Manufacturing method of optical member
By controlling the injection rate and using specific cyclic olefin copolymers, the method addresses surface roughness and mold transferability issues, resulting in optical members with superior smoothness and optical performance.
Patent Information
- Application Number
- JP2020173808
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-15
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2040-10-15
AI Technical Summary
Existing methods for manufacturing cyclic olefin copolymer optical members suffer from surface roughness and inadequate mold transferability, leading to suboptimal optical performance.
The method involves controlling the injection rate of the molten resin composition within the cavity relative to the gate, setting a specific ratio of 1.5 to 6.5, and using an injection compression molding process to enhance mold transferability, ensuring the resin composition is melted at appropriate temperatures and composed of specific cyclic olefin copolymers.
This approach results in optical members with suppressed surface roughness and improved surface smoothness, achieving excellent mold transferability and maintaining desired shapes with enhanced optical properties.
Smart Images

Figure 0007576424000020 
Figure 0007576424000021 
Figure 0007576424000022
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing an optical member. [Background technology]
[0002] Cyclic olefin copolymers have excellent optical properties and are therefore used as optical members such as optical lenses. Techniques relating to a method for producing an optical member made of a cyclic olefin copolymer include those described in Patent Documents 1 and 2, for example.
[0003] Patent Document 1 discloses a method for producing a cyclic olefin resin molded product using an injection molding machine equipped with a specific screw and cylinder. It is described that this manufacturing method suppresses the occurrence of black spots in the resin molded product and provides excellent product yield during continuous operation. However, this document does not disclose anything about the injection rate.
[0004] Patent Document 2 discloses a method for manufacturing an optical recording medium by injection molding, in which the temperature and mold temperature of a cyclic polyolefin-based thermoplastic resin are set within a predetermined range, and the shear rate and the average residence time of the thermoplastic resin in a molding machine are specified. Patent Document 2 also describes a preferred injection speed (paragraph 0037, etc.). It is described that this manufacturing method suppresses the occurrence of silver streaks and provides excellent transferability. However, this document does not describe changing the injection rate of the resin composition depending on the location. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2000-233425 A [Patent Document 2] JP 2001-121569 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, in the manufacturing methods described in Patent Documents 1 and 2, surface roughness may occur on the optical surfaces of the obtained resin molded product, and there is room for improvement in mold transferability. [Means for solving the problem]
[0007] As a result of investigations, the inventors have found that in an injection molding apparatus, the injection rate of the molten resin composition when it passes through a gate is made faster when it is filled into the space (cavity) that forms the molded product in the mold, and that by setting these injection rates at a predetermined ratio, it is possible to improve mold transferability and solve the above-mentioned problems, and have completed the present invention. That is, the present invention can be shown as follows.
[0008] [1] An injection unit comprising a cylinder and a screw inserted into the cylinder; a mold having a cavity for molding an optical member having an optical surface, and a gate serving as an injection port for injecting a molten resin composition from the injection unit into the cavity; A method for producing an optical member using an injection molding apparatus comprising: A step of melting a resin composition containing ethylene or a copolymer of an α-olefin and a cyclic olefin in the cylinder; and using the screw to inject the molten resin composition through the gate to fill the cavity. The injection rate a (cm 3 / sec) of the resin composition in the cavity. 3 / second) is 1.5 to 6.5. [2] The mold comprises a pair of a first mold and a second mold, and is configured such that the first mold moves toward the second mold to compress a space formed between the molds to form the cavity; The filling step includes: The method for manufacturing an optical member described in [1] includes a step of using the screw to inject the molten resin composition into the space through the gate, and moving the first mold toward the second mold to press the resin composition and fill the cavity with the resin composition. [3] The method for producing an optical member according to [1] or [2], wherein the set temperature of the cylinder in the step is a glass transition temperature of the resin composition + 100°C to a glass transition temperature + 180°C. [4] The method for producing an optical member according to [3], wherein the resin composition has a glass transition temperature of 120°C to 160°C. [5] The copolymer, At least one olefin-derived repeating unit (a) represented by the following general formula (I); At least one repeating unit (b) derived from a cyclic olefin selected from the group consisting of a repeating unit represented by the following general formula (II), a repeating unit represented by the following general formula (III), a repeating unit represented by the following general formula (IV), a repeating unit represented by the following general formula (V), and a repeating unit represented by the following general formula (VI), The method for producing an optical member according to any one of [1] to [4], comprising: [ka] (In the above general formula (I), R 300 represents a hydrogen atom or a linear or branched hydrocarbon group having 1 to 29 carbon atoms. [ka] (In the above general formula (II), u is 0 or 1, v is 0 or a positive integer, w is 0 or 1, and R 61 ~R 78 And R a1 and R b1may be the same or different, and each is a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms, a halogenated alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 15 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms; R 75 ~R 78 may be bonded to each other to form a monocyclic or polycyclic ring. [ka] (In the above general formula (III), x and d are 0 or an integer of 1 or more, y and z are 0, 1, or 2, and R 81 ~R 99 may be the same or different, and each is a hydrogen atom, a halogen atom, an aliphatic hydrocarbon group which is an alkyl group having 1 to 20 carbon atoms or a cycloalkyl group having 3 to 15 carbon atoms, an aromatic hydrocarbon group having 6 to 20 carbon atoms, or an alkoxy group; R 89 and R 90 and the carbon atom to which R is bonded. 