Polyglycerin-based alkoxysilane
A (poly)glycerin-based alkoxysilane with a (poly)glycerin skeleton and alkoxysilyl groups addresses the durability issues of existing antifogging compositions by chemically bonding to surfaces, ensuring sustained antifogging performance.
Patent Information
- Application Number
- JP2020176721
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-11-20
- Filing Date
- 2020-10-21
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2040-10-21
AI Technical Summary
Existing antifogging compositions for glass and plastic surfaces have low water resistance and durability, leading to rapid loss of antifogging effect due to peeling off from the substrate.
A (poly)glycerin-based alkoxysilane with a (poly)glycerin skeleton and multiple alkoxysilyl groups is used to chemically bond with the surface, providing sustained antifogging properties.
The (poly)glycerin-based alkoxysilane imparts excellent antifogging properties and durability to glass and plastic surfaces, maintaining effectiveness even under repeated water exposure.
Smart Images

Figure 0007576299000001 
Figure 0007576299000002 
Figure 0007576299000003
Abstract
Description
[Technical field]
[0001] The present invention Poly This relates to glycerin-based alkoxysilanes. [Background technology]
[0002] Substrates such as glass and plastics are highly transparent and are used for optical films, glass, lenses, etc. However, under conditions of high temperature and humidity or large temperature differences, condensation occurs on the substrate surface, causing fogging and impairing visibility, which is a problem.
[0003] A common method for preventing this fogging phenomenon is to prepare a coating film that imparts an anti-fogging effect to the surface of the substrate. For example, a method has been disclosed in which a solution containing a surfactant or a surfactant and a hydrophilic polymer is applied to the surface of the substrate to make the surface hydrophilic and prevent the formation of water droplets (Patent Document 1).
[0004] However, the anti-fogging composition of Patent Document 1 has a problem that the coating has low water resistance due to its high hydrophilicity, and loses its effect when washed away with water. Furthermore, since this anti-fogging composition is not chemically bonded to the glass surface or plastic material, the anti-fogging effect is exhibited immediately after coating, but it easily peels off from the substrate surface, resulting in a decrease in the anti-fogging effect. In other words, the anti-fogging durability is low. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 3-215589 Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide a novel material capable of imparting sustained anti-fogging properties to substrates such as glass and plastics. [Means for solving the problem]
[0007] As a result of intensive research, the present inventors have found that a (poly)glycerin-based alkoxysilane having a (poly)glycerin skeleton with an average degree of polymerization of 1 to 100 and having multiple alkoxysilyl groups at its terminals can solve the above problems, and have thus completed the present invention. Effect of the Invention
[0008] The (poly)glycerin-based alkoxysilane of the present invention imparts anti-fogging properties to substrates such as glass and plastics, and has excellent durability of the anti-fogging effect. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The present invention will be described below based on an embodiment, but the scope of the present invention is not limited to this embodiment, and the present invention also includes modifications made within the scope of the present invention. Note that the range "~" includes the upper and lower limits.
[0010] The present invention relates to a (poly)glycerin-based alkoxysilane having a (poly)glycerin skeleton with an average degree of polymerization of 1 to 100 and having multiple alkoxysilyl groups at its terminals. Note that (poly)glycerin refers to glycerin or polyglycerin.
[0011] The average degree of polymerization of the (poly)glycerin according to the present invention is 1 to 100, preferably 2 to 20, and most preferably 2 to 15. Here, the average degree of polymerization is calculated from the hydroxyl value by terminal analysis using the following formulas (2) and (3). The hydroxyl value in formula (3) is a numerical value that is an index of the number of hydroxyl groups contained in (poly)glycerin, and refers to the number of milligrams of potassium hydroxide required to neutralize acetic acid required to acetylate the free hydroxyl groups contained in 1 g of (poly)glycerin. The number of milligrams of potassium hydroxide is calculated in accordance with "Standard Testing Methods for Analysis of Fats, Oils and Related Materials, 2013 Edition, Established by Japan Oil Chemists' Society," edited by Japan Oil Chemists' Society. Molecular weight=74n+18 (2) Hydroxyl number = 56110(n+2) / molecular weight (3)
[0012] The (poly)glycerin-based alkoxysilane according to the present invention is preferably a reaction product obtained by reacting (poly)glycerin or a (poly)glycerin derivative having a first reactive functional group at its terminal with an alkoxysilane having a second reactive functional group at its terminal.
