Expandable vinyl chloride resin particles, pre-expanded particles, foamed molded product, and method for producing expandable vinyl chloride resin particles
By incorporating a specific blend of hydrocarbon and ketone blowing agents in expandable vinyl chloride resin particles, the foaming efficiency is improved, leading to high expansion ratio and flame-retardant foam molded articles suitable for fire-resistant insulation.
Patent Information
- Application Number
- JP2020162885
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-29
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2040-09-29
AI Technical Summary
Existing expandable chlorinated vinyl chloride resin particles have limitations in foaming efficiency, which affects the production of foamed molded products with desired flame retardancy and shape flexibility.
The use of expandable vinyl chloride resin particles containing a specific blend of hydrocarbon and ketone blowing agents, with controlled pore structure and composition, enhances foaming efficiency by improving agent retention and compatibility with the resin.
The solution results in pre-expanded particles and foam molded articles with high expansion ratios and excellent flame retardancy, suitable for applications requiring fire resistance and insulation.
Smart Images

Figure 0007576422000001
Abstract
Description
[Technical field]
[0001] The present invention relates to expandable vinyl chloride resin particles, pre-expanded particles, foamed molded articles, and a method for producing expandable vinyl chloride resin particles. [Background technology]
[0002] Resin foams have light weight, heat insulation, and shock-absorbing properties, and have been widely used as insulation materials for houses and the like, and heat-retaining materials for pipes and the like. Among them, styrene resin foam molded products obtained using expandable styrene resin particles containing a foaming agent have a high degree of freedom in shape, and are widely used as insulation materials that can be applied to areas where it is difficult to apply foams of simple shapes such as board shapes obtained by extrusion foaming methods and the like. Since styrene resins are flammable resins, flame retardants are added to styrene resin foam molded products to ensure a certain degree of flame retardancy. However, due to recent fire accidents at construction sites and fire cases in high-rise apartment buildings, higher flame retardancy than before is being required for insulation materials for construction.
[0003] Examples of foams having excellent flame retardancy include resin foam molded articles using vinyl chloride resins or chlorinated vinyl chloride resins, both of which have excellent flame retardancy, as a base resin.
[0004] For example, Patent Documents 1 and 2 describe foams obtained by in-mold expansion molding of pre-expanded chlorinated polyvinyl chloride resin particles containing a solvent compatible with chlorinated polyvinyl chloride resin and a blowing agent. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP-A-64-132 [Patent Document 2] Japanese Patent Publication No. 2-182735 Summary of the Invention [Problem to be solved by the invention]
[0006] The pre-expanded chlorinated polyvinyl chloride resin particles disclosed in Patent Documents 1 and 2 are excellent in flame retardancy and can give foamed molded articles with a high degree of freedom in shape, but there is room for improvement in the foaming efficiency.
[0007] SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to provide expandable vinyl chloride resin particles having excellent expansion efficiency. [Means for solving the problem]
[0008] Means for Solving the Problems The inventors of the present application conducted intensive research to solve the above-mentioned problems and as a result discovered that expandable vinyl chloride resin particles containing a specific foaming agent and having a specific structure contribute to the foaming efficiency, thereby completing the present invention.
[0009] That is, the present invention provides: [1] Expandable polyvinyl chloride resin particles containing a blowing agent, which satisfy the following (a), (b), and (c): (a) The foaming agent contains a hydrocarbon foaming agent and a ketone foaming agent. (b) The content of the foaming agent is 1 to 30% by weight based on 100% by weight of the foamable polyvinyl chloride resin particles. (c) The sum of the log differential pore volumes of pores having diameters of 70 to 500 nm measured in the expandable polyvinyl chloride resin particles by mercury intrusion porosimetry is 0.300 ml / g or less. [2] The expandable polyvinyl chloride resin particles according to the above [1], wherein the ratio of the ketone-based blowing agent is 4 to 70% by weight, when the total amount of the hydrocarbon-based blowing agent and the ketone-based blowing agent is 100% by weight. [3] The expandable polyvinyl chloride resin particles according to the above [1] or [2], wherein the boiling point of the ketone-based blowing agent is 130° C. or lower. [4] The expandable vinyl chloride resin particles according to any one of the above [1] to [3], wherein the hydrocarbon foaming agent contains at least one saturated hydrocarbon having 4 to 6 carbon atoms. [5] The expandable polyvinyl chloride resin particles according to any one of the above [1] to [4], which contain a chlorinated polyvinyl chloride resin. [6] The expandable polyvinyl chloride resin particles according to any one of the above [1] to [5], which contain at least one member selected from the group consisting of a copolymer having an aromatic vinyl monomer and an unsaturated nitrile as a structural unit, an acrylic resin, and a chlorinated polyethylene. [7] Pre-expanded particles of the expandable vinyl chloride resin particles according to any one of the above [1] to [6]. [8] A foamed molded article obtained by using the expandable vinyl chloride resin particles according to any one of the above [1] to [6] or the pre-expanded particles according to the above [7]. [9] A method for producing expandable polyvinyl chloride resin particles that satisfies the following (A), (B), and (C): (A) a step of extruding a foaming agent-containing vinyl chloride resin melt obtained by melt-kneading a vinyl chloride resin composition and a foaming agent through a die having a plurality of holes into pressurized water, cutting the melt with a rotary cutter to form particles, and then cooling and solidifying the melt, (B) the blowing agent includes a hydrocarbon-based blowing agent and a ketone-based blowing agent; (C) The amount of the foaming agent added is 1 to 30 parts by weight based on 100 parts by weight of the vinyl chloride resin composition.
[10] The method for producing expandable polyvinyl chloride resin particles according to the above [9], wherein the ratio of the hydrocarbon-based blowing agent to the ketone-based blowing agent is 96:4 to 30:70 (wt %). Effect of the Invention
[0010] The expandable vinyl chloride resin particles of the present invention have excellent expansion efficiency. According to the expandable vinyl chloride resin particles of the present invention, pre-expanded particles and foamed molded articles having a high expansion ratio can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Unless otherwise specified in this specification, "A to B" representing a numerical range means "A or more and B or less." In addition, "A and / or B" means "A, B, and A and B." In the above Patent Documents 1 and 2, the expansion efficiency of the obtained foam is not disclosed in detail. However, when the ratio of the molded body magnification to the amount of the blowing agent re-impregnated into the pre-expanded particles was calculated, it was 0.6 to 1.9. Therefore, it was considered that there was a problem in further improving the expansion efficiency.
[0012] Therefore, the present inventors conducted extensive research and discovered that the foaming efficiency of expandable polyvinyl chloride resin particles can be improved by containing a specific foaming agent and having a specific structure, which led to the successful development of the present invention.
[0013] (Expandable polyvinyl chloride resin particles) The expandable vinyl chloride resin particles of the present invention are characterized in that they contain 1-30% by weight of a hydrocarbon blowing agent and a ketone blowing agent based on 100% by weight of the expandable vinyl chloride resin particles, and that the sum of the Log differential pore volumes of 70-500 nm diameters measured by mercury intrusion porosimetry is 0.300 ml / g or less. Due to these characteristics, the expandable vinyl chloride resin particles of the present invention can exhibit excellent expansion efficiency.
