polyol component containing no silica was prepared with 97 g of Pluracol 2090 polyol and the amounts of additional ingredients listed in Table 1-2. The polyol component was mixed with polyisocyanate (Suprasec 7007 polyisocyanate; Huntsman) in the amount shown in Table 1-3 (Isocyanate Index=90) in a 400 mL tri-pour cup for 7 seconds using a high torque mixer (CRAFSTMAN 10-Inch Drill Press, Model No. 137.219000) at 3100 rpm at ambient temperature and then transferred to a polyethylene lined box (6 inch×6 inch×3 inch; 15.24×15.24×7.62 cm).Following completion of the foam rise, all foams were fully cured by placing them in a preheated air circulating oven at 70° C. for 30 minutes. Three samples were prepared for each formulation.

[0037] [Table 1-1]

[0038] [Table 1-2]

[0039] [Table 1-3]

[0040] The rectangular foams were characterized by foam density (ASTM D3574, Test A), ball rebound recovery (ASTM D3574, Test H), tensile strength at break (ASTM D3574, Test E), elongation at break (ASTM D3574, Test E), compression deflection at 25%, 50%, and 65% (ASTM D3574, Test C), tear strength (ASTM D-624, Die C), and average cell size (ASTM D3576).

[0041] The actual cell structure of foams with 2% and 4% fumed silica based on the total polyol content (1.3% and 2.5% based on total foam weight, respectively) was uniform, and the cell size was not significantly affected by the fumed silica compared to the control foam (Tables 1-4). However, the foam with 6% fumed silica based on the total polyol content (3.8% based on total foam weight) showed a slightly coarser cell structure. The cell structure became coarser as the amount of fumed silica in the formulation was further increased.

[0042] [Table 1-4]

[0043] Density, resilience, tensile strength and elongation were not significantly affected by the incorporation of 1.3% and 2.5% fumed silica based on total foam mass (Tables 1-4). However, tear strength and compression force deflection (CFD) values ​​increased significantly with the incorporation of such small amounts of fumed silica (Tables 1-4).

[0044] Outgassing was observed during foam rise for foams made with 3.8%, 5.1%, and 6.4% fumed silica (using polyol components with 6%, 8%, and 10% fumed silica), based on the total foam mass. The cell structure was also coarser. This is hypothesized to result from the cell opening effect of the fumed silica. However, the samples showed CFDs of 3.29 ± 0.21, 3.86 ± 0.20, and 4.21 ± 0.46 at 50%, respectively, indicating that the silica still provides reinforcement to the foam.

[0045] Example 2 Additional foams were prepared using the polyol component with 10% fumed silica using the methods described above and the formulations shown in Table 2-1 below, except that the surfactant (Tegostab B 4690 surfactant) and cell opening polyol (Lumulse POE 26 polyol) concentrations in Table 2-1 were adjusted, and propylene carbonate (1,2 propanediol cyclic carbonate 99.7%, Sigma-Aldrich) was added to the polyol component of some formulations to reduce viscosity. Approximately half of the polyol component (amounts shown in Table 2-1) was mixed in a 400 mL tri-pour polyethylene cup with enough isocyanate for an Isocyanate Index of 90 (exact amounts in Table 2-1), mixed for 7 seconds as described in Example 1, poured into a 1000 mL polyethylene tri-pour beaker, and allowed to free rise.

[0046] [Table 2-1]

[0047] As shown in Table 2-1, when the surfactant concentration was increased, the cell structure was not improved (Examples 2-1 and 2-2). However, when the amount of cell opening polyol was decreased, the cell structure was significantly improved (Examples 2-3 and 2-4). Viscosity can also affect the foaming process, and the addition of propylene carbonate also reduced the coarseness of the cell structure, especially in combination with a reduced amount of cell opening polyol (Examples 2-5, 2-6, 2-7).