93 or the carbon atom to which R is bonded 91 may be bonded directly or via an alkylene group having 1 to 3 carbon atoms, and when y=z=0, R 95 and R 92 or R 95 and R 99 may be bonded to each other to form a monocyclic or polycyclic aromatic ring. [ka] (In the above general formula (IV), n and m are each independently 0, 1 or 2, q is 1, 2 or 3, and R 18 ~R 31 each independently represents a hydrogen atom, a halogen atom other than a fluorine atom, or a hydrocarbon group having 1 to 20 carbon atoms which may be substituted with a halogen atom other than a fluorine atom, and when q=1, R 28 and R 29 , R 29 and R 30 , R 30 and R 31may be bonded to each other to form a monocyclic or polycyclic ring, and when q=2 or 3, R 28 and R 28 , R 28 and R 29 , R 29 and R 30 , R 30 and R 31 , R 31 and R 31 may be bonded to each other to form a monocyclic or polycyclic ring, and the monocyclic or polycyclic ring may be an aromatic ring. [ka] (In the above general formula (V), R 100 , R 101 may be the same or different, and represent a hydrogen atom or a hydrocarbon group having 1 to 5 carbon atoms, and f is 1≦f≦18. [ka] (In the above general formula (VI), q is 1, 2 or 3; R 32 ~R 39 each independently represents a hydrogen atom, a halogen atom other than a fluorine atom, or a hydrocarbon group having 1 to 20 carbon atoms which may be substituted with a halogen atom other than a fluorine atom, and when q=1, R 36 and R 37 , R 37 and R 38 , R 38 and R 39 may be bonded to each other to form a monocyclic or polycyclic ring, and when q=2 or 3, R 36 and R 36 , R 36 and R 37 , R 37 and R 38 , R 38 and R 39 , R 39 and R 39 may be bonded to each other to form a monocyclic or polycyclic ring, the monocyclic or polycyclic ring may have a double bond, and the monocyclic or polycyclic ring may be an aromatic ring. [6] The repeating unit (b) derived from the cyclic olefin in the copolymer is bicyclo[2.2.1]-2-heptene, tetracyclo[4.4.0.1 2,5 .1 7,10 The method for producing an optical member according to [5], comprising repeating units derived from at least one compound selected from the group consisting of 1-3-dodecene and benzonorbornadiene. [7] The method for producing an optical member according to [5] or [6], wherein the olefin-derived repeating unit (a) in the copolymer contains an ethylene-derived repeating unit. Effect of the Invention
[0009] According to the method for producing an optical member of the present invention, since the mold transferability is excellent, it is possible to obtain an optical member having a desired shape and excellent surface smoothness in which surface roughness of the optical surface is suppressed. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a schematic cross-sectional view of a mold of an injection molding apparatus. [Diagram 2] FIG. 2 is an optical microscope photograph of the surface (optically effective surface) of the lens obtained in Example 1. [Diagram 3] FIG. 3 is an optical microscope photograph showing the surface roughness that occurred on the surface (optically effective surface) of the lens obtained in Comparative Example 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In all drawings, similar components are given similar reference symbols and their description will be omitted as appropriate. In addition, "~" indicates "above" to "below" unless otherwise specified. First, an injection molding apparatus used in the method for producing an optical member according to this embodiment will be described.
[0012] <Injection molding equipment> As shown in FIG. 1, an injection molding apparatus 10 of this embodiment includes an injection unit 20 and a mold 30.
[0013] The injection unit 20 comprises a cylinder 22 and a screw 24 inserted into the cylinder 22, and is connected to a hopper 26 for feeding a resin composition. The resin composition fed from the hopper 26 is heated and melted in the cylinder 22, and the screw 24 transports the molten resin composition forward and can inject it into the cavity 36 by piston motion. The injection rate of the molten resin can be changed by the forward speed of the screw 24.
[0014] The preferred ranges of the diameters of the cylinder 22, the screw 24, the nozzle, etc. are not particularly limited, as they vary depending on the specifications of the injection molding machine and the size of the molded product. The mold 30 is made up of a first mold 32 and a second mold 34, and has a cavity 36 between these molds for molding an optical member having an optical surface.
[0015] The cavity 36 communicates with a gate 38, which serves as an injection port for injecting the molten resin from the injection unit 20 into the cavity 36. The gate 38 communicates with a runner 40 and a sprue 44, and is configured so that the molten resin injected from the injection unit 20 can be injected and filled into the cavity 36.
[0016] The cavity 36 is an area for molding a desired optical member, and the optical member has a cross-sectional shape of one side convex and one side concave, both sides convex, both sides concave, one side flat and one side concave, one side flat and one side convex, one side flat and one side flat, etc. The optical member may have a circular, elliptical, etc. shape in a plan view.
[0017] The width a between the first mold 32 and the second mold 34 in the cavity 36 can be set to 2 mm or more and 15 mm or less, preferably 2.5 mm or more and 12 mm or less, and more preferably 2.5 mm or more and 10 mm or less. The width of the gate 38 (the width between the first mold 32 and the second mold 34) is about 30% or more and 100% or less of the width a.
[0018] The first mold 32 exposes a molding surface 32a for forming the optical surface of the optical member within the cavity 36. The shape of the molding surface 32a is set to match the shape of the optical surface of the optical member, and may be a convex, concave, or planar shape in cross section, or may be a circle, ellipse, or the like in a plan view. The width of the molding surface 32a (diameter in the case of a circle) is indicated by b in FIG.
[0019] The area of the molding surface 32a is 310 mm 2 More than 5030mm 2 Less than 415mm, preferably 2 More than 2850mm 2 Less than 490mm, more preferably 2 More than 2000mm 2 When the molding surface 32a has a circular shape in a plan view, the diameter b can be set to 20 mm or more and 80 mm or less, preferably 23 mm or more and 60 mm or less, and more preferably 25 mm or more and 50 mm or less.
