Highly corrosion-resistant aluminum alloy

By adding Ti, Cr, and Zr to aluminum alloys with controlled impurities, the alloy achieves enhanced corrosion resistance and mechanical strength for automotive components in saltwater environments.

JP7576345B2Active Publication Date: 2024-10-31WHEEL CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022569161
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-31
Publication Date
2024-10-31
Estimated Expiration
2041-03-31

AI Technical Summary

Technical Problem

Existing aluminum alloys used in vehicles, such as 3003, 3004, and 3014, do not meet the requirements for high tensile strength, yield strength, and corrosion resistance in saltwater environments, particularly in automotive components like receiver dryers and refrigerant lines.

Method used

Incorporating specific amounts of Ti, Cr, and Zr into the aluminum alloy composition, along with controlled levels of Cu, Si, and Fe, to enhance corrosion resistance and mechanical properties.

Benefits of technology

The alloy exhibits improved corrosion resistance and maintains high tensile and yield strength levels in saltwater environments, suitable for automotive components and other applications requiring durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576345000004
    Figure 0007576345000004
  • Figure 0007576345000005
    Figure 0007576345000005
  • Figure 0007576345000006
    Figure 0007576345000006
Patent Text Reader

Abstract

The present invention relates to a highly corrosion-resistant aluminum alloy containing, by weight percent, 0.1% or less (excluding 0%) of Cu, 0.15% or less (excluding 0%) of Si, 0.2% or less (excluding 0%) of Fe, 0.9 to 1.5% of Mn, and one or more of 0.03 to 0.15% of Ti, 0.03 to 0.15% of Cr, and 0.03 to 0.15% of Zr, with the balance consisting of Al and unavoidable impurities. The highly corrosion-resistant aluminum alloy of the present invention can provide an aluminum alloy with improved corrosion resistance in saltwater environments at excellent levels of tensile strength and yield strength by further adding Ti, Cr, and Zr to the aluminum alloy, or by adding these elements in equal amounts.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The technical concept of the present invention relates to highly corrosion resistant aluminum alloys, and more particularly to aluminum alloys with improved corrosion resistance in salt water environments at superior tensile and yield strength levels. [Background technology]

[0002] Generally, aluminum alloys, which are widely used in vehicles, are made by adding various elements (Mn, Si, Mg, Cu, Zn, Cr, etc.) to improve strength mainly through precipitation hardening, since pure aluminum has low strength. Aluminum has excellent corrosion resistance because an oxide film protects the base material in an environment of pH 4.5 to 8.5, but because it has a high tendency to ionize, it corrodes severely when it comes into contact with Fe, Cu, Pb, etc. in a corrosive environment, and it corrodes severely even if only a small amount of mercury is present in the ppm range.

[0003] The 3xxx series aluminum alloys are alloys with Mn as the main additive, and are non-heat-treatable alloys that have various properties through cooling processing. Compared to pure aluminum, they have slightly higher strength, good weldability, corrosion resistance, and formability. In particular, 3003 aluminum alloy is a representative alloy of this series, and is an alloy that has a slightly increased strength without decreasing the formability and corrosion resistance of pure aluminum due to the addition of Mn. Such alloys have a wide range of applications, such as aluminum-based utensils, building materials, and containers. 3004 and 3014 aluminum alloys, which are alloys equivalent to 3003 and have about 1% by weight of Mg added, are alloys with even higher strength. However, they do not meet the formability and strength required for part characteristics that require higher quality, and they also have the problem of corrosion occurring in saltwater environments.

[0004] Therefore, there is a need for an aluminum alloy composition having excellent tensile strength and yield strength levels and improved corrosion resistance in salt water environments that can be applied to pipe structures used as refrigerant lines, cooling water lines, and variable speed oil cooler lines in automotive receiver driers or automotive refrigerant delivery systems. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Registration No. 04411803 [Patent Document 2] Korean Patent Publication No. 10-2005-0035447 Summary of the Invention [Problem to be solved by the invention]

[0006] The technical problem to be solved by the technical idea of ​​the present invention is to provide an aluminum alloy having improved corrosion resistance in a salt water environment at excellent levels of tensile strength and yield strength by further adding Ti, Cr and Zr components to the aluminum alloy, particularly by adding these components in equal amounts. [Means for solving the problem]

[0007] The highly corrosion-resistant aluminum alloy according to the technical idea of ​​the present invention for solving the above technical problems can contain, by weight, Cu: 0.1% or less (excluding 0%), Si: 0.15% or less (excluding 0%), Fe: 0.2% or less (excluding 0%), Mn: 0.9 to 1.5%, as well as one or more of Ti: 0.03 to 0.15%, Cr: 0.03 to 0.15%, and Zr: 0.03 to 0.15%, with the balance being Al and unavoidable impurities.