[0014] Generally, it is difficult for a hydrocarbon-based foaming agent to be impregnated into a vinyl chloride resin pellet. In the present invention, by allowing a ketone-based foaming agent to coexist with a hydrocarbon-based foaming agent, the ketone-based foaming agent penetrates between the molecules of the vinyl chloride resin and expands the molecular chains, creating a space in which the hydrocarbon-based foaming agent, which is originally not compatible with the vinyl chloride resin, can easily penetrate between the molecules of the vinyl chloride resin, and the ketone-based foaming agent exerts an effect as a compatibilizer between the vinyl chloride resin and the hydrocarbon-based foaming agent, so that it is considered that the amount of the hydrocarbon-based foaming agent dissolved in the vinyl chloride resin is increased. In addition, in the present invention, by controlling the fine pores of the expandable vinyl chloride resin particles, the dispersion of the foaming agent, including the hydrocarbon-based foaming agent, in the expandable vinyl chloride resin particles is effectively controlled, and the retention of the foaming agent in the expandable vinyl chloride resin particles is improved. In addition, the effect of the ketone-based foaming agent is that it reduces the viscosity of the vinyl chloride resin during foaming to a viscosity suitable for obtaining a high expansion ratio, and since it is itself a foaming agent, it is considered to contribute to the foaming efficiency.
[0015] (Vinyl chloride resin) The vinyl chloride resin used in the present invention is not particularly limited, and examples thereof include polyvinyl chloride (vinyl chloride homopolymer); vinyl chloride-vinyl acetate copolymer, vinyl chloride-(meth)acrylic acid copolymer, vinyl chloride-methyl (meth)acrylate copolymer, vinyl chloride-ethyl (meth)acrylate copolymer, vinyl chloride-maleic acid ester copolymer, vinyl chloride-ethylene copolymer, vinyl chloride-propylene copolymer, vinyl chloride-styrene copolymer, vinyl chloride-isobutylene copolymer, vinyl chloride-vinylidene chloride copolymer, vinyl chloride-styrene-maleic anhydride terpolymer, vinyl chloride-styrene-acrylonitrile terpolymer, vinyl chloride-butadiene copolymer, and the like. Examples of the vinyl chloride-based copolymers include vinyl chloride copolymers of vinyl chloride and other monomers copolymerizable with vinyl chloride, such as vinyl chloride-isoprene copolymers, vinyl chloride-chlorinated propylene copolymers, vinyl chloride-vinylidene chloride-vinyl acetate terpolymers, vinyl chloride-acrylonitrile copolymers, and vinyl chloride-various vinyl ether copolymers; vinyl chloride-based copolymers after chlorination, and vinyl chloride-based polymers (polyvinyl chloride and polyvinyl chloride-based copolymers may be collectively referred to as "vinyl chloride-based polymers") that have been modified (chlorinated, etc.). In addition, chlorinated polyolefins having a chemical structure similar to polyvinyl chloride, such as chlorinated polyethylene, may be used. Among these, from the viewpoint of flame retardancy, it is preferable to include vinyl chloride-based polymers and chlorinated vinyl chloride-based polymers, and among them, chlorinated vinyl chloride-based polymers are particularly preferable from the viewpoint of excellent flame retardancy and foamability. As the vinyl chloride-based resin, one or a mixture of two or more of these may be used. In this specification, the term "vinyl chloride polymer" refers to polyvinyl chloride and / or vinyl chloride copolymer. In addition, in this specification, a chlorinated vinyl chloride polymer may be referred to as a chlorinated vinyl chloride resin.
[0016] As one embodiment of the present invention, the average degree of polymerization of the vinyl chloride polymer is not particularly limited, but the lower limit is preferably 300 or more, more preferably 400 or more. On the other hand, the upper limit is preferably 3000 or less, more preferably 1500 or less. If the average degree of polymerization is within the above range, a high expansion ratio tends to be obtained. The average degree of polymerization of the chlorinated vinyl chloride polymer is regarded as the average degree of polymerization of the vinyl chloride polymer before chlorination. The average degree of polymerization is measured in accordance with JIS K6720-2.
[0017] In one embodiment of the present manufacturing method, the vinyl chloride resin preferably contains a chlorinated vinyl chloride polymer as a main component from the viewpoint of foaming property. Although not particularly limited, the content of the chlorinated vinyl chloride polymer is preferably 50% by weight or more, more preferably 60% by weight or more, even more preferably 70% by weight or more, and most preferably 80% by weight or more in 100% by weight of the vinyl chloride resin. On the other hand, the upper limit is preferably 100% by weight of the chlorinated vinyl chloride polymer in 100% by weight of the vinyl chloride resin.
[0018] Chlorinated vinyl chloride polymers are usually produced by using a vinyl chloride polymer as a raw material, supplying chlorine to the vinyl chloride polymer dispersed in an aqueous medium, and chlorinating the polymer in an aqueous medium by irradiating the polymer with a mercury lamp for photochlorination or by heating the polymer for chlorination, or by chlorinating the vinyl chloride polymer in a gas phase by irradiating the polymer with a mercury lamp. Examples of the vinyl chloride polymer as a raw material include the polyvinyl chloride and vinyl chloride copolymers exemplified above.
[0019] In one embodiment of the present invention, the weight average molecular weight of the chlorinated vinyl chloride polymer is not particularly limited, but is preferably in the range of 30,000 to 400,000. If the weight average molecular weight is in the above range, a high expansion ratio tends to be obtained. The weight average molecular weight is evaluated by gel permeation chromatography in terms of polystyrene.
[0020] As one embodiment of the present invention, the chlorine content of the chlorinated vinyl chloride polymer is preferably in the range of 60% by weight to 75% by weight from the viewpoint of ensuring expandability. More preferably, it is 64% by weight to 70% by weight. The higher the chlorine content, the higher the expansion ratio tends to be, but on the other hand, if the chlorine content is too high, the melt viscosity increases, and the processability tends to be significantly impaired. The chlorine content of the chlorinated vinyl chloride polymer is measured in accordance with JIS K7385 B method.
[0021] In one embodiment of the present invention, as the vinyl chloride resin, a chlorinated vinyl chloride polymer may be used alone or in combination of two or more kinds.
[0022] (foaming agent) The expandable vinyl chloride resin particles of the present invention contain a hydrocarbon-based blowing agent and a ketone-based blowing agent as blowing agents.
[0023] (Hydrocarbon blowing agent) As one embodiment of the present invention, the hydrocarbon-based blowing agent may be a known hydrocarbon-based blowing agent, and is not particularly limited, but examples thereof include the following blowing agents. For example, normal butane, isobutane, normal pentane, isopentane, neopentane, cyclopentane, normal hexane, cyclohexane, etc. In the present invention, only one of these may be used, or two or more may be used in combination.
[0024] As an embodiment of the present invention, it is preferable that the hydrocarbon-based blowing agent contains at least one saturated hydrocarbon having 4 to 6 carbon atoms (4, 5, and 6 carbon atoms). When the carbon number of the blowing agent is 4 or more, the volatility is low and the blowing agent is less likely to escape from the expandable vinyl chloride resin particles, so that the blowing agent remains sufficiently in the expansion process when actually used, making it possible to obtain sufficient foaming power and facilitating high expansion ratio, which is preferable. In addition, when the carbon number is 6 or less, the boiling point of the blowing agent is not too high, so that sufficient foaming power is easily obtained by heating during pre-expansion, and there is a tendency that high foaming is easy to achieve. Examples of saturated hydrocarbons having 4 to 6 carbon atoms include normal butane, isobutane, normal pentane, isopentane, neopentane, cyclopentane, normal hexane, and cyclohexane. As the saturated hydrocarbons having 4 to 6 carbon atoms, it is preferable to use at least pentane from the viewpoint of the solubility and retention of the blowing agent in the resin. These hydrocarbon-based blowing agents may be used alone or in combination of two or more.