[0020] The second mold 34 exposes a molding surface 34a for forming the optical surface of the optical member within the cavity 36. The shape of the molding surface 34a is set to match the shape of the optical surface of the optical member, and may be a convex, concave, or planar shape in cross section, or may be a circle, ellipse, or the like in plan view. The width of the molding surface 34a (or the diameter in the case of a circle) is indicated by c in FIG. 1.
[0021] The area of the molding surface 34a is 310 mm 2 More than 5030mm 2 Less than 415mm, preferably 2 More than 2850mm 2 Less than 490mm, more preferably 2 More than 2000mm 2When the molding surface 34a has a circular shape in a plan view, the diameter c can be set to 20 mm or more and 80 mm or less, preferably 23 mm or more and 60 mm or less, and more preferably 25 mm or more and 50 mm or less.
[0022] The preferred numerical ranges for the widths of the runner 40 and the sprue 44 are not particularly limited as long as the injection rate ratio b / a of the resin composition, which will be described later, is ensured.
[0023] In this embodiment, the portion constituting the molding surface 32a of the first mold 32 is configured to be slidable, and the portion moves toward the second mold to compress the space formed between these molds, thereby forming the cavity, so that the injection compression molding apparatus can also be configured.
[0024] <Method of manufacturing optical members> The method for producing an optical member according to this embodiment uses the above-mentioned injection molding apparatus and includes the following steps. Step a: In a cylinder 22, a resin composition containing ethylene or a copolymer of an α-olefin and a cyclic olefin is melted. Step b: Using the screw 24, the molten resin composition is injected through the gate 38 to fill the cavity.
[0025] [Step a] In this process, a resin composition containing ethylene or a copolymer of an α-olefin and a cyclic olefin is charged into a cylinder 22 via a hopper 26, and the resin composition is heated and melted in the cylinder 22. Furthermore, the screw 24 in the cylinder 22 is rotated to move the resin composition to an injection nozzle.
[0026] The temperature of the molten resin composition (cylinder set temperature) can be appropriately determined depending on the glass transition temperature (Tg) and melting point (Tm) of the resin, but is usually "Tg+100° C." to "Tg+180° C.", preferably "Tg+120° C." to "Tg+170° C." The screw rotation speed is not particularly limited, but is usually appropriately selected in the range of 10 to 300 rpm. The resin composition in this embodiment will be described.
[0027] (Resin composition) The resin composition of the present embodiment contains a copolymer of ethylene or an α-olefin and a cyclic olefin.
[0028] The cyclic olefin compound constituting the copolymer according to this embodiment is not particularly limited, and examples thereof include cyclic olefin monomers described in paragraphs 0037 to 0063 of WO 2006 / 118261.
[0029] From the viewpoint of further improving heat resistance and improving moldability while maintaining a good balance between the transparency and refractive index of the resulting molded article, the copolymer according to this embodiment preferably has at least one olefin-derived repeating unit (a) represented by the following general formula (I) and at least one cyclic olefin-derived repeating unit (b) selected from the group consisting of repeating units represented by the following general formula (II), repeating units represented by the following general formula (III), repeating units represented by the following general formula (IV), repeating units represented by the following general formula (V), and repeating units represented by the following general formula (VI).
[0030] For example, the repeating unit (a) may contain two or more types, such as ethylene and propylene. The repeating unit (b) may contain two or more types selected from repeating units represented by the same general formula, or may contain two or more types selected from repeating units represented by different general formulas.
[0031] [ka]
[0032] In the above general formula (I), R 300 represents a hydrogen atom or a linear or branched hydrocarbon group having 1 to 29 carbon atoms.
[0033] [ka]
[0034] In the above general formula (II), u is 0 or 1, v is 0 or a positive integer, preferably an integer of 0 or more and 2 or less, more preferably 0 or 1, w is 0 or 1, R 61 ~R 78 And R a1 and R b1 may be the same or different, and each is a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms, a halogenated alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 15 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms; R 75 ~R 78 may be bonded to each other to form a monocyclic or polycyclic ring.
[0035] [ka]
[0036] In the above general formula (III), x and d are 0 or an integer of 1 or more, preferably an integer of 0 or more and 2 or less, more preferably 0 or 1, y and z are 0, 1, or 2, and R 81 ~R 99 may be the same or different, and each is a hydrogen atom, a halogen atom, an aliphatic hydrocarbon group which is an alkyl group having 1 to 20 carbon atoms or a cycloalkyl group having 3 to 15 carbon atoms, an aromatic hydrocarbon group having 6 to 20 carbon atoms, or an alkoxy group; R 89 and R 90 and the carbon atom to which R is bonded. 93 or the carbon atom to which R is bonded91 may be bonded directly or via an alkylene group having 1 to 3 carbon atoms, and when y=z=0, R 95 and R 92 or R 95 and R 99 may be bonded to each other to form a monocyclic or polycyclic aromatic ring.
[0037] [ka]
[0038] In the above general formula (IV), n and m are each independently 0, 1 or 2, and q is 1, 2 or 3. m is preferably 0 or 1, and more preferably 1. n is preferably 0 or 1, and more preferably 0. q is preferably 1 or 2, and more preferably 1.
[0039] R 18 ~R 31 each independently represents a hydrogen atom, a halogen atom other than a fluorine atom, or a hydrocarbon group having 1 to 20 carbon atoms which may be substituted with a halogen atom other than a fluorine atom; R 18 ~R 31 are each independently preferably a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, and more preferably a hydrogen atom.