[0008] In some embodiments of the present invention, all of Ti: 0.03 to 0.15%, Cr: 0.03 to 0.15%, and Zr: 0.03 to 0.15% may be contained.

[0009] In some embodiments of the present invention, the Ti: 0.03 to 0.15%, the Cr: 0.03 to 0.15%, and the Zr: 0.03 to 0.15% may all be contained, and the Ti, Cr, and Zr may be contained in equal amounts.

[0010] In some embodiments of the present invention, all of Ti: 0.05 to 0.1%, Cr: 0.05 to 0.1%, and Zr: 0.05 to 0.1% may be contained.

[0011] In some embodiments of the present invention, the Ti: 0.05-0.1%, the Cr: 0.05-0.1%, and the Zr: 0.05-0.1% may all be contained, and the Ti, Cr, and Zr may be contained in equal amounts. Effect of the Invention

[0012] The highly corrosion-resistant aluminum alloy according to the technical concept of the present invention can provide an aluminum alloy having improved corrosion resistance at excellent tensile strength and yield strength levels by further adding Ti, Cr and Zr components to the aluminum alloy, or in particular by adding these components in equal amounts.

[0013] The effects of the present invention described above are merely illustrative, and the effects of the present invention are not limited to these effects. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a block diagram showing an automobile air conditioner / engine cooling system. [Diagram 2] This is a diagram of an automobile air conditioner (heat exchanger) and a receiver-drier. [Diagram 3] 3a and 3b are photographs showing before and after evaluation of corrosion resistance of a receiver-drier manufactured using an aluminum alloy composition according to an embodiment of the present invention. [Figure 4] 4a and 4b are photographs showing before and after evaluation of corrosion resistance of a receiver-drier manufactured using an aluminum alloy composition according to a comparative example of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. The embodiments of the present invention are provided to more completely explain the technical idea of ​​the present invention to those skilled in the art, and the following embodiments can be modified into various other forms. The scope of the technical idea of ​​the present invention is not limited to the following embodiments. Rather, these embodiments are provided to make the present disclosure more faithful and complete, and to fully convey the technical idea of ​​the present invention to those skilled in the art. As used herein, the term "and / or" includes any one and all combinations of more than one of the listed items. The same reference numerals refer to the same elements. Furthermore, various elements and regions in the drawings are depicted diagrammatically. Therefore, the technical idea of ​​the present invention is not limited by the relative sizes or spacings depicted in the accompanying drawings.

[0016] The present alloy can be used as a material for the receiver-drier 10, the expansion valve 70 for expanding the refrigerant, and the pipe 30 and hose 40, 60 that connect them, which are used in an automobile air conditioner / engine cooling system. The condenser 20 in an automobile air conditioner operates to remove heat from gas or vapor, and liquefaction occurs when sufficient heat is removed. The condenser 20 is a type of radiator that releases heat from the gas refrigerant supplied from the compressor 50 into the atmosphere to turn it into a liquid refrigerant, and the more heat it releases, the better. The high-temperature, high-pressure refrigerant sent from the compressor 50 is cooled and liquefied by the temperature of the outside air, and then sent to the long cylindrical aluminum receiver-drier 10. The receiver-drier 10 is a tank that stores the refrigerant and serves to remove moisture from the refrigerant. When an automobile is operated for a long period of time, internal corrosion occurs due to condensed water generated from the inside. Moreover, external corrosion also occurs severely due to snow removal agents such as calcium chloride that are spread on road surfaces in winter. Therefore, the present alloy is required to have excellent properties of high corrosion resistance.

[0017] The high corrosion-resistant aluminum alloy according to the present invention, by weight, contains Cu: 0.1% or less (excluding 0%), Si: 0.15% or less (excluding 0%), Fe: 0.2% or less (excluding 0%), Mn: 0.9 to 1.5%, and in addition, contains one or more of Ti: 0.03 to 0.15%, Cr: 0.03 to 0.15%, and Zr: 0.03 to 0.15%, and the balance can consist of Al and unavoidable impurities.