[0048] Example 3 Open cell polyurethane foams were produced using the method described in Example 1 (Isocyanate Index 90) with the polyol component having 0% (comparative), 6%, 8%, and 10% CAB-O-SIL TG-6110 fumed silica in the polyol component formulations shown in Table 3-1 (similar to Examples 2-6) mixed with the amount of isocyanate shown below and dispensed into 6" x 6" x 3" polyethylene lined boxes and free-risen as described in Example 1. The resulting foams had 0%, 3.8%, 5.1%, and 6.4% fumed silica. The cell structure of all foams was uniform. Three samples were prepared for each formulation.

[0049] [Table 3-1]

[0050] The results of cell size measurements and mechanical testing (performed as described in Example 1) are given in Table 3-2. The cell size of the foams with 3.8% fumed silica was significantly smaller than that of the comparative foam. The cell size increased with the loading of fumed silica, however, was consistently smaller than that of the comparative foam. The recovery force and elongation at break decreased as the amount of FS in the formulation increased. The tensile strength, tear strength and CFD values ​​of the foams prepared with FS were significantly higher compared to the control foam at the same density.

[0051] [Table 3-2]

[0052] Example 4 A polyol component without silica (comparative) and polyol components containing 2%, 4%, 6%, 8%, and 10% fumed silica according to the formulation of Example 1 were sealed in a sealed cabinet at ambient temperature and aged. After two weeks, the polyol component with 2% fumed silica was a thick liquid and flowed only slowly, while the remaining samples with higher fumed silica concentrations had a pasty appearance and did not flow when inverted. In contrast, the control composition remained fluid.

[0053] Additional polyol component formulations were prepared with 10% fumed silica as shown in Table 4-1 below, but the viscosities of those formulations aged for various times at ambient temperature are also shown (the arrows indicate that the viscosity was still increasing when the measurement was made). Viscosity was measured with a Brookfield Viscometer, Model LVF, according to ASTM D-4878.

[0054] [Table 4-1]

[0055] The viscosity of the polyol component prepared without the Dabco 33LV catalyst and without any diethanolamine (DEA) did not change over time (Example 4-3). The viscosity of the polyol component containing either one of the two products (Dabco 33LV or DEA) increased over time (Examples 4-2 and 4-4). The polyol component prepared with DEA ​​and without Dabco 33LV had a paste consistency after only three days. The polyol component prepared with Dabco 33LV and without DEA turned into a very viscous liquid after six days.

[0056] The viscosity of the polyol component prepared with triethanolamine (TEOA) instead of DEA and without Dabco 33LV changed little, if at all, after 6 days of storage (Example 4-6). The change in viscosity of the polyol component prepared with TEOA and Dabco 33LV was comparable to that of the polyol component prepared with Dabco 33LV but without either amine chain extender (Examples 4-2 and 4-5). The results clearly indicate that fumed silica interacts more with secondary amines than with tertiary amines. Furthermore, the use of amine chain extenders or crosslinkers may not be essential for open cell PU systems using fumed silica.

[0057] Example 5 CAB-O-SIL TG-6110 hydrophobic fumed silica (Cabot Corporation) was dispersed in Pluracol 2090 polyether triol (BASF) as described above to form a 15 wt. % dispersion. This dispersion was mixed with additional ingredients including Poly-G 85-29, an ethylene oxide capped polyether polyol triol (Monument Chemical) in the ratios shown in Table 5-1 below to form a polyol component. As in Example 1, this silica-polyol dispersion was used as a drop-in replacement for an equal amount of neat polyol by weight to prepare polyol components having silica concentrations of 0%, 2%, 4%, 6%, 8%, and 10%. A total of 223.34 g of the polyol component was mixed with 131.52 g of Suprasec 7007 polyisocyanate (to obtain an Isocyanate Index of 90) in a 1000 mL tri-pour polyethylene cup for 7 seconds using a high torque mixer (CRAFSTMAN 10-Inch Drill Press, Model No. 137.219000) at 3100 rpm at ambient temperature, and then poured into a 12 inch x 12 inch x 2 inch (30 cm x 30 cm x 5 cm) aluminum mold preheated to 70°C before the liquid mixture became cloudy and began to expand. After pouring, the mold was sealed and cured for 260 seconds before it was opened and the foam removed from the mold. All molded foams were aged in ambient air for at least one week prior to testing. The foam pads were hand crushed (i.e., hand compressed to open the cell windows) immediately after removal from the mold. In addition to the tests described in Example 1, the foams were subjected to the following tests in accordance with ASTM D-3574: dry constant deflection compression set (Test D), wet aged compression set (Test D with wet heat aging of Test L), wet aged load (CFD) drop (Test C with wet heat aging of Test L, 55° C. and 95% relative humidity for 22 hours, and also Test J2, Test C with steam autoclave aging, 120° C. for 5 hours). The molded foams were also evaluated for CFD at 25%, 50%, and 65% deflection, but with a 60 second hold time, as described in Example 1. Two foam samples were run with each formulation.