[0040] Also, when q=1, R 28 and R 29 , R 29 and R 30 , R 30 and R 31 may be bonded to each other to form a monocyclic or polycyclic ring, and when q=2 or 3, R 28 and R 28 , R 28 and R 29 , R 29 and R 30 , R 30 and R 31 , R 31 and R 31may be bonded to each other to form a monocyclic or polycyclic ring, and the monocyclic or polycyclic ring may be an aromatic ring.
[0041] [ka]
[0042] In the above general formula (V), R 100 , R 101 may be the same or different and represent a hydrogen atom or a hydrocarbon group having 1 to 5 carbon atoms, and f is 1≦f≦18.
[0043] [ka]
[0044] In the above general formula (VI), q is 1, 2 or 3; R 32 ~R 39 each independently represents a hydrogen atom, a halogen atom other than a fluorine atom, or a hydrocarbon group having 1 to 20 carbon atoms which may be substituted with a halogen atom other than a fluorine atom, and when q=1, R 36 and R 37 , R 37 and R 38 , R 38 and R 39 may be bonded to each other to form a monocyclic or polycyclic ring, and when q=2 or 3, R 36 and R 36 , R 36 and R 37 , R 37 and R 38 , R 38 and R 39 , R 39 and R 39 may be bonded to each other to form a monocycle or polycycle, the monocycle or polycycle may have a double bond, and the monocycle or polycycle may be an aromatic ring.
[0045] Among the repeating units (b) represented by general formula (II), (III), (IV), (V) or (VI), it is preferable to have a repeating unit represented by general formula (II). It is also preferred that the polymer contains a repeating unit represented by general formula (II) and any of repeating units represented by general formulas (III), (IV), (V) and (VI). It is more preferable that the repeating unit has the general formula (II) or (VI).
[0046] The olefin monomer, which is one of the copolymerization raw materials of the copolymer according to this embodiment, undergoes addition copolymerization to form the constitutional unit represented by the above general formula (I). Specifically, an olefin monomer represented by the following general formula (Ia) corresponding to the above general formula (I) is used.
[0047] [ka]
[0048] In the above general formula (Ia), R 300 represents a hydrogen atom or a linear or branched hydrocarbon group having 1 to 29 carbon atoms. Examples of the olefin monomer represented by the above general formula (Ia) include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 4,4-dimethyl-1-pentene, 4-ethyl-1-hexene, 3-ethyl-1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-eicosene. From the viewpoint of obtaining a molded product having better heat resistance, mechanical properties, and optical properties, ethylene and propylene are preferred, and ethylene is particularly preferred. Two or more types of olefin monomers represented by the above general formula (Ia) may be used.
[0049] When the total of the structural units constituting the cyclic olefin copolymer according to this embodiment is taken as 100 mol %, the proportion of the olefin-derived repeating unit (a) is preferably 5 mol % or more and 95 mol % or less, more preferably 20 mol % or more and 90 mol % or less, even more preferably 40 mol % or more and 85 mol % or less, and particularly preferably 50 mol % or more and 80 mol % or less. The proportion of repeating units (a) derived from olefins is as follows: 13 It can be measured by C-NMR.
[0050] Cyclic olefin monomer (b), which is one of the copolymerization raw materials of the copolymer according to this embodiment, is addition copolymerized to form a repeating unit (b) derived from a cyclic olefin represented by the above general formula (II), the above general formula (III), the above general formula (IV), the above general formula (V) or the above general formula (VI). Specifically, cyclic olefin monomer (b) represented by general formulas (IIa), (IIIa), (IVa), (Va) and (VIa) corresponding to the above general formula (II), the above general formula (III), the above general formula (IV), the above general formula (V) and the above general formula (VI) are used.
[0051] [ka]
[0052] In the above general formula (IIa), u is 0 or 1, v is 0 or a positive integer, preferably an integer of 0 or more and 2 or less, more preferably 0 or 1, w is 0 or 1, R 61 ~R 78 And R a1 and R b1 may be the same or different, and each is a hydrogen atom, a halogen atom, an alkyl group having 1 to 20 carbon atoms, a halogenated alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 15 carbon atoms, or an aromatic hydrocarbon group having 6 to 20 carbon atoms; R 75 ~R 78 may be bonded to each other to form a monocyclic or polycyclic ring.
[0053] [ka]
[0054] In the above general formula (IIIa), x and d are 0 or an integer of 1 or more, preferably an integer of 0 or more and 2 or less, more preferably 0 or 1, y and z are 0, 1, or 2, and R 81 ~R 99 may be the same or different, and each is a hydrogen atom, a halogen atom, an aliphatic hydrocarbon group which is an alkyl group having 1 to 20 carbon atoms or a cycloalkyl group having 3 to 15 carbon atoms, an aromatic hydrocarbon group having 6 to 20 carbon atoms, or an alkoxy group; R 89 and R 90 and the carbon atom to which R is bonded. 93 or the carbon atom to which R is attached 91 may be bonded directly or via an alkylene group having 1 to 3 carbon atoms, and when y=z=0, R 95 and R 92 or R 95 and R 99 may be bonded to each other to form a monocyclic or polycyclic aromatic ring.
[0055] [ka]
[0056] In the above general formula (IVa), n and m are each independently 0, 1 or 2, and q is 1, 2 or 3. m is preferably 0 or 1, and more preferably 1. n is preferably 0 or 1, and more preferably 0. q is preferably 1 or 2, and more preferably 1.
[0057] R 18 ~R 31 each independently represents a hydrogen atom, a halogen atom other than a fluorine atom, or a hydrocarbon group having 1 to 20 carbon atoms which may be substituted with a halogen atom other than a fluorine atom; R 18~R 31 are each independently preferably a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, and more preferably a hydrogen atom.