[0018] In the alloy, Cu serves to improve the strength and ductility of the alloy due to the hardening effect. Cu is preferably adjusted to a range of more than 0 wt.% to 0.1 wt.% (0 wt.% < Cu ≦ 0.1 wt.%). More preferably, Cu is adjusted to a range of more than 0 wt.% to 0.05 wt.% (0 wt.% < Cu ≦ 0.05 wt.%). When Cu exceeds 0.1 wt.%, it is preferably added at 0.1 wt.% or less as the corrosion resistance decreases, and more preferably added at 0.05 wt.% or less.

[0019] In the alloy, Si serves to improve the strength while deteriorating the corrosion resistance. Si precipitates to improve the mechanical properties. Si is preferably adjusted to a range of more than 0 wt.% to 0.15 wt.% (0 wt.% < Si ≦ 0.15 wt.%). More preferably, Si is adjusted to a range of more than 0 wt.% to 0.05 wt.% (0 wt.% < Si ≦ 0.05 wt.%). When Si exceeds 0.15 wt.%, not only does the formability decrease, but the surface quality of the formed product may also decrease, and it is preferably added at 0.05 wt.% or less.

[0020] In the alloy, Fe can contribute to the improvement of strength by increasing the density of the alloy. Fe is preferably adjusted to a range of more than 0 wt.% to 0.2 wt.% (0 wt.% < Fe ≤ 0.2 wt.%). More preferably, Fe is adjusted to a range of 0.05 wt.% or more to 0.15 wt.% (0.05 wt.% ≤ Fe ≤ 0.15 wt.%). When Fe exceeds 0.2 wt.%, it not only reduces ductility but also may reduce extrudability and productivity, and may cause corrosion of the material. Therefore, the upper limit of Fe is preferably 0.2 wt.% or less, and more preferably 0.15 wt.% or less. Alternatively, Fe is 0.09 wt % or less.

[0021] In the alloy, Mn does not significantly weaken the corrosion resistance, but plays a role in increasing the softening resistance at high temperatures and improving the surface treatment characteristics. Also, the strength is improved by the solid solution strengthening effect and the fine precipitate dispersion effect. Mn is preferably adjusted to a range of 0.9 wt.% or more to 1.5 wt.% (0.9 wt.% ≤ Mn ≤ 1.5 wt.%). More preferably, Mn is adjusted to a range of 1.0 wt.% or more to 1.5 wt.% (1.0 wt.% ≤ Mn ≤ 1.5 wt.%). When Mn is less than 0.9 wt.%, the effect cannot be expected, and when Mn exceeds 1.5 wt.%, the castability deteriorates, which is not good.

[0022] In the alloy, Ti plays a role in improving the formability and strength by refining the crystal grains. Ti is preferably adjusted to a range of 0.03 wt.% or more to 0.15 wt.% (0.03 wt.% ≤ Ti ≤ 0.15 wt.%). More preferably, Ti is adjusted to a range of 0.05 wt.% or more to 0.1 wt.% (0.05 wt.% ≤ Ti ≤ 0.1 wt.%). When Ti is less than 0.03 wt.%, the effect cannot be expected, and when Ti exceeds 0.15 wt.%, a large amount of large and coarse intermetallic compounds such as TiAl3 are produced, which deteriorates the mechanical properties of the alloy, which is not good. When Ti is less than 0.03 wt.%, the effect cannot be expected, and when Ti exceeds 0.15 wt.%, the mechanical properties deteriorate, which is not good.

[0023] Cr forms a compound with Al in the alloy and distributes at the grain boundaries to suppress precipitation during aging treatment and improve the elongation rate. Cr is preferably adjusted to a range of 0.03 wt.% or more to 0.15 wt.% (0.03 wt.%≦Cr≦0.15 wt.%). More preferably, Cr is adjusted to a range of 0.05 wt.% or more to 0.1 wt.% (0.05 wt.%≦Cr≦0.1 wt.%). If Cr is less than 0.03 wt.%, no effect can be expected, and if Cr is more than 0.15 wt.%, the strength decreases, which is not good.

[0024] Zr plays a role in improving the strength and corrosion resistance of the alloy at high temperatures. Zr is preferably adjusted to a range of 0.03 wt.% or more to 0.15 wt.% (0.03 wt.%≦Zr≦0.15 wt.%). More preferably, Zr is adjusted to a range of 0.05 wt.% or more to 0.1 wt.% (0.05 wt.%≦Zr≦0.1 wt.%). If Zr is less than 0.03 wt.%, no effect can be expected, and if Zr is more than 0.15 wt.%, cracks and breakage occur, which is not good.

