Low thermal expansion alloy
A cost-effective low thermal expansion alloy with improved hot workability is achieved through optimized element ratios and inclusion formation, addressing manufacturing challenges and strain rate issues in existing Invar-based alloys.
Patent Information
- Application Number
- JP2022005149
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-01-17
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2042-01-17
AI Technical Summary
Existing Invar-based alloys face challenges in achieving low thermal expansion and excellent hot workability while maintaining cost-effectiveness, with issues such as high manufacturing costs due to the need for expensive low-S raw materials and difficulties in controlling boron addition, and questionable strain rate methods for evaluating hot workability.
A low thermal expansion alloy composition is developed with specific ranges of C, Si, Mn, S, Ni, Co, Nb, Ca, and Fe, optimized to form NbC and CaS inclusions, ensuring stable hot workability and low thermal expansion, using conventional production methods.
The alloy achieves a thermal expansion coefficient comparable to ceramics or quartz glass with excellent hot workability, suitable for high-thermal stability applications, and is produced at a lower cost by controlling element ratios and inclusions.
Smart Images

Figure 0007576585000001 
Figure 0007576585000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a low thermal expansion alloy having excellent hot workability. [Background technology]
[0002] Invar alloys have little thermal deformation and excellent dimensional stability, so hot-worked Invar alloys are widely used as parts materials for electronics and semiconductor-related equipment, laser processing machines, and ultra-precision processing equipment.
[0003] General-purpose Invar alloys are low-thermal expansion Fe alloys with high Ni content, and since they solidify in austenite single phase structure, coarse columnar crystals tend to form in the ingots used for hot working. As a result, low-melting-point coarse sulfide inclusions segregate at grain boundaries, making it easy for cracks to occur starting from the sulfide inclusions during hot working.
[0004] Patent Document 1 proposes an Invar alloy that has high strength, excellent hot workability, low manufacturing cost, and a low thermal expansion coefficient. The alloy in Patent Document 1 contains, by weight, C: 0.015-0.10%, Si: 0.35% or less, Mn: 1.0% or less, P: 0.015% or less, S: 0.0010% or less, Cr: 0.3% or less, Ni: 35-37%, Mo: 0-0.5%, V: 0-0.05%, Al: 0.01% or less, Nb: 0.15% or more but less than 1.0%, Ti: 0.003% or less, N: 0.005% or less, B: 0.0005-0.005%, and the balance being Fe and unavoidable impurities.
[0005] Patent Document 2 also proposes an Invar-based low thermal expansion alloy with excellent hot workability. The alloy of Patent Document 2 contains, by mass%, C: 0.04% or less, Si: more than 0.15 and 0.5% or less, Mn: 0.5% or less, S: 0.050% or less, Ni: 31 to 36%, Co: 2 to 6.5%, Al: more than 0.03 and 0.20% or less, Mg: 0 to 0.05%, Ca: 0 to 0.02%, Ce: 0 to 0.05%, La: 0 to 0.05%, Ti: 0 to 0.05%, B: 0.001 to 0.020%, and N: 0.0050% or less, with the balance being Fe and unavoidable impurities, and has an average thermal expansion coefficient of 1×10 at 25 to 100° C. -6 ~8×10 -6 / °C or less, and the reduction in area measured in a tensile test at 900°C is 50% or more. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 10-17997 [Patent Document 2] JP 2018-145491 A Summary of the Invention [Problem to be solved by the invention]
[0007] The Invar alloy disclosed in Patent Document 1 aims to improve hot workability by extremely reducing the S content to 0.0010% or less (preferably 0.0005% or less). To achieve this, it is necessary to use expensive low-S raw materials, and molten steel desulfurization using advanced equipment is indispensable, which poses problems of significant restrictions and increased manufacturing costs.
[0008] In addition, in the Invar alloy disclosed in Patent Document 2, B plays an important role in improving hot workability. However, since B has an extremely low solubility in steel and has a high affinity with oxygen and nitrogen, it is difficult to add B in a narrow control range on the order of ppm, and there is a problem that it is difficult to reliably prevent ingot cracking during hot forging. In addition, when the reduction of area, which is an index of hot workability evaluation, is measured, the strain rate of the tensile test is 0.07 to 0.08 s -1 Since this is an extremely small strain rate compared to the actual hot working conditions, there is doubt as to its validity as a test method for evaluating the hot workability of alloy materials.