[0058] Also, when q=1, R 28 and R 29 , R 29 and R 30 , R 30 and R 31 may be bonded to each other to form a monocyclic or polycyclic ring, and when q=2 or 3, R 28 and R 28 , R 28 and R 29 , R 29 and R 30 , R 30 and R 31 , R 31 and R 31 may be bonded to each other to form a monocyclic or polycyclic ring, and the monocyclic or polycyclic ring may be an aromatic ring.
[0059] [ka]
[0060] In the above general formula (Va), R 100 , R 101 may be the same or different and represent a hydrogen atom or a hydrocarbon group having 1 to 5 carbon atoms, and f is 1≦f≦18.
[0061] [ka]
[0062] In the above general formula (VIa), q is 1, 2 or 3, preferably 1 or 2, and more preferably 1.
[0063] R 32 ~R 39each independently represents a hydrogen atom, a halogen atom other than a fluorine atom, or a hydrocarbon group having 1 to 20 carbon atoms which may be substituted with a halogen atom other than a fluorine atom. R 32 ~R 39 are each independently preferably a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, and more preferably a hydrogen atom.
[0064] Also, when q=1, R 36 and R 37 , R 37 and R 38 , R 38 and R 39 may be bonded to each other to form a monocyclic or polycyclic ring, and when q=2 or 3, R 36 and R 36 , R 36 and R 37 , R 37 and R 38 , R 38 and R 39 , R 39 and R 39 may be bonded to each other to form a monocycle or polycycle, the monocycle or polycycle may have a double bond, and the monocycle or polycycle may be an aromatic ring.
[0065] Examples of the hydrocarbon group having 1 to 20 carbon atoms include, independently, an alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 15 carbon atoms, and an aromatic hydrocarbon group. More specifically, examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, an amyl group, a hexyl group, an octyl group, a decyl group, a dodecyl group, and an octadecyl group. Examples of the cycloalkyl group include a cyclohexyl group. Examples of the aromatic hydrocarbon group include an aryl group or an aralkyl group such as a phenyl group, a tolyl group, a naphthyl group, a benzyl group, and a phenylethyl group. These hydrocarbon groups may be substituted with a halogen atom other than a fluorine atom.
[0066] By using the olefin monomer represented by the above-mentioned general formula (Ia) or the cyclic olefin monomer (b) represented by the general formula (IIa), (IIIa), (IVa), (Va) or (VIa) as the copolymerization component, the solubility of the cyclic olefin polymer (A) in a solvent is further improved, resulting in good moldability and improved product yield.
[0067] Specific examples of the cyclic olefin monomer (b) represented by the general formula (IIa), (IIIa) or (Va) that can be used include the compounds described in paragraphs 0037 to 0063 of WO 2006 / 118261.
[0068] Specifically, bicyclo-2-heptene derivatives (bicyclohept-2-ene derivatives), tricyclo-3-decene derivatives, tricyclo-3-undecene derivatives, tetracyclo-3-dodecene derivatives, pentacyclo-4-pentadecene derivatives, pentacyclopentadecadiene derivatives, pentacyclo-3-pentadecene derivatives, pentacyclo-4-hexadecene derivatives, pentacyclo-3-hexadecene derivatives, hexacyclo-4-heptadecene derivatives, and heptacyclo-5-eicosene derivatives. conductors, heptacyclo-4-eicosene derivatives, heptacyclo-5-heneicosene derivatives, octacyclo-5-docosene derivatives, nonacyclo-5-pentacosene derivatives, nonacyclo-6-hexacosene derivatives, cyclopentadiene-acenaphthylene adducts, 1,4-methano-1,4,4a,9a-tetrahydrofluorene derivatives, 1,4-methano-1,4,4a,5,10,10a-hexahydroanthracene derivatives, and cycloalkylene derivatives having 3 to 20 carbon atoms.
[0069] Among the cyclic olefin monomers (b) represented by the general formula (IIa), (IIIa), (IVa), (Va) or (VIa), the cyclic olefin represented by the general formula (IIa) is preferred.
[0070] It is also preferable to use a cyclic olefin represented by general formula (IIa) and any one of cyclic olefins represented by general formulas (IIIa), (IVa), (Va) and (VIa).
[0071] Examples of the cyclic olefin monomer (b) represented by the above general formula (IIa) include bicyclo[2.2.1]-2-heptene (also called norbornene), tetracyclo[4.4.0.1 2,5 .1 7,10 ]-3-dodecene (also called tetracyclododecene) is preferably used, and tetracyclo[4.4.0.1 2,5 .1 7,10 It is more preferable to use ]-3-dodecene. These cyclic olefins have a rigid ring structure, and therefore have the advantage that the elastic modulus of the copolymer and the molded article is easily maintained.
[0072] As the cyclic olefin monomer (b) represented by the above general formula (VIa), it is preferable to use a monomer in which q=1 in formula (VIa). Since these cyclic olefins have one benzene ring, they have the advantage that it is easier to obtain a resin composition that is less likely to be colored than when they have two or more benzene rings. In particular, it is preferable to use benzonorbornadiene. The advantage of using benzonorbornadiene is that it has an aromatic ring, so the refractive index of the resin composition can be increased.
[0073] When the total of the structural units constituting the copolymer according to this embodiment is taken as 100 mol %, the proportion of the repeating units (b) derived from the cyclic olefin monomer (b) is preferably 5 mol % or more and 95 mol % or less, more preferably 10 mol % or more and 80 mol % or less, even more preferably 15 mol % or more and 60 mol % or less, and particularly preferably 20 mol % or more and 50 mol % or less.