[0025] (Ketone-based foaming agent) As an embodiment of the present invention, the ketone-based foaming agent may be a known ketone-based foaming agent, and is not particularly limited, but examples thereof include the following foaming agents. For example, acetone, methyl ethyl ketone, diethyl ketone, methyl propyl ketone, methyl butyl ketone, methyl isobutyl ketone, methyl hexyl ketone, ethyl propyl ketone, ethyl butyl ketone, diisobutyl ketone, cyclohexanone, diacetone alcohol, etc. These may be used alone or in combination of two or more. By using a hydrocarbon-based foaming agent and a ketone-based foaming agent in combination, the solubility of the hydrocarbon-based foaming agent in the vinyl chloride resin may be further improved.
[0026] In one embodiment of the present invention, the ketone-based foaming agent preferably contains a ketone-based foaming agent having a boiling point of 130° C. or less. If the boiling point of the ketone-based foaming agent is 130° C. or less, the ketone also acts as a foaming agent during heating and foaming, so that a high foaming ratio is easily obtained. In addition, the ketone is easily volatilized from the resin during foaming, and the viscosity of the resin increases at the completion of foaming, so that the bubble film is less likely to break, and a high foaming ratio is easily obtained. Examples of the ketone-based foaming agent having a boiling point of 130° C. or less include acetone, methyl ethyl ketone, diethyl ketone, methyl propyl ketone, methyl isobutyl ketone, ethyl propyl ketone, and methyl butyl ketone. As the ketone-based foaming agent having a boiling point of 130° C. or less, it is preferable to use at least acetone, since it easily contributes as a foaming agent. These ketone-based foaming agents may be used alone or in combination of two or more.
[0027] As one embodiment of the present invention, the ratio of the hydrocarbon-based foaming agent and the ketone-based foaming agent contained in the expandable vinyl chloride resin particles is preferably hydrocarbon-based foaming agent / ketone-based foaming agent=96-30 / 4-70 (wt%), more preferably hydrocarbon-based foaming agent / ketone-based foaming agent=90-40 / 10-60 (wt%), and particularly preferably hydrocarbon-based foaming agent / ketone-based foaming agent=85-50 / 15-50 (wt%), when the total of the hydrocarbon-based foaming agent and the ketone-based foaming agent is 100 wt%. By having the hydrocarbon-based foaming agent and the ketone-based foaming agent in the above ranges, it is possible to increase the amount of the hydrocarbon-based foaming agent dissolved in the vinyl chloride resin, and also to increase the foaming efficiency, thereby enabling high foaming.
[0028] (Other foaming agents) The expandable vinyl chloride resin particles of the present invention may contain the above-mentioned hydrocarbon-based and ketone-based blowing agents as the blowing agents, but may also contain other blowing agents. As the other blowing agents, known blowing agents can be used, and are not particularly limited, but examples thereof include the following blowing agents. For example, ethers such as dimethyl ether, diethyl ether, methyl ethyl ether, isopropyl ether, n-butyl ether, diisopropyl ether, furan, furfural, 2-methylfuran, tetrahydrofuran, and tetrahydropyran, saturated alcohols having 1 to 4 carbon atoms such as methanol, ethanol, propyl alcohol, i-propyl alcohol, butyl alcohol, i-butyl alcohol, and t-butyl alcohol, carboxylates such as methyl formate, ethyl formate, propyl formate, butyl formate, amyl formate, methyl propionate, and ethyl propionate, and halogenated aryl such as methyl chloride and ethyl chloride. Examples of the foaming agents that can be used include hydrofluoroolefins such as alkyl, trans-1,3,3,3-tetrafluoropropene (trans-HFO-1234e), cis-1,3,3,3-tetrafluoropropene (cis-HFO-1234ze), 2,3,3,3-tetrafluoropropene (trans-HFO-1234yf), trans-1-chloro-3,3,3-trifluoropropene (trans-HCFO-1233zd), cis-1-chloro-3,3,3-trifluoropropene (cis-HCFO-1233zd), or chlorinated hydrofluoroolefins, water, carbon dioxide, nitrogen, and other inorganic foaming agents, and chemical foaming agents such as azo compounds and tetrazole. These other foaming agents may be used alone or in combination of two or more.
[0029] The expandable vinyl chloride resin particles of the present invention have a foaming agent content of 1 to 30% by weight, preferably 2 to 25% by weight, based on 100% by weight of the expandable vinyl chloride resin particles. By controlling the foaming agent content within the above-mentioned predetermined range, it is possible to easily obtain expanded beads having a high expansion ratio and foamed molded articles having excellent surface beauty. The more preferred range is 3 to 22% by weight, and even more preferably 4 to 20% by weight.
[0030] (Processing aids) As one embodiment of the present invention, the expandable vinyl chloride resin particles may contain a processing aid. The processing aid may be any processing aid commonly used for vinyl chloride resins, and may include, for example, a copolymer having an aromatic vinyl monomer and an unsaturated nitrile monomer as structural units, such as a styrene-acrylonitrile copolymer, an impact modifier such as an acrylic resin, a methyl methacrylate-butadiene-styrene polymer, and chlorinated polyethylene. In order to easily obtain expanded particles and foamed molded articles with a high expansion ratio, it is preferable to contain at least one selected from the group consisting of a copolymer having an aromatic vinyl monomer and an unsaturated nitrile monomer as structural units, an acrylic resin, and a chlorinated polyethylene. Among them, from the viewpoint of improving the flowability of the vinyl chloride resin and improving the molding processability, it is more preferable to use a copolymer having an aromatic vinyl monomer and an unsaturated nitrile monomer as structural units and / or an acrylic resin in combination with chlorinated polyethylene.
[0031] In one embodiment of the present invention, the use of a copolymer having an aromatic vinyl monomer and an unsaturated nitrile monomer as structural units in a vinyl chloride resin is excellent in the effect of facilitating the production of expanded beads and expanded molded articles having a high expansion ratio, particularly in pre-expansion and expansion molding under steam heating conditions.
[0032] Examples of the aromatic vinyl monomer in the copolymer having an aromatic vinyl monomer and an unsaturated nitrile monomer as structural units include styrene derivatives such as styrene, α-methylstyrene, ethylstyrene, halogenated styrene, etc. Examples of the unsaturated nitrile monomer include acrylonitrile, methacrylonitrile, etc.
[0033] Within the scope of not impairing the effects of the present invention, the copolymer having an aromatic vinyl monomer and an unsaturated nitrile monomer as structural units may have structural units derived from monomers other than the aromatic vinyl monomer and the unsaturated nitrile monomer (other copolymerizable monomers). Examples of the other copolymerizable monomers include (meth)acrylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, N-butyl (meth)acrylate, isobutyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate, (meth)acrylic acid, maleic anhydride, and N-substituted maleimide.
[0034] The preferred range of the unsaturated nitrile monomer in the copolymer having an aromatic vinyl monomer and an unsaturated nitrile monomer as structural units is 5 to 45% by weight, more preferably 8 to 35% by weight, and even more preferably 10 to 30% by weight, based on 100% by weight of the entire copolymer having an aromatic vinyl monomer and an unsaturated nitrile monomer as structural units. By being in the above range, expanded beads and expanded molded articles with a high expansion ratio can be easily obtained.