[0013] The (poly)glycerin or (poly)glycerin derivative having a first reactive functional group at its terminal is preferably a compound represented by the structure of the following formula (1). [ka] (n, p, q, and r each represent the number of repeating units, n is an integer of 1 to 20, and p, q, and r each are integers of 0 to 50. AO represents an alkylene oxide having 1 to 4 carbon atoms. R1 may be the same or different and represents hydrogen or a reactive functional group having any one selected from the group consisting of a thiol group, a (meth)acryloyl group, an epoxy group, and an allyl group at its terminal.)
[0014] Examples of AO include ethylene oxide (EO), propylene oxide (PO), and butylene oxide (BO), and preferably ethylene oxide (EO). p, q, and r in formula (1) each represent the average number of alkylene oxides added to one hydroxyl group of polyglycerin, and each is preferably 0 to 50, and more preferably 1 to 20. The sum of p, q, and r (p+q+r) is more preferably 1 to 130, and even more preferably 5 to 120.
[0015] Specific examples of (poly)glycerin or (poly)glycerin derivatives having a first reactive functional group at an end include (poly)glycerin, (poly)glycerin alkylene oxide adducts, (poly)glycerin (alkylene oxide) thioglycolic acid esters, (poly)glycerin (alkylene oxide) 3-mercaptopropionic acid esters, (poly)glycerin (alkylene oxide) (meth)acrylates, (poly)glycerin (alkylene oxide) (poly)glycidyl ethers, (poly)glycerin (alkylene oxide) (poly)allyl ethers, and the like.
[0016] The second reactive functional group is not particularly limited, and examples thereof include a vinyl group, an isocyanate group, a thiol group, a (meth)acryloyl group, an epoxy group, a hydroxyl group, and an amino group. Examples of alkoxysilanes having a second reactive functional group at the end include vinyltrimethoxysilane, vinyltriethoxysilane, 3-isocyanatepropyltriethoxysilane, 3-isocyanatepropyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-aminopropyltrimethoxysilane, 3-hydroxypropyltriethoxysilane, and 3-aminopropyltriethoxysilane.
[0017] The (poly)glycerin-based alkoxysilane of the present invention is preferably obtained by reacting a first reactive functional group contained in the terminal of (poly)glycerin or a (poly)glycerin derivative with a second reactive functional group at the terminal of an alkoxysilane.Specific examples include reaction products of (poly)glycerin, (poly)glycerin alkylene oxide adduct, or (poly)glycerin derivative having a thiol group at the terminal with an alkoxysilane having any one of a vinyl group, an isocyanate group, an epoxy group, or an amino group at the terminal; reaction products of (poly)glycerin derivative having a (meth)acryloyl group at the terminal, or (poly)glycerin derivative having an allyl group at the terminal with an alkoxysilane having a vinyl group, a thiol group, or a (meth)acryloyl group at the terminal; reaction products of (poly)glycerin derivative having an epoxy group at the terminal with an alkoxysilane having a thiol group, a hydroxyl group, or an amino group at the terminal, and the like. In the resulting reaction product, it is preferable that 20 to 100% of the first reactive functional groups of the (poly)glycerin or (poly)glycerin derivative are reacted and bonded, and it is more preferable that 50 to 100% of the first reactive functional groups are reacted and bonded.
[0018] The polyglycerin-based alkoxysilane of the present invention can be suitably used as an anti-fogging agent, a dew condensation inhibitor, or a stress relaxation agent.When used as an anti-fogging agent, a dew condensation inhibitor, or a stress relaxation agent, it can also be made into a coating composition containing silicate monomers such as TMOS and TEOS, silicate oligomers such as methyl silicate and ethyl silicate, polysilsesquioxane, etc., within a range that does not impair the effect.The cured coating film obtained by curing this coating composition has excellent anti-fogging properties for substrates such as glass and plastic, and is suitably used as an anti-fogging coating agent for automobile windshields, lamp covers, camera lenses, goggles, etc. EXAMPLES
[0019] The present invention will be described below with reference to examples, but the present invention is not limited to these examples.