[0074] The copolymer type of the copolymer according to the present embodiment is not particularly limited, but may be, for example, a random copolymer, a block copolymer, etc. In the present embodiment, it is preferable to use a random copolymer as the copolymer according to the present embodiment, from the viewpoint of obtaining an optical member having excellent optical properties such as transparency, refractive index, and birefringence and high precision. The copolymer according to this embodiment may contain one or more of the copolymers described above.
[0075] The copolymer according to the present embodiment is a copolymer of ethylene and tetracyclo[4.4.0.1 2,5 .1 7,10 ]-3-dodecene, random copolymers of ethylene and bicyclo[2.2.1]-2-heptene, and random copolymers of ethylene and tetracyclo[4.4.0.1 2,5 .1 7,10 ]-3-dodecene and benzonorbornadiene are preferred, and ethylene and tetracyclo[4.4.0.1 2,5 .1 7,10 ]-3-dodecene and ethylene / tetracyclo[[4.4.0.1 2,5 .1 7,10 A random copolymer of 1-dodecene and benzonorbornadiene is more preferred.
[0076] (Other Ingredients) In addition to the cyclic olefin copolymer, the resin composition in this embodiment may contain known additives as optional components within a range that does not impair the excellent physical properties of the optical member in this embodiment.
[0077] Examples of the additives include hydrophilic stabilizers, hydrophilic agents, antioxidants, secondary antioxidants, lubricants, release agents, anti-fogging agents, weather resistance stabilizers, light resistance stabilizers, ultraviolet absorbers, antistatic agents, and metal deactivators. Among the above, the resin in this embodiment preferably contains a hydrophilic stabilizer, which is more preferable since the deterioration of optical performance under high temperature and high humidity conditions can be suppressed by containing a hydrophilic stabilizer.
[0078] The hydrophilic stabilizer is preferably a fatty acid ester of a fatty acid and a polyhydric alcohol, more preferably a fatty acid ester of a fatty acid and a polyhydric alcohol having one or more ether groups.
[0079] In this embodiment, the lower limit of the content of the copolymer in the resin composition is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more, when the entire resin composition is taken as 100% by mass. By having the content of the copolymer in the resin composition be equal to or more than the above lower limit, the optical performance can be further improved. The upper limit of the content of the cyclic olefin copolymer (A) in the resin composition is not particularly limited, but is, for example, 100 mass % or less.
[0080] The glass transition temperature (Tg) of the resin composition of this embodiment is preferably 120 to 160° C., more preferably 125 to 155° C., and even more preferably 130 to 150° C. When the glass transition temperature (Tg) of the resin composition is in the above range, by combining with the injection speed ratio and the set temperature of the cylinder in this embodiment described later, the molded product has excellent mold transferability, a desired shape, and is more suppressed in surface roughness of the optical surface. Furthermore, when the molded product is used as an optical component that requires heat resistance, such as an in-vehicle camera lens or a camera lens for a mobile device, sufficient heat resistance can be obtained.
[0081] In this embodiment, when there are multiple glass transition temperatures, such as when the resin composition contains two or more types of the copolymers or contains other components having a glass transition temperature, the higher glass transition temperature is used.
[0082] The glass transition temperature (Tg) of the resin composition of this embodiment can be measured, for example, using an RDC220 manufactured by SII Nanotechnology Inc., by heating the resin composition in a nitrogen atmosphere from room temperature to 200°C at a heating rate of 10°C / min, holding the temperature for 5 minutes, then cooling the resin composition to 30°C at a heating rate of 10°C / min, holding the temperature for 5 minutes, and then heating the resin composition to 200°C at a heating rate of 10°C / min.
[0083] [Step b] In this step, the molten resin composition obtained in step a is injected through a gate 38 using a screw 24 to fill the cavity 36 .
[0084] Specifically, the nozzle at the tip of the cylinder 22 opens and the screw 24 moves forward, causing the molten resin composition to pass through the sprue 44 and the runner 40 and be injected via the gate 38 .
[0085] From the viewpoint of the effect of the present invention, the injection rate a (cm 3 / sec) of the molten resin composition in the cavity 36, 3 The ratio b / a (the number of times per second) can be set to 1.5 to 6.5, preferably 2.0 to 6.0, and more preferably 2.5 to 5.5.
[0086] By satisfying the injection rate ratio b / a, the mold transferability is excellent, and therefore it is possible to provide optical components such as optical lenses having a desired shape and excellent surface smoothness with reduced surface roughness on the optical surface.
[0087] The injection rate of the sprue 44 and the runner 40 is not particularly limited, but from the viewpoint of productivity, it is preferably equal to or higher than the injection rate of the molten resin composition passing through the gate 38 .
[0088] The injection rate and filling rate of the molten resin can be changed by adjusting the forward movement speed of the screw 24, and the injection rate and filling rate of the molten resin can be determined by the forward movement speed.
[0089] The step b can also be carried out using an injection compression molding machine. 1, an injection compression molding device can be used that is configured so that the first mold 32 moves toward the second mold 34 to compress the space formed between these molds and form the cavity 36. Specifically, a portion that constitutes the molding surface 32a of the first mold 32 is configured to be slidable, and the portion moves toward the second mold 34 to compress the space formed between these molds and form the cavity 36.
[0090] In step b, when an injection compression molding apparatus is used, the screw 24 is used to inject the molten resin composition into the space through the gate 38, and the portion constituting the molding surface 32a of the first mold 32 is moved toward the second mold 34 to compress the space into the shape of the cavity 36, thereby pressing the molten resin composition and filling the cavity 36 with the molten resin composition.