[0025] In particular, it may contain all of Ti: 0.03-0.15%, Cr: 0.03-0.15%, and Zr: 0.03-0.15%. It may also contain all of Ti: 0.03-0.15%, Cr: 0.03-0.15%, and Zr: 0.03-0.15%, but the Ti, Cr, and Zr may be contained in equal amounts. More preferably, it may contain Ti: 0.05-0.1%, Cr: 0.05-0.1%, and Zr: 0.05-0.1%.

[0026] As described above, the highly corrosion-resistant aluminum alloy according to the present invention may contain, by weight percent, Cu: 0.1% or less (excluding 0%), Si: 0.15% or less (excluding 0%), Fe: 0.2% or less (excluding 0%), Mn: 0.9 to 1.5%, as well as one or more of Ti: 0.03 to 0.15%, Cr: 0.03 to 0.15%, and Zr: 0.03 to 0.15%, with the balance being Al and unavoidable impurities.

[0027] More preferably, the alloy contains all of Ti: 0.05-0.1%, Cr: 0.05-0.1%, and Zr: 0.05-0.1%, and by containing the Ti, Cr, and Zr in equal amounts, the alloy improves corrosion resistance in a salt water environment with excellent tensile strength and yield strength levels.

[0028] The process of the present invention will now be described in detail with reference to the following examples and experimental examples.

[0029] Aluminum alloy preparation Table 1 shows the composition of a highly corrosion-resistant aluminum alloy according to an embodiment of the present invention in terms of weight percent. Aluminum alloy compositions according to the present invention (Examples 1 to 10) and comparative aluminum alloy compositions (Comparative Examples 1 to 5) were prepared with the following composition ratios. Comparative Examples 4 and 5 used the compositions of conventional 3005 and 3004 alloys. In Table 1, the aluminum alloys, apart from the alloy composition, consist of the remainder Al and unavoidable impurities.

[0030] [Table 1] Preparation of test specimens and mechanical evaluation Among the alloys according to the present invention, three types of alloys, Examples 2 to 4, were used to prepare test pieces according to the ASTM standard, and the yield strength and tensile strength were measured at room temperature using a tensile tester. As a result, as shown in Table 2, all of Examples 2 to 4 of the present invention had a tensile strength of 180 N / mm 2 The above characteristics were shown. In addition to Examples 2, 3, and 4, the tensile strength of the alloys according to the other examples was also 180 N / mm 2 The above characteristics were shown. The tensile strength of the comparative example measured under the same conditions was 180N / mm 2 It was determined that the quality was inferior to that of the

[0031] [Table 2] Fabrication of receiver-driers and evaluation of their corrosion resistance An aluminum billet is manufactured from the aluminum alloy compositions according to Examples 1 to 10 of the present invention and the aluminum alloy compositions to be compared (Comparative Examples 1 and 5), and the billet is extruded and drawn to manufacture an aluminum pipe. Then, the left and right ends of the aluminum pipe are formed and bent to form into a receiver-dryer shape, thereby manufacturing a receiver-dryer.

[0032] After manufacturing receiver-driers with thicknesses of 1.6T and 1.8T, a corrosion resistance evaluation was performed. Figure 2 shows photographs of a receiver-drier manufactured with an aluminum alloy composition according to an embodiment of the present invention before and after the corrosion resistance evaluation, and Figures 4a and 4b show photographs of a receiver-drier manufactured with an aluminum alloy composition according to a comparative example of the present invention before and after the corrosion resistance evaluation. As shown in Figure 4b, a leak can be confirmed after the corrosion resistance evaluation.

[0033] Table 3 shows the results of a corrosion resistance test completed on a receiver-drier manufactured with the aluminum alloy composition in Table 1. The corrosion resistance test (SWAAT - Seawater Acidified Test) examines the corrosion resistance by exposing the sample to a mist of salt water according to the regulations to accelerate corrosion. 2 ) nitrogen pressure is applied, and the test is carried out for 500 to 2000 hours with the following conditions: concentration: synthetic sea salt 42g / 1L, spray amount: 1 to 2ml / h, specific gravity: 1.0255 to 1.0400, pH: 2.8 to 3.0 (complying with ASTM G85 94-A3).