[0020] [Synthesis Example 1] In a reaction vessel equipped with a thermometer, a stirrer, and a Dean-Stark apparatus, 764 g of EO60 mol adduct of tetraglycerin (polyglycerin with an average degree of polymerization of 4), 163 g of 3-mercaptopropionic acid, 900 g of toluene, and 45 g of p-toluenesulfonic acid were charged, and the temperature was raised to a toluene reflux atmosphere while stirring, and a dehydration condensation reaction was carried out over about 6 hours. After the reaction was completed, the mixture was neutralized using sodium bicarbonate and extracted with ethyl acetate:toluene = 50:50. The organic layer was distilled under reduced pressure to obtain 367 g of 3-mercaptopropionic acid ester of tetraglycerin EO60 mol adduct. In a reaction vessel equipped with a stirrer, 319 g of 3-mercaptopropionic acid ester of tetraglycerin EO60 mol adduct and 81 g of vinyltrimethoxysilane were charged, and the mixture was stirred for 45 minutes while irradiating with UV light, and 400 g of alkoxysilane compound A1 was obtained. Incidentally, 100% of the hydroxyl groups at the terminals of the polyglycerin derivative were reacted.
[0021] [Synthesis Example 2] In a reaction vessel equipped with a thermometer and a stirrer, 425 g of EO 60 mole adduct of tetraglycerin, 210 g of 3-isocyanatepropyltriethoxysilane (manufactured by TCI), and 0.13 g of dibutyltin dilaurate were charged and stirred for 4 hours in an incubator set at 40°C to obtain 635 g of alkoxysilane compound A2. Note that 100% of the hydroxyl groups at the terminals of the polyglycerin derivative were reacted.
[0022] [Synthesis Example 3] In a reaction vessel equipped with a thermometer and a stirrer, 66 g of EO 40 mole adduct of diglycerin, 34 g of 3-isocyanatepropyltriethoxysilane (manufactured by TCI), and 0.01 g of dibutyltin dilaurate were charged and stirred for 12 hours in an incubator set at 60°C to obtain 100 g of alkoxysilane compound A3. Note that 100% of the hydroxyl groups at the terminals of the polyglycerin derivative were reacted.
[0023] [Synthesis Example 4] In a reaction vessel equipped with a thermometer and a stirrer, 66 g of EO 120 mole adduct of decaglycerin, 34 g of 3-isocyanatepropyltriethoxysilane (manufactured by TCI), and 0.01 g of dibutyltin dilaurate were charged and stirred for 4 hours in an incubator set at 40°C to obtain 100 g of alkoxysilane compound A4. Note that 100% of the hydroxyl groups at the terminals of the polyglycerin derivative were reacted.
[0024] [Synthesis Example 5] In a reaction vessel equipped with a thermometer and a stirrer, 28 g of EO 6 mole adduct of tetraglycerin, 72 g of 3-isocyanatepropyltriethoxysilane (manufactured by TCI), and 0.01 g of dibutyltin dilaurate were charged and stirred for 11 hours in an incubator set at 60°C to obtain 100 g of alkoxysilane compound A5. Note that 100% of the hydroxyl groups at the terminals of the polyglycerin derivative were reacted.
[0025] [Synthesis Example 6] In a reaction vessel equipped with a thermometer and a stirrer, 29 g of EO 7 mole adduct of tetraglycerin, 71 g of 3-isocyanatepropyltriethoxysilane (manufactured by TCI), and 0.01 g of dibutyltin dilaurate were charged and stirred for 6 hours in an incubator set at 60°C to obtain 100 g of alkoxysilane compound A6. Note that 100% of the hydroxyl groups at the terminals of the polyglycerin derivative were reacted.