[0091] The length of compression from the space to the cavity 36 (compression allowance) varies depending on the size of the cavity 36, but can be set to 500 to 5000 μm, preferably 1000 to 4000 μm, and more preferably 1500 to 3000 μm. In addition to adjusting the injection rate, applying stress due to compression molding to the molten resin composition improves mold transferability, making it possible to obtain optical components having a desired shape and a smooth surface with reduced surface roughness on the optical surface, and furthermore, to obtain optical components with smaller birefringence.
[0092] After step b, the resin in the mold is cooled and solidified according to a conventional method, and then the mold is opened and the resin molded product (optical component) is taken out. The cooling time is not particularly limited, but is usually 1 to 500 seconds.
[0093] [Optical components] The resin molded product (optical member) obtained by the manufacturing method of this embodiment has a circular effective optical surface (diameter b) and another circular effective optical surface (diameter c) on the back surface thereof. The manufacturing method of this embodiment is excellent in terms of mold transferability, and the optical surfaces of the obtained optical members are prevented from having surface roughness.
[0094] The optical member according to this embodiment contains the cyclic olefin copolymer (A), and therefore has excellent optical performance. Therefore, it can be suitably used as an optical member in an optical system that requires highly accurate identification of an image. The optical member is a part used in optical equipment, and specifically includes a sensor lens, a pickup lens, a projector lens, a prism, an fθ lens, an imaging lens, a light guide plate, etc., and from the viewpoint of the effect according to this embodiment, it can be suitably used as an fθ lens, an imaging lens, a sensor lens, a prism, or a light guide plate.
[0095] Examples of the lens shape include a convex lens with spherical surfaces on both sides, a concave lens with spherical surfaces on both sides, a lens with one spherical and convex surface and the other aspheric surface, a lens with one spherical and concave surface and the other aspheric surface, a diffractive lens, a Fresnel lens, a wafer lens, a wafer lens array, and a laminate of wafer lens arrays.
[0096] In particular, since the optical member according to this embodiment has a desired shape and the surface roughness of the optical surface is suppressed, it can be used not only for the above-mentioned conventional optical member applications, but also for optical members such as in-vehicle camera lenses and camera lenses for mobile devices (mobile phones, smartphones, tablets, etc.). Examples of in-vehicle camera lenses and camera lenses for mobile devices include view camera lenses, sensing camera lenses, lenses for light convergence in head-up displays, lenses for light diffusion in head-up displays, and lenses in various optical devices such as cameras for personal computers, cameras for mobile phones, cameras for smartphones, cameras for tablet terminals, cameras for mobile devices, digital cameras, and cameras for medical devices. Note that the in-vehicle camera may be one that captures visible images, infrared images, or both, and in the case of visible images, it may be a black-and-white image or a color image. In addition, examples of applications other than the above include automobile interior panels, automobile lamp lenses, automobile inner lenses, automobile lens protective covers, automobile light guides, and the like. The optical member according to this embodiment can be particularly suitably used for in-vehicle applications.
[0097] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted as long as they do not impair the effects of the present invention. EXAMPLES
[0098] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these.
[0099] <Production Example> <Preparation of Resin Composition> (Catalyst Preparation) VO(OC2H5)Cl2 was diluted with cyclohexane to prepare a vanadium catalyst with a vanadium concentration of 6.7 mmol / L-cyclohexane. 1.5 Cl 1.5) was diluted with cyclohexane to prepare an organoaluminum compound catalyst having an aluminum concentration of 107 mmol / L-hexane.
[0100] (polymerization) A stirred polymerization vessel (inner diameter 500 mm, reaction volume 100 L) was used to continuously polymerize ethylene and tetracyclo[4.4.0.1 2,5 .1 7,10 A copolymerization reaction was carried out with ethylene and 1-3-dodecene. Here, ethylene was fed into the polymerization vessel together with hydrogen gas. When carrying out this copolymerization reaction, the vanadium catalyst prepared by the above method was fed into the polymerization vessel in such an amount that the vanadium catalyst concentration relative to the cyclohexane used as the polymerization solvent in the polymerization vessel was 0.6 mmol / L. In addition, ethylaluminum sesquichloride, an organoaluminum compound, was fed into the polymerization vessel in such an amount that Al / V=18.0. The polymerization temperature was set to 8°C, and the polymerization pressure was set to 1.8 kg / cm. 2 As G, the copolymerization reaction was carried out continuously.
[0101] (Decalcification) Ethylene and tetracyclo[4.4.0.1 2,5 .1 7,10 The polymerization reaction was terminated by adding water and a 25% by weight aqueous solution of sodium hydroxide as a pH regulator to the copolymer solution. The catalyst residues present in the copolymer were removed (demineralized) from the copolymer solution. 2,5 .1 7,10 To a cyclohexane solution (polymer concentration 7.7% by mass) of a copolymer of 3-dodecene and pentaerythrityl-tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate] was added as a stabilizer such that the amount added to the copolymer was 0.4 parts by mass per 100 parts by mass of the copolymer. Then, before entering the flash drying process, the copolymer was temporarily dried in a 1.0 m 3 The mixture was mixed for 1 hour using a stirring tank.
[0102] (Desolvation) 20kg / cm as heat source 2 A cyclohexane solution of the copolymer, in which the concentration of the copolymer in the cyclohexane solution was 5% by mass, was supplied at a rate of 150 kg / h to a double-tube heater (outer tube diameter 2B, inner tube diameter 3 / 4B, length 21 m) using G water vapor, and heated to 180°C. 25kg / cm as heat source 2 Using a double-tube flash dryer (outer tube diameter 2B, inner tube diameter 3 / 4B, length 27m) and a flash hopper (volume 200L) using G steam, the cyclohexane solution of the copolymer that had been subjected to the heating step was used to remove most of the unreacted monomers together with the polymerization solvent cyclohexane, resulting in flash-dried molten ethylene and tetracyclo[4.4.0.1 2,5 .1 7,10 A random copolymer with 1,3-dihydro-1,3-diphenylphosphine (1,3-diphenylphosphine)-3-dodecene (cyclic olefin copolymer) was obtained. The glass transition temperature Tg (°C) of the cyclic olefin copolymer was evaluated by the method described below and was found to be 155°C.