[0035] A preferred example of the copolymer having an aromatic vinyl monomer and an unsaturated nitrile monomer as structural units is a styrene-acrylonitrile copolymer. The copolymer having an aromatic vinyl monomer and an unsaturated nitrile monomer as structural units may be used alone or in combination of two or more. In a preferred embodiment, a styrene-acrylonitrile copolymer is used as at least one of the copolymers having an aromatic vinyl monomer and an unsaturated nitrile monomer as structural units. It is preferable to use a copolymer having an aromatic vinyl monomer and an unsaturated nitrile monomer as structural units, the weight average molecular weight of which is higher than the weight average molecular weight of the vinyl chloride resin used, since it is easy to ensure a high expansion ratio. The weight average molecular weight of the copolymer having an aromatic vinyl monomer and an unsaturated nitrile monomer as structural units is evaluated in terms of polystyrene molecular weight by gel permeation chromatography. As the copolymer having an aromatic vinyl monomer and an unsaturated nitrile monomer as structural units, for example, Blendex 869 manufactured by Galata can be used.
[0036] Specific examples of acrylic resins include polymethyl methacrylate obtained by polymerizing methyl methacrylate, methacrylic acid alkyl esters having 2 to 8 carbon atoms in the alkyl group such as n-butyl methacrylate, acrylic acid alkyl esters having 1 to 8 carbon atoms in the alkyl group such as ethyl acrylate, and copolymers of at least one monomer copolymerizable with these, such as butylene, substituted styrene, and acrylonitrile. It is preferable to use an acrylic resin having a weight average molecular weight higher than that of the vinyl chloride resin used, since it is easy to ensure a high expansion ratio. The weight average molecular weight of the acrylic resin is evaluated in terms of polystyrene molecular weight by gel permeation chromatography. As the acrylic resin, for example, Kane Ace PA-40 manufactured by Kaneka can be used.
[0037] The chlorinated polyethylene may be any known chlorinated polyethylene used in vinyl chloride resins, and the chlorine content of the chlorinated polyethylene is measured in accordance with JIS K7385 B method.
[0038] The content of the processing aid is not particularly limited as long as it is within a range that does not impair the effects of the present invention, but is preferably 1 to 50 parts by weight, more preferably 5 to 50 parts by weight, and even more preferably 8 to 30 parts by weight, relative to 100 parts by weight of the vinyl chloride resin. When the content is 1 part by weight or more, expanded beads and / or expanded molded articles having a high expansion ratio are easily obtained, and when it is 50 parts by weight or less, expanded beads and / or expanded molded articles having excellent flame retardant performance can be obtained.
[0039] (Other additives) As long as the effects of the present invention are not impaired, the composition may contain, as necessary, flame retardants, stabilizers, lubricants, nucleating agents, foaming assistants, antistatic agents, radiation heat transfer inhibitors, plasticizers, solvents, and colorants such as pigments and dyes.
[0040] As the flame retardant, known flame retardants can be used, and examples thereof include bromine-based flame retardants, phosphorus-based flame retardants, boron-based flame retardants, intumescent flame retardants such as ammonium polyphosphate and melamine cyanurate, hydroxide compounds such as aluminum hydroxide and magnesium hydroxide, and flame retardant assistants such as antimony oxide, zinc oxide, and zinc borate.
[0041] The stabilizer may be any of those conventionally used in vinyl chloride resins. Examples include tin stabilizers, antioxidants such as phenolic compounds, phosphorus compounds, and amine compounds, epoxy stabilizers, and zeolites. The amount of each stabilizer used is not particularly limited as long as it does not impair the effects of the present invention, but is preferably 10 parts by weight or less per 100 parts by weight of vinyl chloride resin.
[0042] Examples of the lubricant include waxes such as ester wax and polyethylene wax, and fatty acid metal salts such as calcium stearate and zinc stearate.
[0043] Examples of the nucleating agent include inorganic compounds such as silica, calcium silicate, wollastonite, kaolin, clay, mica, zinc oxide, calcium carbonate, sodium hydrogen carbonate, zeolite, and talc.
[0044] Examples of the radiation heat transfer inhibitor include substances that have the property of reflecting, scattering, or absorbing light in the near infrared or infrared region, such as graphite, graphene, carbon black, expanded graphite, titanium oxide, and aluminum.
[0045] The plasticizer may be a substance that is compatible with vinyl chloride resins, such as bis(2-ethylhexyl) phthalate, diisononyl phthalate, epoxidized soybean oil, triphenyl phosphate, or tris(2-ethylhexyl) trimellitate.
[0046] As long as the effects of the present invention are not impaired, the vinyl chloride resin may be used in combination with other resins (thermoplastic resins or thermosetting resins).
[0047] When other resins are used in combination, the amount of the other resins is not particularly limited as long as it does not impair the effects of the present invention, but is preferably 0 to 99 parts by weight per 100 parts by weight of the vinyl chloride resin.
[0048] The expandable vinyl chloride resin particles of the present invention have a sum of Log differential pore volumes of pores having a diameter of 70 to 500 nm measured by mercury intrusion porosimetry of 0.300 ml / g or less. The sum of Log differential pore volumes is preferably 0.250 ml / g or less, more preferably 0.200 ml / g or less, and even more preferably 0.150 ml / g or less. By making the sum of Log differential pore volumes 0.300 ml / g or less, the dispersion of the blowing agent can be effectively suppressed, and the retention of the blowing agent can be improved. The sum of Log differential pore volumes referred to here can be determined by the measurement method described below.
[0049] In one embodiment of the present invention, the shape of the expandable polyvinyl chloride resin particles is not particularly limited as long as the shape of the particles allows the expandable resin particles described below to be pre-expanded and expanded, but this includes not only general granular objects (for example, small rounded particles such as spherical, approximately spherical, convex lens-like, concave lens-like, spindle-like, etc.) but also particles with depressions. In one embodiment of the present invention, the particle weight of the expandable polyvinyl chloride resin particles is preferably 0.5 to 10 mg / particle, more preferably 1 to 8 mg / particle, and even more preferably 2.5 to 7 mg / particle, from the viewpoint of ensuring the fillability of the expanded particles into a molding die and thus the moldability such as the surface beauty of the expanded molded article.
[0050] In one embodiment of the present invention, from the viewpoint of reducing the rate at which the foaming agent escapes from the foamable polyvinyl chloride resin particles or increasing the expansion ratio, the true density of the foamable polyvinyl chloride resin particles is set to 1100 kg / m 3 It is preferable that the resistance is 1150 kg / m or more. 3 More preferably, 1200kg / m 3 More preferably, 1250 kg / m 3 The true density referred to here can be determined by the measurement method described later. In one embodiment of the expandable vinyl chloride resin particles of the present invention, the maximum expansion ratio (times) / amount of foaming agent during expansion (wt%) is preferably 1.0 or more, more preferably 1.5 or more, even more preferably 2.0 or more, and particularly preferably 2.4 or more. If the maximum expansion ratio (times) / amount of foaming agent during expansion (wt%) is within the above range, high expansion is possible with a small amount of foaming agent, and it can be said that the foaming efficiency is excellent. In other words, the expandable vinyl chloride resin particles having excellent expansion efficiency are intended to mean expandable vinyl chloride resin particles that have good retention of the foaming agent relative to the amount of foaming agent used during the production of the expandable vinyl chloride resin particles, and that can be expanded at a high magnification during pre-expansion and / or expansion molding even if the amount of foaming agent contained in the expandable vinyl chloride resin particles is small. The maximum expansion ratio here is the highest expansion ratio when expansion evaluation is performed in a heated air atmosphere, and the amount of blowing agent during expansion is the weight change rate when the expandable polyvinyl chloride resin particles used in the expansion evaluation in a heated air atmosphere are heated at 150°C for 30 minutes, and can be determined specifically by the measurement method described below. Note that, since the amount of blowing agent in the expandable polyvinyl chloride resin particles changes over time, the maximum expansion ratio and the amount of blowing agent during expansion use values measured on the same day.