[0009] An object of the present invention is to provide a low thermal expansion alloy that has a low thermal expansion coefficient equivalent to that of low thermal expansion ceramics and quartz glass, and has excellent hot workability, which can be provided stably at low cost. [Means for solving the problem]
[0010] The present inventors have conducted extensive research to obtain a low thermal expansion alloy that has a low thermal expansion coefficient equivalent to that of low thermal expansion ceramics and quartz glass, and has excellent hot workability that can be provided stably at low cost. As a result, they have found that a low thermal expansion alloy with excellent hot workability can be obtained stably at low cost by adding each element within a range based on the relational formula for the combination of each element of C and Nb, and S and Ca.
[0011] The present invention has been completed based on the above findings, and provides the following means.
[0012] (1) by mass%, C: 0.05-0.12%, Si: 0.2% or less, Mn: 0.2-0.5, S: 0.01% or less, Ni: 31.0-33.0%, Co: 4.0-6.0, Nb: 0.35-0.88%, Ca: 0.035% or less; It is expressed as Ni+0.8Co. Ni equivalent: 35.5~36.5%, When the carbon content is [C] and the niobium content is [Nb], if [C]≧[Nb]×7.74, it is expressed as [Nb]×1.13, and if [C]<[Nb]×7.74, it is expressed as [C]×8.74. Stoichiometric NbC: 0.40-1.0%, 2.0≦Ca / S≦4.0, and the balance being Fe and unavoidable impurities. The average thermal expansion coefficient at 10-40°C is 0.5×10-6 / °C or less.
[0013] (2) The strain rate is 1 s -1 The low thermal expansion alloy according to (1), characterized in that the reduction in area at 900°C in the above tensile test is 60% or more. Effect of the Invention
[0014] According to the present invention, a low thermal expansion alloy having a low thermal expansion coefficient equivalent to that of low thermal expansion ceramics and quartz glass, excellent hot workability, and capable of being stably provided at low cost can be obtained. Therefore, the low thermal expansion alloy of the present invention is suitable for materials requiring high thermal dimensional stability and good internal quality. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, an embodiment of the present invention will be described in detail. In the following description, "%" regarding the composition of a component represents "mass %" unless otherwise specified. In the following description, the thermal expansion coefficient may be referred to as α.
[0016] First, the composition of the components will be described.
[0017] When Nb is contained in the alloy, C combines with Nb to form NbC, which suppresses the coarsening of crystal grains, and accordingly suppresses the coarsening of low-melting-point sulfides, and has the effect of preventing hot cracking. An effective hot crack prevention effect can be obtained by controlling the C and Nb contents so that the amount of NbC is within a certain range. However, if the C content is less than 0.05%, the hot crack prevention effect is small, and if it exceeds 0.12%, NbC becomes excessive, which leads to a decrease in hot workability and a decrease in tool life that cannot be ignored. In addition, C in excess of the amount necessary for NbC formation dissolves in the matrix, increasing the C concentration in the matrix and promoting aging (long-term dimensional change). Therefore, the C content is set to the range of 0.05 to 0.12%.
[0018] Although Si may be added as a deoxidizer, if the Si content exceeds 0.2%, α increases, so the Si content is set to 0.2% or less.
[0019] Mn is added because it combines with a deoxidizer and S to form MnS, improving hot workability. However, if the Mn content is less than 0.2%, the effect is not sufficient, and if it exceeds 0.5%, the desired α cannot be obtained due to the increase in α. Therefore, the Mn content is set to the range of 0.2 to 0.5%.
[0020] S is an element contained as an unavoidable impurity, and exists mostly as sulfide inclusions. When sulfide inclusions segregate at grain boundaries, hot workability is significantly deteriorated, but they can be rendered harmless by adding Ca, as described below. However, if the S content exceeds 0.01%, the amount of Ca added to render the inclusions harmless increases, decreasing the cleanliness of the molten metal and instead deteriorating the hot workability. Therefore, the S content is set to 0.01% or less.