[0058] [Table 5-1]

[0059] Molded foams prepared with 0%, 1.3%, 2.5%, and 3.8% FS based on total foam weight (0%, 2%, 4%, and 6% FS based on total polyol content, respectively) showed uniform surface (skin) and uniform external cell structure. Some defects on the skin were observed for foams prepared with 5.1% and 6.3% fumed silica based on total foam weight (8% and 10% FS based on total polyol content, respectively). However, the cell structure of those foams was uniform despite minor skin defects. The mechanical properties of the resulting foams are listed in Table 5-2. The resilience of the molded foams decreased with increasing concentration of fumed silica.

[0060] [Table 5-2]

[0061] Example 6 CAB-O-SIL TG-6110 (Example 6-x) and CT1221 (Example 6-Cx) silica (Cabot Corporation, CT1221 silica is 180-250m 2A 15% dispersion of 1,2-difluorophenyl ether (having a BET surface area of ​​100 / g and trimethylsilyl groups on the surface) was prepared in Jeffol G 31-28, a glycerin-based ethylene oxide capped triol (Huntsman) as described in Example 1. The polyol component was prepared as described in Example 1 using the formulation shown in Table 6-1 (Voranol-Voractiv 6340 polyether polyol (Dow), Dabco NE300 blowing catalyst (Evonik), Dabco NE1091 gelling catalyst (Evonik), Dabco DC193 surfactant (Evonik), propylene carbonate (see Example 2), and diethanolamine LF 85% (Webb Chemical)). The polyol components were mixed with Lupranate T80 isocyanate (a mixture of 2,4- and 2,6-toluene diisocyanates, Huntsman) in the amounts specified in Table 6-2 (Isocyanate Index of 90) and poured into polyethylene lined boxes as described in Example 1 ("Free Rise Foams"). Free rise foams were prepared in replicates. The polyurethane formulations specified in Table 6-2 were scaled up to 250% in Example 6-C1 and 257% in Examples 6-1 and 6-2 to prepare molded foams according to the method set forth in Example 5. The molded foams were prepared in replicates. The foams were evaluated as described above.

[0062] [Table 6-1a]

[0063] [Table 6-1b]

[0064] [Table 6-2]

[0065] Table 6-2 shows that stable foams were prepared with the lower surface area TG-6110 silica. It is hypothesized that the cell opening properties of the silica compensate for the absence of a cell opening polyol in the formulation. However, foams with the higher surface area CT-1221 silica collapsed even in the absence of a cell opening polyol. Foam stability was not improved by changing the surfactant concentration, using alternative dispersants for Tegostab dispersant, partially replacing it with Dabco DC 193 surfactant, adding propylene carbonate, or reducing the silica concentration.

[0066] In addition to the above tests, the foams were characterized for hysteresis loss according to ASTM D-3574 (Procedure B-CFD Hysteresis Loss). Table 6-3 shows the mechanical and other properties of molded foams containing TG-6110 silica compared to a control without silica. The introduction of TG-6110 silica increased the CFD and did not significantly affect the resilience of the free rise foams. In molded foams, the introduction of TG-6110 silica increased the CFD and tear strength, but did not significantly affect the tensile strength.