[0051] (Method of producing expandable polyvinyl chloride resin particles) The method for producing expandable vinyl chloride resin particles of the present invention (hereinafter, the "method for producing expandable vinyl chloride resin particles" may be referred to as the "method for producing expandable particles") comprises the steps of: (A) extruding a foaming agent-containing molten vinyl chloride resin through a die having multiple holes into pressurized water, cutting the extrudate with a rotary cutter immediately thereafter to form particles, and cooling and solidifying the extrudate; (B) the foaming agent comprises a hydrocarbon foaming agent and a ketone foaming agent; and (C) the amount of the foaming agent added is 1 to 30 parts by weight per 100 parts of vinyl chloride resin.
[0052] In the method for producing the expandable particles of the present invention, in the vinyl chloride resin melt containing the foaming agent, a hydrocarbon foaming agent and a ketone foaming agent are used in combination as foaming agents in the foaming agent-containing vinyl chloride resin melt, which is melt-kneaded with the vinyl chloride resin, thereby promoting the dissolution of the hydrocarbon foaming agent in the vinyl chloride resin, and controlling the fine pores formed in the resulting expandable vinyl chloride resin particles, thereby producing expandable vinyl chloride resin particles with excellent foaming efficiency. In other words, the method for producing the expandable particles of the present invention can be said to be one embodiment of the preferred method for producing the expandable vinyl chloride resin particles of the present invention.
[0053] One embodiment of a method for producing expandable particles includes a production method in which a vinyl chloride resin and, if necessary, various additives are supplied to an extruder and melt-kneaded, a foaming agent is dissolved / dispersed in the molten mixture by the extruder or by dispersion equipment downstream of the extruder, the molten mixture of the foaming agent-containing vinyl chloride resin composition is extruded through a die having many small holes attached downstream of the extruder into a cutter chamber filled with pressurized circulating water, and immediately after extrusion, the molten mixture is cut by a rotating cutter in contact with the die and cooled and solidified by the pressurized circulating water to obtain expandable vinyl chloride resin particles.
[0054] An embodiment of the method for producing the expandable particles will be described below. The components and the like used in the method for producing the expandable particles are the same as those of the expandable polyvinyl chloride resin particles described above, except for the matters described below.
[0055] In one embodiment of the method for producing expandable particles, a general extruder can be used as the extruder, specifically, a single screw extruder, a twin screw extruder, a tandem extruder, etc. Examples of the tandem extruder include a single screw extruder connected to two single screw extruders, and a twin screw extruder connected to a single screw extruder. In addition, an extruder may be used in combination with a dispersion device such as a static mixer or a stirrer without a screw.
[0056] In one embodiment of the method for producing expandable particles, it is preferable to gel the vinyl chloride resin sufficiently. If the gelation is not sufficient, when the resin is made into expandable resin particles, the speed at which the foaming agent escapes from the expandable resin particles may increase, and the foaming agent tends not to contribute to the expansion, and as a result, it may be difficult to obtain expanded particles and foamed molded articles having a high expansion ratio or a high closed cell ratio.
[0057] In the method for producing the expandable particles of the present invention, the amount of the foaming agent added is 1 to 30 parts by weight, preferably 2 to 25 parts by weight, more preferably 3 to 20 parts by weight, and further preferably 4 to 15 parts by weight, relative to 100 parts by weight of the vinyl chloride resin. By adjusting the amount of the foaming agent added within the above-mentioned predetermined range and controlling the foaming agent content in the expandable vinyl chloride resin particles, it becomes easier to obtain pre-expanded particles with a high expansion ratio, and an expanded molded article with a high expansion ratio can be easily obtained.
[0058] From the viewpoint of the balance between foaming properties and foaming agent retention, the ratio of the hydrocarbon-based foaming agent and the ketone-based foaming agent is preferably 96:4 to 30:70 (weight %), more preferably 90:10 to 40:60 (weight %), and further preferably 85:15 to 50:50 (weight %).
[0059] In one embodiment of the method for producing expandable particles, the resin temperature during resin melt kneading may affect the decomposition of the vinyl chloride resin and additives, so the resin temperature of the resin melt at the tip of the extruder is preferably 130 to 250 ° C, more preferably 140 to 240 ° C, and even more preferably 150 to 220 ° C. The resin temperature of the resin melt at the tip of the extruder is a value measured by a temperature sensor attached to the tip of the extruder. When two or more extruders are attached upstream of the die, the tip temperature of the most downstream extruder is taken as the resin temperature of the resin melt at the tip of the extruder in this specification. If the resin temperature is 130 ° C or higher, the resin viscosity decreases and sufficient melt kneading in the extruder is possible. If the resin temperature exceeds 250 ° C, there is a risk of decomposition of the vinyl chloride resin, the vinyl chloride resin used in combination if necessary, and additives, which may result in deterioration of the expandable vinyl chloride resin particles and lead to a decrease in foaming performance.
[0060] (Conditions of the granulation process) The conditions for the granulation step in the method for producing expandable polyvinyl chloride resin particles will be described below.
[0061] In one embodiment of the method for producing expandable particles, the tip pressure of the extruder attached upstream of the die is preferably 4 to 20 MPa, more preferably 6 to 18 MPa, and even more preferably 7 to 15 MPa. The extruder tip pressure is a value measured by a pressure sensor attached to the tip of the extruder. When two or more extruders are attached upstream of the die, the tip pressure of the most downstream extruder is defined as the extruder tip pressure in this specification. If the extruder tip pressure is 4 MPa or more, the foaming agent is easily dissolved and dispersed in the resin during melt kneading, and expandable vinyl chloride resin particles can be stably obtained. On the other hand, if the extruder tip pressure is 20 MPa or less, shear heat generation during melt kneading can be suppressed, and decomposition of the vinyl chloride resin and additives is less likely to occur.
[0062] In one embodiment of the method for producing expandable particles, the temperature of the molten resin immediately before being extruded from the die is preferably Tg+20°C or higher, more preferably Tg+20°C to Tg+130°C, even more preferably Tg+30°C to Tg+110°C, and particularly preferably Tg+40°C to Tg+90°C, where Tg is the glass transition temperature of the resin without the foaming agent. In addition, for vinyl chloride resins, the glass transition temperature increases with an increase in the chlorine content, so it is preferable to appropriately adjust the temperature according to the chlorine content of the vinyl chloride resin used. If the temperature is Tg+20°C or higher, the viscosity of the extruded molten resin is low, small hole clogging is unlikely to occur, and the actual small hole opening rate is not reduced, so that the shape of the obtained expandable vinyl chloride resin particles can be prevented from becoming distorted or irregular. On the other hand, if the temperature is Tg+130°C or lower, the extruded molten resin is easily solidified, is less likely to wrap around the rotary cutter, and can be cut stably.
[0063] In one embodiment of the method for producing expandable particles, the die is not particularly limited, but examples thereof include dies having small holes preferably with a diameter of 0.3 mm to 2.0 mm, more preferably 0.4 mm to 1.5 mm.