[0026] [Synthesis Example 7] In a reaction vessel equipped with a thermometer and a stirrer, 31 g of EO 8 mole adduct of tetraglycerin, 69 g of 3-isocyanatepropyltriethoxysilane (manufactured by TCI), and 0.01 g of dibutyltin dilaurate were charged and stirred for 5 hours in an incubator set at 60°C to obtain 100 g of alkoxysilane compound A7. Note that 100% of the hydroxyl groups at the terminals of the polyglycerin derivative were reacted.
[0027] [Synthesis Example 8] In a reaction vessel equipped with a thermometer and a stirrer, 37 g of EO 12 mole adduct of tetraglycerin, 63 g of 3-isocyanatepropyltriethoxysilane (manufactured by TCI), and 0.01 g of dibutyltin dilaurate were charged and stirred for 5 hours in an incubator set at 60°C to obtain 100 g of alkoxysilane compound A8. Note that 100% of the hydroxyl groups at the terminals of the polyglycerin derivative were reacted.
[0028] [Synthesis Example 9] In a reaction vessel equipped with a thermometer and a stirrer, 44 g of EO 12 mole adduct of tetraglycerin, 56 g of 3-isocyanatepropyltriethoxysilane (manufactured by TCI), and 0.01 g of dibutyltin dilaurate were charged and stirred for 2 hours in an incubator set at 60°C to obtain 100 g of alkoxysilane compound A9. Note that 75% of the hydroxyl groups at the terminals of the polyglycerin derivative were reacted.
[0029] [Synthesis Example 10] In a reaction vessel equipped with a thermometer and a stirrer, 54 g of EO 12 mole adduct of tetraglycerin, 46 g of 3-isocyanatepropyltriethoxysilane (manufactured by TCI), and 0.01 g of dibutyltin dilaurate were charged and stirred for 2 hours in an incubator set at 60°C to obtain 100 g of alkoxysilane compound A10. Note that 50% of the hydroxyl groups at the terminals of the polyglycerin derivative were reacted.
[0030] [Synthesis Example 11] In a reaction vessel equipped with a thermometer and a stirrer, 73 g of EO 60 mole adduct of tetraglycerin, 27 g of 3-isocyanatepropyltriethoxysilane (manufactured by TCI), and 0.01 g of dibutyltin dilaurate were charged and stirred for 12 hours in an incubator set at 60°C to obtain 100 g of alkoxysilane compound A11. Note that 75% of the hydroxyl groups at the terminals of the polyglycerin derivative were reacted.
[0031] [Synthesis Example 12] In a reaction vessel equipped with a thermometer and a stirrer, 80 g of EO 60 mole adduct of tetraglycerin, 20 g of 3-isocyanatepropyltriethoxysilane (manufactured by TCI), and 0.01 g of dibutyltin dilaurate were charged and stirred for 6 hours in an incubator set at 60°C to obtain 100 g of alkoxysilane compound A12. Note that 50% of the hydroxyl groups at the terminals of the polyglycerin derivative were reacted.
[0032] <Example 1> 1.0g of alkoxysilane compound A1, 1.5g of 1-methoxy-2-propanol, 0.27g of water, and 0.1g of 0.1wt% aqueous nitric acid solution were uniformly stirred and mixed to obtain a coating composition. The coating composition was then applied to a hydrophilically treated glass plate (76mm x 52mm x 1.2mm) to a thickness of about 30μm, and the plate was heated and dried at 150°C for 30 minutes to obtain a hardened coating film. The glass plate was immersed in an alkaline solution (a mixture of 500mL of isopropanol, 41.6g of potassium hydroxide, and 83.3g of ion-exchanged water) for 15 hours, and then washed with a 0.2mol / L aqueous hydrochloric acid solution and ion-exchanged water to obtain a hydrophilic treatment.
[0033] <Examples 2 to 12> Coating compositions and cured coating films were prepared in the same manner as in Example 1, except that the alkoxysilane compound A1 used in Example 1 was changed to alkoxysilane compounds A2 to A12.