[0067] [Table 6-3]

[0068] Example 7 A 15% dispersion of CAB-O-SIL TG-6110 and CT 1221 silica was prepared in Jeffol G 31-28, a glycerin-based ethylene oxide capped triol (Huntsman), as described above. A polyol component having 6% by weight silica was prepared using the formulation shown in Table 7-1 (containing Lumulse POE 26 ethoxylated glycerin, Tegostab B 4690 surfactant, diethanolamine LF 85% crosslinker, Dabco 33 LV triethylenediamine, and Toyocat ET bis(2-dimethylaminoethyl)ether), as described in Example 1. The polyol component was mixed with Suprasec 7007 isocyanate in the amounts listed in Table 7-1, as described in Example 1, and poured into a polyethylene lined box ("free rise foam"), as described in Example 1, to form a foam having 3.8% by weight silica. The appearance of the foam was evaluated visually.

[0069] [Table 7-1]

[0070] The foam made without silica and the two foams made with the lower surface area TG-6110 silica all showed uniform, fine cell structure. The foam made with the higher surface area CT-1221 silica and Lumulse POE cell opening polyol showed partial foam collapse, while the foam made with CT-1221 silica and no cell opening polyol showed coarse cells in the foam core.

[0071] Example 8 Fumed silica (see Table 8-1 below, all silicas from Cabot Corporation) was mixed with Voranol 220-046 polyether polyol (Dow) at a loading of 6% by weight in a Hauschild Speedmixer DAC-150 until a Hegman grind value of 5 was obtained. The dispersion was evaluated in a TA Instruments AR2000 Rheometer at 25°C with a 4 cm parallel plate geometry and a 500 micron gap. The viscosity data is shown in Figure 1. The data shows that fumed silica treated with octylsilyl groups or siloxane polymers dramatically increases the viscosity compared to fumed silica treated with alkylsilyl groups having 3 or less than 2 carbons.

[0072] [Table 8-1]

[0073] Example 9 CAB-O-SIL TG-6110 (circles) and CT-1221 (triangles) silicas were mixed with Voranol 6340 (closed symbols) and Jeffol G 31-28f (open symbols) polyols at a 15% loading as described in Example 1. Viscosity was measured as in Example 8 and plotted versus shear rate. The results are shown in Figure 2 and show that the higher surface area CT-1221 silica also results in a dramatic increase in viscosity.

[0074] Example 10 CAB-O-SIL TG-6110 (circles) and L90 (triangles) silicas were mixed with Voranol 232-034 (closed symbols) polyol at a 10% loading as described in Example 1. Viscosity was measured as in Example 8 and plotted against shear rate. The interaction of the hydrophobic TG-6110 silica and the untreated hydrophilic L90 silica with the amine catalyst was evaluated by adding 1 wt. % triethanolamine to the sample, mixing for 30 seconds in a SpeedMixer (Flackteck, Landrum, SC), incubating the sample at ambient temperature for 30 minutes, and then measuring the viscosity again (open symbols). The results are shown in Figure 3 and show that the untreated L90 silica causes a dramatic increase in the viscosity of the polyol. In a polymerization system, such an increase in viscosity can prevent the proper development of bubbles in the foam.

[0075] The foregoing description of preferred embodiments of the invention has been presented for purposes of illustration and description. It is not intended to be exhaustive or to limit the invention to the precise form disclosed. Modifications and variations are possible in light of the above teachings or may be acquired from practice of the invention. The embodiments were chosen and described in order to explain the principles of the invention and its practical application so as to enable those skilled in the art to use the invention in various embodiments and with various modifications as adapted to the particular intended use. It is intended that the scope of the invention be defined by the appended claims and their equivalents.

Claims

1. 1. A method for producing a flexible polyurethane foam, comprising the steps of: A polyol composition is provided comprising at least a first polyol and 2-10% by weight of a fumed silica having a surface area of ​​50-150 m 2 / g, said first polyol having a weight average molecular weight of 3000-6000 and a functionality of 2.5-3.5, and said fumed silica having C1-C3 alkylsilyl groups on its surface. combining the polyol composition, a polyisocyanate having a functionality of 1.8 to 2.5, water, and a tertiary amine catalyst to form a prepolymer composition; and polymerizing said prepolymer composition to form an open cell foam structure having a density of 29-64 kg / m 3 (1.8-4 pcf) and one or both of a) a ball bounce (ASTM D3574, Test H) recovery of 40%-70%, and b) a dry compression set of 3%-15%; The method comprising:

2. The method of claim 1, wherein the flexible polyurethane foam exhibits a density of 29-48 kg / m 3 (1.8-3 pcf) or a density of 32-64 kg / m 3 (2-4 pcf).