[0064] In one embodiment of the method for producing expandable particles, the cutting device for cutting the molten resin extruded into the circulating pressurized cooling water is not particularly limited, but examples thereof include a device in which the molten resin is cut into small pellets by a rotating cutter that comes into contact with a die, and then transported to a centrifugal dehydrator to be dehydrated and aggregated without being foamed in the pressurized circulating cooling water.
[0065] The conditions of the pressurized circulating cooling water should be adjusted depending on the types and contents of the resin, additives, foaming agent, etc. used, but the conditions are preferably such that foaming of the molten resin extruded from the die is suppressed and the resin is stably cut by the cutter. Specifically, the temperature condition of the pressurized circulating cooling water is preferably 40°C to 99°C, more preferably 60°C to 90°C.
[0066] As for the pressure conditions, it is preferable to adjust the pressure so that the expansion ratio of the resulting expandable polyvinyl chloride resin particles is 1.0 to 1.25 times. The expansion ratio of the expandable polyvinyl chloride resin particles is determined based on the true density (kg / m 3 ) is the true density (kg / m 3 The true density of the base resin and expandable polyvinyl chloride resin particles referred to here is calculated by dividing the weight W (kg) of polyvinyl chloride resin pellets or expandable polyvinyl chloride resin particles by the volume V (m 3 Specifically, it can be determined by the measurement method described below. Although it depends on the type of foaming agent used, the pressure condition is preferably 0.6 to 2.0 MPa, more preferably 0.7 to 1.8 MPa, and further preferably 0.8 to 1.6 MPa.
[0067] (Polyvinyl chloride resin foam particles and their manufacturing method) The expandable polyvinyl chloride resin particles of the present invention can be used for a foamed molded article after being pre-expanded 2 to 110 times by a heating medium such as heated air or steam to form expanded polyvinyl chloride resin particles (corresponding to pre-expanded particles). The steam that can be used may be saturated steam or superheated steam.
[0068] The heating temperature during foaming should be appropriately adjusted depending on the glass transition temperature and melting point of the resin and the content of the foaming agent, but is preferably 90° C. or higher, and more preferably 100° C. or higher. On the other hand, from the viewpoint of suppressing the variation in expansion ratio among the foamed beads and preventing the shrinkage of the foamed beads, the heating temperature is preferably 150° C. or lower, and more preferably 130° C. or lower.
[0069] (Polyvinyl chloride resin foam molded product and its manufacturing method) The obtained polyvinyl chloride resin foam particles are molded (e.g., molded in a mold) using a conventional molding machine, for example, with steam, to produce a polyvinyl chloride resin foam molded article. Depending on the shape of the mold used, a molded article with a complex shape or a block-like molded article can be obtained.
[0070] The vinyl chloride resin foamed particles and the vinyl chloride resin foamed molded article thereof of the present invention preferably have an average cell diameter of 70 to 1000 μm, more preferably 90 to 800 μm, and even more preferably 100 to 600 μm. By having an average cell diameter within the above range, a vinyl chloride resin foamed molded article having higher heat insulating properties can be obtained. When the average cell diameter is 70 μm or more, there is a tendency that the expansion ratio can be easily increased, and when it is 1000 μm or less, an increase in thermal conductivity, i.e., a deterioration in heat insulating performance can be avoided.
[0071] The vinyl chloride resin foamed beads and the vinyl chloride resin foamed molded article thereof of the present invention preferably have a closed cell ratio of 70% or more, more preferably 80% or more, and even more preferably 90% or more. When the closed cell ratio is within the above-mentioned range, the foamed beads are easily expanded during molding, the foamed beads have good moldability, and the surface properties of the resulting foamed molded article are improved. In addition, when the closed cell ratio is within the above-mentioned range, the strength of the foamed molded article, such as the compressive strength, tends to be increased.
[0072] (Applications of foamed molded products) The foamed molded article molded using the expandable polyvinyl chloride resin particles of the present invention has a high expansion ratio and a high closed cell ratio, and is excellent in flame retardancy. Therefore, it is suitable for achieving weight reduction and high insulation of products and components that require flame retardancy and fire resistance. For example, it is suitable for various applications such as building insulation materials, ceiling materials, core materials for metal sandwich panels, food container boxes, cold storage boxes, cushioning materials, agricultural and fishery boxes, bathroom insulation materials, and hot water tank insulation materials.
[0073] One embodiment of the present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. An embodiment obtained by appropriately combining the technical means disclosed in different embodiments is also included in the technical scope of one embodiment of the present invention. EXAMPLES
[0074] Hereinafter, one embodiment of the present invention will be specifically described based on examples and comparative examples, but the present invention is not limited to these.
[0075] The measurement and evaluation methods in the following examples and comparative examples are as follows.
[0076] <Measurement of particle weight of expandable polyvinyl chloride resin particles> Using an electronic balance capable of measuring to the nearest 0.01 mg, the weight of 100 randomly sampled expandable polyvinyl chloride resin particles was measured, and the particle weight was calculated using the following formula. Grain weight (mg) = [Weight of 100 grains (mg)] / 100
[0077] <True density measurement of polyvinyl chloride resin pellets (base resin)> After blending polyvinyl chloride resin with auxiliary materials such as processing aids, stabilizers, and lubricants to obtain a uniform mixture, it is melted and kneaded in an extruder. The weight of the polyvinyl chloride resin pellets obtained, W3 (kg), is submerged in a measuring cylinder containing ethanol, and the volume V1 (m3) is calculated from the rise in the liquid level of the measuring cylinder (submersion method). 3 ) was calculated using the following formula: True density of polyvinyl chloride resin pellets (kg / m3 )=(W3 / V1) Based on the above method, the true density of the vinyl chloride resin pellets used in the examples and comparative examples was 1430 kg / m 3 This value was used as the density of the base resin used in the examples and comparative examples.
[0078] <Measurement of expansion ratio of polyvinyl chloride resin foam particles> A polyvinyl chloride resin foam particle with a weight of W4 (kg) is submerged in a measuring cylinder containing ethanol, and the volume V2 (m 3 ) was obtained and calculated using the following formula. From the above <Measurement of true density of polyvinyl chloride resin pellets (base resin)>, the base resin density was 1430 kg / m 3 was used. Expansion ratio of polyvinyl chloride resin foam particles (times) = 1430 / (W4 / V2)
[0079] <Evaluation of foaming of expandable polyvinyl chloride resin particles> The expandable polyvinyl chloride resin particles obtained in the examples and comparative examples were measured for the maximum expansion ratio of the polyvinyl chloride resin expanded particles and the amount of the blowing agent contained in the expandable polyvinyl chloride resin particles (amount of the blowing agent during expansion) according to the following measurement method. Note that, in order to properly evaluate the expansion of the expandable polyvinyl chloride resin particles, the following measurements were carried out on the same day.
[0080] <Evaluation of maximum expansion ratio of polyvinyl chloride resin foam particles> A part of the obtained expandable polyvinyl chloride resin particles was put into an oven (forced convection constant temperature dryer SOFW-600, manufactured by AS ONE Corporation) heated to 130°C, and expanded under a heated air atmosphere at a temperature of 130°C by changing the heating time, to obtain expanded particles for each heating time. The heating time was changed at 30 second intervals, such as 30 seconds, 60 seconds, and 90 seconds after putting into the oven, and heating was continued until shrinkage of the expanded particles due to overheating (decrease in the expansion particle expansion ratio) was confirmed. The expansion ratio of the expanded particles obtained for each heating time was measured based on (measurement of expansion ratio of expanded polyvinyl chloride resin particles described above), and the highest expansion ratio among these was determined as the maximum expansion ratio of the expanded polyvinyl chloride resin particles.