[0021] Ni is an essential element that lowers α together with Co, which will be described later. The low thermal expansion alloy of the present invention is intended to be used together with low thermal expansion ceramics, optical glass, etc., as will be described later, and α is adjusted to the desired 0.5 ppm / °C or less by the synergistic effect with Co, which will be described later. However, if the content is less than 31.0%, the stability of the structure at low temperatures decreases, and if it exceeds 33.0%, the amount of Co according to the Ni equivalent range described later becomes small, making it impossible to obtain the desired α. Therefore, the Ni content is set to the range of 31.0 to 33.0%.
[0022] Co is added together with the above-mentioned Ni to obtain an extremely small α of 0.5 ppm / °C or less. For this purpose, the Co content must be 4.0% or more. However, according to the Ni equivalent range described later, if the Co content exceeds 6.0%, the Ni content becomes small and the stability of the structure at low temperatures decreases. Therefore, the Co content is set to the range of 4.0 to 6.0%.
[0023] The Ni equivalent is expressed as Ni + 0.8 × Co, and is an index for obtaining a desired α. The low thermal expansion alloy of the present invention is intended to be used together with low thermal expansion ceramics, optical glass, etc., and in order to adjust α to the desired value of 0.5 ppm / °C or less, the Ni equivalent is set to a range of 35.5 to 36.5%.
[0024] Ca is an important element for improving hot workability. As described above, Ca combines with S to form CaS, which converts sulfides into CaS with a high melting point, thereby generating sulfides within the grains and preventing segregation to grain boundaries. Furthermore, it changes the shape of inclusions to spherical shapes, preventing stress concentration during hot working. If the Ca content exceeds 0.035%, it is in excess of the upper limit of S concentration of 0.01% in the alloy of the present invention, and the cleanliness of the molten metal decreases, resulting in a decrease in the effect of improving hot workability. Therefore, the Ca content is set to 0.035% or less.
[0025] Ca / S is an important index for controlling the morphology of sulfides to CaS. If Ca / S is less than 2.0, the morphology of MnS cannot be sufficiently controlled, and sulfides are difficult to spheroidize. On the other hand, if Ca / S exceeds 4.0, coarse Ca-based oxides are generated, and the effect of preventing hot cracking is reduced. Therefore, Ca / S is set to the range of 2.0 to 4.0.
[0026] Nb combines with C to form NbC, which inhibits the coarsening of crystal grains as described above, thereby inhibiting the coarsening of low melting point sulfides and preventing hot cracking. As described above, a significant effect of preventing hot cracking can be obtained by controlling C and Nb so that the amount of NbC falls within a certain range. However, if the Nb content is less than 0.35% or exceeds 0.88%, the desired amount of NbC cannot be obtained. Therefore, the Nb content is set to 0.35 to 0.88%.
[0027] As described above, NbC has the effect of suppressing the coarsening of crystal grains, and its stoichiometric content is expressed as [Nb] × 1.13 when [C] ≧ [Nb] × 7.74, when [C] < [Nb] × 7.74, and as [C] × 8.74, when [C] < [Nb] × 7.74, when [C] ≧ [Nb] × 7.74. If the stoichiometric NbC content is less than 0.40%, the crack prevention effect is small, and if it exceeds 1.0%, NbC becomes excessive and hot workability is deteriorated. Therefore, the stoichiometric NbC content range is set to 0.40 to 1.0%.
[0028] The balance of the composition is Fe and inevitable impurities. The inevitable impurities refer to substances that are inevitably mixed in from raw materials, the production environment, etc., when a steel having the composition specified in the present invention is industrially produced.
[0029] By using an alloy having the above chemical components, it is possible to obtain a low thermal expansion part having excellent hot workability.
[0030] The low thermal expansion alloy having the composition of the present invention is intended to be used together with low thermal expansion ceramics, optical glass, etc., and has an average thermal expansion coefficient of 0.5×10 at 10 to 40°C. -6 / ℃ or less.
[0031] The apparatus and method used for producing the low thermal expansion alloy of the present invention are not particularly limited, and conventional apparatus and methods can be used. After hot working the cast ingot, a low thermal expansion member can be obtained by a predetermined machining process or the like.