[0034] Distilled water was placed in the tank, and synthetic sea salt was added according to the amount of distilled water, and stirred until completely dissolved. Acetic acid was added according to the amount of distilled water, and after stirring, the test solution was confirmed to meet the condition values ​​using a specific gravity meter and a pH meter. A trial run was performed for one hour to confirm that the spray volume met the conditions, and the sample was placed in the chamber. The atmosphere in the chamber was adjusted to 49°C, and tests were performed for 250 cycles (500 hr), 500 cycles (1,000 hr), and 1,000 cycles (2,000 hr) under the conditions of 30 minutes of spraying and 90 minutes of leaving.

[0035] [Table 3] As shown in Table 3, in the corrosion resistance evaluation after the 250 cycle_5000 hr test, all of the Examples and Comparative Examples showed good results with no leaks. After the 500 cycle_1,000 hr test, leaks that did not occur in Examples 1 to 10 were observed in Comparative Examples 1 to 5, respectively. In particular, in the case of the receiver-driers manufactured to a thickness of 1.6T, leaks occurred in all of Comparative Examples 1 to 5. Therefore, it was confirmed that the receiver-driers manufactured from the aluminum alloys of Examples 1 to 10 according to the composition of the present invention have sufficient corrosion resistance for use as receiver-driers because no leaks occurred at both thicknesses of 1.6T and 1.8T in a saltwater environment of 500 cycles_1,000 hr.

[0036] Furthermore, corrosion resistance was evaluated in a harsh environment of 1000 cycles_2,000 hr. As a result of the experiment, it was confirmed that in the case of Examples 2 to 4, leaks did not occur even in a harsh environment of 1000 cycles_2,000 hr for both thicknesses of 1.6T and 1.8T, and therefore excellent corrosion resistance was obtained. It was confirmed that Examples 2 to 4 have excellent corrosion resistance when the composition contains Ti, Cr, and Zr in equal amounts within the range of 0.05 to 0.1%.

[0037] As described above, the highly corrosion-resistant aluminum alloy according to the present invention can provide an aluminum alloy with improved corrosion resistance in a saltwater environment with excellent tensile strength and yield strength levels. The highly corrosion-resistant aluminum alloy according to the present invention can be applied to all aluminum parts other than receiver-driers, and can achieve the same effects. Therefore, the highly corrosion-resistant aluminum alloy can be used to manufacture not only automobile receiver-driers, but also pipe structures used as refrigerant lines, cooling water lines, and variable-speed oil cooler lines in automobile refrigerant transport systems by extrusion and drawing methods.

[0038] In addition, the highly corrosion-resistant aluminum alloy according to the present invention can be used in a variety of products that need to be prevented from corrosion, such as refrigerators, washing machines, home air conditioners, heat sinks for LEDs, electrical appliances, roofing materials, chemical equipment, kitchen appliances, and ship exterior materials.

[0039] It will be apparent to those skilled in the art to which the technical idea of ​​the present invention pertains that the technical idea of ​​the present invention described above is not limited to the above-mentioned embodiments and accompanying drawings, and that various substitutions, modifications and changes can be made without departing from the technical idea of ​​the present invention. [Explanation of symbols]

[0040] 10 Receiver dryer 20 Condenser 30 Pipe 40 Horse 50 Compressor 60 Hose 70 Expansion valve 80 Evaporator

Claims

1. A highly corrosion-resistant aluminum alloy containing, by weight percent, Cu: 0.1% or less (excluding 0%), Si: 0.15% or less (excluding 0%), Fe: 0.09% or less (excluding 0%), Mn: 0.9 to 1.5%, Ti, Cr and Zr, with the balance being Al and unavoidable impurities, wherein the Ti, Cr and Zr are contained in the same weight percents, and the weight percents are set to 0.03 to 0.15 weight percent, thereby improving the corrosion resistance of the highly corrosion-resistant aluminum alloy in a salt water environment, and the contents of the Ti, Cr and Zr are the same to two decimal places.

2. 2. The highly corrosion-resistant aluminum alloy according to claim 1, wherein the Ti, Cr and Zr are each 0.05 to 0.1 wt %.

Citation Information

Patent Citations

  • Aluminum alloy, microchannel aluminum flat pipe and preparation method of microchannel aluminum flat pipe

    CN108531783A

  • JP04411803B

  • High corrosion resistant aluminum alloy, clad material thereof, and its production

    JP1999241136A

  • Aluminum alloy material for piping excellent in corrosion resistance and workability