[0081] <Measurement of the amount of blowing agent contained in expandable polyvinyl chloride resin particles> Based on the results of measurement of the normal pentane content and the acetone content in the expandable polyvinyl chloride resin particles described below, the sum of normal pentane and acetone contained in the expandable polyvinyl chloride resin particles was determined as the amount of blowing agent.
[0082] <Evaluation of n-pentane content in foamable polyvinyl chloride resin> The normal pentane content in the expandable polyvinyl chloride resin particles was measured by placing about 0.35 g of expandable polyvinyl chloride resin particles in a sealable glass container of about 130 cc (hereinafter referred to as "sealed container") and removing the air from the sealed container using a vacuum pump. The sealed container was then heated at 190 for 15 minutes, and the blowing agent in the expandable resin particles was removed into the sealed container. After the sealed container returned to room temperature, helium was introduced into the sealed container to return it to atmospheric pressure, and the measurement was performed using gas chromatography with the following equipment and measurement conditions. Equipment used: Gas chromatograph GC-2014 [Shimadzu Corporation] Column used: G-Column G-950 25UM [manufactured by Chemicals Evaluation and Research Institute, Japan] Measurement conditions; Column temperature: 110℃ Carrying gas: High purity helium Carry gas flow rate: 40mL / min Detector: TCD
[0083] <Evaluation of acetone content in foamable polyvinyl chloride resin> The acetone content in the expandable polyvinyl chloride resin particles was measured by dissolving 1.0 g of the expandable polyvinyl chloride resin particles in 20 mL of tetrahydrofuran and using gas chromatography under the following apparatus and measurement conditions. Equipment used: Gas chromatograph GC-2014 [Shimadzu Corporation] Column used: G-Column G-100 3UM [manufactured by Chemicals Evaluation and Research Institute, Japan] Measurement conditions; Column temperature: 70℃ · Carrier gas: High-purity helium · Carrier gas flow rate: 20 mL / min · Detector: FID
[0084] <Evaluation of the sum of Log differential pore volumes> The obtained foamed vinyl chloride resin particles were evaluated for the sum of Log differential pore volumes under the following conditions using Autopore IV 9500 (manufactured by Micromeritics, USA).
[0085] 0.35 g of the foamed vinyl chloride resin particles was weighed as a sample and then added to the cell described below. The cell used was a cell for powder, with a sample chamber volume of 5 cc, a maximum measurement volume of 0.366 cc, a total stem volume of 0.392 cc, a maximum mercury head pressure of 4.45 psia, a cell constant of 11.117 μL / pF, and external dimensions of I 215 mm, H 230 mm, and D 1.473 mm. Also, the Correction method was set to None and the measurement was performed without correction. The cell with the sample was evacuated to 50 μmHg and further evacuated for 5 minutes. After filling the evacuated cell with mercury at a pressure of 1.52 psia, the pressure was increased from 2 to 33000 psia to perform porosity evaluation. In the specification, the amount of mercury that penetrated into the sample within the pressure range of 20 to 33000 psia is referred to as porosity. The amount of mercury that penetrated into the pores can be determined from the displacement of the mercury column in the sample container. The displacement is calculated from the change in capacitance between the mercury and the electrodes on the tube wall of the sample container. Autopore IV 9500 calculates the displacement of the mercury column from the measured capacitance using a capacitance-type detector and calculates the amount of mercury (porosity) that penetrated into the sample.
[0086] The pressure profile during measurement was as follows. The pressure was increased to the specified pressure and the measurement was performed with an equilibrium time of 10 seconds.
[0087] 2psia、3psia、4psia、5.5psia、7psia、8.5psia、10.5psia、13psia、16psia、20psia、23psia、25psia、30psia、40psia、50psia、60psia、75psia、90psia、115psia、140psia、175psia、220psia、270psia、330psia、420psia、520psia、640psia、700psia、800psia、990psia、1200psia、1300psia、1400psia、1500psia、1600psia、1700psia、1900psia、2050psia、2200psia、2350psia、2500psia、2650psia、2700psia、2850psia、3000psia、3250psia、3500psia、3750psia、4000psia、4250psia、4500psia、4740psia、5000psia、5300psia、5500psia、5750psia、6000psia、6250psia、6500psia、6750psia、7000psia、7500psia、8000psia、8500psia、9000psia、9300psia、9600psia、10050psia、10500psia、11000psia、11500psia、12000psia、12600psia、13100psia、13650psia、14000psia、14340psia、14600psia、15000psia、15450psia、15800psia、16200psia、16650psia、17000psia、17350psia、17700psia、18100psia、18450psia、18800psia、19200psia、19800psia、20300psia、20800psia、21200psia、21650psia、22050psia、22650psia、23200psia、23750psia、24100psia、24650psia、25050psia、25450psia、25900psia、26450psia、26950psia、27400psia、27800psia、28250psia、29000psia、29500psia、30000psia, 30450psia, 30900psia, 31300psia, 31800psia, 32350psia, 33000psia, The pore radius during measurement is calculated as r = 2δcosθ / P. r: pore radius, δ: surface tension of mercury, θ: contact angle of mercury, P: intrusion pressure. The pores present in the sample were calculated with the contact angle of mercury set to 130° and the surface tension set to 485 dynes / cm. The intrusion contact angle and the withdrawal contact angle were both set to 130°, and the mercury density was set to 13.5335 g / ml. From the obtained data, the sum of the log differential pore volumes (ml / g) of pores with diameters of 70 to 500 nm was taken as the sum of the log differential pore volumes of pores with diameters of 70 to 500 nm.
[0088] The raw materials used in the examples and comparative examples are shown below. (Vinyl chloride resin) (A-1) Chlorinated polyvinyl chloride resin [Kaneka Corporation, H716S, average degree of polymerization 600, chlorine content 67.6% by weight] (Processing aids) (B-1) Acrylic resin [Kane Ace PA-40, manufactured by Kaneka Corporation] (B-2) Styrene-acrylonitrile copolymer (Galata, Blendex 869, weight average molecular weight 2.86 million, ratio of acrylonitrile-derived components in the copolymer: 20% by weight) (foaming agent) (C-1) Normal pentane [manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.] (C-2) Acetone [Fujifilm Wako Pure Chemical Industries, Ltd.]
[0089] Example 1 [Preparation of expandable polyvinyl chloride resin particles] To 100 parts by weight of vinyl chloride resin (A-1), 13 parts by weight of processing aid (B-2), 5 parts by weight of butyltin mercapto stabilizer, 3 parts by weight of lubricant (ester wax, polyethylene wax), and 5 parts by weight of chlorinated polyethylene with a chlorine content of 35% by weight were added, and the resulting mixture was blended to obtain a uniform mixture, which was then melt-kneaded in a co-rotating intermeshing twin-screw extruder to obtain pellets (vinyl chloride resin composition) with the above-mentioned blending ratio. The obtained pellets were melt-kneaded in a φ40mm co-rotating intermeshing twin-screw extruder at a feed rate of 40 kg / hr. From the middle of the φ40mm co-rotating intermeshing twin-screw extruder, 8.6 parts by weight of normal pentane (C-1) and 3.9 parts by weight of acetone (C-2) were pressed into the extruder with respect to 100 parts by weight of the pellets. After that, the extruder was cooled to a resin temperature of 165°C through a continuous pipe attached to the tip of the twin-screw extruder, a single-screw extruder, a gear pump, and a diverter valve, and extruded at a discharge rate of 45 kg / hr into pressurized circulating water at a temperature of 70°C and 1.3 MPa from a die attached downstream of the diverter valve and set at 230°C with 30 small holes having a diameter of 1.0 mm and a land length of 3.5 mm. The extruder tip pressure at this time was 12 MPa, and the resin temperature of the melt (i.e., the resin temperature of the resin melt at the tip of the extruder) was 167°C. The extruded molten resin is cut and pelletized by a rotating cutter that comes into contact with the die, and then transferred to a centrifugal dehydrator to produce pellets with a weight of 5.5 mg and a true density of 1280 kg / m 3 As a result, expandable polyvinyl chloride resin particles of the above formula were obtained.