[0032] The hot workability of the low thermal expansion alloy of the present invention can be evaluated by measuring the reduction of area in a hot working reproduction test such as the Thermec Master test. Specifically, the low thermal expansion alloy of the present invention has a reduction of area of 1s at 900°C. -1 The reduction in area measured in a tensile test at the above strain rate is preferably 60% or more.
[0033] Furthermore, a heat treatment may be performed to further reduce the thermal expansion coefficient. When this heat treatment is performed, it is performed before machining, i.e., after hot working. The specific heat treatment conditions are that the alloy material after hot working is heated to preferably 750 to 1050°C, more preferably 850 to 950°C, and held at that temperature for 0.5 to 2 hours per 25 mm of material thickness, and then rapidly cooled. The cooling rate is 100°C / min or more.
[0034] After the low thermal expansion heat treatment, the material may be held at 300 to 350° C. for 1 to 4 hours per 25 mm of wall thickness, and then subjected to stress relief annealing by slow cooling, such as furnace cooling. EXAMPLES
[0035] The molten metal having the composition shown in Table 1 obtained by air melting was cast into a mold of φ120×270, and the obtained ingot was used as a test material for the evaluation test described later.
[0036] The hot workability of the alloy was evaluated by holding the ingot at 850°C for 2 hours, water cooling, and then holding it at 325°C for 4 hours and furnace cooling, after which test pieces of φ10mm×100mm were taken and subjected to tensile tests under the conditions shown in Table 2, and the reduction of area was measured. The measurement results are shown in Table 1.
[0037] The hot workability of the alloy was confirmed by hot forging the ingot to 75 mm x 540 mm, machining the forged product on all six sides to remove surface scale, and forming a product of 70 mm x 400 mm. The surface was then subjected to a penetrant inspection. The hot workability was evaluated as follows: "○" indicates that no indications due to scratches were observed, and "×" indicates that an indication was observed. The forged product was then held at 850°C for 2 hours, water-cooled, and then held at 325°C for 4 hours, furnace-cooled. Test pieces of φ6 mm x 50 mm were then taken for measuring the thermal expansion coefficient, and the average thermal expansion coefficient between 10 and 40°C was measured. The results of these measurements are also shown in Table 1.
[0038] As shown in Table 1, the low thermal expansion alloy of the present invention has an average thermal expansion coefficient of 0.5 ppm / °C or less between 10 and 40°C, and further has a thermal expansion coefficient of 3.1 s in a tensile test at 900°C. -1At this high strain rate, a reduction in area of 60% or more was achieved.
[0039] In contrast, in the comparative examples, the target properties of at least one of hot workability and thermal expansion coefficient were not obtained.
[0040] [Table 1]
[0041] [Table 2]
Claims
【Request 1】 The alloy contains, by mass%, C: 0.05-0.12%, Si: 0.2% or less, Mn: 0.2-0.5%, S: 0.01% or less, Ni: 31.0-33.0%, Co: 4.0-6.0%, Nb: 0.35-0.88%, and Ca: 0.035% or less. The Ni equivalent expressed as Ni+0.8Co is 35.5-36.5%, the C content is [C], and the Nb content is [Nb ], when [C] ≥ [Nb] x 7.74, it is represented by [Nb] x 1.13, and when [C] < [Nb] x 7.74, it is represented by [C] x 8.
74. Stoichiometric NbC: 0.40 to 1.0%, and 2.0 ≤ Ca / S ≤ 4.0, with the balance being Fe and unavoidable impurities, and the average thermal expansion coefficient at 10 to 40°C is 0.5 x 10 -6 / °C or less. 【Request 2】 Strain rate is 1s -1 2. The low thermal expansion alloy according to claim 1, characterized in that the reduction in area at 900° C. in the above tensile test is 60% or more.
Citation Information
Patent Citations
Free-cutting casting alloy combining high strength with low thermal expansion and its production
JP1989055364A
Low thermal expansion cast iron and production thereof
JP1996269613A
High strength invar alloy excellent in hot workability
JP1998017997A
High strength low thermal expansion alloy
JP1998310845A
Low thermal expansion alloy