3. The method of claim 1 or 2, wherein the polyisocyanate comprises hexamethylene diisocyanate (HDI), phenylene diisocyanate (PDI), 2,4-toluene diisocyanate (2,4-TDI), 2,6-toluene diisocyanate (2,6-TDI), 4,4'-diphenylmethane diisocyanate (MDI), an isomeric mixture of diphenylmethane diisocyanate, or a mixture of two or more thereof.

4. The method of any one of claims 1 to 3, wherein the first polyol comprises a polyether polyol or a polyester polyol.

5. The method of any one of claims 1 to 4, wherein the polyol composition further comprises a second polyol, the second polyol having a weight average molecular weight of 2,000 to 10,000.

6. The fumed silica is 50 to 150 m 2 / g or 50 to 100m 2 The method of any one of claims 1 to 5, wherein the SiO2 has a BET surface area of ​​1 / g.

7. 7. The method of any one of claims 1 to 6, wherein polymerizing the prepolymer composition to form an open cell foam structure comprises filling the prepolymer composition into a mold having one side open to the atmosphere.

8. The method of claim 7, wherein the flexible polyurethane foam has a density of from 29 to 48 kg / m 3 (1.8 to 3 pcf).

9. The method of any one of claims 1 to 6, wherein polymerizing the prepolymer composition to form an open-cell foam structure comprises filling the prepolymer composition into a mold and closing the mold.

10. The method of claim 9, wherein the flexible polyurethane foam has a density of 32 to 64 kg / m 3 (2 to 4 pcf).

11. The method according to any one of claims 1 to 10, wherein the C1 to C3 alkylsilyl group is trimethylsilyl or dimethylsilyl.

12. 12. The method of any one of claims 1 to 11, wherein the flexible polyurethane foam has a 30% to 155% improved compression force deflection at 50%, as measured by ASTM D3574, versus a flexible polyurethane foam produced by the same method, but with silica replaced with an equal part by weight of the first polyol.

13. 50 to 150 m 2 1. A flexible polyurethane foam comprising 2 to 10 weight percent fumed silica having a surface area of ​​100 / g, said fumed silica having C1-C3 alkylsilyl groups on its surface, said flexible polyurethane foam having a ball bounce (ASTM D3574, Test H) recovery of 40% to 70%, a dry compression set of 3% to 15%, or both.

14. The fumed silica is 50 to 150 m 2 / g or 50 to 100m 2 14. The flexible polyurethane foam of claim 13 having a BET surface area of ​​1 / g.

15. The flexible polyurethane foam of claim 13 or 14, wherein the C1-C3 alkylsilyl group is trimethylsilyl or dimethylsilyl.

16. The flexible polyurethane foam of any one of claims 13 to 15, wherein the foam is a molded foam or a free rise foam.

17. The flexible polyurethane foam of any one of claims 13 to 16, wherein the polyurethane comprises a polyether polyurethane or a polyester polyurethane.

18. The flexible polyurethane foam of any one of claims 13 to 17 having a density of 29 to 64 kg / m 3 (1.8 to 4 pcf).

19. 19. The flexible polyurethane foam of any one of claims 13 to 18, having a compression force deflection at 50%, as measured by ASTM D3574, that is 30% to 155% greater than a flexible polyurethane foam having the same composition but in which the silica is replaced with a polyol.

Citation Information

Patent Citations

  • Production of low-density high-elastic soft polyurethane foam having excellent durability

    JP2000080267A

  • Polyol composition and method for producing polyurethane using the same

    JP2012077100A

  • Dispersion comprising a liquid phase and a solid phase

    US20130085197A1