[0090] [Evaluation of foaming of expandable polyvinyl chloride resin particles] The resulting expandable polyvinyl chloride resin particles were aged for 3 days at 10°C, and then the amount of blowing agent during expansion and expansion evaluation were carried out according to the above-mentioned <Measurement of the amount of blowing agent contained in expandable polyvinyl chloride resin particles> and <Evaluation of maximum expansion ratio of expanded polyvinyl chloride resin particles>. As a result, the amount of blowing agent during expansion was 9.7% by weight, and the maximum expansion ratio of the expanded particles was 32.6 times. The maximum expansion ratio / amount of blowing agent during expansion was 3.4.
[0091] Example 2 The same procedure as in Example 1 was repeated except that the amount of acetone (C-2) added was changed from 3.9 parts by weight to 2.2 parts by weight, the die temperature was set to 245°C, and the pressurized circulating water temperature was changed to 85°C. The pellet weight was 5.4 mg and the true density was 1300 kg / m 3 The pressure at the tip of the extruder was 14 MPa, and the resin temperature of the molten material was 167°C.
[0092] The amount of foaming agent during foaming and foaming evaluation were carried out for the obtained expandable polyvinyl chloride resin particles in the same manner as in Example 1. As a result, the amount of foaming agent during foaming was 8.7% by weight, and the maximum expansion ratio of the expanded particles was 27.2 times. The maximum expansion ratio / amount of foaming agent during foaming was 3.1.
[0093] Example 3 The same procedure as in Example 2 was repeated except that the amount of acetone (C-2) added was changed from 2.2 parts by weight to 0.9 parts by weight, resulting in a particle weight of 6.0 mg and a true density of 1330 kg / m 3 The pressure at the tip of the extruder was 14 MPa, and the resin temperature of the molten material was 167°C.
[0094] The amount of foaming agent during foaming and foaming evaluation were carried out for the obtained expandable polyvinyl chloride resin particles in the same manner as in Example 1. As a result, the amount of foaming agent during foaming was 8.2% by weight, and the maximum expansion ratio of the expanded particles was 25.9 times. The maximum expansion ratio / amount of foaming agent during foaming was 3.2.
[0095] Example 4 The same procedure as in Example 1 was repeated except that 13 parts by weight of the processing aid (B-2) was changed to 13 parts by weight of (B-1). The grain weight was 5.4 mg and the true density was 1260 kg / m 3 The pressure at the tip of the extruder was 15 MPa, and the resin temperature of the molten material was 167°C.
[0096] The amount of foaming agent during foaming and foaming evaluation were carried out for the obtained expandable polyvinyl chloride resin particles in the same manner as in Example 1. As a result, the amount of foaming agent during foaming was 9.0% by weight, and the maximum expansion ratio of the expanded particles was 24.6 times. The maximum expansion ratio / amount of foaming agent during foaming was 2.7.
[0097] Comparative Example 1 The same procedure as in Example 4 was carried out except that the amount of acetone (C-2) added was changed from 3.9 parts by weight to 0 parts by weight, and the amount of normal pentane (C-1) added was changed from 8.6 parts by weight to 12.5 parts by weight, resulting in a particle weight of 5.6 mg and a true density of 1320 kg / m 3The pressure at the tip of the extruder was unstable at 4 to 11 MPa. The resin temperature of the molten material was 167°C.
[0098] The amount of foaming agent during foaming and foaming evaluation were carried out for the obtained expandable polyvinyl chloride resin particles in the same manner as in Example 1. As a result, the amount of foaming agent during foaming was 5.5% by weight, and the maximum expansion ratio of the expanded particles was 5.0 times. The maximum expansion ratio / amount of foaming agent during foaming was 0.9.
[0099] [Table 1]
Claims
1. Expandable polyvinyl chloride resin particles containing a blowing agent, which satisfy the following (a), (b), (c), and (d): (a) The foaming agent contains a hydrocarbon foaming agent and a ketone foaming agent. (b) The content of the foaming agent is 1 to 30% by weight based on 100% by weight of the expandable polyvinyl chloride resin particles. (c) The sum of the log differential pore volumes of pores having diameters of 70 to 500 nm measured by mercury intrusion porosimetry in the expandable polyvinyl chloride resin particles is 0.300 ml / g or less. (d) Contains chlorinated polyvinyl chloride resin.
2. 2. The expandable polyvinyl chloride resin particles according to claim 1, wherein the ratio of the ketone-based blowing agent is 4 to 70% by weight, when the total amount of the hydrocarbon-based blowing agent and the ketone-based blowing agent is 100% by weight.
3. 3. The expandable polyvinyl chloride resin particles according to claim 1, wherein the boiling point of the ketone foaming agent is 130° C. or lower.
4. 4. The expandable polyvinyl chloride resin particles according to claim 1, wherein the hydrocarbon foaming agent contains at least one saturated hydrocarbon having 4 to 6 carbon atoms.
5. The expandable polyvinyl chloride resin particles according to any one of claims 1 to 4, comprising at least one selected from the group consisting of a copolymer having an aromatic vinyl monomer and an unsaturated nitrile as structural units, an acrylic resin, and a chlorinated polyethylene.
6. 6. The pre-expanded particles of the expandable polyvinyl chloride resin particles according to claim 1.
7. 7. A foamed molded article obtained by using the expandable vinyl chloride resin particles according to any one of claims 1 to 5 or the pre-expanded particles according to claim 6.
8. A method for producing expandable polyvinyl chloride resin particles that satisfies the following (A), (B), (C), and (D): (A) a step of extruding a foaming agent-containing vinyl chloride resin melt obtained by melt-kneading a vinyl chloride resin composition and a foaming agent through a die having a plurality of holes into pressurized water, cutting the extrudate with a rotary cutter to form particles, and then cooling and solidifying the extrudate, (B) the blowing agent includes a hydrocarbon-based blowing agent and a ketone-based blowing agent; (C) the amount of the foaming agent added is 1 to 30 parts by weight based on 100 parts by weight of the vinyl chloride resin composition; (D) The expandable polyvinyl chloride resin particles contain a chlorinated polyvinyl chloride resin.
9. 9. The method for producing expandable polyvinyl chloride resin particles according to claim 8, wherein the ratio of the hydrocarbon-based blowing agent to the ketone-based blowing agent is 96:4 to 30:70 (wt %).
Citation Information
Patent Citations
JP1963-015232B
JP1967-024073B
Manufacture of vinyl chloride resin foamed material
JP1982036631A
Expandable vinyl chloride type resin composition
JP1982137328A
Preparation of molded PVC resin foam
JP1983087135A