[0103] (Extrusion) Rikemal DO-100 (Riken Vitamin Co., Ltd.) as a fatty acid ester was heated at 100°C for 4 hours and in a molten state, 0.9 parts by mass per 100 parts by mass of the cyclic olefin copolymer was directly charged into a vented twin-screw kneading extruder, kneaded with the cyclic olefin copolymer charged through the resin charging section of the extruder, and pelletized using an underwater pelletizer attached to the outlet of the extruder. The resulting pellets were dried with hot air at 100°C for 4 hours to obtain a resin composition.
[0104] [Glass transition temperature Tg(℃)] The glass transition temperature Tg of the resin composition was measured under an N2 (nitrogen) atmosphere using a DSC-6220 manufactured by Shimadzu Science Co., Ltd. The resin composition was heated from room temperature to 200°C at a heating rate of 10°C / min, held for 5 minutes, then cooled to -20°C at a heating rate of 10°C / min, and held for 5 minutes. The glass transition temperature (Tg) of the resin composition was obtained from the endothermic curve when the temperature was raised to 200°C at a heating rate of 10°C / min. The glass transition temperature (Tg) was 130°C.
[0105] (Production of optical components) <Example 1> The obtained resin composition was injection molded to produce an optical lens using an injection molding machine (ROBOSHOT α-S30iA manufactured by Fanuc Corporation) as shown in Fig. 1 under conditions of a cylinder 22 temperature of 260°C and a mold 30 temperature of 130°C. The injection rate was set by the short shot method described below, by checking the position of the resin flow front passing through gate 38 and varying the speed. The injection rate was before passing through gate 38 (sprue 44 and runner 40): 0.76 cm 3 / s, when passing through gate 38: 0.18 cm 3 / s, effective lens surface: 0.76cm 3 / s. (Injection rate setting (short shot method)) The forward distance of the screw 24 was gradually increased from the metering completion position in the cylinder 22, and an investigation was conducted into how far the leading edge of the resin flow was injected into the molding area (inside the cavity 36) of the mold 30 depending on the forward distance of the screw 24. At this time, no holding pressure was applied to prevent the resin from being injected due to holding pressure. Using this method, the forward distance (cm) and forward time (seconds) of the screw 24 when the leading edge of the resin flow passed through the gate 38 were measured. The forward speed of the screw 24 was controlled by the injection molding machine 10, and the injection rate was set using the following formula. Formula: Injection rate (cm 3 / s) = Cross-sectional area inside the cylinder 22 of the injection molding machine (cm 2 ) x forward speed of screw 24 (cm / s)
[0106] <Comparative Examples 1 to 5> A resin molded article (optical member) was prepared in the same manner as in Example 1, except that the conditions shown in Table 1 were used.
[0107] [Surface roughness] The optically effective surface of the optical member molded by the molding surface 32a of the first mold 32 was observed under an optical microscope (30x). The evaluation was based on the following criteria. (standard) 〇: No surface roughness ×: Surface roughness occurs
[0108] FIG. 2 shows an optical microscope photograph of the optically effective surface (no surface roughness) of the optical component obtained in Example 1, and FIG. 3 shows an optical microscope photograph showing the surface roughness that occurred on the optically effective surface of the optical component obtained in Comparative Example 5.
[0109] [Table 1] [Explanation of symbols]
[0110] 10 Injection molding equipment 20 Launch unit 22 cylinders 24 Screw 26 Hopper 30 Mold 32 First Mold 32a Molding surface 34 Second Mold 34a Molding surface 36 Cavity 38 Gate 40 Runner 44 sprues
Claims
1. an injection unit comprising a cylinder and a screw inserted into the cylinder; a mold having a cavity for molding an optical member having an optical surface, and a gate serving as an injection port for injecting a molten resin composition from the injection unit into the cavity; A method for producing an optical member using an injection molding apparatus comprising: In the cylinder, ethylene and tetracyclo[4.4.0.1 2,5 .1 7,10 a step of melting a resin composition containing an addition polymer of ]-3-dodecene; and using the screw to inject the molten resin composition through the gate to fill the cavity. The injection rate a (cm) of the resin composition when passing through the gate 3 / sec) of the resin composition in the cavity, b (cm 3 / second) is 1.5 to 6.
5.
2. the mold is composed of a pair of a first mold and a second mold, and the first mold is configured to move toward the second mold to compress a space formed between the molds to form the cavity, The filling step includes:
2. The method for manufacturing an optical component according to claim 1, further comprising the steps of: using the screw to inject the molten resin composition into the space through the gate; and moving the first mold toward the second mold to press the resin composition and fill the cavity with the resin composition.
3. A method for manufacturing an optical component described in claim 1 or 2, wherein the set temperature of the cylinder in the process of melting the resin composition is between the glass transition temperature of the resin composition + 100°C and the glass transition temperature + 180°C.
4. The method for producing an optical member according to claim 3, wherein the resin composition has a glass transition temperature of 120°C to 160°C.
Citation Information
Patent Citations
Injection controlling device
JP1986263724A
Molding method and molding
JP1999300778A
Manufacture of cyclic olefin-based resin molding body
JP2000233425A
Toric lens
JP2001074915A
Method for producing optical recording medium
JP2001121569A