[0034] The anti-fogging properties of the cured coating films of Examples 1 to 12 were evaluated by the steam anti-fogging property described below. Furthermore, the cured coating films of Examples 1 and 2 were also evaluated for anti-fogging durability. (Steam anti-fogging) The cured coating film was placed 2.0 cm above the surface of water adjusted to 50° C., and the cured coating film was visually evaluated for clouding and the time it took for the coating film to become cloudy was measured. (Anti-fog durability) The anti-fogging durability was evaluated by wiping off the moisture adhering to the coating surface with paper after the above-mentioned steam anti-fogging evaluation, leaving the coating surface to stand at 25°C and 60RH% for 15 minutes, and then placing the cured coating 2.0 cm above the liquid surface of water adjusted to 50°C. This operation was repeated five times in total.
[0035] <Comparative Example 1> The vapor anti-fogging properties and anti-fogging durability were evaluated using glass plates that were immersed in an alkaline solution (a mixture of 500 mL of isopropanol, 41.6 g of potassium hydroxide, and 83.3 g of ion-exchanged water) for 15 hours and then washed with a 0.2 mol / L aqueous hydrochloric acid solution and ion-exchanged water.
[0036] The blended compositions and evaluation results of Examples 1 to 12 and Comparative Example 1 are shown in Tables 1 and 2. The blended compositions of Examples 1 and 2 in Table 1 were newly formulated.
[0037] [Table 1]
[0038] [Table 2]
[0039] Examples 1 to 12, which used the cured coating film obtained from the (poly)glycerin-based alkoxysilane of the present invention, had sufficient anti-fogging properties compared to Comparative Example 1, which was not coated with the cured coating film. Moreover, Examples 1 and 2 maintained their anti-fogging properties even after repeated anti-fogging tests. The evaluation results of Examples 1 to 12 reveal that the cured coating film obtained from the (poly)glycerin-based alkoxysilane of the present invention has sufficient anti-fogging properties and anti-fogging durability.
Claims
1. A polyglycerin-based alkoxysilane having a polyglycerin skeleton with an average degree of polymerization of 2 to 20 and a plurality of alkoxysilyl groups at its terminals, the polyglycerin being a reaction product obtained by reacting either a polyglycerin having a first reactive functional group at its terminal or a polyglycerin derivative having a first reactive functional group at its terminal with an alkoxysilane having a second reactive functional group at its terminal, the first reactive functional group is a reactive functional group containing at its terminal any one selected from the group consisting of a hydroxyl group, a thiol group, a (meth)acryloyl group, an epoxy group, and an allyl group; The polyglycerin-based alkoxysilane is characterized in that the second reactive functional group is one selected from the group consisting of a vinyl group, an isocyanate group, a thiol group, a (meth)acryloyl group, an epoxy group, a hydroxyl group, and an amino group.
2. A polyglycerin-based alkoxysilane having a polyglycerin skeleton with an average degree of polymerization of 2 to 20 and a plurality of alkoxysilyl groups at its terminals, the polyglycerin being a reaction product obtained by reacting either a polyglycerin having a first reactive functional group at its terminal or a polyglycerin derivative having a first reactive functional group at its terminal with an alkoxysilane having a second reactive functional group at its terminal, the first reactive functional group is either a hydroxyl group or a thiol group, The polyglycerin-based alkoxysilane is characterized in that the second reactive functional group is either a vinyl group or an isocyanate group.
3. The glycerin derivative has a first reactive functional group at its terminal and is soluble in ethylene oxide or 3. The method according to claim 1 or 2, characterized in that propylene oxide is added. The polyglycerin-based alkoxysilane described above.
Citation Information
Patent Citations
Anti-fogging covering
JP1991215589A
Moisture-curable resin composition
JP2000063510A
Room temperature setting composition
JP2001072854A
Method for producing oxyalkylene polymer containing hydrolyzable silyl group and curable composition
JP2002088148A
Polymeric material, and adhesive and coating composition composed of and based on multi-alkoxysilyl-functional prepolymer
JP2010077432A